A method for fabricating a solar cell

By forming multiple layers of low-thickness photosensitive emulsion films on the surface of the solar cell substrate and performing multiple printing exposures, the problem of uneven copper grid line thickness was solved, achieving uniformity of metal grid line width and improving solar cell conversion efficiency.

CN123124482APending Publication Date: 2026-11-17TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510622515.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, uneven copper grid lines lead to low solar cell conversion efficiency, mainly due to the difficulty in controlling the bottom width of the patterned grooves.

Method used

By employing a segmented processing method, multiple layers of low-thickness photosensitive adhesive film are formed on the surface of the solar cell substrate. Metal grid pattern is formed by printing and exposure in stages to ensure uniform exposure and cross-linking reaction of the photosensitive adhesive layer and control the width uniformity of the patterned grooves.

Benefits of technology

It improves the uniformity of the width of the metal grid lines and the conversion efficiency of the solar cell, reduces light scattering and lateral diffusion during the development process, and enhances the photoelectric conversion performance of the cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124482A_ABST
    Figure CN123124482A_ABST
Patent Text Reader

Abstract

This application relates to a method for fabricating a solar cell, comprising: forming a photosensitive adhesive layer on the surface of a solar cell substrate; performing a first printing exposure on a first region of the photosensitive adhesive layer, the first region being the region outside a first grid line pattern, the first grid line pattern being identical to a preset grid line pattern, and the grid line width corresponding to the first grid line pattern being greater than the grid line width corresponding to the preset grid line pattern; and performing a second printing exposure on a second region of the photosensitive adhesive layer after the first printing exposure, the second region being the region outside a second grid line pattern, the second grid line pattern being identical to the preset grid line pattern, and the grid line width corresponding to the second grid line pattern being equal to the grid line width corresponding to the preset grid line pattern. This application can effectively improve the width uniformity of the metal grid lines in the solar cell, thereby improving the conversion efficiency of the solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of solar cell manufacturing technology, and in particular to a method for preparing a solar cell. Background Technology

[0002] In related technologies, to achieve cost reduction and efficiency improvement, the fabrication process of heterojunction solar cells is as follows: A copper seed layer is first deposited on a TCO (Transparent Conductive Oxides) film using PVD (Physical Vapor Deposition) sputtering technology for conductivity. Next, a photosensitive adhesive layer is coated onto the copper seed layer and exposed during printing. Then, patterned grooves are formed on the photosensitive adhesive layer through development, and copper grid lines are electroplated within these patterned grooves. However, because the width of the bottom of the patterned grooves is difficult to control, the electroplated copper grid lines tend to be uneven in thickness, resulting in low conversion efficiency of the solar cell. Summary of the Invention

[0003] This application provides a method for fabricating a solar cell, which can effectively improve the uniformity of the width of the metal grid lines in the solar cell, thereby improving the conversion efficiency of the solar cell.

[0004] The method for preparing a solar cell provided in this application includes:

[0005] A photosensitive adhesive layer is formed on the surface of the solar cell substrate;

[0006] A first printing exposure is performed on a first area of ​​the photosensitive adhesive layer. The first area is the area outside the first grid line pattern. The first grid line pattern is the same as the preset grid line pattern, and the grid line width corresponding to the first grid line pattern is greater than the grid line width corresponding to the preset grid line pattern.

[0007] A second printing exposure is performed on the second region of the photosensitive emulsion layer after the first printing exposure. The second region is the region outside the second grid line pattern. The second grid line pattern is the same as the preset grid line pattern, and the grid line width corresponding to the second grid line pattern is equal to the grid line width corresponding to the preset grid line pattern.

[0008] In some implementations, the first printing exposure satisfies at least one of the following (i) to (iii):

[0009] (i) The width of the gate line corresponding to the first gate line pattern is 3μm to 5μm larger than the width of the gate line corresponding to the preset gate line pattern;

[0010] (ii) The exposure energy of the first printing exposure is 70 mJ / cm². 2 ~100mj / cm2 ;

[0011] (iii) The exposure time of the first printing exposure is 250ms to 350ms.

[0012] In some embodiments, the second printing exposure satisfies at least one of the following (iv) to (vii):

[0013] (iv) The exposure energy for the second printing exposure is 80 mJ / cm². 2 ~100mj / cm 2 ;

[0014] (v) The exposure energy of the second printing exposure is greater than or equal to the exposure energy of the first printing exposure;

[0015] (vi) The exposure time for the second printing exposure is 250ms to 350ms;

[0016] (vii) The exposure time of the second printing exposure is equal to the exposure time of the first printing exposure.

[0017] In some implementations, the first printing exposure satisfies at least one of the following (viii) to (ix), and the second printing exposure satisfies at least one of the following (x) to (xi):

[0018] (viii) The first printing exposure is performed using a first mask, wherein the first mask and the photosensitive adhesive layer have a first gap in the thickness direction of the solar cell substrate;

[0019] (ix) In (viii), the width of the first gap in the thickness direction is 60 μm to 80 μm;

[0020] (x) The second printing exposure is performed using a second mask, wherein the second mask and the photosensitive adhesive layer have a second gap in the thickness direction of the solar cell substrate;

[0021] (xi) In (x), the width of the second gap in the thickness direction is 60 μm to 80 μm.

[0022] In some embodiments, the width of the first gap in the thickness direction is equal to the width of the second gap in the thickness direction.

[0023] In some embodiments, the photosensitive adhesive layer comprises multiple layers of photosensitive adhesive films sequentially stacked in the thickness direction of the solar cell substrate;

[0024] The process of forming a photosensitive adhesive layer on the surface of a solar cell substrate includes sequentially forming multiple layers of the photosensitive adhesive film on the surface of the solar cell substrate.

[0025] Forming the photosensitive film includes:

[0026] Photosensitive adhesive is coated onto the surface of the solar cell substrate or the surface of the previously formed photosensitive adhesive film;

[0027] The coated photosensitive emulsion is baked to form a photosensitive emulsion film.

[0028] In some embodiments, the photosensitive adhesive layer comprises a first photosensitive adhesive film and a second photosensitive adhesive film sequentially stacked in the thickness direction of the solar cell substrate;

[0029] The process of forming a photosensitive adhesive layer on the surface of a solar cell substrate includes:

[0030] The first photosensitive film is formed on the surface of the solar substrate;

[0031] The second photosensitive film is formed on the first photosensitive film.

[0032] In some embodiments, forming the first photosensitive adhesive film on the surface of the solar substrate includes coating the surface of the solar cell substrate with photosensitive adhesive; and subjecting the photosensitive adhesive coated on the surface of the solar cell substrate to a first baking treatment to form the first photosensitive adhesive film.

[0033] The step of forming a second photosensitive film on the first photosensitive film includes coating a photosensitive adhesive onto the surface of the first photosensitive film; and subjecting the photosensitive adhesive coated onto the surface of the first photosensitive film to a second baking treatment to form the second photosensitive film.

[0034] In some embodiments, the formation of the photosensitive adhesive layer on the surface of the solar cell substrate satisfies at least one of the following (xii) to (xiv):

[0035] (xii) The thickness of the first photosensitive film is 6μm to 8μm;

[0036] (xiii) The temperature of the first baking treatment is 95℃~105℃;

[0037] (xiv) The duration of the first baking treatment is 2 min to 3 min.

[0038] In some embodiments, the formation of the photosensitive adhesive layer on the surface of the solar cell substrate satisfies at least one of the following (xv) to (xvii):

[0039] (xv) The thickness of the photosensitive adhesive layer is 14μm to 16μm;

[0040] (xvi) The temperature of the second baking treatment is 105℃~115℃;

[0041] (xvii) The duration of the second baking treatment is 3 min to 4 min.

[0042] Compared with the prior art, the beneficial effects of the embodiments of this application are as follows: the method for preparing the solar cell includes: forming a photosensitive adhesive layer on the surface of a solar cell substrate; performing a first printing exposure on a first region of the photosensitive adhesive layer, the first region being the region outside the first grid line pattern, the first grid line pattern being the same as a preset grid line pattern, and the grid line width corresponding to the first grid line pattern being greater than the grid line width corresponding to the preset grid line pattern; performing a second printing exposure on a second region of the photosensitive adhesive layer after the first printing exposure, the second region being the region outside the second grid line pattern, the second grid line pattern being the same as the preset grid line pattern, and the grid line width corresponding to the second grid line pattern being equal to the grid line width corresponding to the preset grid line pattern. Based on the above technical solution, the first grid pattern is the same as the second grid pattern, but the grid width corresponding to the first grid pattern is greater than the grid width corresponding to the second grid pattern. Therefore, the first region is located within the second region. During the second printing exposure, the first region will be exposed again, which can ensure that the first region of the photosensitive adhesive layer is fully exposed, improve the cross-linking effect at the bottom of the first region, and make the cross-linking reaction at the bottom of the first region more uniform. This prevents the first region of the photosensitive adhesive layer from being dissolved during the subsequent development process, thereby controlling the width of the metal grid lines of the solar cell within the grid width corresponding to the first grid pattern, effectively improving the uniformity of the width of the metal grid lines of the solar cell and the conversion efficiency of the solar cell. Attached Figure Description

[0043] Figure 1 This is a schematic flowchart illustrating a method for fabricating a solar cell according to an embodiment of this application.

[0044] Figure 2 This is a schematic diagram of the solar cell substrate structure provided in step S11 of one embodiment of this application.

[0045] Figure 3 This is a schematic diagram of the structure of the intermediate obtained in step S111 in one embodiment of this application.

[0046] Figure 4 This is a schematic diagram of the structure of the intermediate obtained in step S112 in one embodiment of this application.

[0047] Figure 5 This is a schematic diagram of the structure of the intermediate obtained in step S12 of one embodiment of this application.

[0048] Figure 6 This is a schematic diagram of the principle of step S12 in one embodiment of this application.

[0049] Figure 7 This is a schematic diagram of the structure of the intermediate obtained in step S13 of one embodiment of this application.

[0050] Figure 8 This is a schematic diagram of the principle of step S13 in one embodiment of this application.

[0051] Figure 9 This is a schematic diagram of the structure of the intermediate obtained in step S14 of one embodiment of this application.

[0052] Figure 10 This is a schematic diagram of the structure of the solar cell obtained in step S15 of one embodiment of this application.

[0053] Figure 11 This is a scanning electron microscope image of the patterned groove cross-section in the intermediate obtained in Example 1.

[0054] Figure 12 The image shows a scanning electron microscope (SEM) image of the patterned groove cross-section in the intermediate obtained in Comparative Example 1.

[0055] Figure 13 This is a scanning electron microscope image of the cross-section of the copper grid lines in the solar cell obtained in Comparative Example 1. Detailed Implementation

[0056] To facilitate understanding of this application, a more complete description will be provided below with reference to the accompanying drawings. Preferred embodiments of this application are shown in the drawings. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of this application.

[0057] It should be noted that when a component is said to be "fixed to" another component, it can be directly attached to the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component.

[0058] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein in the specification of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application.

[0059] As used in this article, the description of "a1~a2" means "greater than or equal to a1" and "less than or equal to a2". For example, if x is 0~1, it means: 0≤x≤1.

[0060] like Figure 1As shown, this is a method for preparing a solar cell according to one embodiment of this application.

[0061] like Figure 1 As shown, the method for fabricating this solar cell includes the following steps S11 to S13:

[0062] Step S11: A photosensitive adhesive layer 200 is formed on the surface of the solar cell substrate 100.

[0063] In some embodiments, the solar cell substrate 100 can be a heterojunction (HJT) cell substrate. Please refer to [reference needed]. Figure 2 As shown, the solar cell substrate 100 includes a silicon wafer substrate 110, a first intrinsic amorphous silicon layer 120 stacked on the upper surface of the silicon wafer substrate 110, a second intrinsic amorphous silicon layer 130 stacked on the lower surface of the silicon wafer substrate 110, an N-type doped amorphous silicon layer 140 stacked on the side of the first intrinsic amorphous silicon layer 120 away from the silicon wafer substrate 110, a P-type doped amorphous silicon layer 150 stacked on the side of the second intrinsic amorphous silicon layer 130 away from the silicon wafer substrate 110, a first conductive layer 160 stacked on the side of the N-type doped amorphous silicon layer 140 away from the silicon wafer substrate 110, a second conductive layer 170 stacked on the side of the P-type doped amorphous silicon layer 150 away from the silicon wafer substrate 110, and metal seed layers 180 respectively stacked on the side of the first conductive layer 160 away from the silicon wafer substrate 110 and the side of the second conductive layer 170 away from the silicon wafer substrate 110. As an example, the metal seed layer 180 can be a copper seed layer. The photosensitive adhesive layer 200 is formed on the side of the metal seed layer 180 away from the silicon substrate 110.

[0064] In some embodiments, the photosensitive adhesive layer 200 includes multiple photosensitive adhesive films sequentially stacked in the thickness direction of the solar cell substrate 100.

[0065] In this embodiment, step S11 specifically includes: sequentially forming multiple layers of photosensitive adhesive film on the surface of the solar cell substrate 100.

[0066] The formation of the photosensitive film includes:

[0067] Photosensitive adhesive is coated onto the surface of the solar cell substrate 100 or the surface of the previously formed photosensitive adhesive film;

[0068] The coated photosensitive emulsion is baked to form a photosensitive emulsion film.

[0069] In related technologies, the coating process utilizes high film thickness technology, achieving a photosensitive emulsion layer thickness exceeding 10 μm. During the baking process, the heat radiation from the oven triggers the evaporation of solvents in the photosensitive emulsion. However, this heat radiation propagates from top to bottom, and its intensity gradually decreases. Consequently, the solvent evaporation rate differs between the top and bottom of the photosensitive emulsion layer after baking, resulting in a higher residual solvent content at the bottom than at the top. The thicker the photosensitive emulsion layer, the greater this difference in residual solvent content. This residual solvent affects the refractive index of the photosensitive emulsion layer, interfering with light propagation during subsequent printing exposure. It causes light scattering or attenuation during penetration, leading to uneven exposure. Consequently, the portion near the top of the photosensitive emulsion layer is fully cross-linked, while the portion near the bottom is under-cross-linked. This leads to the following situation during the subsequent development process: the developer not only dissolves the unexposed photosensitive emulsion, but also causes a certain lateral diffusion effect on the photosensitive emulsion in the exposed area that has not fully cross-linked. This lateral diffusion causes the bottom width of the patterned groove to widen, resulting in uneven thickness of the subsequently formed metal grid lines and reducing the photoelectric conversion efficiency of the solar cell.

[0070] In this embodiment, a segmented processing method is adopted to divide the high-thickness photosensitive adhesive layer 200 into multiple layers of low-thickness photosensitive adhesive films stacked sequentially. During the baking process, the solvent in the low-thickness photosensitive adhesive films is more easily and completely removed, minimizing the amount of solvent residue at the bottom of the photosensitive adhesive layer 200. This reduces light diffraction and scattering reactions during the printing exposure process, resulting in more uniform exposure of the photosensitive adhesive layer 200. Consequently, the width uniformity of the patterned groove 201 is high, which in turn improves the uniformity of the width of the subsequently formed metal grid lines 400, thereby improving the photoelectric conversion efficiency of the solar cell.

[0071] As one implementation method, the thickness of each layer of photosensitive film can be approximately the same, which not only simplifies the process but also allows the solvent in each layer of photosensitive film to be removed more uniformly.

[0072] In some embodiments, the photosensitive adhesive layer 200 includes a first photosensitive adhesive film 210 and a second photosensitive adhesive film 220, which are sequentially stacked in the thickness direction of the solar cell substrate 100. The thickness of the photosensitive adhesive layer 200 is 14 μm to 16 μm, and the thickness of the first photosensitive adhesive film 210 is 6 μm to 8 μm. The thickness of the second photosensitive adhesive film 220 is the difference between the thickness of the photosensitive adhesive layer 200 and the thickness of the first photosensitive adhesive film 210. As an example, the thickness of the photosensitive adhesive layer 200 can be, but is not limited to, 14 μm, 15 μm, or 16 μm. The thickness of the first photosensitive adhesive film 210 can be, but is not limited to, 6 μm, 7 μm, or 8 μm.

[0073] In this embodiment, step S11 specifically includes steps S111 to S112:

[0074] Step S111: Form the first photosensitive film 210 on the surface of the solar substrate. Please refer to [link / reference]. Figure 3 As shown.

[0075] Specifically, step S111 may include steps S1111 to S1112:

[0076] Step S1111: Apply photosensitive adhesive to the surface of the solar cell substrate 100.

[0077] Step S1112: The photosensitive adhesive coated on the surface of the solar cell substrate 100 is subjected to a first baking treatment to form a first photosensitive adhesive film 210.

[0078] In one embodiment, the temperature of the first baking treatment is 95°C to 105°C. As an example, the temperature of the first baking treatment can be, but is not limited to, 95°C, 98°C, 100°C, 102°C, 104°C, or 105°C.

[0079] In one implementation, the duration of the first baking process is 2 to 3 minutes. As an example, the duration of the first baking process can be, but is not limited to, 2 minutes, 2.5 minutes, or 3 minutes.

[0080] Step S112: Form a second photosensitive film 220 on the first photosensitive film 210. Please refer to [link / reference]. Figure 4 As shown.

[0081] Specifically, step S112 may include steps S1121 to S1122:

[0082] Step S1121: Photosensitive adhesive is coated on the surface of the first photosensitive film 210.

[0083] Step S1122: The photosensitive adhesive coated on the surface of the first photosensitive film 210 is subjected to a second baking treatment to form a second photosensitive film 220.

[0084] In one embodiment, the temperature of the second baking treatment is 105°C to 115°C. As an example, the temperature of the first baking treatment can be, but is not limited to, 105°C, 108°C, 110°C, 112°C, 114°C, or 115°C.

[0085] In one implementation, the second baking process lasts for 3 to 4 minutes. As an example, the first baking process can last for, but is not limited to, 3 minutes, 3.5 minutes, or 4 minutes.

[0086] In this embodiment, the high-thickness photosensitive adhesive layer 200 is divided into a low-thickness first photosensitive adhesive film 210 and a low-thickness photosensitive adhesive film 220. The first photosensitive adhesive film 210 is first coated and baked to thoroughly remove the solvent from it. Then, the second photosensitive adhesive film 220 is coated and baked to thoroughly remove the solvent from it, thereby thoroughly removing the solvent from the photosensitive adhesive layer 200 and minimizing the amount of solvent residue at the bottom of the photosensitive adhesive layer 200.

[0087] Step S12: Perform a first printing exposure on the first region 200a of the photosensitive adhesive layer 200. The first region 200a is the area outside the first grating pattern 200b. The first grating pattern 200b is the same as the preset grating pattern, and the grating width W1 corresponding to the first grating pattern 200b is greater than the grating width corresponding to the preset grating pattern. Please refer to [reference needed]. Figure 5 As shown.

[0088] The designed first grid line pattern 200b is laser-printed onto the photosensitive adhesive layer 200 and then exposed. The first region 200a of the photosensitive adhesive layer 200 undergoes photosensitive denaturation, distinguishing it from the unexposed region (i.e., the first grid line pattern 200b), thus forming the first grid line pattern 200b on the photosensitive adhesive layer 200. Please refer to [reference needed]. Figure 6 As shown.

[0089] Step S13: Perform a second printing exposure on the second region 200c of the photosensitive adhesive layer 200 after the first printing exposure. The second region 200c is the region outside the second grating pattern 200d. The second grating pattern 200d is the same as the preset grating pattern, and the grating width W2 corresponding to the second grating pattern 200d is equal to the grating width corresponding to the preset grating pattern. Please refer to [reference needed]. Figure 7 As shown.

[0090] The designed second grid pattern 200d is laser-printed onto the photosensitive adhesive layer 200 and then exposed. The second region 200c of the photosensitive adhesive layer 200 undergoes photoreactivity, becoming distinct from the unexposed region (i.e., the second grid pattern 200d), thus forming the second grid pattern 200d on the photosensitive adhesive layer 200. Please refer to [reference needed]. Figure 8 As shown. The second grid pattern 200d is the same as the preset grid pattern, and the grid width W2 corresponding to the second grid pattern 200d is equal to the grid width corresponding to the preset grid pattern. In other words, the second grid pattern 200d is the preset grid pattern, and the second printing exposure can form the preset grid pattern on the photosensitive adhesive layer 200.

[0091] During the printing exposure process under high film thickness conditions, light cannot penetrate the entire exposure area of ​​the photosensitive emulsion layer 200 uniformly. Light scattering or attenuation during penetration leads to uneven cross-linking reactions. The portion near the top of the photosensitive emulsion layer 200 is fully cross-linked, while the portion near the bottom is insufficiently cross-linked. Consequently, during subsequent development, the developer not only dissolves the unexposed photosensitive emulsion but also causes lateral diffusion to the insufficiently cross-linked photosensitive emulsion in the exposed area. This lateral diffusion results in a wider bottom width of the patterned groove 201.

[0092] In this embodiment, both the first gate pattern 200b and the second gate pattern 200d are identical to the preset gate pattern. Furthermore, the gate width W1 corresponding to the first gate pattern 200b is greater than the gate width corresponding to the preset gate pattern, and the gate width W2 corresponding to the second gate pattern 200d is equal to the gate width corresponding to the preset gate pattern. That is, the first region 200a is located within the second region 200c. In addition to including the first region 200a, the second region 200c also includes a third region 200e, which is the region between the first region 200a and the preset gate pattern (the second gate pattern 200d).

[0093] If only one printing exposure is performed, the cross-linking reaction at the bottom of the photosensitive adhesive layer 200 is not as strong as that at the top, resulting in lateral diffusion during subsequent development. This diffusion area is uncontrolled and continues to spread laterally. In this embodiment, the first region 200a is exposed for the first printing exposure. During the second printing exposure, the second region 200c (comprising the first region 200a and the third region 200e) is exposed. In other words, during the second printing exposure, the first region 200a is exposed again, while the third region 200e is exposed for the first time, ensuring sufficient exposure for the first region 200a. During subsequent development, the maximum lateral diffusion area is limited to the third region 200e and does not continue to spread laterally into the first region 200a. This allows for more precise control over the bottom morphology and width of the patterned groove 201 formed during development.

[0094] In some embodiments, the gate line width W1 corresponding to the first gate line pattern 200b is 3μm to 5μm larger than the gate line width corresponding to the preset gate line pattern. As an example, the difference between the gate line width W1 corresponding to the first gate line pattern 200b and the gate line width corresponding to the preset gate line pattern can be, but is not limited to, 3μm, 4μm or 5μm.

[0095] In some implementations, the exposure energy of the first printing exposure is 70 mJ / cm². 2 ~100mj / cm 2As an example, the exposure energy of the first printing exposure can be, but is not limited to, 70 mJ / cm². 2 80mj / cm 2 90mj / cm 2 Or 100mJ / cm 2 .

[0096] In some implementations, the exposure time of the first printing exposure is 250ms to 350ms. As an example, the exposure time of the first printing exposure can be, but is not limited to, 250ms, 260ms, 280ms, 290ms, 300ms, 320ms, 340ms, or 350ms.

[0097] In some implementation methods, please refer to Figure 6 As shown, in step 12, a first printing exposure is performed using a first mask 310, and the first mask 310 and the photosensitive adhesive layer 200 have a first gap in the thickness direction of the solar cell substrate 100.

[0098] In one implementation, the width of the first gap in the thickness direction is 60 μm to 80 μm. As an example, the width of the first gap in the thickness direction can be, but is not limited to, 60 μm, 70 μm, or 80 μm.

[0099] In this embodiment, the first gap determines the focal length of the first printing exposure, which directly affects the size and morphology of the subsequently formed patterned groove 201. In this embodiment, the width of the first gap in the thickness direction is 60μm to 80μm, which allows the size and morphology of the patterned groove 201 to be in an optimal state.

[0100] In some implementations, the exposure energy for the second printing exposure is 80 mJ / cm². 2 ~100mj / cm 2 As an example, the exposure energy for the second printing exposure can be, but is not limited to, 80 mJ / cm². 2 90mj / cm 2 Or 100mJ / cm 2 .

[0101] In some implementations, the exposure time of the second printing exposure is 250ms to 350ms. As an example, the exposure time of the second printing exposure can be, but is not limited to, 250ms, 260ms, 280ms, 290ms, 300ms, 320ms, 340ms, or 350ms.

[0102] In some implementation methods, please refer to Figure 8As shown, in step S13, a second printing exposure is performed using a second mask 320, and the second mask 320 and the photosensitive adhesive layer 200 have a second gap in the thickness direction of the solar cell substrate 100.

[0103] In one implementation, the width of the second gap in the thickness direction is 60 μm to 80 μm. As an example, the width of the second gap in the thickness direction can be, but is not limited to, 60 μm, 70 μm, or 80 μm.

[0104] In one implementation, the width of the first gap in the thickness direction can be equal to the width of the second gap in the thickness direction.

[0105] In this embodiment, the second gap determines the focal length of the second printing exposure, which directly affects the size and morphology of the subsequently formed patterned groove 201. In this embodiment, the width of the second gap in the thickness direction is 60μm to 80μm, which allows the size and morphology of the patterned groove 201 to be in an optimal state.

[0106] In one implementation, the exposure time of the second printing exposure is equal to the exposure time of the first printing exposure.

[0107] In this embodiment, the exposure time of the second printing exposure is equal to the exposure time of the first printing exposure. The total light intensity received by the photosensitive emulsion layer 200 can be controlled by adjusting the exposure energy of the two printing exposures, which can increase the process tolerance to a certain extent, allowing for some fluctuations without significantly affecting the final result. The exposure energy of the second printing exposure can be greater than that of the first printing exposure, allowing the third region 200e to harden more thoroughly, thereby further reducing lateral diffusion during the development process. Alternatively, the exposure energy of the second printing exposure can be equal to that of the first printing exposure.

[0108] In some embodiments, after step S13, the method for fabricating a solar cell further includes steps S14 to S15:

[0109] Step S14: Remove the grid line region (the region other than the second region 200c) of the photosensitive adhesive layer 200 to form a patterned groove 201 on the photosensitive adhesive layer 200. Please refer to [link / reference]. Figure 9 As shown.

[0110] As one implementation, step S14 specifically includes: using a sodium carbonate solution to clean and remove the unexposed photosensitive adhesive layer 200 (grid line area) to form a patterned groove 201, exposing the metal seed layer 180 of the grid line area.

[0111] Step S15: Electroplating is performed to form metal grid lines 400 within the patterned groove 201. Please refer to [reference needed]. Figure 10 As shown.

[0112] In one embodiment, the metal grid line 400 is electroplated in a copper sulfate electroplating solution. The metal grid line 400 can be a copper grid line.

[0113] The present application will be further illustrated below through specific embodiments and comparative examples.

[0114] Example 1

[0115] This embodiment provides a method for fabricating a solar cell, including the following steps:

[0116] Step 1-1: The silicon substrate 110 is texturized and cleaned to form a uniform "positive pyramid" textured surface on the silicon wafer. The silicon substrate 110 is an N-type single-crystal silicon wafer, and the base size of the pyramid structure of the textured surface is 2μm to 8μm.

[0117] In steps 1-2, a first intrinsic amorphous silicon layer 120 and an N-type doped amorphous silicon layer 140 are sequentially deposited on the upper surface of the texturized silicon wafer substrate 110 using a PECVD plasma deposition equipment. A second intrinsic amorphous silicon layer 130 and a P-type doped amorphous silicon layer 150 are sequentially deposited on the lower surface of the texturized silicon wafer substrate 110 using the same PECVD equipment. The thickness of the first intrinsic amorphous silicon layer 120 is 3 nm to 6 nm, the thickness of the second intrinsic amorphous silicon layer 130 is 3 nm to 9 nm, the thickness of the N-type doped amorphous silicon layer 140 is 5 nm to 10 nm, and the thickness of the P-type doped amorphous silicon layer 150 is 5 nm to 15 nm.

[0118] Steps 1-3 involve depositing a first conductive layer 160 and a second conductive layer 170 on the N-type doped amorphous silicon layer 140 and the P-type doped amorphous silicon layer 150, respectively, using a PVD magnetron sputtering apparatus. The first conductive layer 160 and the second conductive layer 170 are both ITO (Indium Tin Oxide) transparent conductive films, with thicknesses ranging from 90 nm to 110 nm.

[0119] Steps 1-4 involve depositing copper seed layers on the first conductive layer 160 and the second conductive layer 170 using a PVD magnetron sputtering apparatus. The thickness of the copper seed layer is 100 nm to 250 nm.

[0120] Steps 1-5: Apply photosensitive emulsion to the copper seed layer, completely covering it. Perform a first baking treatment on the photosensitive emulsion applied to the copper seed layer to form a first photosensitive emulsion film 210. The temperature of the first baking treatment is 95℃~105℃, the duration of the first baking treatment is 2min~3min, and the thickness of the first photosensitive emulsion film 210 is 6μm~8μm.

[0121] Steps 1-6: Photosensitive emulsion is coated onto the surface of the first photosensitive emulsion film 210, completely covering the first photosensitive emulsion film 210. The photosensitive emulsion coated on the first photosensitive emulsion film 210 is then subjected to a second baking treatment to form a second photosensitive emulsion film 220. The second photosensitive emulsion film 220 and the first photosensitive emulsion film 210 together constitute the photosensitive emulsion layer 200. The temperature of the second baking treatment is 105℃~115℃, the duration of the second baking treatment is 3min~4min, and the film thickness of the photosensitive emulsion layer 200 is 14μm~16μm.

[0122] Steps 1-7: Using the first mask 310, a first printing exposure is performed on the first region 200a of the photosensitive adhesive layer 200. The first region 200a is the area outside the first grating pattern 200b. The first grating pattern 200b is the same as the preset grating pattern, but the grating width W1 corresponding to the first grating pattern 200b is 4μm larger than the grating width corresponding to the preset grating pattern. The exposure energy for the first printing exposure is 70mJ / cm². 2 ~100mj / cm 2 The exposure time for the first printing exposure is 250ms to 350ms. The first mask 310 and the photosensitive adhesive layer 200 have a first gap in the thickness direction of the solar cell substrate 100, and the width of the first gap in the thickness direction is 60μm to 80μm.

[0123] Steps 1-8: Using the second mask 320, a second printing exposure is performed on the second region 200c of the photosensitive emulsion layer 200 after the first printing exposure. The second region 200c is the area outside the second grid pattern 200d. The second grid pattern 200d is the same as the preset grid pattern, and the grid width W2 corresponding to the second grid pattern 200d is equal to the grid width corresponding to the preset grid pattern. The second mask 320 and the photosensitive emulsion layer 200 have a second gap in the thickness direction of the solar cell substrate 100. The width of the first gap in the thickness direction is equal to the width of the second gap in the thickness direction. The exposure time of the second printing exposure is equal to the exposure time of the first printing exposure. The exposure energy of the second printing exposure is greater than the exposure energy of the first printing exposure, and the exposure energy of the second printing exposure is 80 mJ / cm². 2 ~100mj / cm 2 .

[0124] Steps 1-9: Use sodium carbonate solution to clean and remove the unexposed photosensitive emulsion layer 200 (grid area) to form patterned grooves 201, exposing the copper seed layer of the grid area.

[0125] Steps 1-10 involve wrapping the four corner edges and corner locations of the solar cell substrate 100 with edge-sealing adhesive. For example, the width of the edge-sealing adhesive is less than or equal to 50 μm, and the thickness of the edge-sealing adhesive is 10 μm to 15 μm.

[0126] Steps 1-11: Electroplating copper grid lines in a copper sulfate electroplating solution.

[0127] Comparative Example 1

[0128] This comparative example provides a method for fabricating a solar cell, including the following steps:

[0129] Step 2-1 involves texturing and cleaning the silicon wafer substrate to form a uniform "positive pyramid" textured surface. The silicon wafer substrate is an N-type monocrystalline silicon wafer, and the base dimension of the pyramid structure of the textured surface is 2μm to 8μm.

[0130] Step 2-2: Using a PECVD plasma deposition system, a first intrinsic amorphous silicon layer and an N-type doped amorphous silicon layer are sequentially deposited on the upper surface of the texturized silicon wafer substrate. Similarly, a second intrinsic amorphous silicon layer and a P-type doped amorphous silicon layer are sequentially deposited on the lower surface of the texturized silicon wafer substrate using the same PECVD system. The thickness of the first intrinsic amorphous silicon layer is 3 nm to 6 nm, the thickness of the second intrinsic amorphous silicon layer is 3 nm to 9 nm, the thickness of the N-type doped amorphous silicon layer is 5 nm to 10 nm, and the thickness of the P-type doped amorphous silicon layer is 5 nm to 15 nm.

[0131] Steps 2-3 involve depositing a first conductive layer and a second conductive layer on the N-type doped amorphous silicon layer and the P-type doped amorphous silicon layer, respectively, using a PVD magnetron sputtering apparatus. The first and second conductive layers are ITO (Indium Tin Oxide) transparent conductive films, with thicknesses ranging from 90 nm to 110 nm.

[0132] Steps 2-4 involve depositing copper seed layers on the first and second conductive layers using a PVD magnetron sputtering apparatus. The thickness of the copper seed layer is 100 nm to 250 nm.

[0133] Steps 2-5: Apply photosensitive emulsion to the copper seed layer, completely covering it. The thickness of the photosensitive emulsion layer should be controlled between 14 μm and 16 μm.

[0134] Steps 2-6 involve using a photomask to laser-print the designed grid pattern onto a photosensitive emulsion layer, followed by exposure. The exposure energy is 70 mJ / cm². 2 ~100mj / cm 2 The exposure time is 250ms to 350ms, and the photomask and the photosensitive emulsion layer have a gap of 60μm to 80μm in the thickness direction of the solar cell substrate.

[0135] Steps 2-7: Use sodium carbonate solution to clean and remove the unexposed photosensitive emulsion layer (grid line area) to form patterned grooves and expose the copper seed layer in the grid line area.

[0136] Steps 2-8 involve wrapping the four corner edges and corner locations of the solar cell substrate with edge-sealing adhesive. For example, the width of the edge-sealing adhesive is less than or equal to 50 μm, and the thickness of the adhesive is 10 μm to 15 μm.

[0137] Steps 2-9 involve electroplating copper grid lines in a copper sulfate electroplating solution.

[0138] Result comparison:

[0139] The patterned grooves obtained in Comparative Example 1 and the grid lines of the solar cell obtained in Comparative Example 1 were tested using scanning electron microscopy (SEM). The test results are shown in [link to SEM]. Figure 12 and Figure 13 As shown.

[0140] Please refer to Figure 12 As shown, in the same solar cell obtained in Comparative Example 1, there are significant differences in the width of the bottom of the patterned groove. Figure 12 The bottom width of the patterned groove shown in (12a) is 28.12 μm, while Figure 12 The bottom width of the patterned groove shown in (12b) is 48.22 μm.

[0141] In the same solar cell obtained in Comparative Example 1 Figure 13 The grid lines shown in (13a) are in Figure 12 The grid lines formed within the patterned grooves shown in (12a) Figure 13 The grid lines shown in (13b) are in Figure 12 The grid lines formed within the patterned grooves shown in (12b) are composed of... Figure 13 It can be seen that the grid lines shown in (13a) and (13b) not only have significant differences in morphology, but also significant differences in the bottom width of the grid lines.

[0142] The patterned groove 201 obtained in Example 1 was tested using a scanning electron microscope (SEM). The test results are shown in [link to SEM]. Figure 11 As shown.

[0143] Please refer to Figure 11 As shown, in the same solar cell obtained in Example 1, the difference in the bottom width of the patterned groove 201 is within 3 μm. Figure 11 The bottom width of the patterned groove 201 shown in (11a) is 28.12 μm. Figure 11 The bottom width of the patterned groove 201 shown in (11b) is 28.68 μm. Figure 11The bottom width of the patterned groove 201 shown in (11c) is 27.70 μm. Figure 11 The bottom width of the patterned groove 201 shown in (11d) is 27.65 μm. Figure 11 The bottom width of the patterned groove 201 shown in (11e) is 28.68 μm. Figure 11 The bottom width of the patterned groove 201 shown in (11f) is 28.54 μm. Figure 11 The bottom width of the patterned groove 201 shown in the middle (11g) is 28.16μm. Figure 11 The bottom width of the patterned groove 201 shown in Figure 11h is 29.99 μm. Figure 11 The bottom width of the patterned groove 201 shown in (11i) is 29.20 μm. Figure 11 The bottom width of the patterned groove 201 shown in (11j) is 27.37 μm. Figure 11 The bottom width of the patterned groove 201 shown in (11k) is 27.56 μm. Figure 11 The bottom width of the patterned groove 201 shown in (11l) is 28.40 μm.

[0144] In the different solar cells obtained in Example 1, the difference in the bottom width of the patterned groove 201 is within 4 μm.

[0145] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0146] The above embodiments merely illustrate preferred implementations of this application, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the scope of protection of this application. Therefore, the scope of protection of this patent application should be determined by the appended claims.

Claims

1. A method for fabricating a solar cell, characterized in that, include: A photosensitive adhesive layer is formed on the surface of the solar cell substrate; A first printing exposure is performed on a first area of ​​the photosensitive adhesive layer. The first area is the area outside the first grid line pattern. The first grid line pattern is the same as the preset grid line pattern, and the grid line width corresponding to the first grid line pattern is greater than the grid line width corresponding to the preset grid line pattern. A second printing exposure is performed on the second region of the photosensitive emulsion layer after the first printing exposure. The second region is the region outside the second grid line pattern. The second grid line pattern is the same as the preset grid line pattern, and the grid line width corresponding to the second grid line pattern is equal to the grid line width corresponding to the preset grid line pattern.

2. The method for preparing a solar cell as described in claim 1, characterized in that, The first print exposure satisfies at least one of the following (i) to (iii): (i) The width of the gate line corresponding to the first gate line pattern is 3μm to 5μm larger than the width of the gate line corresponding to the preset gate line pattern; (ii) The exposure energy of the first printing exposure is 70 mJ / cm². 2 ~100mj / cm 2 ; (iii) The exposure time of the first printing exposure is 250ms to 350ms.

3. The method for preparing a solar cell as described in claim 1, characterized in that, The second printing exposure satisfies at least one of the following (iv) to (vii): (iv) The exposure energy for the second printing exposure is 80 mJ / cm². 2 ~100mj / cm 2 ; (v) The exposure energy of the second printing exposure is greater than or equal to the exposure energy of the first printing exposure; (vi) The exposure time for the second printing exposure is 250ms to 350ms; (vii) The exposure time of the second printing exposure is equal to the exposure time of the first printing exposure.

4. The method for preparing a solar cell as described in claim 1, characterized in that, The first printing exposure satisfies at least one of the following (viii) to (ix), and the second printing exposure satisfies at least one of the following (x) to (xi): (viii) The first printing exposure is performed using a first mask, wherein the first mask and the photosensitive adhesive layer have a first gap in the thickness direction of the solar cell substrate; (ix) In (viii), the width of the first gap in the thickness direction is 60 μm to 80 μm; (x) The second printing exposure is performed using a second mask, wherein the second mask and the photosensitive adhesive layer have a second gap in the thickness direction of the solar cell substrate; (xi) In (x), the width of the second gap in the thickness direction is 60 μm to 80 μm.

5. The method for preparing a solar cell as described in claim 4, characterized in that, The width of the first gap in the thickness direction is equal to the width of the second gap in the thickness direction.

6. The method for preparing a solar cell as described in claim 1, characterized in that, The photosensitive adhesive layer comprises multiple layers of photosensitive adhesive film sequentially stacked in the thickness direction of the solar cell substrate; The process of forming a photosensitive adhesive layer on the surface of a solar cell substrate includes sequentially forming multiple layers of the photosensitive adhesive film on the surface of the solar cell substrate. Forming the photosensitive film includes: Photosensitive adhesive is coated onto the surface of the solar cell substrate or the surface of the previously formed photosensitive adhesive film; The coated photosensitive emulsion is baked to form a photosensitive emulsion film.

7. The method for preparing a solar cell as described in claim 1, characterized in that, The photosensitive adhesive layer comprises a first photosensitive adhesive film and a second photosensitive adhesive film sequentially stacked in the thickness direction of the solar cell substrate; The process of forming a photosensitive adhesive layer on the surface of a solar cell substrate includes: The first photosensitive film is formed on the surface of the solar substrate; The second photosensitive film is formed on the first photosensitive film.

8. The method for preparing a solar cell as described in claim 7, characterized in that, The step of forming the first photosensitive adhesive film on the surface of the solar substrate includes coating the surface of the solar cell substrate with photosensitive adhesive; and subjecting the photosensitive adhesive coated on the surface of the solar cell substrate to a first baking treatment to form the first photosensitive adhesive film. The step of forming a second photosensitive film on the first photosensitive film includes coating a photosensitive adhesive onto the surface of the first photosensitive film; and subjecting the photosensitive adhesive coated onto the surface of the first photosensitive film to a second baking treatment to form the second photosensitive film.

9. The method for preparing a solar cell as described in claim 8, characterized in that, The formation of a photosensitive adhesive layer on the surface of the solar cell substrate satisfies at least one of the following (xii) to (xiv): (xii) The thickness of the first photosensitive film is 6μm to 8μm; (xiii) The temperature of the first baking treatment is 95℃~105℃; (xiv) The duration of the first baking treatment is 2 min to 3 min.

10. The method for preparing a solar cell as described in claim 8, characterized in that, The formation of a photosensitive adhesive layer on the surface of the solar cell substrate satisfies at least one of the following (xv) to (xvii): (xv) The thickness of the photosensitive adhesive layer is 14μm to 16μm; (xvi) The temperature of the second baking treatment is 105℃~115℃; (xvii) The duration of the second baking treatment is 3 min to 4 min.