Plasma rapid annealing device
The plasma rapid annealing device forms plasma on the surface of the copper substrate for photovoltaic ribbons, which solves the problems of oxidation and pollution during annealing, achieves rapid annealing and deoxidation, and is suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202420323763.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-21
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2034-02-21
AI Technical Summary
The existing copper substrate used in photovoltaic ribbons is easily oxidized during the annealing process and requires cleaning and flux coating, resulting in environmental pollution and slow heating rate, making it difficult to be suitable for large-scale industrial production.
A plasma rapid annealing device is used to form plasma in the reaction chamber and use reducing gas ions to bombard the surface of the substrate to achieve rapid annealing and deoxidation, eliminating the need for flux coating steps.
It achieves rapid annealing of copper substrates, reduces oxidation phenomena, improves annealing efficiency, avoids environmental pollution, and is suitable for large-scale industrial production.
Smart Images

Figure CN221797591U_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal annealing, and in particular to a plasma rapid annealing device. Background Art
[0002] Photovoltaic welding ribbon is an important part of photovoltaic modules. It belongs to the electrical connection part and is used in the series or parallel connection of solar cells. It plays an important role in collecting current and conducting electricity, and ensures the stability of the output voltage and power of photovoltaic modules. Therefore, the quality of photovoltaic welding ribbon directly affects the current collection efficiency of solar silicon cells, and has a great impact on the power and efficiency of photovoltaic modules. This requires that photovoltaic welding ribbon has excellent characteristics such as low yield strength, high tensile strength, high elongation and high conductivity to meet the use requirements.
[0003] At present, photovoltaic welding ribbons are first subjected to a severe plastic deformation process and then annealed to obtain mechanical properties of low yield strength, high tensile strength and high elongation. Constant temperature annealing or DC pulse short-circuit annealing is commonly used in the industry to anneal the copper substrate for photovoltaic welding strips, but it is found that after the copper substrate has been subjected to severe plastic deformation process, drawing oil will remain on its surface, and its surface needs to be cleaned before constant temperature annealing or short-circuit annealing; at the same time, it is also found that these two annealing processes have some shortcomings; constant temperature annealing uses thermal radiation and heat transfer to heat the copper substrate, and its heating rate is slow, which is difficult to use for large-scale industrial production; and when DC pulse short-circuit annealing is used, if the copper substrate of one of the parallel stations breaks, it is easy to hit the copper substrate of the adjacent station, and the welding strip will spark; both also have the following common shortcomings: when the copper substrate is heated, the copper substrate will react with oxygen in the air to cause oxidation of the copper substrate surface, and after annealing is completed, it is necessary to coat the surface with flux before entering the tin furnace for tinning, and waste liquids such as flux will also cause environmental pollution problems.
[0004] Therefore, there is an urgent need for an annealing technology that can reduce the oxidation of the surface of the copper substrate for photovoltaic welding strips without the need for cleaning. Utility Model Content
[0005] The present application provides a plasma rapid annealing device, which can solve the problem in the prior art that the copper substrate for photovoltaic welding strips is oxidized during the annealing process and the copper substrate must be cleaned before annealing.
[0006] In order to solve one or more of the above technical problems, the technical solution adopted in this application is:
[0007] The present application provides a plasma rapid annealing device, comprising:
[0008] A reaction chamber having a built-in channel with openings at both ends, wherein the built-in channel is used for a substrate to pass through the reaction chamber, and one side of the reaction chamber is connected to a gas extraction component for controlling the pressure in the reaction chamber;
[0009] A combined gas source, connected to the reaction chamber, for providing carrier gas and reducing gas to the reaction chamber;
[0010] A generator is disposed on the outer wall of the reaction chamber, and the generator is electrically connected to a radio frequency power source so that the generator generates an electric field in the reaction chamber, thereby breaking down the carrier gas and the reducing gas to form a plasma; wherein the ions in the plasma bombard the surface of the substrate to heat the substrate, and the reducing gas ions in the plasma are used to reduce oxides on the surface of the substrate;
[0011] The conveying assembly is used for conveying the substrate to continuously pass through the reaction chamber, and the conveying assembly includes a grounding member in contact with the substrate.
[0012] Furthermore, the openings at both ends of the built-in channel are respectively connected to a first flange component and a second flange component, the first flange component has a first channel connected to the corresponding opening, the second flange component has a second channel connected to the corresponding opening, and the first channel and the second channel are both used for passing through the gap of the substrate.
[0013] Further, a first operating channel connected to the first channel is formed on the side wall of the first flange assembly, the cross-sectional area of the first operating channel is more than twice the cross-sectional area of the first channel, a first mounting joint is detachably connected to the first operating channel, a first stabilizing channel for the substrate to fit through is formed in the first mounting joint, and the first stabilizing channel is connected to the first channel;
[0014] The side wall of the second flange assembly is provided with a second operating channel connected to the second channel, the cross-sectional area of the second operating channel is more than twice the cross-sectional area of the second channel, a second mounting joint is detachably connected to the second operating channel, a second mounting joint is provided with a second stabilizing channel for the substrate to fit through, and the second stabilizing channel is connected to the second channel.
[0015] Furthermore, a gas inlet intersecting and communicating with the first channel is formed on the side wall of the first flange assembly, the gas inlet is connected to the combined gas source, and the carrier gas and the reducing gas enter the reaction chamber through the gas inlet.
[0016] Furthermore, a second air extraction port intersecting and communicating with the second channel is formed on a side wall of the second flange component, and the second air extraction port is communicated with the air extraction component to maintain the pressure in the reaction chamber.
[0017] Furthermore, a first gas extraction port intersecting and communicating with the first channel is formed on the side wall of the first flange assembly. The first gas extraction port is connected to the gas extraction assembly through a first gas extraction pipeline. A throttle valve for controlling the gas extraction rate is provided in the first gas extraction pipeline to allow the carrier gas and the reducing gas to enter the reaction chamber and reduce the amount of air entering the reaction chamber.
[0018] Furthermore, the reaction chamber includes a quartz tube or a ceramic tube.
[0019] Furthermore, the generator includes a stainless steel electrode or a copper spiral coil.
[0020] According to the specific embodiments provided in this application, this application discloses the following technical effects:
[0021] The substrate is passed through the reaction chamber by means of a conveying component, and the reaction chamber is evacuated before the carrier gas and the reducing gas are introduced, thereby providing an atmosphere for the formation of plasma, and the reducing gas is used to reduce the oxide on the surface of the substrate, thereby eliminating the step of applying flux in the subsequent process; after the power is started and the generating element is connected, an electric field is formed in the reaction chamber to break through the carrier gas and the reducing gas and form plasma, and the ions in the plasma continuously bombard the substrate, converting kinetic energy into heat energy, thereby achieving annealing of the substrate and cleaning the surface of the substrate, and the reducing gas ions in the plasma reduce the oxide on the surface of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 A schematic diagram of the structure of a plasma rapid annealing device provided in an embodiment of the present application;
[0024] Figure 2 A schematic diagram of the structure of the reaction chamber provided in an embodiment of the present application;
[0025] Figure 3 A structural schematic diagram of the connection relationship between the reaction chamber and the first flange assembly provided in an embodiment of the present application;
[0026] Figure 4A schematic diagram of the structure of a first flange assembly provided in an embodiment of the present application;
[0027] Figure 5 A schematic diagram of the structure of a second flange assembly provided in an embodiment of the present application;
[0028] Figure 6 A schematic diagram of the steps of the annealing method provided in an embodiment of the present application;
[0029] Figure 7 A schematic diagram of the structure of a plasma rapid annealing device in which the generating element provided in an embodiment of the present application is a copper spiral coil.
[0030] Reference numerals: 1, reaction chamber; 11, built-in channel; 12, opening; 13, substrate;
[0031] 2. Air extraction assembly; 21. Mechanical pump; 22. Second air extraction pipeline;
[0032] 3. Combined gas source; 31. Carrier gas source; 32. Reduction gas source;
[0033] 4. Occurrence;
[0034] 5. Transmission assembly; 51. Grounding piece; 52. Pay-off machine; 53. Transport roller; 54. Take-up machine;
[0035] 6. RF power supply; 61. RF matching device;
[0036] 7, first delivery pipeline; 71, main pipeline; 72, first gas path; 721, first switch valve; 722, first flow regulating valve; 73, second gas path; 731, second switch valve; 732, second flow regulating valve;
[0037] 8. first flange assembly; 81. first channel;
[0038] 82, first air extraction joint; 821, first air extraction port; 822, first air extraction pipeline; 8221, throttle valve;
[0039] 83, air inlet flange; 831, first threaded hole; 832, first mounting column; 833, first operating channel; 834, first mounting joint; 8341, first stabilizing channel; 835, air inlet;
[0040] 84. A first fixing flange;
[0041] 9. Second flange assembly; 91. Second channel; 92. Second fixed flange; 93. Second exhaust joint; 931. Second operating channel; 932. Second mounting joint; 9321. Second stabilizing channel; 933. Second exhaust port. DETAILED DESCRIPTION
[0042] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments in the present application belong to the scope of protection of the present application.
[0043] As described in the background technology, in order to make the photovoltaic welding ribbon have excellent properties such as low yield strength, high tensile strength, high elongation and high electrical conductivity to meet the use requirements, it is currently necessary to subject the copper substrate of the photovoltaic welding ribbon to severe plastic deformation before annealing. However, the two annealing processes currently used, namely, constant temperature annealing and DC pulse short-circuit annealing, have some shortcomings. For example, constant temperature annealing uses thermal radiation and heat transfer to heat the copper substrate, and its heating rate is slow, which is difficult to use for large-scale industrial production. When DC pulse short-circuit annealing is used, due to There are multiple parallel identical production lines during the processing of soldering strips. If the copper substrate of one of the parallel workstations is broken, the broken copper substrate is easy to hit the copper substrate of the adjacent workstation, causing a short circuit and sparking of the soldering strip. At the same time, both have the following common shortcomings: when the copper substrate for photovoltaic soldering strips is heated, the copper substrate will react with oxygen in the air to cause oxidation of the copper substrate surface, and after annealing is completed, flux needs to be coated on its surface before it can enter the tin furnace for tinning, and waste liquids such as flux will also cause environmental pollution problems.
[0044] In order to solve one or more of the above-mentioned technical problems in the prior art, the present application creatively proposes a plasma rapid annealing device, which uses a conveying component to pass the substrate through a reaction chamber, and then introduces a carrier gas and a reducing gas after the reaction chamber is evacuated, thereby providing an atmosphere for the formation of plasma, and using the reducing gas to reduce the oxides on the surface of the substrate; after starting the power supply and connecting the generating element, an electric field is formed in the reaction chamber to break through the carrier gas and the reducing gas and form a plasma, and the ions in the plasma continuously bombard the substrate, converting kinetic energy into thermal energy, thereby achieving annealing of the substrate and having a cleaning effect on the surface of the substrate.
[0045] The plasma rapid annealing device and annealing method of the present application are described in detail below in conjunction with various embodiments and drawings.
[0046] Example 1
[0047] Reference Figure 1 As shown, the plasma rapid annealing device includes a reaction chamber 1, a gas extraction component 2, a combined gas source 3, a generator 4 and a conveying component 5. The gas extraction component 2 and the combined gas source 3 are respectively connected to the reaction chamber 1, the generator 4 is arranged on the side wall of the reaction chamber 1, and the generator 4 is electrically connected to the radio frequency power supply 6. The conveying component 5 is used to transport the substrate 13 to continuously pass through the reaction chamber 1, and the conveying component 5 includes a grounding component 51 in contact with the substrate 13.
[0048] In this embodiment, the substrate is a copper substrate.
[0049] Further, see Figure 1 and Figure 2 As shown, the reaction chamber 1 has a built-in channel 11 with openings 12 at both ends. The built-in channel 11 is used for the substrate 13 to pass through the reaction chamber 1. The user can pass the substrate 13 into the built-in channel 11 through the opening 12 at one end, and pass through the reaction chamber 1 through the opening 12 at the other end. Start the exhaust component 2 to extract the air in the reaction chamber 1 so that the pressure in the reaction chamber 1 meets the process requirements, then start the combined gas source 3 to pass a certain amount of carrier gas and reducing gas into the reaction chamber 1, and then start the radio frequency power supply 6 to transmit the electrical signal to the generator 4 to generate an electric field in the reaction chamber 1, thereby breaking through the carrier gas and reducing gas and forming plasma. The ions in the plasma continuously bombard the surface of the substrate 13, converting kinetic energy into heat energy to heat the substrate 13 and clean the surface of the substrate 13; at the same time, the reducing gas ions in the plasma reduce the oxides on the surface of the substrate 13. The conveying component 5 continuously inputs the substrate 13 into the reaction chamber 1 for annealing and outputs the annealed substrate 13 from the reaction chamber 1. During the transportation process, the grounding member 51 pours the charged particles on the substrate 13 into the ground to form a closed loop.
[0050] Preferably, the openings 12 at both ends are coaxially arranged with the axis of the built-in channel 11 , so as to facilitate the substrate 13 to pass through the reaction chamber 1 and reduce the wear of the substrate 13 .
[0051] Preferably, the reaction chamber 1 is in a hollow cylindrical shape, which facilitates the insertion of the substrate 13 and the subsequent assembly of parts.
[0052] Specifically, the grounding member 51 is in the shape of a roller, and plays the role of conveying the substrate 13 while grounding. The conveying assembly 5 includes a pay-off machine 52, a transport roller 53 and a take-up machine 54; the pay-off machine 52, the grounding member 51, the reaction chamber 1, the transport roller 53 and the take-up machine 54 are arranged at intervals along a straight line to facilitate the conveying of the substrate 13. The pay-off machine 52 continuously pays out the substrate 13, the grounding member 51 and the transport roller 53 support and restrict the substrate 13 and convey the substrate 13 in a direction close to the take-up machine 54, reducing the tension of the substrate 13 during transportation, and the take-up machine 54 continuously takes back the substrate 13 that has completed annealing.
[0053] Preferably, the generator 4 is nested in the side wall at the center of the reaction chamber 1 to facilitate forming a stable and uniform electric field in the reaction chamber 1 .
[0054] In this embodiment, the reaction chamber 1 is a quartz tube, but it can be understood that the quartz tube is only an exemplary and non-restrictive description in the embodiment of the present application. Without violating the concept of the utility model of the present application, any known type of tube with good insulation and heat resistance can be used as the reaction chamber 1 in the present application, such as a ceramic tube.
[0055] Reference Figure 2 , Figure 3 and Figure 4 As shown, the openings 12 at both ends of the built-in channel 11 are respectively connected to the first flange component 8 and the second flange component 9. The first flange component 8 has a first channel 81 connected to the corresponding opening 12, and the second flange component 9 has a second channel 91 connected to the corresponding opening 12. The first channel 81 and the second channel 91 are both used for passing through the gap of the substrate 13.
[0056] Preferably, the first channel 81 and the second channel 91 are both coaxially arranged with the inner channel 11 .
[0057] Specifically, the first flange assembly 8 includes a first gas extraction joint 82, an air inlet flange 83, and a first fixed flange 84. The first fixed flange 84 is sleeved on one end of the reaction chamber 1 and fixedly connected to the reaction chamber 1; the air inlet flange 83 is fixedly connected to a side of the first fixed flange 84 away from the reaction chamber 1, and a first threaded hole 831 is provided on the side of the air inlet flange 83 away from the first fixed flange 84. The first gas extraction joint 82 is connected to a first mounting column 832 threadedly connected to the first threaded hole 831; the first channel 81 runs through the first gas extraction joint 82, the air inlet flange 83 and the first fixed flange 84 from one end of the first gas extraction joint 82 away from the reaction chamber 1.
[0058] Preferably, a ring groove for placing an O-ring is provided on one side of the inlet flange 83 away from the first fixed flange 84. A sealing ring (not shown) in a squeezed state is provided between the first fixed flange 84 and the inlet flange 83 to seal the connection between the reaction chamber 1 and the first fixed flange 84.
[0059] Furthermore, a first operating channel 833 coaxial with the first channel 81 is provided at one end of the first exhaust connector 82 away from the reaction chamber 1. The cross-sectional area of the first operating channel 833 is more than twice the cross-sectional area of the first channel 81. The first operating channel 833 is a threaded hole. The first operating channel 833 is threadedly connected with a first mounting connector 834. The first mounting connector 834 is provided with a first stable channel 8341 for the substrate 13 to fit through. The first stable channel 8341 is coaxial with and communicates with the first channel 81. When the substrate 13 needs to be replaced, the first mounting connector 834 only needs to be screwed out of the first operating channel 833. The cross-sectional area of the first operating channel 833 is much larger than the cross-sectional area of the substrate 13, which is convenient for users to replace the substrate 13.
[0060] The cross section involved in this embodiment refers to the cross section in its own radial direction.
[0061] Preferably, a sealing ring groove for placing an O-ring is provided on a side of the first exhaust connector 82 away from the reaction chamber 1 .
[0062] Further, see Figure 1 and Figure 4 As shown, the side wall of the air inlet flange 83 is provided with an air inlet 835 intersecting and communicating with the first channel 81 . The air inlet 835 is connected to the combined gas source 3 through the first delivery pipeline 7 , so that the carrier gas and the reducing gas can enter the reaction chamber 1 through the air inlet 835 .
[0063] The combined gas source 3 includes a carrier gas source 31 and a reducing gas source 32, and the first delivery pipeline 7 includes a main pipeline 71. One end of the main pipeline 71 is connected to the air inlet 835, and the other end thereof is connected to the first gas pipeline 72 and the second gas pipeline 73. The first gas pipeline 72 is connected to the carrier gas source 31, and the second gas pipeline 73 is connected to the reducing gas source 32. A first switch valve 721 and a first flow regulating valve 722 are sequentially arranged on the first gas pipeline 72 along the direction from the carrier gas source 31 to the air inlet flange 83. The first switch valve 721 is used to control the opening and closing of the carrier gas source 31, and the first flow regulating valve 722 is used to control the flow of the carrier gas in the first gas pipeline 72. A second switch valve 731 and a second flow regulating valve 732 are sequentially arranged on the second gas pipeline 73 along the direction from the reducing gas source 32 to the air inlet flange 83. The second switch valve 731 is used to control the opening and closing of the reducing gas source 32, and the second flow regulating valve 732 is used to control the flow of the reducing gas in the second gas pipeline 73.
[0064] Specifically, refer to Figure 1 , Figure 3 and Figure 5 As shown, the second flange assembly 9 includes a second fixed flange 92 and a second gas extraction joint 93. The second fixed flange 92 is sleeved on the other end of the reaction chamber 1 and fixedly connected to the reaction chamber 1; the second gas extraction joint 93 is fixedly connected to the side of the second fixed flange 92 away from the reaction chamber 1; the second channel 91 passes through the second gas extraction joint 93 and the second fixed flange 92 from the end of the second gas extraction joint 93 away from the reaction chamber 1.
[0065] Furthermore, a second operating channel 931 coaxial with the second channel 91 is provided at one end of the second exhaust joint 93 away from the reaction chamber 1, and the cross-sectional area of the second operating channel 931 is more than twice the cross-sectional area of the second channel 91, so as to facilitate the movement of the substrate 13; the second operating channel 931 is a threaded channel, and the second operating channel 931 is threadedly connected with a second mounting joint 932, and a second stabilizing channel 9321 for the substrate 13 to fit through is provided in the second mounting joint 932, and the second stabilizing channel 9321 is coaxial with the second channel 91.
[0066] Furthermore, a second gas extraction port 933 orthogonally intersecting the second channel 91 is formed on the side wall of the second gas extraction joint 93 , and the second gas extraction port 933 is connected to the gas extraction component 2 to maintain the pressure in the reaction chamber 1 .
[0067] In this embodiment, the air extraction component 2 includes a mechanical pump 21, which is connected to the second air extraction port 933 through a second air extraction pipeline 22. After the mechanical pump 21 is started, the air in the reaction chamber 1 can be continuously extracted, so that the pressure in the reaction chamber 1 meets the process requirements. The reaction chamber 1 is connected to a pressure gauge so that the user can know the pressure in the reaction chamber 1 in time.
[0068] Furthermore, a first air extraction port 821 orthogonally intersecting the first channel 81 is provided on the side wall of the first air extraction joint 82, and the first air extraction port 821 is connected to the second air extraction pipeline 22 through the first air extraction pipeline 822, and further connected to the mechanical pump 21. A throttle valve 8221 for controlling the air extraction rate is provided in the first air extraction pipeline 822, so as to allow the carrier gas and the reducing gas to enter the reaction chamber 1 and reduce the air entering the reaction chamber 1; thus, only one mechanical pump 21 is used to complete the vacuuming of the reaction chamber 1 and to deliver the carrier gas and the reducing gas into the reaction chamber 1.
[0069] Specifically, after the mechanical pump 21 extracts the air in the reaction chamber 1 and meets the process requirements, the first switch valve 721 and the second switch valve 731 are opened, and the first flow regulating valve 722 and the second flow regulating valve 732 are adjusted to adjust the amount of carrier gas and reducing gas flowing into the reaction chamber 1, and the throttle valve 8221 is adjusted to control the extraction rate of the mechanical pump 21, so as to achieve the goal of preventing air from entering the reaction chamber 1 while allowing the mixed gas of carrier gas and reducing gas to enter the reaction chamber 1.
[0070] Example 2
[0071] Corresponding to the above-mentioned embodiment 1, the present application further provides an annealing method, wherein in this embodiment, the same or similar contents as those of the above-mentioned embodiment 1 can be referred to the above introduction, and will not be described in detail later. Figure 6 As shown, the method includes:
[0072] S100, opening the exhaust assembly to extract the air in the reaction chamber until the pressure in the reaction chamber reaches a preset vacuum degree;
[0073] Specifically, the substrate 13 on the pay-off machine 52 is placed on the grounding member 51, and then sequentially passes through the first stable channel, the first channel 81, the built-in channel 11, the second channel 91, and the second stable channel, and then placed on the transport roller 53, and wound on the take-up machine 54. The mechanical pump 21 is turned on, and the air in the reaction chamber 1 is discharged from the reaction chamber 1 through the second exhaust pipe and the mechanical pump 21, so that the vacuum degree in the reaction chamber 1 reaches the preset vacuum degree.
[0074] The preset vacuum degree ranges from 0 to 200 Pa.
[0075] S200, opening the combined gas source 3 to introduce carrier gas and reducing gas into the reaction chamber 1 until the gas pressure in the reaction chamber 1 reaches a preset pressure;
[0076] Specifically, the first switch valve 721 and the second switch valve 731 are opened, and the first flow regulating valve 722 and the second flow regulating valve 732 are adjusted to control the flow of the carrier gas and the reducing gas into the reaction chamber 1. At this time, the mechanical pump 21 is still working, so as to suck the gas in the carrier gas source 31 and the reducing gas source 32 into the first pipeline, and then the throttle valve 8221 is controlled to prevent air from entering the reaction chamber 1, and at the same time, the carrier gas and the reducing gas can enter the reaction chamber 1 and the pressure in the reaction chamber 1 reaches the preset pressure, thereby providing an annealing atmosphere for the reaction chamber 1.
[0077] The preset pressure ranges from 400 to 8000 Pa. The carrier gas includes argon or nitrogen, and the reducing gas includes hydrogen or ammonia.
[0078] S300, using a conveying assembly to continuously move the substrate through the reaction chamber at a preset speed;
[0079] Specifically, the wire pay-off machine 52 and the wire take-up machine 54 are started simultaneously, so that the substrate 13 passes through the reaction chamber 1 at a preset speed.
[0080] Among them, the preset speed range is 40 to 300 m / min.
[0081] S400, turning on the radio frequency power supply, which transmits an electrical signal to the generator at a preset frequency and preset power to form plasma in the reaction chamber.
[0082] The preset frequency ranges from 1.5 MHz to 13.56 MHz, and the preset power ranges from 100 W to 20 kW.
[0083] Specifically, after turning on the RF power supply 6, the frequency and power of the RF power supply 6 are adjusted to the preset frequency and preset power to form a uniform and stable electric field in the reaction chamber 1, thereby breaking down the carrier gas and the reducing gas in the reaction chamber 1 to form plasma. The plasma adheres to the surface of the substrate 13, and the ions in the plasma continuously bombard the surface of the substrate 13, converting kinetic energy into thermal energy, and finally completing plasma annealing; at the same time, the reducing gas ions reduce the oxides on the surface of the substrate 13.
[0084] Preferably, a radio frequency matcher 61 is electrically connected between the generator 4 and the radio frequency power supply 6, which can ensure that the radio frequency power supply 6 can effectively transmit energy to the generator 4 to provide maximum power transmission and system efficiency.
[0085] Example 3
[0086] Corresponding to the above-mentioned embodiments 1 and 2, the present application also provides an annealing method.
[0087] As a specific implementation method, refer to Figure 1 As shown, the carrier gas is argon, and the reducing gas is hydrogen; the generating element 4 is stainless steel, and the substrate 13 is a copper substrate for photovoltaic welding strips.
[0088] First, turn on the mechanical pump 21 to evacuate the reaction chamber 1 until the air pressure in the reaction chamber 1 reaches below 200Pa. Then turn on the carrier gas source 31 and the reducing gas source 32 to allow argon and hydrogen to enter the reaction chamber 1 and adjust the first flow regulating valve 722 and the second flow regulating valve 732 to make the pressure in the reaction chamber 1 between 400 and 8000Pa. Then turn on the pay-off machine 52 and the take-up machine 54 at the same time to transport the copper substrate for photovoltaic welding strip to the vacuum chamber at a speed of 50m / min. Then turn on the RF power supply 6, and by adjusting the power supply frequency and power, a lavender plasma is formed in the reaction chamber 1 and attached to the surface of the copper substrate for photovoltaic welding strip, and finally the annealing treatment of the copper substrate for photovoltaic welding strip is completed.
[0089] As shown in Table 1, the mechanical properties of the copper substrate after annealing are characterized. By comparing with the copper substrate without annealing, it can be found that the yield strength of the copper substrate after low-pressure Ar-H2 capacitive plasma discharge annealing is greatly reduced. Under the process conditions of the copper substrate's linear speed of 50 / min and the RF power supply 6 discharge power of 450W, the yield strength of the copper substrate is reduced to 62MPa; the elongation is also greatly improved compared with the unannealed sample, from the original 2.4% to 29%. At the same time, after the copper substrate is annealed quickly, it is found that the surface of the copper substrate is clean, and the oxide on the surface of the copper substrate disappears after the annealing is completed. It can be seen that the annealing speed of Ar-H2 capacitive plasma discharge annealing is fast, and it can not only enable the sample to achieve certain mechanical properties, but also has a certain cleaning and deoxidation ability, so that the copper substrate does not need to be coated with flux during subsequent tinning.
[0090] Table 1 Mechanical properties test of samples annealed by argon and hydrogen capacitive coupled plasma
[0091] Power supply power / W Unprocessed 150 300 450 Line speed / m / min 50 50 50 50 Diameter / mm 0.395 0.395 0.395 0.395 Yield strength / MPa 254 173 114 62 Tensile strength / MPa 255 241 238 226 Elongation 2.40% 19.30% 26.50% 29%
[0092] As a specific implementation, the carrier gas is nitrogen, the reducing gas is hydrogen; the generator 4 is stainless steel, and the substrate 13 is a copper substrate for photovoltaic welding strips.
[0093] First, turn on the mechanical pump 21 to evacuate the reaction chamber 1 until the gas pressure in the reaction chamber 1 reaches below 200Pa. Then turn on the carrier gas source 31 and the reducing gas source 32 to allow argon and hydrogen to enter the reaction chamber 1 and adjust the first flow regulating valve 722 and the second flow regulating valve 732 to make the pressure in the reaction chamber 1 between 400 and 8000Pa. Then turn on the wire unwinding machine 52 and the wire take-up machine 54 at the same time to transport the copper substrate to the vacuum chamber at a speed of 50m / min. Then turn on the RF power supply 6, and by adjusting the power supply frequency and power, a purple plasma is formed in the reaction chamber 1 and attached to the surface of the copper substrate, and finally the annealing treatment of the copper substrate is completed.
[0094] As shown in Table 2, under the process conditions of the copper substrate's linear speed of 50 / min and the RF power supply 6 discharge power of 450W, the yield strength of the copper substrate dropped to 68MPa; the elongation reached 28.75%. The surface was clean and free of oxidation. Compared with argon as a carrier gas, the annealing effect of nitrogen capacitively coupled plasma was slightly worse. The annealing effect of low-pressure capacitively coupled plasma on the copper substrate for photovoltaic welding strips will also vary due to the different types of carrier gas and reducing gas.
[0095] Table 2 Mechanical properties test of nitrogen and hydrogen capacitive coupled plasma annealing samples
[0096] Power supply power / W Unprocessed 150 300 450 Line speed / m / min 50 50 50 50 Diameter / mm 0.395 0.395 0.395 0.395 Yield strength / MPa 254 190.15 121.1 68 Tensile strength / MPa 255 243.2 229.8 228 Elongation 2.40% 17.0% 25.50% 28.75%
[0097] As an implementation method, refer to Figure 7 As shown, the carrier gas is argon, the reducing gas is hydrogen; the generating element 4 is a copper solenoid, and the substrate 13 is a copper substrate for photovoltaic welding strips.
[0098] First, the copper spiral coil is connected to the RF power supply 6, and then the mechanical pump 21 is started to extract the air in the reaction chamber 1, so that the pressure in the reaction chamber 1 drops below 200Pa, and the carrier gas source 31 and the reducing gas source 32 are turned on to make the argon gas and hydrogen flow into the reaction chamber 1, and the first flow regulating valve 722 and the second flow regulating valve 732 are adjusted to make the pressure in the reaction chamber 1 between 400 and 8000Pa, and then the pay-off machine 52 and the take-up machine 54 are turned on at the same time to transport the copper substrate to the reaction chamber 1 at a speed of 50m / min. The RF power supply 6 is turned on and the frequency and power of the RF power supply 6 are adjusted, so that the lavender plasma is generated in the reaction chamber 1 and attached to the surface of the copper substrate, and finally the annealing treatment of the copper substrate is completed.
[0099] As shown in Table 3, under the process conditions of a line speed of 50 m / min and a RF power supply 6 power of 450 W, the yield strength of the copper substrate can be reduced to 53.12 MPa, and the elongation can reach 26.5%. At the same time, the surface of the copper substrate is clean and free of oxides.
[0100] Table 3 Mechanical properties test of samples annealed by argon and hydrogen inductively coupled plasma
[0101] Power supply power / W Unprocessed 150 300 450 Line speed / m / min 50 50 50 50 Diameter / mm 0.395 0.395 0.395 0.395 Yield strength / MPa 254 112.15 85.88 53.12 Tensile strength / MPa 255 229 227 226.15 Elongation 2.40% 23.75% 26.50% 26.50%
[0102] As an implementation mode, the carrier gas is nitrogen, the reducing gas is hydrogen; the generating element 4 is a copper solenoid, and the substrate 13 is a copper substrate for photovoltaic welding strips.
[0103] First, the copper spiral coil is connected to the RF power supply 6, and then the mechanical pump 21 is started to extract the air in the reaction chamber 1, so that the pressure in the reaction chamber 1 drops below 200Pa, and the carrier gas source 31 and the reducing gas source 32 are turned on to allow nitrogen and hydrogen to flow into the reaction chamber 1, and the first flow regulating valve 722 and the second flow regulating valve 732 are adjusted to make the pressure in the reaction chamber 1 between 400 and 8000Pa, and then the pay-off machine 52 and the take-up machine 54 are turned on at the same time to transport the copper substrate to the reaction chamber 1 at a speed of 50m / min. The RF power supply 6 is turned on and the frequency and power of the RF power supply 6 are adjusted, so that purple plasma is generated in the reaction chamber 1 and attached to the surface of the copper substrate, and finally the annealing treatment of the copper substrate is completed.
[0104] As shown in Table 4, under the process conditions of a line speed of 50 m / min and a RF power supply 6 power of 450 W, the yield strength of the copper substrate can be reduced to 59.12 MPa, and the elongation can reach 26.5%. At the same time, the surface of the copper substrate is clean and free of oxides.
[0105] Table 4 Mechanical properties test of nitrogen and hydrogen inductively coupled plasma annealing samples
[0106]
[0107]
[0108] The above is a detailed introduction to a plasma rapid annealing device provided by the present application. The principles and implementation methods of the present application are described in detail using specific examples. The description of the above embodiments is only used to help understand the method and core idea of the present application. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present application.
[0109] In the description of the present application, it should be understood that the terms "vertical", "parallel", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present application, unless otherwise specified, "multiple" means two or more.
[0110] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0111] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A plasma rapid annealing device, characterized in that: The device comprises: A reaction chamber having a built-in channel with openings at both ends, wherein the built-in channel is used for a substrate to pass through the reaction chamber, and one side of the reaction chamber is connected to a gas extraction component for controlling the pressure in the reaction chamber; A combined gas source, connected to the reaction chamber, for providing carrier gas and reducing gas to the reaction chamber; A generator is disposed on the outer wall of the reaction chamber, and the generator is electrically connected to a radio frequency power source so that the generator generates an electric field in the reaction chamber, thereby breaking down the carrier gas and the reducing gas to form a plasma; wherein the ions in the plasma are used to bombard the surface of the substrate to heat the substrate, and the reducing gas ions in the plasma are used to reduce oxides on the surface of the substrate; The conveying assembly is used for conveying the substrate to continuously pass through the reaction chamber, and the conveying assembly includes a grounding member in contact with the substrate.
2. The plasma rapid annealing device according to claim 1, characterized in that: The openings at both ends of the built-in channel are respectively connected to a first flange component and a second flange component. The first flange component has a first channel connected to the corresponding opening, and the second flange component has a second channel connected to the corresponding opening. The first channel and the second channel are both used for passing through the gap of the substrate.
3. The plasma rapid annealing device according to claim 2, characterized in that: A first operating channel connected to the first channel is formed on the side wall of the first flange component, the cross-sectional area of the first operating channel is more than twice the cross-sectional area of the first channel, a first mounting joint is detachably connected to the first operating channel, a first stabilizing channel for the substrate to fit through is formed in the first mounting joint, and the first stabilizing channel is connected to the first channel; The side wall of the second flange assembly is provided with a second operating channel connected to the second channel, the cross-sectional area of the second operating channel is more than twice the cross-sectional area of the second channel, a second mounting joint is detachably connected to the second operating channel, a second mounting joint is provided with a second stabilizing channel for the substrate to fit through, and the second stabilizing channel is connected to the second channel.
4. The plasma rapid annealing device according to claim 2, characterized in that: The side wall of the first flange assembly is provided with an air inlet intersecting and communicating with the first channel, the air inlet is connected to the combined gas source, and the carrier gas and the reducing gas enter the reaction chamber through the air inlet.
5. The plasma rapid annealing device according to claim 2, characterized in that: A second air pumping port intersecting and communicating with the second channel is formed on the side wall of the second flange component, and the second air pumping port is connected to the air pumping component to maintain the pressure in the reaction chamber.
6. The plasma rapid annealing device according to claim 4, characterized in that: A first gas extraction port intersecting and communicating with the first channel is formed on the side wall of the first flange assembly. The first gas extraction port is connected to the gas extraction assembly through a first gas extraction pipeline. A throttle valve for controlling the gas extraction rate is provided in the first gas extraction pipeline to allow the carrier gas and the reducing gas to enter the reaction chamber and reduce the amount of air entering the reaction chamber.
7. The plasma rapid annealing device according to claim 1, characterized in that: The reaction chamber includes a quartz tube or a ceramic tube.
8. The plasma rapid annealing device according to claim 1, characterized in that: The generating element includes a stainless steel electrode or a copper spiral coil.
Citation Information
Cited By
Plasma rapid annealing device and annealing method
CN118064684A