A polymer-based all-solid-state electrolyte, its preparation method and application

By designing a polymer-based all-solid-state electrolyte with a soft-hard-soft three-layer structure, the contradiction between mechanical stability and interfacial affinity in traditional electrolytes has been resolved, achieving high mechanical strength and good electrode contact, thereby improving the performance and production efficiency of lithium-ion batteries.

CN123120854APending Publication Date: 2026-11-17SHUNDE POLYTECHNIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611252180.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polymer-based all-solid-state electrolytes struggle to balance mechanical stability and interfacial affinity. Traditional multilayer composite structures suffer from poor interfacial compatibility, weak interlayer bonding, and cumbersome preparation processes, which affect lithium-ion transport kinetics and industrial production.

Method used

A polymer-based all-solid-state electrolyte consisting of a first soft layer, a hard layer, and a second soft layer is used. The molecular weight is controlled by adjusting the amount of initiator and the polymerization time. Combined with the soft-hard-soft three-layer synergistic structure design, the middle hard layer ensures mechanical strength, while the soft layers on both sides improve the electrode interface contact. In-situ polymerization is used to form a tightly bonded interface.

Benefits of technology

It achieves high mechanical strength and good electrode interface affinity, reduces interface impedance, accelerates lithium-ion transport, and improves the capacity and rate performance of all-solid-state lithium-ion batteries, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120854A_ABST
    Figure CN123120854A_ABST
Patent Text Reader

Abstract

This invention discloses a polymer-based all-solid-state electrolyte, its preparation method, and its applications. The polymer-based all-solid-state electrolyte of this invention comprises a first soft layer, a hard layer, and a second soft layer stacked sequentially. Each of the first, hard, and second soft layers comprises an acrylate-methyl methacrylate copolymer and a lithium salt. The number-average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer is greater than that in the first soft layer and also greater than that in the second soft layer. The polymer-based all-solid-state electrolyte of this invention exhibits tight interlayer bonding, balancing high mechanical strength with good electrode interface affinity, making it suitable for use in all-solid-state lithium-ion batteries. Furthermore, its preparation process is simple, low-cost, and environmentally friendly, making it suitable for large-scale industrial production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solid-state battery technology, specifically relating to a polymer-based all-solid-state electrolyte, its preparation method, and its application. Background Technology

[0002] With the rapid development of new energy storage and power battery fields, all-solid-state lithium-ion batteries have become a key research direction for next-generation energy storage devices due to their advantages such as high theoretical energy density and high safety. Polymer-based all-solid-state electrolytes have attracted widespread attention because of their good flexibility and processability, and they are easier to achieve close contact with electrodes compared to inorganic ceramic electrolytes. However, traditional monolayer polymer solid-state electrolytes struggle to balance mechanical stability and interfacial affinity: while low molecular weight polymers offer good flexibility and can improve electrolyte / electrode interface contact, they lack mechanical strength; and while high molecular weight polymers have excellent mechanical properties, they are too rigid, resulting in poor adhesion to the electrode interface, high interfacial impedance, and impact on ion transport kinetics.

[0003] To address these issues, existing technologies have developed multilayer composite polymer electrolyte systems. These systems typically employ two or more monomers with different chemical compositions to prepare each layer of the membrane, which is then assembled using hot-pressing to form the multilayer composite structure. However, this system suffers from poor interfacial compatibility between different monomer systems, weak interlayer bonding, and cumbersome preparation processes. Meanwhile, some approaches use monomers with different ratios to construct soft-hard bonding layers, but these formulations are complex, and the differences in interlayer composition increase ion transport resistance. Furthermore, the preparation of conventional multilayer polymer electrolytes mostly involves first forming individual membranes and then hot-pressing them together, resulting in significant interfacial defects that hinder lithium-ion cross-layer transport. Moreover, the separate layer-by-layer membrane preparation method increases the process complexity, making it unsuitable for large-scale industrial production.

[0004] Therefore, it is of great significance to develop a polymer-based all-solid-state electrolyte that has a simple preparation process, tight interlayer bonding, and a good combination of high mechanical strength and good electrode interface affinity.

[0005] The above statements are merely background information related to the present invention and do not necessarily constitute prior art. Summary of the Invention

[0006] The purpose of this invention is to provide a polymer-based all-solid-state electrolyte, its preparation method, and its application.

[0007] The technical solution adopted in this invention is:

[0008] A polymer-based all-solid-state electrolyte comprises a first soft layer, a hard layer, and a second soft layer stacked sequentially. The first soft layer comprises an acrylate-methyl methacrylate copolymer and a lithium salt. The hard layer comprises an acrylate-methyl methacrylate copolymer and a lithium salt. The second soft layer comprises an acrylate-methyl methacrylate copolymer and a lithium salt. The number-average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer is greater than that of the acrylate-methyl methacrylate copolymer in the first soft layer and also greater than that of the acrylate-methyl methacrylate copolymer in the second soft layer.

[0009] Preferably, the acrylate is at least one of glycidyl acrylate, glycidyl methacrylate, and 4-(ethylene oxide-2-ylmethoxy)butyl acrylate (also known as 4-hydroxybutyl acrylate glycidyl ether).

[0010] Preferably, the number average molecular weight of the acrylate-methyl methacrylate copolymer in the first soft layer is 1000 g / mol to 9999 g / mol.

[0011] Preferably, the composition of the first soft layer further includes inorganic fast ion conductor ceramic filler.

[0012] Preferably, the number average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer is 10,000 g / mol to 100,000 g / mol.

[0013] Preferably, the hard layer further comprises inorganic fast ion conductor ceramic filler.

[0014] Preferably, the number average molecular weight of the acrylate-methyl methacrylate copolymer in the second soft layer is 1000 g / mol to 9999 g / mol.

[0015] Preferably, the composition of the second soft layer further includes inorganic fast ion conductor ceramic filler.

[0016] Preferably, the inorganic fast ion conductor ceramic filler is at least one of phosphorus-silicon-oxygen-nitrogen ion conductors, garnet-type lithium ion conductors, perovskite-type ion conductors, anti-perovskite ion conductors, and sulfide ion conductors.

[0017] Preferably, the acrylate-methyl methacrylate copolymer is copolymerized from acrylate and methyl methacrylate, and the amount of acrylate used accounts for 10% to 90% of the total mass of acrylate and methyl methacrylate.

[0018] More preferably, the acrylate-methyl methacrylate copolymer is copolymerized from acrylate and methyl methacrylate, and the amount of acrylate accounts for 50% to 70% of the total mass of acrylate and methyl methacrylate.

[0019] Preferably, the lithium salt is at least one of LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), and LiFSI (lithium bis(fluorosulfonyl)imide).

[0020] A method for preparing the polymer-based all-solid-state electrolyte as described above includes the following steps:

[0021] 1) Mix acrylate, methyl methacrylate and lithium salt evenly, or mix acrylate, methyl methacrylate, lithium salt and inorganic fast ion conductor ceramic filler evenly to obtain copolymer precursor base liquid;

[0022] 2) The initiator is added to the copolymerization precursor base solution, and the soft layer preparation solution and hard layer preparation solution are obtained by controlling the amount of initiator added. The amount of initiator added in the soft layer preparation solution is greater than that in the hard layer preparation solution.

[0023] 3) After the hard layer preparation solution is applied, a polymerization reaction is carried out to form a hard layer;

[0024] 4) After coating the soft layer preparation solution onto the two surfaces of the hard layer, a polymerization reaction is carried out to form the first soft layer and the second soft layer, thus obtaining a polymer-based all-solid electrolyte.

[0025] Preferably, the initiator in step 2) is a thermal initiator or a photoinitiator. If a thermal initiator is selected, the polymerization method is isothermal thermal polymerization, the polymerization temperature is controlled at 50℃~80℃, the polymerization time of the hard layer preparation solution is 3h~24h (preferably 3h~8h), and the polymerization time of the soft layer preparation solution is 0.5h~3h (preferably 1h~2h). If a photoinitiator is selected, the polymerization method is ultraviolet curing, the ultraviolet wavelength is 320nm~380nm, the curing temperature is ambient temperature, the photocuring time of the hard layer preparation solution is 8min~60min (preferably 30min~40min), and the photocuring time of the soft layer preparation solution is 2min~8min (preferably 3min~6min).

[0026] Preferably, the thermal initiator is azobisisobutyronitrile (AIBN).

[0027] Preferably, the photoinitiator is benzoin dimethyl ether.

[0028] Preferably, the amount of initiator added to the soft layer preparation solution in step 2) is 2.5% to 5.0% of the total mass of acrylate and methyl methacrylate.

[0029] More preferably, the amount of initiator added to the soft layer preparation solution in step 2) is 4.0% to 5.0% of the total mass of acrylate and methyl methacrylate.

[0030] Preferably, the amount of initiator added to the hard layer preparation solution in step 2) is 0.1% to 2.5% of the total mass of acrylate and methyl methacrylate.

[0031] More preferably, the amount of initiator added to the hard layer preparation solution in step 2) is 1.0% to 2.0% of the total mass of acrylate and methyl methacrylate.

[0032] An all-solid-state lithium-ion battery comprising the aforementioned polymer-based all-solid-state electrolyte.

[0033] Preferably, the positive electrode in the all-solid-state lithium-ion battery comprises a positive electrode active material, a conductive agent, and a binder.

[0034] Preferably, the positive electrode active material in the positive electrode is at least one of ternary positive electrode material, lithium iron phosphate, lithium manganese oxide, and lithium-rich manganese-based positive electrode material.

[0035] Preferably, the conductive agent in the positive electrode is at least one of super carbon black, Super P, acetylene black, carbon nanotubes, and graphene.

[0036] Preferably, the binder in the positive electrode is polyvinylidene fluoride (PVDF).

[0037] Preferably, the negative electrode in the all-solid-state lithium-ion battery comprises a negative electrode active material, a conductive agent, and a binder.

[0038] Preferably, the negative electrode active material in the negative electrode is at least one of graphite and silicon-carbon composite materials.

[0039] Preferably, the conductive agent in the negative electrode is at least one of super carbon black, Super P, acetylene black, carbon nanotubes, and graphene.

[0040] Preferably, the binder in the negative electrode is a carboxymethyl cellulose (CMC)-styrene-butadiene rubber (SBR) composite.

[0041] The beneficial effects of the present invention are: the polymer-based all-solid electrolyte of the present invention has a tight interlayer bonding, which takes into account both high mechanical strength and good electrode interface affinity, making it suitable for use in all-solid lithium-ion batteries. Moreover, its preparation process is simple, low-cost, green and pollution-free, making it suitable for large-scale industrial production and application.

[0042] Specifically:

[0043] 1) This invention forms a polymer with high ionic conductivity using acrylates. The molecular weight of the polymer is controlled by the synergistic regulation of the initiator dosage and polymerization time. Combined with a soft-hard-soft three-layer synergistic structure design, on the one hand, the middle hard layer ensures the mechanical strength and dimensional stability of the electrolyte membrane, and on the other hand, the soft layers on both sides improve the contact compatibility between the electrolyte and the electrode interface, reduce the interfacial impedance, and accelerate the lithium-ion interfacial transport kinetics. The soft layer can be tightly attached to the electrode surface, increasing the effective contact area between the active material and the electrolyte, improving the overall structural stability of the battery, and thus significantly improving the capacity and rate performance of the all-solid-state lithium-ion battery.

[0044] 2) This invention employs in-situ polymerization to directly generate soft layers on both sides of the hard layer, unlike the traditional method of independent film fabrication followed by hot-pressing composite. This creates an integrated bonding interface between the layers, resulting in strong interlayer adhesion, reduced interface defects, and improved rapid cross-layer transport of lithium ions. The high molecular weight hard polymer layer in the middle possesses excellent mechanical strength and high ionic conductivity, effectively suppressing dendrite growth and enhancing ion conduction rate. The low molecular weight soft polymer layers on both sides exhibit excellent flexibility, allowing them to closely adhere to the positive and negative electrode surfaces, increasing the effective contact area between the active material and the electrolyte, significantly reducing the electrolyte / electrode interface impedance, improving lithium ion interfacial transport dynamics, and enhancing the capacity and rate performance of the all-solid-state lithium-ion battery. Attached Figure Description

[0045] Figure 1 This is a schematic diagram of the structure of the polymer-based all-solid-state electrolyte of the present invention.

[0046] Figure 2 The image shows the infrared spectrum of the polymer-based all-solid-state electrolyte in Example 1.

[0047] Figure 3 The graph shows the cycle performance test results of the lithium-ion all-solid-state batteries in Examples 1, 4 and Comparative Example 1.

[0048] Figure 4 Impedance spectra of lithium-ion all-solid-state batteries from Examples 1, 4, and Comparative Example 1 after 30 cycles.

[0049] Explanation of reference numerals in the attached figures: 10, first soft layer; 20, hard layer; 30, second soft layer. Detailed Implementation

[0050] The present invention will be further explained and described below with reference to specific embodiments.

[0051] Example 1:

[0052] A polymer-based all-solid-state electrolyte (structural schematic diagram shown) Figure 1 As shown in the figure, its preparation method is as follows:

[0053] 1) At room temperature, 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate and LiTFSI are stirred and mixed evenly. The mass ratio of 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate and LiTFSI is 6.5:3.5:2 to obtain the copolymer precursor base liquid (transparent solution).

[0054] 2) Add azobisisobutyronitrile to the copolymerization precursor base solution and stir to mix evenly. By controlling the addition amount of azobisisobutyronitrile to 4.0 wt% (the percentage of the mass of azobisisobutyronitrile to the total mass of 4-(ethylene oxide-2-ylmethoxy)butyl acrylate and methyl methacrylate) and 1.5 wt%, respectively, soft layer preparation solution and hard layer preparation solution are obtained.

[0055] 3) After coating with the hard layer preparation liquid, the mixture is thermally polymerized at a constant temperature of 60℃ for 6 hours to form a hard layer;

[0056] 4) The soft layer preparation solution is coated on both surfaces of the hard layer and thermally polymerized at a constant temperature of 60℃ for 1.5h to form the first soft layer and the second soft layer, thus obtaining a polymer-based all-solid electrolyte.

[0057] Performance testing:

[0058] 1) The number average molecular weight of the acrylate-methyl methacrylate copolymer in the first and second soft layers was 6284 g / mol, and the number average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer was 25640 g / mol, as determined by gel permeation chromatography (GPC).

[0059] 2) The infrared spectrum of the polymer-based all-solid-state electrolyte in this embodiment is as follows: Figure 2 As shown.

[0060] Depend on Figure 2 It can be seen that the expected copolymer was obtained by polymerizing two monomers: 4-(ethylene oxide-2-ylmethoxy)butyl acrylate and methyl methacrylate.

[0061] A lithium-ion all-solid-state battery is prepared by the following method:

[0062] a) Mix ternary NCM811, acetylene black and PVDF (binder) in a mass ratio of 8:1:1, then use NMP as a solvent to prepare the positive electrode slurry, and then prepare the positive electrode;

[0063] b) Mix graphite, acetylene black and CMC / SBR (binder) in a mass ratio of 8:1:1, then use deionized water as a solvent to prepare the negative electrode slurry, and then prepare the negative electrode.

[0064] c) Using the polymer-based all-solid-state electrolyte of this embodiment as the electrolyte, a button-type all-solid-state battery is assembled in an argon glove box to obtain a lithium-ion all-solid-state battery.

[0065] Note: After the lithium-ion all-solid-state battery is manufactured, its electrochemical performance and AC impedance are tested in a constant temperature environment of 25℃. The cycle performance test voltage is 2.5V~4.1V.

[0066] Example 2:

[0067] A polymer-based all-solid-state electrolyte (structural schematic diagram shown) Figure 1 As shown in the figure, its preparation method is as follows:

[0068] 1) At room temperature, 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate and LiPF6 are stirred and mixed evenly. The mass ratio of 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate and LiPF6 is 5:5:2 to obtain the copolymer precursor base liquid (transparent solution).

[0069] 2) Azobisisobutyronitrile was added to the copolymerization precursor base solution and stirred until homogeneous. The soft layer preparation solution and hard layer preparation solution were obtained by controlling the addition amount of azobisisobutyronitrile to 4.0wt% and 1.5wt%, respectively.

[0070] 3) After coating with the hard layer preparation liquid, the mixture is thermally polymerized at a constant temperature of 60℃ for 6 hours to form a hard layer;

[0071] 4) The soft layer preparation solution is coated on both surfaces of the hard layer and thermally polymerized at a constant temperature of 60℃ for 1.5h to form the first soft layer and the second soft layer, thus obtaining a polymer-based all-solid electrolyte.

[0072] Performance testing:

[0073] GPC testing revealed that the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the first and second soft layers was 7520 g / mol, and the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer was 27834 g / mol.

[0074] A lithium-ion all-solid-state battery is prepared by the following method:

[0075] a) Mix lithium iron phosphate, acetylene black and PVDF in a mass ratio of 8:1:1, then use NMP as a solvent to prepare a positive electrode slurry, and then prepare the positive electrode;

[0076] b) Mix graphite, acetylene black and CMC / SBR in a mass ratio of 8:1:1, then use deionized water as a solvent to prepare the negative electrode slurry, and then prepare the negative electrode.

[0077] c) Using the polymer-based all-solid-state electrolyte of this embodiment as the electrolyte, a button-type all-solid-state battery is assembled in an argon glove box to obtain a lithium-ion all-solid-state battery.

[0078] Note: After the lithium-ion all-solid-state battery is manufactured, its electrochemical performance and AC impedance are tested in a constant temperature environment of 25℃. The cycle performance test voltage is 2.5V~3.9V.

[0079] Example 3:

[0080] A polymer-based all-solid-state electrolyte (structural schematic diagram shown) Figure 1 As shown in the figure, its preparation method is as follows:

[0081] 1) At room temperature, 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate, LiTFSI and garnet-type Li7La3Zr2O 12 The ceramic powder is uniformly dispersed by ultrasonication, containing 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate, LiTFSI, and garnet-type Li7La3Zr2O. 12 The ceramic powders were mixed in a mass ratio of 6.5:3.5:2:1 to obtain a copolymer precursor base liquid (transparent solution).

[0082] 2) Azobisisobutyronitrile was added to the copolymerization precursor base solution and stirred until homogeneous. The soft layer preparation solution and hard layer preparation solution were obtained by controlling the addition amount of azobisisobutyronitrile to 4.0wt% and 1.5wt%, respectively.

[0083] 3) After coating with the hard layer preparation liquid, the mixture is thermally polymerized at a constant temperature of 60℃ for 6 hours to form a hard layer;

[0084] 4) The soft layer preparation solution is coated on both surfaces of the hard layer and thermally polymerized at a constant temperature of 60℃ for 1.5h to form the first soft layer and the second soft layer, thus obtaining a polymer-based all-solid electrolyte.

[0085] Performance testing:

[0086] GPC testing revealed that the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the first and second soft layers was 6342 g / mol, and the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer was 25893 g / mol.

[0087] A lithium-ion all-solid-state battery is prepared by the following method:

[0088] a) Mix ternary NCM811, acetylene black and PVDF in a mass ratio of 8:1:1, then use NMP as a solvent to prepare the positive electrode slurry, and then prepare the positive electrode;

[0089] b) Mix graphite, acetylene black and CMC / SBR in a mass ratio of 8:1:1, then use deionized water as a solvent to prepare the negative electrode slurry, and then prepare the negative electrode.

[0090] c) Using the polymer-based all-solid-state electrolyte of this embodiment as the electrolyte, a button-type all-solid-state battery is assembled in an argon glove box to obtain a lithium-ion all-solid-state battery.

[0091] Note: After the lithium-ion all-solid-state battery is manufactured, its electrochemical performance and AC impedance are tested in a constant temperature environment of 25℃. The cycle performance test voltage is 2.5V~4.1V.

[0092] Example 4:

[0093] A polymer-based all-solid-state electrolyte (structural schematic diagram shown) Figure 1 As shown in the figure, its preparation method is as follows:

[0094] 1) At room temperature, 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate and LiFSI are stirred and mixed evenly. The mass ratio of 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate and LiFSI is 5:5:2 to obtain the copolymerization precursor base liquid (transparent solution).

[0095] 2) Add benzoin dimethyl ether to the copolymer precursor base solution and stir to mix evenly. By controlling the addition amount of benzoin dimethyl ether to 4.5wt% and 1.0wt%, respectively, soft layer preparation solution and hard layer preparation solution are obtained.

[0096] 3) After applying the hard layer preparation solution, cure it with ultraviolet light at a wavelength of 350nm for 35 minutes to form a hard layer;

[0097] 4) The soft layer preparation solution is coated on both surfaces of the hard layer and cured with ultraviolet light at a wavelength of 350 nm for 5 min to form the first soft layer and the second soft layer, thus obtaining the polymer-based all-solid electrolyte.

[0098] Performance testing:

[0099] GPC testing revealed that the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the first and second soft layers was 7488 g / mol, and the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer was 27690 g / mol.

[0100] A lithium-ion all-solid-state battery is prepared by the following method:

[0101] a) Lithium iron phosphate, acetylene black and PVDF (binder) are mixed in a mass ratio of 8:1:1, and NMP is used as a solvent to prepare the positive electrode slurry, and then the positive electrode is prepared.

[0102] b) Mix graphite, acetylene black and CMC / SBR (binder) in a mass ratio of 8:1:1, then use deionized water as a solvent to prepare the negative electrode slurry, and then prepare the negative electrode.

[0103] c) Using the polymer-based all-solid-state electrolyte of this embodiment as the electrolyte, a button-type all-solid-state battery is assembled in an argon glove box to obtain a lithium-ion all-solid-state battery.

[0104] Note: After the lithium-ion all-solid-state battery is manufactured, its electrochemical performance and AC impedance are tested in a constant temperature environment of 25℃. The cycle performance test voltage is 2.5V~4.1V.

[0105] Comparative Example 1:

[0106] A polymer-based all-solid-state electrolyte is prepared as follows:

[0107] 1) At room temperature, 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate and LiTFSI are stirred and mixed evenly. The mass ratio of 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate and LiTFSI is 6.5:3.5:2 to obtain the copolymer precursor base liquid (transparent solution).

[0108] 2) Add azobisisobutyronitrile to the copolymerization precursor base solution and stir to mix evenly. The amount of azobisisobutyronitrile added is 1.5wt%, and the hard layer preparation solution is obtained.

[0109] 3) After coating the hard layer preparation liquid, the mixture is thermally polymerized at a constant temperature of 60℃ for 6 hours to form a hard layer, thus obtaining a polymer-based all-solid electrolyte.

[0110] Performance testing:

[0111] The number-average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer was 25412 g / mol, as determined by GPC testing.

[0112] A lithium-ion all-solid-state battery is prepared by the following method:

[0113] a) Mix ternary NCM811, acetylene black and PVDF in a mass ratio of 8:1:1, then use NMP as a solvent to prepare the positive electrode slurry, and then prepare the positive electrode;

[0114] b) Mix graphite, acetylene black and CMC / SBR in a mass ratio of 8:1:1, then use deionized water as a solvent to prepare the negative electrode slurry, and then prepare the negative electrode.

[0115] c) Using the polymer-based all-solid-state electrolyte from this comparative example as the electrolyte, a coin-type all-solid-state battery was assembled in an argon glove box to obtain a lithium-ion all-solid-state battery.

[0116] Note: After the lithium-ion all-solid-state battery is manufactured, its electrochemical performance and AC impedance are tested in a constant temperature environment of 25℃. The cycle performance test voltage is 2.5V~4.1V.

[0117] Comparative Example 2:

[0118] A polymer-based all-solid-state electrolyte is prepared as follows:

[0119] 1) At room temperature, 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate and LiTFSI are stirred and mixed evenly. The mass ratio of 4-(ethylene oxide-2-ylmethoxy)butyl acrylate, methyl methacrylate and LiTFSI is 6.5:3.5:2 to obtain the copolymer precursor base liquid (transparent solution).

[0120] 2) Add azobisisobutyronitrile to the copolymerization precursor base solution and stir to mix evenly. The amount of azobisisobutyronitrile added is 4.0 wt%, and the soft layer preparation solution is obtained.

[0121] 3) After coating the soft layer preparation solution, the mixture is kept at a constant temperature of 60℃ for 1.5h to form a soft layer and obtain a polymer-based all-solid electrolyte.

[0122] Performance testing:

[0123] The number-average molecular weight of the acrylate-methyl methacrylate copolymer in the soft layer was found to be 5975 g / mol using GPC testing.

[0124] A lithium-ion all-solid-state battery is prepared by the following method:

[0125] a) Mix ternary NCM811, acetylene black and PVDF in a mass ratio of 8:1:1, then use NMP as a solvent to prepare the positive electrode slurry, and then prepare the positive electrode;

[0126] b) Mix graphite, acetylene black and CMC / SBR in a mass ratio of 8:1:1, then use deionized water as a solvent to prepare the negative electrode slurry, and then prepare the negative electrode.

[0127] c) Using the polymer-based all-solid-state electrolyte from this comparative example as the electrolyte, a coin-type all-solid-state battery was assembled in an argon glove box to obtain a lithium-ion all-solid-state battery.

[0128] Note: After the lithium-ion all-solid-state battery is manufactured, its electrochemical performance and AC impedance are tested in a constant temperature environment of 25℃. The cycle performance test voltage is 2.5V~4.1V.

[0129] Comparative Example 3:

[0130] A polymer-based all-solid-state electrolyte is prepared as follows:

[0131] 1) Methyl methacrylate and LiTFSI were stirred and mixed evenly at room temperature. The mass ratio of methyl methacrylate to LiTFSI was 5:1 to obtain the copolymer precursor base liquid (transparent solution).

[0132] 2) Azobisisobutyronitrile was added to the copolymerization precursor base solution and stirred until homogeneous. The soft layer preparation solution and hard layer preparation solution were obtained by controlling the addition amount of azobisisobutyronitrile to 4.0wt% and 1.5wt%, respectively.

[0133] 3) After coating with the hard layer preparation liquid, the mixture is thermally polymerized at a constant temperature of 60℃ for 6 hours to form a hard layer;

[0134] 4) The soft layer preparation solution is coated on both surfaces of the hard layer and thermally polymerized at a constant temperature of 60℃ for 1.5h to form the first soft layer and the second soft layer, thus obtaining a polymer-based all-solid electrolyte.

[0135] Performance testing:

[0136] GPC testing revealed that the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the first and second soft layers was 5634 g / mol, and the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer was 25115 g / mol.

[0137] A lithium-ion all-solid-state battery is prepared by the following method:

[0138] a) Mix ternary NCM811, acetylene black and PVDF in a mass ratio of 8:1:1, then use NMP as a solvent to prepare the positive electrode slurry, and then prepare the positive electrode;

[0139] b) Mix graphite, acetylene black and CMC / SBR in a mass ratio of 8:1:1, then use deionized water as a solvent to prepare the negative electrode slurry, and then prepare the negative electrode.

[0140] c) Using the polymer-based all-solid-state electrolyte from this comparative example as the electrolyte, a coin-type all-solid-state battery was assembled in an argon glove box to obtain a lithium-ion all-solid-state battery.

[0141] Note: After the lithium-ion all-solid-state battery is manufactured, its electrochemical performance and AC impedance are tested in a constant temperature environment of 25℃. The cycle performance test voltage is 2.5V~4.1V.

[0142] Performance testing:

[0143] The cycle performance test results of the lithium-ion all-solid-state batteries in Examples 1, 4, and Comparative Example 1 are shown in the figure below. Figure 3 As shown, the impedance spectra of the lithium-ion all-solid-state batteries in Examples 1, 4, and Comparative Example 1 after 30 cycles are as follows. Figure 4 As shown in the table below, the tensile strength and ionic conductivity of the polymer-based all-solid-state electrolytes in Examples 1-4 and Comparative Examples 1-3, as well as the capacity retention (cycle performance) of the lithium-ion all-solid-state batteries in Examples 1-4 and Comparative Examples 1-3, are all tested.

[0144] Table 1. Test data for tensile strength, ionic conductivity, and capacity retention.

[0145]

[0146] Note:

[0147] Tensile strength: The polymer-based all-solid electrolyte sample was cut into a standard dumbbell-shaped tensile specimen with a total length of 75 mm, a gauge length of 20 mm, a gauge width of 4 mm, and a thickness of 100 μm. The tensile rate was 5 mm / min, and the tensile test was terminated when the specimen completely broke. The maximum tensile force at the time of breakage of each specimen was recorded. The tensile strength was obtained by dividing the maximum tensile force by the cross-sectional area of ​​the specimen.

[0148] Ionic conductivity: The polymer-based all-solid electrolyte sample was cut into circular sheets with a diameter of 16 mm and a thickness of 100 μm in an anhydrous and oxygen-free argon glove box. Two stainless steel discs, each with a diameter of 16 mm, were used as blocking electrodes, which were completely attached to the electrolyte. The test was conducted at a constant temperature of 25 °C using an electrochemical workstation with a scanning frequency range of 10 Hz. 6 Hz~10 -1 Hz, amplitude is 5mV.

[0149] Capacity retention rate: The lithium-ion all-solid-state batteries in Examples 1-4 and Comparative Examples 1-3 were placed at 25°C (room temperature) and subjected to charge-discharge cycle tests at a charge-discharge rate of 0.5C / 0.5C. Except for Example 2, where the charge-discharge voltage was 2.5V-3.9V, the others were 2.5V-4.1V. The capacity retention rate was obtained by recording the discharge capacity of the 50th cycle and dividing it by the discharge capacity of the 1st cycle.

[0150] Depend on Figure 3 , Figure 4 As shown in Table 1:

[0151] 1) The polymer-based all-solid electrolytes in Examples 1 to 4 have high tensile strength and excellent ionic conductivity, which are beneficial to improving the stability and cycle life of lithium-ion all-solid batteries. The polymerization of acrylate monomers can form polymers with high ionic conductivity, which improves the conduction rate of lithium ions in solid electrolytes.

[0152] 2) The polymer-based all-solid electrolyte in Comparative Example 3 was prepared using monomers that did not contain 4-(ethylene oxide-2-ylmethoxy)butyl acrylate and had no epoxy side chain structure. The ability of the polymer chain segments to conduct lithium ions was greatly reduced, and its ionic conductivity was significantly lower than that of the polymer-based all-solid electrolyte in Example 1.

[0153] 3) Comparing the polymer-based all-solid-state electrolytes in Example 1, Comparative Example 1 and Comparative Example 2, it can be seen that the strength of the soft layer is significantly lower than that of the hard layer, which is beneficial for achieving a tight fit with the porous electrode;

[0154] 4) Comparing the polymer-based all-solid-state electrolytes in Example 1, Example 4 and Comparative Example 1, it can be seen that the soft layers on both sides in the soft-hard-soft structure design can improve the contact compatibility between the electrolyte and the electrode interface, reduce the interface impedance, and accelerate the lithium-ion interface transport dynamics, thereby improving the capacity retention of lithium-ion all-solid-state batteries.

[0155] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A polymer-based all-solid-state electrolyte, characterized in that, The composition includes a first soft layer, a hard layer, and a second soft layer stacked sequentially; the first soft layer comprises an acrylate-methyl methacrylate copolymer and a lithium salt; the hard layer comprises an acrylate-methyl methacrylate copolymer and a lithium salt; the second soft layer comprises an acrylate-methyl methacrylate copolymer and a lithium salt; the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer is greater than that of the acrylate-methyl methacrylate copolymer in the first soft layer, and also greater than that of the acrylate-methyl methacrylate copolymer in the second soft layer.

2. The polymer-based all-solid-state electrolyte according to claim 1, characterized in that: The acrylate is at least one of glycidyl acrylate, glycidyl methacrylate, and 4-(ethylene oxide-2-ylmethoxy)butyl acrylate.

3. The polymer-based all-solid-state electrolyte according to claim 1 or 2, characterized in that: The number-average molecular weight of the acrylate-methyl methacrylate copolymer in the first soft layer is 1000 g / mol to 9999 g / mol; and / or, the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the hard layer is 10000 g / mol to 100000 g / mol; and / or, the number-average molecular weight of the acrylate-methyl methacrylate copolymer in the second soft layer is 1000 g / mol to 9999 g / mol.

4. The polymer-based all-solid-state electrolyte according to claim 1 or 2, characterized in that: The acrylate-methyl methacrylate copolymer is copolymerized from acrylate and methyl methacrylate, with the amount of acrylate accounting for 10% to 90% of the total mass of acrylate and methyl methacrylate.

5. The polymer-based all-solid-state electrolyte according to claim 1 or 2, characterized in that: The lithium salt is at least one of LiPF6, LiBF4, LiClO4, LiTFSI, and LiFSI.

6. The polymer-based all-solid-state electrolyte according to claim 1 or 2, characterized in that: The first soft layer further comprises inorganic fast ion conductor ceramic filler; and / or, the hard layer further comprises inorganic fast ion conductor ceramic filler; and / or, the second soft layer further comprises inorganic fast ion conductor ceramic filler.

7. A method for preparing a polymer-based all-solid-state electrolyte as described in any one of claims 1 to 6, characterized in that, Includes the following steps: 1) Mix acrylate, methyl methacrylate and lithium salt evenly, or mix acrylate, methyl methacrylate, lithium salt and inorganic fast ion conductor ceramic filler evenly to obtain copolymer precursor base liquid; 2) The initiator is added to the copolymerization precursor base solution, and the soft layer preparation solution and hard layer preparation solution are obtained by controlling the amount of initiator added. The amount of initiator added in the soft layer preparation solution is greater than that in the hard layer preparation solution. 3) After the hard layer preparation solution is applied, a polymerization reaction is carried out to form a hard layer; 4) After coating the soft layer preparation solution onto the two surfaces of the hard layer, a polymerization reaction is carried out to form the first soft layer and the second soft layer, thus obtaining a polymer-based all-solid electrolyte.

8. The preparation method according to claim 7, characterized in that: Step 2) The initiator is a thermal initiator or a photoinitiator.

9. The preparation method according to claim 7 or 8, characterized in that: In step 2), the amount of initiator added to the soft layer preparation solution is 2.5% to 5.0% of the total mass of acrylate and methyl methacrylate; and / or, in step 2), the amount of initiator added to the hard layer preparation solution is 0.1% to 2.5% of the total mass of acrylate and methyl methacrylate.

10. A fully solid-state lithium-ion battery, characterized in that, It includes the polymer-based all-solid-state electrolyte according to any one of claims 1 to 6.