A waterless disperse dye printing process for polyester fabrics

By introducing a crosslinking reaction between vinyl-modified sodium lignin sulfonate and guanidine salt into polyester fabrics, the problems of high energy consumption, pollution, poor color fastness, and stiff hand feel in digital inkjet printing of polyester fabrics have been solved, achieving waterless, zero-emission, and high-definition printed finished products, and simplifying the process.

CN123108959APending Publication Date: 2026-11-17杭州达峪科技有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611274027.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing digital inkjet printing technology for polyester fabrics suffers from problems such as high energy consumption and pollution, poor color fastness, stiff hand feel, complex processes, and high equipment requirements. In particular, it is difficult to achieve high color fastness and soft hand feel under waterless washing conditions.

Method used

Vinyl-modified sodium lignosulfonate is used as the crosslinking functional component in the ink. It undergoes a two-phase crosslinking reaction with guanidine salt or cationic polymer pretreated slurry at high temperature to form a three-dimensional crosslinking network, which fixes the dye inside the fiber and avoids the water washing step.

Benefits of technology

It achieves waterless, zero-emission, and high-definition printed finished products, while maintaining high color fastness and a soft hand feel, simplifying the process and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention belongs to the field of digital printing and green dyeing and finishing technology for textiles, specifically involving a waterless disperse dye printing process for polyester fabrics. The process mainly includes: (1) pre-treating the polyester fabric with a guanidine salt sizing agent by padding; (2) padding; (3) drying; (4) digital printing with disperse dye printing ink; (5) pre-drying; and (6) baking to fix the color. The finished digitally printed polyester fabric can be obtained without washing. Addressing the problems of existing traditional processes requiring washing, high energy consumption, and heavy pollution; and existing waterless processes having poor color fastness, a stiff hand feel, complex processes, and high costs, this invention simplifies the process flow, eliminating water washing and achieving zero emissions. It solves the technical contradiction of the incompatibility between color fastness and hand feel in existing waterless processes, achieving a balance between high color fastness and a soft hand feel, and obtaining high print clarity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of digital printing and green dyeing and finishing technology for textiles, specifically relating to a waterless disperse dye printing process for polyester fabrics. Background Technology

[0002] Digital inkjet printing on polyester fabrics mainly uses disperse dye inks, and existing technologies have the following main problems: (i) Traditional processes require water washing, resulting in high energy consumption and heavy pollution. Traditional disperse dye printing processes require washing the fabric after high-temperature color fixing to remove unfixed dyes and auxiliaries. This process consumes a large amount of water resources and discharges wastewater containing chemical residues, which does not meet the requirements of green manufacturing.

[0003] (II) Poor colorfastness and stiff hand feel in waterless washing processes. Although existing waterless washing processes improve diffusion by grinding powdered disperse dyes into nano-sized liquid disperse dyes, poor colorfastness still exists. Printing and dyeing plants typically use printing adhesives in conjunction with these processes, but this has two major drawbacks: when the adhesive is added to the disperse dye paste for co-printing, the adhesive's coating of the dye is insufficient, resulting in poor colorfastness; increasing the amount used leads to a stiffer hand feel. Printing the disperse dye first and then padding with the adhesive before finishing also results in a noticeably stiffer hand feel. The colorfastness and hand feel of printed fabrics produced by either of these methods do not reach the levels of traditional water-washing processes.

[0004] (iii) Pre-treatment to prevent ink seepage is required, and the process is cumbersome. Polyester fabrics have a smooth surface and few polar groups, making it easy for ink droplets to spread along the capillary movement between fibers, resulting in unclear outlines of the printed pattern. Existing technologies usually require pre-treatment of polyester fabrics, such as plasma treatment, high-energy ray treatment, and polyvinyl alcohol treatment, which increases the complexity and cost of the process.

[0005] (iv) Existing waterless ink solutions have limitations. Some existing solutions use temperature-viscosity responsive direct-injection thermosensitive disperse dye inks that do not require pretreatment, but these require heating to a specific temperature using a heating pad, which increases equipment requirements; others use cationic reagents in combination with anionic ink systems, but the color fastness problem under waterless conditions has not yet been solved.

[0006] (v) Limitations of existing technical literature. Existing patent literature, such as the invention patent of Zhejiang Yingfeng Technology with publication number CN118599337A and publication date September 6, 2024, adopts a scheme that introduces vinyl groups into both ink dispersants and pretreatment agents to achieve two-phase crosslinking in the steaming stage. However, its technical solution requires steam fixing, which has high equipment requirements. Another example is the invention patent of Nantong New Century Textile with publication number CN120925340A and publication date November 11, 2025, which uses guanidine salt pretreatment agents to achieve reduction-free cleaning. However, its pretreatment agents are mainly composed of guanidine salts, β-cyclodextrin, pH adjusters, and nonionic thickeners. The ink side is a high-temperature dispersed ink containing ordinary anionic dispersants. It does not introduce crosslinkable vinyl functional monomers, nor does it disclose the synergistic crosslinking mechanism between ink and slurry and the corresponding comparative verification. Summary of the Invention

[0007] To address the shortcomings and deficiencies of the existing technologies, the present invention aims to provide a waterless disperse dye printing process for polyester fabrics, applicable to digital direct-to-garment printing. This process enables the production of printed products that meet colorfastness requirements without the need for washing or reduction cleaning after printing, achieving both high colorfastness and a soft hand feel. It simplifies the process flow, achieving waterless printing and zero emissions, and yields high-definition printed products.

[0008] To achieve the objective of this invention, the inventors provide the following technical solution: This invention provides a waterless disperse dye printing process for polyester fabrics, mainly including the following steps: (1) Polyester fabric is pretreated and sized by padding. Padding provides better uniformity. The amount of pretreatment sizing agent applied needs to be adjusted according to the fabric weight, with a suitable increase for heavy and thick fabrics. The composition of the pretreatment sizing agent formula by mass percentage is: guanidine salt 5-20%; thickener 0.5-3%; deionized water balance. Guanidine salt is the main component of the sizing agent, which inhibits ink bleeding. Thickener adjusts the viscosity of the sizing agent. Deionized water is used as the solvent for the sizing agent. Guanidine salt can significantly reduce the mobility of disperse dyes in the ink, and the ink droplets printed on it will not spread along the fabric capillary, making the printed pattern clear. Polyester fabric pretreated with guanidine salt does not require reduction washing and water washing after baking and color development by direct-to-garment printing with high-temperature disperse dye ink.

[0009] (2) Roll dry, with a roll residue of 55-65%; preferably 60%. Too high a roll residue will affect the feel, while too low a roll residue will affect the firmness.

[0010] (3) Drying: Dry at 100-120℃ for 2-3 minutes; (4) Digital inkjet printing, using disperse dye printing ink. The formulation of disperse dye printing ink is shown in the table below: From this table, it can be seen that the disperse dye printing ink consists of the following final components by mass percentage: Disperse dye 2.0-4.2%; used after nano-grinding. The technical solution of the present invention is illustrated by CI Disperse Blue 79 as a typical example in the examples. It can be understood that disperse dyes similar to CI Disperse Blue 79, such as CI Disperse Blue 301, Disperse Blue SF-RG, etc., can be used as substitutes and achieve the purpose of the invention.

[0011] Vinyl-modified sodium lignosulfonate 1.25-5.25%; Moisturizer 10-20%; Viscosity modifier 0-0.7%; Surfactant 0.2-0.6%; pH adjuster 0.02-0.07%; Defoamer 0.1-0.3%; Deionized water balance (5) Pre-drying: Dry at 100-120℃ for 1-2 minutes; preferably 110℃ for 2 minutes. This process removes moisture and prevents migration.

[0012] (6) Baking for color fixation: Treat the product at 180-195℃ for 5-7 minutes. No washing is required to obtain the finished product. The preferred temperature is 185℃ for 7 minutes. This process ensures complete cross-linking reaction.

[0013] This invention achieves waterless digital disperse printing of polyester through the synergistic effect of ink formulation and matching paste, and also eliminates the need for steam fixing. The entire process requires no washing or reduction cleaning, achieving zero wastewater discharge. The core technology of this invention lies in the two-phase cross-linking mechanism of ink and paste, the core idea of ​​which is as follows: On the ink side: a cross-linkable functional component—a vinyl-modified dispersant, such as the vinyl-modified sodium lignosulfonate used in this invention—is introduced into the ink system. The dispersant carries vinyl reactive functional groups, which cause it to undergo a cross-linking reaction with the slurry during the baking stage, thus "locking" the dye inside and on the surface of the fiber.

[0014] On the slurry side: design pretreated slurries containing guanidine salts or cationic polymers. Guanidine salts or cationic polymers provide reaction sites (active groups such as amino and hydroxyl groups), which can both prevent ink bleeding and provide cross-linking reaction sites to promote dye fixation.

[0015] Synergistic mechanism: During the baking stage (180–195℃), the vinyl groups in the ink and the active groups in the paste undergo a two-phase cross-linking polymerization reaction to form a three-dimensional cross-linking network structure, which anchors the disperse dye molecules inside and on the surface of the fiber. The unfixed floating dye is fixed in situ by the cross-linking network and cannot migrate to the fiber surface, thus achieving efficient fixation of the dye and in-situ fixation of the floating dye.

[0016] No-wash principle: Since the floating dye is fixed by the cross-linking network and the dye has been fully applied to the inside of the fiber, satisfactory color fastness can be achieved without washing to remove the floating dye.

[0017] Preferably, in this invention, the guanidine salt in process step (1) is polyhexamethylene biguanide hydrochloride.

[0018] Preferably, in this invention, the humectant in step (4) is selected from one or more of ethylene glycol, propylene glycol, diethylene glycol or glycerin.

[0019] Preferably, in this invention, the surfactant in process step (4) is an acetylenic diol nonionic surfactant.

[0020] Preferably, in this invention, the vinyl-modified sodium lignin sulfonate in step (4) is obtained according to the following preparation method: (a) Weigh out sodium lignosulfonate and dissolve it in a solvent, wherein the solvent is derived from at least one of ethanol, water, N,N-dimethylformamide, chloroform, and dimethyl sulfoxide; (b) Add alkali, such as NaOH or KOH, and stir to dissolve under an inert atmosphere; (c) Add vinyl ethylene oxide to initiate a ring-opening reaction at 60–80°C for 24–36 h; the mass ratio of feed materials is: sodium lignosulfonate: vinyl ethylene oxide: alkali = 1:0.2–0.4:0.02. (d) After the reaction is completed, the reaction solution is purified and dried to obtain vinyl-modified sodium lignosulfonate.

[0021] Preferably, in this invention, the ink properties in step (4) satisfy the following: The zeta potential is -40 to -56 mV; the surface tension is 30-35 mN / m; the viscosity is 1.5-2.2 mPa•s; the conductivity is 6-7 μS / cm; and the pH value is 7-9. The ink's physical properties meet the requirements of digital printheads, and it has good printhead compatibility.

[0022] Preferably, in this invention, the average particle size D of the disperse dye in step (4) is... 50 The particle size distribution ranges from 100 to 300 nm; the particle size dispersibility index (PDI) is 0.2 to 0.5.

[0023] Compared with the prior art, the beneficial effects of the present invention are: (1) No water washing and zero discharge: The digital printing of polyester is water-free, eliminating the washing and restoration cleaning processes after printing, simplifying the process flow, greatly reducing water consumption, and achieving zero wastewater discharge.

[0024] (2) Balancing high color fastness and soft hand feel: This invention resolves the technical contradiction in existing waterless washing processes where color fastness and hand feel are mutually exclusive. Excellent color fastness: After cross-linking and fixation, the color fastness of printed fabrics can reach or exceed the level of traditional water-washing processes—both the color fastness to rubbing and the color fastness to soaping can reach level 4. Soft hand feel: Unlike traditional waterless washing solutions with high adhesive usage, this invention achieves color fixation through chemical cross-linking, resulting in printed fabrics with a soft hand feel.

[0025] (3) High printing clarity: The guanidine salt in the paste effectively prevents ink bleeding, ensuring clear outlines and no bleeding of the printed pattern without adding complicated pretreatment processes.

[0026] (4) The process of the present invention can improve the dye uptake rate and fixation rate: through the synergistic design of ink and paste, the dye can be efficiently uptaken and firmly fixed during the baking stage.

[0027] (5) Simplified process flow: A short process of waterless printing, namely “printing → drying → baking → finished product”, is realized, which greatly improves production efficiency. Detailed Implementation

[0028] The present invention will be described in more detail below with reference to the embodiments. It should be understood that the implementation of the present invention is not limited to the embodiments below, and any modifications and / or alterations made to the present invention will fall within the protection scope of the present invention.

[0029] In this invention, unless otherwise specified, all parts and percentages are by weight, and all equipment and raw materials are commercially available or commonly used in the industry. Unless otherwise specified, the methods used in the embodiments are general techniques in the art.

[0030] Description of main raw materials in the embodiments: The vinyl-modified sodium lignosulfonate in the examples was obtained according to the following preparation method: (a) Weigh out sodium lignosulfonate and dissolve it in a solvent, wherein the solvent is derived from at least one of ethanol, water, N,N-dimethylformamide, chloroform, and dimethyl sulfoxide; (b) Add alkali, such as NaOH or KOH, and stir to dissolve under an inert atmosphere; (c) Add vinyl ethylene oxide to initiate a ring-opening reaction at 60–80°C for 24–36 h; the mass ratio of feed materials is: sodium lignosulfonate: vinyl ethylene oxide: alkali = 1:0.2–0.4:0.02. (d) After the reaction is completed, the reaction solution is purified and dried to obtain vinyl-modified sodium lignosulfonate.

[0031] Example 1 1. Prepare the pretreatment paste and ink for the printing process according to the formula. ①Slurry formulation: Polyhexamethylene biguanide hydrochloride: 15 wt% Sodium carboxyethyl cellulose (thickener): 2 wt%. Deionized water: Balance.

[0032] ②Ink formula: The ink's physical properties, as tested, are as follows: The zeta potential is -47 mV; the surface tension is 30 mN / m; the viscosity is 1.8 mPa•s; the conductivity is 6.4 μS / cm; and the pH value is 7.5. The ink's physical properties meet the requirements of digital printheads, and it exhibits good printhead compatibility.

[0033] II. The process is as follows: polyester greige fabric → pretreatment sizing (paddling, using the sizing agent of this invention) → padding (residual rate 55-65%) → drying (100-120℃×2-3min) → digital inkjet printing (using the ink of this invention) → pre-drying (100-120℃×1-2min) → baking and color fixing (180-195℃×5-7min) → finished product (printing can be achieved without washing).

[0034] The main process parameters for printing are: Sizing method: padding, roll-out rate 60%. Drying: 120℃ × 2 min Pre-baking: 110℃ × 2 min, Printing: Industrial-grade printheads are used. Baking: 185℃ × 7 min.

[0035] III. Relevant tests were conducted on the finished waterless printed polyester fabrics, and the results are shown in Tables 1-3.

[0036] Example 2 1. Prepare the pretreatment paste and ink for the printing process according to the formula. ①Slurry formulation: Polyhexamethylene biguanide hydrochloride: 20 wt% Sodium carboxyethyl cellulose (thickener): 3 wt%. Deionized water: Balance.

[0037] ②Ink formula: The ink's physical properties, as tested, are as follows: The zeta potential is -50mV; the surface tension is 32mN / m; the viscosity is 2.0mPa•s; the conductivity is 7μS / cm; and the pH value is 7. The ink's physical properties meet the requirements of digital printheads, and it exhibits good printhead compatibility.

[0038] II. The process is as follows: polyester greige fabric → pretreatment sizing (pad-drying, using the sizing agent of this invention) → pad-drying (55-65% pad-drying rate) → drying (100-120℃×2-3min) → digital inkjet printing (using the ink of this invention) → pre-baking (100-120℃×1-2min) → baking and color fixing (180-195℃×5-7min) → finished product (printing is achieved without water washing). The main process parameters for printing are: Sizing method: padding, roll-out rate 60%. Drying: 120℃ × 2 min Pre-baking: 110℃ × 2 min, Printing: Industrial-grade printheads are used. Baking: 185℃ × 7 min.

[0039] III. Relevant tests were conducted on the finished waterless printed polyester fabrics, and the results are shown in Tables 1-3.

[0040] Example 3 1. Prepare the pretreatment paste and ink for the printing process according to the formula. ①Slurry formulation: Polyhexamethylene guanidine hydrochloride: 8wt% Sodium carboxyethyl cellulose (thickener): 0.6 wt%. Deionized water: Balance.

[0041] ②Ink formula: The ink's physical properties, as tested, are as follows: The zeta potential is -50 mV; the surface tension is 30 mN / m; the viscosity is 1.7 mPa•s; the conductivity is 6.5 μS / cm; and the pH value is 7.2. The ink's physical properties meet the requirements of digital printheads, and it exhibits good printhead compatibility.

[0042] II. The process is as follows: polyester greige fabric → pretreatment sizing (pad-drying, using the sizing agent of this invention) → pad-drying (55-65% pad-drying rate) → drying (100-120℃×2-3min) → digital inkjet printing (using the ink of this invention) → pre-baking (100-120℃×1-2min) → baking and color fixing (180-195℃×5-7min) → finished product (printing is achieved without water washing). The main process parameters for printing are: Sizing method: padding, roll-out rate 60%. Drying: 120℃ × 2 min Pre-baking: 110℃ × 2 min, Printing: Industrial-grade printheads are used. Baking: 185℃ × 7 min.

[0043] III. Relevant tests were conducted on the finished waterless printed polyester fabrics, and the results are shown in Tables 1-3.

[0044] Performance testing The waterless printed polyester fabric of the present invention was tested according to relevant standards. The test results for dry rubbing fastness, wet rubbing fastness, washing fastness, and print clarity are as follows: I. Colorfastness to rubbing: According to the test method in GB / T 3920-2008 "Textiles - Tests for colorfastness to rubbing", the adhesion of dye to the fabric is mainly evaluated through a standardized rubbing process. A major feature of waterless printing is that it eliminates the traditional post-printing washing process, thus placing higher demands on colorfastness.

[0045] (1) Test method ①Prepare samples: Cut at least two samples with a size of 50mm×140mm, one for dry friction and one for wet friction.

[0046] ②Prepare the friction cloth: Use a 50mm×50mm square cotton friction cloth that conforms to the standard (GB / T 7568.2). Dry friction cloth can be used directly, while wet friction cloth needs to be soaked in distilled water and then taken out to control its moisture content between 95% and 100%.

[0047] ③ Instrument Setup: Lay the sample flat and fix it on the test platform of the friction instrument. Wrap the friction cloth around the friction head and lower the support so that the friction head presses vertically onto the sample. Set the key parameters of the instrument. Friction head pressure: downward pressure is (9 ± 0.2) N; reciprocating stroke linear stroke is (104 ± 3) mm; friction speed: (60 ± 2) reciprocating motions per minute; number of friction cycles: 10.

[0048] ④ Operation test: Start the instrument and let the friction head complete 10 reciprocating friction cycles under the specified parameters.

[0049] (2) Result evaluation: After the test, the rubbing cloth is compared with the staining gray scale of GB / T 251 to evaluate its staining level. The results are divided into 1-5 levels, with level 5 being the best and level 1 being the worst. If the sample is a printed fabric, the test should be conducted at a position where the rubbing head can simultaneously rub multiple colors.

[0050] II. Color fastness to washing / soap washing: The test is conducted according to GB / T 3921-2008 "Textiles - Tests for color fastness to washing". The core principle is to sew the sample to a standard lining fabric and mechanically agitate and wash it in a specific soap solution. The color fastness is measured by evaluating the color change of the sample and the staining of the lining.

[0051] (1) Test method: ① Cut a 40mm×100mm sample from the fabric.

[0052] ② Sew the front of the sample to a standard lining fabric of the same size along one short side. The lining can be a multifiber fabric (usually more convenient), or a single-fiber lining fabric of polyester and cotton can be selected specifically.

[0053] ③ Place the combined samples into a wash fastness tester, wash them in soap solution at a specific temperature, and then rinse and dry them. Finally, use a gray scale to assess the color change of the samples and the staining grade of the lining.

[0054] (2) Result evaluation: The grades are divided into 1-5, with 5 being the best and 1 being the worst.

[0055] Third, regarding print clarity, there is currently no unified mandatory national standard. However, in academic research and industrial applications, a comprehensive evaluation system combining subjective assessment and objective testing has been established.

[0056] Subjective evaluation: A group of trained observers (such as those without color blindness or color weakness) were organized to score the printed straight lines with a design line width of 0.4 mm under a D65 standard light source. Sharp edges, no burrs, and no blurring were rated as "excellent".

[0057] Objective evaluation: Images are acquired using a high-precision scanner (≥2400 dpi) or a stereomicroscope. The actual line width W1 is measured, and the line width expansion rate η = (W1−W0) / W0×100%, where W0 is the designed line width. η≤10% is judged as "basically no bleed," and η≤5% is judged as "no bleed at the line edge."

[0058] In addition to the contents disclosed in Table 4, this invention achieves comprehensive balance in terms of waterless washing, high color fastness, and soft hand feel, while the technical solutions of Yingfeng Technology (CN118599337A) and Nantong New Century Textile (CN120925340A) only partially achieve these aspects. Regarding printhead compatibility data, this invention discloses complete physical property parameters, while neither Yingfeng Technology (CN118599337A) nor Nantong New Century Textile (CN120925340A) has disclosed such data. In terms of ink + paste synergistic crosslinking, Yingfeng Technology (CN118599337A) requires steam (100-102℃ saturated steam) to trigger the process, which has high equipment requirements, increases equipment investment and energy consumption, and limits the continuity of the process; Nantong New Century Textile (CN120925340A) does not address this; this invention only requires baking to achieve the desired result, lowering the application threshold.

[0059] It should be noted that the above embodiments are merely preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any equivalent substitutions, improvements, or adjustments made to the raw material composition, proportions, or preparation steps of the present invention under the guidance of the formulation system and core ideas of the present invention shall still fall within the scope of protection covered by the claims of the present invention.

Claims

1. A waterless disperse dye printing process for polyester fabrics, characterized in that... The main processes include the following steps: (1) The polyester fabric is pretreated by padding and sizing, wherein: the composition of the pretreatment sizing formula is as follows by mass percentage: guanidine salt 5-20%, thickener 0.5-3% and deionized water balance; (2) Roll dry, with a residual rate of 55-65%; (3) Drying: Dry at 100-120℃ for 2-3 minutes; (4) Digital inkjet printing: The disperse dye printing ink used consists of the following final components by weight percentage: disperse dye 2.0-4.2%, vinyl-modified sodium lignosulfonate 1.25-5.25%, humectant 10-20%, viscosity modifier 0-0.7%, surfactant 0.2-0.6%, pH adjuster 0.02-0.07%, defoamer 0.1-0.3%, and deionized water as the balance. (5) Pre-drying: Dry at 100-120℃ for 1-2 minutes; (6) Baking and color fixing: fix the color at a temperature of 180-195℃ for 5-7 minutes. The finished product can be obtained without washing.

2. The waterless disperse dye printing process for polyester fabrics according to claim 1, characterized in that, The guanidine salt used in step (1) is polyhexamethylene biguanide hydrochloride.

3. The waterless disperse dye printing process for polyester fabrics according to claim 1, characterized in that, The humectant in step (4) is selected from one or more of ethylene glycol, propylene glycol, diethylene glycol or glycerin.

4. The waterless disperse dye printing process for polyester fabrics according to claim 1, characterized in that, The surfactant used in step (4) is an acetylenic diol nonionic surfactant.

5. The waterless disperse dye printing process for polyester fabrics according to claim 1, characterized in that, The vinyl-modified sodium lignosulfonate in step (4) is obtained according to the following preparation method: (a) Weigh out sodium lignosulfonate and dissolve it in a solvent, wherein the solvent is derived from at least one of ethanol, water, N,N-dimethylformamide, chloroform, and dimethyl sulfoxide; (b) Add alkali, such as NaOH or KOH, and stir to dissolve under an inert atmosphere; (c) Add vinyl ethylene oxide to initiate a ring-opening reaction at 60–80°C for 24–36 h; the mass ratio of feed materials is: sodium lignosulfonate: vinyl ethylene oxide: alkali = 1:0.2–0.4:0.

02. (d) After the reaction is completed, the reaction solution is purified and dried to obtain vinyl-modified sodium lignosulfonate.

6. The waterless disperse dye printing process for polyester fabrics according to claim 1, characterized in that, The ink properties in process step (4) satisfy the following requirements: The zeta potential is -40 to -56 mV; the surface tension is 30-35 mN / m; the viscosity is 1.5-2.2 mPa•s; the electrical conductivity is 6-7 μS / cm; and the pH value is 7-9.

7. The waterless disperse dye printing process for polyester fabrics according to claim 1, characterized in that, The average particle size of the disperse dye in process step (4) is 100-300 nm; the particle size dispersibility index (PDI) is 0.2-0.5.

Citation Information

Patent Citations

  • Washing-free disperse dye printing ink and printing process thereof

    CN118599337A

  • Polyester fabric and reduction-cleaning-free ink-jet printing method thereof

    CN120925340A