Particle-reinforced titanium matrix composite preform and its preparation method

By combining vacuum melting, forging, plasma rotating electrode atomization, and hot isostatic pressing, the problems of uneven microstructure and process complexity of particle-reinforced titanium matrix composites were solved, achieving a balance between high strength and high plasticity, improving material utilization and performance, and exhibiting excellent mechanical properties, especially at high temperatures.

CN123108345APending Publication Date: 2026-11-17AVIC BEIJING AERONAUTICAL MFG TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611213398.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for preparing particle-reinforced titanium matrix composites suffer from problems such as uneven microstructure, complex processes, low material utilization, and difficulty in achieving both high strength and high ductility and toughness.

Method used

TiBw-reinforced titanium matrix composite ingots were prepared by vacuum melting and then forged multiple times above the β phase transformation point. Spherical powders were prepared by plasma rotating electrode atomization and then hot isostatic pressing to control the size and distribution of the TiBw reinforcing phase, thus eliminating intermediate machining steps.

Benefits of technology

It achieves a good balance between uniform material structure, high strength and high plasticity, shortens the production cycle, improves material utilization, reduces production costs, and maintains excellent mechanical properties at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108345A_ABST
    Figure CN123108345A_ABST
Patent Text Reader

Abstract

This invention provides a particle-reinforced titanium matrix composite billet and its preparation method. The method includes: preparing a TiBw-reinforced titanium matrix composite billet by vacuum melting; directly precision forging it into a bar at 50℃~150℃ above the β phase transformation point through 2~6 heat treatments; preparing spherical powder with a particle size ≤250μm using a plasma rotating electrode atomization method; and loading the powder into a sleeve for hot isostatic pressing, with process parameters of temperature 950~1200℃, pressure 50~200MPa, and holding at temperature and pressure for 0.5~6h. This invention eliminates the traditional multi-heat free forging and numerous machining processes, resulting in a shorter process and higher material utilization. The TiBw reinforcing phase in the obtained billet is smaller than 50μm and uniformly distributed, with a room temperature tensile strength ≥1076MPa and elongation ≥5%, and a 650℃ tensile strength ≥500MPa and elongation ≥12%, exhibiting excellent comprehensive mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of composite material manufacturing technology, and more specifically, to a particle-reinforced titanium-based composite material blank and its preparation method. Background Technology

[0002] Titanium and titanium alloys are widely used in aerospace and high-end equipment manufacturing due to their high specific strength and excellent corrosion resistance. However, the high-temperature strength, wear resistance, and creep resistance of traditional titanium alloys are gradually becoming insufficient to meet the requirements of next-generation high-performance components. Particle-reinforced titanium matrix composites (TMCs) significantly improve the stiffness, high-temperature strength, and wear resistance of materials by introducing high-hardness, high-modulus ceramic particles (such as TiB and TiC) into a titanium matrix.

[0003] In existing technologies for preparing particle-reinforced titanium matrix composites, large-size ingots are typically prepared by casting, followed by multiple free forging or rolling processes for billet preparation and shaping. However, these existing technologies suffer from the following significant drawbacks: 1. Traditional free forging processes cannot completely eliminate component segregation and reinforcement agglomeration during the casting process, resulting in uneven distribution of TiBw whiskers, which seriously affects the mechanical properties of the material.

[0004] 2. After forging, large-sized ingots often require extensive machining to produce bars for powder making, resulting in low material utilization and long production cycles.

[0005] 3. If the cast ingot is directly atomized into powder, the high brittleness of the cast structure will easily lead to a high rate of hollow powder and many satellite balls, which will affect the densification effect of subsequent hot isostatic pressing (HIP).

[0006] 4. For some applications that require extremely high toughness (such as the eccentric rotor of a cycloidal rotor pump), existing composite materials often struggle to balance high strength and high elongation.

[0007] Therefore, it is of great significance to develop a simple, low-cost method for preparing titanium-based composite material blanks that can produce uniform microstructure and excellent comprehensive mechanical properties. Summary of the Invention

[0008] (a) Technical problems to be solved The technical problem to be solved by the present invention is the existing technical problems of uneven structure, complex process, low material utilization and difficulty in achieving both high strength and high toughness in the preparation of particle-reinforced titanium matrix composites.

[0009] (II) Technical Solution To achieve the above objectives, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides a method for preparing a particle-reinforced titanium-based composite material preform, comprising the following steps: S1. TiBw reinforced titanium matrix composite ingots were prepared by vacuum melting method; S2. The billet is forged 2 to 6 times at a temperature range of 50°C to 150°C above the β phase transformation point to prepare a precision forged bar. S3. Using the plasma rotating electrode atomization method, TiB-reinforced titanium-based composite spherical powder is prepared from precision-forged bars; S4. The spherical powder is loaded into a sleeve and subjected to hot isostatic pressing to obtain a titanium-based composite material blank. The hot isostatic pressing process parameters are: temperature 950~1200℃, pressure 50~200MPa, and holding time 0.5~6h.

[0010] In the above technical solution, step S2 involves direct precision forging in the β single-phase region, effectively breaking down the coarse TiBw whiskers and original grains in the as-cast microstructure. Step S3, through the rapid solidification process of plasma rotating electrode atomization, further refines the microstructure, obtaining fine equiaxed crystals and dispersed TiBw. In step S4, during hot isostatic pressing, TiBw fractures and rearranges under high temperature and pressure. The synergistic effect of these three processes ultimately controls the size of the TiBw reinforcing phase in the billet to below 50 μm and ensures its extremely uniform distribution, overcoming the technical difficulties of coarse and unevenly distributed reinforcing phases in traditional casting methods. Compared with the lengthy traditional process of "melting + multi-stage free forging + rough machining + fine machining + powder making," this solution uses direct precision forging in step S2, directly forging the billet into bars that meet the requirements of the powder making electrode, eliminating a large number of intermediate machining processes. This greatly shortens the production cycle, significantly improves the material utilization rate from billet to final product, and reduces production costs. The billets prepared by this method achieve a good balance between high strength and high plasticity. The hot isostatic pressing process (temperature 950~1200℃, pressure 50~200 MPa) ensures sufficient powder densification while avoiding excessive growth of TiBw. The resulting billets achieve a room temperature tensile strength exceeding 1076 MPa, while maintaining a room temperature elongation above 5.0%. Even at 650℃, they retain a tensile strength exceeding 500 MPa and an elongation exceeding 12.0%, demonstrating excellent high-temperature performance and superplastic potential. This provides billets with more uniform microstructure and superior performance for subsequent hot working.

[0011] Preferably, the volume fraction of TiBw in the TiBw-reinforced titanium matrix composite ingot is 0.5% to 5%. Limiting the TiBw volume fraction to this range ensures the composite's strength while preventing a sharp decrease in plasticity due to excessive reinforcing phase. When the TiBw content is below 0.5%, the reinforcing effect is not significant; above 5%, the material becomes more brittle, increasing processing difficulty. This preferred range is crucial for achieving a balance between high strength and good plasticity.

[0012] Preferably, the particle size of the TiB-reinforced titanium-based composite spherical powder is ≤250 μm. Controlling the powder particle size to ≤250 μm (preferably 53~150 μm) is beneficial for subsequent hot isostatic pressing. On the one hand, finer powder has higher surface energy and sintering activity, enabling higher density to be achieved at lower temperatures and pressures; on the other hand, powder in this particle size range has good flowability, facilitating packing and filling, and ensuring the uniformity of the billet structure. Furthermore, this also matches the process characteristics of the plasma rotating electrode atomization method, helping to obtain powder with high sphericity, reducing hollow powder and satellite spheres, thereby improving the mechanical properties of the final billet.

[0013] Preferably, before step S4, the method further includes the following steps: adding TiB2 powder to the spherical powder for mixing, wherein the volume fraction of the TiB2 powder is 0~5% and the particle size of the TiB2 powder is 1~5μm; the ball milling parameters are: ball-to-material ratio (2~8):1, rotation speed 100~300r / min, and ball milling time 5~15h.

[0014] In the above technical solution, by adding TiB2 powder, the total amount and proportion of reinforcing phase in the final billet can be further adjusted based on the original TiBw content. The newly added micron-sized TiB2 powder (1~5μm) reacts with the matrix during the subsequent hot isostatic pressing process, generating fine TiBw in situ. This forms a multi-scale reinforcing structure with the original TiBw in the atomized powder, further improving the overall performance of the material. The ball-to-powder ratio (2~8:1), rotation speed (100~300 r / min), and time (5~15 h) used are all low-energy ball milling parameters, the purpose of which is to uniformly mix the powder rather than grind and crush it. This ensures that the high sphericity and particle size distribution of the original spherical powder are not destroyed, thus not affecting its flowability and sintering performance.

[0015] Preferably, the TiB2 powder has a volume fraction of 0.5%.

[0016] Preferably, in step S4, the process parameters for hot isostatic pressing are: temperature 1050~1170℃, pressure 120~150MPa, and heat and pressure holding time 4h.

[0017] Preferably, in step S1, the vacuum melting method is three-stage vacuum consumable electrode melting.

[0018] Preferably, the titanium-based composite material is a TiBw / TA15, TiBw / Ti6242, or TiBw / IMI834 composite material.

[0019] Secondly, the present invention provides a titanium-based composite material blank prepared by the preparation method described above, wherein the size of the TiBw reinforcing phase in the blank is less than 50 μm; the room temperature elongation of the blank is ≥5.0%, and the room temperature tensile strength is ≥1076 MPa.

[0020] Preferably, the blank has an elongation of ≥12.0% at 650℃ and a tensile strength of ≥500MPa.

[0021] (III) Beneficial Effects The above-described technical solution of the present invention has at least the following advantages: 1. This invention utilizes a combination of direct precision forging and rotary electrode atomization powder production. The forging process breaks down coarse, cast grains, followed by rapid solidification via atomization, resulting in a fine equiaxed grain structure. During subsequent hot isostatic pressing, the TiBw whiskers fracture and rearrange under thermal drive, ultimately controlling the size to below 50 μm with extremely uniform distribution, thus eliminating macroscopic segregation.

[0022] 2. This invention eliminates the numerous machining processes following forging in traditional processes, directly using precision-forged bars as PREP electrodes, which significantly improves material utilization and shortens the production cycle.

[0023] 3. The billet prepared by this invention achieves a good balance between strength and plasticity. The room temperature tensile strength exceeds 1076 MPa while the elongation remains above 5%; especially at a high temperature of 650℃, the elongation can reach more than 12%, showing excellent superplastic potential, which is very beneficial for subsequent isothermal forging or hot forming.

[0024] 4. By introducing a low-energy ball milling mixing step, this invention allows for flexible adjustment of the final content and type of the reinforcing phase, enabling customized control of material properties. Attached Figure Description

[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0026] Figure 1 The image shows the microstructure of the particle-reinforced titanium matrix composite material blank prepared in the first specific embodiment of the present invention. Figure 2 The image shows the microstructure of the particle-reinforced titanium matrix composite material blank prepared in the second specific embodiment of the present invention. Figure 3 The image shows the microstructure of the titanium matrix composite material blank prepared in the third specific embodiment of the present invention. Figure 4 This is a metallographic photograph of the microstructure of the particle-reinforced titanium matrix composite material blank prepared in the fourth specific embodiment of the present invention. Detailed Implementation

[0027] To make the technical problems to be solved, the technical solutions, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the present invention and are not intended to limit the present invention.

[0028] The specific implementation of the present invention will be described in more detail below with reference to specific embodiments: Example 1 1. Prepare 200 kg of 2.0 vol% TiB / TA15 composite material ingot (TiBw reinforced titanium matrix composite material ingot) by three vacuum consumable electrode melting. Then, forge the titanium matrix composite material ingot into Ф40×400 mm bars by six forging cycles at 1100~1150℃. 2. Titanium-based composite spherical powder (TiB-reinforced titanium-based composite spherical powder) is prepared in a plasma rotating electrode powder preparation equipment, wherein the electrode rotation speed is 27000~28000 r / min; 3. The prepared spherical powder of 53~150um and 0.5vol%TiB2 powder were ball-milled and mixed. The TiB2 powder size was 1~5μm, the ball-to-powder ratio was 3:1, the rotation speed was 200r / min, and the ball milling was carried out for 5~8h. The titanium-based composite material billet was prepared by hot isostatic pressing at 1170℃ / 135MPa / 4h. 4. For example Figure 1 As shown, a fine and uniform titanium-based composite material blank of TiBw was obtained, with a room temperature strength of 1076 MPa and a room temperature elongation of 6.0%; a tensile strength of 500 MPa and an elongation of 16.0% at 650℃.

[0029] Example 2: 1. Prepare 300 kg of 3.5 vol% TiB / Ti6242 composite material ingot (TiBw reinforced titanium matrix composite material ingot) by three vacuum consumable electrode melting. Then, forge the titanium matrix composite material ingot into Ф50×400 mm bars by six forging cycles at 1100~1150℃. 2. Titanium-based composite spherical powder (TiB-reinforced titanium-based composite spherical powder) is prepared in a plasma rotating electrode powder preparation equipment, wherein the electrode rotation speed is 24000~26000 r / min; 3. The prepared spherical powder of 53~150um was subjected to hot isostatic pressing at 1050℃ / 150MPa / 4h to prepare titanium-based composite material blanks; 4. For example Figure 2 As shown, a titanium-based composite material blank with fine and uniform TiBw distribution was obtained, with a room temperature strength of up to 1100 MPa and a room temperature elongation of 6.0%; a tensile strength of 550 MPa and an elongation of over 12.0% at 650℃ were obtained.

[0030] Example 3: 1. A 3.5 vol% TiB / IMI834 composite ingot (TiBw reinforced titanium matrix composite ingot) was prepared by three-stage vacuum consumable electrode melting, and the titanium matrix composite ingot was precision forged into Ф50×400mm bars; 2. Titanium-based composite spherical powder (TiB-reinforced titanium-based composite spherical powder) is prepared in a plasma rotating electrode powder preparation equipment, wherein the electrode rotation speed is 27000~28000 r / min; 3. The prepared spherical powder of 53~150um and 0.5vol%TiB2 powder were ball-milled and mixed. The TiB2 powder size was 1~5μm, the ball-to-powder ratio was 3:1, the rotation speed was 250r / min, and the ball milling was carried out for 5~8h. The titanium-based composite material ingot was prepared by hot isostatic pressing at 1150℃ / 120MPa / 4h. 4. For example Figure 3 As shown, the TiBw in the billet is finely and uniformly distributed in the matrix, and there is no large-scale aggregation of TiBw. 5. The room temperature strength of the billet can reach 1169 MPa, and the room temperature elongation reaches 5.0%; the tensile strength at 650℃ is 500 MPa, and the elongation reaches 15.1%.

[0031] Example 4: 1. Prepare 150 kg of 3.5 vol% TiB / Ti6242 composite material ingot (TiBw reinforced titanium matrix composite material ingot) by three vacuum consumable electrode melting. Precision forge the titanium matrix composite ingot into Ф50×400 mm bars at 1100~1150℃. 2. Spherical powder of titanium-based composite material (TiB-reinforced titanium-based composite spherical powder) is prepared in a plasma rotating electrode powder preparation equipment, wherein the electrode rotation speed is 24000~26000 r / min; 3. The prepared spherical powder of 53~150um was subjected to hot isostatic pressing at 1050℃ / 150MPa / 4h to prepare titanium-based composite material blanks; 4. For example Figure 4 As shown, a titanium-based composite material blank with fine and uniform TiBw distribution was obtained, with a room temperature strength of up to 1100 MPa and a room temperature elongation of 6.0%; a tensile strength of 550 MPa and an elongation of over 12.0% at 650℃ were obtained.

[0032] In summary, this invention has successfully prepared particle-reinforced titanium-based composite material billets with uniform microstructure and excellent comprehensive mechanical properties through a specific process route, thus solving the pain points of the prior art.

[0033] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a particle-reinforced titanium matrix composite preform, characterized in that, Includes the following steps: S1. TiBw reinforced titanium matrix composite ingots were prepared by vacuum melting method; S2. The billet is forged 2 to 6 times in a temperature range of 50°C to 150°C above the β phase transformation point to prepare a precision forged bar. S3. Using the plasma rotating electrode atomization method, TiB-reinforced titanium-based composite spherical powder is prepared from precision-forged bars; S4. The spherical powder is loaded into a sleeve and subjected to hot isostatic pressing to obtain a titanium-based composite material blank. The hot isostatic pressing process parameters are: temperature 950~1200℃, pressure 50~200 MPa, and holding time 0.5~6 h.

2. The method for preparing the particle-reinforced titanium matrix composite preform as described in claim 1, characterized in that, The volume fraction of TiBw in the TiBw-reinforced titanium matrix composite ingot is 0.5% to 5%.

3. The method for preparing the particle-reinforced titanium matrix composite preform as described in claim 2, characterized in that, The particle size of the TiB-reinforced titanium-based composite spherical powder is ≤250μm.

4. The method for preparing the particle-reinforced titanium matrix composite preform as described in claim 1, characterized in that, Before step S4, the following steps are also included: adding TiB2 powder to the spherical powder for mixing, wherein the volume fraction of TiB2 powder is 0~5% and the particle size of TiB2 powder is 1~5μm; the ball milling parameters are: ball-to-material ratio (2~8):1, rotation speed 100~300 r / min, and ball milling time 5~15 h.

5. The method for preparing the particle-reinforced titanium matrix composite preform as described in claim 4, characterized in that, The TiB2 powder has a volume fraction of 0.5%.

6. The method for preparing the particle-reinforced titanium matrix composite preform as described in claim 1, characterized in that, In step S4, the process parameters for hot isostatic pressing are: temperature 1050~1170℃, pressure 120~150 MPa, and holding time 4 h.

7. The method for preparing the particle-reinforced titanium matrix composite preform as described in claim 1, characterized in that, In step S1, the vacuum melting method is three-stage vacuum consumable electrode melting.

8. The method for preparing the particle-reinforced titanium matrix composite preform as described in claim 1, characterized in that, The titanium-based composite material is a TiBw / TA15, TiBw / Ti6242, or TiBw / IMI834 composite material.

9. A particle-reinforced titanium-based composite material preform prepared by the preparation method according to any one of claims 1 to 8, characterized in that, The size of the TiBw reinforcing phase in the billet is less than 50 μm; the room temperature elongation of the billet is ≥5.0%, and the room temperature tensile strength is ≥1076 MPa.

10. The particle-reinforced titanium matrix composite preform as described in claim 9, characterized in that, The billet has an elongation of ≥12.0% at 650℃ and a tensile strength of ≥500 MPa.