A wear-resistant and impact-resistant two-dimensional polyaramid composite material for protective components of high-end equipment and its preparation method

Through the synergistic effect of two-dimensional polyaramid with silane-treated chopped aramid fibers and silicon-containing flame retardants, the interfacial bonding performance of high-end equipment protective component materials has been improved, solving the weight and corrosion resistance problems of traditional metal materials and achieving improvements in the wear resistance, impact resistance and flame retardancy of the materials.

CN123107350APending Publication Date: 2026-11-17HONGRUN QINGYUAN (FOSHAN) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611211539.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing high-end equipment protective components use metal materials that suffer from high weight, insufficient corrosion resistance, long processing cycles, and difficulties in structural forming. Furthermore, existing polymer composite materials cannot simultaneously meet the requirements for wear resistance, impact resistance, and dimensional stability. The two-dimensional polyaramid and resin interface bonding is insufficient, resulting in severe fiber pull-out and interface debonding phenomena.

Method used

Two-dimensional polyaramid and silane-treated chopped aramid fibers are used for synergistic reinforcement. Combined with polyphthalamide, polyamide 66 and silicone flame retardant, the dispersion and interfacial bonding properties of the reinforcing components in the resin matrix are improved, forming a multi-scale reinforced structure, which improves the wear resistance, impact resistance, heat resistance and flame retardancy of the material.

Benefits of technology

It achieves a balance between wear resistance, impact resistance, heat resistance and flame retardancy in the protective components of high-end equipment, reduces the weight of materials and increases the freedom of structural design, thus meeting the usage requirements of high-end equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of materials technology and discloses a wear-resistant and impact-resistant two-dimensional polyaramid composite material for high-end equipment protective components and its preparation method. The composite material comprises, by weight, 55-65 parts of polyphthalamide, 15-20 parts of polyamide 66, 12-16 parts of two-dimensional polyaramid, 1-3 parts of a silicon-containing flame retardant, 0.1-0.2 parts of antioxidant 1010, 0.6-1 parts of chopped aramid fibers, and 0.2-0.3 parts of lubricant. In the preparation process, all components except the chopped aramid fibers are first mixed at high speed. Then, the premix and silane-treated chopped aramid fibers are fed into a twin-screw extruder through the main feed port and side feed port, respectively. The mixture is then melt-blended, cooled, pelletized, and dried to obtain the composite material. The material obtained by this invention possesses good wear resistance, impact resistance, heat resistance, and flame retardancy, making it suitable for components such as protective covers, wear-resistant liners, and protective shells for high-end equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials technology, specifically to a wear-resistant and impact-resistant two-dimensional polyaramid composite material for protective components of high-end equipment and its preparation method. Background Technology

[0002] Protective covers, guide rail guards, wear-resistant liners, transmission mechanism protective shells, and impact-resistant baffles in high-end engineering equipment, mining machinery, rail transit equipment, aviation ground support equipment, and precision machining equipment typically need to withstand long-term particle erosion, sliding friction, periodic vibration, foreign object impact, and alternating loads. While traditional metal protective components possess high rigidity and load-bearing capacity, they suffer from problems such as large weight, insufficient corrosion resistance, long processing cycles, and difficulties in forming complex structures. Replacing some metal components with high-performance polymer composite materials can reduce equipment weight and increase structural design freedom; however, the surface wear resistance, dimensional stability, and impact resistance of ordinary polymer materials still cannot simultaneously meet the requirements of high-end equipment.

[0003] Existing technologies typically improve the strength and stiffness of polymer materials by adding glass fibers, carbon fibers, or aramid fibers, or by adding hard particles such as silicon carbide, alumina, and silica to improve wear resistance. However, insufficient interfacial bonding between chopped fibers and the resin matrix can easily occur, leading to fiber pull-out and interfacial debonding under impact loads. Hard inorganic particles, on the other hand, tend to agglomerate in the resin and form localized stress concentration points. While this can reduce surface wear, it often results in a decrease in the material's impact toughness. Furthermore, simply increasing the inorganic filler content can reduce melt flowability, making injection molding of complex protective components more difficult.

[0004] Two-dimensional polyarylamide nanosheets possess high in-plane strength, heat resistance, and crack resistance. Their layered structure can extend crack propagation paths and facilitate the formation of a two-dimensional load-bearing network within the polymer matrix. However, the strong intermolecular hydrogen bonds on the surface of two-dimensional polyarylamide nanosheets make them prone to layer stacking and aggregation, resulting in limited interfacial wettability with thermoplastic resins and hindering the full realization of their two-dimensional reinforcement effect. Furthermore, existing two-dimensional polyarylamide composites typically focus on improving tensile strength or barrier properties, with insufficient research on the uniform distribution of wear-resistant phases, impact energy dissipation, and the synergistic construction of multi-scale fiber layer structures, making it difficult to simultaneously achieve high wear resistance, impact resistance, and dimensional stability.

[0005] Therefore, it is necessary to provide a composite material through the synergistic effect of two-dimensional polyaramid, silane-treated chopped aramid fibers, and a silicon-containing flame retardant, in order to improve the dispersion and interfacial bonding properties of the two-dimensional polyaramid and chopped aramid fibers in the resin matrix, while taking into account the wear resistance, impact resistance, heat resistance, and flame retardancy of the material. Summary of the Invention

[0006] To overcome the shortcomings of the prior art, the present invention aims to provide a wear-resistant and impact-resistant two-dimensional polyaramid composite material for high-end equipment protective components and its preparation method. The composite material is enhanced by the synergistic reinforcement of two-dimensional polyaramid and silane-treated chopped aramid fibers, and by the addition of polyphthalamide, polyamide 66 and a silicon-containing flame retardant. This improves the dispersibility and interfacial bonding performance of the reinforcing components in the resin matrix, thus taking into account the wear resistance, impact resistance, heat resistance, flame retardancy and processing performance of the material.

[0007] To achieve the above objectives, the present invention provides the following technical solution: a wear-resistant and impact-resistant two-dimensional polyaramid composite material for protective components of high-end equipment, comprising the following components by weight: 55-65 parts by weight of polyphthalamide, 15-20 parts by weight of polyamide 66, 12-16 parts by weight of two-dimensional polyaramid, 1-3 parts by weight of silicone flame retardant, 0.1-0.2 parts by weight of antioxidant 1010, 0.6-1 parts by weight of chopped aramid fiber, and 0.2-0.3 parts by weight of lubricant.

[0008] Furthermore, the chopped aramid fiber has a length of 1-5 mm and a diameter of 8-20 μm; the chopped aramid fiber is impregnated with a 0.5-2.0% (by mass) α-aminopropyltriethoxysilane hydrolysate and dried at 80-120°C for 1-3 hours before use.

[0009] Furthermore, the preparation method of the silicon-containing flame retardant is as follows: S1. Add 18.4-18.6 g of melamine and 300 mL of 1,4-dioxane to a three-necked flask. After the melamine is completely dissolved, add an aqueous solution containing 8.6-8.9 g of 2-amino-2-methyl-propanol and 3.8-4 g of sodium hydroxide dropwise to the flask at 0-5 °C. After reacting for 2-3 hours, raise the temperature of the system to 45-50 °C, and then add 8.6-8.9 g of 2-amino-2-methyl-propanol... A 0.9 g aqueous solution of 2-amino-2-methyl-propanol and 3.8-4 g sodium hydroxide was slowly added dropwise to a three-necked flask. After reacting for 2-3 hours, the system temperature was raised to 80-85℃. Finally, an aqueous solution containing 8.6-8.9 g of 2-amino-2-methyl-propanol and 3.8-4 g of sodium hydroxide was slowly added dropwise to the three-necked flask. After the addition was complete, the entire reaction system was maintained at 80-85℃ for 8-12 hours. After the reaction was completed, after post-processing, intermediate 1 was obtained. S2. Intermediate 1 and triethylamine were added sequentially to a three-necked flask containing 200 mL of acetonitrile. Then, diphenyldichlorosilane was added at 0-5 °C. The reaction was carried out for 1-1.5 h, and then the temperature was increased to react for another 8-10 h. After the reaction was completed, the precipitate was filtered out and washed with deionized water and 1,4-dioxane, respectively. The precipitate was then dried in a forced-air drying oven to obtain a silicon-containing flame retardant.

[0010] Further, in step S1, the post-processing involves first cooling the solution in the three-necked flask to room temperature, then precipitating the precipitate with deionized water, washing the white precipitate three times with deionized water, and then drying it.

[0011] Furthermore, in step S2, the ratio of intermediate 1, triethylamine, and diphenyldichlorosilane is 6.1-6.4g: 6.02-6.13g: 0.028-0.03mol.

[0012] Furthermore, in step S2, the heating temperature is 35-40℃.

[0013] Furthermore, it includes the following steps: S1. First, add polyphthalamide, polyamide 66, two-dimensional polyarylamide, silicone flame retardant, antioxidant 1010 and lubricant into a high-speed mixer and mix at 500-1000 r / min for 5-10 min to obtain a premix; S2. The premix is ​​added through the main feed port of the twin-screw extruder, and the chopped aramid fibers are added through the side feed port of the twin-screw extruder. The mixture is melt-blended and extruded under the conditions of 270-320°C in each temperature zone and 200-400 r / min in the screw speed to obtain the extruded strip. S3. The extruded strip is water-cooled or air-cooled and then pelletized, and dried at 90-120°C to obtain the wear-resistant and impact-resistant two-dimensional polyaramid composite material for high-end equipment protective components.

[0014] Furthermore, the drying time in step S3 is 3-6 hours.

[0015] Compared with the prior art, the present invention has the following beneficial technical effects: This invention uses polyphthalamide and polyamide 66 to form a composite resin matrix. By utilizing the good heat resistance, rigidity and dimensional stability of polyphthalamide and the good toughness and processing properties of polyamide 66, the resulting composite material has heat resistance, mechanical properties and melt processing properties.

[0016] This invention introduces a two-dimensional polyarylamide, utilizing its layered structure and high in-plane strength to form a two-dimensional load-bearing structure within a resin matrix. When the material is subjected to friction or impact, the two-dimensional polyarylamide can disperse external loads, hinder rapid crack propagation, and extend the crack propagation path, thereby reducing material wear and improving its resistance to impact damage.

[0017] This invention utilizes chopped aramid fibers impregnated with α-aminopropyltriethoxysilane hydrolysate, which improves the interfacial bonding strength between the chopped aramid fibers and the polyamide resin matrix, reducing fiber pull-out and interfacial debonding under impact loads. The chopped aramid fibers and two-dimensional polyaramid work together to form a multi-scale reinforced fiber sheet structure, further enhancing the material's abrasion resistance, impact resistance, and structural stability.

[0018] The silicon-containing flame retardant used in this invention contains triazine and silicon-containing structures, which can promote the formation of a stable carbonized protective layer in the material during heating, blocking the transfer of heat and combustible gases. This improves the flame retardant performance and high-temperature stability of the composite material at a lower addition amount, and reduces the adverse effects of the flame retardant on the mechanical properties and processing fluidity of the material. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0020] 0.63 g of melamine and 1.30 g of 1,3,5-pyridinetricarboxylic acid chloride were added to a reaction flask, followed by the addition of 4 mL of pyridine and 40 mL of N-methylpyrrolidone. The mixture was stirred at room temperature for 30 h to obtain a crude product. The crude product was washed successively with anhydrous ethanol, ultrapure water, and acetone, sonicated for 25 min, and then centrifuged at 8000 r / min for 4 min to separate the solid and liquid phases. The solid was retained and washed twice with each solvent as described above. Finally, the product was vacuum dried at 65 °C for 15 h and cooled to room temperature to obtain a two-dimensional polyarylamide. The two-dimensional polyarylamide was added to a zirconia ball mill jar, using zirconia balls with a diameter of 0.3 mm as the grinding medium, with a ball-to-material mass ratio of 20:1, and ground at 1200 r / min to obtain a two-dimensional polyarylamide with a transverse dimension of approximately 70 nm.

[0021] The polyphthalamide is an unreinforced PPA resin from the Amodel A-1000 series manufactured by Solvay Specialty Polymers; the polyamide 66 is a PA66 resin of Ultramid A3KR01 manufactured by BASF Europe; and the lubricant is calcium stearate.

[0022] Preparation of Silicon-Containing Flame Retardants Add 18.5 g of chloronitrile and 300 mL of 1,4-dioxane to a three-necked flask and stir until the chloronitrile is completely dissolved. Prepare three separate reaction solutions, each containing 8.75 g of 2-amino-2-methyl-propanol and 3.9 g of sodium hydroxide.

[0023] The first portion of the reaction solution was slowly added dropwise to a three-necked flask at 3°C, and the reaction continued for 2.5 hours after the addition was complete. The reaction system was then heated to 48°C, and the second portion of the reaction solution was slowly added dropwise, and the reaction continued for 2.5 hours after the addition was complete. The reaction system was then heated to 82°C, and the third portion of the reaction solution was slowly added dropwise, and the reaction was maintained at 82°C for 10 hours after the addition was complete. After the reaction was completed, the reaction solution was cooled to room temperature, deionized water was added to precipitate a white precipitate, which was filtered, washed three times with deionized water, and dried to obtain intermediate 1.

[0024] 6.25 g of intermediate 1 and 6.08 g of triethylamine were sequentially added to a three-necked flask containing 200 mL of acetonitrile. 0.029 mol of diphenyldichlorosilane was slowly added at 3 °C with stirring. After the addition was complete, the reaction was carried out at 3 °C for 1.25 h, and then the temperature was increased to 38 °C for 9 h. After the reaction was complete, the mixture was filtered, and the resulting precipitate was washed with deionized water and 1,4-dioxane, respectively, and then dried in a forced-air drying oven to obtain a silicon-containing flame retardant.

[0025] Example 1 This embodiment provides a wear-resistant and impact-resistant two-dimensional polyaramid composite material for protective components of high-end equipment, comprising, by weight, 55 parts of polyphthalamide, 15 parts of polyamide 66, 12 parts of two-dimensional polyaramid, 1 part of silicone flame retardant, 0.1 part of antioxidant 1010, 0.6 parts of chopped aramid fiber and 0.2 parts of lubricant.

[0026] The chopped aramid fibers have a length of 1 mm and a diameter of 8 μm. The chopped aramid fibers are immersed in a 0.5% (w / w) α-aminopropyltriethoxysilane hydrolysate to fully wet the fibers. After removal, they are dried at 80°C for 1 hour to obtain silane-treated chopped aramid fibers.

[0027] The preparation method of the composite material in this embodiment includes the following steps: S1. Add 55 parts of polyphthalamide, 15 parts of polyamide 66, 12 parts of two-dimensional polyarylamide, 1 part of silicone flame retardant, 0.1 part of antioxidant 1010 and 0.2 parts of lubricant to a high-speed mixer and mix at 500 r / min for 5 min to obtain a premix.

[0028] S2. The premix obtained in step S1 is added through the main feed port of a twin-screw extruder, and 0.6 parts of silane-treated chopped aramid fibers are added through the side feed port of the twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set sequentially to 270℃, 280℃, 290℃, 300℃, 305℃, 300℃, and 295℃, with the die head temperature at 295℃ and the screw speed at 200 r / min. Melt blending extrusion is performed to obtain extruded strips. S3. The extruded strips obtained in step S2 are water-cooled, drawn, and pelletized, and then dried at 90℃ for 3 hours to obtain a wear-resistant and impact-resistant two-dimensional polyaramid composite material for high-end equipment protective components.

[0029] Example 2 This embodiment provides a wear-resistant and impact-resistant two-dimensional polyaramid composite material for protective components of high-end equipment, which, by weight, includes 60 parts of polyphthalamide, 17.5 parts of polyamide 66, 14 parts of two-dimensional polyaramid, 2 parts of silicone flame retardant, 0.15 parts of antioxidant 1010, 0.8 parts of chopped aramid fiber and 0.25 parts of lubricant.

[0030] The chopped aramid fibers have a length of 3 mm and a diameter of 14 μm. The chopped aramid fibers are immersed in a 1.0% (w / w) α-aminopropyltriethoxysilane hydrolysate to fully wet the fibers. After removal, they are dried at 100°C for 2 hours to obtain silane-treated chopped aramid fibers.

[0031] The preparation method of the composite material in this embodiment includes the following steps: S1. Add 60 parts of polyphthalamide, 17.5 parts of polyamide 66, 14 parts of two-dimensional polyarylamide, 2 parts of silicone flame retardant, 0.15 parts of antioxidant 1010 and 0.25 parts of lubricant to a high-speed mixer and mix at 750 r / min for 8 min to obtain a premix.

[0032] S2. The premix obtained in step S1 is added through the main feed port of a twin-screw extruder, and 0.8 parts of silane-treated chopped aramid fibers are added through the side feed port of the twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set sequentially to 275℃, 285℃, 295℃, 305℃, 315℃, 310℃, and 305℃, with the die head temperature at 305℃ and the screw speed at 300 r / min. Melt blending extrusion is performed to obtain extruded strips. S3. The extruded strips obtained in step S2 are water-cooled, drawn, and pelletized, and then dried at 105℃ for 4.5 h to obtain a wear-resistant and impact-resistant two-dimensional polyaramid composite material for high-end equipment protective components.

[0033] Example 3 This embodiment provides a wear-resistant and impact-resistant two-dimensional polyaramid composite material for protective components of high-end equipment, comprising, by weight, 65 parts of polyphthalamide, 20 parts of polyamide 66, 16 parts of two-dimensional polyaramid, 3 parts of silicone flame retardant, 0.2 parts of antioxidant 1010, 1 part of chopped aramid fiber and 0.3 parts of lubricant.

[0034] The chopped aramid fibers have a length of 5 mm and a diameter of 20 μm. The chopped aramid fibers are immersed in a 2.0% (w / w) α-aminopropyltriethoxysilane hydrolysate to fully wet the fibers. After removal, they are dried at 120°C for 3 hours to obtain silane-treated chopped aramid fibers.

[0035] The preparation method of the composite material in this embodiment includes the following steps: S1. Add 65 parts of polyphthalamide, 20 parts of polyamide 66, 16 parts of two-dimensional polyarylamide, 3 parts of silicone flame retardant, 0.2 parts of antioxidant 1010 and 0.3 parts of lubricant to a high-speed mixer and mix at 1000 r / min for 10 min to obtain a premix.

[0036] S2. The premix obtained in step S1 is added through the main feed port of a twin-screw extruder, and one part of silane-treated chopped aramid fiber is added through the side feed port of the twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set sequentially to 280℃, 290℃, 300℃, 310℃, 320℃, 315℃, and 310℃, with the die head temperature at 310℃ and the screw speed at 400 r / min. Melt blending extrusion is performed to obtain extruded strips. S3. The extruded strips obtained in step S2 are air-cooled, drawn, and pelletized, and then dried at 120℃ for 6 hours to obtain a wear-resistant and impact-resistant two-dimensional polyaramid composite material for high-end equipment protective components.

[0037] Comparative Example 1 The only difference between this comparative example and Example 2 is that no silicone flame retardant was added, and an equal amount of polyphthalamide was used to make up the difference.

[0038] This comparative example, by weight, includes 62 parts of polyphthalamide, 17.5 parts of polyamide 66, 14 parts of two-dimensional polyaramid, 0.15 parts of antioxidant 1010, 0.8 parts of silane-treated chopped aramid fibers, and 0.25 parts of calcium stearate.

[0039] Comparative Example 2 The only difference between this comparative example and Example 2 is that the amount of silicone flame retardant was reduced from 2 parts to 0.5 parts, and 1.5 parts of polyphthalamide were used to make up the difference.

[0040] This comparative example, by weight, includes 61.5 parts of polyphthalamide, 17.5 parts of polyamide 66, 14 parts of two-dimensional polyaramid, 0.5 parts of silicone flame retardant, 0.15 parts of antioxidant 1010, 0.8 parts of silane-treated chopped aramid fiber, and 0.25 parts of calcium stearate.

[0041] Comparative Example 3 Compared with Example 2, the only difference in this comparative example is that the amount of silicone flame retardant was increased from 2 parts to 5 parts, and the amount of polyphthalamide was reduced from 60 parts to 57 parts.

[0042] This comparative example, by weight, includes 57 parts of polyphthalamide, 6617.5 parts of polyamide, 14 parts of two-dimensional polyaramid, 5 parts of silicone flame retardant, 10100.15 parts of antioxidant, 0.8 parts of silane-treated chopped aramid fiber, and 0.25 parts of calcium stearate.

[0043] Comparative Example 4 The only difference between this comparative example and Example 2 is that two-dimensional polyarylamide is not added, and 14 parts of polyphthalamide are used as an equal substitute.

[0044] This comparative example, by weight, includes 74 parts of polyphthalamide, 6617.5 parts of polyamide, 2 parts of silicone flame retardant, 10100.15 parts of antioxidant, 0.8 parts of silane-treated chopped aramid fiber, and 0.25 parts of calcium stearate.

[0045] Comparative Example 5 The only difference between this comparative example and Example 2 is that the amount of two-dimensional polyarylamide was reduced from 14 parts to 8 parts, and 6 parts of polyphthalamide were used to make up the difference.

[0046] This comparative example, by weight, includes 66 parts of polyphthalamide, 17.5 parts of polyamide 66, 8 parts of two-dimensional polyaramid, 2 parts of silicone flame retardant, 0.15 parts of antioxidant 1010, 0.8 parts of silane-treated chopped aramid fiber, and 0.25 parts of calcium stearate.

[0047] Comparative Example 6 Compared with Example 2, the only difference in this comparative example is that the amount of two-dimensional polyarylamide is increased from 14 parts to 20 parts, and the amount of polyphthalamide is correspondingly reduced from 60 parts to 54 parts.

[0048] This comparative example, by weight, includes 54 parts of polyphthalamide, 6617.5 parts of polyamide, 20 parts of two-dimensional polyaramid, 2 parts of silicone flame retardant, 10100.15 parts of antioxidant, 0.8 parts of silane-treated chopped aramid fiber, and 0.25 parts of calcium stearate.

[0049] Comparative Example 7 Compared with Example 2, the total amount of two-dimensional polyarylamide and silicone flame retardant in this comparative example remained at 16 parts, but the amount of the two was adjusted to 10 parts of two-dimensional polyarylamide and 6 parts of silicone flame retardant, with a mass ratio of 5:3.

[0050] This comparative example, by weight, includes 60 parts of polyphthalamide, 17.5 parts of polyamide 66, 10 parts of two-dimensional polyaramid, 6 parts of silicone flame retardant, 0.15 parts of antioxidant 1010, 0.8 parts of silane-treated chopped aramid fiber, and 0.25 parts of calcium stearate.

[0051] Comparative Example 8 Compared with Example 2, the total amount of two-dimensional polyarylamide and silicone flame retardant in this comparative example remained at 16 parts, but the amount of the two was adjusted to 15.5 parts of two-dimensional polyarylamide and 0.5 parts of silicone flame retardant, with a mass ratio of 31:1.

[0052] This comparative example, by weight, includes 60 parts of polyphthalamide, 17.5 parts of polyamide 66, 15.5 parts of two-dimensional polyaramid, 0.5 parts of silicone flame retardant, 0.15 parts of antioxidant 1010, 0.8 parts of silane-treated chopped aramid fiber, and 0.25 parts of calcium stearate.

[0053] Performance testing The composite materials obtained in Examples 1-3 and Comparative Examples 1-8 were vacuum dried at 120°C for 4 hours, and then standard samples were prepared by injection molding using an injection molding machine. The temperatures of each section of the injection molding machine barrel were set to 280°C, 290°C, 300°C, 310°C, and 305°C, the mold temperature was 1005°C, and the injection pressure was 80-100 MPa. The injection-molded samples were conditioned for 48 hours in an environment with a temperature of 232°C and a relative humidity of 50-10% according to GB / T2918-2018 before testing. GB / T2918-2018 is the current standard for conditioning plastic samples.

[0054] 1. Tensile strength test The test was conducted in accordance with GB / T1040.2-2022 "Determination of tensile properties of plastics - Part 2: Test conditions for molded and extruded plastics".

[0055] 2. Bending strength test Three-point bending test was performed according to GB / T9341-2008 "Determination of bending properties of plastics".

[0056] 3. Notched impact strength test The test was conducted in accordance with GB / T1843-2008 "Determination of Impact Strength of Plastic Cantilever Beams".

[0057] 4. Sliding wear performance test The test was conducted in accordance with GB / T3960-2016 "Test Method for Sliding Friction and Wear of Plastics".

[0058] 5. Load deformation temperature test The test was conducted in accordance with GB / T1634.2-2019 "Determination of load deformation temperature of plastics - Part 2: Plastics and hard rubber".

[0059] 6. Limiting Oxygen Index Test The test was conducted in accordance with GB / T2406.2-2009 "Determination of flammability of plastics by oxygen index method - Part 2: Room temperature test".

[0060] 7. Vertical Burning Performance Test Vertical burning tests were conducted in accordance with GB / T2408-2021 "Determination of the flammability of plastics - Horizontal and Vertical Methods".

[0061] Table 1: Performance Tests of Examples and Comparative Examples As shown in Table 1, Comparative Example 1, which did not contain any silicon-containing flame retardant, exhibited similar tensile strength, flexural strength, and impact strength to Example 2, but its limiting oxygen index was only 23.9%, resulting in a vertical flammability rating of HB. In Example 2, compared to Comparative Example 1, the limiting oxygen index increased by 8.9 percentage points, and the flammability rating improved from HB to V-0.

[0062] The above results indicate that polyphthalamide, polyamide 66, two-dimensional polyaramid, and chopped aramid fibers alone cannot enable the composite material to achieve stable V-0 flame retardant performance. Silicone-containing flame retardants are necessary components to achieve high flame retardant performance.

[0063] In Comparative Example 2, the amount of silicon-containing flame retardant was only 0.5 parts, its limiting oxygen index was 26.6%, and its vertical burning rating was only V-2. Although Comparative Example 2 still maintained relatively good mechanical properties, its flame retardant properties could not meet the requirements of high-end equipment protective components for self-extinguishing upon removal of flame and suppression of burning drips.

[0064] In Comparative Example 3, the amount of silicon-containing flame retardant was increased to 5 parts, its limiting oxygen index increased to 35.2% and reached V-0 level, but the tensile strength decreased to 146.1 MPa, the flexural strength decreased to 209.0 MPa, the notched impact strength decreased to 16.6 kJ / m, and the wear volume increased to 6.6 mm.

[0065] Compared to Comparative Example 3, Example 2 showed an increase in tensile strength of approximately 9.0%, flexural strength of approximately 7.9%, notched impact strength of approximately 18.7%, and a reduction in wear volume of approximately 22.7%. This indicates that while excessive silicon-containing flame retardant can further improve the limiting oxygen index, it also increases the probability of contact and agglomeration between flame retardant particles, reduces the interfacial continuity between the flame retardant and the polyamide resin matrix, and creates localized stress concentrations, leading to a decrease in the mechanical properties and wear resistance of the material.

[0066] Therefore, the amount of silicon-containing flame retardant used is not necessarily better the higher it is. Controlling it to 1-3 parts by weight can achieve V-0 flame retardant performance while avoiding the adverse effects of excessive flame retardant on the material's mechanical properties and abrasion resistance.

[0067] Comparative Example 4, without the addition of two-dimensional polyarylamide, exhibited a tensile strength of 132.5 MPa, a flexural strength of 189.8 MPa, a notched impact strength of 14.3 kJ / m, a wear volume of 10.9 mm, and a load deformation temperature of 219 °C. Compared to Comparative Example 4, Example 2 showed an increase in tensile strength of approximately 20.2%, a flexural strength of approximately 18.9%, a notched impact strength of approximately 37.8%, a wear volume reduction of approximately 53.2%, and a load deformation temperature increase of 22 °C. These results demonstrate that two-dimensional polyarylamide significantly contributes to the mechanical properties, impact resistance, wear resistance, and heat resistance of the composite material. The lamellar structure of two-dimensional polyarylamide can form a two-dimensional load-bearing structure within the polyamide resin matrix, dispersing local stress when the material is subjected to external impact, and consuming impact energy through lamellar deflection, crack passivation, and extended crack propagation paths. During sliding friction, the two-dimensional lamellar structure can also inhibit surface material peeling, thereby significantly reducing the wear volume. In Comparative Example 5, the amount of two-dimensional polyarylamide was reduced to 8 parts, and its tensile strength, flexural strength, and impact strength were 145.0 MPa, 205.7 MPa, and 16.5 kJ / m, respectively, while the wear volume increased to 8.0 mm. This indicates that when the amount of two-dimensional polyarylamide is too low, it is difficult to form a continuous and effective two-dimensional load-bearing and crack-resistant structure in the resin matrix, and its effect on improving wear resistance and impact resistance is limited. In Comparative Example 6, the amount of two-dimensional polyarylamide was increased to 20 parts, and its load deformation temperature increased to 245°C, but the notched impact strength decreased to 15.8 kJ / m, and the wear volume increased to 6.8 mm. Compared with Comparative Example 6, Example 2 showed an increase of approximately 24.7% in notched impact strength and a decrease of 25.0% in wear volume. This result indicates that when the amount of two-dimensional polyarylamide is too high, although it can improve the rigidity and thermal deformation stability of the material, the layers are prone to stacking and agglomeration due to hydrogen bonding, preventing the polyamide melt from fully wetting each two-dimensional layer. Agglomerated areas can form localized rigid defects and stress concentration points, which can make them more prone to crack initiation and surface peeling during impact or friction.

[0068] Therefore, limiting the amount of two-dimensional polyarylamide to 12 to 16 parts by weight can form an effective two-dimensional reinforcing network while avoiding agglomeration and embrittlement caused by excessive lamellar layers.

[0069] In Example 2, the mass ratio of two-dimensional polyarylamide to silicone flame retardant was 7:1. In Comparative Example 7, the total amount of both remained at 16 parts, but the two-dimensional polyarylamide and silicone flame retardant were adjusted to 10 parts and 6 parts, respectively, with a mass ratio of 5:3. Although the limiting oxygen index of Comparative Example 7 reached 36.1%, the tensile strength, flexural strength, and notched impact strength decreased to 140.2 MPa, 200.4 MPa, and 15.0 kJ / m, respectively, and the wear volume increased to 8.2 mm. Compared with Comparative Example 7, Example 2 showed an increase in tensile strength of approximately 13.6%, an increase in flexural strength of approximately 12.6%, an increase in notched impact strength of approximately 31.3%, and a decrease in wear volume of approximately 37.8%. Although the limiting oxygen index of Example 2 was lower than that of Comparative Example 7, it still reached 32.8% and had V-0 flame retardant performance, which met the flame retardant requirements. This indicates that when the proportion of silicon-containing flame retardant is too high and the proportion of two-dimensional polyarylamide is too low, the material will have excessive flame retardant properties but significantly insufficient wear resistance and impact resistance, and will not be able to obtain the comprehensive performance suitable for high-end equipment protective components.

[0070] In Comparative Example 8, the two-dimensional polyarylamide and the silicon-containing flame retardant were 15.5 parts and 0.5 parts, respectively, with a mass ratio of 31:1. This material exhibited relatively good tensile strength, flexural strength, and impact strength, but its limiting oxygen index was only 26.9%, and its vertical flammability rating was V-2. In Example 2, compared to Comparative Example 8, the limiting oxygen index increased by 5.9 percentage points, the vertical flammability rating improved from V-2 to V-0, and the wear volume decreased from 5.8 mm to 5.1 mm. These results indicate that when the mass ratio of two-dimensional polyarylamide to silicon-containing flame retardant is too high, the silicon-containing flame retardant is insufficient to form a continuous and dense silicon-containing carbonized protective layer when the material is heated, thus failing to achieve stable V-0 flame retardant performance.

[0071] Comparative Examples 7 and 8, when the total amount of two-dimensional polyarylamide and silicon-containing flame retardant is the same or similar, show significantly different comprehensive properties when only the relative amount of the two is changed. This indicates that the material performance does not depend on the simple total amount of the two, but on the appropriate ratio between the two-dimensional polyarylamide and the silicon-containing flame retardant.

[0072] As can be seen from the test results of Example 2 and the comparative examples, the technical effect of the present invention is not a simple superposition of the effects of each component, but rather a multi-scale synergistic effect formed between the two-dimensional polyaramid, the silicon-containing flame retardant and the silane-treated short-cut aramid fiber.

[0073] Two-dimensional polyaramids primarily form layered load-bearing and crack-blocking structures, improving the material's abrasion resistance, impact resistance, and heat resistance. Short-cut aramid fibers bridge the two-dimensional layers and the polyamide resin matrix, bearing and transmitting large-scale impact loads. Silane treatment enhances the interfacial bonding between the short-cut aramid fibers and the polyamide resin, reducing fiber pull-out and interfacial debonding. The triazine and silicon-containing structures in silicone flame retardants promote the formation of a stable char layer when the material is heated, improving the limiting oxygen index and vertical flammability rating. Simultaneously, within appropriate dosage ranges, silicone flame retardants do not significantly disrupt the load-bearing network formed by the two-dimensional polyaramids. When there is insufficient two-dimensional polyaramid, the material cannot form an effective two-dimensional crack-blocking network; when there is excessive two-dimensional polyaramid, the impact and abrasion resistance decreases due to layer stacking. When there is insufficient silicone flame retardant, the material cannot achieve a V-0 rating; when there is excessive silicone flame retardant, although the limiting oxygen index continues to increase, the mechanical properties and abrasion resistance of the material decrease. In particular, Comparative Examples 7 and 8 show that even if the total amount of two-dimensional polyarylamide and silicone flame retardant remains unchanged, simply changing their ratio does not yield the same overall performance as in Example 2. This demonstrates that the dosage range of 12–16 parts by weight of two-dimensional polyarylamide and 1–3 parts by weight of silicone flame retardant has significant selective value and cannot be directly obtained by conventionally increasing the amount of reinforcing agent or flame retardant.

[0074] It should be noted that, in this document, the terms include, encompass, or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, the inclusion of a defined element by a statement does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0075] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high-end equipment protection component wear resistant impact resistant two-dimensional polyaramid composite material, characterized in that, By weight, it includes the following components: 55-65 parts by weight of polyphthalamide, 15-20 parts by weight of polyamide 66, 12-16 parts by weight of two-dimensional polyaramid, 1-3 parts by weight of silicone flame retardant, 0.1-0.2 parts by weight of antioxidant 1010, 0.6-1 parts by weight of chopped aramid fiber, and 0.2-0.3 parts by weight of lubricant.

2. The high-end equipment guard component wear-resistant impact-resistant two-dimensional polyaramid composite material according to claim 1, characterized in that, The chopped aramid fibers have a length of 1–5 mm and a diameter of 8–20 μm; The chopped aramid fibers are impregnated with 0.5-2.0% (by mass) of α-aminopropyltriethoxysilane hydrolysate and dried at 80-120°C for 1-3 hours before use.

3. The high-end equipment guard component wear resistant impact resistant two-dimensional polyaramid composite material of claim 1, wherein, The preparation method of the silicon-containing flame retardant is as follows: S1. Add 18.4-18.6 g of melamine and 300 mL of 1,4-dioxane to a three-necked flask. After the melamine is completely dissolved, add an aqueous solution containing 8.6-8.9 g of 2-amino-2-methyl-propanol and 3.8-4 g of sodium hydroxide dropwise to the flask at 0-5 °C. After reacting for 2-3 hours, raise the temperature of the system to 45-50 °C, and then add 8.6-8.9 g of 2-amino-2-methyl-propanol... A 0.9 g aqueous solution of 2-amino-2-methyl-propanol and 3.8-4 g sodium hydroxide was slowly added dropwise to a three-necked flask. After reacting for 2-3 hours, the system temperature was raised to 80-85℃. Finally, an aqueous solution containing 8.6-8.9 g of 2-amino-2-methyl-propanol and 3.8-4 g of sodium hydroxide was slowly added dropwise to the three-necked flask. After the addition was complete, the entire reaction system was maintained at 80-85℃ for 8-12 hours. After the reaction was completed, after post-processing, intermediate 1 was obtained. S2. Intermediate 1 and triethylamine were added sequentially to a three-necked flask containing 200 mL of acetonitrile. Then, diphenyldichlorosilane was added at 0-5 °C. The reaction was carried out for 1-1.5 h, and then the temperature was increased to react for another 8-10 h. After the reaction was completed, the precipitate was filtered out and washed with deionized water and 1,4-dioxane, respectively. The precipitate was then dried in a forced-air drying oven to obtain a silicon-containing flame retardant.

4. The high-end equipment guard component wear-resistant impact-resistant two-dimensional polyaramid composite material according to claim 3, characterized in that, In step S1, the post-processing involves first cooling the solution in the three-necked flask to room temperature, then precipitating the precipitate with deionized water, washing the white precipitate three times with deionized water, and then drying it.

5. The high-end equipment guard component wear resistant impact resistant two-dimensional polyaramid composite material of claim 3, wherein, In step S2, the ratio of intermediate 1, triethylamine, and diphenyldichlorosilane is 6.1-6.4 g: 6.02-6.13 g: 0.028-0.03 mol.

6. The high-end equipment guard component wear resistant impact resistant two-dimensional polyaramid composite material of claim 3, wherein, In step S2, the heating temperature is 35-40℃.

7. A method for preparing a wear-resistant and impact-resistant two-dimensional polyaramid composite material for high-end equipment protective components as described in any one of claims 1-6, characterized in that, Includes the following steps: S1. First, add polyphthalamide, polyamide 66, two-dimensional polyarylamide, silicone flame retardant, antioxidant 1010 and lubricant into a high-speed mixer and mix at 500-1000 r / min for 5-10 min to obtain a premix; S2. The premix is ​​added through the main feed port of the twin-screw extruder, and the chopped aramid fibers are added through the side feed port of the twin-screw extruder. The mixture is melt-blended and extruded under the conditions of 270-320°C in each temperature zone and 200-400 r / min in the screw speed to obtain the extruded strip. S3. The extruded strip is water-cooled or air-cooled and then pelletized, and dried at 90-120°C to obtain the wear-resistant and impact-resistant two-dimensional polyaramid composite material for high-end equipment protective components.

8. The preparation method of the wear-resistant and impact-resistant two-dimensional polyaramid composite material for high-end equipment protective components according to claim 7, characterized in that, The drying time for step S3 is 3-6 hours.