Silicon-free double-layer fluorocarbon optical release film, method and components

By using a silicon-free double-layer fluorocarbon optical release film structure, the problems of silicon migration contamination in silicone release films and insufficient adhesion of fluoropolymer release film coatings are solved, achieving a balance between coating stability and optical performance at high temperatures, making it suitable for high-end flexible displays and foldable modules.

CN123107570APending Publication Date: 2026-11-17ZHEJIANG RIJIU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611262858.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicone release films suffer from silicon migration contamination at high temperatures, leading to a decrease in residual adhesion of thermosetting OCA adhesive films. Fluorine release film coatings also exhibit insufficient adhesion and poor interface stability, making it difficult to meet the reliability requirements of high-end flexible displays and foldable modules.

Method used

The film employs a silicon-free double-layer fluorocarbon optical release film structure, comprising a PET substrate layer, a corona-modified layer, an anchoring layer, and a release layer. It is formed through high-voltage corona discharge and cross-linking curing. Both the anchoring layer and the release layer are perfluorocarbon systems. The corona-modified layer enhances interfacial adhesion, and the anchoring layer and the release layer form a dense cross-linked network to ensure stable bonding between the coating and the substrate.

Benefits of technology

It achieves silicon-free contamination, low and stable release force, coating does not peel off or damage the adhesive layer, has excellent high temperature resistance, is suitable for long-term service stability of high-end display devices, and meets the production process requirements of optical display materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107570A_ABST
    Figure CN123107570A_ABST
Patent Text Reader

Abstract

This invention discloses a silicon-free double-layer fluorocarbon optical release film, method, and components. The release film comprises, from bottom to top: a PET substrate layer with a thickness of 25-100 μm; a corona-modified layer formed on the surface of the PET substrate layer by high-voltage corona discharge, with a modification depth of 5-20 nm; and an anchoring layer disposed on the surface of the corona-modified layer, formed by cross-linking and curing an anchoring layer coating solution, with a dry film thickness of 25-100 nm. The anchoring layer coating solution comprises, by weight, 1.2 ~2.4 parts of hydroxyl-terminated perfluorocarbon resin, 0.12~0.3 parts of polyisocyanate crosslinking agent, and the balance being a first solvent; a release layer, disposed on the surface of the anchoring layer, formed by thermally initiated free radical crosslinking and curing of the release layer coating liquid, with a dry film thickness of 25~100 nm. The release layer coating liquid comprises, by 100 parts by weight, 0.5~1.2 parts of perfluoroalkyl ether modified perfluoroacrylate copolymer, 0.03~0.08 parts of thermally decomposable free radical initiator, and the balance being a second solvent. This invention exhibits low release force, good stability, excellent temperature resistance, and superior optical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of adhesive film technology, specifically relating to a silicone-free double-layer fluorocarbon optical release film, method, and components. Background Technology

[0002] In existing technologies, thermosetting OCA adhesive films such as folded OCA and curved OCA usually need to be used in conjunction with release films during the bonding, hot pressing and subsequent curing processes to achieve isolation protection and easy peeling.

[0003] Currently, the release films commonly used in the industry are mainly divided into two categories: silicone release films and fluorinated release films. Both can meet the basic release requirements in conventional processes, but they have the following obvious application limitations in high-reliability scenarios such as high-end flexible displays and foldable modules:

[0004] 1. Silicone release films use polysiloxane as the core release functional component. During hot pressing (80~120℃) and high-temperature post-curing (130~180℃), incompletely cross-linked small-molecule cyclosiloxanes in the film layer are prone to migration, which can then penetrate to the OCA adhesive film interface and form silicon contamination. Related studies have confirmed that trace amounts of silicon contamination (<1ng / cm²) can significantly reduce the residual adhesion of the OCA adhesive film, lowering its residual adhesion rate to below 80%, thereby causing reliability problems such as adhesive failure, interface delamination, bubbles, and warping, making it difficult to meet the stability requirements of long-term service of high-end display devices.

[0005] 2. While fluoropolymer release films can fundamentally avoid silicon migration contamination, their extremely low fluoropolymer surface energy results in poor interfacial compatibility with conventional PET substrates. The coating adheres solely through physical adsorption, lacking stable chemical bonding and mechanical interlocking, leading to insufficient coating adhesion. Under the high-temperature conditions of OCA film hot pressing and post-curing, localized fluoropolymer coating peeling, powdering, or detachment along with the OCA film is prone to occur. Furthermore, under long-term storage or temperature fluctuations, the interfacial stability between the coating and substrate continuously decreases, and the release force increases significantly with storage time and temperature, deviating from the stable low release force range. This causes uneven peeling force, film lifting during tearing, and adhesive layer damage, severely impacting the process yield and product reliability of folded and curved OCA.

[0006] Therefore, in order to address the above-mentioned technical problems, it is necessary to provide a silicon-free double-layer fluorocarbon optical release film, method, and component. Summary of the Invention

[0007] The purpose of this invention is to provide a silicon-free double-layer fluorocarbon optical release film, method, and components.

[0008] To achieve the above objectives, a specific embodiment of the present invention provides the following technical solution:

[0009] The silicon-free double-layer fluorocarbon optical release film, from bottom to top, includes:

[0010] PET substrate layer, film thickness is 25~100μm;

[0011] The corona-modified layer is formed on the surface of the PET substrate layer by high-voltage corona discharge, with a modification depth of 5~20nm;

[0012] An anchoring layer, disposed on the surface of the corona-modified layer, is formed by cross-linking and curing of the anchoring layer coating liquid, with a dry film thickness of 25~100nm. The anchoring layer coating liquid comprises, by weight, 1.2~2.4 parts of hydroxyl-terminated perfluorocarbon resin, 0.12~0.3 parts of polyisocyanate cross-linking agent and the balance being a first solvent.

[0013] The release layer, located on the surface of the anchoring layer, is formed by thermally initiated free radical cross-linking and curing of the release layer coating liquid. The dry film thickness is 25~100nm. The release layer coating liquid consists of 0.5~1.2 parts perfluoroalkyl ether modified perfluoroacrylate copolymer, 0.03~0.08 parts thermally decomposable free radical initiator, and the balance being a second solvent, per 100 parts by weight. Both the anchoring layer and the release layer are perfluorocarbon systems and do not contain organosilicon compounds.

[0014] In one or more embodiments of the present invention, the conditions for forming the corona-modified layer are: corona power 2kW.

[0015] In one or more embodiments of the present invention, the first solvent is selected from ethyl acetate, propylene glycol methyl ether acetate, and mixtures thereof. Preferably, the first solvent is a mixture of 67-69 parts ethyl acetate and 29.68-30.3 parts ethyl acetate.

[0016] In one or more embodiments of the present invention, the second solvent is selected from hydrofluoroethers.

[0017] In one or more embodiments of the present invention, the hydroxyl-terminated perfluorocarbon resin is selected from hydroxyl-terminated perfluoropolyether, hydroxyl-terminated perfluoroolefin copolymer, and hydroxyl-terminated perfluoropolyether modified fluorinated acrylate oligomer; and / or, the polyisocyanate crosslinking agent is selected from aliphatic polyisocyanate crosslinking agents, alicyclic polyisocyanate crosslinking agents, and blocked aliphatic polyisocyanate crosslinking agents.

[0018] In one or more embodiments of the present invention, the perfluoroalkyl ether modified perfluoroacrylate copolymer is selected from at least one of perfluoroacrylate copolymers containing perfluoropolyether side chains, perfluoroalkyl methacrylate and perfluoropolyether methacrylate copolymers, and perfluoropolyether and perfluoroalkyl acrylate copolymers with terminal olefin bonds; and / or, the thermally decomposable free radical initiator is selected from at least one of azobisisobutyronitrile, azobisisovalerate, and dicumyl peroxide.

[0019] In one or more embodiments of the present invention, a method for preparing a silicon-free double-layer fluorocarbon optical release film includes: the anchoring layer and the release layer are separately cured after coating.

[0020] In one or more embodiments of the present invention, the curing is carried out in stages at high temperature, and the specific stages are as follows: the high temperature curing for the anchoring layer is: zone 1 temperature 75~85℃, zone 2 temperature 115~125℃, zone 3 temperature 145~155℃, with a total baking time of 20~30s; and / or, the high temperature curing for the release layer is: zone 1 temperature 85~95℃, zone 2 temperature 125~135℃, zone 3 temperature 155~165℃, with a total baking time of 15~25s.

[0021] Compared with the prior art, the silicon-free double-layer fluorocarbon optical release film, method and components of the present invention solve the problem of high-temperature silicon migration contamination of organosilicon release films, which leads to the attenuation of residual adhesion and bonding failure of thermosetting OCA; secondly, it solves the problem of single-layer fluorine release films relying solely on physical adsorption, which easily leads to coating peeling and powdering at high temperatures; and thirdly, it solves the problem of poor interface stability of single-layer fluorine release films, which cause significant drift of release force under high and low temperature aging.

[0022] In summary, the present invention has the following advantages:

[0023] Silicon-free: Pure fluorocarbon system, without any added organosilicon components. XPS testing showed no detectable silicon on the surface, making it suitable for folded OCA and thermosetting OCA products that are highly sensitive to silicon contamination. Low and stable release force: Release force is controlled within the ultra-light release range of 2.7~4.95gf / 25mm (NITTO31B test tape). The peeling process does not pull or damage the OCA adhesive layer, and the long-term storage performance fluctuates little. Strong coating adhesion: Adopting a corona activation + double-layer fluorocarbon anchoring structure, the coating has excellent adhesion to the substrate and between layers, with no peeling or powdering under high-temperature processes. Excellent temperature resistance: It can withstand short-term high-temperature baking at 180℃, meeting the requirements of mainstream production processes such as OCA hot pressing and post-curing. Excellent optical performance: Both coatings are nanoscale ultra-thin structures, which will not cause an increase in haze or a decrease in light transmittance, fully complying with the standards for optical display materials. Attached Figure Description

[0024] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0025] Figure 1 This is a schematic diagram of the structure of a silicon-free double-layer fluorocarbon optical release film in one embodiment of the present invention.

[0026] Explanation of key figure labels:

[0027] 1-PET substrate layer; 2-Corona modified layer; 3-Anchoring layer; 4-Release layer. Detailed Implementation

[0028] To enable those skilled in the art to better understand the technical solutions in this disclosure, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments disclosed herein. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this disclosure.

[0029] The abbreviated codes of this invention are listed below:

[0030] OCA (Optically Clear Adhesive)

[0031] AR (Anti-Reflection);

[0032] AF (Anti-Fingerprint)

[0033] PET (Polyethylene Terephthalate).

[0034] PP (Polypropylene);

[0035] PE (Polyethylene);

[0036] XPS (X-ray Photoelectron Spectroscopy).

[0037] This invention provides a silicon-free double-layer fluorocarbon optical release film, comprising, from bottom to top:

[0038] PET substrate layer, film thickness is 25~100μm;

[0039] A corona-modified layer is formed on the surface of the PET substrate layer, with a modification depth of 5~20nm;

[0040] An anchoring layer, disposed on the surface of the corona-modified layer, is formed by cross-linking and curing of an anchoring layer coating liquid containing terminal hydroxyl perfluorocarbon resin, polyisocyanate cross-linking agent and first solvent, with a dry film thickness of 25~100nm.

[0041] Release layer, located on the surface of anchoring layer, is formed by thermally initiated free radical cross-linking and curing of release layer coating liquid containing perfluoroalkyl ether modified perfluoroacrylate copolymer, thermally decomposable free radical initiator and second solvent, with a dry film thickness of 25~100nm.

[0042] Both the anchoring layer and the release layer are perfluorocarbon systems and do not contain organosilicon compounds.

[0043] The PET substrate layer uses optical-grade PET film with a light transmittance of ≥90% and a haze of ≤1.0%.

[0044] The corona-modified layer is an interface layer formed by in-situ oxidation and activation modification of the PET substrate surface by high-voltage corona discharge. This interface layer contains polar functional groups of hydroxyl (–OH) and carboxyl (–COOH) grafted onto the PET molecular chain, and the surface may have a nanoscale micro-uneven structure.

[0045] In the aforementioned corona-modified layer, the polar functional groups can form hydrogen bonds with the active groups within the anchoring layer. Simultaneously, the nano-microscopic uneven structure enables mechanical interlocking between the anchoring layer and the PET substrate interface. Under the combined effect of these two factors, the interfacial adhesion between the coating and the PET substrate is significantly improved, effectively preventing coating peeling and suppressing abnormal drift of the release force. The modification depth of the corona-modified layer can be controlled by adjusting the high-voltage corona discharge power and processing speed, representing a conventional surface modification process in this field.

[0046] In the anchoring layer, the hydroxyl-terminated perfluorocarbon resin includes one of the following: hydroxyl-terminated perfluoropolyether, hydroxyl-terminated perfluoroolefin copolymer, and hydroxyl-terminated perfluoropolyether-modified fluorinated acrylate oligomer, preferably hydroxyl-terminated perfluoropolyether. For example, the hydroxyl-terminated perfluorocarbon resin can be selected from at least one of Synesqo Fluorolink D10-H, Fluorolink D4000, Wisbonya PFPE-OH-7100, and Fluorolink Alcohol-3000, more preferably Synesqo Fluorolink D10-H. It should be noted that there are currently no standardized commercially available finished products for hydroxyl-terminated perfluoroolefin copolymers and hydroxyl-terminated perfluoropolyether-modified fluorinated acrylate oligomers; they can be obtained through artificial synthesis, graft modification, or copolymerization, and can be readily prepared by those skilled in the art using existing fluorocarbon synthesis processes.

[0047] The polyisocyanate crosslinking agent is selected from one or more combinations of aliphatic polyisocyanate crosslinking agents, alicyclic polyisocyanate crosslinking agents, and blocked aliphatic polyisocyanate crosslinking agents, preferably hexamethylene diisocyanate trimer. For example, the polyisocyanate crosslinking agent may be selected from at least one of Covestro Desmodur N3300, Desmodur N3600, Wanhua Chemical WANNATE HT-100, Asahi Kasei Durnate TPA-100, and Tosoh Coronate HXR, more preferably Covestro Desmodur N3300.

[0048] Optionally, the anchoring layer is obtained by curing an anchoring layer coating solution formed by 1.2-2.4 parts of hydroxyl-terminated perfluorocarbon resin, 0.12-0.3 parts of polyisocyanate crosslinking agent, 67-69 parts of ethyl acetate, and 29.68-30.3 parts of propylene glycol methyl ether acetate, with the solid content of the anchoring layer coating solution being 1.32%-2.7%; in this case, the first solvent is obtained by compounding ethyl acetate and propylene glycol methyl ether acetate.

[0049] The main chain of the hydroxyl-terminated perfluorocarbon resin is a perfluorocarbon segment or a perfluoropolyether segment, with active hydroxyl groups at the molecular ends, which is used to improve the interlayer anchoring bond and the overall temperature resistance of the coating. The isocyanate group (–NCO) contained in the polyisocyanate crosslinking agent can undergo an addition reaction with the hydroxyl group (–OH) contained in the hydroxyl-terminated perfluorocarbon resin to generate urethane bonds (–NH–CO–O–), forming a dense three-dimensional crosslinked network structure, which further improves the coating adhesion and heat resistance. The first solvent, which is a mixture of ethyl acetate and propylene glycol methyl ether acetate, is used to adjust the viscosity of the anchoring layer coating liquid. After curing, it can completely evaporate without residue and does not affect the optical performance of the product.

[0050] Preferably, the molar ratio of –NCO to –OH is 0.8:1 to 1.5:1, more preferably 1.0:1 to 1.2:1.

[0051] Optionally, by weight, the release layer is obtained by curing a release layer coating liquid formed from 0.5 to 1.2 parts of perfluoroalkyl ether modified perfluoroacrylate copolymer, 0.03 to 0.08 parts of thermally decomposable free radical initiator, and 99.83 to 99.47 parts of hydrofluoroether, wherein the solid content of the release layer coating liquid is 0.53% to 1.17%; in this case, the second solvent is hydrofluoroether.

[0052] The perfluoroalkyl ether modified perfluoroacrylate copolymer is selected from at least one of the following: perfluoroacrylate copolymers containing perfluoropolyether side chains, perfluoroalkyl methacrylate and perfluoropolyether methacrylate copolymers, and perfluoroalkyl methacrylate copolymers with terminal olefin bonds. For example, the perfluoroalkyl ether modified perfluoroacrylate copolymer may be selected from at least one of Synesqo Fluorolink MD 700, Synesqo Fluorolink E 200, Daikin DAIFREE Z-201, Wisbon PFPE-AC-6200, and Fluorolink FL-PFPE-Acrylate-1500; more preferably, Synesqo Fluorolink MD 700.

[0053] The thermally decomposable free radical initiator is selected from at least one of azobisisobutyronitrile, azobisisovalerate, and dicumyl peroxide. For example, the thermally decomposable free radical initiator may be selected from at least one of Chemours VAZO-64, Fujifilm Wakako V-60, Fujifilm Wakako V-59, and Noryon Perkadox BC-FF, more preferably Chemours VAZO-64.

[0054] The hydrofluoroether is a hydrofluoroether-based fluorinated solvent, which may be selected from at least one of 3M Novec 7100, 3M Novec 7200, 3M Novec 7300, InnoFluo-449, CL7100, and Fluere-7300, and is more preferably 3M Novec 7100.

[0055] Among them, the perfluoroalkyl ether modified perfluoroacrylate copolymer contains reactive groups on its molecular chain that can undergo cross-linking by free radicals. Under the action of free radicals generated by thermally decomposable free radical initiators, it undergoes a cross-linking reaction to form a stable low surface energy release coating, which can endow the coating with ultra-low surface energy and achieve a low and stable release effect; the thermally decomposable free radical initiator decomposes upon heating to generate free radicals. Hydrofluoroethers have excellent compatibility with perfluororesins, evaporate completely without residue, and do not degrade the optical properties of the film.

[0056] The hydroxyl-terminated perfluorocarbon resin and the perfluoroalkyl ether-modified perfluoroacrylate copolymer selected in the embodiments of the present invention are both commercially available optical-grade perfluoro resins with a number-average molecular weight controlled between 5,000 and 20,000; the hydrofluoroether used is an electronic-grade hydrofluoroether solvent, which is suitable for optical thin film coating processes.

[0057] The present invention will be further described below with reference to embodiments and comparative examples, and performance tests will be conducted on the silicon-free double-layer fluorocarbon optical release films provided in each embodiment. Specifically, to verify the technical effects of the present invention, the following test methods were used to perform performance testing on each embodiment and comparative example:

[0058] This invention uses comparative examples and embodiments to verify the excellent release stability of the silicon-free double-layer fluorocarbon optical release film of this invention. Specifically, the coating solutions corresponding to the anchoring layer and release layer are applied to the respective substrate surfaces using microgravure coating and segmented high-temperature curing processes, respectively, and then cured. The microgravure coating process parameters include: a coating roller mesh of 120 mesh and a production line speed of 80 m / min.

[0059] The high-temperature curing process for the anchoring layer is as follows: Zone 1 temperature 75~85℃, Zone 2 temperature 115~125℃, Zone 3 temperature 145~155℃, with a total baking time of 20~30s; and / or, the high-temperature curing process for the release layer is as follows: Zone 1 temperature 85~95℃, Zone 2 temperature 125~135℃, Zone 3 temperature 155~165℃, with a total baking time of 15~25s. Preferably, the high-temperature curing process for the anchoring layer includes: Zone 1 temperature 80℃, Zone 2 temperature 120℃, Zone 3 temperature 150℃, with a total baking time of 25s; the high-temperature curing process for the release layer includes: Zone 1 temperature 90℃, Zone 2 temperature 130℃, Zone 3 temperature 160℃, with a total baking time of 20s.

[0060] To ensure consistency in experimental variables, all examples and comparative examples used the same batch of optical-grade PET substrate, the same type of reagents, the same corona treatment parameters, and the same coating and curing processes. Specifically, the corona treatment power used for corona modification was 2kW; the hydroxyl-terminated perfluorocarbon resin was selected from Synesqo Fluorolink D10-H, the hexamethylene diisocyanate trimer from Covestro Desmodur N3300, the perfluoroalkyl ether-modified perfluoroacrylate copolymer from Synesqo Fluorolink MD 700, the azobisisobutyronitrile from Chemours VAZO-64, and the hydrofluoroether from 3M Novec 7100.

[0061] The performance testing method is as follows:

[0062] 1) Release force test: NITTO 31B test tape was used, with a peel angle of 180° and a peel speed of 300mm / min. The unit is gf / 25mm.

[0063] 2) Constant temperature aging test: The ambient humidity is 50%RH. The test is set at 25℃ for normal temperature aging and 80℃ for high temperature aging. The aging cycles are 10d, 30d, 60d and 90d respectively.

[0064] 3) XPS silicon element detection and residual adhesion rate testing are performed in accordance with the general testing methods in the optical release film industry.

[0065] Example Group 1

[0066] Example 1

[0067] A silicon-free double-layer fluorocarbon optical release film, comprising the following film layer structures from bottom to top:

[0068] PET substrate layer: made of optical grade PET, with a thickness of 50μm;

[0069] Corona-modified layer: formed by in-situ oxidation and activation modification of the PET substrate surface by high-voltage corona discharge, with a modification depth of 10nm;

[0070] Anchoring layer: The anchoring layer coating solution is applied to the corona-modified layer and then cross-linked and cured to form a dry film with a thickness of 62.5 nm. The anchoring layer coating solution, by weight, comprises 1.8 parts of hydroxyl-terminated perfluorocarbon resin, 0.2 parts of hexamethylene diisocyanate trimer, 68 parts of ethyl acetate, and 30 parts of propylene glycol methyl ether acetate. The solid content of the anchoring layer coating solution is 2.0%.

[0071] Release layer: After the release layer coating liquid is applied to the anchoring layer, it is cured by thermal initiation of free radical cross-linking, and the dry film thickness is 43.8 nm. The release layer coating liquid comprises, by mass, 0.8 parts of perfluoroalkyl ether modified perfluoroacrylate copolymer, 0.05 parts of azobisisobutyronitrile, and 99.15 parts of hydrofluoroether. The solid content of the release layer coating liquid is 0.85%.

[0072] Example 2

[0073] A silicon-free double-layer fluorocarbon optical release film, comprising the following film layer structures from bottom to top:

[0074] PET substrate layer: made of optical grade PET, with a thickness of 50μm;

[0075] Corona-modified layer: formed by in-situ oxidation and activation modification of the PET substrate surface by high-voltage corona discharge, with a modification depth of 10nm;

[0076] Anchoring layer: The anchoring layer coating solution is applied to the corona-modified layer and then cross-linked and cured to form a dry film with a thickness of 29.2 nm. The anchoring layer coating solution, by weight, comprises 1.2 parts of hydroxyl-terminated perfluorocarbon resin, 0.12 parts of hexamethylene diisocyanate trimer, 69 parts of ethyl acetate, and 29.68 parts of propylene glycol methyl ether acetate. The solid content of the anchoring layer coating solution is 1.32%.

[0077] Release layer: After the release layer coating liquid is applied to the anchoring layer, it is cured by thermal initiation of free radical cross-linking, and the dry film thickness is 28.5 nm. The release layer coating liquid comprises, by mass, 0.5 parts of perfluoroalkyl ether modified perfluoroacrylate copolymer, 0.03 parts of azobisisobutyronitrile, and 99.47 parts of hydrofluoroether, and the solid content of the release layer coating liquid is 0.53%.

[0078] Example 3

[0079] A silicon-free double-layer fluorocarbon optical release film, comprising the following film layer structures from bottom to top:

[0080] PET substrate layer: made of optical grade PET, with a thickness of 50μm;

[0081] Corona-modified layer: formed by in-situ oxidation and activation modification of the PET substrate surface by high-voltage corona discharge, with a modification depth of 10nm;

[0082] Anchoring layer: The anchoring layer coating solution is applied to the corona-modified layer and then cross-linked and cured to form a dry film with a thickness of 98.5 nm. The anchoring layer coating solution, by weight, comprises 2.4 parts of hydroxyl-terminated perfluorocarbon resin, 0.3 parts of hexamethylene diisocyanate trimer, 67.0 parts of ethyl acetate, and 30.3 parts of propylene glycol methyl ether acetate. The solid content of the anchoring layer coating solution is 2.7%.

[0083] Release layer: After the release layer coating liquid is applied to the anchoring layer, it is cured by thermal initiation of free radical cross-linking, and the dry film thickness is 95.6 nm. The release layer coating liquid comprises, by mass, 1.2 parts of perfluoroalkyl ether modified perfluoroacrylate copolymer, 0.08 parts of azobisisobutyronitrile, and 98.83 parts of hydrofluoroether. The solid content of the release layer coating liquid is 1.17%.

[0084] Comparative Example 1

[0085] A traditional silicone optical release film comprises the following film layers from bottom to top:

[0086] PET substrate layer: made of optical grade PET, with a thickness of 50μm;

[0087] Corona-modified layer: formed by in-situ oxidation and activation modification of the PET substrate surface by high-voltage corona discharge, with a modification depth of 10nm;

[0088] Release layer: A traditional silicone release agent is applied to a corona-modified layer and then cross-linked and cured to form a dry film with a thickness of 100 nm.

[0089] By weight, the conventional silicone release agent component comprises 100 parts DOWSIL™ LTC761, 0.8 parts Syl-Off™ 7672, 1.5 parts Syl-Off™ 4000, and MEK / MIBK composite solvent, and the solid content of the conventional silicone release agent component is 3%.

[0090] Comparative Example 2

[0091] A silicon-free single-layer perfluorinated optical release film, comprising the following film layer structures from bottom to top:

[0092] PET substrate layer: made of optical grade PET, with a thickness of 50μm;

[0093] Corona-modified layer: formed by in-situ oxidation and activation modification of the PET substrate surface by high-voltage corona discharge, with a modification depth of 10nm;

[0094] Release layer: The release layer coating liquid is applied to the corona-modified layer and then cured by thermally initiated free radical cross-linking, with a dry film thickness of 60.0 nm. The release layer coating liquid comprises, by mass, 0.8 parts of perfluoroalkyl ether modified perfluoroacrylate copolymer, 0.05 parts of azobisisobutyronitrile, and 99.15 parts of hydrofluoroether, and has a solid content of 0.85%.

[0095] The optical release films provided in the above embodiments and comparative examples were subjected to XPS silicon element detection and residual adhesion rate testing according to the general testing methods in the optical release film industry. The test results of each embodiment and comparative example are shown in Table 1:

[0096]

[0097] Table 1

[0098] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film (exemplary example: Crown New Material CR-7202F), and the release force test value (unit: gf / 25mm) was continuously tracked at 25°C. The test results of each embodiment and comparative example are shown in Table 2:

[0099]

[0100] Table 2

[0101] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film, and the release force test value (unit: gf / 25mm) at 80°C was continuously tracked. The test results of each embodiment and comparative example are shown in Table 3.

[0102]

[0103] Table 3

[0104] Based on the test data of each embodiment and comparative example in Tables 1-3, it can be seen that:

[0105] The present invention incorporates a polyisocyanate crosslinking agent in the anchoring layer, which can crosslink with hydroxyl-terminated perfluorocarbon resin to form a dense three-dimensional network structure, significantly improving the coating's temperature resistance and shrinkage stress resistance. Comparative Example 2, a single-layer fluorine coating structure, lacks a dedicated anchoring base coating, resulting in low crosslinking density and insufficient adhesion to the substrate. Under high-temperature environments, coating displacement and loss of surface fluorine functional components easily occur, ultimately leading to a significant increase in release force, making it unsuitable for high-temperature processes such as OCA hot pressing and post-curing. The embodiments of the present invention, by adjusting the proportions of each functional layer, can flexibly control the coating thickness and release force, covering the application scenarios of different specifications of folded OCA and curved OCA products. Furthermore, the use of a pure fluorine system combined with a double-layer anchoring coating structure completely solves the silicon transfer contamination problem of traditional silicone release films and overcomes the defects of poor adhesion and insufficient high-temperature stability of ordinary single-layer fluorine release films. Its overall performance is significantly superior to existing organosilicon release films and single-layer fluorine release film products. This product has a residual adhesion rate of 93%~95%, and all indicators meet the standards of high-end optical release films. It can be widely used in the field of high-end optical adhesive films such as folded OCA and curved OCA.

[0106] Example Group 2: Corona-modified layer (Variables: modification depth / presence or absence of corona layer)

[0107] Example 1-1: PET substrate, corona modification depth 5nm, the rest is the same as in Example 1.

[0108] Examples 1-2: PET substrate, corona modification depth 12nm, the rest is the same as Example 1 (baseline).

[0109] Examples 1-3: PET substrate, corona modification depth 20nm, the rest is the same as in Example 1.

[0110] Comparative Example 1-1: Corona-free PET substrate, with direct coating of anchoring layer, the rest is the same as in Example 1.

[0111] Comparative Examples 1-2: Corona discharge depth 3nm (below the lower limit of protection), the rest is the same as in Example 1.

[0112] Comparative Examples 1-3: Corona discharge depth 25nm (exceeding the protection limit), the rest is the same as Example 1.

[0113] The optical release films provided in the above embodiments and comparative examples were subjected to XPS silicon element detection and residual adhesion rate testing according to the general testing methods in the optical release film industry. The test results of each embodiment and comparative example are shown in Table 1-1:

[0114]

[0115] Table 1-1

[0116] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film (exemplary example: Crown New Material CR-7202F), and the release force test value (unit: gf / 25mm) was continuously tracked at 25°C. The test results of each embodiment and comparative example are shown in Table 1-2:

[0117]

[0118] Table 1-2

[0119] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film, and the release force test value (unit: gf / 25mm) at 80°C was continuously tracked. The test results of each embodiment and comparative example are shown in Tables 1-3:

[0120]

[0121] Table 1-3

[0122] The above comparison shows that: no corona / insufficient depth: poor adhesion of the anchoring layer, and a significant increase in release force due to high temperature aging; depth exceeding the standard by 25nm: excessive oxidation of the PET surface, increased film haze, and brittle substrate.

[0123] Example Group 3: Anchoring Layer (Variables: hydroxyl-terminated fluorocarbon resin, amount of polyisocyanate, NCO / OH molar ratio)

[0124] Example 2-1: 1.2 parts of anchoring layer resin, 0.12 parts of crosslinking agent (lower limit ratio, molar ratio 0.8:1), the rest is the same as in Example 1.

[0125] Example 2-2: 1.8 parts of anchoring layer resin and 0.2 parts of crosslinking agent (intermediate ratio, molar ratio 1.1:1), the rest is the same as in Example 1.

[0126] Examples 2-3: 2.4 parts of anchoring layer resin, 0.3 parts of crosslinking agent (upper limit ratio, molar ratio 1.5:1), the rest is the same as in Example 1.

[0127] Comparative Example 2-1: 0.8 parts resin (less than 1.2 parts), 0.08 parts crosslinking agent, the rest is the same as in Example 1, but the crosslinking density is insufficient.

[0128] Comparative Example 2-2: 3.0 parts of resin (more than 2.4 parts), 0.36 parts of crosslinking agent, the rest is the same as in Example 1. Excess crosslinking agent absorbs water and turns white.

[0129] Comparative Examples 2-3: No polyisocyanate crosslinking agent was added, only hydroxyl-terminated fluorocarbon resin was used, and the rest was the same as in Example 1, without crosslinking network.

[0130] The optical release films provided in the above embodiments and comparative examples were subjected to XPS silicon element detection and residual adhesion rate testing according to the general testing methods in the optical release film industry. The test results of each embodiment and comparative example are shown in Table 2-1:

[0131]

[0132] Table 2-1

[0133] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film (exemplary example: Crown New Material CR-7202F), and the release force test value (unit: gf / 25mm) was continuously tracked at 25°C. The test results of each embodiment and comparative example are shown in Table 2-2:

[0134]

[0135] Table 2-2

[0136] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film, and the release force test value (unit: gf / 25mm) at 80°C was continuously tracked. The test results of each embodiment and comparative example are shown in Table 2-3:

[0137]

[0138] Table 2-3

[0139] The above comparison shows that: without crosslinking agent or with too low resin content, the anchoring layer is prone to falling off and the high-temperature release force drifts; with excessive resin or crosslinking agent content, the coating surface becomes sticky and the optical haze increases.

[0140] Example Group 4: Release Layer (Variables: Perfluoroacrylate, Amount of thermal initiator added)

[0141] Example 3-1: 0.5 parts copolymer, 0.03 parts initiator (lower limit), the rest is the same as in Example 1.

[0142] Example 3-2: 0.8 parts copolymer, 0.05 parts initiator (intermediate reference), the rest is the same as in Example 1.

[0143] Example 3-3: 1.2 parts copolymer, 0.08 parts initiator (upper limit), the rest is the same as in Example 1.

[0144] Comparative Example 3-1: 0.3 parts copolymer, 0.02 parts initiator, the rest are the same as in Example 1, the surface fluorine component is insufficient, and the release force is too high.

[0145] Comparative Example 3-2: 1.5 parts copolymer, 0.12 parts initiator, the rest are the same as in Example 1. The coating is over-crosslinked and the peel resistance increases.

[0146] Comparative Example 3-3: No thermal decomposition initiator, otherwise the same as Example 1, unable to crosslink, surface is easily worn and has serious residue.

[0147] The optical release films provided in the above embodiments and comparative examples were subjected to XPS silicon element detection and residual adhesion rate testing according to the general testing methods in the optical release film industry. The test results of each embodiment and comparative example are shown in Table 3-1:

[0148]

[0149] Table 3-1

[0150] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film (exemplary example: Crown New Material CR-7202F), and the release force test value (unit: gf / 25mm) was continuously tracked at 25°C. The test results of each embodiment and comparative example are shown in Table 3-2:

[0151]

[0152] Table 3-2

[0153] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film, and the release force test value (unit: gf / 25mm) at 80°C was continuously tracked. The test results of each embodiment and comparative example are shown in Table 3-3:

[0154]

[0155] Table 3-3

[0156] The above comparison shows that the copolymer is too low in surface energy, with a release force >6gf; it lacks initiator, the surface layer is not cross-linked, and a large amount of residual adhesive remains after storage.

[0157] Example Group 5: Membrane Structure System (Variables: Double-layer anchoring structure / Single-layer fluorine membrane / Organosilicon system)

[0158] Example 4-1: Anchoring 25nm + Release 25nm (thin double layer), the rest is the same as Example 1.

[0159] Example 4-2: Anchoring 62.5nm + release 43.8nm (standard double layer), the rest is the same as Example 1.

[0160] Example 4-3: Anchoring 100nm + Release 100nm (thick double layer), the rest is the same as Example 1.

[0161] Comparative Example 4-1: The anchoring layer uses silicone resin (disrupting the silicone-free system), and the rest is the same as in Example 1.

[0162] The optical release films provided in the above embodiments and comparative examples were subjected to XPS silicon element detection and residual adhesion rate testing according to the general testing methods in the optical release film industry. The test results of each embodiment and comparative example are shown in Table 4-1:

[0163]

[0164] Table 4-1

[0165] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film (exemplary example: Crown New Material CR-7202F), and the release force test value (unit: gf / 25mm) was continuously tracked at 25°C. The test results of each embodiment and comparative example are shown in Table 4-2:

[0166]

[0167] Table 4-2

[0168] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film, and the release force test value (unit: gf / 25mm) at 80°C was continuously tracked. The test results of each embodiment and comparative example are shown in Table 4-3:

[0169]

[0170] Table 4-3

[0171] The above comparison shows that single-layer fluorine film has poor adhesion and a sharp increase in aging release force; the organosilicon system has silicon contamination, resulting in a significant decrease in residual adhesion; and the presence of silicon in the anchoring layer directly negates the core advantage of this invention being silicon-free.

[0172] Example 6: Curing Process (Variables: Segmented Baking Temperature / Duration)

[0173] Example 5-1: Anchoring and curing at 80 / 120 / 150℃ for 25s; release at 90 / 130 / 160℃ for 20s (standard process), the rest is the same as in Example 1.

[0174] Example 5-2: Anchoring total baking time 20s, release total baking time 18s (lower limit time), the rest is the same as Example 1.

[0175] Example 5-3: Anchoring total baking time 30s, release total baking time 25s (maximum duration), the rest is the same as Example 1.

[0176] Comparative Example 5-1: Single layer cured at 120℃ constant temperature, the rest is the same as in Example 1, without segmentation, the solvent boils and pinholes appear.

[0177] Comparative Example 5-2: The total curing time was only 10 seconds, and the rest was the same as in Example 1. The cross-linking was incomplete and the adhesion was poor.

[0178] Comparative Example 5-3: The maximum curing temperature was increased to 180℃, and the rest was the same as in Example 1. The fluoropolymer underwent thermal decomposition, and the coating became foggy.

[0179] The optical release films provided in the above embodiments and comparative examples were subjected to XPS silicon element detection and residual adhesion rate testing according to the general testing methods in the optical release film industry. The test results of each embodiment and comparative example are shown in Table 5-1:

[0180]

[0181] Table 5-1

[0182] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film (exemplary example: Crown New Material CR-7202F), and the release force test value (unit: gf / 25mm) at 25°C was continuously tracked. The test results of each embodiment and comparative example are shown in Table 5-2:

[0183]

[0184] Table 5-2

[0185] The optical release films provided in each embodiment and comparative example were respectively coated with the contracted folded OCA adhesive film, and the release force test value (unit: gf / 25mm) at 80°C was continuously tracked. The test results of each embodiment and comparative example are shown in Table 5-3:

[0186]

[0187] Table 5-3

[0188] The above comparison shows that insufficient cross-linking and reduced coating temperature resistance and adhesion occur when the coating is not segmented or baked for too long; excessively high temperatures (180℃) degrade fluorocarbon resin and deteriorate optical properties.

[0189] It will be apparent to those skilled in the art that this disclosure is not limited to the details of the exemplary embodiments described above, and that this disclosure can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of this disclosure is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within this disclosure. No reference numerals in the claims should be construed as limiting the scope of the claims.

[0190] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A silicon-free double-layer fluorocarbon optical release film, comprising, from bottom to top: PET substrate layer, film thickness is 25~100μm; The corona-modified layer is formed on the surface of the PET substrate layer by high-voltage corona discharge, with a modification depth of 5~20nm; An anchoring layer, disposed on the surface of the corona-modified layer, is formed by cross-linking and curing of the anchoring layer coating liquid, with a dry film thickness of 25~100nm. The anchoring layer coating liquid comprises, by weight, 1.2~2.4 parts of hydroxyl-terminated perfluorocarbon resin, 0.12~0.3 parts of polyisocyanate cross-linking agent, and the balance being a first solvent. A release layer, disposed on the surface of the anchoring layer, is formed by thermally initiated free radical cross-linking and curing of the release layer coating liquid, with a dry film thickness of 25~100nm. The release layer coating liquid comprises, by weight, 0.5~1.2 parts of perfluoroalkyl ether modified perfluoroacrylate copolymer, 0.03~0.08 parts of thermally decomposable free radical initiator, and the balance being a second solvent.

2. The silicon-free, double-sided fluorocarbon optical release film according to claim 1, wherein, The conditions for forming the corona-modified layer are: corona power 2-8kW.

3. The silicon-free, double-sided fluorocarbon optical release film of claim 1, wherein, The first solvent is selected from ethyl acetate, propylene glycol methyl ether acetate, and mixtures thereof.

4. The silicon-free, double-sided fluorocarbon optical release film of claim 3, wherein, The first solvent is a mixture of 67-69 parts of ethyl acetate and 29.68-30.3 parts of ethyl acetate.

5. The silicon-free, two-layer fluorocarbon optical release film of claim 1, wherein, The second solvent is selected from hydrofluoroethers.

6. The silicon-free double-layer fluorocarbon optical release film according to claim 1, characterized in that, The hydroxyl-terminated perfluorocarbon resin is selected from hydroxyl-terminated perfluoropolyethers, hydroxyl-terminated perfluoroolefin copolymers, hydroxyl-terminated perfluoropolyether-modified fluorinated acrylate oligomers; and / or, The polyisocyanate crosslinking agent is selected from aliphatic polyisocyanate crosslinking agents, alicyclic polyisocyanate crosslinking agents, and blocked aliphatic polyisocyanate crosslinking agents.

7. The silicon-free double-layer fluorocarbon optical release film according to claim 1, characterized in that, The perfluoroalkyl ether modified perfluoroacrylate copolymer is selected from at least one of the following: perfluoroacrylate copolymers containing perfluoropolyether side chains, perfluoroalkyl methacrylate copolymers with perfluoropolyether methacrylate, and perfluoroalkyl methacrylate copolymers with terminal olefin bonds; and / or, The thermally decomposable free radical initiator is selected from at least one of azobisisobutyronitrile, azobisisovalerate, and dicumyl peroxide.

8. A method for preparing a silicon-free double-layer fluorocarbon optical release film according to any one of claims 1-7, comprising: The anchoring layer and the release layer are cured independently after coating.

9. The preparation method according to claim 8, characterized in that, The curing process employs segmented high-temperature curing, specifically: the high-temperature curing for the anchoring layer is as follows: Zone 1 temperature 75~85℃, Zone 2 temperature 115~125℃, Zone 3 temperature 145~155℃, with a total baking time of 20~30s; and / or, The high-temperature curing temperature corresponding to the release layer is: Zone 1 temperature 85~95℃, Zone 2 temperature 125~135℃, Zone 3 temperature 155~165℃, and the total baking time is 15~25s.

10. A display assembly, comprising a display body and a silicon-free double-layer fluorocarbon optical release film according to any one of claims 1-7 disposed on the display body.