A green, environmentally friendly, and biodegradable cigarette tipping paper and its production method
By using a three-layer coating structure and combining citrate and calcium ion crosslinking, the problems of moisture resistance stability and rapid disintegration after disposal of cigarette tipping paper in a short period of time are solved, thus realizing the production of environmentally friendly and biodegradable cigarette tipping paper.
Patent Information
- Application Number
- CN202611367208.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cigarette tipping paper is difficult to maintain moisture resistance and stability in a short period of time, and it rapidly hydrolyzes after being discarded. Existing technical solutions cannot balance normal performance and environmental friendliness.
The coating employs a three-layer structure, including a first coating containing citrate, a second coating containing oxidized starch, and a third coating containing calcium ion-crosslinked alginate. By controlling the spatial arrangement and material composition of the coatings, the migration of citrate under different conditions is achieved, and the crosslinking state of the coatings is adjusted, thereby maintaining stability during normal use and promoting disintegration after disposal.
It achieves the ability to maintain the wet stability of cigarette tipping paper in a short period of time, while rapidly disintegrating it after disposal, reducing the environmental burden. It is suitable for existing production equipment and takes into account both performance and environmental protection requirements.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention relates to the field of cigarette packaging materials and functional paper processing technology, specifically to a green, environmentally friendly, and biodegradable cigarette tipping paper with a layered coating structure and its production method. Background Technology
[0002] Cigarette tipping paper is used to connect the filter to the cigarette and cover the outer perimeter of the filter. During production and use, tipping paper typically needs to meet requirements for printability, rewinding and slitting suitability, splicing suitability, surface abrasion resistance, and a certain degree of wet stability. Especially during cigarette use, the end of the tipping paper closest to the lips may come into contact with saliva. If the coating on the tipping paper's surface lacks sufficient moisture resistance, problems such as decreased strength, surface stickiness, ink peeling, or paper layer damage can easily occur. Therefore, existing tipping papers typically improve their stability during processing, storage, and use by enhancing the continuity, density, or water resistance of the surface coating.
[0003] While the aforementioned moisture-resistant treatment is beneficial for the normal use of tipping paper, the continuous and relatively stable coating restricts the penetration of environmental moisture into the base paper fibers after the tipping paper is discarded. This allows the paper to maintain its integrity for a longer period in damp, rainy, or soiled environments, thus delaying paper disintegration and subsequent biodegradation. When tipping paper covers the outer periphery of the filter, it may also constrain the filter material to some extent, making it less likely for discarded cigarette butts to loosen and reducing the contact between the filter material and moisture, air, and microorganisms.
[0004] To address the aforementioned issues, existing technologies propose improving the environmental degradation performance of tobacco materials by employing biodegradable raw materials, hydrophilic coatings, water-sensitive adhesives, or water-dispersible materials. These solutions typically increase the hydrophilicity or water sensitivity of the material itself, causing it to swell, dissolve, or decrease in strength upon contact with water. However, tipping paper may also come into contact with moisture during normal use. Simply increasing the hydrophilicity of the material can easily cause the tipping paper to soften prematurely under conditions of short-term saliva contact, high humidity storage, or splicing, making it difficult to maintain the wet stability required for normal use. Conversely, further increasing the water resistance and cross-linking degree of the coating would reduce the rate at which moisture penetrates the paper layer after disposal, making it difficult for the tipping paper to disintegrate quickly.
[0005] Anionic polysaccharides such as alginate and low-methoxyl pectin can form ionic cross-linked structures under the action of calcium ions, resulting in materials with a certain degree of wet integrity. Citrate can coordinate with calcium ions and can therefore also be used to regulate the calcium ion-involved cross-linking process. However, in typical material processing, direct blending of citrate with alginate and calcium salts may affect the normal formation of the cross-linked structure, resulting in insufficient initial moisture resistance of the coating; if the two are completely isolated, it is difficult to produce the corresponding effect in the waste environment. Current technology lacks a structural design suitable for continuous coating production of tipping paper, which keeps interacting substances separated during production, storage, and short-term oral contact, while gradually contacting them under continuous wetting or repeated wet-drying conditions, thereby transforming the tipping paper from a stable structure in the use state to a structure that is easily disintegrated.
[0006] Therefore, there is a need for a new cigarette tipping paper that balances short-term moisture resistance and post-disposal water dispersibility without sacrificing normal performance, and that can be produced using existing gravure printing, coating, drying, rewinding and slitting equipment. Summary of the Invention
[0007] In view of this, the present invention proposes a green, environmentally friendly, and biodegradable cigarette tipping paper and its production method to solve the problem that existing tipping papers cannot simultaneously achieve short-term moisture resistance and rapid hydrolysis after disposal.
[0008] The technical solution of this invention is implemented as follows: This invention provides a green, environmentally friendly, and biodegradable cigarette tipping paper, comprising tipping paper base paper. At least one surface of the tipping paper base paper is sequentially coated with a first coating, a second coating, and a third coating in a direction away from the tipping paper base paper. The first coating covers a portion of the surface of that one side of the tipping paper base paper, such that the surface includes a coated area covered by the first coating and an uncoated area not covered by the first coating. The first coating contains citrate and oxidized starch. The citrate is selected from at least one of sodium citrate, potassium citrate, and ammonium citrate. The dry coating weight of the first coating is 0.08–0.35 g / m³. 2 The second coating contains oxidized starch and shellac, and covers the first coating and the uncoated area. The dry coating weight of the second coating is 0.20–0.70 g / m². 2 The third coating covers the outer surface of the second coating. The third coating contains calcium-crosslinked alginate and low-methoxyl pectin. The dry coating weight of the third coating is 0.60–1.40 g / m². 2The dry coating amount of the first, second, and third coatings is based on the total area of one side surface of the tipping paper base paper. The amount of calcium per unit area in the third coating is determined by subtracting the background calcium amount of an equal area of uncoated tipping paper base paper from the total calcium amount measured by acid digestion of the finished tipping paper, and then converting it according to the total area of one side surface. The ratio of the amount of citrate per unit area in the first coating to the amount of calcium per unit area in the third coating is 0.40 to 1.50:1. The amount of citrate per unit area is also based on the total area of one side surface of the tipping paper base paper.
[0009] The first, second, and third coatings are arranged in the order described above. The first coating is applied only to a portion of the surface of the base paper on one side. The second coating covers the first coating and the portion of the base paper not covered by the first coating, thereby separating the citrate in the first coating from the third coating and regulating the entry of moisture and the migration of citrate from the first coating to the third coating. The third coating covers the second coating, where alginate and low-methoxyl pectin form a cross-linked structure through calcium ions, constituting a wet protective layer on the outer side of the tipping paper.
[0010] Under normal storage and short-term exposure to moisture, the second coating restricts the migration of citrate from the first coating to the third coating, allowing the third coating to maintain a relatively intact calcium ion cross-linking structure. During continuous wetting or repeated wet-drying processes, moisture gradually enters the first coating, causing citrate to dissolve and migrate through the second coating to the third coating. Once in the third coating, citrate alters the state of calcium ions, gradually weakening the ion cross-linking structure and promoting further penetration of moisture into the tipping paper base paper.
[0011] It should be noted that the above-described process is used to help understand the interaction between the layers of the present invention and does not constitute a limitation on the scope of protection of the present invention. The technical effect of the present invention is mainly produced by the spatial arrangement of the first, second and third coatings, the material composition of each layer, the dry coating amount of each layer, and the molar relationship between citrate and calcium per unit area, rather than by any single component or single parameter independently.
[0012] In some embodiments, the tipping paper base paper is made primarily of plant fibers. The tipping paper base paper can be made from wood pulp fiber, bamboo pulp fiber, hemp pulp fiber, or a combination thereof. The basis weight, thickness, air permeability, and surface smoothness of the tipping paper base paper can be selected according to the specifications of the cigarette product and the requirements of the cigarette-making process.
[0013] In some embodiments, the citrate is selected from at least one of sodium citrate, potassium citrate, and ammonium citrate, preferably sodium citrate. Sodium citrate has good solubility in water-based coatings, making it easy to formulate with oxidized starch into a first coating suitable for gravure printing.
[0014] In some embodiments, the raw materials for the first coating, by solid mass, include 55-80 parts sodium citrate, 15-35 parts oxidized starch, 2-8 parts carboxymethyl cellulose, and 1-5 parts glycerol. Oxidized starch is used to fix the sodium citrate and improve the adhesion of the first coating to the surface of the base paper; carboxymethyl cellulose is used to adjust the viscosity and film-forming state of the first coating; and glycerol is used to adjust the flexibility of the first coating, reducing the possibility of brittleness during drying and rewinding.
[0015] In some embodiments, the coating area formed by the first coating is one or a combination of at least two of the following: discontinuous stripes, intersecting grids, dot matrix, wavy lines, or forked lines. The first coating is applied only to a portion of the surface of the feedstock on one side, which allows for control over the amount of citrate applied per unit area and reduces the impact of the first coating on the overall flexibility, air permeability, and adhesion of the feedstock.
[0016] In some embodiments, the projected area of the first coating on the surface of the splicing paper accounts for 5% to 25% of the total surface area of that side. The dry coating weight of the first coating is 0.08 to 0.35 g / m². 2 Unless otherwise stated, the dry coating amount of the first, second, and third coatings in this application is calculated based on the total area of the side surface of the tipping paper on which the coatings are applied.
[0017] In some embodiments, when the coating area is distributed in the form of discontinuous stripes or intersecting grids, the line width of the discontinuous stripes or intersecting grids is 0.15–0.80 mm; the net spacing between adjacent stripes in the discontinuous stripes or the net spacing between adjacent parallel grid lines in the intersecting grids is 1.0–5.0 mm. The first coating layer can be set away from the overlap bonding area of the tipping paper, or the distribution of the coating area can be adjusted according to the printed graphic area, perforated area, and cutting position of the tipping paper.
[0018] In some embodiments, the raw materials for the second coating, by solid mass, include 45-70 parts of oxidized starch, 15-35 parts of shellac, 0.5-4 parts of nanocellulose, and 3-10 parts of plasticizer. The plasticizer is selected from at least one of glycerol, sorbitol, and triethyl citrate. Oxidized starch constitutes the continuous phase of the second coating, shellac is used to adjust the moisture resistance and water transfer rate of the second coating, nanocellulose is used to improve the continuity and mechanical stability of the second coating, and the plasticizer is used to reduce the brittleness of the second coating.
[0019] In some embodiments, the second coating covers the first coating and the surrounding area of the base paper where the first coating is not applied. The dry coating weight of the second coating is 0.20–0.70 g / m². 2 Preferably, the concentration is 0.30–0.55 g / m³. 2 When the coating amount of the second coating is below a suitable range, its isolation effect on the first coating is limited; when the coating amount of the second coating is too high, the migration time of citrate under continuous wetting conditions is prolonged, which is not conducive to the timely disintegration of the splice paper.
[0020] In some embodiments, the raw materials for the third coating, based on the mass parts of the solid raw materials before crosslinking, include 50-75 parts sodium alginate, 15-35 parts low-methoxyl pectin, 0.5-4 parts nanocellulose, and 3-10 parts plasticizer. The plasticizer is selected from at least one of glycerol and sorbitol.
[0021] In some embodiments, the degree of esterification of the low-methoxyl pectin is 20%–45%, and the mass ratio of sodium alginate to low-methoxyl pectin is 1.5–4.0:1. Sodium alginate and low-methoxyl pectin jointly participate in calcium ion crosslinking, enabling the third coating to maintain wet integrity while possessing flexibility suitable for splicing paper curling, rewinding, and slitting.
[0022] In some embodiments, the third coating covers the outer surface of the second coating and is formed by reacting a third coating precursor containing sodium alginate and low-methoxyl pectin with a crosslinking liquid containing a calcium salt. The calcium salt is selected from at least one of calcium lactate, calcium chloride, calcium gluconate, and calcium acetate, preferably at least one of calcium lactate and calcium chloride. The dry coating weight of the third coating is 0.60–1.40 g / m². 2 Preferably, it is 0.75–1.20 g / m 2 .
[0023] In some embodiments, the ratio of the amount of citrate per unit area in the first coating to the amount of calcium per unit area in the third coating is 0.60 to 1.10:1. The amounts of citrate and calcium per unit area are based on the total area of one side of the tipping paper where the coating is applied. The amount of citrate per unit area in the first coating is calculated based on the actual dry coating amount of citrate used, its mass proportion in the first coating solid, and its relative molecular mass; the amount of calcium per unit area in the third coating is determined by subtracting the background calcium content of an equal area of uncoated tipping paper from the total calcium content measured by acid digestion of the finished tipping paper, and then converting the result by area.
[0024] When the molar ratio of citrate to calcium per unit area is too low, the third coating may still maintain a high degree of cross-linking after continuous wetting; when the ratio is too high, citrate may affect the cross-linking structure of the third coating earlier during high humidity storage or short-term wetting. Controlling the ratio of the two within the appropriate range is beneficial to creating a suitable working window between short-term moisture resistance and disintegration after continuous wetting.
[0025] In some embodiments, the dry coating weight of the first coating is 0.12–0.28 g / m². 2 The dry coating weight of the second coating is 0.30–0.55 g / m². 2 The dry coating weight of the third coating is 0.75–1.20 g / m². 2 The three coating layers work together to control the amount of citrate stored, the migration of moisture and citrate through the second coating, and the initial degree of crosslinking of the third coating.
[0026] In some embodiments, a water-based decorative ink layer may also be provided on the outer side of the third coating. The water-based decorative ink layer can be formed using water-based inks commonly used in the tipping paper industry, and its dry coating amount and graphic distribution are determined according to the appearance requirements of the tipping paper. The water-based decorative ink layer does not cover or only partially covers the overlap bonding area of the tipping paper.
[0027] The present invention also provides a method for producing the above-mentioned green and environmentally friendly biodegradable cigarette tipping paper, comprising the following steps: S1, applying a first coating containing citrate and oxidized starch to a portion of at least one side surface of the tipping paper base paper, so that the side surface forms a coated area covered by the first coating and an uncoated area not covered by the first coating, wherein the citrate is selected from at least one of sodium citrate, potassium citrate and ammonium citrate, and drying to form a first coating, wherein the dry coating weight of the first coating is 0.08-0.35 g / m². 2 S2. Apply a second coating containing oxidized starch and shellac to the surface of one side, covering the first coating and the uncoated area. Dry to form the second coating, with a dry coating weight of 0.20–0.70 g / m². 2 S3. Apply a third coating containing sodium alginate and low-methoxyl pectin to the surface of the second coating, so that the third coating covers the outer surface of the second coating to form a third coating precursor; S4. Apply a crosslinking liquid containing calcium salt to the third coating precursor, and form a third coating through crosslinking and drying. The dry coating weight of the formed third coating is 0.60-1.40 g / m². 2The dry coating amount of the first, second, and third coatings is based on the total area of one side surface of the tipping paper base paper. The amount of calcium per unit area in the third coating is determined by subtracting the background calcium amount of an equal area of uncoated tipping paper base paper from the total calcium amount measured by acid digestion of the finished tipping paper, and then converting it according to the total area of one side surface. The ratio of the amount of citrate per unit area in the first coating to the amount of calcium per unit area in the third coating is 0.40 to 1.50:1. The amount of citrate per unit area is also based on the total area of one side surface of the tipping paper base paper.
[0028] In some embodiments, in step S1, citrate is dissolved in water, and oxidized starch, carboxymethyl cellulose, and glycerol are added and dispersed by stirring to obtain a first coating. The first coating is applied to a portion of the surface of the tipping paper base paper using gravure printing, and the printing plate forms coated and uncoated areas. The drying temperature of the first coating is 55–75°C.
[0029] In some embodiments, in step S2, oxidized starch, shellac, nanocellulose, and plasticizer are dispersed in water to obtain a second coating. The second coating is applied to the side of the first coating using gravure coating, anilox roller coating, or flexographic coating, so that the second coating covers the first coating and the uncoated area. The drying temperature of the second coating is 65–90°C.
[0030] In some embodiments, in step S3, sodium alginate, low-methoxyl pectin, nanocellulose, and a plasticizer are dispersed in water to obtain a third coating. The third coating is applied to the surface of the second coating and covers the outer surface of the second coating to form a precursor for the third coating.
[0031] In some embodiments, in step S4, the mass fraction of calcium salt in the crosslinking solution is 0.5% to 2.5%, and the crosslinking solution is applied to the outer side of the third coating precursor by gravure transfer, spraying, or roller coating. The wet application amount of the crosslinking solution is 0.5 to 2.5 g / m³. 2 The wet application amount is based on the total area of the side surface of the feedstock paper where the coating is applied. The drying temperature after crosslinking is 75–105°C.
[0032] In some embodiments, the first, second, and third coatings are dried separately, with each subsequent coating applied only after the previous one has reached surface dryness, to reduce mixing between adjacent coatings during the production process. Each drying step can be accomplished using hot air drying, infrared-assisted drying, or a combination of both.
[0033] In some embodiments, after the third coating is formed, water-based decorative ink is printed on the outside of the third coating, and the paper is humidified, perforated, rewound and slit according to product requirements to obtain green, environmentally friendly and biodegradable cigarette tipping paper.
[0034] The present invention has the following advantages over the prior art: This invention does not achieve post-disposal decomposition performance by simply increasing the hydrophilicity of the tipping paper material. Instead, it applies a first coating containing citrate to a portion of the surface of the base paper, then covers the first coating and the uncovered portion of the base paper with a second coating, and finally covers the second coating with a calcium-crosslinked third coating. This effectively separates the citrate and calcium-crosslinked polysaccharide in a dry state. The second coating restricts citrate migration during production, storage, and short-term moisture contact, maintaining the necessary wet integrity of the third coating. Under continuous wetting or repeated wet-drying conditions, moisture gradually penetrates each coating, allowing citrate to migrate from the second coating to the third coating and affect its calcium-crosslinking state. This transforms the tipping paper from a relatively stable state for use into a state that is easily absorbent, decomposes, and disperses fibers. By controlling the local coating structure of the first coating, the coverage relationship of the second coating, the calcium crosslinking system of the third coating, the dry coating amount of each layer, and the molar relationship between citrate and calcium per unit area, premature instability caused by direct blending can be reduced, and problems caused by excessive isolation leading to difficulty in triggering post-disposal decomposition can be avoided. This achieves a balance between normal use stability and post-disposal decomposition. Each coating is mainly composed of water-based starch, shellac, alginate, pectin and other materials. The production process can be integrated with existing gravure printing, coating and drying equipment for tipping paper, which facilitates continuous production and helps reduce the environmental burden caused by tipping paper maintaining its intact structure for a long time after disposal. Detailed Implementation
[0035] The present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, all raw materials used are commercially available industrial-grade raw materials, and all percentage contents and parts are by weight.
[0036] I. Raw Materials and Testing Conditions The tipping paper used in this embodiment is plant fiber tipping paper with a basis weight of 32.0 g / m³. 2 The thickness is 38.5 μm, the moisture content is 5.6%, and the longitudinal dry tensile strength is 1.52 kN / m. No permanent wet-strength resin is added to the tipping paper base paper.
[0037] Sodium citrate is trisodium citrate dihydrate with a purity of not less than 99.0%; the carboxyl content of oxidized starch is 0.35%–0.55%, and the viscosity of a 12% aqueous dispersion at 25°C is 25–45 mPa·s; the degree of substitution of carboxymethyl cellulose is 0.75–0.90; the aqueous shellac is a dewaxed shellac ammonium salt dispersion with a solid content of 25% and a pH of 7.8–8.5; the nanocellulose is a cellulose nanofiber dispersion with a solid content of 2% and an average fiber diameter of 10–50 nm; the sodium alginate is low-viscosity sodium alginate, and the viscosity of a 1% aqueous solution at 25°C is 80–150 mPa·s; the degree of esterification of low-methoxyl pectin is determined by the following method; the calcium salt is anhydrous calcium chloride; and the plasticizer is glycerol or a mixture of glycerol and sorbitol.
[0038] In this application, the degree of esterification of low-methoxyl pectin is determined by acid-base titration. After dispersing the pectin sample and removing free acid, the free carboxyl groups are titrated with a standard sodium hydroxide solution. Subsequently, excess sodium hydroxide is added to saponify the esterified carboxyl groups. After acidification, the carboxyl groups released during saponification are titrated with a standard sodium hydroxide solution. The percentage of esterified carboxyl groups to total carboxyl groups is calculated based on the amount of alkali consumed before and after saponification, and this percentage is taken as the degree of esterification. When using commercially available low-methoxyl pectin, the results can be verified against the inspection report of the same batch of raw materials.
[0039] The dry coating weight of each coating was determined by the difference in oven-dry mass per unit area of the sample before and after coating. The dry coating weights of the first, second, and third coatings were all based on the total area of the surface of the tipping paper on the side where the coating was applied. The amount of citrate per unit area in the first coating was calculated based on the actual dry coating weight of citrate, its mass ratio in the solid of the first coating, and its relative molecular mass. The amount of calcium per unit area in the third coating was determined using acid digestion-inductively coupled plasma atomic emission spectrometry: the total calcium content of the finished tipping paper was measured, and the background calcium content of the uncoated tipping paper of the same batch with an equal area was deducted, and then converted according to the total area of the surface of the tipping paper on the side where the coating was applied.
[0040] The ratio of the amount of citrate per unit area in the first coating to the amount of calcium per unit area in the third coating is calculated according to formula (1): M = nCit / nCa (1) In the formula, M is the ratio of the amount of citrate to calcium per unit area; nCit is the amount of citrate per unit area in the first coating, in mmol / m². 2 nCa represents the amount of calcium per unit area in the third coating, expressed in mmol / m². 2Both nCit and nCa are based on the total area of the side surface of the tipping paper with coating. nCa is calculated by subtracting the background calcium content of the uncoated tipping paper of the same batch from the total calcium content of the finished tipping paper.
[0041] II. General Formulation Methods for Coatings 1. Preparation of the first coating Take 60% of the formula amount of deionized water, heat to 60℃, add sodium citrate and glycerin, and stir until completely dissolved. Separately, add oxidized starch to 30% of the formula amount of deionized water, keep warm and stir at 85℃ for 30 minutes to fully gelatinize the oxidized starch, cool to 50℃ and then add the sodium citrate solution. Add carboxymethyl cellulose after pre-dispersing it with the remaining deionized water, continue stirring for 30 minutes, and filter through a 200-mesh filter to obtain the first coating.
[0042] The solid content of the first coating is adjusted to 8.0%–10.0%, the viscosity at 25℃ is adjusted to 35–65 mPa·s, and the pH value is adjusted to 7.0–8.0.
[0043] 2. Preparation of the second coating Oxidized starch was added to deionized water and stirred at 85°C for 30 minutes to obtain oxidized starch paste. The temperature was then lowered to 45°C, and aqueous shellac dispersion, nanocellulose dispersion and plasticizer were added while stirring. Stirring was continued for 40 minutes, and the mixture was filtered through a 200-mesh filter to obtain the second coating.
[0044] The solid content of the second coating is adjusted to 8.0%–11.0%, the viscosity at 25℃ is adjusted to 45–90 mPa·s, and the pH value is adjusted to 7.5–8.5.
[0045] 3. Preparation of the third coating Sodium alginate was slowly added to deionized water and stirred at 50°C for 60 minutes. The mixture was then allowed to stand to defoam, yielding a sodium alginate solution. Low-methoxyl pectin was added to another portion of deionized water and stirred at 55°C for 45 minutes, yielding a low-methoxyl pectin solution. The two solutions were mixed, and nanocellulose dispersion and a plasticizer were added. The mixture was stirred for another 40 minutes and then filtered through a 150-mesh screen to obtain the third coating.
[0046] The solid content of the third coating is adjusted to 8.0%–10.0%, the viscosity at 25℃ is adjusted to 90–180 mPa·s, and the pH value is adjusted to 6.5–7.5.
[0047] 4. Preparation of crosslinking solution Anhydrous calcium chloride was added to deionized water and stirred until completely dissolved to prepare a calcium chloride crosslinking solution with a mass fraction of 2.0%.
[0048] III. General Production Methods for Tipping Paper The tipping paper base paper is equilibrated in an environment with a temperature of 23℃ and a relative humidity of 50% for 24 hours before coating.
[0049] A first coating is applied to a portion of the surface of the tipping paper base using gravure printing. The first coating forms a coating area according to a predetermined pattern of discontinuous stripes or intersecting grids, wherein the line width of the discontinuous stripes or intersecting grids is 0.15–0.80 mm; the net spacing between adjacent stripes in the discontinuous stripes or the net spacing between adjacent parallel grid lines in the intersecting grids is 1.0–5.0 mm. The first coating is dried to surface dry in a first hot air zone.
[0050] A second coating is applied to the side where the first coating is located using a full-page gravure coating method, so that the second coating covers the first coating and the area of the original paper around the first coating where the first coating is not applied, and is dried in a second hot air zone to form the second coating.
[0051] A third coating is applied to the surface of the second coating using a full-page gravure coating method and pre-dried at 50–60°C for 2–3 seconds to allow the surface of the third coating to set while maintaining its cross-linkable state internally. Subsequently, a calcium chloride cross-linking solution is applied using a reverse gravure transfer method, and after a 1–3 second delay, it is dried sequentially through three hot air zones at temperatures of 75–85°C, 90–105°C, and 55–70°C, respectively, to form the third coating.
[0052] After the third coating is formed, water-based decorative ink is printed on the outside of the third coating according to product requirements. Then, the paper is conditioned, laser-drilled, rewound, and slit. All samples are subjected to the same laser-drilling conditions to control the air permeability of the finished tipping paper to approximately 350 CU.
[0053] The production line operates at a speed of 100m / min. The first, second, and third coatings are applied and dried separately to avoid large-scale mixing of adjacent coatings in an undried state.
[0054] IV. Example 1 The first coating material, by solids by weight, comprises 55 parts sodium citrate, 35 parts oxidized starch, 6 parts carboxymethyl cellulose, and 4 parts glycerol. The first coating employs a discontinuous stripe pattern with a pattern coverage of 5% and a dry coating weight of 0.08 g / m². 2 The first drying temperature is 55℃.
[0055] The second coating material includes 70 parts oxidized starch, 18 parts water-based shellac, 2 parts nanocellulose, and 10 parts glycerol, with a dry coating weight of 0.20 g / m². 2 The second drying temperature is 65℃.
[0056] Based on the solids content before crosslinking, the third coating material includes 53 parts sodium alginate, 35 parts low-methoxyl pectin, 2 parts nanocellulose, and 10 parts glycerol. The degree of esterification of the low-methoxyl pectin is 20%, and the dry coating weight of the third coating is 0.60 g / m². 2 .
[0057] The wet application rate of the calcium chloride crosslinking solution is 2.08 g / m³. 2 After deducting the background calcium in the original paper, the amount of calcium per unit area in the third coating is 0.374 mmol / m². 2 The amount of citrate per unit area in the first coating is 0.150 mmol / m². 2 The ratio of the two is 0.40:1.
[0058] V. Example 2 Based on solids by weight, the first coating material comprises 60 parts sodium citrate, 32 parts oxidized starch, 5 parts carboxymethyl cellulose, and 3 parts glycerol. The first coating employs a combination of discontinuous stripes and dot matrix patterns, with a pattern coverage of 10% and a dry coating weight of 0.12 g / m². 2 The first drying temperature is 60℃.
[0059] The second coating material includes 65 parts oxidized starch, 24 parts water-based shellac, 2 parts nanocellulose, and 9 parts glycerin, with a dry coating weight of 0.30 g / m². 2 The second drying temperature is 72℃.
[0060] The third coating material consists of 58 parts sodium alginate, 30 parts low-methoxyl pectin, 3 parts nanocellulose, and 9 parts glycerol. The degree of esterification of the low-methoxyl pectin is 28%, and the dry coating weight of the third coating is 0.80 g / m². 2 .
[0061] The wet application rate of the calcium chloride crosslinking solution is 2.26 g / m³. 2 The amount of calcium per unit area in the third coating is 0.408 mmol / m². 2 The amount of citrate per unit area in the first coating is 0.245 mmol / m². 2 The ratio of the two is 0.60:1.
[0062] VI. Example 3 Based on solids by weight, the first coating material comprises 65 parts sodium citrate, 28 parts oxidized starch, 4 parts carboxymethyl cellulose, and 3 parts glycerol. The first coating uses a cross-grid pattern with a coverage of 15%, a line width of 0.40 mm, a spacing of 2.5 mm between adjacent grid lines, and a dry coating weight of 0.16 g / m². 2 The first drying temperature is 65℃.
[0063] The second coating material includes 60 parts oxidized starch, 30 parts water-based shellac, 2 parts nanocellulose, and 8 parts glycerin, with a dry coating weight of 0.42 g / m². 2 The second drying temperature is 80℃.
[0064] The third coating material consists of 65 parts sodium alginate, 25 parts low-methoxyl pectin, 2 parts nanocellulose, and 8 parts glycerol. The degree of esterification of the low-methoxyl pectin is 32%, and the dry coating weight of the third coating is 0.95 g / m². 2 .
[0065] The wet application rate of the calcium chloride crosslinking solution is 2.31 g / m³. 2 The amount of calcium per unit area in the third coating is 0.416 mmol / m². 2 The amount of citrate per unit area in the first coating is 0.354 mmol / m². 2 The ratio of the two is 0.85:1.
[0066] VII. Example 4 Based on solids by weight, the first coating material comprises 65 parts sodium citrate, 28 parts oxidized starch, 4 parts carboxymethyl cellulose, and 3 parts glycerol. The first coating employs a combination of intersecting grids and branching lines, with a pattern coverage of 20% and a dry coating weight of 0.22 g / m². 2 The first drying temperature is 68℃.
[0067] The second coating material includes 55 parts oxidized starch, 35 parts water-based shellac, 2 parts nanocellulose, and 8 parts glycerin, with a dry coating weight of 0.55 g / m². 2 The second drying temperature is 85℃.
[0068] The third coating material consists of 70 parts sodium alginate, 22 parts low-methoxyl pectin, 2 parts nanocellulose, and 6 parts glycerol. The degree of esterification of the low-methoxyl pectin is 38%, and the dry coating weight of the third coating is 1.20 g / m². 2 .
[0069] The wet application rate of the calcium chloride crosslinking solution is 2.35 g / m³. 2 The amount of calcium per unit area in the third coating is 0.423 mmol / m². 2 The amount of citrate per unit area in the first coating is 0.486 mmol / m². 2 The ratio of the two is 1.15:1.
[0070] VIII. Example 5 Based on solids by weight, the first coating material comprises 55 parts sodium citrate, 35 parts oxidized starch, 6 parts carboxymethyl cellulose, and 4 parts glycerol. The first coating employs a combination of cross-grid and dot matrix patterns, with a pattern coverage of 25% and a dry coating weight of 0.35 g / m².2 The first drying temperature is 72℃.
[0071] The second coating material includes 51 parts oxidized starch, 35 parts water-based shellac, 4 parts nanocellulose, and 10 parts glycerol, with a dry coating weight of 0.70 g / m². 2 The second drying temperature is 90℃.
[0072] The third coating material consists of 75 parts sodium alginate, 19 parts low-methoxyl pectin, 1 part nanocellulose, and 5 parts glycerol. The degree of esterification of the low-methoxyl pectin is 45%, and the dry coating weight of the third coating is 1.40 g / m². 2 .
[0073] The wet application rate of the calcium chloride crosslinking solution is 2.42 g / m³. 2 The amount of calcium per unit area in the third coating is 0.436 mmol / m². 2 The amount of citrate per unit area in the first coating is 0.655 mmol / m². 2 The ratio of the two is 1.50:1.
[0074] Table 1. Main process parameters of Examples 1-5
[0075] IX. Comparative Example Comparative Example 1 Except for the absence of a first coating, the composition of raw materials, coating amount and production conditions are the same as in Example 3.
[0076] Comparative Example 2 Instead of a separate first coating, sodium citrate in the same amount as in Example 3 was directly added to the third coating; the amounts of other raw materials and production conditions for the second and third coatings were the same as in Example 3. When the calcium chloride crosslinking liquid was applied, the precursor of the third coating showed localized viscosity increases and slight flocculation.
[0077] Comparative Example 3 Except for the absence of a second coating, which allows the first and third coatings to be directly adjacent, the raw material composition, coating amount, and production conditions are the same as in Example 3.
[0078] Comparative Example 4 Except for the second coating, the dry coating amount is adjusted to 0.10 g / m². 2 Except for the raw materials, the other raw material composition and production conditions are the same as in Example 3.
[0079] Comparative Example 5 Except for the second coating, the dry coating weight is adjusted to 0.90 g / m². 2 Except for the raw materials, the other raw material composition and production conditions are the same as in Example 3.
[0080] Comparative Example 6 Keeping the amount of calcium per unit area in the third coating constant, the amount of sodium citrate in the first coating is reduced so that the ratio of citrate to calcium per unit area is 0.20:1; the remaining conditions are the same as in Example 3.
[0081] Comparative Example 7 Keeping the amount of calcium per unit area in the third coating constant, the amount of sodium citrate in the first coating is increased so that the ratio of citrate to calcium per unit area is 1.80:1; the remaining conditions are the same as in Example 3.
[0082] Comparative Example 8 Sodium chloride in the first coating was replaced with sodium chloride in the same amount as in Example 3, while the composition of other raw materials and production conditions were the same as in Example 3.
[0083] Comparative Example 9 Except for the absence of calcium chloride crosslinking solution, the composition of other raw materials, coating amount and production conditions are the same as in Example 3. The sodium alginate and low methoxy pectin in the third coating are not crosslinked with calcium ions.
[0084] Comparative Example 10 A commercially available water-based acrylic emulsion was applied to the entire surface of the same tipping paper base paper, resulting in a dry coating weight of 1.0 g / m². 2 An acrylic coating was applied, and then conventional moisture-resistant coated tipping paper was prepared using the same decorative printing, perforation, rewinding, and slitting conditions as in Example 3.
[0085] 10. Performance Testing Methods 1. Conditioning the sample All samples were conditioned for 24 hours in a standard environment of 23°C and 50% relative humidity before testing. Unless otherwise specified, each test was performed in duplicate, and the results were taken as the arithmetic mean.
[0086] 2. Dry tensile strength The test was conducted in accordance with GB / T 12914—2018. The sample width was 15 mm, the clamping distance was 100 mm, and the tensile speed was 20 mm / min. The longitudinal tensile strength of the spliced paper was tested.
[0087] 3. Tensile strength retention rate after artificial saliva contact Artificial saliva was prepared with 0.4g sodium chloride, 0.4g potassium chloride, 0.8g calcium chloride dihydrate, 0.7g disodium hydrogen phosphate, and 1.0g urea per liter of deionized water, and the pH was adjusted to 6.8. A 15mm × 150mm sample was completely immersed in the artificial saliva at 37℃ for 10min and 20min respectively. After removing the sample, a nonwoven fabric was used to gently press each side of the sample once to absorb the surface liquid, and the wet tensile strength was tested within 30s. The tensile strength retention rate after contact with the artificial saliva was calculated according to formula (2): Rsaliva=Fsaliva / Fdry×100% (2) In the formula, Rsaliva is the tensile strength retention rate after contact with artificial saliva; Fsaliva is the tensile strength of the sample after artificial saliva treatment; and Fdry is the dry tensile strength of the samples in the same batch.
[0088] 4. Tensile strength retention rate after continuous water immersion The sample was completely immersed in 25°C deionized water and kept for 30 min, 60 min and 120 min respectively. After being taken out, the wet tensile strength was tested in the same way as the artificial saliva test, and the retention rate relative to the dry tensile strength was calculated.
[0089] 5. Wet-dry cycle test The sample was immersed in deionized water at 25°C for 10 minutes, then removed and dried at 40°C for 50 minutes, constituting one wet-dry cycle. After completing the first, second, and third wet-dry cycles, the sample was immersed in water again for 10 minutes, and its wet tensile strength retention rate was tested.
[0090] 6. Time to crack and disintegrate in water Cut a 100mm × 100mm sample and place it in a covered container containing 500mL of deionized water. Shake the sample at 25℃ and 60r / min. Timing begins from the moment the sample is immersed in the water. Record the time when a through-crack with a length of at least 5mm appears on the sample surface as the first crack time; record the time when the sample completely separates and the area of the largest continuous fragment is no greater than 25mm². 2 When no continuous, intact coating exceeding 5 mm in length is observed, the time to complete disintegration is recorded. If the above condition is not met even after a test time of 360 minutes, it is recorded as greater than 360 minutes.
[0091] 7. Selectivity difference in water process The water process selectivity difference is calculated according to formula (3): ΔR=Rsaliva,10 Rwater, 120 (3) In the formula, ΔR represents the water process selectivity difference; Rsaliva,10 represents the tensile strength retention rate after 10 min of artificial saliva contact at 37°C; and Rwater,120 represents the tensile strength retention rate after 120 min of continuous immersion in deionized water at 25°C. The larger ΔR is, the more significant the difference between the sample maintaining strength under short-term oral contact conditions and the decrease in strength after continuous water exposure.
[0092] 8. Wet rubbing fastness The printed tipping paper was immersed in artificial saliva at 37°C for 10 minutes. After removal, it was rubbed 10 times with a white cotton cloth under a 500g load. The cotton cloth was evaluated on a scale of 1 to 5 based on the degree of staining and coating damage. A grade of 5 indicates that no obvious staining or coating damage was observed, while a grade of 1 indicates severe staining and coating peeling.
[0093] 9. Warpage Cut a 100mm×100mm sample and lay it flat for 2 hours under standard conditions. Measure the maximum warping height of the four corners of the sample relative to the horizontal plane and take the maximum value among the four corners as the warping degree.
[0094] 10. Breathability After laser drilling was performed on each sample under the same conditions, the air permeability was tested in accordance with GB / T 23227—2018.
[0095] 11. Stability under high temperature and high humidity storage The sample was stored in an environment of 40℃ and 75% relative humidity for 30 days. After being taken out, it was equilibrated in a standard environment for 24 hours, and then the tensile strength retention rate was tested after 10 minutes of contact with artificial saliva.
[0096] 12. Calcium retention in the third coating The cut area is 100cm 2 The calcium content of the samples was tested separately for untreated samples, samples treated with artificial saliva at 37°C for 10 min, and samples treated with deionized water at 25°C for 120 min. The calcium content of the samples was determined using inductively coupled plasma atomic emission spectrometry after nitric acid digestion, with the background calcium content of the original paper subtracted.
[0097] 13. Degradation performance under composting conditions Referring to GB / T 19277.1—2025, the final aerobic biodegradation capacity of the samples was tested under controlled composting conditions of 58℃±2℃. Microcrystalline cellulose was used as a positive reference material. Three parallel tests were set up for each sample, and the relative biodegradation rate on day 28, day 56 and day 90 was calculated based on the amount of carbon dioxide released.
[0098] XI. Test Results The results of normal use performance tests for the examples and comparative examples are shown in Table 2.
[0099] Table 2 Normal Use and Storage Performance
[0100] As shown in Table 2, Examples 1-5 maintained high tensile strength after short-term contact with artificial saliva and exhibited good wet rubbing fastness, dimensional stability, and perforation permeability. Among them, Examples 2-4 showed better overall performance under normal use.
[0101] In Comparative Example 2, sodium citrate was directly added to the third coating. Sodium citrate affected the cross-linking structure during the calcium ion cross-linking process, resulting in a significant decrease in initial dry tensile strength, strength after artificial saliva treatment, and wet rubbing fastness. In Comparative Example 3, after the second coating was removed, the first and third coatings were directly adjacent, and the premature effect also occurred. In Comparative Example 9, no calcium ion cross-linking was performed, and the third coating could not form a sufficiently stable wet structure.
[0102] The performance of each sample under continuous water immersion and wet-drying cycle conditions is shown in Table 3.
[0103] Table 3 Performance after continuous moisture exposure
[0104] Tables 2 and 3 together show that Examples 2-4 have a high strength retention rate after short-term contact with artificial saliva, but the strength retention rate decreases significantly after continuous water immersion or multiple wet-dry cycles, exhibiting a large difference in water process selectivity.
[0105] Comparative Example 1, without the sodium citrate first coating, exhibited good resistance to artificial saliva, but maintained high strength and was difficult to disintegrate after continuous water immersion and wet-dry cycles. Comparative Example 8, which replaced sodium citrate with sodium chloride, also did not show a rapid decrease in strength after continuous water immersion, indicating that this effect was not solely caused by the dissolution or hygroscopic effect of common water-soluble salts in the first coating.
[0106] While Comparative Examples 2, 3, and 4 decomposed relatively quickly in water, their short-term contact performance with artificial saliva was significantly insufficient, indicating that direct blending, omitting the second coating, or using an excessively thin second coating all lead to premature instability. Comparative Example 5 had an excessively thick second coating, resulting in better resistance to artificial saliva, but it still struggled to decompose after continuous water immersion. This demonstrates that the second coating is not simply a coating layer to increase water resistance; its application amount needs to be coordinated with the first and third coatings.
[0107] To further investigate the effect of the dry coating amount of the second coating, while keeping other conditions of Example 3 unchanged, the dry coating amount of the second coating was adjusted to 0 and 0.10 g / m², respectively. 2 0.20g / m 2 0.30g / m 20.42g / m 2 0.55g / m 2 0.70g / m 2 and 0.90g / m 2 The test results are shown in Table 4.
[0108] Table 4. Effect of the dry coating amount of the second coating on the selectivity of the moisture journey.
[0109] Table 4 shows that as the dry coating amount of the second coating increases, the stability of the artificial saliva after short-term contact initially improves significantly; however, when the dry coating amount of the second coating increases further, the disintegration time after continuous water immersion is significantly prolonged, and the selectivity difference in the water process decreases. The dry coating amount of the second coating is between 0.20 and 0.70 g / m². 2 Within this range, it can balance the two properties to a certain extent, specifically 0.30–0.55 g / m³. 2 The overall effect is better within the scope.
[0110] To further investigate the molar ratio of citrate to calcium per unit area, the second and third coatings of Example 3 were kept unchanged. By changing the amount of sodium citrate applied in the first coating, samples with different molar ratios were obtained, and the results are shown in Table 5.
[0111] Table 5. Effect of the molar ratio of citrate to calcium on water process selectivity.
[0112] Table 5 shows that when the molar ratio of citrate to calcium is too low, the third coating still maintains a high wet strength after continuous water immersion. As the molar ratio increases, the rate of strength decline after continuous water immersion accelerates. When the molar ratio is further increased to 1.80:1, the strength retention rate after short-term contact with artificial saliva decreases significantly. Therefore, a higher molar ratio of citrate to calcium is not necessarily better; rather, a larger difference in water process selectivity is achieved within a certain range, with a range of 0.60–1.10:1 showing the best overall effect.
[0113] The calcium retention results of the third coating in Example 3 and some comparative examples are shown in Table 6.
[0114] Table 6. Calcium retention in the third coating after different liquid treatments
[0115] As shown in Table 6, in Example 3, after short-term treatment with artificial saliva, most of the calcium in the third coating was still retained; after continuous treatment with deionized water for 120 minutes, the calcium retention rate decreased significantly. Comparative Example 1 did not contain sodium citrate, and Comparative Example 8 used sodium chloride instead of sodium citrate; both showed relatively high calcium retention rates after continuous water immersion. In Comparative Example 2, because sodium citrate was directly blended with the third coating, calcium ion crosslinking was affected during the film-forming stage, resulting in lower initial calcium content and lower stability after artificial saliva treatment.
[0116] The above results correspond to the spatial arrangement of the first, second, and third coatings. Without theoretical constraints, continuous moisture exposure causes sodium citrate in the first coating to gradually dissolve and migrate through the second coating to the third coating, thereby affecting the retention state of calcium ions in the third coating; short-term artificial saliva contact is insufficient to allow the above migration process to proceed fully, and the ionic environment in artificial saliva is conducive to the third coating maintaining its integrity for a short period of time.
[0117] The composting degradation performance of each sample is shown in Table 7.
[0118] Table 7 Relative biodegradation rate under controlled composting conditions
[0119] As shown in Table 7, the tipped paper of this invention exhibits a high level of biodegradability under controlled composting conditions. Compared to Comparative Example 1, which does not have a first coating, the examples show a faster decomposition process in the early and middle stages, indicating that the tipped paper first experiences coating instability and paper layer disintegration under the influence of moisture, which is beneficial for increasing the contact between the paper fibers and the composting medium. Comparative Example 10, which uses a conventional acrylic coating, shows a significantly slower biodegradation process because the continuous water-resistant coating remains intact for a long time.
[0120] In summary, this invention, by applying a first coating containing sodium citrate to a portion of the surface of the base paper, covering the first coating and the uncovered portion of the base paper with a second coating, and finally covering the second coating with a calcium-crosslinked polysaccharide third coating, allows the interacting components to remain separated during preparation, storage, and short-term artificial saliva contact, while gradually interacting under continuous water immersion or repeated wet-drying conditions. This layered structure differs from directly adding sodium citrate to the calcium crosslinking system, and also from simply using a water-soluble coating or increasing the hydrophilicity of the material. Within an appropriate range of the second coating amount and the molar ratio of citrate to calcium, the tip paper can simultaneously achieve the wet stability required for normal use and rapid disintegration performance under waste conditions, exhibiting significant selectivity in the moisture history process.
[0121] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A green, environmentally friendly, and biodegradable cigarette tipping paper, comprising tipping paper base paper, characterized in that, At least one side surface of the tipping paper is sequentially coated with a first coating, a second coating, and a third coating in a direction away from the tipping paper. The first coating covers a portion of the side surface of the tipping paper, such that the side surface includes a coated area covered by the first coating and an uncoated area not covered by the first coating. The first coating contains citrate and oxidized starch, wherein the citrate is selected from at least one of sodium citrate, potassium citrate, and ammonium citrate, and the dry coating weight of the first coating is 0.08–0.35 g / m³. 2 ; The second coating contains oxidized starch and shellac, and covers the first coating and the uncoated area. The dry coating weight of the second coating is 0.20–0.70 g / m². 2 ; The third coating covers the outer surface of the second coating. The third coating contains calcium-crosslinked alginate and low-methoxyl pectin. The dry coating weight of the third coating is 0.60–1.40 g / m². 2 The dry coating amount of the first, second, and third coatings is based on the total area of one side surface of the tipping paper base paper. The amount of calcium per unit area in the third coating is determined by subtracting the background calcium amount of an equal area of uncoated tipping paper base paper from the total calcium amount measured by acid digestion of the finished tipping paper, and then converting it according to the total area of one side surface. The ratio of the amount of citrate per unit area in the first coating to the amount of calcium per unit area in the third coating is 0.40 to 1.50:
1. The amount of citrate per unit area is also based on the total area of one side surface of the tipping paper base paper.
2. The green and environmentally friendly biodegradable cigarette tipping paper according to claim 1, characterized in that, The citrate is sodium citrate; by solid mass, the raw materials for the first coating include 55-80 parts sodium citrate, 15-35 parts oxidized starch, 2-8 parts carboxymethyl cellulose and 1-5 parts glycerol.
3. The green and environmentally friendly biodegradable cigarette tipping paper according to claim 1 or 2, characterized in that, The coating area is distributed in the form of discontinuous stripes, cross grids, or dot matrix; the projected area of the first coating on one side surface of the tipping paper accounts for 5% to 25% of the total area of that side surface; when the coating area is distributed in the form of discontinuous stripes or cross grids, the line width of the discontinuous stripes or cross grids is 0.15 to 0.80 mm, and the net spacing between adjacent stripes in the discontinuous stripes or the net spacing between adjacent parallel grid lines in the cross grids is 1.0 to 5.0 mm.
4. The green and environmentally friendly biodegradable cigarette tipping paper according to claim 1, characterized in that, The raw materials for the second coating, by solid mass, include 45-70 parts of oxidized starch, 15-35 parts of shellac, 0.5-4 parts of nanocellulose, and 3-10 parts of plasticizer.
5. The green and environmentally friendly biodegradable cigarette tipping paper according to claim 1, characterized in that, Based on the mass fraction of the solid raw materials before crosslinking, the raw materials of the third coating include 50-75 parts of sodium alginate, 15-35 parts of low-methoxyl pectin, 0.5-4 parts of nanocellulose, and 3-10 parts of plasticizer; the degree of esterification of the low-methoxyl pectin is 20%-45%, and the mass ratio of sodium alginate to the low-methoxyl pectin is 1.5-4.0:
1.
6. The green and environmentally friendly biodegradable cigarette tipping paper according to claim 1, characterized in that, The ratio of the amount of citrate per unit area in the first coating to the amount of calcium per unit area in the third coating is 0.60–1.10:1; the dry coating weight of the first coating is 0.12–0.28 g / m². 2 The dry coating weight of the second coating is 0.30–0.55 g / m². 2 The dry coating weight of the third coating is 0.75–1.20 g / m². 2 .
7. A method for producing green, environmentally friendly, and biodegradable cigarette tipping paper, characterized in that, Includes the following steps: S1. A first coating containing citrate and oxidized starch is applied to a portion of at least one side surface of the tipping paper base paper, forming a coated area covered by the first coating and an uncoated area not covered by the first coating on that side surface. The citrate is selected from at least one of sodium citrate, potassium citrate, and ammonium citrate. The coating is dried to form a first coating layer, and the dry coating weight of the first coating layer is 0.08–0.35 g / m². 2 ; S2. Apply a second coating containing oxidized starch and shellac to one side surface, covering the first coating and the uncoated area with the second coating, and dry to form the second coating. The dry coating weight of the second coating is 0.20–0.70 g / m². 2 ; S3. Apply a third coating containing sodium alginate and low-methoxyl pectin to the surface of the second coating, so that the third coating covers the outer surface of the second coating to form a third coating precursor; S4. Apply a calcium salt-containing crosslinking solution to the third coating precursor, and form the third coating through crosslinking and drying. The dry coating weight of the formed third coating is 0.60–1.40 g / m². 2 Wherein, the dry coating amount of the first coating, the second coating and the third coating is based on the total area of the surface of one side of the tipping paper base paper; the amount of calcium per unit area in the third coating is determined by subtracting the background calcium amount of the uncoated tipping paper base paper of the same batch from the total calcium amount measured by acid digestion of the finished tipping paper, and then converting it according to the total area of the surface of one side; the ratio of the amount of citrate per unit area in the first coating to the amount of calcium per unit area in the third coating is 0.40 to 1.50:1, and the amount of citrate per unit area is also based on the total area of the surface of one side of the tipping paper base paper.
8. The production method of green and environmentally friendly biodegradable cigarette tipping paper according to claim 7, characterized in that, In step S1, the first coating is applied by gravure printing and the drying temperature is 55-75℃; in step S2, the second coating is applied by gravure coating and the drying temperature is 65-90℃.
9. The method for producing green and environmentally friendly biodegradable cigarette tipping paper according to claim 7 or 8, characterized in that, In step S3, the mass ratio of sodium alginate to low-methoxyl pectin in the third coating is 1.5–4.0:1; in step S4, the calcium salt is at least one of calcium lactate and calcium chloride, the mass fraction of the calcium salt in the crosslinking solution is 0.5%–2.5%, and the wet application rate of the crosslinking solution is 0.5–2.5 g / m³. 2 The amount of wet application is based on the total area of one side surface of the tipping paper base paper, and the drying temperature after crosslinking is 75-105℃.
10. The production method of green and environmentally friendly biodegradable cigarette tipping paper according to claim 7, characterized in that, The ratio of the amount of citrate per unit area in the first coating to the amount of calcium per unit area in the third coating is 0.60–1.10:1; the dry coating weights of the first, second, and third coatings are 0.12–0.28 g / m², respectively. 2 0.30~0.55g / m 2 and 0.75~1.20g / m 2 .