Anode, all-solid-state battery including cathode, and method for manufacturing the same.
By employing a double-layer structure in the positive electrode of the all-solid-state battery to adjust the particle size ratio of the binder and solid electrolyte, the problem of reduced adhesion strength was solved, resulting in higher adhesion and ion conductivity, and improved mechanical stability and power performance of the battery.
Patent Information
- Application Number
- CN202511697891.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2025-11-19
- Publication Date
- 2026-11-17
AI Technical Summary
During the cathode coating process of all-solid-state batteries, adhesive migration leads to a decrease in adhesive strength, affecting mechanical integrity and interface stability, thus limiting their practical application in high-performance applications.
A double-layer positive electrode structure is adopted, wherein the binder content in the first positive electrode active material layer is higher than that in the second layer, and the particle size of the first solid electrolyte is larger than that in the second layer. The adhesive force and ion conductivity are optimized by adjusting the composition ratio and particle size of each layer.
It improves the adhesion and ionic conductivity of the positive electrode, reduces the interface resistance, and enhances the mechanical stability and power performance of the all-solid-state battery.
Smart Images

Figure CN123120611A_ABST
Abstract
Description
[0001] Cross-references to related applications This application claims the benefit of priority to Korean Patent Application No. 10-2025-0064205, filed with the Korean Intellectual Property Office on May 16, 2025, the entire contents of which are incorporated herein by reference. Technical Field
[0002] This invention relates to a positive electrode that can improve adhesion while increasing power, and to an all-solid-state battery including the positive electrode and a method for manufacturing the same. Background Technology
[0003] Renewedly, secondary batteries have been widely adopted in various applications, including electric vehicles and portable electronic devices. Among these, all-solid-state batteries are under active development to achieve higher energy densities. These batteries aim to improve safety and performance—particularly energy density and lifespan—by replacing conventional liquid electrolytes with solid-state electrolytes.
[0004] Despite the numerous advantages of all-solid-state batteries, several manufacturing challenges remain, particularly during the cathode coating process. A key issue is the migration of the binder during coating, which leads to reduced bond strength. This weakened adhesion compromises the mechanical integrity between the cathode active material and the current collector. Consequently, over time, the interface becomes more susceptible to delamination or microstructure degradation, especially under repeated charge-discharge cycles. This degradation is a major cause of decreased long-term stability and reliability in all-solid-state batteries, limiting their practical and effective use in high-performance applications.
[0005] To mitigate the loss of adhesive strength, researchers have explored increasing the binder content or using binders with inherently stronger adhesive properties. While these methods improve mechanical adhesion, they often introduce undesirable side effects. Specifically, higher binder concentrations increase resistance within the cathode layer, thereby reducing the overall power output and energy efficiency of the battery. To overcome this problem, alternative strategies have focused on improving ionic conductivity by introducing smaller-particle-size solid electrolytes or increasing their volume fraction in the electrode. However, these improvements tend to reduce the effectiveness of the binder, further complicating the electrode manufacturing process. Reduced adhesive force leads to poor layer cohesion, coating inhomogeneity, and difficulty in achieving uniform thickness, all of which pose significant obstacles to large-scale production. Therefore, balancing mechanical stability, electrical performance, and processing performance remains a key challenge in developing high-performance all-solid-state battery cathodes.
[0006] Therefore, for the practical commercialization of all-solid-state batteries, it is necessary to focus on the development of cathodes that improve both adhesion strength and power performance. Summary of the Invention
[0007] This disclosure provides, in some respects, a positive electrode and an all-solid-state battery including the positive electrode, which can improve the adhesion between the base material and the composite material, minimize the resistance between the interfaces, and improve the ionic conductivity to exhibit power characteristics.
[0008] In another aspect, this disclosure provides a method for manufacturing a positive electrode that minimizes the resistance between the interfaces of the positive electrode layers.
[0009] To address this problem, this disclosure provides a positive electrode, an all-solid-state battery including the positive electrode, and a method for manufacturing the positive electrode.
[0010] More specifically, (1) this disclosure provides a positive electrode comprising: a positive electrode current collector; a first positive electrode active material layer stacked on the positive electrode current collector and comprising a first solid electrolyte, a positive electrode active material, and a binder; and a second positive electrode active material layer stacked on the first positive electrode active material layer and comprising a second solid electrolyte, a positive electrode active material, and a binder. In this case, the content of the binder included in the first positive electrode active material layer relative to the total weight of the first positive electrode active material layer is higher than the content of the binder included in the second positive electrode active material layer relative to the total weight of the second positive electrode active material layer.
[0011] (2) The positive electrode provided in (1) of this disclosure has a higher content of positive active material in the first positive active material layer relative to the sum of the weight of the first solid electrolyte and the positive active material in the first positive active material layer than the content of positive active material in the second positive active material layer relative to the sum of the weight of the second solid electrolyte and the positive active material in the second positive active material layer.
[0012] (3) This disclosure provides the positive electrode as described in (1) or (2), wherein the average particle size (D) of the first solid electrolyte is... 50 The average particle size of the second solid electrolyte is greater than that of the second solid electrolyte (D). 50 ).
[0013] (4) This disclosure provides a positive electrode in any one of (1) to (3), wherein the average particle size (D) of the first solid electrolyte is... 50 The thickness ranges from 2.5 μm to 4.5 μm.
[0014] (5) The present disclosure provides a positive electrode according to any one of (1) to (4), wherein the content of the positive active material included in the first positive active material layer is 80 wt% to 90 wt% based on the sum of the weights of the positive active material included in the first positive active material layer and the first solid electrolyte.
[0015] (6) The present disclosure provides a positive electrode according to any one of (1) to (5), wherein the content of the first solid electrolyte included in the first positive electrode active material layer is 10 wt% to 30 wt% based on the sum of the weights of the positive electrode active material and the first solid electrolyte included in the first positive electrode active material layer.
[0016] (7) The present disclosure provides a positive electrode according to any one of (1) to (6), wherein the content of the binder included in the first positive electrode active material layer is 2 wt% to 3.5 wt% based on the total weight of the first positive electrode active material layer.
[0017] (8) The present disclosure provides a positive electrode according to any one of (1) to (7), wherein the average particle size (D) of the second solid electrolyte is... 50 The thickness ranges from 0.5 μm to 4.5 μm.
[0018] (9) The present disclosure provides a positive electrode according to any one of (1) to (8), wherein the content of the positive electrode active material included in the second positive electrode active material layer is 70 wt% to 80 wt% based on the sum of the weights of the positive electrode active material included in the second positive electrode active material layer and the second solid electrolyte.
[0019] (10) The present disclosure provides a positive electrode according to any one of (1) to (9), wherein the content of the binder included in the second positive electrode active material layer is from 0.5 wt% to 2 wt% based on the total weight of the second positive electrode active material layer.
[0020] (11) The present disclosure provides a positive electrode according to any one of (1) to (10), wherein the adhesive comprises at least one selected from butadiene rubber (BR), styrene-butadiene rubber (SBR), styrene-butadiene-styrene block copolymer (SBS), nitrile rubber (NBR) and hydrogenated nitrile rubber (HNBR).
[0021] (12) This disclosure provides a positive electrode in which the thickness ratio of the first positive electrode active material layer, calculated by the following formula 1, is 0.2 to 0.5.
[0022] [Formula 1] The thickness ratio of the first positive electrode active material layer = (13) This disclosure provides a positive electrode as described in any one of (1) to (12), wherein the ratio of the total thickness of the positive electrode to the thickness of the current collector is 4 to 8.
[0023] (14) This disclosure provides an all-solid-state battery comprising a positive electrode, a negative electrode and a solid electrolyte layer as described in (1).
[0024] (15) This disclosure provides a method for manufacturing a positive electrode, comprising the steps of: stacking a positive electrode current collector, a first positive electrode active material slurry, and a second positive electrode active material slurry in sequence to form a positive electrode slurry stack; and drying the positive electrode slurry stack, wherein the first positive electrode active material slurry comprises a first solid electrolyte, a positive electrode active material, and a binder; the second positive electrode active material slurry comprises a second solid electrolyte, a positive electrode active material, and a binder, and the content of the binder included in the first positive electrode active material slurry relative to the total weight of the first positive electrode active material slurry is higher than the content of the binder included in the second positive electrode active material slurry relative to the total weight of the second positive electrode active material slurry.
[0025] (16) The present disclosure provides a method for manufacturing a positive electrode as described in (15), wherein drying is performed at a temperature of 70°C to 110°C.
[0026] (17) This disclosure provides a method for manufacturing a positive electrode as described in (15) or (16), wherein forming a positive electrode slurry stack comprises: preparing each of a first positive electrode active material slurry and a second positive electrode active material slurry, and simultaneously applying the first positive electrode active material slurry and the second positive electrode active material slurry to a positive electrode current collector.
[0027] (18) This disclosure provides a method for manufacturing a positive electrode as described in (15) or (16), wherein forming a positive electrode slurry stack comprises: preparing each of a first positive electrode active material slurry and a second positive electrode active material slurry, applying the first positive electrode active material slurry to a positive electrode current collector, and applying the second positive electrode active material slurry to the first positive electrode active material slurry.
[0028] (19) This disclosure provides a method for manufacturing a positive electrode as described in (17), wherein the preparation of the slurry includes mixing a binder of a concentration of 5.5 wt% to 8 wt% and in solution with each of a first positive electrode active material slurry and a second positive electrode active material slurry. Attached Figure Description
[0029] The above and other objects, features and advantages of this disclosure will become more apparent from the following detailed description taken in conjunction with the accompanying drawings: Figure 1 This is a conceptual diagram showing the positive electrode shape according to this disclosure; and Figure 2 This is a graph showing the relationship between capacity retention and cycle number of all-solid-state batteries using a positive electrode manufactured according to embodiments and comparative examples of this disclosure. Detailed Implementation
[0030] This disclosure will be described in detail below.
[0031] The terms or words used in this specification and claims should not be interpreted as having the common dictionary meaning, but rather should be interpreted as relating to the technical scope of the invention, based on the fact that the inventors can properly define the terms and concepts in order to best interpret the invention.
[0032] positive electrode The present invention provides a positive electrode comprising: a positive electrode current collector; a first positive electrode active material layer stacked on the positive electrode current collector and comprising a first solid electrolyte, a positive electrode active material, and a binder; and a second positive electrode active material layer stacked on the first positive electrode active material layer and comprising a second solid electrolyte, a positive electrode active material, and a binder. In this case, the content of the binder in the first positive electrode active material layer relative to the total weight of the first positive electrode active material layer is higher than the content of the binder in the second positive electrode active material layer relative to the total weight of the second positive electrode active material layer.
[0033] The construction of the positive electrode according to the present invention will be described in detail below.
[0034] In this embodiment, the positive electrode may include a positive electrode current collector that transfers electrons generated from the positive electrode active material to the outside and transfers electrons introduced from the outside to the positive electrode active material during charging. The positive electrode current collector may include various materials without particular limitation, as long as the material is suitable for use in the positive electrode current collector. For example, materials used for the positive electrode current collector may include stainless steel, copper, aluminum, nickel, or titanium.
[0035] In this embodiment, the thickness of the positive electrode current collector is at least 10 μm, at least 10.5 μm, at least 11 μm, at least 11.5 μm, at least 12 μm, at least 12.5 μm, at least 13 μm, or at least 13.5 μm, and may be at most 20 μm, at most 19.5 μm, at most 19 μm, at most 18.5 μm, at most 18 μm, at most 17.5 μm, at most 17 μm, or at most 16.5 μm. The energy density of the positive electrode may be further increased within the above ranges.
[0036] According to this disclosure, each of the first and second positive electrode active material layers may include a positive electrode active material. The positive electrode active material may include various materials without particular limitation, as long as the material can intercalate or deintercalate lithium ions and is typically used in all-solid-state batteries. The positive electrode active material may be an oxide active material or a sulfide active material. Preferably, the positive electrode active material may be an oxide active material, more preferably an NCM-type active material.
[0037] In one embodiment, the positive electrode includes a first positive electrode active material layer stacked on a positive electrode current collector. The first positive electrode active material layer can increase the adhesion between the positive electrode active material layer and the positive electrode current collector, and can improve the durability of the positive electrode. Therefore, the content of the adhesive and the ratio of the positive electrode active material included in the first positive electrode active material layer can be set to be higher than the content of the adhesive and the ratio of the positive electrode active material included in the second positive electrode active material layer.
[0038] In other words, the weight content of the binder included in the first positive electrode active material layer can be higher than the weight content of the binder included in the second positive electrode active material layer. Furthermore, the content of the positive electrode active material included in the first positive electrode active material layer relative to the sum of the weights of the first solid electrolyte and the positive electrode active material included in the first positive electrode active material layer can be higher than the content of the positive electrode active material included in the second positive electrode active material layer relative to the sum of the weights of the second solid electrolyte and the positive electrode active material included in the second positive electrode active material layer.
[0039] In this embodiment, the first solid electrolyte included in the first positive electrode active material layer can be an inorganic solid electrolyte, such as a sulfide solid electrolyte, an oxide solid electrolyte, a halide solid electrolyte, or a solid polymer electrolyte. Preferably, the first solid electrolyte can be a sulfide solid electrolyte.
[0040] In the embodiments, the sulfide solid electrolyte can be any common sulfide solid electrolyte, without particular limitation. Preferably, the sulfide solid electrolyte includes at least one selected from the following: Li₂S-P₂S₅, Li₂S-P₂S₅-LiI, Li₂S-P₂S₅-LiCl, Li₂S-P₂S₅-LiBr, Li₂S-P₂S₅-Li₂O, Li₂S-P₂S₅-Li₂O-LiI, Li₂S-SiS₂, Li₂SSiS₂-LiI, Li₂S-SiS₂-LiBr, Li₂S-SiS₂-LiCl, Li₂S-SiS₂-B₂S₃-LiI, Li₂S-SiS₂-P₂S₅-LiI, Li₂S-B₂S₃, Li₂S-P₂S₅-Z m S n (Where "m" and "n" are positive numbers; "Z" is one of Ge, Zn, and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (Where "x" and "y" are positive numbers; M is one of P, Si, Ge, B, Al, Ga, and In) and Li 10 GeP2S 12 .
[0041] In this embodiment, the oxide solid electrolyte can be any common oxide solid electrolyte, without particular limitation. Preferably, the oxide solid electrolyte includes at least one selected from the group consisting of Li. 1+x+y Al x Ti 2-x Si y P 3- y O 12 (0) <x<2、0≤y<3)、BaTiO3、Pb(Zr,Ti)O3(PZT)、Pb 1-x La x Zr 1-y Ti y O3 (PLZT) (0≤x<1, 0≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3 (PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2、0<y<3)、Li x Al y Ti z (PO4)3(0 <x<2、0<y<1、0<z<3)、Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1, 0≤y≤1), Li x La y TiO3 (0 <x<2、0<y<3)、Li2O、LiOH、Li2CO3、LiAlO2、Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2、Li 3+x La3M2O 12 (M=Te, Nb, or Zr; 0≤x≤10) and Li7La3Zr 2-x Ta x O 12 (0) <x<2,LLZ-Ta)。
[0042] In the embodiment, the solid polymer electrolyte may be various conventional solid polymer electrolytes without particular limitation. Preferably, the solid polymer electrolyte comprises at least one selected from the group consisting of polyethylene oxide, poly(diallyldimethylammonium) TFSI), Cu3N, Li3N, LiPON, Li3PO4·Li2S·SiS2, Li2S·GeS2·Ga2S3, Li2O·11Al2O3, Na2O·11Al2O3, (Na,Li) 1+x Ti 2-x Al x (PO4)3 (0.1≤x≤0.9), Li 1+x Hf 2-x Al x (PO4)3 (0.1≤x≤0.9), Na3Zr2Si2PO 12 , Li3Zr2Si2PO 12 , Na5ZrP3O 12 , Na5TiP3O 12 , Na3Fe2P3O 12 , Na4NbP3O 12 , Na-silicate, Li 0.3 La 0.5 TiO3, Na5MSi4O 12 ("M" is a rare earth element such as Nd, Gd or Dy), Li5ZrP3O 12 , Li5TiP3O 12 , Li3Fe2P3O 12 , Li4NbP3O 12 , Li 1+x (M,Al,Ga) x (Ge 1-y Ti y ) 2-x (PO4)3 (x≤0.8; 0≤y≤1.0; "M" is Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm or Yb), Li 1+x+y Q x Ti 2-x Si y P 3-y O 12 (0<x≤0.4; 0<y≤0.6; "Q" is Al or Ga), Li6BaLa2Ta2O 12 , Li7La3Zr2O 12 , Li5La3Nb2O 12 , Li5La3M2O 12 ("M" is Nb or Ta) and Li 7+x A x La3- x Zr2O 12 (0<x<3; "A" is Zn).
[0043] In an embodiment, the halide-based solid electrolyte may include Li element, M element ("M" is a metal other than Li) and X element (X is a halogen). For example, "X" may be F, Cl, Br and I. In particular, the halide-based solid electrolyte may suitably include at least one of Br or Cl as "X". In addition, "M" may be a metal element such as Sc, Y, B, Al, Ga and In.
[0044] In an embodiment, the average particle diameter (D 50 ) may be at least 2.5 μm, at least 2.6 μm, at least 2.7 μm, at least 2.8 μm, at least 2.9 μm, or at least 3.0 μm, and may be at most 4.5 μm, at most 4.4 μm, at most 4.3 μm, at most 4.2 μm, at most 4.1 μm, or at most 4.0 μm. Within the above range, the deterioration rate during the charge-discharge process can be reduced. Accordingly, the mechanical strength of the first positive electrode active material layer can be improved.
[0045] In an embodiment, based on the sum of the weights of the positive electrode active material and the first solid electrolyte included in the first positive electrode active material layer, the content of the positive electrode active material included in the first positive electrode active material layer may be at least 80 wt%, at least 80.5 wt%, at least 81 wt%, at least 81.5 wt%, at least 82 wt%, at least 82.5 wt%, or at least 83 wt%, and may be at most 90 wt%, at most 89.5 wt%, at most 89 wt%, at most 88.5 wt%, at most 88 wt%, at most 87.5 wt%, or at most 87 wt%. Within the above range, the coverage of the binder can be increased. Accordingly, the adhesive force of the positive electrode can be improved.
[0046] In an embodiment, based on the sum of the weights of the positive electrode active material and the first solid electrolyte included in the first positive electrode active material layer, the content of the first solid electrolyte included in the first positive electrode active material layer may be at least 10 wt%, at least 11 wt%, at least 12 wt%, at least 13 wt%, at least 14 wt%, or at least 15 wt%, and may be at most 30 wt%, at most 29 wt%, at most 28 wt%, at most 27 wt%, at most 26 wt%, or at most 25 wt%. Within the above range, the binder coverage can be increased. Accordingly, the adhesive force of the positive electrode can be improved.
[0047] In this embodiment, based on the total weight of the first positive electrode active material layer, the content of the binder included in the first positive electrode active material layer can be at least 2 wt%, at least 2.05 wt%, at least 2.10 wt%, at least 2.15 wt%, at least 2.20 wt%, at least 2.25 wt%, or at least 2.30 wt%, and can be at most 3.50 wt%, at most 3.45 wt%, at most 3.40 wt%, at most 3.35 wt%, at most 3.30 wt%, at most 3.25 wt%, or at most 3.20 wt%. Within the above ranges, the adhesive strength of the first positive electrode active material layer can be improved. Therefore, the durability of the positive electrode is further increased.
[0048] In this embodiment, the coverage of the adhesive included in the first positive electrode active material layer can be at least 15 μm, at least 15.5 μm, at least 16 μm, at least 16.5 μm, at least 17 μm, at least 17.5 μm, at least 18 μm, at least 18.5 μm, at least 19 μm, at least 19.5 μm, or at least 20 μm, and can be at most 25 μm, at most 24.5 μm, at most 24 μm, at most 23.5 μm, at most 23 μm, at most 22.5 μm, at most 22 μm, at most 21.5 μm, at most 21 μm, or at most 20.5 μm. Within the above ranges, the adhesion of the first positive electrode active material layer is greatly improved. The adhesive coverage is a numerical value that quantitatively represents the degree of coating of the particle surface by the adhesive. The adhesive coverage can be calculated by dividing the volume of the adhesive included in the first positive electrode active material layer by the sum of the surface areas of the solid materials (such as the positive electrode active material and the solid electrolyte) included in the first positive electrode active material.
[0049] In this embodiment, the adhesive comprises at least one selected from butadiene rubber (BR), styrene-butadiene rubber (SBR), styrene-butadiene-styrene block copolymer (SBS), nitrile rubber (NBR), and hydrogenated nitrile rubber (HNBR). Preferably, the adhesive may be BR.
[0050] When the adhesive includes BR, SBR or SBS, the content of polar functional groups (-COOH groups, -OH groups, -OR groups) in the adhesive may be at least 5 wt%, at least 5.5 wt%, at least 6 wt%, at least 6.5 wt%, at least 7 wt%, at least 7.5 wt%, at least 8 wt%, at least 8.5 wt%, at least 9 wt%, at least 9.5 wt%, or at least 10 wt%, and may be at most 20 wt%, at most 19.5 wt%, at most 19 wt%, at most 18.5 wt%, at most 18 wt%, at most 17.5 wt%, at most 17 wt%, at most 16.5 wt%, at most 16 wt%, at most 15.5 wt%, or at most 15 wt%. Furthermore, when the adhesive includes NBR-type rubber, the acrylonitrile content in the adhesive may be at least 10 wt%, at least 11 wt%, at least 12 wt%, at least 13 wt%, at least 14 wt%, at least 15 wt%, at least 16 wt%, at least 17 wt%, or at least 18 wt%, and at most 28 wt%, at most 27 wt%, at most 26 wt%, at most 25 wt%, at most 24 wt%, at most 23 wt%, at most 22 wt%, at most 21 wt%, or at most 20 wt%.
[0051] According to this disclosure, the positive electrode may include a second positive electrode active material layer stacked on a first positive electrode active material layer. The second positive electrode active material layer may have a surface in contact with the solid electrolyte layer to improve ion conductivity, thereby improving the battery output.
[0052] According to this disclosure, the positive electrode may include a first positive electrode active material layer (to improve adhesion) and a second positive electrode active material layer (to improve battery power characteristics) to maximize the effect of the first positive electrode active material layer and the second positive electrode active material layer, while minimizing the interface between the first positive electrode active material layer and the second positive electrode active material layer, thereby achieving optimal performance.
[0053] According to this disclosure, the second solid electrolyte included in the second positive electrode active material layer may comprise a material of the same type as the first solid electrolyte described above. The average particle size (D) of the second solid electrolyte... 50The ion migration path can be at least 0.5 μm, at least 0.75 μm, at least 1 μm, at least 1.25 μm, at least 1.5 μm, at least 1.75 μm, or at least 2.0 μm, and at most 4.5 μm, at most 4.25 μm, at most 4 μm, at most 3.75 μm, at most 3.5 μm, at most 3.25 μm, or at most 3.0 μm. Within the above range, the ion migration path can be optimized. Therefore, the ion conductivity can be improved. Therefore, the battery power can be improved.
[0054] In this embodiment, based on the sum of the weights of the positive electrode active material and the second solid electrolyte included in the second positive electrode active material layer, the content of the positive electrode active material included in the second positive electrode active material layer can be at least 70 wt%, at least 70.5 wt%, at least 71 wt%, at least 71.5 wt%, at least 72 wt%, at least 72.5 wt%, or at least 73 wt%, and can be at most 80 wt%, at most 79.5 wt%, at most 79 wt%, at most 78.5 wt%, at most 78 wt%, at most 77.5 wt%, or at most 77 wt%. Within the above ranges, the binder coverage can be reduced, thereby increasing the ionic conductivity. Therefore, the power characteristics can be improved.
[0055] In this embodiment, based on the sum of the weights of the positive electrode active material and the second solid electrolyte included in the second positive electrode active material layer, the content of the second solid electrolyte included in the second positive electrode active material layer can be at least 10 wt%, at least 11 wt%, at least 12 wt%, at least 13 wt%, at least 14 wt%, or at least 15 wt%, and can be at most 30 wt%, at most 29 wt%, at most 28 wt%, at most 27 wt%, at most 26 wt%, or at most 25 wt%. Within the above ranges, the binder coverage can be reduced, thereby increasing the ionic conductivity. Therefore, the power characteristics can be improved.
[0056] In this embodiment, based on the total weight of the second positive electrode active material layer, the content of the binder included in the second positive electrode active material layer can be at least 0.5 wt%, at least 0.55 wt%, at least 0.6 wt%, at least 0.65 wt%, at least 0.7 wt%, at least 0.75 wt%, or at least 0.8 wt%, and at most 2 wt%, at most 1.9 wt%, at most 1.8 wt%, at most 1.7 wt%, at most 1.6 wt%, at most 1.5 wt%, or at most 1.4 wt%. Within the above ranges, the ionic conductivity of the second positive electrode active material layer can be improved. Therefore, the power characteristics can be improved. In this case, the binder can be the same as the binder included in the first positive electrode active material layer.
[0057] In this embodiment, the adhesive coverage in the second positive electrode active material layer can be at least 5 μm, at least 5.5 μm, at least 6 μm, at least 6.5 μm, or at least 7 μm, and at most 10 μm, at most 9.5 μm, at most 9 μm, at most 8.5 μm, at most 8 μm, or at most 7.5 μm. Within the above ranges, the ionic conductivity of the second positive electrode active material layer can be significantly improved.
[0058] According to this disclosure, the average particle size of the first solid electrolyte can be larger than that of the second solid electrolyte. In this case, the first positive electrode active material layer can improve the mechanical strength of the positive electrode, and the second positive electrode active material layer can improve the ionic conductivity of the positive electrode. Therefore, both mechanical strength and power characteristics can be improved.
[0059] Each of the first and second positive electrode active material layers may additionally include a conductive material. The conductive material may include typical materials used in typical positive electrodes, without specific limitations. Preferably, the conductive material may include at least one selected from: carbon-based materials, such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, and carbon nanotubes; metallic materials, in the form of metal powders or fibers containing copper, nickel, aluminum, or silver; and conductive polymers, such as polyphenylene derivatives.
[0060] According to this disclosure, the thickness of the first positive electrode active material layer can be at least 25 μm, at least 26 μm, at least 27 μm, at least 28 μm, at least 29 μm, at least 30 μm, at least 31 μm, at least 32 μm, at least 33 μm, at least 34 μm, or at least 35 μm, and at most 65 μm, at most 64 μm, at most 63 μm, at most 62 μm, at most 61 μm, at most 60 μm, at most 59 μm, at most 58 μm, at most 57 μm, at most 56 μm, at most 55 μm, at most 54 μm, at most 53 μm, at most 52 μm, at most 51 μm, at most 50 μm, at most 49 μm, at most 48 μm, at most 47 μm, at most 46 μm, or at most 45 μm. Within the above ranges, the power characteristics of the electrode can be further improved.
[0061] Furthermore, according to this disclosure, the thickness of the second positive electrode active material layer can be at least 50 μm, at least 51 μm, at least 52 μm, at least 53 μm, at least 54 μm, at least 55 μm, at least 56 μm, at least 57 μm, at least 58 μm, at least 59 μm, or at least 60 μm, and at most 85 μm, at most 84 μm, at most 83 μm, at most 82 μm, at most 81 μm, at most 80 μm, at most 79 μm, at most 78 μm, at most 77 μm, at most 76 μm, at most 75 μm, at most 74 μm, at most 73 μm, at most 72 μm, at most 71 μm, or at most 70 μm. Within the above ranges, the energy density of the positive electrode can be further improved.
[0062] According to this disclosure, in the positive electrode, the thickness ratio of the first positive electrode active material layer calculated by the following formula 1 can be at least 0.20, at least 0.22, at least 0.24, at least 0.26, at least 0.28 or at least 0.30, and at most 0.50, at most 0.48, at most 0.46, at most 0.44, at most 0.42 or at most 0.40.
[0063] [Formula 1] The thickness ratio of the first positive electrode active material layer = Within the aforementioned range, the adhesion of the first positive electrode active material layer can be greatly improved, and the power characteristics of the second positive electrode active material layer can be greatly improved, enabling the positive electrode to be optimized.
[0064] According to this disclosure, the ratio of the total thickness of the positive electrode to the thickness of the current collector can be at least 4.0, at least 4.1, at least 4.2, at least 4.3, at least 4.4, at least 4.5, at least 4.6, at least 4.7, at least 4.8, at least 4.9, or at least 5.0, and at most 8.0, at most 7.9, at most 7.8, at most 7.7, at most 7.6, at most 7.5, at most 7.4, at most 7.3, at most 7.2, at most 7.1, or at most 7.0. Within the above range, the intended function of each layer can be effectively achieved.
[0065] All-solid-state batteries This disclosure provides an all-solid-state battery comprising a positive electrode, a negative electrode, and a solid electrolyte layer.
[0066] The negative electrode and solid electrolyte can include materials used in typical all-solid-state batteries, without particular limitations.
[0067] Methods for manufacturing positive electrodes This invention provides a method for manufacturing a positive electrode, the method comprising: sequentially stacking a first positive electrode active material slurry and a second positive electrode active material slurry to form a positive electrode slurry stack; and drying the positive electrode slurry stack. The first positive electrode active material slurry comprises a first solid electrolyte, a positive electrode active material, and a binder; the second positive electrode active material slurry comprises a second solid electrolyte, a positive electrode active material, and a binder, wherein the content of the binder in the first positive electrode active material slurry relative to the total weight of the first positive electrode active material slurry is higher than the content of the binder in the second positive electrode active material slurry relative to the total weight of the second positive electrode active material slurry.
[0068] The method for manufacturing the positive electrode according to this disclosure will be described in detail below.
[0069] According to the method for manufacturing the positive electrode disclosed herein, the positive electrode slurry stack is formed by stacking a first positive electrode active material slurry and a second positive electrode active material slurry and drying them as a whole, thereby minimizing the resistance caused by the interface between the two layers. The ionic conductivity and power characteristics of the positive electrode manufactured by this method can be improved.
[0070] Furthermore, the method for manufacturing the positive electrode according to this disclosure can be the method described above for manufacturing the positive electrode. Therefore, the positive electrode active material, solid electrolyte, and binder used in the method for manufacturing the positive electrode can be used as described above.
[0071] According to an embodiment of the present invention, in a method for manufacturing a positive electrode, forming a positive electrode slurry stack may include the following steps: preparing a first positive electrode active material slurry and a second positive electrode active material slurry, and simultaneously applying the first positive electrode active material slurry and the second positive electrode active material slurry onto a current collector. In this case, the first positive electrode active material slurry and the second positive electrode active material slurry can be applied in close contact with each other, thereby minimizing the interfacial resistance between the layers and reducing the resistance of the resulting positive electrode.
[0072] According to another embodiment of the present invention, in a method for manufacturing a positive electrode, forming a positive electrode slurry stack may include the following steps: preparing a first positive electrode active material slurry and a second positive electrode active material slurry (or a slurry preparation step); applying the first positive electrode active material slurry onto a positive electrode current collector; and applying the second positive electrode active material onto the first positive electrode active material slurry. According to this disclosure, when preparing the positive electrode, the slurry can be applied in a wet-on-wet manner. Therefore, the resistance at the bilayer interface can be minimized.
[0073] The slurry preparation step may include mixing a binder in solution with each of the first positive electrode active material slurry and the second positive electrode active material slurry. In this case, the solid content concentration of each positive electrode active material slurry can be adjusted according to the amount of binder solution mixed.
[0074] The solid content concentration of each positive electrode active material slurry can be at least 50 wt%, at least 51 wt%, at least 52 wt%, at least 53 wt%, at least 54 wt%, at least 55 wt%, at least 56 wt%, at least 57 wt%, at least 58 wt%, at least 59 wt%, or at least 60 wt%, and at most 70 wt%, at most 69 wt%, at most 68 wt%, at most 67 wt%, at most 66 wt%, at most 65 wt%, at most 64 wt%, at most 63 wt%, at most 62 wt%, at most 61 wt%, or at most 60 wt%. Within the above range, the stability of the slurry can be improved.
[0075] In this case, the concentration of the binder can be at least 5.5 wt%, at least 5.6 wt%, at least 5.7 wt%, at least 5.8 wt%, at least 5.9 wt%, or at least 6.0 wt%, and at most 8 wt%, at most 7.9 wt%, at most 7.8 wt%, at most 7.7 wt%, at most 7.6 wt%, at most 7.5 wt%, at most 7.4 wt%, at most 7.3 wt%, at most 7.2 wt%, at most 7.1 wt%, or at most 7.0 wt%. Within the above range, the concentration of each positive electrode active material slurry can be easily adjusted when introducing the binder solution.
[0076] The drying step can be performed at temperatures of at least 70°C, at least 71°C, at least 72°C, at least 73°C, at least 74°C, at least 75°C, at least 76°C, at least 77°C, at least 78°C, at least 79°C, or at least 80°C, and at most 110°C, at most 109°C, at most 108°C, at most 107°C, at most 106°C, at most 105°C, at most 104°C, at most 103°C, at most 102°C, at most 101°C, or at most 100°C. Within these ranges, both the first and second positive electrode active materials can be effectively dried. Therefore, the layers can be more tightly packed together, thereby reducing the interfacial resistance.
[0077] In the following description, although the invention will be presented in more detail by way of embodiments and experimental examples, the invention is not limited to the embodiments and experimental examples. However, the embodiments of the invention can have various modifications, and the scope of the invention is not limited to the following embodiments. Embodiments of the invention are provided to describe the invention more completely to those skilled in the art.
[0078] Implementation Method 1 250-350 g of NCM-type active material and 60-80 g of sulfide-based solid electrolyte with a particle size of 2.5-4.5 μm (used as the first solid electrolyte) are dry-mixed using a P / D mixer. Then, a carbon-based conductive material, a polyethylene dispersant, and a butyrate ester solvent are additionally introduced, and the result is mixed again. A solution containing 6-7 wt% BR-COOH (butadiene rubber-COOH) is introduced as a binder in an amount of 100-130 g, and the result is mixed to prepare the first positive electrode active material slurry. Separately, a second positive electrode active material slurry is prepared in the same manner as the first positive electrode active material slurry, except that 200-300 g of NCM-type active material and 80-100 g of sulfide-based solid electrolyte with a particle size of 0.5-4.5 μm (used as the second solid electrolyte) are used, which differs from the first positive electrode active material slurry. Subsequently, the first and second positive electrode active material slurries were sequentially applied to an Al current collector with a thickness of 15 μm, and the resulting material was dried at 90°C to manufacture the positive electrode. The total thickness of the obtained positive electrode was 105 μm. In the obtained positive electrode, the thickness of the first positive electrode active material layer formed by the first positive electrode active material slurry and the thickness of the second positive electrode active material layer formed by the second positive electrode active material slurry were both 45 μm.
[0079] In this case, the binder content is calculated as 2.5 wt% or 1 wt% based on the total weight of the first positive electrode active material layer or the second positive electrode active material layer.
[0080] Implementation Method 2 Compared to Embodiment 1, the positive electrode is manufactured in the same manner as in Embodiment 1, except that the amount of adhesive introduced is adjusted so that the adhesive content is calculated to be 2 wt% or 1.5 wt% based on the total weight of the first positive electrode active material layer or the second positive electrode active material layer. The total thickness of the obtained positive electrode, the thickness of the first positive electrode active material layer, and the thickness of the second positive electrode active material layer are all the same as in Embodiment 1.
[0081] Comparative Example 1 Compared to Embodiment 1, the positive electrode is manufactured in the same manner as in Embodiment 1, except that for the first positive electrode active material slurry, 230 g to 330 g of positive electrode active material and 70 g to 90 g of the first solid electrolyte are used; for the second positive electrode active material slurry, 230 g to 330 g of positive electrode active material is used, and the amount of the introduced binder is adjusted so that the binder content is calculated to be 1.75 wt% and 1.75 wt% based on the total weight of the first positive electrode active material layer and the second positive electrode active material layer, respectively. The total thickness of the obtained positive electrode, the thickness of the first positive electrode active material layer, and the thickness of the second positive electrode active material layer are all the same as in Embodiment 1.
[0082] Comparative Example 2 Compared with Comparative Example 1, the positive electrode was manufactured in the same manner as in Comparative Example 1, except that the amount of adhesive introduced was adjusted so that the adhesive content was calculated to be 2 wt% and 2 wt% based on the total weight of the first positive electrode active material layer and the second positive electrode active material layer, respectively. The total thickness of the obtained positive electrode, the thickness of the first positive electrode active material layer, and the thickness of the second positive electrode active material layer were all the same as in Embodiment 1.
[0083] Comparative Example 3 Compared to Comparative Example 1, the positive electrode was manufactured in the same manner as in Comparative Example 1, except that for the first positive electrode active material slurry, 200 g to 300 g of positive electrode active material and 80 g to 100 g of the first solid electrolyte were used; for the second positive electrode active material slurry, 200 g to 300 g of positive electrode active material were used, and the amount of the introduced binder was adjusted so that the binder content was calculated to be 2 wt% and 2 wt% based on the total weight of the first positive electrode active material layer and the second positive electrode active material layer, respectively. The total thickness of the obtained positive electrode, the thickness of the first positive electrode active material layer, and the thickness of the second positive electrode active material layer were all the same as in Embodiment 1.
[0084] Comparative Example 4 Compared to Comparative Example 1, the positive electrode was manufactured in the same manner as in Comparative Example 1, except that for the first positive electrode active material slurry, 200 g to 300 g of positive electrode active material and 80 g to 100 g of the first solid electrolyte were used; for the second positive electrode active material slurry, 250 g to 350 g of positive electrode active material were used, and the amount of the introduced binder was adjusted so that the binder content was calculated to be 2 wt% and 2 wt% based on the total weight of the first positive electrode active material layer and the second positive electrode active material layer, respectively. The total thickness of the obtained positive electrode, the thickness of the first positive electrode active material layer, and the thickness of the second positive electrode active material layer were all the same as in Embodiment 1.
[0085] The content of binder included in each of the first positive electrode active material layer and the second positive electrode active material layer, the weight ratio of positive electrode active material to solid electrolyte, and the content of binder included in the positive electrode active material layer in the positive electrode manufactured according to the embodiments and comparative examples are summarized in Table 1.
[0086] Table 1 Experiment Example 1: Evaluating the adhesive force and resistivity characteristics of the positive electrode To evaluate the adhesion and resistance characteristics of the positive electrodes manufactured in the embodiments and comparative examples, the adhesion [gf / mm] and DC-IR [Ω] were measured using the following methods, and the measurement results are summarized in Table 2.
[0087] [Measurement Method] Adhesive force [gf / mm]: A positive electrode sample measuring 25 mm × 150 mm was prepared using a 180° peel strength tester. Half of the positive electrode sample was attached to a glass slide (25 mm × 75 mm) with double-sided adhesive tape. The positive electrode was peeled at a speed of 30 mm / min, and the force in the 20 to 40 mm section was measured using a tester manufactured by Daeyoung Precision. The average adhesive force was calculated by dividing the measurement result by the width of the positive electrode sample.
[0088] DC-IR [Ω]: A full cell is manufactured and activated using a positive electrode. Specifically, the negative electrode, solid electrolyte layer, and positive electrode are sequentially stacked in a pouch, followed by pouch sealing and subsequent WIP processing. The full cell is then charged at 0.33 C and discharged at 50% SOC for 10 seconds, and the difference between the resting voltage and the final discharge voltage is measured. Specifically, the voltage is recorded using a battery testing system (PNE, model SC(1A)). This difference, along with the current density, is applied to the formula “V=IR” to calculate the internal resistance.
[0089] [Table 2] As can be seen, compared with the positive electrodes according to Comparative Examples 1, 3 and 4, the positive electrode manufactured according to the embodiment of the present invention exhibits higher adhesion and lower internal resistance.
[0090] Therefore, the positive electrode according to the present invention exhibits higher adhesion and lower resistance, enabling the current in the all-solid-state battery including the positive electrode to flow smoothly, thereby improving energy efficiency and power characteristics.
[0091] Experiment Example 2: Evaluation of the performance of all-solid-state batteries A solid-state battery was fabricated by sequentially stacking a positive electrode, a sulfide-based solid electrolyte, a negative electrode including a Ni / Cu substrate, and a Si / C-type negative electrode active material, manufactured according to the embodiments and comparative examples, and pressing them under high pressure. Furthermore, at room temperature, the charging conditions were set to 0.2 C, and the discharging conditions were sequentially changed to 0.2 C-0.33 C-0.5 C-0.2 C. Specifically, the capacity was recorded using a battery testing system (PNE, model SC(1A)). Then, the capacity retention rate after a total of 8 charge / discharge cycles was displayed graphically, as shown below. Figure 2 As shown.
[0092] from Figure 2 It can be seen that the all-solid-state battery including the positive electrode manufactured according to an embodiment of the present invention exhibits a higher capacity retention rate than the all-solid-state battery including the positive electrode manufactured according to the comparative example. Furthermore, the all-solid-state battery including the positive electrode manufactured according to an embodiment of the present invention also demonstrates higher resilience and stability after high-rate discharge than the all-solid-state battery including the positive electrode manufactured according to the comparative example.
[0093] The results above show that the cathode according to the present invention exhibits higher adhesion and lower resistance, enabling close and uniform contact between the active material and the current collector. Furthermore, due to the low internal resistance of the cathode, electrons and ions can be transported smoothly. Therefore, the all-solid-state battery including the cathode according to the present invention can maintain a more stable electrode structure during charge / discharge, thereby improving its power characteristics.
[0094] According to this disclosure, the positive electrode can exhibit higher adhesion and lower resistivity. Therefore, the active material can maintain close and uniform contact with the current collector. Furthermore, the positive electrode has lower internal resistance for smooth electron and ion transport. Thus, an all-solid-state battery including the positive electrode according to the invention can stably maintain its electrode structure during charge / discharge, thereby improving power characteristics.
[0095] Furthermore, according to this disclosure, in the method for manufacturing the positive electrode, the resistance of the first positive electrode active material layer and the second positive electrode active material layer included in the positive electrode can be minimized. Therefore, the prepared positive electrode can exhibit higher adhesion and lower resistance characteristics.
[0096] In the foregoing, although the present invention has been described with reference to exemplary embodiments and accompanying drawings, the present invention is not limited thereto. Those skilled in the art can make various modifications and alterations to the present invention without departing from the spirit and scope of the invention as claimed in the claims.
Claims
1. A positive electrode, comprising: Positive current collector; A first positive electrode active material layer is stacked on the positive electrode current collector, the first positive electrode active material layer comprising a first solid electrolyte, a positive electrode active material and a binder; and A second positive electrode active material layer is stacked on top of the first positive electrode active material layer. The second positive electrode active material layer includes a second solid electrolyte, a positive electrode active material, and a binder. The content of the adhesive in the first positive electrode active material layer relative to the total weight of the first positive electrode active material layer is higher than the content of the adhesive in the second positive electrode active material layer relative to the total weight of the second positive electrode active material layer.
2. The positive electrode according to claim 1, wherein the content of the positive electrode active material included in the first positive electrode active material layer relative to the sum of the weights of the first solid electrolyte and the positive electrode active material included in the first positive electrode active material layer is higher than the content of the positive electrode active material included in the second positive electrode active material layer relative to the sum of the weights of the second solid electrolyte and the positive electrode active material included in the second positive electrode active material layer.
3. The positive electrode according to claim 1, wherein the average particle size D of the first solid electrolyte is... 50 The average particle size D of the second solid electrolyte is greater than 50 .
4. The positive electrode according to claim 1, wherein the average particle size D of the first solid electrolyte is... 50 The range is from 2.5 μm to 4.5 μm.
5. The positive electrode according to claim 1, wherein the content of the positive active material included in the first positive active material layer is 80 wt% to 90 wt% based on the sum of the weights of the positive active material and the first solid electrolyte included in the first positive active material layer.
6. The positive electrode according to claim 1, wherein the content of the first solid electrolyte included in the first positive electrode active material layer is from 10 wt% to 30 wt%, based on the sum of the weights of the positive electrode active material and the first solid electrolyte included in the first positive electrode active material layer.
7. The positive electrode according to claim 1, wherein the content of the binder included in the first positive electrode active material layer is from 2 wt% to 3.5 wt% based on the total weight of the first positive electrode active material layer.
8. The positive electrode according to claim 1, wherein the average particle size D of the second solid electrolyte is... 50 The range is from 0.5 μm to 4.5 μm.
9. The positive electrode according to claim 1, wherein the content of the positive electrode active material included in the second positive electrode active material layer is 70 wt% to 80 wt% based on the sum of the weights of the positive electrode active material included in the second positive electrode active material layer and the second solid electrolyte.
10. The positive electrode according to claim 1, wherein the content of the binder included in the second positive electrode active material layer is from 0.5 wt% to 2 wt% based on the total weight of the second positive electrode active material layer.
11. The positive electrode according to claim 1, wherein the adhesive comprises: It is selected from at least one of butadiene rubber (BR), styrene-butadiene rubber (SBR), styrene-butadiene-styrene block copolymer (SBS), nitrile rubber (NBR), and hydrogenated nitrile rubber (HNBR).
12. The positive electrode according to claim 1, wherein the thickness ratio of the first positive electrode active material layer calculated by the following formula 1 is 0.2 to 0.
5. [Formula 1] The thickness ratio of the first positive electrode active material layer = 。 13. The positive electrode according to claim 1, wherein the ratio of the total thickness of the positive electrode to the thickness of the current collector is 4 to 8.
14. An all-solid-state battery, comprising: The positive electrode according to claim 1; negative electrode; and Solid electrolyte layer.
15. A method for manufacturing a positive electrode, comprising the following steps: A positive electrode slurry stack is formed by sequentially stacking a positive electrode current collector, a first positive electrode active material slurry, and a second positive electrode active material slurry. and The positive electrode slurry stack is dried. The first positive electrode active material slurry includes: The first solid electrolyte, positive electrode active material, and binder The second positive electrode active material slurry includes: The second solid electrolyte, positive electrode active material, and binder, and The content of the binder in the first positive electrode active material slurry relative to the total weight of the first positive electrode active material slurry is higher than the content of the binder in the second positive electrode active material slurry relative to the total weight of the second positive electrode active material slurry.
16. The method of claim 15, wherein the drying step is carried out at a temperature of 70°C to 110°C.
17. The method of claim 15, wherein the step of forming the positive electrode slurry stack comprises: Slurry preparation, wherein each of the first positive electrode active material slurry and the second positive electrode active material slurry is prepared; and Simultaneously, the first positive electrode active material slurry and the second positive electrode active material slurry are applied to the positive electrode current collector.
18. The method of claim 15, wherein the step of forming the positive electrode slurry stack comprises: Slurry preparation, wherein each of the first positive electrode active material slurry and the second positive electrode active material slurry is prepared; The first positive electrode active material slurry is applied to the positive electrode current collector; and The second positive electrode active material slurry is applied onto the first positive electrode active material slurry.
19. The method of claim 17, wherein the slurry preparation comprises: A binder with a concentration of 5.5 wt% to 8 wt% in solution is mixed with each of the first positive electrode active material slurry and the second positive electrode active material slurry.
Citation Information
Patent Citations
Method and apparatus for transmission and reception of qoe measurement confignration informatation between base stations in dual connectivity in communication system
KR1020250064205A