A system and method for the resource utilization of coal gasification fine slag.

By integrating processes such as grinding, flotation, alkali fusion, and building material preparation, the problems of low resource recovery rate and environmental pollution in the resource utilization of coal gasification fine slag have been solved, realizing efficient and full-scale resource utilization of coal gasification fine slag to produce high-value-added geopolymer building materials and other products.

CN123106032APending Publication Date: 2026-11-17INNER MONGOLIA YIDONG GROUP JIUDING CHEMICAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611391834.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for treating coal gasification slag have problems such as low resource recovery rate, low product added value, poor process integration, and environmental pollution risks.

Method used

The integrated process of multiple units, including grinding, flotation, alkali fusion, adsorption, and building material preparation, achieves carbon resource recovery and mineral component transformation through grinding classification, flotation separation, alkali fusion treatment, wastewater treatment, and geopolymer preparation, forming a closed-loop system.

Benefits of technology

It achieves full utilization of coal gasification slag, with high resource recovery rate, increased product added value, reduced environmental pollution, and internal heat recovery and utilization to produce a variety of high value-added products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106032A_ABST
    Figure CN123106032A_ABST
Patent Text Reader

Abstract

This invention discloses a system and method for the resource utilization of coal gasification fine slag, belonging to the field of solid waste treatment and resource utilization technology. The system includes a grinding unit, a classification and screening unit, a slurry flotation unit, a dewatering and drying unit, an alkali fusion unit, an adsorption unit, a solid-liquid separation unit, and a geopolymer preparation unit connected in sequence. After grinding and classification, the coal gasification fine slag is separated into gasification residual carbon and decarbonization tailings by slurry flotation. Part of the residual carbon is burned for heating, and part is treated by alkali fusion. The decarbonization tailings are used for adsorption treatment of coal gasification wastewater after alkali fusion. After adsorption, the system undergoes solid-liquid separation; the filtrate meets discharge standards or is reused, and the dried filter cake is used to prepare geopolymers or building material fillers. This invention achieves full utilization of carbon and mineral components in coal gasification fine slag, with high system integration, high product added value, and good environmental and economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid waste resource utilization technology, and in particular to a system and method for the resource utilization of coal gasification fine slag. Background Technology

[0002] The large amount of fine slag produced during coal gasification contains unburned carbon components and siliceous aluminum mineral components. Traditional treatment methods mainly involve landfilling or simple stockpiling, which not only occupies land resources but also poses environmental pollution risks. Although some existing technologies have attempted to decarbonize or utilize coal gasification fine slag through flotation, these methods generally suffer from low resource recovery rates, low product added value, and poor process integration.

[0003] Therefore, developing a highly efficient, clean, and fully-capacitated process for the resource utilization of coal gasification fine residue is of significant practical importance and economic benefit. Summary of the Invention

[0004] The purpose of this invention is to provide a system and method for the resource utilization of coal gasification fine slag, achieving multi-objective synergistic treatment of carbon resource recovery, mineral component conversion, wastewater treatment, and high-value-added building material preparation.

[0005] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: This invention provides a system for the resource utilization of coal gasification fine slag, including a grinding unit and a classification and screening unit for processing coal gasification fine slag into qualified fine powder, a slurry conditioning unit for conditioning the qualified fine powder into slurry, a flotation unit for separating gasification residual carbon and decarbonization tailings from the slurry-conditioned material, a gasification residual carbon treatment unit connected to the outlet of the gasification residual carbon obtained by the flotation unit, and a decarbonization tailings treatment unit connected to the outlet of the decarbonization tailings obtained by the flotation unit. The gasification residue treatment unit includes a dehydration and drying unit for dehydrating and drying the gasification residue, a filtrate collection tank for receiving the filtrate obtained from the dehydration and drying unit, an adsorption process unit for receiving the dried residue obtained from the dehydration and drying unit, and a wastewater treatment unit for receiving the adsorption-treated coal gasification wastewater produced by the adsorption process unit. The directly combustible portion obtained from the adsorption process unit and the saturated adsorbent obtained from the wastewater treatment unit are used to perform heat recovery through combustion, which is used for preheating or drying within the system. The decarbonization tailings treatment unit includes an alkali fusion treatment unit for activating the decarbonization tailings; after treatment by the alkali fusion treatment unit, alkali fusion products, alkali fusion flue gas, and alkali fusion residue are obtained; the alkali fusion products are then subjected to a water quenching process and then enter a grinding process to finally obtain activated powder. A portion of the filtrate collected in the filtrate collection tank is used for slurry preparation in the slurry preparation unit, and another portion is used for alkaline activation solution. The alkaline activation solution is mixed with the active powder in dry powder form and then molded with additives. After curing, a geopolymer product is obtained.

[0006] Furthermore, the grinding unit is used to grind the coal gasification slag to obtain fine powder; the classification and screening unit is connected to the grinding unit and is used to classify the grinding product, separating coarse particles and qualified fine powder, wherein the coarse particles are returned to the grinding unit for further grinding.

[0007] Furthermore, the wastewater treatment unit treats the coal gasification wastewater using an adsorbent, and discharges or reuses the treated wastewater after it meets the standards.

[0008] Furthermore, the remaining tailings obtained from the decarbonization tailings treatment unit are subjected to a solid-liquid separation process, and the filtrate enters the filtrate collection tank, which also yields a filter cake; the heat from the filter cake after combustion is transferred to the heat recovery system.

[0009] Furthermore, the alkali fusion flue gas is treated by a dust removal process to meet emission standards, and the alkali fusion residue is returned to the grinding or building materials process.

[0010] Furthermore, the active powder is processed into geopolymer building materials through a dry powder mixing subunit, a molding subunit, and a curing subunit; the dry powder mixing subunit is used to dry mix the active powder with additives; the molding subunit is used to mold the mixture into a blank; and the curing subunit is used to cure the molded blank.

[0011] Furthermore, the geopolymer product is a geopolymer building material.

[0012] This embodiment provides a method for the resource utilization of coal gasification fine slag, including the following steps: S1 Raw Material Pretreatment Stage: The fine slag from coal gasification first enters the grinding unit, and after grinding, it is sent to the classification and screening unit. Coarse particles are returned to the grinding unit for further grinding, while qualified fine powder enters the slurry preparation unit, where water and flotation reagents are added to prepare a slurry of a certain concentration. S2 Flotation Separation Stage: The slurry after conditioning enters the flotation unit. Utilizing the hydrophobic properties of gasification residue and hydrophilic properties of tailings ash, high-carbon products are obtained through flotation separation, specifically gasification residue and decarbonization tailings ash. S3 Gasification Residue Treatment Stage: Gasification residue enters the dehydration and drying unit to remove moisture, resulting in dried residue. The filtrate enters the filtrate collection tank. The dried residue, with its well-developed pores and certain calorific value, is sent to the adsorption process unit for adsorbing organic matter and heavy metals in coal chemical wastewater. The saturated residue (saturated adsorbent) and a portion of the unused dried residue (the directly combustible portion) are sent to the heat recovery system for combustion. The heat generated is used for preheating, drying, or heating the alkali fusion unit within the system. Wastewater treated by the wastewater treatment unit is discharged or reused after meeting standards. S4 Decarbonization Tailings Treatment Stage: The decarbonization tailings enter the alkali fusion treatment unit, where they are mixed with solid alkali in a specific ratio and calcined at 500-900℃ for 1-3 hours to destroy the stable silicon-aluminum crystal structure (such as mullite and quartz) in the tailings. The resulting alkali fusion product is immediately water-quenched: the high-temperature molten material is poured into cold water for rapid cooling. This process has two effects: ① Thermal stress causes the material to spontaneously disintegrate into loose particles; ② Rapid cooling "freezes" the high-energy disordered (amorphous) structure formed at high temperature, resulting in high chemical activity. The water-quenched material enters the grinding process and is ground to a specific surface area >400 m². 2 / kg, to obtain active powder. The alkali fusion flue gas is discharged in compliance with standards after dust removal treatment; the alkali fusion residue (a small amount of inert components that have not been completely reacted) is returned to the grinding unit or used as an admixture in building materials; S5 geopolymer preparation stage: The active powder and additives (such as standard sand, water-reducing agents, and retarders) are uniformly mixed in the dry powder mixing sub-unit. A portion of the filtrate from the filtrate collection tank is used as the alkali activation solution (additional alkali is added if necessary to adjust the modulus). The dry powder mixture and the alkali activation solution are stirred and mixed in the molding sub-unit and pressed into a green body. The green body is cured in the curing sub-unit (e.g., steam curing at 60-80℃ for 24 hours, or natural curing for 28 days), finally yielding geopolymer building material products (such as bricks, blocks, paving bricks, etc.).

[0013] Compared with the prior art, the beneficial technical effects of the present invention are as follows: Full utilization of resources: The system recovers and utilizes internal heat, treats and reuses wastewater, and reduces external discharge; it realizes the separation and conversion of carbon components and mineral components in coal gasification fine slag, with carbon components used for combustion and energy supply, and mineral components used for the preparation of high-value-added geopolymers; High degree of process integration: It organically integrates multiple units such as grinding, flotation, alkali fusion, adsorption, and building material preparation to form a closed-loop system; it can produce a variety of products such as gasification residue, activated powder, geopolymer building materials, and fillers to meet market demands. Attached Figure Description

[0014] The present invention will be further described below with reference to the accompanying drawings. Figure 1This is a system flow diagram for the resource utilization of coal gasification fine residue of the present invention. Detailed Implementation

[0015] Example 1 Raw materials: Fine slag from a coal gasification plant, with an initial moisture content of 48% (dry basis) and a carbon content of 25.0% (dry basis). Dry basis chemical composition: SiO2 46.2%, Al2O3 19.5%, Fe2O3 5.8%, CaO 4.1%, loss on ignition 25.0%. Coal gasification wastewater quality: COD 2000 mg / L, volatile phenols 250 mg / L, ammonia nitrogen 120 mg / L.

[0016] step: Grinding and Classification: The coal gasification fine slag (wet basis) is directly fed into the rod mill, with a grinding concentration of 65% and a grinding time of 25 minutes. After classification by a high-frequency vibrating screen (200 mesh), the undersize yield is 82% (i.e., 82% of the fineness is -200 mesh). The qualified fine powder enters the slurry mixing tank; the coarse particles on the screen are returned to the mill.

[0017] Flotation separation: The qualified fine powder was slurry adjusted to a pulp concentration of 20%, and 1000 g / t of collector (diesel oil) and 500 g / t of frother (No. 2 oil) were added. The mixture was then floated in a mechanically stirred flotation machine for 6 minutes. The result was: Gasification residue: yield 22.5%, dry basis calorific value 4520 kcal / kg (rounded to 4500 kcal / kg), loss on ignition 72.3%.

[0018] Decarbonization tailings: yield 77.5%, loss on ignition 2.1%, silicon and aluminum content (SiO2+Al2O3) 71.8%.

[0019] Gasification Residue Treatment: The gasification residue is dehydrated by a belt filter, and the filtrate (pH≈9) is collected in a filtrate tank. Approximately 40% of the dried residue is directly fed into a hot blast furnace for combustion, generating hot air for the alkali fusion and drying units; the remaining 60% of the dried residue is loaded into an adsorption column for treating coal gasification wastewater (space velocity 2 h⁻¹). -1 (The bed height is 1.5 m). After adsorption, the COD of the wastewater is reduced to 320 mg / L, volatile phenols to 12 mg / L, and ammonia nitrogen to 45 mg / L. The saturated carbon residue is also sent to the hot blast stove for combustion after discharge, and the hot blast system meets the heat energy needs of the entire plant.

[0020] Alkali fusion and water quenching of decarbonized tailings: Take 1000 kg of decarbonized tailings and mix it with solid NaOH at a mass ratio of 1:0.8. Then, calcine it in a rotary kiln at 750℃ for 1.5 hours.

[0021] The high-temperature alkali fusion product falls directly into a water quenching tank (water temperature 25℃, water volume 12 times the product mass). The material instantly disintegrates into loose particles of 0.5-3 mm. After water quenching, the slurry is filtered, and the filtrate (containing excess alkali) is sent to a filtrate collection tank.

[0022] Water-quenched solid slag was milled in a ball mill for 30 minutes to obtain active powder with a specific surface area of ​​535 m². 2 / kg, the XRD pattern shows typical amorphous diffuse peaks.

[0023] Activated powder adsorption of wastewater: The above-mentioned activated powder was loaded into another adsorption tower to treat the same batch of coal gasification wastewater (initial COD 2000 mg / L, volatile phenols 250 mg / L). The contact time was controlled at 1 hour, and the powder dosage was 5% of the wastewater mass. After adsorption, the wastewater COD decreased to 150 mg / L, and volatile phenols <2 mg / L, meeting the indirect discharge standard. The activated powder after adsorption saturation (moisture content approximately 45%) was directly used as a geopolymer raw material without drying.

[0024] Preparation of geopolymer bricks: Take 1000 kg of dry powder equivalent to saturated adsorption active powder (wet basis), add 1200 kg of standard sand and 8 kg of powdered water-reducing agent, and dry mix for 3 minutes in a horizontal mixer. Take the mixed filtrate (including flotation dewatering filtrate and water-quenched filtrate, with a total alkalinity of 4.8% based on Na2O) from the filtrate collection tank as the alkali activation solution, with a dosage of 35% of the mass of the dry powder mixture (approximately 770 kg). Add an additional 10 kg of industrial water glass (modulus 2.2, solid content 45%) to adjust the modulus. Add the alkali activation solution to the dry powder and forcibly stir for 5 minutes to obtain a plastic slurry with a slump of 60 mm. Pour the slurry into a standard brick mold of 240 mm × 115 mm × 53 mm and vibrate to form (vibration frequency 50 Hz, time 30 seconds).

[0025] The molded blank is steam cured at 60℃ for 24 hours, then demolded and naturally cured for 28 days.

[0026] Product performance: 28-day compressive strength (average): 26.3 MPa (>25 MPa), minimum value for a single piece: 24.8 MPa.

[0027] Flexural strength: 4.2 MPa. Softening coefficient: 0.88. Drying shrinkage: 0.045%.

[0028] Leaching toxicity: According to the method of HJ / T 299-2007, the leaching concentrations of heavy metals (Pb, Cr, Cd, As) were all lower than the Class V limit of the "Surface Water Environmental Quality Standard".

[0029] It meets national standards: it meets the MU25 grade requirements of GB / T 21144-2007 "Solid Concrete Bricks" and also meets the requirements of GB 6566-2010 "Limits of Radionuclides in Building Materials".

[0030] Technical and economic indicators: residual calorific value of 4500 kcal / kg, the entire system has a surplus of heat source. Approximately 1.2 m³ of geopolymer bricks are produced per ton of dry-based coal gasification slag. 3 The direct cost is approximately 180 yuan / m². 3 The market price is approximately 300 yuan / m² 3 It co-processes 2.5 tons of coal gasification wastewater, saving wastewater treatment costs.

[0031] Example 2 (Comparison: Brick making directly from active powder without adsorption) The procedure is basically the same as in Example 1, but step 5 (active powder adsorption of wastewater) is omitted. The active powder obtained in step 4 is directly mixed with the alkaline activation solution to make bricks. Results: The 28-day compressive strength is 31.2 MPa, higher than the 26.3 MPa of bricks made after adsorption. This indicates that the adsorption of wastewater slightly reduces the strength, but still meets the MU25 standard, and achieves the additional benefit of co-treating wastewater, resulting in better overall economic efficiency.

[0032] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A system for the resource utilization of coal gasification fine slag, characterized in that, It includes a grinding unit and a classification and screening unit for processing coal gasification slag into qualified fine powder, a slurry conditioning unit for conditioning the qualified fine powder, a flotation unit for separating gasification residue and decarbonization tailings from the slurry-conditioned material, a gasification residue treatment unit connected to the gasification residue outlet of the flotation unit, and a decarbonization tailings treatment unit connected to the decarbonization tailings outlet of the flotation unit. The gasification residue treatment unit includes a dehydration and drying unit for dehydrating and drying the gasification residue, a filtrate collection tank for receiving the filtrate obtained from the dehydration and drying unit, an adsorption process unit for receiving the dried residue obtained from the dehydration and drying unit, and a wastewater treatment unit for receiving the adsorption-treated coal gasification wastewater produced by the adsorption process unit. The directly combustible portion obtained from the adsorption process unit and the saturated adsorbent obtained from the wastewater treatment unit are used to perform heat recovery through combustion, which is used for preheating or drying within the system. The decarbonization tailings treatment unit includes an alkali fusion treatment unit for activating the decarbonization tailings; after treatment by the alkali fusion treatment unit, alkali fusion products, alkali fusion flue gas, and alkali fusion residue are obtained; the alkali fusion products are then subjected to a water quenching process and then enter a grinding process to finally obtain activated powder. A portion of the filtrate collected in the filtrate collection tank is used for slurry preparation in the slurry preparation unit, and another portion is used for alkaline activation solution. The alkaline activation solution is mixed with the active powder in dry powder form and then molded with additives. After curing, a geopolymer product is obtained.

2. The system for resource utilization of coal gasification fine slag according to claim 1, characterized in that: The grinding unit is used to grind the coal gasification slag to obtain fine powder; the classification and screening unit is connected to the grinding unit and is used to classify the grinding product, separating coarse particles and qualified fine powder, wherein the coarse particles are returned to the grinding unit for further grinding.

3. The system for resource utilization of coal gasification fine slag according to claim 1, characterized in that: The wastewater treatment unit treats coal gasification wastewater using an adsorbent, and the treated wastewater is discharged or reused after meeting the standards.

4. The system for resource utilization of coal gasification fine slag according to claim 1, characterized in that: The remaining tailings obtained from the decarbonization tailings treatment unit are processed by a solid-liquid separation process. The filtrate enters the filtrate collection tank and a filter cake is obtained. The heat from the filter cake after combustion is transferred to the heat recovery system.

5. The system for resource utilization of coal gasification fine slag according to claim 1, characterized in that: The alkali fusion flue gas is treated by a dust removal process to meet emission standards, and the alkali fusion residue is returned to the grinding or building materials process.

6. The system for resource utilization of coal gasification fine slag according to claim 1, characterized in that: The active powder is processed into geopolymer building materials through a dry powder mixing subunit, a molding subunit, and a curing subunit; the dry powder mixing subunit is used to dry mix the active powder with additives; the molding subunit is used to mold the mixture into a blank; and the curing subunit is used to cure the molded blank.

7. The system for resource utilization of coal gasification fine slag according to claim 1, characterized in that: The geopolymer product is a geopolymer building material.

8. A method for the resource utilization of coal gasification fine slag, comprising the system for the resource utilization of coal gasification fine slag according to any one of claims 1-7, characterized in that: S1 Raw Material Pretreatment Stage: The fine slag from coal gasification first enters the grinding unit, and after grinding, it is sent to the classification and screening unit. Coarse particles are returned to the grinding unit for further grinding, while qualified fine powder enters the slurry preparation unit, where water and flotation reagents are added to prepare a slurry of a certain concentration. S2 Flotation Separation Stage: The slurry after conditioning enters the flotation unit. Utilizing the hydrophobic properties of gasification residue and hydrophilic properties of tailings ash, high-carbon products are obtained through flotation separation, specifically gasification residue and decarbonization tailings ash. S3 Gasification Residue Treatment Stage: Gasification residue enters the dehydration and drying unit to remove moisture, resulting in dried residue. The filtrate enters the filtrate collection tank. The dried residue, with its well-developed pores and certain calorific value, is sent to the adsorption process unit for adsorbing organic matter and heavy metals in coal chemical wastewater. The saturated residue (saturated adsorbent) and a portion of the unused dried residue (the directly combustible portion) are sent to the heat recovery system for combustion. The heat generated is used for preheating, drying, or heating the alkali fusion unit within the system. Wastewater treated by the wastewater treatment unit is discharged or reused after meeting standards. S4 Decarbonization Tailings Treatment Stage: The decarbonization tailings enter the alkali fusion treatment unit, where they are mixed with solid alkali in a specific ratio and calcined at 500-900℃ for 1-3 hours to destroy the stable silicon-aluminum crystal structure (such as mullite and quartz) in the tailings. The resulting alkali fusion product is immediately water-quenched: the high-temperature melt is poured into cold water for rapid cooling. The water-quenched material then enters the grinding process, where it is ground to a specific surface area >400 m². 2 / kg, to obtain active powder. The alkali fusion flue gas is discharged in compliance with standards after dust removal treatment; the alkali fusion residue (a small amount of inert components that have not been completely reacted) is returned to the grinding unit or used as an admixture in building materials; S5 geopolymer preparation stage: The active powder and additives are uniformly mixed in the dry powder mixing subunit. A portion of the filtrate from the filtrate collection tank is used as the alkali activation solution (additional alkali is added if necessary to adjust the modulus). The dry powder mixture and alkali activation solution are stirred and mixed in the molding subunit and pressed into a green body. The green body is cured in the curing subunit to finally obtain the geopolymer building material product.