An environmentally friendly artistic coating with formaldehyde removal and antibacterial functions and its preparation method

By using a specific combination of coating components and preparation processes, the problems of secondary formaldehyde release and emulsion instability in coatings have been solved, resulting in coatings with long-lasting formaldehyde removal and antibacterial effects, suitable for the field of environmentally friendly artistic coatings.

CN123107480APending Publication Date: 2026-11-17YUNNAN MENESEN BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611575832.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing formaldehyde-removing coatings are prone to secondary formaldehyde release during long-term use, and their effective formaldehyde removal period is generally short. In addition, the introduction of formaldehyde-removing and antibacterial additives may lead to local demulsification and storage instability of the coating emulsion system.

Method used

A specific combination of customized high-acrylate copolymer emulsion, polyethylene glycol 400, micron-sized zinc borate, sodium gluconate and dicyandiamide is used to stabilize metal ions by forming complexes in the coating, promote formaldehyde reaction and inhibit secondary release, while controlling the dispersion and stirring process of the emulsion to maintain system stability.

Benefits of technology

It achieves long-lasting formaldehyde removal, inhibits secondary formaldehyde release, and maintains the stability of the coating while possessing antibacterial properties, meeting the requirements for long-term washability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107480A_ABST
    Figure CN123107480A_ABST
Patent Text Reader

Abstract

This application relates to the field of coating manufacturing and discloses an environmentally friendly artistic coating with formaldehyde removal and antibacterial functions, as well as its preparation method. The coating is mainly composed of a customized high-acrylate copolymer emulsion, polyethylene glycol 400, micron-sized zinc borate, sodium gluconate, dicyandiamide, 2-amino-2-methyl-1-propanol, and inorganic pigments and fillers. By constructing a polar microenvironment within the emulsion matrix using polyethylene glycol 400, and combining it with the locally coordinated complexes formed by zinc borate, sodium gluconate, and dicyandiamide, the coating can capture and convert free formaldehyde through nucleophilic addition reactions, while simultaneously slowly releasing active zinc ions to achieve antibacterial function. The preparation method employs a stepwise feeding, pH locking, and low-rate dripping process, effectively avoiding the problem of system demulsification and flocculation. The product of this invention features a long formaldehyde removal cycle, inhibition of secondary formaldehyde release, stable antibacterial performance, and resistance to flocculation during liquid storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating manufacturing technology, specifically to an environmentally friendly artistic coating with formaldehyde removal and antibacterial functions and its preparation method. Background Technology

[0002] As people's demands for indoor living environment quality increase, the application of environmentally friendly interior wall coatings is becoming increasingly widespread. Artistic coatings, as a wall material that combines decoration and functionality, often need to improve indoor air quality while satisfying visual aesthetics. Since the release of formaldehyde from interior decoration materials and furniture is a long-term, slow process, developing coating products that can effectively remove free formaldehyde has become a key focus of the industry.

[0003] Most formaldehyde-removing coatings on the market rely on conventional methods such as physical adsorption using porous materials or photocatalytic degradation. Physical adsorption can quickly reduce formaldehyde concentration in the air initially, but the adsorption sites easily reach saturation. When indoor temperature or humidity changes, the adsorbed formaldehyde molecules can easily be released again, causing secondary pollution. Photocatalytic products typically require specific intensities of ultraviolet light to activate their catalytic activity, and their actual formaldehyde removal efficiency is often limited in low-light indoor environments. Some coatings that use chemical elimination methods suffer from uncontrollable reactions or short effective periods.

[0004] To enhance the overall environmental performance of coatings, some products incorporate metal ion-based antibacterial agents in addition to formaldehyde removal. However, in common acrylic emulsion systems, directly free metal ions can easily disrupt the electric double layer structure on the surface of emulsion particles. This loss of electrostatic repulsion can lead to irreversible aggregation of emulsion particles, causing instability phenomena such as localized demulsification, flocculation, or even gelation during the production, formulation, or storage stages of the coating. Maintaining the long-term stability of the liquid coating system while preserving the activity of functional additives is a critical technological challenge that urgently needs to be addressed in this field. Summary of the Invention

[0005] The technical problem solved by this invention is that existing formaldehyde-removing coatings often experience secondary formaldehyde release during long-term use, and the effective formaldehyde removal period is generally short.

[0006] On the other hand, if formaldehyde removal and antibacterial additives are introduced into the system, it often leads to problems such as local demulsification and storage instability of the coating emulsion system.

[0007] To address the above problems, the present invention provides the following technical solution:

[0008] In a first aspect, the present invention provides an environmentally friendly artistic coating with formaldehyde removal and antibacterial functions, employing the following technical solution:

[0009] An environmentally friendly artistic paint with formaldehyde removal and antibacterial functions is made from raw materials comprising the following parts by weight:

[0010] Customized high 250-350 parts of acrylate copolymer emulsion;

[0011] 10-20 parts of polyethylene glycol 400;

[0012] 10–25 parts of micron-sized zinc borate;

[0013] 1-3 parts sodium gluconate;

[0014] Dicyandiamide 5-15 parts;

[0015] 1 to 3 parts of 2-amino-2-methyl-1-propanol;

[0016] 100-150 parts of rutile titanium dioxide;

[0017] 160–211 parts of heavy calcium carbonate;

[0018] 5-10 parts of dispersant;

[0019] 2-4 parts of defoamer;

[0020] Thickener 5-10 parts;

[0021] 300-350 parts of deionized water.

[0022] By adopting the above technical solution, due to the use of polyethylene glycol 400 and customized high-performance polyethylene glycol 400, the high-performance polyethylene glycol 400 can be used to achieve the desired high efficiency. The specific combination of acrylate copolymer emulsion, micron-sized zinc borate, sodium gluconate and dicyandiamide allows the components to interact at the microscopic level, thus contributing to a long-lasting formaldehyde removal and antibacterial effect, and inhibiting the secondary release of formaldehyde to a certain extent.

[0023] Its core reaction and mechanism of action are as follows:

[0024] Customized high After the acrylate copolymer emulsion is cured into a film, the substrate usually has high rigidity.

[0025] Polyethylene glycol 400, as a small molecule polymer with terminal hydroxyl groups and a polyether backbone, can be interspersed and dispersed between the molecular chains of the above emulsion.

[0026] The introduction of this component creates certain polar micro-regions within the rigid coating, which in turn increases the penetration and diffusion rate of free formaldehyde molecules in the air into the dry film, enabling formaldehyde molecules to cross the gas-solid interface and enter the reaction sites inside the coating.

[0027] In deionized water, 2-amino-2-methyl-1-propanol is mainly used to provide a weakly alkaline environment, which promotes the slow dissociation of zinc ions from the micron-sized zinc borate surface.

[0028] Considering that sodium gluconate molecules contain multiple hydroxyl and carboxyl groups, and dicyandiamide molecules contain multiple amino and imino groups, zinc ions tend to undergo polydentate chelation coordination with the carboxyl oxygen of sodium gluconate and the amino nitrogen of dicyandiamide, forming a sterically hindered ternary coordination supramolecular complex in the coating system.

[0029] This complexation state can largely maintain the uniform and stable suspension of dicyandiamide and zinc-containing species in the emulsion system, thereby reducing the tendency of emulsion demulsification or flocculation precipitation caused by free metal ions.

[0030] When formaldehyde molecules entering the polar microregion come into contact with the above complex, the carbonyl group of formaldehyde and the free amino group of dicyandiamide can undergo nucleophilic addition and dehydration condensation reactions. The reaction process typically includes:

[0031] ;

[0032] ;

[0033] In this process, the central zinc ion, through the polarization effect of the coordination bond, helps to reduce the reaction activation energy of the carbonyl carbon of formaldehyde and accelerate the nucleophilic addition rate.

[0034] The generated hydroxymethyl derivative further undergoes a cross-linking reaction with adjacent amino groups within the system, forming a stable spatial network polymer product.

[0035] This chemical bond irreversibly transforms free formaldehyde into a solid high-molecular-weight product, thereby effectively blocking the reverse desorption reaction pathway of formaldehyde and better controlling the secondary release of formaldehyde.

[0036] Micron-sized zinc borate provides long-lasting antibacterial protection within the coating.

[0037] When the system continuously consumes formaldehyde, the change in the spatial configuration of dicyandiamide may cause a shift in the local equilibrium of the original coordination complex, prompting the continuous and slow release of trace amounts of active zinc ions and borate ions from the coating film.

[0038] The released active zinc ions can penetrate the bacterial cell wall, destroy the sulfhydryl structure of bacterial proteases, and cause the bacteria to lose their ability to divide and reproduce, thus exhibiting corresponding antibacterial functions.

[0039] Preferably, an environmentally friendly artistic paint with formaldehyde removal and antibacterial functions is made from raw materials comprising the following parts by weight: customized high The composition includes 300 parts of acrylate copolymer emulsion, 15 parts of polyethylene glycol 400, 15 parts of micron-sized zinc borate, 2 parts of sodium gluconate, 10 parts of dicyandiamide, 2 parts of 2-amino-2-methyl-1-propanol, 120 parts of rutile titanium dioxide, 198 parts of heavy calcium carbonate, 8 parts of dispersant, 3 parts of defoamer, 7 parts of thickener, and 320 parts of deionized water.

[0040] By adopting the above technical solution, the volume concentration of inorganic fillers and organic materials in the coating system reaches a more suitable balance point.

[0041] This ratio can largely maintain the distribution density of polar microenvironments in the dry film, while minimizing the reduction of the physical and mechanical density of the coating surface, so as to better meet the requirements of long-term washability.

[0042] Preferably, the chemical formula of the micron-sized zinc borate is 2ZnO·3B2O3·3.5H2O, and its median diameter D50 is 5.0μm to 10.0μm;

[0043] The average molecular weight of polyethylene glycol 400 is 380 g / mol to 420 g / mol.

[0044] By adopting the above technical solution, zinc borate powder with a particle size between 5.0μm and 10.0μm can easily form a dense filler with rutile titanium dioxide and heavy calcium carbonate during stacking, which helps to avoid rough coating or sedimentation caused by large particles.

[0045] Polyethylene glycol with a molecular weight in the range of 380 g / mol to 420 g / mol exhibits a liquid state with suitable viscosity, and can maintain good compatibility with acrylate molecular chains without the introduction of external volatile organic solvents.

[0046] Preferred, customized high The acrylate copolymer emulsion was prepared from a copolymer raw material comprising the following parts by weight:

[0047] 615 to 640 parts methyl methacrylate, 345 to 370 parts butyl acrylate, and 15 parts methacrylic acid; custom high-performance methacrylate is available. The theoretical glass transition temperature of acrylate copolymer emulsions is 25.8℃ to 30.2℃.

[0048] By adopting the above technical solution, a high proportion of methyl methacrylate hard monomers are copolymerized with butyl acrylate soft monomers, and an appropriate amount of methacrylic acid is introduced into the copolymer chain to provide carboxyl functional groups, so that the copolymer emulsion has a relatively high glass transition temperature at room temperature.

[0049] The inherent hardness of this polymer can provide good mechanical strength after film formation, thus mitigating to some extent the softening and stickiness issues that may result from the addition of polyethylene glycol 400.

[0050] Preferred, customized high The preparation method of the acrylate copolymer emulsion includes the following steps:

[0051] Step 1: Mix methyl methacrylate, butyl acrylate and methacrylic acid to obtain the total monomer;

[0052] Sodium dodecyl ether sulfate, isomeric alcohol polyoxyethylene ether, and a portion of deionized water were mixed evenly, and then the total monomer was added and stirred to obtain a pre-emulsion.

[0053] Step 2: Dissolve ammonium persulfate in deionized water to prepare an initiator aqueous solution;

[0054] Step 3: Take a portion of the pre-emulsion and deionized water and add them to the reaction flask. Heat the mixture to 78°C, add a portion of the initiator aqueous solution, and react at a constant temperature to obtain the seed emulsion.

[0055] Step 4: Control the temperature inside the reaction flask at 82°C, and simultaneously add the remaining pre-emulsion and initiator aqueous solution at a uniform rate;

[0056] Step 5: After the addition is complete, heat to 86℃ and maintain the temperature for reaction, then cool to 35℃, adjust the pH of the system to 7.8 using ammonia, and filter to obtain the final product.

[0057] By adopting the above technical solutions, using seed emulsion polymerization process and anionic and nonionic composite emulsion system, it is helpful to make the synthesized copolymer emulsion have a narrow and uniform particle size distribution.

[0058] The subsequent heating and holding treatments, as well as pH adjustment, aim to promote the complete conversion of monomers and maintain the electrostatic repulsion stability of the emulsion microparticle surface, thus providing a relatively stable matrix for subsequent coating formulation.

[0059] Secondly, the present invention provides a method for preparing an environmentally friendly artistic coating with formaldehyde removal and antibacterial functions, using the following technical solution:

[0060] A method for preparing an environmentally friendly artistic coating with formaldehyde removal and antibacterial functions includes the following steps:

[0061] Step 1: Mix some deionized water, dispersant, and defoamer, then add rutile titanium dioxide, heavy calcium carbonate, and micron-sized zinc borate in sequence, and perform high-shear dispersion to obtain the basic slurry.

[0062] Step 2: Reduce the shearing speed and add customized high-strength... The acrylate copolymer emulsion was stirred at low speed, and then polyethylene glycol 400 was added and stirred at low speed continuously.

[0063] Step 3: Add 2-amino-2-methyl-1-propanol while stirring at low speed to adjust the pH of the system to 8.5 to 9.0. Then dissolve sodium gluconate in deionized water to prepare an aqueous solution and add it dropwise to the system while maintaining low-speed stirring.

[0064] Step 4: Dissolve dicyandiamide in deionized water to prepare a transparent solution, add it dropwise to the system while maintaining low-speed stirring; Step 5: Add thickener, stir evenly, and then filter to obtain the finished product.

[0065] By adopting the above technical solution, the system instability problem during the introduction of functional additives can be effectively avoided due to the specific feeding sequence and shearing conditions.

[0066] From the perspective of reaction control, high-shear dispersed inorganic fillers in the absence of emulsion mainly rely on mechanical force to break up powder agglomeration.

[0067] After the system reduces its shear rate, an acrylic emulsion that is sensitive to shear is then introduced.

[0068] To prevent changes in the deprotonated state of the emulsion carboxyl groups due to sudden changes in pH, the weakly alkaline pH of the system was adjusted and stabilized with 2-amino-2-methyl-1-propanol before the introduction of the core coordinating agent.

[0069] In addition, sodium gluconate and dicyandiamide are introduced sequentially by adding the solution dropwise, allowing organic molecules to slowly penetrate to the interface between zinc borate particles and the emulsion under low-speed stirring, and form a stable coordination structure in situ. This greatly reduces the risk of gelation caused by local material accumulation.

[0070] Preferably, in step 1, the linear velocity of the high-shear dispersion disc is 20 m / s to 25 m / s, the dispersion time is 30 min to 45 min, and the fineness of the resulting base slurry is controlled to be ≤40 μm.

[0071] By adopting the above technical solution, it is beneficial to achieve a suitable grinding fineness for inorganic pigments and fillers such as rutile titanium dioxide and heavy calcium carbonate, reduce the probability of coarse particles damaging the dry film density during film formation, and at the same time, allow micron-sized zinc borate to be better dispersed to expose sufficient interfaces for subsequent coordination reactions.

[0072] Preferably, in step 4, the pretreatment of dicyandiamide is performed by adding dicyandiamide to deionized water and dissolving it in a water bath at a temperature controlled of 40°C to 45°C to form a transparent solution before adding it dropwise.

[0073] By adopting the above technical solution, given the limited solubility of dicyandiamide in room temperature water, directly adding it to the coating in powder form can easily lead to uneven distribution within the system and the formation of crystal clumps.

[0074] By preparing a transparent solution using water bath heating and then slowly adding it dropwise, dicyandiamide molecules are homogeneously distributed within the coating system, thereby increasing the effective collision probability of formaldehyde capture sites to some extent.

[0075] Preferably, in steps 2 to 5, the linear velocity of the dispersion disc during low-speed stirring is 3m / s to 5m / s.

[0076] By adopting the above technical solution, the low shear force with a linear velocity in the range of 3m / s to 5m / s usually only maintains the macroscopic convective mixing of materials and does not cause obvious mechanical tearing of the protective layer of emulsion particles.

[0077] This helps maintain the molecular configuration integrity during the assembly of coordination complexes and reduces the possibility of demulsification caused by high shear.

[0078] Preferably, in step 3, after the sodium gluconate aqueous solution is added dropwise, the mixture is stirred at a low speed for 20 to 30 minutes.

[0079] In step 4, keep stirring at a low speed for 15 to 20 minutes throughout the entire process of adding the dicyandiamide solution and after the addition is completed.

[0080] By adopting the above technical solution, relatively sufficient thermodynamic and kinetic time is provided for ion migration and coordination bond formation between material interfaces.

[0081] If the mixing time is too short, it often leads to incomplete complexation reaction and increased concentration of free metal ions, which in turn affects the long-term storage stability of the coating product.

[0082] This invention provides an environmentally friendly artistic coating with formaldehyde removal and antibacterial functions, and its preparation method. It possesses the following beneficial effects:

[0083] 1. This invention introduces polyethylene glycol 400 into a customized high-Tg acrylate copolymer emulsion, constructing polar microregions within a rigid coating film that facilitate formaldehyde diffusion. Free formaldehyde molecules entering these microregions undergo nucleophilic addition reactions with the free amino groups of dicyandiamide, transforming them into solid, high-molecular-weight products. This method of immobilizing free formaldehyde through chemical bonding interrupts the reverse formaldehyde removal pathway, maintaining formaldehyde removal effectiveness over a longer period and effectively suppressing secondary formaldehyde release.

[0084] 2. The coating formulation of this invention utilizes micron-sized zinc borate to form a specific local coordination state with sodium gluconate and dicyandiamide in a weakly alkaline environment. When the system continuously consumes formaldehyde, causing a change in the spatial configuration of dicyandiamide, the local coordination equilibrium shifts, prompting the slow release of trace amounts of active zinc ions from the coating film. These released zinc-containing species can disrupt the bacterial cell wall and its protease structure, enabling the coating to exhibit corresponding environmentally responsive antibacterial properties while possessing formaldehyde removal capabilities.

[0085] 3. Regarding the preparation process, this invention employs a step-by-step feeding and low-shear control strategy. After dispersing inorganic pigments and fillers under high shear, the stirring speed is reduced, and the weakly alkaline pH of the system is pre-locked using 2-amino-2-methyl-1-propanol. Then, sodium gluconate and dicyandiamide are slowly introduced dropwise as a solution. This specific process sequence avoids localized high-concentration accumulation of materials and abrupt changes in the system's pH, reducing the risk of emulsion flocculation and demulsification caused by free metal ions or high shear forces, thus ensuring the long-term storage stability of the finished coating. Attached Figure Description

[0086] Figure 1 The following are comparative graphs of the electrochemical impedance and infrared spectroscopy of the dry film of the present invention, wherein (a) is a comparative graph of the electrochemical impedance of the dry film of Example 2 and Comparative Example 2, and (b) is a comparative graph of the infrared spectroscopy of the dry film of Example 2, the dry film of Comparative Example 2 and pure polyethylene glycol 400.

[0087] Figure 2 The following are the formaldehyde consumption concentration curves and solid-state nuclear magnetic resonance spectra of the present invention, wherein (a) is the decay curve of free formaldehyde concentration in the sealed chamber of Example 2 and Comparative Example 5 over time, and (b) is the 13C solid-state nuclear magnetic resonance spectrum of the dry film before and after formaldehyde absorption in Example 2.

[0088] Figure 3 This is a comparison diagram of the Stormer viscosity changes before and after the liquid-phase accelerated thermal storage of the present invention;

[0089] Figure 4 The following is a test chart of the formaldehyde purification rate and secondary release amount of the present invention, wherein (a) is a purification rate decay curve of Example 2, Comparative Example 2 and Comparative Example 5 in three consecutive formaldehyde injection strokes, and (b) is a comparison chart of the secondary release amount of formaldehyde of the corresponding test objects in the nitrogen purging stage.

[0090] Figure 5 The diagram shows the differential environmental antibacterial rate linkage response of the present invention, wherein (a) is a trend diagram of the antibacterial rate of Example 2 and Comparative Example 2 against Escherichia coli under different pretreatment environments, and (b) is a trend diagram of the antibacterial rate of the corresponding test object against Staphylococcus aureus under different pretreatment environments.

[0091] Figure 6 This is a physical and mechanical comparison test diagram of the washability of the coating of the present invention. Detailed Implementation

[0092] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0093] The main raw materials and reagents used in the following examples and comparative examples have the following sources and specifications. Reagents not specifically mentioned are all commercially available analytical grade or higher grade products.

[0094] 2-Amino-2-methyl-1-propanol, CAS No. 124-68-5, purity ≥95.0wt%.

[0095] Dicyandiamide, CAS No. 461-58-5, purity ≥99.0wt%.

[0096] Sodium gluconate, CAS No. 527-07-1, purity ≥98.0wt%.

[0097] Polyethylene glycol 400, CAS number 25322-68-3, has an average molecular weight of 380 g / mol to 420 g / mol.

[0098] Micron-sized zinc borate, CAS number 1332-07-6, chemical formula 2ZnO·3B2O3·3.5H2O, powder median diameter D50 is 5.0μm~10.0μm.

[0099] Methyl methacrylate, CAS number 80-62-6, purity ≥99.5wt%.

[0100] Butyl acrylate, CAS No. 141-32-2, purity ≥99.0wt%.

[0101] Methacrylic acid, CAS number 79-41-4, purity ≥99.0wt%.

[0102] Preparation Example 1:

[0103] This preparation example provides a customized high-performance solution. A method for preparing an acrylate copolymer emulsion includes the following steps:

[0104] (1) Mix 615g of methyl methacrylate, 370g of butyl acrylate and 15g of methacrylic acid as the total monomer.

[0105] Mix 10g sodium dodecyl ether sulfate, 10g isomeric alcohol polyoxyethylene ether, and 400g deionized water thoroughly.

[0106] The total monomer was added to the above mixed solution and stirred continuously at 1200 rpm for 30 minutes to obtain a pre-emulsion.

[0107] (2) Dissolve 5g of ammonium persulfate completely in 100g of deionized water to prepare an initiator aqueous solution.

[0108] (3) In a reaction flask equipped with a reflux condenser, a thermometer and a mechanical stirrer, add 71g of the pre-emulsion and 470g of deionized water, start stirring and heat to 78°C, then add 21g of the initiator aqueous solution, and react at a constant temperature for 15min to obtain the seed emulsion.

[0109] (4) Adjust and control the temperature inside the reaction flask at 82°C, and use a double-dropping funnel to simultaneously and uniformly add the remaining pre-emulsion and the remaining initiator aqueous solution for 180 min.

[0110] (5) After the addition is complete, heat the system to 86°C and keep it at that temperature for 60 min.

[0111] The system was then cooled to 35°C, and the pH was adjusted to 7.8 using 25.0 wt% ammonia solution. The mixture was then filtered through a 200-mesh filter to obtain the customized high-quality product. Acrylic ester copolymer emulsion (its theoretical glass transition temperature is approximately 25.8°C).

[0112] Preparation Example 2:

[0113] This preparation example provides a customized high-performance solution. The preparation method of acrylate copolymer emulsion includes the following steps: (1) mixing 630g of methyl methacrylate, 355g of butyl acrylate and 15g of methacrylic acid as total monomer.

[0114] Mix 10g sodium dodecyl ether sulfate, 10g isomeric alcohol polyoxyethylene ether, and 400g deionized water thoroughly.

[0115] The total monomer was added to the above mixed solution and stirred continuously at 1200 rpm for 30 minutes to obtain a pre-emulsion.

[0116] (2) Dissolve 5g of ammonium persulfate completely in 100g of deionized water to prepare an initiator aqueous solution.

[0117] (3) In a reaction flask equipped with a reflux condenser, a thermometer and a mechanical stirrer, add 71g of the pre-emulsion and 470g of deionized water, start stirring and heat to 78°C, then add 21g of the initiator aqueous solution, and react at a constant temperature for 15min to obtain the seed emulsion.

[0118] (4) Adjust and control the temperature inside the reaction flask at 82°C, and use a double-dropping funnel to simultaneously and uniformly add the remaining pre-emulsion and the remaining initiator aqueous solution for 180 min.

[0119] (5) After the addition is complete, heat the system to 86°C and keep it at that temperature for 60 min.

[0120] The system was then cooled to 35°C, and the pH was adjusted to 7.8 using 25.0 wt% ammonia solution. The mixture was then filtered through a 200-mesh filter to obtain the customized high-quality product. Acrylic ester copolymer emulsion (its theoretical glass transition temperature is approximately 28.4°C).

[0121] Preparation Example 3:

[0122] This preparation example provides a customized high-performance solution. A method for preparing an acrylate copolymer emulsion includes the following steps:

[0123] (1) Mix 640g of methyl methacrylate, 345g of butyl acrylate and 15g of methacrylic acid as the total monomer.

[0124] Mix 10g sodium dodecyl ether sulfate, 10g isomeric alcohol polyoxyethylene ether, and 400g deionized water thoroughly.

[0125] The total monomer was added to the above mixed solution and stirred continuously at 1200 rpm for 30 minutes to obtain a pre-emulsion.

[0126] (2) Dissolve 5g of ammonium persulfate completely in 100g of deionized water to prepare an initiator aqueous solution.

[0127] (3) In a reaction flask equipped with a reflux condenser, a thermometer and a mechanical stirrer, add 71g of the pre-emulsion and 470g of deionized water, start stirring and heat to 78°C, then add 21g of the initiator aqueous solution, and react at a constant temperature for 15min to obtain the seed emulsion.

[0128] (4) Adjust and control the temperature inside the reaction flask at 82°C, and use a double-dropping funnel to simultaneously and uniformly add the remaining pre-emulsion and the remaining initiator aqueous solution for 180 min.

[0129] (5) After the addition is complete, heat the system to 86°C and keep it at that temperature for 60 min.

[0130] The system was then cooled to 35°C, and the pH was adjusted to 7.8 using 25.0 wt% ammonia solution. The mixture was then filtered through a 200-mesh filter to obtain the customized high-quality product. Acrylic ester copolymer emulsion (its theoretical glass transition temperature is approximately 30.2℃).

[0131] Example 1:

[0132] This embodiment provides an environmentally friendly artistic coating with formaldehyde removal and antibacterial functions, and its preparation method, including the following steps:

[0133] (1) Add 275g of deionized water, 5g of dispersant and 2g of defoamer into the mixing tank, turn on the high-speed disperser, adjust the linear speed of the dispersing disc to 3m / s and stir for 5min.

[0134] Subsequently, 150g of rutile titanium dioxide, 211g of heavy calcium carbonate, and 10g of micron-sized zinc borate were added sequentially and at a uniform rate. After the addition was complete, the linear speed of the disperser was increased to 20m / s, and high-shear dispersion was carried out for 30 minutes. The fineness of the slurry was then measured to be ≤40μm.

[0135] (2) Rapidly reduce the linear speed of the disperser and maintain it at 3 m / s. Slowly add 250 g of the customized high-millimeter-based concentrate synthesized in Preparation Example 1 to the mixing tank. Acrylic copolymer emulsion, stirred at low speed for 10 minutes.

[0136] Subsequently, 10g of polyethylene glycol 400 was added to the system at a uniform rate, and the mixture was stirred continuously for 15 minutes while maintaining the low shear rate.

[0137] (3) While stirring at 3 m / s, add 1 g of 2-amino-2-methyl-1-propanol and use an online pH meter to monitor in real time to precisely adjust and lock the pH value of the system at 8.5.

[0138] Dissolve 1g of sodium gluconate completely in 25g of deionized water to prepare a homogeneous aqueous solution. Then slowly add the solution dropwise into the container. After the addition is complete, maintain low-speed stirring for 20 minutes.

[0139] (4) Dissolve 5g of dicyandiamide completely in another 50g of deionized water, and keep the water bath temperature at 40℃ to ensure that a completely transparent true solution is formed.

[0140] The obtained transparent dicyandiamide solution was slowly added dropwise to the above coating mixture. During the entire addition process and after the addition was completed, the mixture was stirred at a linear speed of 3 m / s for 15 min.

[0141] (5) Add 5g of thickener slowly while stirring at 3m / s, continuously monitor the Stormer viscosity of the system, continue stirring for 10 minutes and then stop the machine. Filter and purify the product through a 100-mesh filter bag and fill it to obtain the finished product.

[0142] Example 2:

[0143] This embodiment provides an environmentally friendly artistic coating with formaldehyde removal and antibacterial functions, and its preparation method, including the following steps:

[0144] (1) Add 198g of deionized water, 8g of dispersant and 3g of defoamer into the mixing tank, turn on the high-speed disperser, adjust the linear speed of the dispersing disc to 4m / s and stir for 5min.

[0145] Subsequently, 120g of rutile titanium dioxide, 198g of heavy calcium carbonate, and 15g of micron-sized zinc borate were added sequentially and at a uniform rate. After the addition was complete, the linear speed of the disperser was increased to 22m / s, and high-shear dispersion was carried out for 40 minutes. The fineness of the slurry was then measured to be ≤40μm.

[0146] (2) Rapidly reduce the linear speed of the disperser and maintain it at 4 m / s. Slowly add 300 g of the customized high-millimeter-based product synthesized in Preparation Example 2 to the mixing tank. Acrylic copolymer emulsion, stirred at low speed for 12 minutes.

[0147] Subsequently, 15g of polyethylene glycol 400 was added to the system at a uniform rate, and the mixture was stirred continuously for 18 minutes while maintaining the low shear rate.

[0148] (3) While stirring at 4 m / s, add 2 g of 2-amino-2-methyl-1-propanol and use an online pH meter to monitor in real time to precisely adjust and lock the pH value of the system at 8.8.

[0149] Dissolve 2g of sodium gluconate completely in 22g of deionized water to prepare a homogeneous aqueous solution. Then slowly add the solution dropwise into the container. After the addition is complete, maintain low-speed stirring for 25 minutes.

[0150] (4) Dissolve 10g of dicyandiamide completely in 100g of deionized water, and maintain the water bath temperature at 42℃ to ensure the formation of a completely transparent true solution. Slowly add the obtained transparent dicyandiamide solution dropwise to the above coating mixture. During and after the dropwise addition, maintain a linear velocity of 4m / s and stir for 18min.

[0151] (5) Add 7g of thickener slowly while stirring at 4m / s, continuously monitor the Stormer viscosity of the system, continue stirring for 10min and then stop the machine. Filter and purify through a 100-mesh filter bag, and then fill to obtain the finished product.

[0152] Example 3:

[0153] This embodiment provides an environmentally friendly artistic coating with formaldehyde removal and antibacterial functions, and its preparation method, including the following steps:

[0154] (1) Add 130g of deionized water, 10g of dispersant and 4g of defoamer into the mixing tank, turn on the high-speed disperser, adjust the linear speed of the dispersing disc to 5m / s and stir for 5min.

[0155] Subsequently, 100g of rutile titanium dioxide, 160g of heavy calcium carbonate, and 25g of micron-sized zinc borate were added sequentially and at a uniform rate.

[0156] After feeding is complete, increase the linear speed of the disperser to 25m / s and continue high-shear dispersion for 45min. The fineness of the slurry is then tested to be ≤40μm.

[0157] (2) Rapidly reduce the linear speed of the disperser and maintain it at 5 m / s.

[0158] Slowly add 350g of the customized high-molecular-weight compound synthesized in Preparation Example 3 to the mixing tank. Acrylic copolymer emulsion, stirred at low speed for 15 minutes.

[0159] Subsequently, 20g of polyethylene glycol 400 was added to the system at a uniform rate, and the mixture was stirred continuously for 20 minutes while maintaining this low shear rate.

[0160] (3) While stirring at 5 m / s, add 3 g of 2-amino-2-methyl-1-propanol and use an online pH meter to monitor in real time to precisely adjust and lock the pH value of the system at 9.0.

[0161] Dissolve 3g of sodium gluconate completely in 20g of deionized water to prepare a homogeneous aqueous solution. Then slowly add the solution dropwise into the container. After the addition is complete, maintain low-speed stirring for 30 minutes.

[0162] (4) Dissolve 15g of dicyandiamide completely in 150g of deionized water, and maintain the water bath temperature at 45℃ to ensure the formation of a completely transparent true solution. Slowly add the obtained transparent dicyandiamide solution dropwise to the above coating mixture. During the entire dropwise addition process and after the addition is completed, maintain a linear velocity of 5m / s and stir for 20min.

[0163] (5) Add 10g of thickener slowly while stirring at 5m / s, continuously monitor the Stormer viscosity of the system, continue stirring for 10min and then stop the machine. Filter and purify the product through a 100-mesh filter bag and fill it to obtain the finished product.

[0164] Example 4:

[0165] This embodiment provides an environmentally friendly artistic coating with formaldehyde removal and antibacterial functions, and its preparation method, including the following steps:

[0166] (1) Add 198g of deionized water, 8g of dispersant and 3g of defoamer into the mixing tank, turn on the high-speed disperser, adjust the linear speed of the dispersing disc to 3m / s and stir for 5min.

[0167] Subsequently, 120g of rutile titanium dioxide, 198g of heavy calcium carbonate, and 15g of micron-sized zinc borate were added sequentially and at a uniform rate.

[0168] After feeding is complete, increase the linear speed of the disperser to 25m / s and continue high-shear dispersion for 30 minutes. The fineness of the slurry is then tested to be ≤40μm.

[0169] (2) Rapidly reduce the linear speed of the disperser and maintain it at 3 m / s.

[0170] Slowly add 300g of the customized high-molecular-weight compound synthesized in Preparation Example 2 to the mixing tank. The acrylate copolymer emulsion was stirred at low speed for 10 minutes. Then, 15g of polyethylene glycol 400 was added to the system at a uniform rate, and the mixture was stirred continuously at this low shear rate for 15 minutes.

[0171] (3) While stirring at 3 m / s, add 2 g of 2-amino-2-methyl-1-propanol and use an online pH meter to monitor in real time to precisely adjust and lock the pH value of the system at 8.5.

[0172] Dissolve 2g of sodium gluconate completely in 22g of deionized water to prepare a homogeneous aqueous solution. Then slowly add the solution dropwise into the container. After the addition is complete, maintain low-speed stirring for 20 minutes.

[0173] (4) Dissolve 10g of dicyandiamide completely in another 100g of deionized water, and keep the water bath temperature at 42℃ to ensure that a completely transparent true solution is formed.

[0174] The obtained transparent dicyandiamide solution was slowly added dropwise to the above coating mixture. During the entire addition process and after the addition was completed, the mixture was stirred at a linear speed of 3 m / s for 15 min.

[0175] (5) Add 7g of thickener slowly while stirring at 3m / s, continuously monitor the Stormer viscosity of the system, continue stirring for 10 minutes and then stop the machine. Filter and purify the product through a 100-mesh filter bag and fill it to obtain the finished product.

[0176] Comparative Example 1:

[0177] The difference compared to Example 2 is that sodium gluconate was not added to the formulation, and the missing mass was made up by an equal mass of deionized water.

[0178] Comparative Example 2:

[0179] The difference compared to Example 2 is that polyethylene glycol 400 was not added to the formulation, and the missing mass was made up by an equal mass of deionized water.

[0180] Comparative Example 3:

[0181] Compared with Example 2, the difference is that: all components and their amounts remain unchanged, only the feeding sequence of micron-sized zinc borate, sodium gluconate and dicyandiamide is changed. In the high shear dispersion stage of step (1), micron-sized zinc borate, sodium gluconate and dicyandiamide are added at the same time, and are not added again in subsequent steps.

[0182] In the original Example 2, the 22g and 100g of deionized water used to dissolve sodium gluconate and dicyandiamide, respectively, were still included in the formula by the same mass and added in the form of deionized water in the corresponding subsequent steps. All other operating conditions were the same as in Example 2.

[0183] Comparative Example 4:

[0184] Compared with Example 2, the difference is that 2-amino-2-methyl-1-propanol was not added in step (3), and the pH value of the system was not precisely adjusted and the weak alkalinity was locked.

[0185] Comparative Example 5:

[0186] Compared with Example 2, the difference is that in step (4), 10g of dicyandiamide is replaced with 10g of adipic acid dihydrazide to compare the effect of different formaldehyde scavengers on the system performance under the same mass addition conditions.

[0187] Comparative Example 6:

[0188] The difference from Example 2 is that the customized high-quality synthesized in the preparation example was not used in step (2). Instead of using acrylate copolymer emulsions, it replaces them by an equal mass with ordinary low-... ( Commercially available acrylic copolymer emulsion (approximately 10°C).

[0189] Test Example 1:

[0190] (1) The finished coatings prepared in Example 2 and Comparative Example 2 were selected as experimental objects. They were uniformly coated on polytetrafluoroethylene plates using a wire bar coater, and the thickness of the wet film was controlled to be 200 μm.

[0191] (2) The coated sample was placed in a constant temperature and humidity chamber and surface dried for 7 days at 25°C and 50% relative humidity. Then the coating was peeled off from the polytetrafluoroethylene plate and transferred into a vacuum drying oven. It was continuously vacuum dried at 40°C for 48 hours to remove the residual liquid free water inside the coating and obtain the dry film test sample.

[0192] (3) The dry film sample was subjected to AC impedance spectroscopy using an electrochemical workstation. The dry film was cut and clamped between two polished stainless steel plate electrodes. An AC sinusoidal voltage amplitude was set to 10mV and the scanning frequency range was set to 10^5Hz to 10^-2Hz.

[0193] Collect the real and imaginary parts of the impedance to determine the bulk resistivity of the dry film. And measure the actual thickness of each dry film sample. and the effective contact area between the electrode and the sample ,according to Calculate the ionic conductivity of the dry film, where It is the ionic conductivity. This represents the actual thickness of the dry film. The volume resistivity is determined by the AC impedance spectrum. For effective contact area.

[0194] (4) Fourier transform infrared spectrometer with attenuated total reflection accessory is used to perform in-situ non-destructive testing on the surface chemical structure and functional group characteristics of dry film sample.

[0195] The spectral scanning range was set to 4000 cm⁻¹ to 400 cm⁻¹, and the resolution was set to 4 cm⁻¹. The position parameters of the characteristic absorption peaks of aliphatic ether bonds were extracted and recorded.

[0196] Meanwhile, pure polyethylene glycol 400 liquid was used as a reference sample for infrared spectral scanning under the same conditions.

[0197] Table 1 shows the electrochemical impedance and infrared spectral test data of the coatings in Example 2 and Comparative Example 2.

[0198] Test object AC impedance high-frequency intercept (Ω) Dry film ionic conductivity (S / cm) Wavenumber (cm⁻¹) of characteristic absorption peak of ether oxygen bond (COC) Example 2 Dry Film 3.12×10^6 2.84×10^-7 1089.4 Comparative Example 2: Dry Film 5.86×10^10 1.17×10^-11 No corresponding absorption peak was detected. Pure polyethylene glycol 400 - - 1112.7

[0199] According to Table 1 and Figure 1 According to the data, after the dry film sample of Example 2 was vacuum dried at 40°C for 48 hours, significantly reducing the residual free water content, its ionic conductivity remained on the order of 2.84 × 10^-7 S / cm.

[0200] As a control, the dry film system of Comparative Example 2, which eliminated the polyethylene glycol 400 component, had an ionic conductivity that dropped to 1.17 × 10^-11 S / cm, which is at the baseline level of conductivity of typical insulating polymer materials.

[0201] The conductivity difference between the two, spanning approximately four orders of magnitude, indicates that the ion conductivity of the dry film system is significantly reduced without the addition of polyethylene glycol 400, suggesting that the acrylate copolymer matrix itself is not conducive to the effective migration of ions.

[0202] In Example 2, the presence of polyethylene glycol 400 alters the physical state inside the dry film. Its introduction facilitates the formation of a highly polar local microenvironment within the polymer matrix and may enhance the migration ability of polar components and ions.

[0203] Further analysis using infrared spectroscopy data revealed that the characteristic COC aliphatic ether bond asymmetric stretching vibration absorption peak in pure polyethylene glycol 400 molecules is located at 1112.7 cm⁻¹.

[0204] When it was blended into the coating system of Example 2, the absorption peak underwent a significant red shift, with the center wavenumber shifting to 1089.4 cm⁻¹ towards lower frequencies.

[0205] The wavenumber shift reflects a change in the microchemical environment of the oxygen atom on the ether oxygen bond.

[0206] Under the above vacuum drying conditions, the influence of residual free water was significantly reduced. The red shift of the absorption peak suggests that the local chemical environment of the ether oxygen atoms in the polyethylene glycol segments has changed, which may be related to the ion-dipole interaction or coordination of Zn²⁺ in the system, as well as the interaction with other polar components.

[0207] The aforementioned interactions may alter the local electronic environment of the COC bond and change its effective vibrational constant, resulting in a shift of the characteristic absorption peak toward lower wavenumbers.

[0208] The combined results of the electrochemical and spectroscopic tests indicate that the introduction of polyethylene glycol 400 can significantly improve the ion conductivity of the dry film system, accompanied by changes in the local chemical environment of the ether oxygen groups. These results support the existence of a microscopic mass transfer environment inside the dry film that is conducive to the migration of polar components or ions, providing experimental evidence for subsequent formaldehyde-related reaction processes.

[0209] Test Example 2:

[0210] (1) The finished coatings prepared in Example 2 and Comparative Example 5 were selected as experimental objects. A coating with a wet film thickness of 200 μm was prepared on the glass substrate using a wire bar coater. The coating was placed in a constant temperature and humidity chamber with a temperature of 25℃ and a relative humidity of 50% for 7 days, and then dried naturally and the substrate was peeled off to obtain a dry film sample for testing.

[0211] (2) The dry film samples of Example 2 and Comparative Example 5 were respectively suspended and fixed in the center of a closed environment test chamber with a volume of 1 cubic meter. A quantitative concentration of formaldehyde solution was injected into the heating plate in the chamber using a micro-syringe to allow it to completely evaporate, and the initial concentration of free formaldehyde in the chamber was controlled to be close to 2.00 mg / m³.

[0212] Gas chromatography-mass spectrometry (GC-MS) was used to sample the formaldehyde concentration in a sealed chamber via a sampling tube at predetermined time points. The test lasted for 24 hours.

[0213] After the test, pure nitrogen gas with a purity of 99.999% was continuously purged into the chamber at a flow rate of 1.0 L / min for 2 hours. The gas discharged from the exhaust port during the purging period was collected and the formaldehyde release was measured by a formaldehyde analyzer. The measured results were converted into the secondary formaldehyde release under the specified nitrogen purging conditions.

[0214] (3) Liquid nitrogen was used to perform cryogenic pulverization on the original dry film of Example 2 before the formaldehyde absorption test and the dry film after absorbing formaldehyde in a sealed chamber for 24 hours, and the powder sample was obtained by passing it through a 200-mesh sieve.

[0215] The powder was loaded into a zirconia rotor and 13C cross-polarized magic angle rotating nuclear magnetic resonance was performed using a solid-state high-resolution nuclear magnetic resonance spectrometer.

[0216] The rotor magic angle rotation frequency was set to 10 kHz, the sampling time was 30 ms, and the ¹³C chemical shift data of the sample were recorded. The spectral signals and their changes corresponding to the nitrogen-containing carbon structures related to dicyandiamide in the range of 150 ppm to 175 ppm were extracted and compared.

[0217] Table 2 Formaldehyde consumption concentration curves and secondary release test data for Example 2 and Comparative Example 5

[0218] Sampling time point Example 2: Formaldehyde concentration in the cabin (mg / m³) Formaldehyde concentration in Comparative Example 5 (mg / m³) 0h 2.04 1.98 2h 1.41 1.53 4h 0.83 1.14 8h 0.34 0.87 12h 0.15 0.76 24h 0.05 0.73 Secondary release of nitrogen during purging 0.02 0.31

[0219] According to Table 2 and Figure 2 According to the data, the free formaldehyde concentration in the sealed chamber of Example 2 showed a smooth and continuous downward trend during the 24-hour test period, decreasing from the initial 2.04 mg / m³ to 0.05 mg / m³.

[0220] Under the nitrogen purging conditions described above, the amount of formaldehyde secondary release detected in Example 2 was 0.02 mg / m³.

[0221] The control group, Comparative Example 5, used adipic acid dihydrazide as a substitute component. Its free formaldehyde concentration showed a slowdown and plateau effect after decreasing to around 0.73 mg / m³, and a secondary release of up to 0.31 mg / m³ was detected in the subsequent nitrogen purging stage.

[0222] The difference between the two sets of data indicates that, compared with Comparative Example 5, the system of Example 2 has a more sustained formaldehyde consumption capacity and a lower level of secondary release after purging, suggesting that its formaldehyde binding process may have higher stability and may have a mechanism to inhibit reverse desorption.

[0223] Combination Figure 2(b) The solid-state nuclear magnetic resonance data shows that, before the dry film of Example 2 came into contact with formaldehyde, its ¹³C resonance spectrum showed a characteristic resonance signal at around 158.4 ppm, which can be attributed to the carbon atom signal of the nitrogen-containing carbon structure related to dicyandiamide.

[0224] After 24 hours of formaldehyde absorption reaction, the original signal intensity of 158.4 ppm decreased, and a new broadened resonance signal appeared in the lower magnetic field region of 162.7 ppm.

[0225] The shift of the chemical shift to a lower field indicates that the electronic environment of the relevant carbon atoms has changed, suggesting that the local chemical environment of the nitrogen-containing carbon structure related to dicyandiamide has changed after formaldehyde treatment.

[0226] Considering the possible nucleophilic addition reaction between dicyandiamide and formaldehyde, the above-mentioned peak changes are consistent with the speculation that the chemical environment of the dicyandiamide-related structure changes after the action of formaldehyde, and suggest that there may be an adjustment of the local coordination state in the system.

[0227] Based on the coexistence of sodium gluconate, dicyandiamide, and zinc ions in the system, it is speculated that the changes in the relevant nitrogen-containing structures after the formaldehyde reaction may further affect the local coordination equilibrium of Zn²⁺.

[0228] This change in coordination equilibrium may help reduce the tendency of formaldehyde addition products to undergo reverse dissociation, thereby promoting the system to maintain a continuous formaldehyde consumption capacity.

[0229] The above-mentioned solid-state NMR changes correspond to the macroscopic formaldehyde consumption and low secondary release results, providing supporting evidence for the proposed coordination environment change and reaction equilibrium regulation mechanism.

[0230] Test Example 3:

[0231] (1) The liquid finished coatings prepared in Examples 1 to 4, and Comparative Examples 1, 3 and 4 were selected as test objects.

[0232] Each group of samples was poured into a 500mL tin can, with the filling volume controlled to about 80% of the total volume. The cans were then sealed using a capping machine to ensure airtightness.

[0233] (2) At room temperature of 25°C, open the sealed container and use a Stormer viscometer to measure the initial viscosity of each sample. After the reading stabilizes, record the initial Stormer viscosity in KU.

[0234] The sample was then resealed.

[0235] (3) Place all sealed test samples in an electric heating constant temperature drying oven, set the temperature inside the oven to 50±1℃, and place them continuously for 30 days to simulate the accelerated thermal storage environment.

[0236] (4) After the set period is reached, take the sample out of the constant temperature chamber and let it stand in the room at 25°C for 24 hours to allow its temperature to return to room temperature.

[0237] After opening the can, stir the sample with a glass rod, observe and record the appearance of the sample, including whether there is stratification, flocculation, precipitation or demulsification and clumping.

[0238] (5) Use a Stormer viscometer to determine the final viscosity of each sample after heat storage using the same method as in step (2), and calculate the viscosity change rate before and after storage.

[0239] For samples that have lost fluidity or exhibit severe gelation, record their viscosity as exceeding the instrument's normal range limit.

[0240] Table 3. Test data of liquid-phase accelerated thermal storage in the examples and comparative examples.

[0241] Test object Initial viscosity (KU) Viscosity (KU) after 30 days of heat storage Viscosity change rate (%) Appearance after heat storage Example 1 98.2 100.5 +2.34 The material is uniform in consistency and free from lumps and flocculation. Example 2 101.4 103.1 +1.68 The material is uniform in consistency and free from lumps and flocculation. Example 3 104.7 107.6 +2.77 The material is uniform in consistency and free from lumps and flocculation. Example 4 102.3 105.8 +3.42 The material is uniform in consistency and free from lumps and flocculation. Comparative Example 1 99.7 >145.0 >+45.4 Severe gelation, large clumps Comparative Example 3 115.3 Unable to determine - The system demulsifies, and the aqueous phase separates from the resin phase. Comparative Example 4 98.5 134.2 +36.24 Obvious flocculent material was observed, resulting in extremely poor flowability.

[0242] According to Table 3 and Figure 3 According to the data, after 30 consecutive days of high-temperature accelerated thermal storage at 50°C, the increase in Stormer viscosity in Examples 1 to 4 was controlled within 4%, and the macroscopic appearance remained a uniform fluid state, indicating that the various active components in the system were in a stable suspended or dissolved coexisting state in the aqueous phase.

[0243] In Comparative Example 1, without the addition of sodium gluconate, the sample after heat storage lost its fluidity and showed large-area agglomeration, with the measured viscosity jumping to beyond the upper limit of the range.

[0244] The results indicate that the Zn²⁺ that may be released from micron-sized zinc borate in the aqueous phase lacks the corresponding complexing stabilizing effect after the absence of sodium gluconate containing multiple coordinating groups.

[0245] Under the above conditions, an increase in the concentration of free Zn²⁺ in the system may promote coordination between Zn²⁺ and nitrogen-containing groups in dicyandiamide molecules, and further disturb the colloidal stability balance between emulsion particles and other components, thereby causing flocculation, thickening or even gelation, which is macroscopically manifested as a significant increase in viscosity.

[0246] Comparative Example 3 adopted a one-time blending and feeding process, and its initial viscosity reached 115.3 KU. After heat storage, liquid phase stratification and demulsification occurred.

[0247] This indicates that in the absence of stepwise feeding and feeding sequence control, even if sodium gluconate is present in the formulation, the early direct contact of multiple active components during the high shear dispersion stage may still lead to strong coordination, adsorption, or interparticle interactions, thereby disrupting the colloidal stability of the emulsion system and ultimately resulting in increased viscosity and demulsification after heat storage.

[0248] In Comparative Example 4, without adjusting the pH of the system with 2-amino-2-methyl-1-propanol, the viscosity increased by 36.24%, and obvious flocculation was observed.

[0249] The results indicate that the thermal storage stability of the system is closely related to pH adjustment.

[0250] In the absence of appropriate pH adjustment, the coordination state between gluconate and Zn²⁺ and the colloidal stability of the emulsion system may change, thereby promoting flocculation and increasing viscosity.

[0251] The test results show that the addition of sodium gluconate, the timing of stepwise addition, and the pH adjustment of the system all have a positive effect on the thermal storage stability of the coating. The combination of the three helps to reduce the risk of flocculation, thickening, and demulsification caused by premature interaction of active components, thereby improving the liquid phase storage stability of the system. This indicates that the system in the example has good accelerated thermal storage stability and provides experimental basis for practical storage applications.

[0252] Test Example 4:

[0253] (1) The finished coatings prepared in Examples 1 to 4, as well as Comparative Examples 2 and 5, were selected as experimental subjects.

[0254] According to the requirements of the testing standard, each group of samples was uniformly coated onto the surface-treated calcium silicate board using the brush coating method. The coating amount was controlled at 120g / m². The samples were then placed in a standard curing room (temperature 25±1℃, relative humidity 50±5%) for 7 days to prepare the coating test sample.

[0255] (2) Place the prepared coating sample in an environmental test chamber with a volume of 1.5 cubic meters, and control the temperature inside the chamber to 25°C and the relative humidity to 50%. Inject free formaldehyde into the test chamber to make the initial formaldehyde concentration in the chamber reach 1.50 mg / m³.

[0256] The chamber was sealed for 24 hours, and the final formaldehyde concentration inside was recorded. The formaldehyde purification rate for a single stroke was then calculated.

[0257] (3) Without removing the coating sample, inject formaldehyde a second time into the same test chamber so that the initial concentration in the chamber reaches 1.50 mg / m³ again.

[0258] The formaldehyde purification rate of the second stroke was calculated after a 24-hour closed test.

[0259] Repeat this procedure to complete a total of 3 strokes of the formaldehyde continuous purification performance test.

[0260] (4) After the third stroke test is completed, stop injecting formaldehyde and purge the test chamber with pure nitrogen at a flow rate of 1.5 L / min for 4 hours.

[0261] A formaldehyde collection device was connected to the exhaust end, and the mass of formaldehyde collected during the specified 4-hour nitrogen purging period was determined by the phenol reagent spectrophotometric method. This value was divided by the chamber volume and recorded as the amount of secondary formaldehyde release from the sample under the specified purging conditions.

[0262] Table 4. Test data on the persistent formaldehyde purification rate and secondary release of the examples and comparative examples.

[0263] Test object Purification rate of the first stroke (%) Purification rate of the second stroke (%) Purification rate of the third stroke (%) Secondary release after purging (mg / m³) Example 1 88.6 86.4 85.1 0.03 Example 2 92.3 91.1 89.8 0.01 Example 3 94.1 92.7 91.5 0.02 Example 4 91.8 90.2 88.3 0.02 Comparative Example 2 81.7 53.4 30.6 0.07 Comparative Example 5 87.9 75.8 61.2 0.46

[0264] According to Table 4 and Figure 4 According to the data, after experiencing three consecutive high-concentration formaldehyde injection loads, the purification rate of the third stroke in Examples 1 to 4 remained at a high level of 85% to 92%, with minimal attenuation.

[0265] Meanwhile, the amount of secondary formaldehyde release detected under the specified pure nitrogen purging conditions did not exceed 0.03 mg / m³.

[0266] As a control, Comparative Example 2, which excluded the polyethylene glycol 400 component, still had an initial purification rate of 81.7%, but the data dropped sharply in the second and third strokes, with the third purification rate being only 30.6%.

[0267] The results suggest that, without the addition of polyethylene glycol 400, the migration of formaldehyde and related polar components inside the dry film is significantly restricted, making it difficult to fully utilize the captured components such as dicyandiamide inside the coating.

[0268] As the active sites on the surface that are more readily exposed to formaldehyde are gradually consumed, the system's subsequent formaldehyde purification capacity decreases significantly.

[0269] The introduction of polyethylene glycol 400 in the embodiment system can improve the internal polarity of the dry film and facilitate the migration of formaldehyde and related polar components inside the coating, thereby increasing the possibility of continuous utilization of the trapped components inside the coating.

[0270] On the other hand, in Comparative Example 5, when dicyandiamide was replaced with adipic acid dihydrazide, the multi-stroke purification rate also gradually decreased. The more critical difference was that the nitrogen purging stage in the later stage of the test produced a secondary release of formaldehyde as high as 0.46 mg / m³.

[0271] The above results indicate that, under the conditions of equal mass addition used in this experiment, the adipic acid dihydrazide system exhibits a high level of secondary formaldehyde release, suggesting that the formaldehyde conjugate products formed may undergo a certain degree of reversible dissociation under the test conditions.

[0272] When the external formaldehyde concentration decreases and nitrogen purging is performed, some of the bound formaldehyde may be released again, resulting in a higher amount of secondary release after purging.

[0273] In contrast, the system in the example exhibited a lower amount of secondary release after purging. Combined with the aforementioned solid-state NMR and impedance test results, this supports the possibility that the local chemical environment and coordination state of formaldehyde in the system changed after the reaction, which may be beneficial to improving the stability of the formaldehyde binding product.

[0274] Test Example 5:

[0275] (1) The finished coatings prepared in Examples 1 to 4 and Comparative Example 2 were selected as experimental subjects.

[0276] Each group of samples was uniformly coated on a flat glass substrate, with the wet film thickness controlled at 150 μm. The samples were then naturally dried for 7 days at 25°C and 50% relative humidity, and then cut into test pieces with a size of 50 mm × 50 mm.

[0277] (2) Two independent closed environment pretreatment chambers are set up.

[0278] Clean air filtered by activated carbon is introduced into Environmental Chamber A;

[0279] Formaldehyde mixture was continuously introduced into Environment B, and the free formaldehyde concentration in the chamber was kept constant at 2.50 mg / m³.

[0280] Each set of samples was divided into two parts and placed in chamber A and chamber B respectively, and pretreated for 7 days at 25°C and 50% relative humidity.

[0281] (3) Take out the pretreated sample and test its antibacterial properties according to the relevant test standards.

[0282] The test bacteria selected were Escherichia coli (Gram-negative bacteria) and Staphylococcus aureus (Gram-positive bacteria).

[0283] (4) Prepare bacterial suspensions with concentrations ranging from 1.0×10^5 CFU / mL to 5.0×10^5 CFU / mL.

[0284] A quantitative bacterial suspension is dropped onto the surface of the test sample, covered with a sterilized polyethylene film and pressed flat to remove air bubbles, ensuring uniform contact between the bacterial suspension and the sample surface.

[0285] The sample was placed in a constant temperature and humidity incubator at 37℃ and relative humidity greater than 90% for 24 hours.

[0286] (5) Remove the polyethylene film, rinse the sample and film surface repeatedly with neutralizing eluent, collect the eluent and perform gradient dilution.

[0287] The diluted solution was inoculated onto nutrient agar medium using the plate spread method, and the number of viable colonies was counted after incubation at 37°C for 48 hours.

[0288] The antibacterial rate was calculated by comparing the data with the blank control group that had not undergone antibacterial treatment.

[0289] Table 5. Antibacterial rate test data of the examples and comparative examples after pretreatment in different environments.

[0290] Test object E. coli antibacterial rate (%) after treatment in Chamber A (formaldehyde-free) E. coli antibacterial rate (%) after treatment in Chamber B (containing formaldehyde) Staphylococcus aureus antibacterial rate (%) after treatment in Chamber A (formaldehyde-free) Staphylococcus aureus antibacterial rate (%) after treatment in Chamber B (containing formaldehyde) Example 1 75.8 96.1 77.3 97.4 Example 2 78.4 97.6 81.2 98.9 Example 3 82.1 98.5 83.6 99.1 Example 4 79.5 96.8 80.7 98.2 Comparative Example 2 35.8 37.1 38.4 39.5

[0291] According to Table 5 and Figure 5 According to the data, after pretreatment in Chamber A (formaldehyde-free environment), the antibacterial rate of the surface against Escherichia coli and Staphylococcus aureus in Examples 1 to 4 was in the basic range of 75.8% to 83.6%.

[0292] This fundamental antibacterial property originates from the extremely small amount of background dissociation on the surface of micron-sized zinc borate under a weakly alkaline environment.

[0293] However, when the same coated samples were pretreated in Chamber B (a high-concentration formaldehyde environment), their antibacterial rates against both test strains increased dramatically, reaching a highly efficient sterilization level of 96.1% to 99.1%.

[0294] The above data shows that the coating of the example after formaldehyde pretreatment exhibits a significantly improved antibacterial rate, indicating a clear correlation between the formaldehyde pretreatment process and the change in the antibacterial performance of the coating.

[0295] However, since formaldehyde itself has antibacterial properties, the potential impact of residual or adsorbed formaldehyde in the sample on the test results still needs to be distinguished by further control experiments.

[0296] Based on the aforementioned test results, it is speculated that after formaldehyde enters the coating and reacts with dicyandiamide, it may alter the local coordination equilibrium between nitrogen-containing components and Zn²⁺ in the system.

[0297] The aforementioned changes in coordination state may further affect the dynamic equilibrium between gluconate, Zn²⁺, and micron-sized zinc borate;

[0298] Meanwhile, the polar microenvironment formed by polyethylene glycol 400 is conducive to the migration of related polar components.

[0299] Therefore, after formaldehyde pretreatment, the zinc-related species and borate-related species that can participate in antibacterial activity on the coating surface may change, thus exhibiting an increased antibacterial rate.

[0300] In contrast, Comparative Example 2, which did not add polyethylene glycol 400, maintained an overall antibacterial rate of 35.8% to 39.5% in both formaldehyde-free Chamber A and Chamber B containing a high concentration of formaldehyde. The change in antibacterial rate before and after formaldehyde pretreatment was small, and it did not show the significant improvement seen in Examples 1 to 4.

[0301] The comparative data suggests that, without the addition of polyethylene glycol 400, the migration ability of polar components within the coating film is significantly reduced.

[0302] In this case, the diffusion of formaldehyde into the coating interior and further interactions between related polar components may be limited.

[0303] Therefore, further interaction between gluconate and zinc borate particles may be inhibited, thereby weakening the improvement in antibacterial properties after formaldehyde pretreatment.

[0304] The results of this comparison show that polyethylene glycol 400 plays an important role in improving the antibacterial properties after formaldehyde pretreatment, which is consistent with the aforementioned mechanism hypothesis of "formaldehyde inducing local coordination balance changes and promoting the migration of related active species". This suggests that there may be a synergistic effect among the components, rather than a simple functional additive effect.

[0305] Test Example 6:

[0306] (1) The finished coatings prepared in Examples 1 to 4 and Comparative Example 6 were selected as experimental subjects.

[0307] Coating samples were prepared in accordance with the relevant requirements of GB / T9755-2024 "Synthetic Resin Emulsion Wall Coatings" and the washability was tested in accordance with GB / T9266-2009 "Determination of Scrub Resistance of Architectural Coatings".

[0308] Coated samples were prepared on asbestos-free fiber cement boards that had undergone sanding and solvent cleaning.

[0309] Two coats were applied using a bar coater, with a 6-hour interval between each coat, to control the total dry film thickness to approximately 50 μm.

[0310] (2) Place the prepared coating sample horizontally in a constant temperature and humidity room and cure it continuously for 14 days under the conditions of ambient temperature of 25±1℃ and relative humidity of 50±5% to allow the polymer emulsion to dry fully and complete the film formation process.

[0311] (3) Fix the cured coating sample in the test tank of the scrub resistance tester.

[0312] Use a standard boar bristle brush and soak it in 20°C water for 30 minutes before use to restore the softness of the bristles.

[0313] (4) Inject a 0.5% concentration of laundry detergent aqueous solution into the test tank as a washing medium, and keep the washing medium continuously wetting the coating surface during the test.

[0314] Start the scrub resistance tester and control the brush to perform reciprocating scrubbing motions on the coating surface at a frequency of 37 times / minute.

[0315] (5) Observe the wear condition of the coating surface. When continuous longitudinal damage appears in the middle 10cm area of ​​the coating and the cement board substrate is exposed, stop the instrument operation.

[0316] Record the number of washing cycles at this time as the washability index of the test sample.

[0317] Table 6 shows the test data of the washability of the coatings in the examples and comparative examples.

[0318] Test object Maintenance time (days) Coating state Washability (number of wash cycles) Example 1 14 Even and flat 8642 Example 2 14 Even and flat 10523 Example 3 14 Even and flat 9817 Example 4 14 Even and flat 9256 Comparative Example 6 14 The surface has a slightly sticky feel. 1214

[0319] According to Table 6 and Figure 6 According to the data, the coating samples of Examples 1 to 4 under the above-mentioned scrub resistance test conditions had a cycle count of 8642 to 10523, indicating that the coatings of each example have good scrub resistance.

[0320] In contrast, replacing the film-forming resin with a conventional resin with a low glass transition temperature ( Comparative Example 6, using an acrylic emulsion at approximately 10°C, under the same curing conditions and test medium, showed early dissolution and wear of the coating, exposing the substrate after only 1214 wash cycles.

[0321] This set of data shows that, under the two emulsion systems and the same formulation conditions used in this experiment, the composition and film-forming characteristics of the base emulsion significantly affect the scrub resistance of the polyethylene glycol 400-containing coating.

[0322] In the formulation system, polyethylene glycol 400 was introduced as a key component to enhance the local polarity inside the dry film and promote the migration of related polar components and ions.

[0323] Polyethylene glycol 400, as a low molecular weight polymer, can remain in the acrylate copolymer matrix during the coating film formation process and form a certain degree of physical mixing with the polymer chain segments.

[0324] From the perspective of polymer physics, the introduction of polyethylene glycol 400 may increase the mobility of polymer chain segments and produce a certain plasticizing effect on the matrix.

[0325] Comparative Example 6 uses conventional low When commercially available emulsions are used as a base, the coating film exhibits slight stickiness and a significant reduction in the number of wash cycles in the presence of polyethylene glycol 400.

[0326] The result suggests that the lower Combining emulsion with polyethylene glycol 400 may increase the overall softening of the coating film, which is detrimental to its scrub resistance.

[0327] Custom high-performance graphics used in the embodiments Acrylic copolymer emulsions offer corresponding materials science solutions.

[0328] Compared with the low used in Comparative Example 6 Compared to commercially available emulsions, the custom-made acrylate copolymer emulsion used in the examples has higher theoretical values. Therefore, under the same temperature conditions, the movement of its polymer chain segments is relatively more restricted, and the matrix has relatively high rigidity.

[0329] The plasticizing effect of polyethylene glycol 400 can adjust the rigidity to a certain extent, thus helping to balance film-forming properties and coating mechanical properties.

[0330] As can be seen from the coating state and washability results recorded in Table 6, the coatings of Examples 1 to 4 all remained uniform and smooth, with no obvious film-forming defects observed, and maintained high washability.

[0331] The above physical performance test results indicate that a proper match needs to be made between the film-forming characteristics of the base emulsion and the introduction of polyethylene glycol 400.

[0332] Using higher theory Customized acrylic copolymer emulsions are beneficial for maintaining good mechanical durability of the coating while preserving the polar mass transfer characteristics of the system.

[0333] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. An environmentally friendly artistic paint with formaldehyde removal and antibacterial functions, characterized in that, Is made from raw materials comprising the following parts by weight: Custom high acrylate copolymer emulsion 250-350 parts; Polyethylene glycol 400 10~20 parts; Micron-sized zinc borate 10~25 parts; Sodium gluconate 1~3 parts; Dicyandiamide 5~15 parts; 2-amino-2-methyl-1-propanol 1~3 parts; Rutile titanium dioxide 100~150 parts; Heavy calcium carbonate 160~211 parts; Dispersant 5~10 parts; Defoaming agent 2~4 parts; Thickening agent 5~10 parts; Deionized water 300~350 parts; wherein the polyethylene glycol 400 is dispersed in the custom high The polar micro-environment is formed in the acrylic ester copolymer emulsion matrix, and the micron-sized zinc borate, sodium gluconate and dicyandiamide form a local coordination state in the system.

2. The environment-friendly artistic paint with formaldehyde removal and antibacterial functions according to claim 1, characterized in that, Is made from raw materials comprising the following parts by weight: Custom high Acrylate copolymer emulsion 300 parts, polyethylene glycol 400 15 parts, micron-sized zinc borate 15 parts, sodium gluconate 2 parts, dicyandiamide 10 parts, 2-amino-2-methyl-1-propanol 2 parts, rutile titanium dioxide 120 parts, heavy calcium carbonate 198 parts, dispersant 8 parts, defoamer 3 parts, thickener 7 parts, deionized water 320 parts. 3.The environment-friendly artistic paint with the functions of removing formaldehyde and antibiosis according to claim 1, characterized in that, The micron-sized zinc borate has a chemical formula of and a powder median diameter D50 of 5.0 μm to 10.0 μm. The average molecular weight of the polyethylene glycol 400 is 380 g / mol~420 g / mol. 4.The environment-friendly artistic paint with the functions of removing formaldehyde and antibiosis according to claim 1 or 2, characterized in that, The customized high The acrylate copolymer emulsion is prepared from copolymerization raw materials comprising the following parts by weight: Methyl methacrylate 615-640 parts, butyl acrylate 345-370 parts, methacrylic acid 15 parts; the customized high The theoretical glass transition temperature of the acrylate copolymer emulsion is 25.8-30.2℃. 5.The environment-friendly artistic paint with the functions of removing formaldehyde and antibiosis according to claim 4, characterized in that, The customized high A process for preparing an acrylate copolymer emulsion includes the steps of: (1) The methyl methacrylate, butyl acrylate and methacrylic acid are mixed to obtain total monomers; the sodium dodecyl ether sulfate, isomeric alcohol polyoxyethylene ether and part of the deionized water are uniformly mixed, and then the total monomers are added and stirred to prepare a pre-emulsion; (2) Ammonium persulfate is dissolved in deionized water to prepare an initiator aqueous solution; (3) Part of the pre-emulsion and deionized water are added to a reaction bottle, heated to 78℃, and part of the initiator aqueous solution is added, and a seed emulsion is prepared by constant temperature reaction; (4) The temperature in the reaction bottle is controlled at 82℃, and the remaining pre-emulsion and initiator aqueous solution are added at a constant speed; (5) After the addition is completed, the temperature is raised to 86℃ for reaction, and then the temperature is lowered to 35℃, the pH of the system is adjusted to 7.8 using ammonia water, and filtration is performed to obtain the product.

6. The preparation method of the environment-friendly artistic paint with formaldehyde removal and antibacterial functions according to any one of claims 1-5, characterized in that, Comprise the following steps: S1, part of the deionized water, dispersant and defoaming agent are mixed, and then rutile titanium dioxide, heavy calcium carbonate and micron-sized zinc borate are sequentially added and subjected to high-shear dispersion to prepare a base slurry; S2, reduce the shear rotation speed, add custom high The acrylic ester copolymer emulsion is stirred at low speed, and then polyethylene glycol 400 is added while continuing to stir at low speed. S3, 2-amino-2-methyl-1-propanol is added under low-speed stirring, the pH of the system is adjusted to 8.5~9.0, and then sodium gluconate is dissolved in deionized water to prepare an aqueous solution which is added dropwise to the system while maintaining low-speed stirring; S4, dicyandiamide is dissolved in deionized water to prepare a transparent solution which is added dropwise to the system while maintaining low-speed stirring; S5, a thickening agent is added, and after uniform stirring, the product is obtained by filtration.

7. The preparation method according to claim 6, characterized in that, In the S1 step, the linear speed of the dispersing disc for high-shear dispersion is 20 m / s~25 m / s, and the dispersion time is 30 min~45 min, so as to control the fineness of the prepared base slurry to be ≤40 μm.

8. The preparation method according to claim 6, characterized in that, In the S4 step, the pretreatment operation of dicyandiamide is as follows: dicyandiamide is added to deionized water, and after being dissolved to form a transparent solution under water bath temperature control at 40℃~45℃, it is then added dropwise.

9. The preparation method according to claim 6, characterized in that, In the S2 to S5 steps, the linear speed of the dispersing disc for low-speed stirring is 3 m / s~5 m / s.

10. The method of claim 6, wherein, In the S3 step, after the addition of the sodium gluconate aqueous solution is completed, low-speed stirring is maintained for 20 min~30 min; In the S4 step, low-speed stirring is maintained for 15 min~20 min after the addition of the dicyandiamide solution is completed.