Additive manufacturing method of titanium-based composite material
Through ball mill mixing and vacuum sintering combined with 3D printing technology, the thermal stress problem in additive manufacturing of titanium-based composite materials is solved, and unsupported low-cost and efficient preparation is achieved, and complex structures can be prepared, which improves the mechanical properties of the materials and the mechanical properties of the materials. density.
Patent Information
- Application Number
- CN202411156220.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-26
AI Technical Summary
There are thermal stress problems in the existing additive manufacturing technology of titanium-based composite materials, which leads to high risk of cracking, and it is difficult to prepare complex structures such as hollow components, and the process is complex and costly.
Using ball mill mixed titanium powder and reinforced phase raw materials, vacuum drying and sintering, combined with 3D printing technology, unsupported additive manufacturing is achieved through adhesive bonding, reducing thermal stress, and regulating the tissue structure through particle size ratio to ensure strengthening The mesh distribution of phases.
The titanium-based composite molding under low thermal stress is realized, the process is simplified, the cost is reduced, complex structures such as hollow members can be prepared, and the mechanical properties and density of the materials are improved.
Smart Images

Figure FT_1
Abstract
Description
Technical Field
[0001] The invention relates to an additive manufacturing method, in particular to an additive manufacturing method for a titanium-based composite material. Background Art
[0002] Discontinuously reinforced titanium-based composites have excellent specific strength, specific stiffness, and isotropy, and have broad application prospects, especially titanium-based composites with a network structure of reinforcement phase, which have excellent strength and plasticity. Additive manufacturing technology is a technology that achieves near-net forming of components by stacking materials layer by layer. Using additive manufacturing technology to prepare titanium-based composite components is one of the important directions for future development.
[0003] The additive manufacturing of titanium-based composites is currently mainly based on two methods: laser powder bed melting and laser directed energy deposition. The specific forms are divided into the following three aspects:
[0004] (1) Mix titanium metal powder and reinforcement powder evenly, make the reinforcement phase powder adhere to the surface of the metal powder, and then use laser powder bed technology or powder feeding laser directed energy deposition technology to form. On the one hand, these two additive manufacturing technologies have large thermal stresses. On the other hand, in-situ reactions will occur between metal powder and ceramic powder and release heat, further increasing thermal stress and the risk of cracking during the manufacturing process.
[0005] (2) A titanium-based composite material ingot or rod is prepared in advance by melt casting or powder metallurgy, and then the titanium-based composite material is prepared by gas atomization or rotating electrode method. Although this method can reduce the thermal stress in the manufacturing process, the method is complex, time-consuming and expensive.
[0006] (3) Two powder feeding systems are used to feed titanium alloy powder and ceramic powder into the molten pool according to the preset composition during the printing process. However, due to the lack of pre-mixing, the reinforcement phase is prone to segregation during the printing process, and defects are prone to occur inside, which leads to poor performance.
[0007] In addition, when using the above methods for additive manufacturing, the titanium alloy material is often completely melted, making it difficult to design the organization at the microscale. In addition, when manufacturing many complex structures, complex supports need to be added to the structure to assist the additive manufacturing process, which makes it difficult to prepare some components containing hollow structures using existing technologies. Summary of the invention
[0008] The technical problem to be solved by the present invention is to provide an additive manufacturing method for titanium-based composite materials, during which no support needs to be added and cracking will not be caused by thermal stress. The reinforcement phase of the prepared titanium-based composite material is distributed in a quasi-continuous network and has good mechanical properties.
[0009] In order to solve the above technical problems, the technical solution of the present invention is:
[0010] A method for additive manufacturing of a titanium-based composite material comprises the following steps:
[0011] S1. The titanium powder and the reinforcing phase raw material were put into the ball mill of a planetary ball mill, and the ball mill was filled with argon gas three times and then milled for 3-5h to obtain a mixed powder;
[0012] S2. Place the mixed powder obtained in step S1 in a vacuum drying oven and vacuum dry for 3-6h to obtain a dry powder;
[0013] S3. placing the dry powder and binder obtained in step S2 in a 3D printer, spraying the binder for 3D printing to obtain a 3D printed component;
[0014] S4. Vacuum degreasing the 3D printed component obtained in step S3 for 0.5-1.5h to obtain a degreased 3D printed component;
[0015] S5. Place the degreased 3D printed component obtained in step S4 in a vacuum furnace, and after vacuum sintering, cool it to room temperature in the furnace to obtain a titanium-based composite material.
[0016] Furthermore, in step S1 of the present invention, the weight ratio of titanium powder to reinforcing phase raw material is 1:(0.02-0.05); the titanium powder is composed of small-particle titanium powder and large-particle titanium powder in a weight ratio of 4:6-7:3, wherein the particle size of the small-particle titanium powder is 1-15μm, and the particle size of the large-particle titanium powder is 35-180μm; the reinforcing phase raw material is one of B4C, TiB2 or graphite flakes with a particle size of 0.2-3μm. The main purpose of selecting two titanium powders with different particle sizes is to make the organization present a network structure distribution, and if only titanium powder with a larger particle size is selected, it is difficult to ensure the density in the subsequent sintering process; the reinforcing phase raw material selects powders that can react with titanium in situ during the sintering process, in order to introduce ceramic reinforcing phase.
[0017] Furthermore, in step S1 of the present invention, the ball milling speed is 180-240 rpm, the ball-to-material ratio is 1:1-5:1, and the ball milling jar and the grinding balls are made of stainless steel. The main purpose of ball milling is to evenly mix titanium powder and reinforcing phase powder of different particle sizes.
[0018] Furthermore, in step S2 of the present invention, the temperature of vacuum drying is 110-150° C. The purpose of vacuum drying is to prevent the powder from getting wet and improve the fluidity of the powder.
[0019] Furthermore, in step S3 of the present invention, the binder is composed of ethylene glycol monomethyl ether, diethylene glycol, and water in a volume ratio of 1:2:7, and the layer thickness of the binder during spraying is 0.05-0.25 mm. The main purpose of step S3 is to form the material. The main steps of jet 3D printing are: first, the drawn three-dimensional model is layered by layering software, with a layer thickness of 0.05-0.25 mm; a certain thickness of dry powder in the powder bed is evenly spread in the molding chamber by a scraper, with a thickness of 0.05-0.25 mm; then, the binder is dripped into the powder bed according to the shape after layering, and the next layer is printed after the binder penetrates to a layer thickness.
[0020] Furthermore, in step S4 of the present invention, the temperature of vacuum degreasing is 350-550°C and the vacuum degree is 10 -5 -10 -2 Pa. The main purpose of step S4 is to remove the binder in the 3D printed component.
[0021] Furthermore, in step S5 of the present invention, the vacuum degree of vacuum sintering is 10 -5 -10 -2 The vacuum sintering process is: heating from room temperature to 400°C and then keeping it for 1-2 hours, then heating to 1250-1500°C and keeping it for 4-8 hours. The main purpose of step S5 is to sinter the powder into a compact block material.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1) The present invention uses a binder to bond metal powder to produce a model shape. The temperature of the bonding process is much lower than the melting point of the metal. The metal does not melt during the additive manufacturing process. Therefore, the thermal stress is low, no thermal cracks are generated during the manufacturing process, and the forming rate is high.
[0024] 2) The present invention hardly requires the use of supports to assist the additive manufacturing process, omitting the complicated support design steps before printing and the support removal process after printing. The process is simple and can produce some hollow structures that are difficult to achieve with other additive manufacturing technologies.
[0025] 3) The composition, organization and performance of the material in the method of the present invention are easy to control. Since the powder does not melt during the additive process, the composition of the composite material can be controlled by the metal powder and the reinforcing phase components, and the parameters of the network structure can be controlled by the particle size of the metal powder and the ratio of coarse powder to fine powder, thereby controlling the performance of the material to meet the use requirements.
[0026] 4) The present invention realizes a titanium-based composite material with a network structure by regulating the powder ratio and manufacturing process: the ball milling energy used in the present invention is low, which can ensure that titanium powders of different particle sizes are mixed evenly, and the ceramic phase is wrapped on the surface of the spherical titanium powder; in the additive manufacturing process, only the bonding of the binder and the mixed powder occurs, and the sintering process is solid-phase sintering. The added ceramic powder reacts with titanium in situ to generate a reinforcing phase. This step is an exothermic reaction that is conducive to densification; the larger Ti powder core will not participate in the in-situ reaction process, so there is almost no ceramic reinforcing phase, and then a reinforcing phase depleted area is formed, and the other areas opposite to it are reinforcing phase enriched areas with a high reinforcing phase content. Therefore, only by adopting appropriate powder composition (including powder particle size, powder ratio of different particle sizes, type and content of reinforcing phase) and sintering process can the reinforcing phase be distributed in a network structure and the final sintered material be guaranteed to have a high density (using all fine titanium powders with very small particle sizes is costly and cannot design the organization, while using all large-sized titanium powders is difficult to densify).
[0027] 5) The present invention does not use lasers and sophisticated optical devices, so the equipment used is relatively low in cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings:
[0029] Figure 1 This is a metallographic diagram of the titanium-based composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0030] The present invention will be described in detail below in conjunction with specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0031] Example 1
[0032] Follow these steps to additively manufacture titanium matrix composites:
[0033] S1. 400 g of small-particle titanium powder with a particle size of 8 μm, 600 g of large-particle titanium powder with a particle size of 50 μm, 20 g of TiB2 with a particle size of 2.5 μm, and 3.3 g of graphite flakes with a particle size of 2.5 μm were put into the ball mill of a planetary ball mill. The ball mill was filled and discharged with argon gas three times and then ball milled for 5 h to obtain a mixed powder. The ball mill speed was 200 rpm, the ball-to-material ratio was 2:1, and the ball mill and the grinding balls were made of stainless steel;
[0034] S2. The mixed powder obtained in step S1 was placed in a vacuum drying oven and vacuum dried at 120°C for 4h to obtain a dry powder;
[0035] S3. The dry powder and binder obtained in step S2 are placed in a 3D printer, and the binder is sprayed to form a 3D printed component with a length of 10 mm, a width of 10 mm, and a height of 9.5 mm. The binder is composed of ethylene glycol monomethyl ether, diethylene glycol, and water in a volume ratio of 1:2:7, and the layer thickness of the binder during spraying is 0.1 mm. The main steps of spraying 3D printing are: first, the drawn three-dimensional model is layered by layering software, and the layer thickness is 0.1 mm; a certain thickness of dry powder in the powder bed is evenly spread in the molding chamber by a scraper, and the thickness is 0.1 mm; then the binder is dripped into the powder bed according to the shape after layering, and the next layer is printed after the binder penetrates to the layer thickness;
[0036] S4. Heat the 3D printed component obtained in step S3 at 400°C and 10 -2 Vacuum degreasing for 1 h at a vacuum degree of Pa to obtain a degreased 3D printed component;
[0037] S5. The degreased 3D printed component obtained in step S4 is placed in a vacuum furnace, and after vacuum sintering, the component is cooled to room temperature in the furnace to obtain a titanium-based composite material with a length of 8 mm, a width of 8 mm, and a height of 8 mm. The vacuum degree of vacuum sintering is 10 -2 Pa, the heating rate is 10℃ / min; the vacuum sintering process is: heating from room temperature to 400℃ and keeping it for 1.5h, then heating to 1250℃ and keeping it for 4h.
[0038] During the sintering process, TiB2 reacts with Ti in situ to generate fine TiB whiskers. The mass fraction of TiB is calculated to be 2.74wt% based on the mass fraction of TiB2. Graphite powder reacts with Ti in situ to generate equiaxed Ti2C particles. The mass fraction of Ti2C generated is calculated to be 2.97wt% based on the content of added graphite flakes. After sintering, the microstructure is distributed in a network, such as Figure 1 As shown. The material is divided into a reinforcement phase depleted area and a reinforcement phase enriched area, and the reinforcement phase enriched area forms a three-dimensional network structure. Taking the volume fraction of the reinforcement phase per unit area as a reference, the area below the overall density is the reinforcement phase depleted area, and the area above the overall density is the reinforcement phase enriched area. The reinforcement phase depleted area accounts for 30%, and the reinforcement enriched area accounts for 70%. After sintering, the density of the titanium-based composite material was 96.5% by image method.
[0039] Comparative Example 1
[0040] The difference from Example 1 is that no large-particle titanium powder is used in step S1, and the weight of the small-particle titanium powder is 1000 g.
[0041] Comparative Example 2
[0042] The difference from Example 1 is that small-particle titanium powder is not used in step S1, and the weight of large-particle titanium powder is 1000 g.
[0043] Comparative Example 3
[0044] The preparation steps of the cold-rolled pure titanium plate are as follows: pure titanium (alloy grade TA2) is melted by vacuum consumable arc to obtain a billet, the billet is hot forged at 800°C, and then a 15mm×15mm×120mm prism is removed by wire cutting, and the billet is placed on a rolling mill for cold rolling to obtain a cold-rolled pure titanium plate, with a rolling amount of 50%.
[0045] Experimental example: Hardness test
[0046] The hardness test method refers to the national standard GB / T 4340.1-2024 "Vickers hardness test for metallic materials Part 1: Test method", and the Vickers hardness of Example 1 and Comparative Examples 1-3 are measured respectively, with a loading force of 0.2452N.
[0047] The test results are shown in Table 1:
[0048] Vickers hardness of reinforcement phase depletion zone Vickers hardness of reinforcement phase-rich region Overall Vickers hardness Example 1 356±32 490±64 400±78 Comparative Example 1 315±22 427±36 357±56 Comparative Example 2 - - 361±23 Comparative Example 3 - - 298±21
[0049] Table 1
[0050] As can be seen from Table 1, the overall Vickers hardness of the titanium-based composite material prepared in Example 1 of the present invention is higher than that of Comparative Example 3, indicating that the introduction of the reinforcement phase brings about excellent mechanical properties. The Vickers hardness of the reinforcement phase depleted area, the Vickers hardness of the reinforcement phase enriched area, and the overall Vickers hardness of Comparative Example 1 are all lower than those of Example 1, while the reinforcement phase of Comparative Example 2 is relatively uniformly distributed, without depleted and enriched areas, and the overall Vickers hardness is not as good as that of Example 1, indicating that only using small-particle titanium powder or large-particle titanium powder cannot achieve satisfactory results.
[0051] Example 2
[0052] Follow these steps to additively manufacture titanium matrix composites:
[0053] S1. 700 g of small-particle titanium powder with a particle size of 1 μm, 300 g of large-particle titanium powder with a particle size of 180 μm, and 20 g of B4C with a particle size of 3 μm were put into the ball mill of a planetary ball mill. The ball mill was filled and discharged with argon gas three times and then ball milled for 3 h to obtain a mixed powder. The ball mill speed was 240 rpm, the ball-to-material ratio was 1:1, and the ball mill and the grinding balls were made of stainless steel;
[0054] S2. The mixed powder obtained in step S1 was placed in a vacuum drying oven and vacuum dried at 110°C for 6h to obtain a dry powder;
[0055] S3. The dry powder and binder obtained in step S2 are placed in a 3D printer, and the binder is sprayed to form a 3D printed component. The binder is composed of ethylene glycol monomethyl ether, diethylene glycol, and water in a volume ratio of 1:2:7, and the layer thickness of the binder during spraying is 0.25 mm. The main steps of spraying 3D printing are: first, the drawn three-dimensional model is layered by layering software, and the layer thickness is 0.25 mm; a certain thickness of dry powder in the powder bed is evenly spread in the molding chamber by a scraper, and the thickness is 0.25 mm; then the binder is dripped into the powder bed according to the shape after layering, and the next layer is printed after the binder penetrates to the layer thickness;
[0056] S4. Heat the 3D printed component obtained in step S3 at 350°C and 10 -5 Vacuum degreasing for 0.5 h at a vacuum degree of Pa to obtain a degreased 3D printed component;
[0057] S5. The degreased 3D printed component obtained in step S4 is placed in a vacuum furnace, and after vacuum sintering, the component is cooled to room temperature in the furnace to obtain a titanium-based composite material. The vacuum degree of vacuum sintering is 10 -5 Pa, the heating rate is 10℃ / min; the vacuum sintering process is: heating from room temperature to 400℃ and keeping it for 1h, then heating to 1400℃ and keeping it for 8h.
[0058] Example 3
[0059] Follow these steps to additively manufacture titanium matrix composites:
[0060] S1. 500g of small-particle titanium powder with a particle size of 15μm, 500g of large-particle titanium powder with a particle size of 35μm, and 50g of TiB2 with a particle size of 0.2μm were put into the ball mill of a planetary ball mill. The ball mill was filled and discharged with argon gas three times and then ball milled for 4h to obtain a mixed powder. The ball mill speed was 180rpm, the ball-to-material ratio was 5:1, and the ball mill and the grinding balls were made of stainless steel;
[0061] S2. The mixed powder obtained in step S1 is placed in a vacuum drying oven and dried under vacuum at 150°C for 3h to obtain a dry powder;
[0062] S3. The dry powder and binder obtained in step S2 are placed in a 3D printer, and the binder is sprayed to form a 3D printed component. The binder is composed of ethylene glycol monomethyl ether, diethylene glycol, and water in a volume ratio of 1:2:7. The layer thickness of the binder during spraying is 0.05 mm. The main steps of spraying 3D printing are: first, the drawn three-dimensional model is layered by layering software, and the layer thickness is 0.05 mm; a certain thickness of dry powder in the powder bed is evenly spread in the molding chamber by a scraper, and the thickness is 0.05 mm; then the binder is dripped into the powder bed according to the shape after layering, and the next layer is printed after the binder penetrates to the layer thickness;
[0063] S4. Heat the 3D printed component obtained in step S3 at 550°C and 10 -3 Vacuum degreasing for 1.5 h at a vacuum degree of Pa to obtain a degreased 3D printed component;
[0064] S5. The degreased 3D printed component obtained in step S4 is placed in a vacuum furnace, and after vacuum sintering, the component is cooled to room temperature in the furnace to obtain a titanium-based composite material. The vacuum degree of vacuum sintering is 10 -3 Pa, the heating rate is 10℃ / min; the vacuum sintering process is: heating from room temperature to 400℃ and keeping it for 2h, then heating to 1500℃ and keeping it for 6h.
[0065] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for additive manufacturing of a titanium-based composite material, characterized in that: The following steps are involved: S1. The titanium powder and the reinforcing phase raw material were put into the ball mill of a planetary ball mill, and the ball mill was filled with argon gas three times and then milled for 3-5h to obtain a mixed powder; S2. Place the mixed powder obtained in step S1 in a vacuum drying oven and vacuum dry for 3-6h to obtain a dry powder; S3. placing the dry powder and binder obtained in step S2 in a 3D printer, spraying the binder for 3D printing to obtain a 3D printed component; S4. Vacuum degreasing the 3D printed component obtained in step S3 for 0.5-1.5h to obtain a degreased 3D printed component; S5. Place the degreased 3D printed component obtained in step S4 in a vacuum furnace, and after vacuum sintering, cool it to room temperature in the furnace to obtain a titanium-based composite material.
2. The additive manufacturing method of a titanium-based composite material according to claim 1, characterized in that: In the step S1, the weight ratio of titanium powder and reinforcing phase raw material is 1:(0.02-0.05); the titanium powder is composed of small-particle titanium powder and large-particle titanium powder in a weight ratio of 4:6 to 7:3, wherein the particle size of the small-particle titanium powder is 1-15 μm, and the particle size of the large-particle titanium powder is 35-180 μm; the reinforcing phase raw material is one of B4C, TiB2 or graphite flakes with a particle size of 0.2-3 μm.
3. The additive manufacturing method of a titanium-based composite material according to claim 1, characterized in that: In the step S1, the ball milling speed is 180-240 rpm, the ball-to-material ratio is 1:1-5:1, and the ball milling jar and the grinding balls are made of stainless steel.
4. The additive manufacturing method of a titanium-based composite material according to claim 1, characterized in that: In step S2, the vacuum drying temperature is 110-150°C.
5. The additive manufacturing method of a titanium-based composite material according to claim 1, characterized in that: In the step S3, the binder is composed of ethylene glycol monomethyl ether, diethylene glycol and water in a volume ratio of 1:2:7, and the layer thickness of the binder during spraying is 0.05-0.25 mm.
6. The additive manufacturing method of a titanium-based composite material according to claim 1, characterized in that: In step S4, the vacuum degreasing temperature is 350-550°C and the vacuum degree is 10 -5 -10 -2 Pa.
7. The additive manufacturing method of a titanium-based composite material according to claim 1, characterized in that: In step S5, the vacuum degree of vacuum sintering is 10 -5 -10 -2 Pa, the heating rate is 10℃ / min; the vacuum sintering process is: heating from room temperature to 400℃ and keeping warm for 1-2h, then heating to 1250-1500℃ and keeping warm for 4-8h.
Citation Information
Patent Citations
Low-cost titanium alloy indirect additive manufacturing method
CN111347048A
Method for preparing titanium-based workpiece based on micro spherical titanium-based powder and titanium-based workpiece
CN114682778A
Method for printing titanium alloy through binder
CN116237538A
Titanium-based composite material based on SLM process as well as preparation method and application of titanium-based composite material
CN116673496A
Quasi-continuous reticular titanium-based composite material based on additive manufacturing and preparation method of quasi-continuous reticular titanium-based composite material
CN117161401A
Cited By
Medical degradable metal zinc alloy, manufacturing method and application
CN120362512A