A conductive adhesive for a sulfidized polyacrylonitrile positive electrode, a sulfidized polyacrylonitrile positive electrode, and preparation and application thereof

By introducing PEDOT:PSS into the sulfurized polyacrylonitrile cathode to form a hydrogen bond cross-linking network, the polysulfide shuttle effect and volume expansion problem of lithium-sulfur batteries are solved, thereby improving the cycle stability and rate performance of the battery.

CN123107571APending Publication Date: 2026-11-17SHANGHAI SULFUR TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610952842.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-sulfur batteries suffer from problems such as polysulfide shuttle effect, lithium anode corrosion, and cathode volume expansion, which lead to a decline in cycle life. Furthermore, traditional binders cannot improve electrochemical performance or adapt to volume changes, thus limiting their large-scale production.

Method used

PEDOT:PSS is used as a conductive binder that combines conductive and flexible components. Through hydrogen bonding, a network that combines rigidity and flexibility is formed, which enhances the cycle stability and rate performance of the vulcanized polyacrylonitrile cathode.

Benefits of technology

It improves the electrochemical activity and interfacial compatibility of the sulfurized polyacrylonitrile cathode, reduces the interfacial resistance, enhances the electronic conductivity and flexibility of the electrode, and improves the cycle stability and rate performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107571A_ABST
    Figure CN123107571A_ABST
Patent Text Reader

Abstract

The present application relates to a kind of vulcanized polyacrylonitrile positive electrode conductive adhesive, vulcanized polyacrylonitrile positive electrode and its preparation and application, the adhesive includes at least two components, wherein conductive component is poly (3,4-ethylenedioxythiophene) : poly (styrene sulfonate) (PEDOT:PSS), flexible component forms solid bridging network between electrode particles, and rigid component is combined with flexible component by hydrogen bond and electrostatic interaction, forms effective crosslinking network, cooperatively enhances the toughness of adhesive, while improving the electrochemical activity of SPAN positive electrode.The method proposed in the present application constructs good conductive path in SPAN positive electrode and significantly reduces the adhesive content, and the preparation method is simple, and the application prospect is big.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of secondary battery technology, and relates to a conductive adhesive for a sulfurized polyacrylonitrile positive electrode, its preparation and application. Background Technology

[0002] Currently, developing electrochemical energy storage systems that integrate cost-effectiveness, sustainability, and high energy density is crucial for the widespread application of hybrid energy systems and portable electronic devices. Among various energy storage technologies, lithium-sulfur batteries stand out due to their high energy density of up to 2600 Wh / kg. -1 Energy density, sulfur cathode up to 1675 mAh g -1 With its theoretical specific capacity, abundant sulfur resources, low cost, and environmental friendliness, lithium-sulfur batteries are considered highly promising high-efficiency energy storage devices. However, the commercialization of lithium-sulfur batteries still faces key challenges such as the "shuttle effect" of polysulfides, lithium anode corrosion, and cathode volume expansion, which severely restrict their practical application.

[0003] To improve the cycle life of lithium-sulfur batteries, researchers have adopted various strategies, including designing porous sulfur cathodes to confine polysulfides, protecting lithium metal anodes, developing functional binders and electrolytes, and modifying separators. To overcome the inherent defects of sulfur cathodes, researchers have focused on the design of advanced composite materials. The mainstream strategy is to encapsulate sulfur in various conductive matrices, such as carbon materials, conductive polymers, and metal oxides. However, these methods have failed to fundamentally suppress the dissolution and shuttle effect of polysulfides. To address these issues, researchers developed sulfurized polyacrylonitrile (SPAN) materials, which undergo solid-solid conversion reactions during charge and discharge, effectively preventing polysulfide dissolution and shuttle. SPAN exhibits high sulfur utilization and stable cycle performance in carbonate electrolytes, with a small self-discharge rate. However, SPAN still suffers from significant volume expansion, which can impair electrode structural integrity and lead to a decline in battery cycle life. Furthermore, the slow solid-solid conversion kinetics of SPAN result in limited conductivity, sluggish reaction rates, and poor rate performance of the battery. To address these challenges, researchers typically employ strategies such as doping with heteroatoms, catalytic additives, and conductive carbon materials to enhance the reaction kinetics and cycle durability of SPAN. However, its practical application is often hampered by complex and expensive synthesis processes, limiting its potential for large-scale production. The binder is a key component in electrode fabrication.

[0004] In recent years, researchers have successively applied various aqueous binders to SPAN cathode systems, including sodium carboxymethyl cellulose (CMC), carbonyl-β-cyclodextrin (C-β-CD), sodium alginate (SA), and guar gum (GG). These binders, containing hydroxyl and carboxyl functional groups, exhibit good compatibility with SPAN materials. However, these rigid binders not only easily cause cracks in high-load electrodes during drying but also struggle to accommodate the volume expansion of SPAN materials during cycling, leading to active material stripping and rapid capacity decay. More importantly, they cannot directly improve the electrochemical performance of SPAN. Furthermore, the aforementioned improvement strategies are often limited by complex and expensive synthesis processes, which restricts their feasibility for large-scale production.

[0005] Therefore, there is an urgent need to develop a lithium-sulfur polyacrylonitrile secondary battery that can improve the cycle stability and rate performance of the SPAN cathode while also having a high specific capacity. Summary of the Invention

[0006] The purpose of this invention is to provide a conductive adhesive for vulcanized polyacrylonitrile cathodes, vulcanized polyacrylonitrile cathodes, their preparation and application, and to improve the cycle stability and rate performance of vulcanized polyacrylonitrile cathodes by forming a rigid-flexible conductive crosslinking network in the adhesive.

[0007] The objective of this invention can be achieved through the following technical solutions: In a first aspect, the present invention provides a conductive adhesive for vulcanized polyacrylonitrile cathodes, which is compounded from a conductive component and a flexible component, wherein the conductive component is PEDOT:PSS, i.e., poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate), and the flexible component is one or more of polyvinyl alcohol, polyvinylidene fluoride, carboxymethyl cellulose, guar gum, styrene-butadiene rubber containing carboxyl groups, gum arabic, gum arabic, pectin, konjac gum, carrageenan, guar gum, sesame gum, guar gum, coumarin gum, and gelatin.

[0008] Furthermore, the mass ratio of the flexible component to the conductive component is (1~100):1.

[0009] Furthermore, the mass ratio of the flexible component to the conductive component is (5~100):1.

[0010] In a second aspect, the present invention provides a vulcanized polyacrylonitrile positive electrode, comprising vulcanized polyacrylonitrile, a conductive agent, and a conductive adhesive for the vulcanized polyacrylonitrile positive electrode as described above.

[0011] Furthermore, the conductive agent is one or more of acetylene black Super P, carbon nanotubes, and graphene.

[0012] Furthermore, the mass ratio of the vulcanized polyacrylonitrile, the conductive agent, and the conductive adhesive is (80~95):(2.5~10):(2.5~10).

[0013] In a third aspect, the present invention provides a method for preparing a vulcanized polyacrylonitrile positive electrode, wherein the conductive adhesive is first dissolved in water, and then a conductive agent and a vulcanized polyacrylonitrile positive electrode material are added and mixed to prepare a slurry, which is then coated onto a current collector to obtain a vulcanized polyacrylonitrile positive electrode.

[0014] Furthermore, the current collector is any one of aluminum foil, carbon-coated aluminum foil, copper foil, or carbon-coated copper foil.

[0015] In a fourth aspect, the present invention provides an application of a sulfurized polyacrylonitrile cathode in the preparation of lithium batteries or sodium batteries.

[0016] Furthermore, the lithium battery uses one or more of the following as the negative electrode: metallic lithium, lithium alloy, graphite, and silicon-carbon. The sodium battery uses one or more of metallic sodium, sodium alloy, and hard carbon as the negative electrode.

[0017] Compared with the prior art, the present invention has the following advantages: (1) By introducing PEDOT:PSS into the PVA / GG-SBR binder through a hydrogen bonding crosslinking strategy, not only was the crystallinity of flexible components such as PVA / GG-SBR reduced, giving the binder sufficient flexibility to adapt to the volume changes of SPAN during charging and discharging, but the dispersibility of conductive agents such as CNTs was also improved. In addition, the flexible component forms a stable bridging network between electrode particles, while the conductive rigid component combines with the flexible component through hydrogen bonding and electrostatic interactions to form an effective crosslinking network, synergistically enhancing the toughness of the binder and improving the electrochemical activity of the SPAN cathode. This dual function enhances the electronic conductivity of the electrode during cycling, strengthens the interfacial compatibility between the electrode and the electrolyte, and reduces the interfacial resistance.

[0018] (2) It makes full use of the effective synergistic effect between flexible components such as PVA and conductive components to construct a continuous conductive network and reduce the proportion of inactive adhesives. Attached Figure Description

[0019] Figure 1 The X-ray diffraction patterns of PVA and PEDOT:PSS in Example 4 show the change in crystallinity with the doping of PEDOT:PSS.

[0020] Figure 2 The tensile stress-strain curve of the PVA-PEDOT:PSS series adhesive film in Example 4 shows the change in film flexibility with the doping amount of PEDOT:PSS.

[0021] Figure 3 This is a long-cycle performance graph of electrodes prepared with different PVA binder contents in Example 5 (SPAN loading is 2.8 mg / cm²). -2 The multiplier is C / 2; SPAN / PVA-1: PVA content in the electrode is 10%; SPAN / PVA-2: PVA content in the electrode is 5%.

[0022] Figure 4 This is a long-cycle performance graph of electrodes prepared with different PEDOT:PSS doping levels of binder in Example 5 (SPAN loading of 2.1 mg cm⁻¹). -2 The magnification ratio is C / 2; the binder content in the electrode is 5%; the mass ratio of PVA to PEDOT to PSS in SPAN / PVA-PEDOT:PSS-1 is 100:1.5; the mass ratio of PVA to PEDOT to PSS in SPAN / PVA-PEDOT:PSS-2 is 100:3; the mass ratio of PVA to PEDOT to PSS in SPAN / PVA-PEDOT:PSS-3 is 20:1; and the mass ratio of PVA to PEDOT to PSS in SPAN / PVA-PEDOT:PSS-4 is 10:1.

[0023] Figure 5 This is a long-cycle performance graph of different electrodes in Example 6 (SPAN loading is 1.6 mg cm⁻¹). -2 The multiplier is C / 5.

[0024] Figure 6 This is a long-cycle performance graph of different electrodes in Example 6 (SPAN loading is 1.6 mg cm⁻¹). -2 (The multiplier is 1C).

[0025] Figure 7 This is a rate performance graph of different electrodes at different current densities in Example 6 (SPAN loading is 1.6 mg / cm²). -2 The multipliers are C / 10, C / 5, C / 2, 1C, 2C, 5C, and 10C.

[0026] Figure 8 This is a long-cycle performance graph of the SPAN / PVA-PEDOT: PSS-2 electrode (containing 3.5% binder) and the SPAN / PVA-PEDOT: PSS-3 electrode (containing 2.5% binder) in Example 7 (SPAN loading is 2.2 mg / cm²). -2 The multiplier is C / 2.

[0027] Figure 9 In Example 8, the SPAN loading was 4.6 mg cm⁻¹. -2and 5 mg cm -2 Long-cycle performance of the SPAN / PVA-PEDOT:PSS-1 electrode at 1 / 5 C rate (SPAN loading 4.6 mg / cm³). -2 and 5 mg cm -2 The multiplier is C / 5.

[0028] Figure 10 This is a graph showing the long-cycle performance of electrodes prepared with different CMC and PVDF binder contents in Comparative Example 2 (SPAN loading is 2.3 mg / cm²). -2 The multiplier is C / 2; SPAN / CMC-1: CMC content in the electrode is 10%, SPAN / CMC-2: CMC content in the electrode is 5%, SPAN / PVDF-1: PVDF content in the electrode is 10%, SPAN / PVDF-2: PVDF content in the electrode is 5%. Detailed Implementation

[0029] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.

[0031] As used herein, the terms "and / or," "or / and," and "and / or" encompass any one of two or more of the related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected using at least two conjunctions selected from "and / or," "or / and," and "and / or," it should be understood that, in this application, the technical solution undoubtedly includes solutions connected by "logical AND," and also undoubtedly includes solutions connected by "logical OR."

[0032] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0033] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0034] This document only specifically discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, just as any upper limit can be combined with any other upper limit to form an unspecified range. Furthermore, each individually disclosed point or single value can itself serve as a lower or upper limit and be combined with any other point or single value or with other lower or upper limits to form an unspecified range.

[0035] Unless otherwise specified, the temperature parameters in this application may be either constant temperature processing or processing within a certain temperature range. The constant temperature processing allows temperature fluctuations within the precision range controlled by the instrument, such as ±5°C, ±4°C, ±3°C, ±2°C, or ±1°C.

[0036] In this document, the term "suitable" as used in phrases such as "suitable combination," "suitable method," and "any suitable method" refers to the ability to implement the technical solution of this application, solve the technical problem of this application, and achieve the expected technical effect of this application.

[0037] In this application, terms such as "further," "even further," and "particularly" are used to describe purposes and indicate differences in content, but should not be construed as limiting the scope of protection of this application.

[0038] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified, and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0039] In the description of the application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0040] Unless otherwise specified, all preparations and tests described herein took place at 25°C.

[0041] The terms “comprising,” “including,” “containing,” “having,” “comprising,” or other variations thereof are intended to cover non-closed inclusion, and no distinction is made between these terms. The term “comprising” means that other steps and ingredients may be added without affecting the final result. The compositions and methods / processes of the present invention comprise, consist of, and substantially consist of the essential elements and limitations described herein, as well as any additional or optional ingredients, components, steps, or limitations described herein. No distinction is made between the terms “efficacy,” “performance,” “effect,” and “potency” herein.

[0042] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions. Unless otherwise specified, all technical features and optional technical features of this application can be combined to form new technical solutions.

[0043] Unless otherwise specified, all steps of this application may be performed sequentially or randomly, but sequentially is preferred.

[0044] In the following examples, poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) (PEDOT:PSS, 1.5 wt.%) was purchased from Aladdin Industrial Co., Ltd. (China), catalog number P191136; carboxymethyl cellulose (CMC) and polyvinylidene fluoride (PVDF) were purchased from Shenzhen Jinbang Electric Technology Co., Ltd.; and polyvinyl alcohol (PVA) was purchased from Thermo Fisher Scientific. All reagents were used as is without further purification.

[0045] The SPAN positive electrode is prepared by the following method: First, polyacrylonitrile and sulfur powder are mixed at a mass ratio of 1:8, and then heat-treated at 300℃ for 450 minutes under an inert atmosphere to obtain the SPAN active material. This material is then added to deionized water along with a conductive agent and binder to form a slurry (solid content approximately 29%), which is then coated onto the current collector (the coating amount of the slurry is approximately 1 mL / 75 cm). 2 The conductive agent is Super P and CNTs (in a mass ratio of 10:1), and the current collector is aluminum foil.

[0046] Unless otherwise specified, all other raw materials or processing techniques are commercially available materials or conventional processing techniques in the field.

[0047] Example 1: 0.5 g of solid PVA was heated at 90°C for 1 hour to dissolve it in 4.5 g of deionized water, preparing a 10 wt.% PVA aqueous solution. A certain amount of PEDOT:PSS was added to the prepared PVA aqueous solution, and the mixture was stirred for 1 hour to form a homogeneous and transparent aqueous solution. By changing the doping amount of PEDOT:PSS, binder solutions with different contents can be obtained.

[0048] For comparison, one of the following adhesives was selected: PVA, PVDF, or CMC. The preparation method was as follows: 0.5 g of PVA solid was heated at 90°C for 1 hour to dissolve it in 4.5 g of deionized water to prepare a 10 wt.% PVA aqueous solution; 0.5 g of PVDF solid was dissolved in 4.5 g of NMP to prepare a 10 wt.% solution; and 0.5 g of CMC solid was dissolved in 9.5 g of deionized water to prepare a 5 wt.% CMC aqueous solution.

[0049] Example 2 According to the method in Example 1, adhesive solutions with PVA to PEDOT:PSS mass ratios of 1:0 (i.e., pure PVA solution), 200:1, 100:1, 100:1.5, 50:1, 100:3, 20:1 and 10:1 were prepared respectively.

[0050] Example 3 The PVA-PEDOT:PSS aqueous solution (PVA to PEDOT:PSS mass ratio of 100:1.5) prepared in Example 2 above was poured into a polytetrafluoroethylene mold and crosslinked in situ at 30ºC for 36 hours to obtain a dark blue adhesive film. The pure PVA aqueous solution prepared in Example 1 was poured into a polytetrafluoroethylene mold and vacuum dried overnight at 30°C to obtain a white adhesive film. The pure PVDF adhesive solution prepared in Example 1 was poured into a polytetrafluoroethylene mold and vacuum dried overnight at 80°C to obtain a yellow adhesive film. The pure CMC aqueous solution prepared in Example 1 was poured into a polytetrafluoroethylene mold and vacuum dried at 40ºC for 6 hours to obtain a white adhesive film.

[0051] Example 4 The tensile properties and crystallinity of the different adhesive films in Example 3 were tested.

[0052] XRD test ( Figure 1 The results showed that pure PVA exhibited semi-crystalline properties, with a distinct crystallization peak at 2θ≈20° (corresponding to the (101) crystal plane). During the preparation of the composite film, the hydrogen bond interaction between PVA and PEDOT:PSS restricted the movement of the polymer chains, thereby inhibiting the crystallization of PVA.

[0053] Tensile test ( Figure 2The results show that when the mass ratio of PVA to PEDOT:PSS is 100:1.5, the incorporated PEDOT:PSS can disrupt its crystalline structure, thereby simultaneously improving the toughness and ductility of the binder. However, since PEDOT:PSS is a rigid component, further increasing its content leads to a decrease in the overall flexibility of the binder film, resulting in increased film brittleness and reduced elongation.

[0054] Example 5 A CR2016 coin cell was assembled using a SPAN positive electrode, a Li negative electrode, a PE separator, and an organic electrolyte. The electrolyte composition was 1 mL LiTFSI dissolved in EC, DMC, and FEC, with an EC to DMC mass ratio of 1:1 and an FEC mass fraction of 10% (i.e., 1 M LiTFSI / EC + DMC + 10 wt.% FEC). The electrolyte volume was 40 μL. The SPAN positive electrode loading was 1.6–2.8 mg cm⁻¹. -2 Electrochemical tests were performed on the battery after it had been left to stand for 12 hours. The charge / discharge test voltage range was 1–3 V (vs. Li). + / Li), current density as 1 C = 1675 mAh g -1 calculate.

[0055] Room temperature performance: Figure 3 This figure shows the long-cycle performance of electrodes prepared with different PVA binder contents at a current density of 1 / 2 C. Neither type of electrode is doped with PEDOT:PSS. The ratio of SPAN active material, conductive agent, and binder in the SPAN / PVA-1 electrode is 8:1:1, while the ratio in the SPAN / PVA-2 electrode is 16:2:1. The results show that reducing the PVA content improves the electrochemical performance of the battery, maintaining a performance exceeding 600 mAh g⁻¹ after 150 cycles. -1 The discharge specific capacity and capacity retention rate increased from 83.9% to 88%.

[0056] Figure 4 This is a graph showing the long-cycle performance of electrodes prepared with different PEDOT:PSS doping levels and binder at 1 / 2 C current density. The ratio of SPAN active material, conductive agent, and binder in each SPAN cathode is 16:2:1. The results show that the SPAN / PVA-PEDOT:PSS-1 electrode prepared with a PVA to PEDOT:PSS mass ratio of 100:1.5 exhibits the highest discharge specific capacity, with negligible capacity decay after 150 cycles and a capacity retention of up to 92.3% after 250 cycles.

[0057] Example 6 The battery assembly and testing methods are the same as those in Experiment Example 5 above.

[0058] Figure 5 This figure shows the long-cycle performance of electrodes prepared with different binders at a current density of 1 / 5 C. In the SPAN / PVA-PEDOT:PSS-1 electrode, the ratio of SPAN active material, conductive agent, and binder is 16:2:1, while in the other electrodes, the ratio is 8:1:1. The results show that the SPAN / PVA-PEDOT:PSS-1 electrode prepared with a PVA to PEDOT:PSS mass ratio of 100:1.5 exhibits excellent performance in terms of discharge specific capacity and cycle stability, achieving an initial coulombic efficiency of 81.48% and a sulfur utilization rate as high as 93.8%. After 250 cycles, it still maintains a capacity of 698 mAh g⁻¹. -1 It has a high discharge specific capacity, an ultra-low capacity decay rate (0.035% per cycle), and an 89% capacity retention rate.

[0059] Figure 6 This figure shows the long-cycle performance of electrodes prepared with different binders at a current density of 1 C. In the SPAN / PVA-PEDOT:PSS-1 electrode, the ratio of SPAN active material, conductive agent, and binder is 16:2:1, while in the other electrodes, the ratio is 8:1:1. The results show that when the current density is increased to 1 C, the performance of the SPAN / PVA-PEDOT:PSS-1 electrode remains stable: after 150 cycles, the capacity retention rate is 87%, corresponding to a capacity decay rate of only 0.064% per cycle.

[0060] Figure 7 This figure shows the rate performance of electrodes prepared with different binders at different current densities. In the SPAN / PVA-PEDOT:PSS-1 electrode, the ratio of SPAN active material, conductive agent, and binder is 16:2:1, while in the other electrodes, the ratio is 8:1:1. The results show that even at a high current density of 10 C, the SPAN / PVA-PEDOT:PSS-1 electrode still maintains a rate performance of approximately 300 mAh g⁻¹. -1 The specific capacity. Furthermore, when the current density recovers to 0.1 C, its reversible capacity recovers to approximately 780 mAh g⁻¹. -1 It exhibits excellent rate performance and outstanding structural reversibility.

[0061] Example 7 The battery assembly and testing methods are the same as those in Experiment Example 5 above.

[0062] Figure 8This is a graph showing the long-cycle performance of the SPAN / PVA-PEDOT:PSS-2 and SPAN / PVA-PEDOT:PSS-3 electrodes at a current density of 1 / 2 C. The ratio of SPAN active material, conductive agent, and binder in the SPAN / PVA-PEDOT:PSS-2 electrode is 24:3:1, while the ratio in the SPAN / PVA-PEDOT:PSS-3 electrode is 32:4:1. The results show that after 100 cycles, the capacity retention of SPAN / PVA-PEDOT:PSS-2 is 91.4%, decreasing to 84.2% after 150 cycles, and only 436 mAh g⁻¹ remains after 200 cycles. -1 The discharge specific capacity was [not specified]. In comparison, the SPAN / PVA-PEDOT:PSS-3 electrode exhibited superior cycling stability: the capacity retention rate was 93.7% after 100 cycles, only slightly decreasing to 91.1% after 150 cycles, and still maintained 600 mAh g⁻¹ after 200 cycles. -1 The above discharge specific capacity.

[0063] Example 8 The battery assembly and testing methods are the same as in Experiment 5 above, where the SPAN positive electrode loading is 4.6~5 mg cm⁻¹. -2 .

[0064] Figure 9 The SPAN loading is 4.6 mg cm. -2 and 5 mg cm -2 The graph shows the long-cycle performance of the SPAN / PVA-PEDOT:PSS-1 electrode at a current density of 1 / 5 C. Both electrodes exhibit stable cycling performance. The loading is 4.6 mg / cm³. -2 The electrode maintained 715 mAh g after 100 cycles. -1 The discharge specific capacity corresponds to a capacity retention of 94.1%; the loading capacity is 5 mg cm⁻¹. -2 The electrode retained 695 mAh g after 75 cycles. -1 The discharge specific capacity has a capacity retention rate of 92.2%.

[0065] Comparative Example 1: The electrodes SPAN / PVA-PEDOT:PSS-1, SPAN / PVA-2, SPAN / PVA-PEDOT:PSS-3, and SPAN / PVA-PEDOT:PSS-4 in Example 5 were tested, and the results are as follows.

[0066] The SPAN / PVA-2 electrode (undoped PEDOT:PSS) exhibited the lowest capacity and poor stability during the first 125 cycles, with a significant capacity decrease around the 175th cycle. After 200 cycles, the electrode structure collapsed, resulting in a capacity retention of only 15.5% after 250 cycles. For the SPAN / PVA-PEDOT:PSS-2 and SPAN / PVA-PEDOT:PSS-3 electrodes, the increased PEDOT:PSS doping level led to a decrease in the binder's flexibility, making it unable to adapt to the volume expansion and contraction of the SPAN particles during cycling. The discharge specific capacity of both was lower than that of SPAN / PVA-PEDOT:PSS-1, with capacity retention of 55.9% and 86% respectively after 250 cycles. For the SPAN / PVA-PEDOT:PSS-4 electrode with the highest PEDOT:PSS doping level, although the binder flexibility was significantly reduced, the large amount of PEDOT fixed in the binder network greatly improved the CNT dispersion, thereby increasing the electrode's electronic conductivity. The capacity retention rate still reached 88.8% after 200 cycles. However, after 250 cycles, its discharge specific capacity decreased to below 200 mAh g⁻¹. -1 (See Figure 4 (Comparison between China and the United States).

[0067] Comparative Example 2: Compared to Example 5, the binder in the SPAN positive electrode was adjusted to 5% and 10% CMC or PVDF. The ratio of SPAN active material, conductive agent, and binder in the SPAN / CMC-1 and SPAN / PVDF-1 electrodes was 8:1:1, and the ratio in the SPAN / CMC-2 and SPAN / PVDF-2 electrodes was 16:2:1. Test results: After reducing the CMC and PVDF binder content in the positive electrode, the discharge specific capacity of the corresponding electrodes showed a significant decrease. Specifically, after 150 cycles, the capacity retention of the SPAN / CMC-1 electrode decreased from 86% to 44% of the SPAN / CMC-2 electrode, while the capacity retention of the SPAN / PVDF-1 electrode decreased from 90.8% to 65.4% of the SPAN / PVDF-2 electrode. The discharge specific capacity of both electrodes was below 400 mAh g⁻¹. -1 ( Figure 10 ).

[0068] As can be seen, compared with traditional CMC and PVDF as binders for the SPAN positive electrode, the SPAN / PVA-PEDOT:PSS-1 electrode in Example 5 still exhibits excellent discharge specific capacity and other properties even when the binder content is reduced to about 5%. Comparative Example 3: Compared to Example 6, at a current density of 1 / 5 C, the binder used in the SPAN cathode was adjusted to be 10% pure PVA, pure PVDF, and pure CMC without PEDOT:PSS. Test results: The SPAN / PVDF-1 electrode showed significant capacity decay after 190 cycles, with a capacity retention of 82.4% after 250 cycles. The SPAN / CMC-1 electrode exhibited better cycle stability, with a capacity retention of 88.7% after 250 cycles. The SPAN / PVA-1 electrode showed severe capacity degradation: its discharge specific capacity plummeted to 200 mAh g⁻¹ after 200 cycles. -1 After 250 cycles, the capacity retention was only 7.7% (see...). Figure 5 (Comparison between China and the United States).

[0069] Comparative Example 4: Compared to Example 6, the binder used in the SPAN positive electrode was adjusted to contain 10% pure PVDF, pure CMC, and pure PVA at a current density of 1 C. Test results: The capacity retention rates of the prepared SPAN / PVDF-1, SPAN / CMC-1, and SPAN / PVA-1 electrodes after 150 cycles were only 39.5%, 83.2%, and 41.5%, respectively (see Example 6). Figure 6 (Comparison between China and the United States).

[0070] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A conductive adhesive for vulcanized polyacrylonitrile positive electrodes, characterized in that, It is composed of a conductive component and a flexible component, wherein the conductive component is PEDOT:PSS, and the flexible component is one or more of the following: polyvinyl alcohol, polyvinylidene fluoride, carboxymethyl cellulose, guar gum, styrene-butadiene rubber containing carboxyl groups, gum arabic, peach gum, pectin, konjac gum, carrageenan, guar gum, sesame gum, guar gum, coumarin gum, and gelatin.

2. The conductive adhesive for vulcanized polyacrylonitrile positive electrode according to claim 1, characterized in that, The mass ratio of the flexible component to the conductive component is (1~100):

1.

3. The conductive adhesive for vulcanized polyacrylonitrile positive electrodes according to claim 2, characterized in that, The mass ratio of the flexible component to the conductive component is (5~100):

1.

4. A vulcanized polyacrylonitrile positive electrode, characterized in that, It includes vulcanized polyacrylonitrile, a conductive agent, and a conductive adhesive for vulcanized polyacrylonitrile cathodes as described in any one of claims 1-3.

5. The vulcanized polyacrylonitrile cathode according to claim 4, characterized in that, The conductive agent is one or more of acetylene black Super P, carbon nanotubes, and graphene.

6. The vulcanized polyacrylonitrile cathode according to claim 4, characterized in that, The mass ratio of the vulcanized polyacrylonitrile, the conductive agent, and the conductive adhesive is (80~95):(2.5~10):(2.5~10).

7. The method for preparing a vulcanized polyacrylonitrile cathode as described in claim 4, characterized in that, First, the conductive adhesive is dissolved in water. Then, a conductive agent and a vulcanized polyacrylonitrile cathode material are added and mixed to prepare a slurry. This slurry is then coated onto a current collector to obtain a vulcanized polyacrylonitrile cathode.

8. The method for preparing the vulcanized polyacrylonitrile cathode according to claim 7, characterized in that, The current collector is any one of aluminum foil, carbon-coated aluminum foil, copper foil, or carbon-coated copper foil.

9. The application of the sulfurized polyacrylonitrile cathode as described in claim 4 in the preparation of lithium batteries or sodium batteries.

10. The application according to claim 9, characterized in that, The lithium battery uses one or more of the following as the negative electrode: metallic lithium, lithium alloy, graphite, and silicon-carbon. The sodium battery uses one or more of metallic sodium, sodium alloy, and hard carbon as the negative electrode.