A liquid packaging bag and its manufacturing method
By designing irregularly shaped drain outlets and concave-convex drainage channels in liquid packaging bags, combined with double-sided molds and symmetrical laser cutting, the problems of liquid residue and uneven tearing in liquid packaging bags are solved, achieving efficient liquid discharge and neat tearing effect.
Patent Information
- Application Number
- CN202611581373.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing liquid packaging bags are prone to leaving residue during drainage, the upper and lower films of the easy-tear opening are not aligned, and the channels on the front and back of the drainage structure are misaligned, resulting in poor drainage and poor tearing effect.
The design employs an irregularly shaped drain outlet and a concave-convex structure for the drainage channel. The inner surfaces of the upper and lower films respectively form protrusions and grooves, creating a drainage channel with a convex-convex fit. Combined with double-sided molds and symmetrical laser cutting technology, it ensures precise alignment of the channels on the front and back sides, and completes cutting and heat sealing simultaneously on the bag making production line.
It achieves high-precision alignment of the drainage channel, ensuring complete liquid discharge, neat tear-off without leakage, reducing liquid residue on the wall, and is suitable for continuous industrial production.
Smart Images

Figure CN123105098A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of flexible packaging technology, and in particular to a liquid packaging bag with an irregularly shaped drain outlet and a drainage channel, and a method for manufacturing the same. Background Technology
[0002] Liquid packaging bags are widely used in the packaging of liquid products in industries such as food, daily chemicals, and pharmaceuticals. However, existing liquid packaging bags often suffer from issues during drainage, with contents easily remaining at the bag opening and clinging to the bag walls. This hinders drainage, especially towards the end of the drainage process, where surface tension causes the liquid to adhere to the inner wall of the bag, making complete drainage difficult and resulting in waste and a poor user experience.
[0003] Regarding easy-tear openings, existing technologies mostly use mechanical cutting, which can easily lead to problems such as leakage or uneven tearing. Although there are also solutions using double-sided lasers in the industry, the laser marking process is separated from the bag making process. The upper and lower films are marked separately before bag making and lamination. Due to the influence of film feeding accuracy and repeatability error, the upper and lower films are not aligned accurately, which affects the tearing effect.
[0004] Regarding the flow-guiding structure, existing flow-guiding structures mostly adopt the method of two male molds pressing separately, that is, the upper and lower films are pressed by independent male molds at different stations, and then aligned and bonded after pressing. The channels on the front and back are prone to misalignment, the fit of the flow-guiding channels is low, and the flow-guiding effect is not ideal. Another patent document with publication number CN103640773A discloses a flexible packaging bag with flow channels, which places a single-sided embossed forming steel plate between two stacked films, and forms an indentation line by pressing with upper and lower flat molds with temperature and pressure. However, its forming steel plate only has embossed texture, the upper and lower molds are flat, the films themselves do not form a concave-convex interlocking structure, and its tear line is processed on one side after stacking, still having the problem of insufficient fit between the front and back. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a liquid packaging bag and its manufacturing method, solving technical problems such as excessive liquid residue in existing liquid packaging bags, poor tearing effect due to inaccurate alignment of the upper and lower films of the easy-tear opening, and misalignment of the channels on the front and back of the drainage structure.
[0006] The liquid packaging bag of the present invention is made of two composite films, an upper film and a lower film, which are heat-sealed together and have an irregularly shaped drain outlet; the inner wall of the bag near the irregularly shaped drain outlet has a drainage channel with a concave-convex structure; the irregularly shaped drain outlet has a cutting line that does not cut through the composite film.
[0007] The drainage channel is formed by the concave and convex structures formed on the inner surfaces of the upper and lower films. Both the inner surfaces of the upper and lower films have protrusions protruding into the bag and grooves recessed outward. The protrusions of the upper film correspond to the protrusions of the lower film, and the grooves of the upper film correspond to the grooves of the lower film, so that the upper and lower films form a drainage channel with concave and convex structures on the inner wall of the bag after they are attached.
[0008] The groove has a width of 0.3–5 mm and a height of 0.2–3 mm. After the upper and lower membranes are attached, the grooves of the upper membrane and the corresponding grooves of the lower membrane are joined to form a flow guide channel. The flow guide channel 3 can be a single channel or a combination of multiple parallel or radial channels.
[0009] The cutting line extends from one edge of the irregularly shaped drain outlet to the other edge. The cutting depth of the cutting line is 1–100 μm; the shape of the cutting line is a single straight line, a single curve, or a combination of multiple straight lines and curves.
[0010] The inner layer of the composite membrane is a PE heat-sealing layer; the PE heat-sealing layer contains a hydrophobic silylated polyolefin; the amount of silylated polyolefin added is 5% to 35% of the total mass of the heat-sealing layer. The silylated polyolefin has a melt index of 0.5 to 10 g / 10 min at 190°C and a load of 2.16 kg, a weight-average molecular weight of 50,000 to 300,000, and a silyl group grafting rate of 0.5% to 3.0%.
[0011] The manufacturing method of the liquid packaging bag of the present invention includes the forming of a drainage channel: a double-sided male mold is set between the upper film and the lower film, an upper female mold is set above the upper film and a lower female mold is set below the lower film; the upper female mold and the lower female mold are heated and pressed towards each other, so that the ribs on the upper surface of the male mold located in the middle press the upper film into the groove of the upper female mold, and at the same time, the ribs on the lower surface of the male mold press the lower film into the groove of the lower female mold. Meanwhile, the protrusions on the surfaces of the upper female mold and the lower female mold press the upper film and the lower film into the corresponding recesses on the upper and lower surfaces of the male mold, so that the upper film and the lower film each form a convex-concave structure with both protrusions and recesses, thereby simultaneously forming convex-concave drainage channel indentations on the upper film and the lower film. The upper film and the lower film are heat-sealed and bonded to form a drainage channel.
[0012] The raised ribs on the upper surface of the male mold correspond one-to-one with the raised ribs on the lower surface of the male mold in the vertical direction, and the recesses on the upper surface of the male mold correspond one-to-one with the recesses on the lower surface of the male mold in the vertical direction.
[0013] Because the mold is a double-sided integrated structure, the protrusions and grooves on the upper and lower films are formed in one go at the same station and in the same mold, resulting in high alignment accuracy and perfect matching of the grooves on both sides. The cutting line is formed by two symmetrically arranged laser emitters cutting the upper surface of the upper film and the lower surface of the lower film respectively. The laser only cuts through the surface layer of the composite film, without cutting through the intermediate barrier layer and the inner heat-sealing layer, thus forming a symmetrical, non-penetrating cutting line with consistent depth on both sides. Laser marking is completed synchronously on the bag-making production line, with the upper and lower laser heads positioning and marking synchronously, solving the problem of misalignment between the upper and lower films. The inner layer of the composite film is a PE heat-sealing layer, which contains a hydrophobic material, silylated polyolefin, at a concentration of 5% to 35%, giving the inner wall of the bag low surface energy and reducing liquid residue. The manufacturing process is carried out in the following order: slitting → bottom heat sealing → laser cutting → heat sealing → die cutting.
[0014] The hot-pressing temperature is 60–180°C, the hot-pressing pressure is 0.1–1.0 MPa, and the holding time is 0.5–5 s.
[0015] The master mold is a silicone elastic master mold with a Shore hardness of 30-70A. The master mold can also be a hard aluminum alloy metal master mold.
[0016] The cutting lines are formed by laser lines emitted from laser emitters cutting the surfaces of the upper and lower membranes. Two laser emitters are symmetrically arranged, one above the other, to cut the upper surface of the upper membrane and the other the lower surface of the lower membrane, respectively, forming cutting lines that do not cut through the upper and lower composite membranes. The cutting lines formed on the upper and lower surfaces are symmetrical. Preferably, the laser power is 10–200W, the pulse frequency is 5–60kHz, the scanning speed is 100–5000mm / s, and the defocusing amount is 0–5mm.
[0017] Furthermore, the laser emitter is a carbon dioxide laser with a wavelength of 10.6 μm, a laser power of 5–50 W, a pulse frequency of 1–25 kHz, a scanning speed of 50–400 m / min, and a defocusing amount of +0.2–+2 mm (positive defocusing). The laser emitter is a carbon dioxide laser with a wavelength of 10.6 μm. In some specific embodiments, the manufacturing method of the liquid packaging bag is carried out in the following order: 1) The composite membrane is cut into upper and lower symmetrical membrane sheets by the slitting unit; 2) The bottoms of the upper and lower films are partially heat-sealed by heat-sealing unit A to form the bottom of the liquid packaging bag; 3) The upper and lower films pass through a cutting unit, which consists of two symmetrical laser emitters. The laser lines emitted by the laser emitters cut the surfaces of the upper and lower films, forming cutting lines that do not cut through the upper and lower composite films, and the formed cutting lines are symmetrical. 4) The upper and lower diaphragms pass through a hot pressing unit, which uses an upper female mold, a lower female mold, and a double-sided male mold located between them. After heating and pressing, the drainage channel indentation of the concave-convex structure is formed. 5) The upper and lower films are heat-sealed together by the heat-sealing unit B to form a drainage channel and simultaneously form the heat-sealed edge shape of the irregularly shaped drain outlet, thus obtaining the liquid packaging bag body; 6) The liquid packaging bag body is die-cut by a die-cutting unit to obtain a liquid packaging bag containing an irregularly shaped drain outlet.
[0018] Compared with the prior art, the present invention has the following beneficial effects: (1) Precise alignment of the drainage channel: The mold structure of "upper and lower female mold sandwiching the middle double-sided male mold" is adopted. The concave and convex structures of the upper and lower diaphragms are formed synchronously in the same station and the same mold. The alignment accuracy of the front and back channels is high and the fit is good. The drainage channel is completely closed and the drainage guidance effect is significant.
[0019] (2) Easy-tear opening is neat and reliable: The laser emitters are arranged symmetrically at the top and bottom for synchronous positioning and cutting. The cutting line depth is consistent and the position is symmetrical on both sides. It only cuts through the surface layer of the film without cutting through the inner heat-sealing layer, which ensures uniform tearing force and neat tear opening, and avoids the risk of leakage caused by cutting through. Moreover, the laser cutting is completed synchronously on the bag making production line, and the upper and lower laser heads are positioned synchronously, which solves the problem of misalignment of the upper and lower films.
[0020] (3) Less liquid residue: The concave-convex structure of the drainage channel guides the liquid to the irregularly shaped drainage port for centralized discharge. Combined with the silylated polyolefin liquid-repellent material added to the PE heat-sealing layer, the liquid residue on the wall is significantly reduced, and the drainage is more thorough.
[0021] (4) Reasonable process and suitable for continuous production: The laser cutting and hot pressing composite film convex and concave-convex structure are completed before the side heat sealing, avoiding the impact of post-heat sealing processing on the sealing strength; each process is independent and controllable, the product consistency is good, and it is suitable for industrial continuous production. Attached Figure Description
[0022] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 This is a schematic diagram of the overall structure of the liquid packaging bag of the present invention; Figure 2 This is a schematic diagram of the cross-section of the drainage channel; Figure 3 A magnified view of the irregularly shaped drain outlet and the laser cutting line; Figure 4 This is a schematic diagram of the hot pressing unit structure; Figure 5 This is a schematic diagram of the laser unit.
[0024] Explanation of reference numerals in the attached drawings: 1-Bag body; 2-Irregularly shaped drain outlet; 3-Guide groove; 4-Laser cutting line; 5-Heat-sealed edge; 6-Bag bottom; 7-Upper female mold; 8-Lower female mold; 9-Male mold (double-sided); 10-Upper diaphragm; 11-Lower diaphragm; 12-Upper laser head; 13-Lower laser head; 14-Composite membrane; 15-Groove; 16-Protrusion. Detailed Implementation
[0025] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.
[0026] Therefore, the following detailed description of the embodiments of the invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the invention without inventive effort are within the scope of protection of the invention.
[0027] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0028] like Figure 1-3 The liquid packaging bag shown includes a bag body 1, which is made of an upper film 10 (see...). Figure 4 ) and lower membrane 11 (see Figure 4 The bag is manufactured by heat sealing around its perimeter. A uniquely shaped drain outlet 2 is located at one corner of the upper part of the bag body 1. A drainage channel is located on the inner wall of the bag near the drain outlet 2, and the drain outlet 2 has a laser-cut line 4. The bag body 1 has a heat-sealed edge 5 and a bottom 6. Figure 2As shown, the cross-section of the drainage channel has a concave-convex fit structure. The inner surface of the upper diaphragm 10 has a groove 15 and a protrusion 16, and the inner surface of the lower diaphragm 11 has a corresponding groove 15 and a protrusion 16. After the upper diaphragm 10 and the lower diaphragm 11 are attached, a drainage channel for liquid to pass through is formed between the groove 15 and the protrusion 16.
[0029] The width W of the groove 15 is 0.3–5 mm, and the height H is 0.2–3 mm. For example... Figure 2 As shown, after the upper and lower membranes are attached, the groove 15 of the upper membrane and the corresponding groove 15 of the lower membrane are joined to form a flow guide trough 3. The flow guide trough 3 can be a single channel or a combination of multiple parallel or radial channels. In this embodiment, the flow guide trough 3 is a combination of two radial channels.
[0030] The manufacturing method of the liquid packaging bag of the present invention is as follows: Step 1: Slitting. The composite membrane is slitting into upper and lower symmetrical sheets via a slitting unit; Step 2: Heat sealing the bottom of the bag. The bottoms of the upper and lower films are partially heat-sealed by heat-sealing unit A to form the bottom of the liquid packaging bag; Step 3: Laser cutting. The upper and lower films pass through a cutting unit, which consists of two symmetrical laser emitters. The laser lines emitted by the laser emitters cut the surfaces of the upper and lower films, forming cutting lines that do not cut through the upper and lower composite films, and the formed cutting lines are symmetrical. Step 4: Hot-pressing the drainage channel. The upper and lower diaphragms pass through a hot-pressing unit, which uses an upper female mold, a lower female mold, and a double-sided male mold located between them. After heating and pressing, the drainage channel indentation with the concave and convex structure is formed. Step 5: Side heat sealing. The upper and lower films are heat-sealed together by heat sealing unit B to form a drainage channel and simultaneously form the heat-sealed edge shape of the irregularly shaped drain outlet, thus obtaining the liquid packaging bag body; Step 6: Die-cutting. The liquid packaging bag body is die-cut by the die-cutting unit to obtain a liquid packaging bag containing an irregularly shaped drain outlet.
[0031] Specifically, such as Figure 4As shown, the drainage channel is manufactured using a hot-press molding process. The hot-press unit includes an upper female mold 7, a lower female mold 8, and a male mold 9. The upper female mold 7 is located above the upper diaphragm 10, and its lower surface has grooves and protrusions corresponding to the shapes of the protrusions 16 and grooves 15 on the upper diaphragm 10. The lower female mold 8 is located below the lower diaphragm 11, and its upper surface has grooves and protrusions corresponding to the shapes of the protrusions 16 and grooves 15 on the lower diaphragm 11. The male mold 9 is located between the upper diaphragm 10 and the lower diaphragm 11, and has a double-sided structure. Its upper surface has ribs that mate with the grooves of the upper female mold and recesses that mate with the protrusions of the upper female mold, and its lower surface has ribs that mate with the grooves of the lower female mold and recesses that mate with the protrusions of the lower female mold. During molding, the upper female mold 7 and the lower female mold 8 move towards each other, and are heated and pressurized. The raised ribs on the upper surface of the male mold 9 press the upper diaphragm 10 into the groove of the upper female mold 7, while the raised ribs on the lower surface of the male mold 9 press the lower diaphragm 11 into the groove of the lower female mold 8. Simultaneously, the raised surfaces of the upper and lower female molds 7 and 8 press the upper diaphragm 10 and lower diaphragm 11 into the recesses on the upper and lower surfaces of the male mold 9, respectively. This creates a textured structure with both raised ribs 16 and recesses 15 on the upper and lower diaphragms, thus simultaneously pressing out indentations for the flow channels on both the upper and lower diaphragms. The female mold can be a textured metal mold or a mold made of elastic materials such as silicone, achieving hard pressing and soft forming, resulting in a clearer flow channel outline and less damage to the diaphragm. Because the male mold 9 is an integral double-sided structure, the indentations for the flow channels of the upper and lower diaphragms are formed in one step at the same station, resulting in high alignment accuracy.
[0032] Furthermore, the process parameters for the hot pressing molding are as follows: hot pressing temperature 80–180℃, hot pressing pressure 0.1–1.0 MPa, and holding time 0.5–5 s. Within this parameter range, the composite film is heated to a state where the inner heat-sealing layer softens but does not melt or flow. Under the interlocking of the male and female molds, a clearly defined drainage channel indentation is formed, without the film shrinking or deforming due to excessive temperature, or the heat-sealing layer being punctured. The hot pressing temperature is selected based on the melting point of the inner heat-sealing layer of the composite film; for PE heat-sealing layers, 110–170℃ is preferred. The pressure and holding time are matched according to the groove depth and film thickness of the composite film; the greater the groove depth and the thicker the film, the greater the required pressure and the longer the holding time.
[0033] When the master mold is made of elastic materials such as silicone, the silicone master mold has a Shore A hardness of 40-70, a compression rate of 10%-30% during molding, a springback rate of not less than 80%, a long-term operating temperature range of -60 to 200℃, and can withstand short-term temperatures of 230℃. The silicone master mold undergoes elastic deformation under pressure and evenly covers the diaphragm. After pressure is released, it quickly springs back to its original position, achieving "hard pressure, soft molding": the rigid male mold provides precise concave and convex contours, while the elastic female mold compensates for film thickness tolerances and ensures uniform stress on the diaphragm, thus obtaining a full-contour, dimensionally stable drainage channel structure without damaging the diaphragm. If the Shore A hardness is too low, the master mold lacks rigidity and the channel shape is prone to collapse; if it is too high, the elastic compensation capability decreases and the diaphragm is easily damaged. Therefore, a Shore A hardness of 50-60 is preferred.
[0034] like Figure 3 and Figure 5 As shown, the laser cutting line 4 is positioned at the root of the edge of the irregularly shaped drain port 2. The cutting unit includes an upper laser head 12 (i.e., Figure 5 The upper laser emitter and the lower laser head 13 (i.e., the upper laser emitter) Figure 5 The upper and lower laser emitters are symmetrically arranged and synchronously positioned. The laser emitted by the upper laser head 12 is focused by a focusing lens to irradiate the upper surface of the upper membrane 10, and the laser emitted by the lower laser head 13 is also focused by its focusing lens to irradiate the lower surface of the lower membrane 11, cutting synchronously from top to bottom. The laser only cuts through the surface layer of the composite membrane 14, or through the surface and middle layers without cutting through the inner heat-sealing layer, thus preventing leakage of the bag during transportation. The cutting lines formed on the upper and lower surfaces are symmetrical, with consistent depth, uniform force during tearing, and neat tear edges. A carbon dioxide laser can be used. The shape of the cutting line can be a single straight line, a single curve, or a combination of multiple straight lines and curves, with a cutting depth ranging from 1 to 100 μm, adjusted according to the total thickness of the membrane.
[0035] Furthermore, the carbon dioxide laser has a wavelength of 10.6 μm, a laser power of 5–50 W, a pulse frequency of 1–25 kHz, a scanning speed of 50–400 m / min, and a defocusing amount of +0.2–+2 mm (positive defocusing). By employing positive defocusing, the laser spot diffuses appropriately on the film surface, reducing the energy density. Combined with lower power and higher scanning speed, this achieves a "half-cut" effect, removing only the surface material without damaging the inner layer. By adjusting the power, scanning speed, and defocusing amount, the cutting depth can be precisely controlled within the range of 1–100 μm. The upper and lower laser heads are driven, synchronously positioned, and synchronously emitted by the same control system, ensuring that the positional deviation of the cutting lines on the front and back sides is no greater than 0.05 mm.
[0036] The inner layer of the composite membrane 14 is a PE heat-sealing layer. A liquid-repellent silyl-alkylated polyolefin is added to the PE heat-sealing layer. This material can migrate to the surface of the heat-sealing layer, reducing surface energy and allowing the liquid to form a larger contact angle on the inner wall of the bag, reducing wall adhesion and residue. The amount of silyl-alkylated polyolefin added is 5% to 35% of the total mass of the heat-sealing layer. The outer and middle layers of the composite membrane can be selected according to the barrier requirements of the contents.
[0037] The silylated polyolefin is a graft polymer in which a hydrolyzable alkoxysilyl group is grafted onto the main chain of a polyolefin. It typically uses polyethylene or ethylene-α-olefin copolymer as the main chain, with a -Si(OR)3 group (R being methyl or ethyl) grafted onto the main chain, i.e., trimethoxysilyl [-Si(OCH3)3] or triethoxysilyl [-Si(OC2H5)3]. It is typically prepared by free radical grafting of polyethylene with vinyltrimethoxysilane (VTMS) or vinyltriethoxysilane (VTES). Its repeating structure can be summarized as: -(CH2-CH2). m -CH(Si(OR)3)-CH2-(CH2-CH2) n -
[0038] The silane-grafted polyolefin has a melt index of 0.5–10 g / 10 min at 190°C and a load of 2.16 kg, a weight-average molecular weight of 50,000–300,000, and a silane grafting rate (silane content) of 0.5%–3.0% (mass fraction). Commercially available grades include, but are not limited to, Dow SI-LINK series silane-grafted polyethylene, Borealis Visico series, and similar domestically produced silane-grafted polyolefin products. It can be granulated separately and then blended with the PE heat-sealing matrix resin in a specific ratio, or it can be added online during blown film or cast film formation.
[0039] The hydrophobic mechanism is as follows: During the film-forming thermal processing, low surface energy silane groups migrate and accumulate on the film surface due to thermodynamic incompatibility with the PE matrix (surface segregation), forming a low-energy layer rich in siloxane groups on the heat-sealing layer surface. This increases the contact angle of water and aqueous contents on the inner wall of the bag, reduces their spreading and adhesion abilities, and thus reduces wall residue. This surface enrichment can be verified by the following methods: First, X-ray photoelectron spectroscopy (XPS) is used to determine the silicon / carbon atom ratio (Si / C ratio) on the heat-sealing layer surface. The Si / C ratio on the film surface with added silane-alkylated polyolefin is significantly higher than its bulk average level, proving that silane groups migrate and accumulate on the surface. Second, the static contact angle of deionized water on the heat-sealing layer surface is measured using a contact angle meter. Without the addition, it is about 70° to 75°, and after adding 20% to 30%, it can be increased to over 100°.
[0040] Example 1 The bag is manufactured using a PA / VMPET / PE composite film structure (the PE heat-sealing layer does not contain hydrophobic materials) and the above-described process. The drainage channel consists of four parallel channels; the groove width (W) of groove 15 is 3mm, and the height (H) is 1.5mm. The hot-pressing temperature is 160℃, the pressure is 0.4MPa, and the pressure is held for 1s. A carbon dioxide laser is used for laser cutting, with a cutting depth of 12μm, cutting only through the PA surface layer. The cutting line is straight, and the upper and lower laser heads are synchronously positioned for marking. The irregularly shaped drainage port is located at the upper right corner of the bag, in a beveled nozzle shape.
[0041] Example 2 It is basically the same as Example 1, except that 5% silylated polyolefin is added to the PE heat-sealing layer.
[0042] Example 3 It is basically the same as Example 1, except that the amount of silylated polyolefin added in the PE heat-sealing layer is 10%.
[0043] Example 4 It is basically the same as Example 1, except that the amount of silylated polyolefin added in the PE heat-sealing layer is 15%.
[0044] Example 5 It is basically the same as Example 1, except that the amount of silylated polyolefin added in the PE heat-sealing layer is 20%.
[0045] Example 6 It is basically the same as Example 1, except that the amount of silylated polyolefin added in the PE heat-sealing layer is 25%.
[0046] Example 7 It is basically the same as Example 1, except that the amount of silylated polyolefin added in the PE heat-sealing layer is 30%.
[0047] Example 8 It is basically the same as Example 1, except that the amount of silylated polyolefin added in the PE heat-sealing layer is 35%.
[0048] Liquid drainage tests were conducted on the liquid packaging bags prepared in Examples 1 to 8: 200 mL of an aqueous liquid with a viscosity of 20 mPa·s (CPS) at 25°C was placed in each bag; the bag was inverted (drainage port facing down, with the longitudinal axis of the bag at a 90° angle to the horizontal plane) and allowed to drain; timing was started from the beginning of liquid flow and stopped when the time interval between two adjacent drops exceeded 3 seconds, and the elapsed time was recorded as the drainage time; after drainage, the total mass of the bag and residual liquid was weighed using an analytical balance with an accuracy of 0.01 g, and the mass of the empty bag was subtracted, and this was recorded as the residual amount; 10 samples were tested in each group, and the average value was taken. The results are shown in Table 1 below: Table 1 As shown in the table above, with the increase of the amount of silylated polyolefin added, the drainage time is shortened and the residual amount is reduced. When the addition amount reaches 25% or more, the residual amount tends to stabilize and the liquid-repellent effect is good; the addition amount exceeding 35% has an adverse effect on the heat-sealing strength, so the preferred addition amount is 15% to 30%.
[0049] Example 9 The film employs a PET / VMPET / PE composite structure, with 20% silyl-alkylated polyolefin added to the PE heat-sealing layer. The drainage channel utilizes three radial channels (fanning outwards from the irregularly shaped drain outlet into the bag), and the groove width W of groove 15 is 2.0mm, and the height H is 1.5mm. The master mold is made of silicone material to achieve hard-press soft-forming. The laser cutting line is curved (arc-shaped easy-tear line), using a CO2 laser with a cutting depth of 12μm, and the upper and lower laser heads are synchronously positioned for marking.
[0050] In this embodiment, the bag has a capacity of 200 ml. It was filled with a viscous liquid with a viscosity of 150 CPS and a drainage test was conducted. The drainage time was 12.3 s and the residual amount was 1.2 g.
[0051] Example 10 The system employs a PET / VMPET / PE composite film structure, with 25% silyl-alkylated polyolefin added to the PE heat-sealing layer. The flow channel utilizes a combination of a single main channel and two branch channels on either side. The main channel corresponds to groove 15 with a groove width W of 3.0 mm and a height H of 2.0 mm, while the branch channels correspond to groove 15 with a groove width W of 1.5 mm and a height H of 1.0 mm. The laser cutting line is a combination of straight and curved lines (with a circular anti-crack hole at the end), using a CO2 laser with a cutting depth of 12 μm. The upper and lower laser heads are synchronously positioned and marked.
[0052] In this embodiment, the bag has a capacity of 200 ml. It was filled with a viscous liquid with a viscosity of 150 CPS and a drainage test was conducted. The drainage time was 10.8 s and the residual amount was 0.9 g.
[0053] Comparative Example 1 The difference between this comparative example and Example 5 is that: instead of using a double-sided male mold for one-time synchronous molding, it adopts the existing step-by-step single-press method: the upper film and the lower film are pressed separately in two independent stations by their respective single-sided male molds in conjunction with flat female molds. After pressing, the two films are aligned, bonded, and heat-sealed to make bags. The remaining laser, heat-sealing, and die-cutting processes are the same as in Example 5.
[0054] Comparative Example 2 Referring to the scheme in publication number CN103640773A, a single-sided embossed forming steel plate is placed between two overlapping films, and an indentation line is formed by pressing with upper and lower flat molds with temperature and pressure; the forming steel plate only has embossed textures and no depressions, the upper and lower molds are flat and there is no concave-convex fit, the resulting film only forms a unidirectional indentation line and no concave-convex fit channel, the tear line is processed by single-sided laser processing after overlapping, and the other materials are the same as in Example 5.
[0055] Example 5 (simultaneous molding of double-sided molds combined with simultaneous laser cutting of double-sided molds of the present invention) was compared with Comparative Example 1 and Comparative Example 2. Ten samples were taken from each group, and the alignment deviation of the guide channels on the front and back sides, the channel matching rate (the proportion of channel lengths in which the upper and lower diaphragm protrusions and grooves are completely aligned), and the deviation of the easy-tear line on the front and back sides were measured. The above-mentioned drainage test was also performed. The results are shown in Table 2 below: Table 2 As can be seen from Table 2: (1) The present invention adopts a double-sided male mold and a concave-convex female mold to be formed simultaneously in one step. The alignment deviation of the front and back channels is only 0.03mm, and the channel matching rate is the highest. The first comparative example of step-by-step single pressing is affected by the superposition of two positioning errors. The alignment deviation reaches 0.52mm, and the channel matching rate is only 76%. Some channels cannot form a continuous closed flow channel due to misalignment. The second comparative example only forms a unidirectional indentation line. The diaphragm itself does not have a concave-convex interlocking structure, does not form a channel, and the marks are slight. (2) The present invention uses the upper and lower laser heads to position and mark simultaneously. The deviation of the front and back of the easy-tear line is only 0.02mm, which is significantly better than the two comparative examples. (3) Thanks to the concave-convex flow channel with high matching degree, the drainage time of Example 5 is shortened from 7.8s of the first comparative example and 9.6s of the second comparative example to 4.5s. The residual amount is reduced from 2.4g and 3.5g to 0.8g, which proves that the core invention point of the double-sided male mold synchronous forming brings quantifiable and significant technical effects.
[0056] It should be noted that although the solution disclosed in the prior art CN103640773A also sets a forming steel plate between the two membranes and is extruded by the upper and lower molds, its forming steel plate only has raised patterns and the upper and lower molds are flat. After extrusion, only the indentation lines are formed to open the flat flow channel. The membrane itself does not form a concave-convex mating structure. The male mold of the present invention has mutually cooperating ribs and recesses on its upper and lower surfaces, and the upper and lower female molds have grooves and protrusions. The male mold ribs and female mold grooves interlock, and the female mold protrusions and male mold recesses interlock, so that each membrane itself forms a concave-convex structure with both protrusions and recesses. After the two membranes are bonded together, a three-dimensional flow channel with concave-convex interlocking cross section is formed. Its flow guiding capacity and alignment accuracy are significantly better than the flat flow channel opened by only the indentation lines.
[0057] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A liquid packaging bag made by heat-sealing and bonding two pieces of composite film of an upper film sheet and a lower film sheet; the liquid packaging bag is provided with a special-shaped liquid discharge port, a concave-convex structure drainage channel is provided on the inner wall of the bag body near the special-shaped liquid discharge port, and the special-shaped liquid discharge port is provided with a cutting line that does not cut through the composite film sheet; characterized in that, The drainage channel is formed by the concave and convex structures formed on the inner surfaces of the upper and lower films. The inner surfaces of the upper and lower films each have protrusions protruding into the bag and grooves recessed outward. The protrusions of the upper film correspond to the protrusions of the lower film, and the grooves of the upper film correspond to the grooves of the lower film, so that after the upper and lower films are attached, a drainage channel with concave and convex structures is formed on the inner wall of the bag.
2. The liquid packaging bag of claim 1, wherein, The groove has a width of 0.3–5 mm and a height of 0.2–3 mm.
3. The liquid packaging bag of claim 2, wherein, After the upper diaphragm and the lower diaphragm are attached, the groove of the upper diaphragm and the corresponding groove of the lower diaphragm are joined to form a flow guide channel; the flow guide channel can be a single channel or a combination of multiple parallel or radial channels.
4. The liquid packaging bag of claim 1, wherein, The cutting line extends from one edge of the irregularly shaped drain outlet to the other edge, with a cutting depth of 1 to 100 μm; the shape of the cutting line is a single straight line, a single curve, or a combination of multiple straight lines and curves.
5. The liquid packaging bag of claim 1, wherein, The inner layer of the composite membrane is a PE heat-sealing layer.
6. The liquid packaging bag of claim 5, wherein, The PE heat-sealing layer contains a hydrophobic material, silylated polyolefin, and the amount of silylated polyolefin added is 5% to 35% of the total mass of the heat-sealing layer.
7. A method of manufacturing a liquid packaging bag according to any one of claims 1-6, characterized in that The process includes the formation of the drainage channel: a double-sided male mold is set between the upper and lower diaphragms, an upper female mold is set above the upper diaphragm, and a lower female mold is set below the lower diaphragm; the upper female mold and the lower female mold are heated and pressurized towards each other, so that the ribs on the upper surface of the male mold located in the middle press the upper diaphragm into the groove of the upper female mold, while the ribs on the lower surface of the male mold press the lower diaphragm into the groove of the lower female mold. At the same time, the protrusions on the surfaces of the upper and lower female molds press the upper and lower diaphragms into the corresponding recesses on the upper and lower surfaces of the male mold, respectively, so that the upper and lower diaphragms each form a convex-concave structure with both protrusions and grooves, thereby simultaneously forming drainage channel indentations on the upper and lower diaphragms.
8. The method of manufacturing a liquid packaging pouch according to claim 7, wherein The hot-pressing temperature is 80–180°C, the hot-pressing pressure is 0.1–1.0 MPa, and the holding time is 0.5–5 s.
9. The method of manufacturing a liquid packaging pouch according to claim 8, wherein The master mold is a silicone elastic master mold with a Shore hardness of 40-70A; or the master mold is a hard metal master mold.
10. The method of manufacturing a liquid packaging pouch according to claim 7, wherein Also includes: A laser line emitted by a laser emitter cuts the surface of the upper diaphragm and the surface of the lower diaphragm. The laser emitter is arranged symmetrically at the top and bottom, respectively cutting the upper surface of the upper diaphragm and the lower surface of the lower diaphragm, forming a cutting line that does not cut through the upper diaphragm and the lower diaphragm, and the cutting lines formed on the upper and lower surfaces are symmetrical.
Citation Information
Patent Citations
Soft packaging bag with flow channel and preparation method thereof
CN103640773A