Perovskite-based solar cell, preparation method thereof and photovoltaic module

By constructing a three-dimensional organic-inorganic hybrid elastic network structure between perovskite grains, the mechanical stability problem of perovskite thin films was solved, stress release and grain boundary passivation were achieved, the mechanical strength and stability of the device were improved, and the photoelectric conversion efficiency was maintained.

CN123124571APending Publication Date: 2026-11-17CHINT NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611297414.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies suffer from severe mechanical stability issues during the preparation and use of large-area perovskite thin films, leading to rapid degradation of device performance and making it difficult to effectively suppress stress concentration and crack propagation without sacrificing photoelectric conversion efficiency.

Method used

A three-dimensional organic-inorganic hybrid elastic network structure is constructed in situ at the grain boundaries between perovskite grains to form a continuous mechanical dissipation path, actively absorb and disperse thermal and mechanical stress, enhance grain boundary bonding, passivate dangling bonds and defect states, and inhibit microcrack propagation.

Benefits of technology

It significantly improves the mechanical strength and stability of the device while maintaining photoelectric conversion efficiency, making it suitable for large-area perovskite modules and flexible perovskite solar cells, thus enhancing the overall performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124571A_ABST
    Figure CN123124571A_ABST
Patent Text Reader

Abstract

This application discloses a perovskite-based solar cell, its fabrication method, and a photovoltaic module. The perovskite-based solar cell includes a perovskite absorber layer; the perovskite absorber layer includes multiple perovskite grains, and a three-dimensional organic-inorganic hybrid elastic network structure is distributed at the grain boundaries between at least some of the perovskite grains. This invention, by constructing a three-dimensional organic-inorganic hybrid elastic network structure in situ at the grain boundaries between at least some of the perovskite grains, can form continuous mechanical dissipation paths in stress concentration areas, actively absorb and uniformly disperse local thermal and mechanical stresses, effectively suppress the initiation and propagation of microcracks, and simultaneously enhance grain boundary bonding, preventing interlayer delamination and film fragmentation. This elastic network structure can passivate dangling bonds and defect states at grain boundaries, reduce non-radiative recombination centers, suppress the formation of ion migration channels, and improve the efficiency and stability of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of photovoltaic cell technology, and more specifically, to a perovskite-based solar cell, its preparation method, and a photovoltaic module. Background Technology

[0002] Perovskite solar cells (PSCs) have become a research hotspot in next-generation photovoltaic technology due to their high photoelectric conversion efficiency, low-cost solution-based fabrication, and lightweight flexibility. In recent years, with the efficiency of small-area laboratory devices exceeding 26%, research focus has gradually shifted to the controllable fabrication and long-term stability improvement of large-area modules. However, in the process of moving from the laboratory to industrialization, large-area perovskite thin films face serious mechanical stability issues during fabrication and use.

[0003] In existing technologies, large-area perovskite thin films are prone to thermal and mechanical stress during annealing, bending, or long-term operation. This stress primarily stems from mismatched thermal expansion coefficients between functional layers, internal stress caused by uneven solvent evaporation, and deformation transfer from the flexible substrate. This stress accumulation can lead to cracking, delamination, and grain boundary expansion in the perovskite thin film, resulting in rapid performance degradation or even device failure. Furthermore, in roll-to-roll continuous fabrication processes, high-speed coating and rapid crystallization further exacerbate the stress unevenness problem.

[0004] To alleviate stress problems, existing technologies typically employ the following strategies: 1) Introducing elastic polymer additives: such as adding polymers like PMMA and PVP to perovskite precursors to improve film toughness; 2) Optimizing annealing processes: using gradient heating or rapid thermal annealing to reduce thermal shock; 3) Using flexible interface layers: introducing soft materials into electron transport layers (ETLs) or hole transport layers (HTLs). However, these methods still have significant drawbacks and shortcomings: 1) Poor compatibility of polymer additives: traditional polymers have low lattice matching with perovskite, easily leading to phase separation and affecting carrier transport; 2) Limited stress buffering effect: most additives only play a toughening role and cannot actively absorb or release local stress; 3) Difficulty in achieving in-situ uniform distribution: adding an external buffer layer requires additional process steps, increasing process complexity, and the interface bonding is weak; 4) Poor applicability to large areas: at the module level, the problem of uneven stress distribution is more prominent, and existing technologies struggle to achieve effective buffering across the entire area.

[0005] Therefore, how to improve the perovskite absorber layer so that it can actively suppress stress concentration and crack propagation from the source without sacrificing photoelectric conversion efficiency is a technical problem that urgently needs to be solved. Summary of the Invention

[0006] This application provides a perovskite-based solar cell, its fabrication method, and a photovoltaic module. A three-dimensional organic-inorganic hybrid elastic network structure is constructed in situ at the grain boundaries between at least some perovskite grains. This elastic network structure possesses both high elastic modulus and excellent interfacial adhesion properties, enabling it to form continuous mechanical dissipation paths in stress concentration areas. It actively absorbs and uniformly disperses local thermal and mechanical stresses, effectively suppressing microcrack initiation and propagation, while simultaneously enhancing grain boundary bonding and preventing interlayer delamination and film fragmentation. Furthermore, the organic-inorganic hybrid components in this elastic network structure effectively passivate dangling bonds and defect states at grain boundaries, reduce non-radiative recombination centers, and suppress the formation of ion migration channels. This enhances the mechanical strength of the perovskite thin film while further improving the device's efficiency and stability.

[0007] In a first aspect, a perovskite-based solar cell is provided, the perovskite-based solar cell comprising a perovskite absorber layer.

[0008] The perovskite absorber layer comprises multiple perovskite grains, and at least some of the grain boundaries between the perovskite grains are distributed with a three-dimensional organic-inorganic hybrid elastic network structure.

[0009] This invention constructs a three-dimensional organic-inorganic hybrid elastic network structure in situ at the grain boundaries between at least some perovskite grains. This elastic network structure combines high elastic modulus with excellent interfacial adhesion properties, enabling it to form continuous mechanical dissipation paths in stress concentration areas. It actively absorbs and uniformly disperses local thermal and mechanical stresses, effectively suppressing the initiation and propagation of microcracks, while enhancing grain boundary bonding and preventing interlayer delamination and film fragmentation. Furthermore, the organic-inorganic hybrid components in this elastic network structure can effectively passivate dangling bonds and defect states at grain boundaries, reduce non-radiative recombination centers, and suppress the formation of ion migration channels. Thus, while enhancing the mechanical strength of the perovskite thin film, it further improves the efficiency and stability of the device.

[0010] The three-dimensional organic-inorganic hybrid elastic network structure introduced in this invention has three functions: stress relief, grain boundary passivation, and water and oxygen barrier, which can significantly improve the overall performance of the device.

[0011] The strategy provided by this invention is applicable to devices such as large-area perovskite modules, flexible perovskite solar cells, and crystalline silicon / perovskite tandem cells.

[0012] In some embodiments, the three-dimensional organic-inorganic hybrid elastic network structure includes polydimethylsiloxane segments and silica nanoclusters. The polydimethylsiloxane segments are cross-linked through Si-O-Si bonds to form a three-dimensional organic network, and the silica nanoclusters are embedded in the three-dimensional organic network as cross-linking points.

[0013] In some embodiments, the three-dimensional organic-inorganic hybrid elastic network structure forms coordination bonds with uncoordinated B-site cations on the surface of the perovskite grains through the crosslinking points.

[0014] In some embodiments, the mass ratio of the polydimethylsiloxane segments to the silica nanoclusters is (70-80):(20-30), wherein the polydimethylsiloxane segments are selected in the range of "70-80", for example, 70, 72, 74, 76, 78 or 80, and the silica nanoclusters are selected in the range of "20-30", for example, 20, 22, 24, 26, 28 or 30.

[0015] In some embodiments, the average particle size of the silica nanoclusters is 10-100 nm, for example, it can be 10 nm, 30 nm, 50 nm, 70 nm, 90 nm or 100 nm.

[0016] In some embodiments, the elastic modulus of the perovskite absorber layer is 10-55 GPa, for example, it can be 10 GPa, 30 GPa, 27.4 GPa, 30 GPa, 40 GPa, 50.3 GPa or 55 GPa.

[0017] In some embodiments, the Young's modulus of the perovskite absorber layer is 10-55 GPa, for example, it can be 10 GPa, 14.49 GPa, 20 GPa, 27.4 GPa, 30 GPa, 40 GPa, 50.3 GPa or 55 GPa.

[0018] In some embodiments, the perovskite absorber layer has the general chemical formula ABX3, where A includes any one or a combination of at least two of formamidinium ions, methylamine ions, or cesium ions, B includes lead ions and / or tin ions, and X is a halide ion. Exemplarily, the halide ion can be at least one of chloride ions, bromide ions, or iodide ions.

[0019] In some embodiments, the thickness of the perovskite absorber layer is 300-1000 nm, for example, it can be 300 nm, 400 nm, 500 nm, 600 nm, 700 nm or 800 nm.

[0020] In some embodiments, the average grain size of the perovskite grains is 50-1000 nm, for example, it can be 50 nm, 100 nm, 200 nm, 500 nm, 750 nm, 800 nm, 900 nm or 1000 nm.

[0021] In a second aspect, a method for fabricating a perovskite-based solar cell as described in the first aspect is provided, the method comprising the following steps: Prepare a perovskite precursor solution containing an organic-inorganic hybrid elastomer precursor.

[0022] A perovskite precursor solution is coated onto a substrate using a film-forming process, followed by annealing to obtain a perovskite absorber layer.

[0023] In some embodiments, the organic-inorganic hybrid elastomer precursor comprises a hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer.

[0024] In some embodiments, the mass content of the organic-inorganic hybrid elastomer precursor in the perovskite precursor solution is 0.5-5 wt%, for example, it can be 0.5 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, or 5 wt%.

[0025] In some embodiments, the method for preparing the perovskite precursor solution containing the organic-inorganic hybrid elastomer precursor includes: First, a perovskite precursor solution is prepared, and then an organic-inorganic hybrid elastomer precursor is added and mixed to obtain the perovskite precursor solution containing the organic-inorganic hybrid elastomer precursor.

[0026] In some embodiments, the film-forming process includes any one or a combination of at least two of spin coating, blade coating, slot coating, or inkjet printing.

[0027] In some embodiments, the annealing temperature is 80-150°C, for example, it can be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, etc., and the time is 15-30 minutes, for example, it can be 15 minutes, 20 minutes, 25 minutes or 30 minutes, etc.

[0028] Thirdly, a photovoltaic module is provided, the photovoltaic module comprising the perovskite-based solar cell as described in the first aspect. Attached Figure Description

[0029] Figure 1 This is a comparison chart of the stability of single-junction perovskite solar cells provided in Example 1 and Comparative Example 1 of this application.

[0030] Figure 2 This is a top view of the photovoltaic module provided in this application.

[0031] Figure 3 This is a three-dimensional schematic diagram of the photovoltaic module provided in this application.

[0032] Figure 4 This is a schematic diagram of the photovoltaic system provided in this application.

[0033] The accompanying drawings are not drawn to scale.

[0034] Figure label: 1-Front panel glass; 2-Front layer encapsulant; 3-Battery string layer; 4-Rear layer encapsulant; 5-Back panel glass; 6-Frame; 7-Gathering box; 8-Photovoltaic system; 9-Photovoltaic module. Detailed Implementation

[0035] The descriptions of specific structures or functions implemented according to the concept of this application disclosed in this specification are merely illustrative examples for explaining embodiments based on the concept of this application. Those skilled in the art will understand that embodiments based on the concept of this application can have various variations and forms, and are not limited to the embodiments described in this specification, but also include various modifications, equivalents, or substitutions made within the scope of the purpose, concept, and technology of this application.

[0036] In the description of this application, it should be understood that the use of terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", and "circumferential" indicates the relative orientation or positional relationship between different components, and is only for the convenience of describing this application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.

[0037] Although the terms "first" or "second" may be used to describe various components or components, the components or components should not be limited by the terms. The terms above are used only for the purpose of distinguishing one component or component from another. For example, without departing from the scope of the claims according to the concept of this application, a first battery cell may be referred to as a second battery cell, and similarly, a second battery cell may be referred to as a first battery cell.

[0038] In this application, unless otherwise expressly specified and limited, the terms "connected," "fixed," "set," etc., should be interpreted broadly. For example, when one component is said to "connect" another component, it should be understood that it can be directly or indirectly connected to the other component, meaning that other components may also be present in between. Similarly, the terms "fixed" and "set" should be interpreted broadly in a similar way. Furthermore, the term "connected" can refer to a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can refer to the internal communication of two components or the interaction between two components, unless otherwise expressly limited. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances. In this application, unless otherwise expressly specified and limited, the description of "above" or "below" the second feature can mean that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediate medium. Moreover, "above," "on top of," and "over" the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. The first feature being "below", "under", or "below" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0039] To make the above-mentioned objectives, features and advantages of this application more apparent and understandable, the specific embodiments of this application will be described in detail below with reference to the accompanying drawings.

[0040] The researchers of this application have found that the following strategies are commonly used in traditional technologies to alleviate stress problems: 1) Introducing elastic polymer additives: such as adding polymers such as PMMA and PVP to perovskite precursors to improve film toughness; 2) Optimizing annealing process: using gradient heating or rapid thermal annealing to reduce thermal shock; 3) Using flexible interface layers: introducing soft materials into electron transport layer (ETL) or hole transport layer (HTL).

[0041] However, the above methods still have significant defects and shortcomings: 1) Poor compatibility of polymer additives: Traditional polymers have low matching degree with perovskite lattices, which can easily lead to phase separation and affect carrier transport; 2) Limited stress buffering effect: Most additives only play a toughening role and cannot actively absorb or release local stress; 3) Difficult to achieve in-situ uniform distribution: Adding a buffer layer requires additional process steps, increasing process complexity, and the interface bonding is weak; 4) Poor applicability in large areas: At the module level, the problem of uneven stress distribution is more prominent, and existing technologies are unable to achieve effective buffering in the entire area.

[0042] Therefore, how to improve the perovskite absorber layer so that it can actively suppress stress concentration and crack propagation from the source without sacrificing photoelectric conversion efficiency is a technical problem that urgently needs to be solved.

[0043] Based on this, the present invention provides a perovskite-based solar cell, wherein the perovskite-based solar cell includes a perovskite absorber layer.

[0044] The perovskite absorber layer comprises multiple perovskite grains, and at least some of the grain boundaries between the perovskite grains are distributed with a three-dimensional organic-inorganic hybrid elastic network structure.

[0045] This invention constructs a three-dimensional organic-inorganic hybrid elastic network structure in situ at the grain boundaries between at least some perovskite grains. This elastic network structure combines high elastic modulus with excellent interfacial adhesion properties, enabling it to form continuous mechanical dissipation paths in stress concentration areas. It actively absorbs and uniformly disperses local thermal and mechanical stresses, effectively suppressing the initiation and propagation of microcracks, while enhancing grain boundary bonding and preventing interlayer delamination and film fragmentation. Furthermore, the organic-inorganic hybrid components in this elastic network structure can effectively passivate dangling bonds and defect states at grain boundaries, reduce non-radiative recombination centers, and suppress the formation of ion migration channels. Thus, while enhancing the mechanical strength of the perovskite thin film, it further improves the efficiency and stability of the device.

[0046] The three-dimensional organic-inorganic hybrid elastic network structure introduced in this invention has three functions: stress relief, grain boundary passivation, and water and oxygen barrier, which can significantly improve the overall performance of the device.

[0047] It should be noted that "multiple" refers to two or more. In this invention, "multiple perovskite grains" indicates that the perovskite absorber layer contains at least two perovskite grains, which are adjacent to each other through grain boundaries. It is understood that those skilled in the art can determine the specific number of grains based on the actual area and grain size of the perovskite absorber layer, and this invention does not impose any particular limitation on this.

[0048] In some embodiments, the perovskite-based solar cell is any one of a large-area perovskite module cell, a flexible perovskite solar cell, or a crystalline silicon-perovskite tandem solar cell.

[0049] In some embodiments, the three-dimensional organic-inorganic hybrid elastic network structure includes polydimethylsiloxane segments and silica nanoclusters. The polydimethylsiloxane segments are cross-linked through Si-O-Si bonds to form a three-dimensional organic network, and the silica nanoclusters are embedded in the three-dimensional organic network as cross-linking points.

[0050] In the three-dimensional organic-inorganic hybrid elastic network structure introduced in this invention, polydimethylsiloxane segments can endow the material with excellent flexibility and resilience, while silica nanoclusters can provide mechanical strength and thermal stability. The polydimethylsiloxane segments are cross-linked through Si-O-Si bonds, and silica nanoclusters serve as cross-linking points. This allows the three-dimensional organic-inorganic hybrid elastic network structure to not only have a high elastic modulus and effectively release residual stress, but also to coordinate with uncoordinated B-site ions (such as lead ions) on the perovskite surface through cross-linking points, thus achieving dual passivation.

[0051] In some embodiments, the three-dimensional organic-inorganic hybrid elastic network structure forms coordination bonds with uncoordinated B-site cations on the surface of the perovskite grains through the crosslinking points.

[0052] The three-dimensional organic-inorganic hybrid elastic network structure introduced in this invention forms coordination bonds with uncoordinated B-site cations (such as lead ions) on the surface of perovskite grains through cross-linking points. This reduces the defect state density on the grain surface, suppresses nonradiative recombination, anchors the grains, and enhances structural stability.

[0053] In some embodiments, the mass ratio of the polydimethylsiloxane segments to the silica nanoclusters is (70-80):(20-30), wherein the polydimethylsiloxane segments are selected in the range of "70-80", for example, 70, 72, 74, 76, 78 or 80, and the silica nanoclusters are selected in the range of "20-30", for example, 20, 22, 24, 26, 28 or 30.

[0054] This invention combines polydimethylsiloxane segments and silica nanoclusters in an appropriate mass ratio to construct a three-dimensional interpenetrating network with both high flexibility and high strength in situ at the perovskite grain boundaries. This achieves synergistic effects between the organic and inorganic phases, thereby effectively releasing residual stress inside the film while providing sufficient mechanical support to prevent crack propagation and interlayer delamination caused by stress concentration.

[0055] In some embodiments, the average particle size of the silica nanoclusters is 10-100 nm, for example, it can be 10 nm, 30 nm, 50 nm, 70 nm, 90 nm, or 100 nm. It should be noted that the average particle size refers to the statistical average diameter of the silica nanoclusters when dispersed in the system, which can be obtained by transmission electron microscopy (TEM).

[0056] In some embodiments, the elastic modulus of the perovskite absorber layer is 10-55 GPa, for example, it can be 10 GPa, 30 GPa, 27.4 GPa, 30 GPa, 40 GPa, 50.3 GPa, or 55 GPa. It should be noted that the elastic modulus refers to the material's ability to resist volume change when subjected to volume compression, reflecting the material's stiffness against uniform compression. It can be obtained through nanoindentation testing or dynamic mechanical analysis (DMA) testing.

[0057] In some embodiments, the Young's modulus of the perovskite absorber layer is 10-55 GPa, for example, it can be 10 GPa, 14.49 GPa, 20 GPa, 27.4 GPa, 30 GPa, 40 GPa, 50.3 GPa, or 55 GPa. It should be noted that Young's modulus refers to the ratio of stress to strain under uniaxial tension or compression, used to characterize the tensile or compressive stiffness of a material. It can be obtained through nanoindentation testing or uniaxial tension / bending testing.

[0058] By introducing the aforementioned three-dimensional organic-inorganic hybrid elastic network structure, this invention enables the elastic modulus and Young's modulus of the perovskite absorber layer to meet the above-mentioned ranges. This endows the perovskite thin film with excellent mechanical buffering capabilities while ensuring that the active layer has sufficient structural rigidity and mechanical stability. It effectively overcomes the defect of traditional flexible devices being prone to brittle fracture under repeated bending or thermal stress cycling, and significantly improves the long-term operational reliability and mechanical durability of perovskite solar cells and modules.

[0059] In some embodiments, the perovskite absorber layer has the general chemical formula ABX3, where A includes any one or a combination of at least two of formamidinium ions, methylamine ions, or cesium ions, B includes lead ions and / or tin ions, and X is a halide ion. Exemplarily, the halide ion can be at least one of chloride ions, bromide ions, or iodide ions.

[0060] In some embodiments, the thickness of the perovskite absorber layer is 300-1000 nm, for example, it can be 300 nm, 400 nm, 500 nm, 600 nm, 700 nm or 800 nm.

[0061] In some embodiments, the average grain size of the perovskite grains is 50-1000 nm, for example, it can be 50 nm, 100 nm, 200 nm, 500 nm, 750 nm, 800 nm, 900 nm, or 1000 nm. It should be noted that the average grain size of the perovskite grains can be obtained by SEM scanning electron microscopy.

[0062] In some embodiments, the perovskite solar cell includes, from bottom to top, a substrate, a first charge transport layer, the perovskite absorber layer, a second charge transport layer, and an electrode, wherein the first charge transport layer and the second charge transport layer transport charges of opposite polarities.

[0063] Preferably, the substrate is a rigid substrate or a flexible substrate. For example, a rigid substrate may be ITO conductive glass or FTO conductive glass, making the perovskite solar cell a single-junction perovskite solar cell. Alternatively, a crystalline silicon substrate (such as an HJT heterojunction silicon cell or a TOPCon tunnel oxide passivated contact silicon cell) may be used as the rigid substrate, making the perovskite solar cell a two-terminal or four-terminal perovskite solar cell. A flexible substrate may be a transparent flexible polymer film such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), or polyimide (PI), making the perovskite solar cell a flexible perovskite solar cell.

[0064] Preferably, the first charge transport layer is a hole transport layer, such as a SAM layer (e.g., a MeO-4PACz layer ([2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid layer)) and / or a nickel oxide layer, etc.), and the second charge transport layer is an electron transport layer, such as a C 60 Layers and / or tin oxide layers, etc.

[0065] Preferably, the perovskite absorber layer and the second charge transport layer are further provided with a passivation layer, the passivation layer comprising any one or a combination of at least two of phenylethyl ammonium iodide (PEAI), polyimide (PI), or piperazine dihydroiodide (PDI).

[0066] Preferably, the electrode is made of any one or a combination of at least two of Ag, Au, or Cu.

[0067] The present invention also provides a method for preparing the perovskite-based solar cell as described above, the method comprising the following steps: Prepare a perovskite precursor solution containing an organic-inorganic hybrid elastomer precursor.

[0068] A perovskite precursor solution is coated onto a substrate using a film-forming process, followed by annealing to obtain a perovskite absorber layer.

[0069] In some embodiments, the organic-inorganic hybrid elastomer precursor comprises a hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer.

[0070] It should be noted that the hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer was purchased from the Chromatography Department, model number: Supelco-S#57341-U.

[0071] In some embodiments, the mass content of the organic-inorganic hybrid elastomer precursor in the perovskite precursor solution is 0.5-5 wt%, for example, it can be 0.5 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, or 5 wt%.

[0072] In this invention, the appropriate amount of organic-inorganic hybrid elastomer precursor added ensures the formation of a continuous and uniform three-dimensional stress buffer network at the perovskite grain boundaries, while avoiding insufficient stress release due to insufficient addition or decreased perovskite crystal quality and photoelectric performance degradation due to excessive addition, thus achieving an optimal balance between mechanical stability and photoelectric conversion efficiency.

[0073] In some embodiments, the method for preparing the perovskite precursor solution containing the organic-inorganic hybrid elastomer precursor includes: First, a perovskite precursor solution is prepared, and then an organic-inorganic hybrid elastomer precursor is added and mixed to obtain the perovskite precursor solution containing the organic-inorganic hybrid elastomer precursor.

[0074] In some embodiments, the film-forming process includes any one or a combination of at least two of spin coating, blade coating, slot coating, or inkjet printing.

[0075] In some embodiments, the annealing temperature is 80-150°C, for example, it can be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, etc., and the time is 15-30 minutes, for example, it can be 15 minutes, 20 minutes, 25 minutes or 30 minutes, etc.

[0076] In this invention, under suitable annealing temperature and time, organic-inorganic hybrid elastomer precursors (such as hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomers) can undergo sufficient hydrolysis-condensation and in-situ crosslinking reactions, allowing silica nanoclusters to be firmly embedded as crosslinking nodes in the three-dimensional organic network and effectively coordinating and passivating uncoordinated lead ions on the perovskite surface. Ultimately, a three-dimensional interpenetrating network with stable structure, high elastic modulus, and excellent interfacial adhesion is constructed in-situ at the grain boundaries.

[0077] In some embodiments, the present invention also provides a method for preparing the above-described perovskite-based solar cell, the method comprising the following steps: Provide transparent conductive glass as a rigid substrate.

[0078] A MeO-4PACz solution was coated onto the transparent conductive glass, and a hole transport layer was obtained after annealing.

[0079] A perovskite precursor solution containing an organic-inorganic hybrid elastomer precursor is coated onto the hole transport layer, and then annealed to obtain a perovskite absorber layer.

[0080] C is sequentially prepared on the perovskite absorber layer 60 The electron transport layer is obtained by adding a tin oxide layer and a tin oxide layer.

[0081] A metal electrode is fabricated on the tin oxide layer to obtain a perovskite-based solar cell.

[0082] In some embodiments, the present invention also provides a method for preparing the above-described perovskite-based solar cell, the method comprising the following steps: We provide N-type crystalline silicon wafers.

[0083] Intrinsic hydrogenated amorphous silicon passivation layers are prepared on the front and back sides of the N-type crystalline silicon wafer, respectively. Then, P-type hydrogenated amorphous silicon doped layers and N-type hydrogenated amorphous silicon doped layers are prepared on the front and back sides, respectively.

[0084] An intermediate interconnect layer is deposited on the N-type hydrogenated amorphous silicon doped layer.

[0085] A hole transport layer, a perovskite absorption layer, an electron transport layer, and an IZO layer are sequentially fabricated on the intermediate connecting layer.

[0086] An ITO layer and a metal electrode gate line are sequentially fabricated on the P-type hydrogenated amorphous silicon doped layer.

[0087] Metal electrodes and antireflection layers are sequentially fabricated on the IZO layer to obtain a two-terminal crystalline silicon-perovskite tandem solar cell.

[0088] In some embodiments, the present invention also provides a method for preparing the above-described perovskite-based solar cell, the method comprising the following steps: Provide transparent conductive glass as a rigid substrate.

[0089] Laser scribing is performed on the transparent conductive glass to break the transparent conductive layer, forming P1.

[0090] A hole transport layer is prepared on the transparent conductive glass.

[0091] A perovskite precursor solution containing an organic-inorganic hybrid elastomer precursor is coated onto the hole transport layer, and then annealed to obtain a perovskite absorber layer.

[0092] An electron transport layer is prepared on the perovskite absorber layer, and then laser scribing is performed to sever the hole transport layer, the perovskite absorber layer, and the electron transport layer to form P2.

[0093] Metal electrodes are fabricated on the electron transport layer, and then laser scribing is performed to form P3, resulting in a large-area perovskite component.

[0094] In some embodiments, the present invention also provides a method for preparing the above-described perovskite-based solar cell, the method comprising the following steps: Provides a flexible, transparent conductive substrate.

[0095] A metal oxide layer is prepared on the flexible transparent conductive substrate; A self-assembled monolayer was prepared on the metal oxide layer; A perovskite precursor solution containing an organic-inorganic hybrid elastomer precursor is coated onto the self-assembled monolayer, and then annealed to obtain a perovskite absorber layer.

[0096] An electron transport layer and a metal electrode are sequentially fabricated on the perovskite absorber layer to obtain a flexible perovskite solar cell.

[0097] The present invention also provides a photovoltaic module, the schematic diagram of which is shown below. Figure 2 and Figure 3 As shown, the photovoltaic module includes the perovskite-based solar cell described in the first aspect.

[0098] Preferably, the photovoltaic module includes a front glass panel 1, a front encapsulating film 2, a cell string layer 3, a rear encapsulating film 4, and a back glass panel 5 stacked in sequence, wherein the cell string layer 3 includes a plurality of the perovskite-based solar cells.

[0099] It should be noted that a photovoltaic module is a device that directly converts light energy into electrical energy through the photoelectric effect or photochemical effect. In addition to the above structure, it also includes a frame 6 surrounding the aforementioned layered structure and a junction box 7 located on one side of the back glass 5.

[0100] For example, the front cover may be made of a material with excellent light transmittance, impact resistance, corrosion resistance, and weather resistance, and may optionally include at least one of the following materials: tempered glass, plexiglass, transparent ceramics, organic fibers, or polymers. In some embodiments, the front cover may include at least one of an insulating barrier layer, a fluorinated weather-resistant layer, and a transition adhesive layer.

[0101] Back cover plates typically need to possess insulation, water resistance, aging resistance, weather resistance, and corrosion resistance. They can optionally include at least one of the following composite back covers as the substrate: tempered glass, acrylic glass, metal back cover, or PET film. The PET-based composite back cover can be selected from various types, such as composite (e.g., TPT / KPK, TPE / KPE), coated (e.g., TPC, KPC, CPC), and co-extruded (e.g., PO), depending on the needs of different scenarios.

[0102] Understandably, the choice of materials for the front cover and the back cover does not affect each other, and the same or different materials can be selected depending on the different application scenarios of the components (such as residential photovoltaics and building-integrated photovoltaics).

[0103] The battery string layer 3 includes multiple battery strings, which can be combined in series, parallel, or series-parallel configurations to achieve current collection and output. Further, each battery string is formed by sequentially connecting multiple solar cells (i.e., the perovskite-based solar cells) via connectors. In some embodiments, at least a portion of the connector is electrically connected to the back electrode of one solar cell, and at least another portion of the connector is electrically connected to the front or back electrode of another solar cell to form a battery string. The connector may optionally include conductive elements such as solder ribbons, busbars, or metal clips. In some embodiments, to improve welding performance, oxidation resistance, and weather resistance, the connector material may preferably be a highly conductive metal material, such as at least one of silver, copper, tin, nickel, or their alloys. In some embodiments, to balance conductivity and cost control, the connector material may also be at least one of metal-clad composite materials such as silver-coated copper, copper-coated silver, copper-coated aluminum, aluminum-coated copper, tin-plated copper, or nickel-plated copper. The electrical connection may be selected from one of the following methods: laser welding, spot welding, bonding, ultrasonic welding, resistance welding, or brazing.

[0104] The frame 6 surrounds the periphery of the stacked structure and is mostly made of aluminum alloy or steel alloy. In some embodiments, the frame 6 may also be a fiberglass frame or a plastic frame. The inner side of the frame 6 is usually provided with grooves for filling sealant to achieve a sealed bond with the stacked components formed by the front glass 1, the front adhesive film 2, the battery string layer 3, the rear adhesive film 4, and the back glass 5, thereby blocking moisture and buffering external impacts. In some embodiments, the frame 6 can be connected and assembled using corner brackets.

[0105] Junction box 7 is located on one side of the rear cover and is electrically connected to the terminals of the bus electrodes in the battery string layer 3 via a lead-out busbar for energy extraction. Junction box 7 typically includes a housing and cover made of weather-resistant insulating material, conductive connecting pieces disposed within the housing, and one or more bypass diodes. The bypass diodes are connected in parallel with sub-units of the battery string. The electrical lead-out portion of junction box 7 includes photovoltaic-specific connectors and cables. The cables preferably use cross-linked polyethylene insulating sheaths and tinned copper core wires. In some embodiments, the interior of junction box 7 may also be filled and encapsulated with potting compound to achieve insulation, thermal conductivity, moisture protection, and fixation.

[0106] The present invention also provides a photovoltaic system, the structural schematic diagram of which is shown below. Figure 4 As shown, the photovoltaic system 8 includes the photovoltaic module 9 as described in the third aspect.

[0107] It should be noted that the photovoltaic system 8 can be applied in photovoltaic power plants, such as ground power plants, rooftop power plants, and water-based power plants, as well as in equipment or devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars, solar buildings, etc.

[0108] It is understandable that the application scenarios of photovoltaic system 8 are not limited to this; that is to say, photovoltaic system 8 can be applied in all fields that require solar energy to generate electricity. Taking a photovoltaic power generation system as an example, photovoltaic system 8 may include a photovoltaic array, a combiner box, and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic modules. For example, multiple photovoltaic modules can form multiple photovoltaic arrays. The photovoltaic array is connected to the combiner box, which can collect the current generated by the photovoltaic array. The collected current flows through the inverter and is converted into AC power required by the mains power grid before being connected to the mains power grid to realize solar power supply.

[0109] Example 1 This embodiment provides a perovskite-based solar cell, which, from bottom to top, comprises ITO conductive glass, a hole transport layer, a perovskite absorber layer, a passivation layer, an electron transport layer, and a metal electrode.

[0110] The perovskite absorber layer comprises multiple perovskite grains, and at least some of the grain boundaries between the perovskite grains have a three-dimensional organic-inorganic hybrid elastic network structure. The three-dimensional organic-inorganic hybrid elastic network structure comprises polydimethylsiloxane segments and silica nanoclusters. The polydimethylsiloxane segments are cross-linked through Si-O-Si bonds to form a three-dimensional organic network, and the silica nanoclusters serve as cross-linking points embedded within the three-dimensional organic network. The three-dimensional organic-inorganic hybrid elastic network structure forms coordination bonds with uncoordinated lead ions on the surface of the perovskite grains through these cross-linking points. The mass ratio of the polydimethylsiloxane segments to the silica nanoclusters is 75:25. The average particle size of the silica nanoclusters is 50 nm. The elastic modulus of the perovskite absorber layer is 27.4 GPa, and the Young's modulus of the perovskite absorber layer is 14.4 GPa. The chemical formula of the perovskite absorber layer is (CH(NH2)2PbI3). 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 )3 (band gap is 1.68eV); the thickness of the perovskite absorber layer is 500nm; the average grain size of the perovskite grains is 400nm.

[0111] The hole transport layer is a MeO-4PACz layer, and the electron transport layer includes a 15nm thick C layer. 60The metal electrode consists of a 10 nm thick tin oxide layer and a PI passivation layer with a thickness of 5 nm, and an Ag layer with a thickness of 120 nm.

[0112] This embodiment also provides a method for preparing the above-mentioned perovskite-based solar cell, the method comprising the following steps: (1) Provide ITO conductive glass; clean the ITO conductive glass by sequentially using detergent, deionized water, acetone and anhydrous ethanol for ultrasonic cleaning, each ultrasonic cleaning time being 15 minutes, and then drying it for later use.

[0113] (2) The ethanol solution of MeO-4PACz (concentration of 1 mg / mL) was spin-coated onto the ITO conductive glass at a speed of 3000 rpm for 30 s. After the spin coating was completed, the glass was annealed at 100 °C for 10 min to obtain the MeO-4PACz layer.

[0114] (3) Provide 1.4 mol / L of (CH(NH2)2PbI3) 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 )3. Precursor mother liquor (the solvent consists of DMF and DMSO in a volume ratio of 4:1).

[0115] A hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer was added to the (CH(NH2)2PbI3) compound. 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 )3. In the precursor mother liquor, a perovskite precursor solution is obtained; the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 0.5 wt%.

[0116] The perovskite precursor solution was first spin-coated at 1000 rpm for 40 s, then at 3000 rpm for 20 s, and 200 μL of ethyl acetate was added dropwise during the last 10 s of spin-coating. After spin-coating, the solution was annealed at 100 °C for 20 min to form a perovskite absorber layer with a thickness of 500 nm on the MeO-4PACz layer.

[0117] (4) A passivation layer with a thickness of 5 nm is deposited on the perovskite absorption layer by spin coating.

[0118] (5) A C layer with a thickness of 15 nm is deposited on the passivation layer using a thermal evaporation method. 60 Layer, and then use the ALD method, in the C 60 A 10 nm thick tin oxide layer was prepared on the layer.

[0119] (6) An Ag layer with a thickness of 120 nm is deposited on the tin oxide layer by thermal evaporation.

[0120] Example 2 The difference between this embodiment and Embodiment 1 is that the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 1 wt%.

[0121] The remaining preparation methods and parameters are consistent with those in Example 1.

[0122] Example 3 The difference between this embodiment and Embodiment 1 is that the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 2 wt%.

[0123] The remaining preparation methods and parameters are consistent with those in Example 1.

[0124] Example 4 The difference between this embodiment and Embodiment 1 is that the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 3 wt%.

[0125] The remaining preparation methods and parameters are consistent with those in Example 1.

[0126] Example 5 The difference between this embodiment and Embodiment 1 is that the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 4 wt%.

[0127] The remaining preparation methods and parameters are consistent with those in Example 1.

[0128] Example 6 The difference between this embodiment and Embodiment 1 is that the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 5 wt%.

[0129] The remaining preparation methods and parameters are consistent with those in Example 1.

[0130] Example 7 This embodiment provides a two-terminal crystalline silicon-perovskite tandem solar cell, which includes a crystalline silicon bottom cell and a perovskite top cell. The crystalline silicon bottom cell and the perovskite top cell are connected by an intermediate connecting layer, which is an IZO layer with a thickness of 10 nm. The perovskite top cell includes a perovskite absorber layer as described in Example 1.

[0131] This embodiment also provides a method for fabricating the above-mentioned two-terminal crystalline silicon-perovskite tandem solar cell, the method comprising the following steps: (1) A 150 μm thick N-type single crystal silicon is sequentially pre-cleaned with ozone and deionized water and post-cleaned with a mixture of ozone and hydrofluoric acid. Finally, it is cleaned and etched with a mixture of hydrofluoric acid and nitric acid to form an N-type crystal silicon wafer with double-sided textured surface.

[0132] (2) Using the PECVD method, an intrinsic hydrogenated amorphous silicon passivation layer with a thickness of 2 nm is deposited on the front and back sides of the N-type crystalline silicon wafer, and then a P-type hydrogenated amorphous silicon doped layer with a thickness of 9 nm and an N-type hydrogenated amorphous silicon doped layer with a thickness of 6 nm are deposited on the front and back sides, respectively, to obtain a crystalline silicon bottom cell. (3) A 10 nm thick IZO layer is deposited on the front side of the crystalline silicon bottom cell as an intermediate connection layer.

[0133] (4) Spin-coating an ethanol solution of MeO-4PACz (concentration of 1 mg / mL) onto the intermediate connecting layer at a speed of 3000 rpm for 30 s. After the spin-coating is completed, the layer is annealed at 100 °C for 10 min to obtain the MeO-4PACz layer.

[0134] (5) Provide 1.7 mol / L of (CH(NH2)2PbI3) 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 )3. Precursor mother liquor (solvent composed of DMF and DMSO in a volume ratio of 4:1); hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer is added to the (CH(NH2)2PbI3) 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 )3. In the precursor mother liquor, a perovskite precursor solution is obtained; the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 0.5 wt%.

[0135] The perovskite precursor solution was first spin-coated at 1000 rpm for 40 s, then at 3000 rpm for 20 s, and 200 μL of ethyl acetate was added dropwise during the last 10 s of spin-coating. After spin-coating, the solution was annealed at 100 °C for 20 min to form a perovskite absorber layer with a thickness of 500 nm on the MeO-4PACz layer.

[0136] (6) A PI layer with a thickness of 5 nm is deposited on the perovskite absorption layer as a passivation layer by spin coating.

[0137] (7) A C layer with a thickness of 10 nm is deposited on the passivation layer using a thermal evaporation method. 60 Layer, and then use the ALD method, in the C 60 A 12 nm thick tin oxide layer was prepared on the layer.

[0138] (8) Using PVD, deposit an IZO layer with a thickness of 40 nm on the tin oxide layer and an ITO layer with a thickness of 100 nm on the N-type hydrogenated amorphous silicon doped layer.

[0139] An Ag gate line with a thickness of 180 nm was screen-printed on the ITO layer and sintered and cured. An Ag electrode with a thickness of 1 μm and a MgF2 antireflection layer with a thickness of 90 nm were sequentially thermally deposited on the IZO layer.

[0140] Example 8 This embodiment provides a large-area perovskite module, which includes, from bottom to top, an FTO transparent conductive glass, a hole transport layer, a perovskite absorption layer, an electron transport layer, and a top electrode stacked sequentially.

[0141] The perovskite absorber layer comprises multiple perovskite grains, and at least some of the grain boundaries between the perovskite grains have a three-dimensional organic-inorganic hybrid elastic network structure. The three-dimensional organic-inorganic hybrid elastic network structure comprises polydimethylsiloxane segments and silica nanoclusters. The polydimethylsiloxane segments are cross-linked through Si-O-Si bonds to form a three-dimensional organic network, and the silica nanoclusters serve as cross-linking points embedded within the three-dimensional organic network. The three-dimensional organic-inorganic hybrid elastic network structure forms coordination bonds with uncoordinated lead ions on the surface of the perovskite grains through these cross-linking points. The mass ratio of the polydimethylsiloxane segments to the silica nanoclusters is 75:25. The average particle size of the silica nanoclusters is 50 nm. The elastic modulus of the perovskite absorber layer is 27.5 GPa, and the Young's modulus of the perovskite absorber layer is 14.5 GPa. The chemical formula of the perovskite absorber layer is (CH(NH2)2PbI3). 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 3 (band gap of 1.68 eV); the thickness of the perovskite absorber layer is 500 nm; the average grain size of the perovskite grains is 400 nm.

[0142] The FTO transparent conductive glass includes a glass substrate and a transparent conductive layer disposed on the surface of the glass substrate. The transparent conductive layer has a P1 scribing groove. The hole transport layer, perovskite absorption layer, and electron transport layer are laser-scribed to form a P2 scribing groove, which penetrates the hole transport layer, perovskite absorption layer, and electron transport layer and exposes the transparent conductive layer. The top electrode layer is laser-scribed to form a P3 scribing groove, which penetrates the top electrode, electron transport layer, perovskite absorption layer, and hole transport layer and exposes the transparent conductive layer.

[0143] The hole transport layer is a nickel oxide layer, and the electron transport layer includes a 20nm thick C layer. 60 The electrode consists of a 20 nm thick tin oxide layer and a 110 nm thick Cu layer.

[0144] This embodiment also provides a method for preparing the above-mentioned large-area perovskite module, the method comprising the following steps: (1) Provide FTO conductive glass; clean the FTO conductive glass by sequentially using detergent, deionized water, acetone and anhydrous ethanol for ultrasonic cleaning, each ultrasonic cleaning time is 15 min, and after cleaning, dry it for later use.

[0145] (2) The FTO conductive glass is scratched by infrared nanosecond laser to cut the transparent conductive layer and form P1.

[0146] A 20 nm thick nickel oxide layer was deposited on the FTO conductive glass by magnetron sputtering and then annealed at 90 °C for 15 min to obtain a hole transport layer.

[0147] (3) Provide 1.4 mol / L of (CH(NH2)2PbI3) 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 )3. Precursor mother liquor (the solvent consists of DMF and DMSO in a volume ratio of 4:1).

[0148] A hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer was added to the (CH(NH2)2PbI3) compound. 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 )3. In the precursor mother liquor, a perovskite precursor solution is obtained; the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 0.5 wt%.

[0149] The perovskite precursor solution was first spin-coated at 1000 rpm for 40 s, then at 3000 rpm for 20 s, and 200 μL of ethyl acetate was added dropwise during the last 10 s of spin-coating. After spin-coating, the solution was annealed at 150 °C for 20 min to form a perovskite absorption layer with a thickness of 500 nm on the hole transport layer.

[0150] (4) A C layer with a thickness of 20 nm is deposited on the perovskite absorber layer using a thermal evaporation method. 60 Layer, and then use the ALD method, in the C 60 A 20 nm thick tin oxide layer was prepared on the layer to obtain an electron transport layer.

[0151] P2 is formed by laser scribing using green picosecond lasers.

[0152] (5) A Cu layer with a thickness of 110 nm is deposited on the tin oxide layer as the top electrode by thermal evaporation.

[0153] P3 is formed by laser scribing using green picosecond lasers.

[0154] Example 9 This embodiment provides a flexible perovskite solar cell, which includes a flexible transparent conductive substrate, a metal oxide layer, a MeO-2PACz layer, a perovskite absorber layer, an electron transport layer, a BCP layer, and a metal electrode.

[0155] The flexible transparent conductive substrate is made of PEN; the metal oxide layer is an alumina layer; the perovskite absorber layer comprises multiple perovskite grains, and at least some of the grain boundaries between the perovskite grains have a three-dimensional organic-inorganic hybrid elastic network structure distributed therein; the three-dimensional organic-inorganic hybrid elastic network structure comprises polydimethylsiloxane segments and silica nanoclusters, wherein the polydimethylsiloxane segments are cross-linked through Si-O-Si bonds to form a three-dimensional organic network, and the silica nanoclusters are embedded as cross-linking points. In the described three-dimensional organic network, the three-dimensional organic-inorganic hybrid elastic network structure forms coordination bonds with uncoordinated lead ions on the surface of the perovskite grains through the crosslinking points; the mass ratio of the polydimethylsiloxane segments to the silica nanoclusters is 75:25; the average particle size of the silica nanoclusters is 50 nm; the elastic modulus of the perovskite absorber layer is 27.4 GPa, and the Young's modulus of the perovskite absorber layer is 14.5 GPa; the chemical formula of the perovskite absorber layer is (CH(NH2)2PbI3). 0.83 Cs 0.17 Pb(I 0.82 Br 0.18)3 (band gap is 1.68eV); the thickness of the perovskite absorber layer is 500nm; the average grain size of the perovskite grains is 400nm.

[0156] The electron transport layer is a C material with a thickness of 25 nm. 60 The BCP layer has a thickness of 6 nm, and the metal electrode is an Ag layer with a thickness of 100 nm.

[0157] This embodiment also provides a method for fabricating the above-mentioned flexible perovskite solar cell, the method comprising the following steps: (1) Provide a flexible transparent conductive substrate made of PEN.

[0158] (2) A dispersion of 10% alumina nanoparticles was coated onto the flexible transparent conductive substrate and spin-coated at 5000 rpm for 30 seconds. After the spin-coating was completed, the substrate was annealed at 100°C for 10 minutes to form an alumina layer.

[0159] (3) Spin coat the alumina layer with a concentration of 0.3 mg / mL of MeO-2PACz in isopropanol at a speed of 4000 rpm for 30 seconds, and then anneal at 100°C for 10 minutes to form the MeO-2PACz layer.

[0160] (4) Provide 1.4 mol / L of (CH(NH2)2PbI3) 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 )3. Precursor mother liquor (the solvent consists of DMF and DMSO in a volume ratio of 4:1).

[0161] A hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer was added to the (CH(NH2)2PbI3) compound. 0.83 Cs 0.17 Pb(I 0.82 Br 0.18 )3. In the precursor mother liquor, a perovskite precursor solution is obtained; the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 0.5 wt%.

[0162] The perovskite precursor solution was first spin-coated at 1000 rpm for 10 s, then at 5000 rpm for 40 s, and 450 μL of diethyl ether was added dropwise during the last 20 s of spin-coating. After spin-coating, the solution was annealed at 100 °C for 30 min to form a perovskite absorber layer with a thickness of 500 nm on the MeO-4PACz layer.

[0163] (5) A C layer with a thickness of 25 nm is sequentially deposited on the perovskite absorber layer by thermal evaporation. 60 The layers consist of a 6nm thick BCP layer and a 100nm thick Ag layer.

[0164] Example 10 The difference between this embodiment and Embodiment 1 is that the ratio of polydimethylsiloxane segments to silica nanoclusters is adjusted so that the mass ratio of the polydimethylsiloxane segments to silica nanoclusters is 65:35.

[0165] The remaining preparation methods and parameters are consistent with those in Example 1.

[0166] Example 11 The difference between this embodiment and Embodiment 1 is that the ratio of polydimethylsiloxane segments to silica nanoclusters is adjusted so that the mass ratio of the polydimethylsiloxane segments to silica nanoclusters is 85:15.

[0167] The remaining preparation methods and parameters are consistent with those in Example 1.

[0168] Example 12 The difference between this embodiment and Embodiment 1 is that the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 0.2 wt%.

[0169] The remaining preparation methods and parameters are consistent with those in Example 1.

[0170] Example 13 The difference between this embodiment and Embodiment 1 is that the mass content of the terminal hydroxyl polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is 5.5 wt%.

[0171] The remaining preparation methods and parameters are consistent with those in Example 1.

[0172] Comparative Example 1 The difference between this comparative example and Example 1 is that the perovskite absorber layer does not contain a three-dimensional organic-inorganic hybrid elastic network structure, that is, the perovskite precursor solution in step (3) does not contain hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer.

[0173] The remaining preparation methods and parameters are consistent with those in Example 1.

[0174] Figure 1A stability comparison graph is shown between the single-junction perovskite solar cells provided in Example 1 and Comparative Example 1, with the test condition being continuous illumination for 1000 hours. As can be seen from the graph, after 1000 hours of continuous illumination, the photoelectric conversion efficiency of Example 1 remains above 94% of its initial efficiency, while the photoelectric conversion efficiency of Comparative Example 1 remains around 70% of its initial efficiency.

[0175] Comparative Example 2 The difference between this comparative example and Example 1 is that the hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer is replaced with hydroxyl-terminated polydimethylsiloxane.

[0176] The remaining preparation methods and parameters are consistent with those in Example 1.

[0177] Comparative Example 3 The difference between this comparative example and Example 1 is that the hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer is replaced with silica nanoclusters.

[0178] The remaining preparation methods and parameters are consistent with those in Example 1.

[0179] Performance testing The photoelectric performance of the perovskite-based solar cells provided in the above embodiments and comparative examples was tested: I. Preparatory work before testing 1. Visual inspection, including: Inspect the appearance of the photovoltaic modules for scratches, damage, cracks, or other defects.

[0180] 2. Surface cleaning, including: Wipe the component surface with ultrapure water, ethanol or isopropanol to remove fingerprints, dust and organic residues; After drying the components with nitrogen, let them stand for 10 minutes to avoid surface contamination affecting optical properties.

[0181] 3. Temperature equilibrium, including: The temperature of the components was stabilized at 25℃±0.5℃ using a constant temperature stage, and this temperature condition was maintained during the test.

[0182] 4. Equipment calibration, including: The light source spectrum was calibrated using a standard reference cell to conform to the AM1.5G standard spectral conditions, with a calibration wavelength range of 300 nm to 1200 nm. The irradiance uniformity deviation in the test area does not exceed ±2%, and the measurement error of the temperature sensor used is less than ±0.1℃.

[0183] II. Testing Equipment and Conditions 1. Core equipment IV tester: Keysight B2900A series, with a voltage resolution of 0.1mV and a current resolution of 0.1μA; Solar simulator: Class AAA compliant, with selectable pulsed or steady-state light source (Wacom WXS-200S-20 model). Temperature control console: Temperature regulation is achieved based on a thermoelectric cooling (TEC) module, with a control accuracy of ±0.2℃; Spectral response instrument: equipped with a quantum efficiency (QE) testing system (Bentham PVE300).

[0184] 2. Standard Test Conditions (STC) Irradiance: 1000W / m 2 (AM1.5G standard spectrum); Temperature: 25℃±2℃ (monitored in real time via TEC module); Light spot uniformity: The uniformity of the light spot covering the effective area of ​​the battery is >95%.

[0185] III. Parameter Testing Procedures 1. IV Characteristics (Voc, Isc, Pmax, FF) Testing Test equipment: solar simulator, IV tester and four-wire probe.

[0186] step: (1) Sample placement: Place the photovoltaic module in the center of the light spot of the simulator, and use a light shield to block the edge of the cell by 5mm to avoid light leakage at the edge; (2) IV scan: Apply a scan voltage from -0.5V to Voc+0.5V through an IV tester, set the scan step size to 10mV, and record the IV characteristic curve of the battery simultaneously; (3) Parameter extraction: Extract the open-circuit voltage Voc (voltage when current = 0) and short-circuit current Isc (current when voltage = 0) from the IV curve; (4) Power and fill factor calculation: Calculate the maximum power point on the IV curve (Pmax=Vmpp×Impp).

[0187] Furthermore, the test area in Example 8 was 900 cm². 2 The rest are 1cm 2 .

[0188] The test results are shown in Table 1.

[0189] Table 1 analyze: As shown in Table 1, this invention constructs a three-dimensional organic-inorganic hybrid elastic network structure in situ at the grain boundaries between at least some perovskite grains. This elastic network structure possesses both high elastic modulus and excellent interfacial adhesion characteristics, enabling it to form continuous mechanical dissipation paths in stress concentration areas. It actively absorbs and uniformly disperses local thermal and mechanical stresses, effectively suppressing the initiation and propagation of microcracks, while simultaneously enhancing grain boundary bonding and preventing interlayer delamination and film fragmentation. Furthermore, the organic-inorganic hybrid components in this elastic network structure can effectively passivate dangling bonds and defect states at grain boundaries, reduce non-radiative recombination centers, and suppress the formation of ion migration channels. Thus, while enhancing the mechanical strength of the perovskite thin film, it further improves the efficiency and stability of the device.

[0190] A comparison of Examples 1 and 10-11 shows that if the mass ratio of polydimethylsiloxane segments to silica nanoclusters is too small, there will be too many rigid inorganic nodes in the network, resulting in insufficient flexibility and excessively high elastic modulus of the three-dimensional hybrid network. This makes it unable to effectively absorb and disperse residual stress inside the perovskite film, and excessive SiO2 is prone to agglomeration at grain boundaries, which will damage the uniformity of the film and increase non-radiative recombination centers. If the mass ratio of polydimethylsiloxane segments to silica nanoclusters is too large, the proportion of organic segments in the network will be too high and the number of inorganic crosslinking points will be too small, resulting in insufficient mechanical strength and decreased thermal stability of the three-dimensional network. This makes it difficult to provide sufficient structural support, and the network is prone to plastic deformation or even breakage under stress, thus losing its stress buffering capacity.

[0191] A comparison of Examples 1 and 12-13 shows that if the mass content of the hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is too small, a continuous and dense three-dimensional stress buffer network cannot be formed at the perovskite grain boundaries, resulting in a weak stress release effect and difficulty in effectively suppressing the initiation and propagation of microcracks. The mechanical reinforcement and passivation effects are also not significant. If the mass content of the hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer in the perovskite precursor solution is too large, the excessive elastomer precursor will seriously interfere with the normal crystallization process of the perovskite precursor, leading to a reduction in perovskite grain size, a decrease in crystallinity, and an increase in grain boundary defect density. At the same time, the excessively thick elastomer insulating layer will hinder the effective transport of charge carriers, resulting in a significant decrease in the photoelectric conversion efficiency of the device.

[0192] As can be seen from the comparison between Example 1 and Comparative Example 1, if the perovskite absorber layer does not contain a three-dimensional organic-inorganic hybrid elastic network structure, the perovskite film can only rely on its intrinsic mechanical properties to withstand stress. Under thermal stress cycling or mechanical bending conditions, it is very easy to undergo brittle fracture and interlayer delamination. Furthermore, there is a lack of effective defect passivation at the grain boundaries, resulting in severe non-radiative recombination and poor long-term operational stability and mechanical durability of the device.

[0193] As can be seen from the comparison between Example 1 and Comparative Example 2, if only hydroxyl-terminated polydimethylsiloxane is used, there is a lack of inorganic SiO2 nanoclusters as physical / chemical crosslinking nodes, which cannot form a high-strength three-dimensional interpenetrating network. The material exhibits the soft and elastic properties of a pure organic polymer, with insufficient mechanical strength and thermal stability. Furthermore, the lack of coordination between SiO2 nodes and uncoordinated lead ions on the perovskite surface greatly reduces the grain boundary passivation effect.

[0194] As can be seen from the comparison between Example 1 and Comparative Example 3, if only silica nanoclusters are used, the stress dissipation and buffering mechanism of the flexible segments of terminal hydroxyl polydimethylsiloxane is lacking. The rigid SiO2 nanoparticles are prone to stress concentration at the grain boundaries, which not only fails to effectively release the residual stress inside the film, but may also become a new crack initiation source, aggravating the brittle fracture of the perovskite film, and making it difficult to form a good elastic interface adhesion with the perovskite grains.

Claims

1. A perovskite-based solar cell, characterized in that, The perovskite-based solar cell includes a perovskite absorber layer; The perovskite absorber layer comprises multiple perovskite grains, and at least some of the grain boundaries between the perovskite grains are distributed with a three-dimensional organic-inorganic hybrid elastic network structure.

2. The perovskite-based solar cell according to claim 1, characterized in that, The three-dimensional organic-inorganic hybrid elastic network structure includes polydimethylsiloxane segments and silica nanoclusters. The polydimethylsiloxane segments are cross-linked through Si-O-Si bonds to form a three-dimensional organic network, and the silica nanoclusters are embedded in the three-dimensional organic network as cross-linking points.

3. The perovskite-based solar cell according to claim 2, characterized in that, The three-dimensional organic-inorganic hybrid elastic network structure forms coordination bonds with uncoordinated B-site cations on the surface of the perovskite grains through the crosslinking points.

4. The perovskite-based solar cell according to claim 2, characterized in that, The mass ratio of the polydimethylsiloxane segments to the silica nanoclusters is (70-80):(20-30); And / or, the average particle size of the silica nanoclusters is 10-100 nm.

5. The perovskite-based solar cell according to claim 1, characterized in that, The elastic modulus of the perovskite absorber layer is 15-55 GPa; And / or, the Young's modulus of the perovskite absorber layer is 15-55 GPa.

6. The perovskite-based solar cell according to claim 1, characterized in that, The chemical formula of the perovskite absorber layer is ABX3, where A includes any one or a combination of at least two of formamidinium ions, methylamine ions or cesium ions, B includes lead ions and / or tin ions, and X is a halide ion. And / or, the thickness of the perovskite absorber layer is 300-1000 nm; And / or, the average grain size of the perovskite grains is 50-1000 nm.

7. A method for preparing a perovskite-based solar cell according to any one of claims 1-6, characterized in that, The preparation method includes the following steps: Prepare a perovskite precursor solution containing an organic-inorganic hybrid elastomer precursor; A perovskite precursor solution is coated onto a substrate using a film-forming process, followed by annealing to obtain a perovskite absorber layer.

8. The preparation method according to claim 7, characterized in that, The organic-inorganic hybrid elastomer precursor includes a hydroxyl-terminated polydimethylsiloxane-silica hybrid oligomer; And / or, the mass content of the organic-inorganic hybrid elastomer precursor in the perovskite precursor solution is 0.5-5 wt%.

9. The preparation method according to claim 7, characterized in that, The method for preparing the perovskite precursor solution containing the organic-inorganic hybrid elastomer precursor includes: First, a perovskite precursor solution is prepared, and then an organic-inorganic hybrid elastomer precursor is added and mixed to obtain the perovskite precursor solution containing the organic-inorganic hybrid elastomer precursor. And / or, the film-forming process includes any one or a combination of at least two of spin coating, blade coating, slot coating or inkjet printing; And / or, the annealing temperature is 80-150°C and the time is 15-30 min.

10. A photovoltaic module, characterized in that, The photovoltaic module includes the perovskite-based solar cell as described in any one of claims 1-6.