Construction process for coating concrete crash barriers on bridges

By using a multi-layer composite coating system and modified epoxy resin, the problems of insufficient adhesion and poor toughness in the coating of bridge concrete crash barriers have been solved, achieving efficient and durable protection and improving corrosion resistance and service life.

CN123109063APending Publication Date: 2026-11-17JIABANG (SHANGHAI) NEW MATERIAL TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611317486.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing coating technologies for concrete crash barriers on bridges suffer from insufficient adhesion, poor toughness, and brittleness, failing to effectively prevent the long-term penetration of corrosive media, resulting in a shorter-than-expected protection lifespan and high maintenance costs.

Method used

It adopts a multi-layer composite coating system, including a durable anti-corrosion layer, a repair layer, a fiber reinforcement layer, and a surface protection layer. It uses modified epoxy resin, corundum, and fiber materials to form a dense and tough barrier to isolate corrosive media such as chloride ions and moisture. Combined with a hydrophobic and dust-repellent design, it improves self-cleaning ability.

Benefits of technology

It achieves long-term durable protection, enhances the adhesion between the coating and the substrate, significantly improves impermeability, frost resistance and chemical corrosion resistance, reduces maintenance costs, and extends the service life of bridge concrete crash barriers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to the field of concrete protection technology, specifically to a construction process for coating a concrete crash barrier for bridges. The process includes the following steps: (1) Base surface treatment: grinding with an angle grinder and rust removal and prevention of reinforcing bars; (2) Repair surface cleaning: removing contaminants from the concrete surface after grinding; (3) Durable anti-corrosion layer construction: applying durable anti-corrosion grease material to the cleaned base surface; (4) Intermediate leveling and protective layer material construction: applying repair layer material to the durable anti-corrosion layer; (5) Fiber reinforcement layer construction: applying fiber adhesive to the base surface of the repair layer; (6) Surface protective layer construction: applying self-cleaning topcoat material to the surface of the fiber reinforcement layer; (7) Curing. The crash barrier prepared by this invention has excellent resistance to chloride ion penetration, impermeability, pressure resistance, and durability, and is particularly suitable for coating and protecting concrete crash barriers in bridge engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of concrete protection technology, specifically to a construction process for coating concrete crash barriers for bridges. Background Technology

[0002] With the rapid development of my country's economy, more and more cities are building bridges to alleviate traffic pressure and improve traffic efficiency. However, as their operational lifespan extends, bridges often develop concrete defects, with crash barriers being the most noticeable. Crash barriers, located on both sides or in the middle of the bridge deck, are components designed to ensure vehicle safety and are typically made of reinforced concrete. Due to their location on the bridge deck, they are constantly exposed to sunlight, rain, and de-icing agents, making them susceptible to erosion. This leads to defects such as pitting, exposed aggregate, surface hollowing, dents, chipped corners, and exposed reinforcement, affecting structural durability. In recent years, bridge crash barriers have received increasing attention from administrators. Their repair and painting must ensure the structural durability of the bridge while also considering the needs for quick construction, aesthetic appeal, and ease of cleaning after rain and snow.

[0003] Bridge crash barriers are reinforced concrete structures, and some sections have developed defects such as exposed reinforcement and pitted surfaces due to environmental factors. To ensure durability, the crash barriers require durability repair and protective coating. However, before repair and coating, it is necessary to study the corrosion mechanism of reinforced concrete structures and select appropriate structural forms, materials, and construction techniques to ensure work quality. Traditional protective methods often use single-function coatings or ordinary anti-corrosion materials. Although they can provide some protection in the short term, they generally suffer from insufficient adhesion, poor toughness, and brittleness, failing to effectively prevent the long-term penetration of corrosive media. Especially in harsh environments, their protective lifespan is far shorter than designed expectations, resulting in high maintenance costs and frequent maintenance cycles.

[0004] Currently, while some high-performance anti-corrosion coatings or composite coating systems have emerged on the market—for example, the hydrophilic segments introduced into waterborne epoxy resins to meet environmental protection requirements have ironically become channels for water vapor and chloride ion penetration, reducing their anti-corrosion performance; physically blended nanomaterials are prone to agglomeration and are difficult to disperse uniformly in the resin matrix, failing to fully utilize their nano-reinforcing effect; and simple rubber toughening may come at the cost of sacrificing the coating's strength and barrier properties. Therefore, there is an urgent need in this field to develop a novel, systematic coating application process to provide a long-lasting, reliable, and economical protection solution for bridge concrete crash barriers. Summary of the Invention

[0005] To address the shortcomings of the existing technology, this invention provides a construction process for coating concrete crash barriers for bridges.

[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: A construction process for coating a bridge concrete crash barrier includes the following steps: (1) Base surface treatment construction: The surface of the bridge concrete crash barrier is ground with an angle grinder to smooth out uneven parts, weathered layer, carbonized layer, formwork joints, etc. Exposed steel bars are derusted and rust-proofed. (2) Cleaning the repair surface: After grinding, remove the laitance, oil and loose material from the concrete surface until a solid and clean concrete base surface is exposed; rinse the base surface and carry out subsequent construction after the base surface is dry; (3) Construction of durable anti-corrosion layer: Apply durable anti-corrosion gel material to the cleaned base surface, and apply it in multiple coats until the total dry film thickness is 0.1-0.2mm; (4) Construction of intermediate leveling and protective layer material: Apply repair layer material to the durable anti-corrosion layer, and the dry film thickness is 0.8-1.2mm; (5) Construction of fiber reinforcement layer: Roller apply fiber adhesive to the base surface of the repair layer; adhere the fiber cloth to the adhesive and roll it to ensure that it is fully adhered to the base surface without air bubbles, and apply adhesive to the overlapping area; roll the fiber adhesive again on the surface of the adhered fiber cloth to form a protective layer. (6) Surface protective layer construction: Apply topcoat material to the fiber reinforcement layer in step (5), and the dry film thickness is 0.05-0.15mm; (7) Curing: After the surface protective layer is applied, allow it to cure naturally.

[0007] The construction process of this invention employs a multi-layer composite coating system consisting of a durable anti-corrosion layer, a repair layer, and a surface protective layer, working synergistically to achieve long-term protection of the concrete substrate. The durable anti-corrosion layer is the core and key component of the entire system. First, its rich content of modified epoxy resin, corundum, and fiber-based durable anti-corrosion materials forms a dense and tough barrier, significantly improving the coating's mechanical strength, wear resistance, and impact resistance, effectively resisting physical damage such as vehicle scratches. Second, its excellent chemical inertness and barrier properties effectively prevent corrosive media such as chloride ions, moisture, and carbon dioxide from penetrating into the concrete substrate, fundamentally preventing steel corrosion and concrete deterioration, thus providing durable protection. Building upon this, the repair layer further fills in minor defects, provides a smooth base surface, and increases the overall coating thickness, enhancing the protective effect. The outermost self-cleaning topcoat utilizes hydrophobic and dust-repellent properties, significantly improving the coating's hydrophobicity, enabling it to more effectively repel moisture and dirt, significantly reducing contaminant adhesion, thereby enhancing its self-cleaning ability and corrosion resistance, maintaining aesthetics, providing long-term protection, and reducing maintenance costs. Each functional layer works in a progressive and synergistic manner, complementing each other to form a comprehensive protective system that ensures both internal durability and long-lasting appearance.

[0008] Preferably, the durable anti-corrosion gelling material in step (3) is composed of component A and component B in a weight ratio of (2-4):1; Component A comprises the following raw materials in parts by weight: 50-80 parts by weight of epoxy resin, 10-18 parts by weight of modified epoxy resin, 3-8 parts by weight of dispersant, 1-4 parts by weight of defoamer, and 8-15 parts by weight of filler. Component B comprises the following raw materials in parts by weight: 3-8 parts by weight of corundum, 1-3 parts by weight of coupling agent, 4-8 parts by weight of toughening agent, 8-14 parts by weight of curing agent, 3-6 parts by weight of sodium silicate, 5-10 parts by weight of superabsorbent polymer, and 3-8 parts by weight of reinforcing fiber material.

[0009] Preferably, the repair layer material in step (4) is the concrete surface defect repair layer material prepared in Example 2 of application number 202511081311.X.

[0010] The durable anti-corrosion gel material of this invention is a high-performance composite system in which the components work synergistically: epoxy resin and epoxy resin modified with rubber and graphene serve as a strong film-forming skeleton, providing not only basic adhesion but also toughening and impact resistance through rubber segments and forming a three-dimensional network through graphene sheets, greatly blocking the penetration of corrosive media; corundum and various fillers serve as reinforcing phases, not only improving the density, hardness, and wear resistance of the protective coating but also significantly enhancing its resistance to chemical erosion and improving the coating's hardness and wear resistance; reinforcing fiber materials act as reinforcements similar to steel bars, inhibiting crack propagation. The process involves several steps: first, the coating enhances the toughness and crack resistance of the durable anti-corrosion layer; second, the coupling agent acts as a connector between the inorganic filler and the organic resin, optimizing the interfacial bonding; and third, sodium silicate and superabsorbent polymer can absorb and lock in moisture inside the concrete, helping to reduce moisture migration and improve the coating's impermeability stability, thereby reducing the destructive effects of freeze-thaw cycles on the concrete. Finally, under the action of the curing agent, a dense and stable three-dimensional network is formed, significantly improving the concrete's impermeability, freeze-thaw resistance, chemical erosion resistance, and crack resistance, thus jointly enhancing the impermeability stability and long-term durability of the bridge concrete crash barrier.

[0011] Because the hydrophilic components in conventional resins easily become channels for the penetration of corrosive media such as water vapor, oxygen, and chloride ions, thus accelerating the corrosion of the underlying metal or concrete. The modified epoxy resin added in this invention can effectively solve the core technical problem of the decreased anti-corrosion performance of coatings caused by the introduction of hydrophilic segments in conventional waterborne epoxy resins. This invention constructs a modified epoxy resin with both high crosslinking density and excellent interfacial bonding through a three-step chemical reaction: First, the functional groups on the surface of graphene oxide are used to epoxidize it, introducing active sites for subsequent reactions; then, hydroxyl-terminated butadiene-acrylonitrile rubber is grafted onto the epoxide graphene using isocyanate, successfully combining the toughness of rubber with the strength and barrier properties of graphene; finally, this hybrid material is grafted with epoxy resin, so that the final product simultaneously possesses high functionality. The modified epoxy resin prepared by this invention avoids the drawbacks of simply introducing hydrophilic segments, and has better permeability and adhesion. It can penetrate deep into the tiny pores of the concrete substrate, form mechanical interlocking, hydrogen bonds and polar interface interactions with the concrete, thereby providing a stable base coating and enhancing the bonding force between the coating and the substrate. It provides preliminary anti-corrosion protection for the entire coating system and resists the intrusion of harmful substances such as external moisture and chloride ions.

[0012] Therefore, the application of the modified epoxy resin prepared by the method of this invention in the construction process of bridge concrete crash barrier coating can bring multiple significant and beneficial technical effects: First, the synergistic effect of the highly cross-linked network formed by the epoxy resin and the multiple network effects of the graphene nanosheets greatly prolongs the penetration path of corrosive media such as water, chloride ions, and oxygen, providing excellent physical barrier effects and exhibiting extremely high coating density and shielding properties; Second, the grafted rubber segments effectively toughen the coating, avoiding the inherent brittleness problem of highly cross-linked coatings and significantly enhancing adhesion and toughness; At the same time, the large number of hydroxyl groups generated after resin curing, as well as the good permeability brought by graphene and rubber, allow it to penetrate deep into the micropores of concrete, forming strong mechanical interlocking, hydrogen bonds, and polar interface effects, greatly improving the bonding force between the coating and the substrate; Finally, as the bottom coating, it provides a strong, dense, and firmly adhered foundation for the entire anti-corrosion system, effectively resisting the initial intrusion of harmful external substances and ensuring the long-term durability of the entire coating system.

[0013] Preferably, the modified epoxy resin is prepared by a method comprising the following steps: S1. Graphene oxide is dispersed in an organic solvent, and an alkaline catalyst and epichlorohydrin are added to react and obtain epoxidized graphene. S2. Hydroxyl-terminated liquid rubber and diisocyanate are reacted with a catalyst to generate a prepolymer, and then the epoxide graphene and accelerator are added to react to obtain rubber-modified graphene. S3. The rubber-modified graphene and epoxy resin are grafted in an organic solvent under the action of a tertiary amine catalyst to obtain the modified epoxy resin.

[0014] Furthermore, the tertiary amine catalyst in step S3 is 1,4-diazabicyclo[2.2.2]octane, and the amount of the tertiary amine catalyst is 0.05%-0.50% of the total mass of the rubber-modified graphene and epoxy resin.

[0015] Preferably, the organic solvent is a polar aprotic organic solvent, preferably DMF, DMAc, or DMSO.

[0016] Specifically, the above reaction mechanism is as follows: In step S1, potassium tert-butoxide causes some hydroxyl groups on the surface of graphene oxide to form oxygen-containing active sites with strong nucleophilicity. These active sites undergo nucleophilic substitution reactions with epichlorohydrin, introducing glycidyl ether active structures containing epoxy groups onto the surface of graphene oxide, thereby increasing the number of epoxy active sites on its surface that can be further reacted, thus obtaining epoxidized graphene; In step S2, the terminal hydroxyl groups of the liquid nitrile rubber first undergo an addition reaction with the isocyanate groups of 2,4-toluene diisocyanate under the catalysis of dibutyltin dilaurate, forming a rubber prepolymer containing urethane bonds and retaining some terminal -NCO groups; Subsequently, the residual -NCO groups in the prepolymer mainly undergo addition reactions with the residual hydroxyl groups on the surface of epoxidized graphene to form urethane bonds, thereby connecting the flexible segments of nitrile rubber to the surface of graphene, thus obtaining rubber-modified graphene. Some of the epoxy active sites introduced in step S1 are retained in this process, providing a reaction basis for subsequent interfacial reactions with the epoxy resin system. In step S3, under the catalysis of 1,4-diazabicyclo[2.2.2]octane, the residual carboxyl groups on the surface of the rubber-modified graphene mainly undergo ring-opening esterification reactions with the epoxy groups of bisphenol A type epoxy resin to form β-hydroxy ester structures. At the same time, some hydroxyl groups on the surface can also participate in the ring-opening reaction of epoxy groups to form ether bonds, thereby forming a stable interfacial connection between the rubber-modified graphene and the epoxy resin. Thus, the flexible toughening effect of the nitrile rubber chain segments and the shielding reinforcement effect of the graphene sheets are introduced into the epoxy resin system, which is beneficial to improving the toughness, interfacial compatibility and corrosion barrier properties of the modified epoxy resin.

[0017] Preferably, in step S1, the mass ratio of graphene oxide, alkaline catalyst, and epichlorohydrin is 6-10:1-2:6-10; in step S2, the mass ratio of hydroxyl-terminated liquid rubber, diisocyanate, and epoxide is 8-14:2-3:0.5-1.5; and in step S3, the mass ratio of rubber-modified graphene to epoxy resin is 6-10:15-30.

[0018] The alkaline catalyst is any one of n-butyllithium, potassium tert-butoxide, and sodium hydride.

[0019] Preferably, the reaction conditions in step S1 are 50-70℃ and 300-500rpm for 3-8h; the reaction conditions for the first formation of the prepolymer in step S2 are 80-100℃ for 2-6h, and the reaction conditions for the second formation are 100-120℃ and 300-500rpm for 6-12h; and the reaction in step S3 is carried out under nitrogen protection, 90-110℃, and 300-500 r / min for 3-8h, after which the solvent is removed under reduced pressure.

[0020] Preferably, the filler in component A is selected from one or more of silica, bentonite, calcium carbonate, talc, alumina, and montmorillonite; the dispersant is selected from one or more of sodium dodecylbenzenesulfonate, octylphenol polyoxyethylene ether, and fatty acid monoethanolamide; and the defoamer is selected from one or more of tributyl phosphate, silicone defoamer, and polyether defoamer. The coupling agent in component B is selected from one or more of silane coupling agents, titanate coupling agents, and aluminate coupling agents; the toughening agent is selected from one or more of polyethylene glycol, polypropylene glycol, polyethylene glycol monomethyl ether, polyethylene glycol dimethyl ether, and tetraethylene glycol monooctyl ether; the curing agent is selected from one of aliphatic polyamine curing agents, isocyanate curing agents, acid anhydride curing agents, and aromatic amine curing agents; and the reinforcing fiber material is at least one of sisal fiber, glass fiber, and carbon fiber.

[0021] Preferably, the repair layer material in step (4) is a repair layer material for defects on the concrete surface; the topcoat material in step (6) is a self-cleaning coating material for the concrete surface, an anti-UV coating material for the concrete surface, or a fluorocarbon coating material.

[0022] Preferably, the natural curing time in step (7) is 4-8 days, and hard objects should be avoided from hitting the coating surface during the curing period.

[0023] The bridge concrete crash barrier is obtained by the construction process of coating the bridge concrete crash barrier.

[0024] The beneficial effects of this invention are as follows: 1. Compared with existing technologies, the construction process of the bridge concrete anti-collision wall coating of this invention has a single coating function, which either only focuses on physical shielding or only focuses on surface hydrophobicity. This invention is constructed by sequentially applying multiple layers: a durable anti-corrosion layer, an intermediate repair and leveling layer, a fiber reinforcement layer, and a surface protective layer. In particular, the core durable anti-corrosion layer, by introducing epoxy resin modified with rubber and graphene, not only greatly extends the penetration path of corrosive media by utilizing the graphene network, but also effectively improves the toughness and adhesion of the coating through rubber segments, avoiding the defects of high cross-linked coatings being prone to brittleness. It fundamentally blocks the intrusion of harmful substances such as chloride ions and moisture, providing long-term durability far exceeding that of conventional coatings.

[0025] 2. This invention prepares a modified epoxy resin with high functionality, excellent toughness, and nano-reinforcement through stepwise chemical grafting. This material is not only environmentally friendly and requires no additional diluent during application, making construction simple, but it also deeply penetrates into the micropores of concrete, forming excellent mechanical bonding, hydrogen bonds, and polar interface effects. This significantly improves the adhesion between the coating and the substrate, as well as the overall corrosion resistance, overcoming the difficulties of traditional materials in achieving these dual benefits.

[0026] 3. The concrete crash barrier for bridges prepared by this invention has excellent resistance to chloride ion penetration, impermeability, compressive strength and durability. It reduces the strength loss caused by salt and chloride erosion, and allows the concrete to maintain high compressive strength after salt and chloride wet and dry cycles. It improves the flexibility of the material, reduces the risk of cracking of the base layer, and helps to extend the service life of the concrete structure. It is especially suitable for coating protection of concrete crash barriers for bridge engineering. Detailed Implementation

[0027] The invention will now be described in further detail with reference to specific embodiments, but it should not be construed as limiting the scope of the invention to the following embodiments.

[0028] This application describes some of the raw materials; all other raw materials not described are commercially available. The epoxy resin was purchased from Hubei Zhenzhengfeng New Materials Co., Ltd., brand name MF-4101H.

[0029] The bisphenol A type epoxy resin was purchased from Hubei Maidehao Biotechnology Co., Ltd., model: BE-186EL.

[0030] The corundum was purchased from Gongyi Yuying Refractory Materials Co., Ltd., model: YY-DPS.

[0031] The sisal fiber was purchased from Linyi Yuanma Handicrafts Co., Ltd., item number: 050.

[0032] The carbon fiber was purchased from Forsmann Technology (Beijing) Co., Ltd., item number: 9604003.

[0033] The superabsorbent polymer was purchased from Dongying Qimai New Materials Co., Ltd., model: 200R.

[0034] The hydroxyl-terminated liquid nitrile butadiene rubber was purchased from Jining Tangyi Chemical Co., Ltd., model: SH-820.

[0035] The graphene oxide was purchased from Hebei Ruihuang Metal Materials Co., Ltd., with a particle size of 35,000 mesh.

[0036] The phenolic amine epoxy resin curing agent F-650LV was purchased from Jinan Xingfeifan Environmental Protection New Materials Co., Ltd., model: F-650LV.

[0037] The epoxy fiber mortar was purchased from Tianjin Dongyang Yisheng Building Materials Co., Ltd., with a compressive strength of 40MPa.

[0038] The silicone defoamer was purchased from Shandong Wanhua Tianhe New Materials Co., Ltd., model number: th-5600.

[0039] The commercially available self-cleaning coating material for concrete surfaces was purchased from Henan Juyan Materials Technology Co., Ltd., item number: 022.

[0040] The commercially available high-penetration modified epoxy anti-corrosion coating was purchased from Guangzhou Bijia Suo Building Materials Co., Ltd., with a viscosity of 1000 cps.

[0041] Example 1: A construction process for coating a bridge concrete crash barrier, comprising the following steps: (1) Base surface treatment construction: The surface of the bridge concrete crash barrier is ground with an angle grinder to smooth out uneven parts, weathered layer, carbonized layer, formwork joints, etc. Exposed steel bars are derusted and rust-proofed. (2) Repair surface cleaning: After grinding, remove the floating slurry, impurities, rust, oil, mold, crystallized rock and release agent and other contaminants from the concrete surface until the concrete is exposed. Rinse and dry the cleaned surface, and inspect the base layer to ensure that the surface is firm, clean, dry and free of oil. (3) Construction of durable anti-corrosion layer: Apply durable anti-corrosion grease material to the cleaned concrete anti-collision wall surface of the bridge. The next coat can be applied only after the previous coat is surface dry or fully dry. The coating should be uniform, without any missed areas or drips. The total dry film thickness is 0.15 mm, and the number of coats is 2. (4) Construction of intermediate leveling protective layer material: Apply repair layer material to the durable anti-corrosion layer on the concrete surface in step (3). The coating should be uniform, without any missed areas or drips. The dry film thickness should be 1 mm, and the number of coats should be 1. (5) Construction of fiber reinforcement layer: Apply fiber adhesive to the base surface of the repair layer in step (4) by roller, and control the amount to be 500g / m²; adhere the fiber cloth to the adhesive and roll it to ensure that it is fully adhered to the base surface and free of air bubbles. The overlap length of the fiber cloth is controlled at 80mm, and additional adhesive is applied to the overlap area; apply fiber adhesive again to the surface of the fiber cloth with an amount of 240g / m² to form a protective layer. (6) Surface protective layer construction: Apply durable self-cleaning topcoat material to the fiber reinforcement layer in step (5), the coating is uniform, without omissions or drips, the dry film thickness is 0.1mm, and the number of coats is 1. (7) Curing: After the surface protective layer is applied, avoid impacting the coating surface with hard objects and allow it to cure naturally for 7 days.

[0042] The durable anti-corrosion gelling material in step (3) consists of component A and component B. Component A is prepared from 60 parts by weight of epoxy resin, 12 parts by weight of modified epoxy resin, 5 parts by weight of dispersant, 2 parts by weight of defoamer, and 10 parts by weight of filler. Component B is prepared from 5 parts by weight of corundum, 2 parts by weight of coupling agent, 5 parts by weight of toughening agent, 12 parts by weight of curing agent, 4 parts by weight of sodium silicate, 7 parts by weight of superabsorbent polymer, and 5 parts by weight of reinforcing fiber material. After components A and B are prepared evenly, they are mixed before construction at a mass ratio of 3:1 between the finished product of component A and the finished product of component B. The weight parts of each raw material in component A and component B represent the relative mass ratio between the raw materials within the corresponding component. After component A and component B are prepared independently, they are mixed according to the ratio of the total mass of component A to the total mass of component B of 3:1.

[0043] The filler is a mixture of silica, bentonite, and calcium carbonate in a mass ratio of 1:1:1.

[0044] The dispersant is sodium dodecylbenzenesulfonate.

[0045] The defoamer is silicone defoamer TH-5600.

[0046] The coupling agent is silane coupling agent KH-550.

[0047] The toughening agent is polyethylene glycol monomethyl ether.

[0048] The curing agent is a phenolic amine epoxy resin curing agent F-650LV and tetraethylenepentamine in a mass ratio of 1:1.

[0049] The reinforcing fiber material is a mixture of sisal fiber and carbon fiber in a mass ratio of 1:1.

[0050] The modified epoxy resin is prepared as follows: S1. Under a nitrogen atmosphere, 8 parts by weight of graphene oxide were added to 80 parts by weight of N,N-dimethylformamide and dispersed for 1 h under ultrasonic power of 100 W and ultrasonic frequency of 40 kHz. 1.4 parts by weight of potassium tert-butoxide were added and stirring was continued for 30 min. Then, 8 parts by weight of epichlorohydrin were slowly added and reacted at 60 °C and 400 rpm for 4 h. After centrifugation, washing, and drying, graphene oxide was obtained. S2. Under a nitrogen atmosphere, 10 parts by weight of hydroxyl-terminated liquid nitrile rubber, 2.4 parts by weight of 2,4-toluene diisocyanate, 0.3 parts by weight of dibutyltin dilaurate and 60 parts by weight of N,N-dimethylformamide were mixed and reacted at 90°C for 4 hours to obtain a prepolymer; then 0.8 parts by weight of the above-mentioned epoxide graphene and 0.04 parts by weight of 1,4-diazabicyclo[2.2.2]octane were added, and the mixture was stirred at 110°C and 400 rpm for 8 hours. The solvent was removed by vacuum distillation to obtain rubber-modified graphene. S3. Take 8 parts by weight of the above-mentioned rubber-modified graphene and 80 parts by weight of N,N-dimethylformamide and disperse them for 1 hour under ultrasonic power of 100W and ultrasonic frequency of 40kHz; add 20 parts by weight of bisphenol A type epoxy resin and 0.05 parts by weight of 1,4-diazabicyclo[2.2.2]octane, and stir the reaction for 4 hours under nitrogen protection, 100℃ and 400 r / min. After the reaction is completed, remove the solvent by vacuum distillation to obtain the modified epoxy resin.

[0051] The repair layer material in step (4) is the concrete surface defect repair layer material prepared in Example 2 of application number 202511081311.X.

[0052] The self-cleaning topcoat material used in step (6) is a commercially available self-cleaning coating material for concrete surfaces.

[0053] Example 2: It is basically the same as Example 1, except that the total dry film thickness of the coating in step (3) of the durable anti-corrosion layer construction is 0.1 mm.

[0054] Example 3: It is basically the same as Example 1, except that the total dry film thickness of the coating in step (3) of the durable anti-corrosion layer construction is 0.2 mm.

[0055] Example 4: It is basically the same as Example 1, except that the durable anti-corrosion gel material in step (3) is composed of component A and component B, and the weight ratio of component A to component B is 2:1.

[0056] Example 5: It is basically the same as Example 1, except that the durable anti-corrosion gel material in step (3) is composed of component A and component B, and the weight ratio of component A to component B is 4:1.

[0057] Comparative Example 1: A construction process for coating a bridge concrete crash barrier, comprising the following steps: (1) Base surface treatment construction: The surface of the bridge concrete crash barrier is ground with an angle grinder to smooth out uneven parts, weathered layer, carbonized layer, formwork joints, etc. Exposed steel bars are derusted and rust-proofed. (2) Repair surface cleaning: After grinding, remove the floating slurry, impurities, rust, oil, mold, crystallized rock and release agent and other contaminants from the concrete surface until the concrete is exposed. Rinse and dry the cleaned surface, and inspect the base layer to ensure that the surface is firm, clean, dry and free of oil. (3) Construction of intermediate leveling protective layer material: Apply the repair layer material to the concrete surface in step (2), the coating is uniform, without omissions or drips, the dry film thickness is 1mm, and the number of coats is 1. (4) Construction of fiber reinforcement layer: Apply fiber adhesive to the base surface of the repair layer in step (3) by roller, and control the amount to be 500g / m²; adhere the fiber cloth to the adhesive and roll it to ensure that it is fully adhered to the base surface and free of air bubbles. The overlap length of the fiber cloth is controlled at 80mm, and additional adhesive is applied to the overlap area; apply fiber adhesive again to the surface of the fiber cloth with an amount of 240g / m² to form a protective layer. (5) Surface protective layer construction: Apply durable self-cleaning topcoat material to the fiber reinforcement layer in step (4), the coating is uniform, without omissions or drips, the dry film thickness is 0.1mm, and the number of coats is 1. (6) Curing: After the surface protective layer is applied, avoid impacting the coating surface with hard objects and allow it to cure naturally for 7 days.

[0058] The repair layer material in step (3) is the concrete surface defect repair layer material prepared in Example 2 of application number 202511081311.X.

[0059] The self-cleaning topcoat material in step (5) is a commercially available self-cleaning coating material for concrete surfaces.

[0060] Comparative Example 2: It is basically the same as Example 1, except that: in step (3) the A component of the durable anti-corrosion gel material applied during the construction of the durable anti-corrosion layer is composed of the following parts by weight: 72 parts by weight of epoxy resin, 5 parts by weight of dispersant, 2 parts by weight of defoamer, and 10 parts by weight of filler.

[0061] The filler is a mixture of silica, bentonite, and calcium carbonate in a mass ratio of 1:1:1.

[0062] The dispersant is sodium dodecylbenzenesulfonate.

[0063] The defoamer is silicone defoamer TH-5600.

[0064] Comparative Example 3: It is basically the same as Example 1, except that: in step (3) the A component of the durable anti-corrosion gel material applied during the construction of the durable anti-corrosion layer is composed of the following parts by weight: 60 parts by weight of epoxy resin, 12 parts by weight of modified epoxy resin, 5 parts by weight of dispersant, 2 parts by weight of defoamer, and 10 parts by weight of filler.

[0065] The filler is a mixture of silica, bentonite, and calcium carbonate in a mass ratio of 1:1:1.

[0066] The dispersant is sodium dodecylbenzenesulfonate.

[0067] The defoamer is silicone defoamer TH-5600.

[0068] The modified epoxy resin is prepared as follows: Under a nitrogen atmosphere, 10 parts by weight of hydroxyl-terminated liquid nitrile rubber, 2.4 parts by weight of 2,4-toluene diisocyanate, 0.3 parts by weight of dibutyltin dilaurate and 60 parts by weight of N,N-dimethylformamide are mixed and reacted at 90°C for 4 hours to obtain a prepolymer; 20 parts by weight of bisphenol A type epoxy resin are added and reacted at 100°C under vacuum for 4 hours, and the solvent is removed by vacuum distillation to obtain the modified epoxy resin.

[0069] Comparative Example 4: It is basically the same as Example 1, except that: in step (3) the A component of the durable anti-corrosion gel material applied during the construction of the durable anti-corrosion layer is composed of the following parts by weight: 60 parts by weight of epoxy resin, 12 parts by weight of modified epoxy resin, 5 parts by weight of dispersant, 2 parts by weight of defoamer, and 10 parts by weight of filler.

[0070] The filler is a mixture of silica, bentonite, and calcium carbonate in a mass ratio of 1:1:1.

[0071] The dispersant is sodium dodecylbenzenesulfonate.

[0072] The defoamer is silicone defoamer TH-5600.

[0073] The modified epoxy resin is prepared as follows: Eight parts by weight of graphene oxide and 80 parts by weight of N,N-dimethylformamide were dispersed at an ultrasonic power of 100W and an ultrasonic frequency of 40kHz for 1 hour; 20 parts by weight of bisphenol A epoxy resin were added and placed at 100℃ under vacuum for 4 hours to react; the solvent was removed by vacuum distillation to obtain the modified epoxy resin.

[0074] Comparative Example 5: A construction process for coating a bridge concrete crash barrier, comprising the following steps: (1) Base surface treatment construction: The surface of the bridge concrete crash barrier is ground with an angle grinder to smooth out uneven parts, weathered layer, carbonized layer, formwork joints, etc. Exposed steel bars are derusted and rust-proofed. (2) Repair surface cleaning: After grinding, remove the floating slurry, impurities, rust, oil, mold, crystallized rock and release agent and other contaminants from the concrete surface until the concrete is exposed. Rinse and dry the cleaned surface, and inspect the base layer to ensure that the surface is firm, clean, dry and free of oil. (3) Construction of intermediate leveling protective layer material: Apply repair layer material to the cleaned bridge concrete crash barrier surface. The coating should be uniform, without any missed areas or drips. The dry film thickness should be 1 mm, and the coating should be applied once. (4) Construction of durable anti-corrosion layer: On the repair layer of the concrete surface in step (3), apply durable anti-corrosion gel material. The next coat can be applied only after the previous coat is surface dry or fully dry. The coating should be uniform, without any missed areas or drips. The total dry film thickness is 0.15 mm, and the number of coats is 2. (5) Construction of fiber reinforcement layer: Apply fiber adhesive to the base surface of the durable anti-corrosion layer in step (4) by roller, and control the amount to be 500g / m²; adhere the fiber cloth to the adhesive and roll it to ensure that it is fully adhered to the base surface and free of air bubbles. The overlap length of the fiber cloth is controlled at 80mm, and additional adhesive is applied to the overlap area; apply fiber adhesive again to the surface of the fiber cloth with an amount of 240g / m² to form a protective layer. (6) Surface protective layer construction: Apply durable self-cleaning topcoat material to the surface of the fiber reinforced layer obtained in step (5). The coating is uniform, without omissions or drips. The dry film thickness is 0.1 mm, and the number of coats is 1. (7) Curing: After the surface protective layer is applied, avoid impacting the coating surface with hard objects and allow it to cure naturally for 7 days.

[0075] The repair layer material in step (3) is the same as that in Example 1.

[0076] The durable anti-corrosion gel material in step (4) is the same as that in Example 1.

[0077] Comparative Example 6: It is basically the same as Example 1, except that: in step (3) the durable anti-corrosion layer construction, the durable anti-corrosion grease material applied is a commercially available high-penetration modified epoxy anti-corrosion coating.

[0078] Test Example 1: Uniform preparation of test specimens: In order to eliminate the influence of differences in the properties of different batches of concrete matrix on the test results, all test specimens in Examples 1-5 and Comparative Examples 1-6 were prepared using the same batch of reference concrete.

[0079] The design strength grade of the reference concrete is C50. Each cubic meter of concrete includes: 430 kg of PO 42.5 ordinary Portland cement, 163 kg of water, 720 kg of medium sand, 1090 kg of 5-20 mm continuously graded crushed stone, and 4.3 kg of polycarboxylate superplasticizer, with a water-cement ratio of 0.38. After all raw materials are weighed and mixed at once, the same batch or consecutive batch of concrete is molded into specimens required for subsequent performance tests.

[0080] After demolding, each concrete specimen was cured for 28 days under standard curing conditions of 20±2℃ and relative humidity not less than 95%. After curing, the specimen surfaces were cleaned and dried, and surface treatment and coating were carried out according to the construction processes specified in Examples 1-5 and Comparative Examples 1-6, respectively. After the coating system was completed, it was cured for another 7 days in an environment of 23±2℃ and relative humidity of 50%±10% before testing.

[0081] Different test items use independent specimens. For the same test item, all specimens are from the same batch of concrete. The concrete mix ratio, molding method, initial curing conditions and coating curing conditions are kept consistent. Only the coating system specified in each example or comparative example is changed.

[0082] 1. Chloride ion migration coefficient test: Using the same batch of C50 reference concrete as described above, cylindrical specimens with a diameter of 100 mm and a height of 200 mm were prepared. After standard curing for 28 days, disc specimens with a diameter of 100±1 mm and a height of 50±2 mm were cut from the middle of the specimens. One of the circular end faces was used as the test surface. Corresponding protective systems were formed on the test surface according to the coating processes corresponding to Examples 1-5 and Comparative Examples 1-6, with side sealing. After coating, the specimens were cured for 7 days at 23±2℃ and a relative humidity of 50%±10%.

[0083] An improved test was conducted using the rapid chloride ion migration coefficient method in GB / T 50082-2024, allowing chloride ions to migrate from the test surface with a coating system into the concrete. After the test, the specimen was split axially, and the chloride ion penetration depth was determined by color development with 0.1 mol / L silver nitrate solution. The apparent chloride ion migration coefficient was calculated according to the RCM method in GB / T 50082-2024.

[0084] To facilitate comparison of the relative durability levels of different protection systems, a relative durability index is defined based on the apparent chloride ion migration coefficient of Example 1. I D = D 1 / D i ×100%; In the formula,D 1 represents the apparent chloride ion migration coefficient of Example 1. D i The apparent chloride ion migration coefficient is given by . The relative durability index of Example 1 is defined as 100. Five samples were tested in each group, and the average value was taken. The results are shown in Table 1.

[0085] Table 1. Results of chloride ion migration coefficient test

[0086] Test Example 2: 1. Permeability Pressure Test: Using the same batch of C50 reference concrete as described in Test Example 1, permeability test specimens were formed according to the dimensions specified in GB / T 50082-2024 stepwise pressure method, with 6 specimens per group. After standard curing for 28 days, the coating systems corresponding to Examples 1-5 and Comparative Examples 1-6 were formed on the end face subjected to water pressure, respectively, and the remaining non-test areas were reliably sealed. Curing continued for 7 days after coating.

[0087] The pressure test was conducted in accordance with Section 6.2 of GB / T 50082-2024, with an initial water pressure of 0.1 MPa, increasing by 0.1 MPa every 8 hours, and the back surface was observed continuously. The test was stopped when 3 out of 6 specimens showed signs of seepage, and the water pressure H at this point was taken as the critical seepage resistance pressure described in this application. If leakage occurred around the specimens during the test, the specimens were resealed and the test was repeated.

[0088] 2. Compressive strength test: 150 mm × 150 mm × 150 mm cube specimens were formed using the same batch of C50 reference concrete as described in Test Example 1. After standard curing for 28 days, corresponding coating systems were formed on the outer surface of the specimens according to the construction processes specified in Examples 1-5 and Comparative Examples 1-6, respectively. The specimens were then cured for another 7 days at 23±2℃ and 50%±10% relative humidity.

[0089] The aforementioned salt-chlorine wet-dry cycle is an accelerated erosion pretreatment condition set up in this application based on the service environment of bridge crash barriers subjected to de-icing salt, moisture, and alternating wet and dry conditions. The compressive strength of the concrete after the cycle was determined according to GB / T 50081-2019. To evaluate the influence of different coating systems on the concrete strength retention capacity under salt-chlorine erosion conditions, the specimens were immersed in a 5% (w / w) NaCl aqueous solution at 23±2℃ for 12 h. After wiping off the surface water, they were dried at 50±2℃ for 12 h, constituting one salt-chlorine wet-dry cycle. A total of 30 cycles were performed.

[0090] After the cycle, the specimens were placed at 23±2℃ for 24 h. The coatings on the two opposite pressure surfaces were then ground off and leveled to avoid the coatings affecting pressure transmission. Subsequently, the cubic compressive strength was tested according to GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete". Six parallel specimens were set up for each group, and the average value was taken as the test result.

[0091] 3. Adhesion strength by pull-off test: Using C50 reference concrete from the same batch as the above tests, 300 mm × 300 mm × 50 mm plate-shaped specimens were formed. After standard curing for 28 days, the test surfaces were ground, cleaned, and dried. The corresponding coating systems were formed according to the construction processes of Examples 1-5 and Comparative Examples 1-6, respectively, and cured for 7 days in an environment of 23±2℃ and 50%±10% relative humidity.

[0092] The test was conducted according to GB / T 5210-2006 "Paints and Varnishes - Pull-off Adhesion Test". A 20 mm diameter steel test column was bonded to the surface of the protective layer using a high-strength two-component epoxy adhesive. After the adhesive had fully cured, the column was cut perpendicularly to the concrete substrate. A pull-off adhesion tester was used to continuously apply load perpendicular to the coating surface until failure. The maximum failure load was recorded, and the pull-off adhesion strength was calculated based on the effective area of ​​the test column. Six independent testing points were set up for each group, and the average value of the valid test results was taken.

[0093] Table 2 Results of tests on impermeability, compressive strength and adhesion properties

[0094] The test results above show that this invention, by sequentially applying a durable anti-corrosion layer, an intermediate repair and leveling layer, a fiber reinforcement layer, and a surface protective layer to the treated concrete substrate surface, can effectively improve the chloride ion penetration resistance, water penetration resistance, compressive strength after exposure to salt and chloride corrosion, and adhesion between the coating system and the concrete substrate of the bridge concrete crash barrier. Among these, the durable anti-corrosion layer, as the core protective layer in direct contact with the concrete substrate, plays a crucial role in the overall protective performance.

[0095] Comparing Examples 1-3, it can be seen that when the dry film thickness of the durable anti-corrosion layer increases from 0.10 mm to 0.15 mm, the coating continuity and the ability to block corrosive media are improved; when the dry film thickness continues to increase to 0.20 mm, the various properties are not further improved, indicating that under the material system and construction conditions of the present invention, excessively increasing the film thickness cannot continuously improve the overall protective effect, and around 0.15 mm can better balance the coating density, interface bonding performance and construction stability.

[0096] Comparing Examples 1, 4, and 5, it is evident that the ratio of component A to component B in the durable anti-corrosion gel material significantly affects its overall performance. When the relative amount of component B is too high, the proportions of inorganic reinforcing components, curing components, and hydrophilic components increase accordingly, potentially affecting the formation of the continuous resin phase and the interfacial bonding of the coating. Conversely, when the relative amount of component B is too low, the effective amounts of curing agent, coupling agent, corundum, and reinforcing fiber materials are relatively insufficient, hindering the formation of a fully cured composite network with good reinforcing properties.

[0097] Comparative Example 1, which did not have the durable anti-corrosion layer of the present invention, showed a significant reduction in its various protective properties. This indicates that relying solely on the intermediate repair and leveling layer, fiber reinforcement layer, and surface protective layer is insufficient to fully prevent the migration of moisture and chloride ions into the concrete. This proves that the durable anti-corrosion layer is an important component of the multi-layer protection system of the present invention, playing a long-term barrier role.

[0098] Compared with Example 1, Comparative Example 2 did not add the modified epoxy resin prepared in this invention to the durable anti-corrosion gel material. The resulting protective system showed a decrease in chloride ion penetration resistance, impermeability, and adhesion performance, indicating that the modified epoxy resin plays an important role in improving the density, interfacial bonding stability, and corrosive medium barrier ability of the durable anti-corrosion layer.

[0099] The modified epoxy resin in Comparative Example 3 did not introduce graphene components. Although it retained the flexibility and toughening effect brought by the rubber segments, it lacked the tortuous barrier path formed by the graphene sheets, thus reducing its barrier ability against moisture and chloride ions. Comparative Example 4 did not undergo rubber segment modification, but directly used graphene oxide and epoxy resin for treatment. The interfacial compatibility and dispersion stability of graphene in the resin system were relatively insufficient, and it also lacked the flexibility and toughening effect of the rubber segments. Therefore, its overall protective performance was lower than that of the present invention.

[0100] Comparative Example 5 adjusted the construction sequence of the durable anti-corrosion layer and the intermediate repair and leveling layer, allowing the intermediate repair and leveling layer to contact the concrete substrate first, while the durable anti-corrosion layer could not directly act on the treated concrete substrate, resulting in a reduction in its overall protective performance. This result indicates that the layering sequence of first forming the durable anti-corrosion layer and then constructing the intermediate repair and leveling layer in this invention facilitates the formation of good mechanical bonding, hydrogen bonding, and polar interface interactions between the modified epoxy resin and the concrete substrate, thereby improving the overall stability of the multi-layer protective system.

[0101] Comparative Example 6 used a commercially available high-penetration modified epoxy anti-corrosion coating instead of the durable anti-corrosion gel material of this invention. Its overall performance was still lower than that of this invention, indicating that this invention, through the synergistic combination of modified epoxy resin, inorganic reinforcing components, coupling agents, toughening components, and reinforcing fiber materials, can improve the barrier properties against corrosive media while also ensuring coating toughness and interfacial bonding performance. Therefore, the composition of the durable anti-corrosion gel material, the structure of the modified epoxy resin, and the construction sequence of each functional layer used in this invention work together to improve the long-term protective performance of bridge concrete crash barriers under salt, chloride, and moisture erosion environments.

Claims

1. A construction process for coating a bridge concrete crash barrier, characterized in that, Includes the following steps: (1) Base surface treatment construction: The surface of the bridge concrete crash barrier is ground with an angle grinder to smooth out uneven parts, weathered layer, carbonized layer, formwork joints, etc. Exposed steel bars are derusted and rust-proofed. (2) Cleaning the repair surface: After grinding, remove the laitance, oil and loose material from the concrete surface until a solid and clean concrete base surface is exposed; rinse the base surface and carry out subsequent construction after the base surface is dry; (3) Construction of durable anti-corrosion layer: Apply durable anti-corrosion gel material to the cleaned base surface, and apply it in multiple coats until the total dry film thickness is 0.1-0.2mm; (4) Construction of intermediate leveling and protective layer material: Apply repair layer material to the durable anti-corrosion layer, and the dry film thickness is 0.8-1.2mm; (5) Construction of fiber reinforcement layer: Roller apply fiber adhesive to the base surface of the repair layer; adhere the fiber cloth to the adhesive and roll it to ensure that it is fully adhered to the base surface without air bubbles, and apply adhesive to the overlapping area; roll the fiber adhesive again on the surface of the adhered fiber cloth to form a protective layer. (6) Surface protective layer construction: Apply topcoat material to the fiber reinforcement layer in step (5), and the dry film thickness is 0.05-0.15mm; (7) Curing: After the surface protective layer is applied, allow it to cure naturally.

2. The construction process for coating the bridge concrete crash barrier as described in claim 1, characterized in that, The durable anti-corrosion gel material in step (3) is composed of component A and component B in a weight ratio of (2-4):1; Component A comprises the following raw materials in parts by weight: 50-80 parts by weight of epoxy resin, 10-18 parts by weight of modified epoxy resin, 3-8 parts by weight of dispersant, 1-4 parts by weight of defoamer, and 8-15 parts by weight of filler. Component B comprises the following raw materials in parts by weight: 3-8 parts by weight of corundum, 1-3 parts by weight of coupling agent, 4-8 parts by weight of toughening agent, 8-14 parts by weight of curing agent, 3-6 parts by weight of sodium silicate, 5-10 parts by weight of superabsorbent polymer, and 3-8 parts by weight of reinforcing fiber material.

3. The construction process for coating the bridge concrete crash barrier as described in claim 1, characterized in that, The repair layer material in step (4) is the concrete surface defect repair layer material prepared in Example 2 of application number 202511081311.X.

4. The construction process for coating the bridge concrete crash barrier as described in claim 2, characterized in that, The modified epoxy resin is prepared by a method comprising the following steps: S1. Graphene oxide is dispersed in an organic solvent, and an alkaline catalyst and epichlorohydrin are added to react and obtain epoxidized graphene. S2. Hydroxyl-terminated liquid rubber and diisocyanate are reacted with a catalyst to generate a prepolymer, and then the epoxide graphene and accelerator are added to react to obtain rubber-modified graphene. S3. The rubber-modified graphene and epoxy resin are grafted in an organic solvent under the action of a tertiary amine catalyst to obtain the modified epoxy resin.

5. The construction process for coating the bridge concrete crash barrier as described in claim 4, characterized in that, In step S1, the mass ratio of graphene oxide, alkaline catalyst, and epichlorohydrin is 6-10:1-2:6-10; in step S2, the mass ratio of hydroxyl-terminated liquid rubber, diisocyanate, and epoxide is 8-14:2-3:0.5-1.5; in step S3, the mass ratio of rubber-modified graphene to epoxy resin is 6-10:15-30.

6. The construction process for coating the bridge concrete crash barrier as described in claim 4, characterized in that, The reaction conditions in step S1 are 50-70℃ and 300-500rpm for 3-8h; the reaction conditions for the first formation of the prepolymer in step S2 are 80-100℃ for 2-6h, and the reaction conditions for the second formation are 100-120℃ and 300-500rpm for 6-12h; the reaction conditions in step S3 are nitrogen protection, 90-110℃ and 300-500 r / min for 3-8h, and the solvent is removed under reduced pressure after the reaction is completed.

7. The construction process for coating the bridge concrete crash barrier as described in claim 2, characterized in that, The filler in component A is selected from one or more of silica, bentonite, calcium carbonate, talc, alumina, and montmorillonite; the dispersant is selected from one or more of sodium dodecylbenzenesulfonate, octylphenol polyoxyethylene ether, and fatty acid monoethanolamide; and the defoamer is selected from one or more of tributyl phosphate, silicone defoamer, and polyether defoamer. The coupling agent in component B is selected from one or more of silane coupling agents, titanate coupling agents, and aluminate coupling agents; the toughening agent is selected from one or more of polyethylene glycol, polypropylene glycol, polyethylene glycol monomethyl ether, polyethylene glycol dimethyl ether, and tetraethylene glycol monooctyl ether; the curing agent is selected from one of aliphatic polyamine curing agents, isocyanate curing agents, acid anhydride curing agents, and aromatic amine curing agents; and the reinforcing fiber material is at least one of sisal fiber, glass fiber, and carbon fiber.

8. The construction process for coating the bridge concrete crash barrier as described in claim 1, characterized in that, The repair layer material mentioned in step (4) is a repair layer material for defects on the concrete surface; the topcoat material mentioned in step (6) is a self-cleaning coating material for the concrete surface, an anti-UV coating material for the concrete surface, or a fluorocarbon coating material.

9. The construction process for coating the bridge concrete crash barrier as described in claim 1, characterized in that, The natural curing time described in step (7) is 4-8 days. During the curing period, avoid impacting the coating surface with hard objects.

10. A bridge concrete crash barrier obtained by the construction process of the bridge concrete crash barrier coating as described in any one of claims 1-9.

Citation Information

Patent Citations

  • A repair material for concrete surface defects and preparation method thereof

    CN120573989B