Defluorination composite current collector

By introducing a defluorination layer into the composite current collector to intercept fluorine ions, the problem of corrosion of the conductive layer in lithium-ion batteries is solved and the service life of the battery is extended.

CN221861690UActive Publication Date: 2024-10-18ANHUI JIMAT NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323487566.5
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2024-10-18
Estimated Expiration
2033-12-20

AI Technical Summary

Technical Problem

The conductive layer of the composite current collector in lithium-ion batteries easily reacts with fluoride ions in the electrolyte, leading to corrosion and shortened service life.

Method used

Design a defluorination composite current collector, including a coating area and a blank area. Active materials are arranged on the coating area and between it and the defluorination layer. The defluorination layer consists of an adhesive, a conductive agent and a fluoride ion adsorption material. Composition, with a thickness of 10nm to 2000nm, to intercept fluoride ions and prevent them from contacting the conductive layer.

Benefits of technology

It effectively prevents the reaction between fluoride ions and the composite current collector conductive layer, extending the service life of the composite current collector and lithium-ion battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221861690U_ABST
    Figure CN221861690U_ABST
Patent Text Reader

Abstract

The utility model discloses a defluorination composite current collector in the technical field of composite current collector production, which comprises a current collector body, the current collector body comprises a coating area and a blank area, an active material is arranged on the coating area, and a defluorination layer is arranged between the active material and the coating area. According to the composite current collector, the problems that the conducting layer of the existing composite current collector is easy to react with the conducting layer of the composite current collector, the conducting layer of the composite current collector is corroded, the conducting layer of the composite current collector has defects, and the service lives of the composite current collector and the lithium ion battery are shortened are solved; and fluorine ions are prevented from being in contact with the conducting layer of the composite current collector, so that the fluorine ions are prevented from reacting with the conducting layer of the composite current collector, the conducting layer of the composite current collector is prevented from being corroded, the service life of the composite current collector is prolonged, and the service life of the lithium ion battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of composite current collector production, in particular to a defluorinated composite current collector. Background Art

[0002] A composite current collector is a polymer material with a copper or aluminum layer plated on the top and bottom surfaces of a substrate such as PET or PP. It has a sandwich structure and is also called a conductive film. It is a type of material with multiple good properties and is widely used in lithium-ion batteries. It is mainly used as a battery current collector in lithium-ion batteries.

[0003] Lithium-ion batteries contain electrolytes. Due to the humid and heated environment, lithium hexafluorophosphate in the electrolyte will self-catalytically decompose to produce fluoride ions. However, fluoride ions penetrate into the interior of the composite current collector and easily react with the conductive layer of the composite current collector, corroding the conductive layer of the composite current collector, causing defects in the conductive layer of the composite current collector, shortening the service life of the composite current collector, affecting the normal use of the lithium-ion battery, and shortening the life of the lithium-ion battery.

[0004] The above defects need to be solved urgently. Utility Model Content

[0005] In order to solve the problem that the conductive layer of the existing composite current collector is easy to react with the conductive layer of the composite current collector, corrode the conductive layer of the composite current collector, cause defects in the conductive layer of the composite current collector, and shorten the service life of the composite current collector and the lithium ion battery, the utility model provides a defluorinated composite current collector.

[0006] The technical solution of the utility model is as follows:

[0007] A defluorinated composite current collector comprises a current collector body, wherein the current collector body comprises a coating area and a blank area, an active material is arranged on the coating area, and a defluorinated layer is arranged between the active material and the coating area.

[0008] According to the above-mentioned solution of the utility model, the thickness of the defluorination layer is 10nm to 2000nm.

[0009] According to the above-mentioned solution of the utility model, the current collector body further includes a support layer and a conductive layer arranged on the surface of the support layer, and the coating area and the blank area are arranged on the surface of the conductive layer.

[0010] Furthermore, the conductive layer is made of copper or aluminum.

[0011] According to the utility model of the above scheme, the current collector body also includes a support layer, a base layer arranged on the surface of the support layer, a transition layer is arranged on the surface of the base layer, and the coating area and the blank area are arranged on the surface of the transition layer.

[0012] Furthermore, the base layer is made of copper, nickel, aluminum, silicon nitride, silicon carbide, aluminum oxide or polyethylene glycol.

[0013] According to the above scheme of the utility model, the current collector body also includes a supporting layer, a base layer arranged on the surface of the supporting layer, a transition layer is arranged on the surface of the base layer, a thickening layer is arranged on the surface of the transition layer, and the coating area and the blank area are arranged on the surface of the thickening layer.

[0014] According to the utility model of the above solution, the thickness of the support layer is 3um to 8um.

[0015] According to the above-mentioned solution of the utility model, the thickness of the primer layer is 10nm to 50nm.

[0016] According to the utility model of the above solution, the thickness of the transition layer is 100nm to 500nm.

[0017] According to the utility model of the above scheme, the thickness of the thickened layer is 500nm to 1000nm.

[0018] According to the utility model of the above scheme, a white edge area is also provided on the support layer to ensure smooth rolling.

[0019] According to the utility model of the above scheme, the width of the white edge area is 1 cm to 3 cm.

[0020] The utility model according to the above scheme has the following beneficial effects:

[0021] In the above-mentioned defluorinated composite current collector, a defluorination layer is arranged between the active material and the coating area. The defluorination layer can intercept fluoride ions and prevent the fluoride ions from contacting the conductive layer of the composite current collector, thereby avoiding the reaction between the fluoride ions and the conductive layer of the composite current collector, and further preventing the corrosion of the conductive layer of the composite current collector, thereby extending the service life of the composite current collector and thus extending the life of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a structural schematic diagram of the utility model;

[0023] Figure 2 It is a cross-sectional view of the utility model;

[0024] Figure 3 It is a schematic diagram of the structure of the current collector body in the utility model;

[0025] Figure 4 is a schematic diagram of the structure of a current collector body in an optional embodiment;

[0026] Figure 5 is a schematic diagram of the structure of the current collector body in another optional embodiment;

[0027] Figure 6 Schematic diagram of the structure of the support layer.

[0028] In the figure, 1. current collector body; 11. blank area; 12. coating area; 13. defluorination layer; 14. support layer; 141. coating area; 142. white edge area; 15. conductive layer; 16. base layer; 17. transition layer; 18. thickening layer; 19. active material. DETAILED DESCRIPTION

[0029] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] like Figure 1 , Figure 2 As shown, the utility model provides a defluorinated composite current collector, including a current collector body 1, the current collector body 1 includes a blank area 11 and a coating area 12, the blank area 11 is used for welding with the electrode of the lithium ion battery, the coating area 12 is provided with an active material 19, and a defluorination layer 13 is provided between the active material 19 and the coating area 12.

[0031] Specifically, the defluorination layer 13 includes an adhesive, a conductive agent and a fluoride ion adsorption material, wherein the adhesive serves to bond the conductive agent and the fluoride ion adsorption material to the current collector body 1, the conductive agent serves to make the entire fluoride ion filter layer conductive, reduce the resistance between the active material 19 and the current collector body 1, reduce the internal resistance of the lithium ion battery, and thus improve the conductivity of the lithium ion battery, and the fluoride ion adsorption material serves to adsorb the fluoride ions in the electrolyte, so that the current collector body 1 contacts the electrolyte without fluoride ions, thereby preventing the fluoride ions from corroding the current collector body 1. The utility model provides a defluorination layer 13 between the active material 19 and the coating area 12, and the defluorination layer 13 can intercept the fluoride ions, prevent the fluoride ions from contacting the conductive layer 15 of the composite current collector, thereby avoiding the fluoride ions from reacting with the conductive layer 15 of the composite current collector, and then preventing the conductive layer 15 of the composite current collector from corroding, thereby extending the service life of the composite current collector, and thus extending the life of the lithium ion battery.

[0032] In this embodiment, the content of the conductive agent is 30% to 50%, the content of the binder is 20% to 40%, and the content of the fluoride ion adsorbing material is 10% to 20%. The content of the conductive agent can be designed to be 40%, the content of the binder can be 40%, and the content of the fluoride ion adsorbing material can be 20%. Of course, in actual design, the content of the adhesive, the content of the conductive agent, and the content of the fluoride ion adsorbing material can be designed according to actual needs. In addition, the defluorination layer 13 can also be designed to be composed of a conductive agent and a fluoride ion adsorbing material, or the defluorination layer 13 can be designed to be composed of conductive wire and a fluoride ion adsorbing material. The fluoride ion adsorbing material can be designed to be nano zeolite. In actual design, the composition of the defluorination layer 13 can be designed according to actual needs.

[0033] In the present embodiment, the conductive agent can be designed as a conductive carbon material, such as conductive carbon black, conductive carbon powder, acetylene black, graphene or conductive graphite (such as natural graphite or artificial graphite), Ketjen black, graphite sheet, carbon nanotube, etc. The binder can be designed as PVDF, or PAA (polyacrylic acid), water-based polyacrylate, polyvinyl acetate or styrene butadiene (SBR) emulsion, etc. The fluoride ion adsorption material can be designed as a defluoridation agent, which can be clinoptilolite, activated alumina, activated magnesium oxide, fly ash, hydroxy calcium phosphate, oxidized calcium resin, etc. Of course, in actual design, the composition of the conductive agent, binder and fluoride ion adsorption material can be designed according to actual needs.

[0034] like Figure 3 As shown, in this embodiment, the current collector body 1 also includes a support layer 14 and a conductive layer 15. The conductive layer 15 can be formed on the surface of the support layer 14 by magnetron sputtering coating or vacuum evaporation coating. In addition, the material of the support layer 14 can be HIPS, PCTFE, PMMA, FEP, PFA, PTFE, PMP, HDPE, LDPE, LLDPE, PMP, PP, UHMWPE, PS, HIPS, ABS, EVA, SAN, ECTFE, ETFE, PPE, PE, SMA, MABS, PPE, PBT, PSU, CP, LCP, PA6-10, PBT, PEI, PET, PETG, POM, etc. Of course, in actual design, the material of the support layer 14 can be designed according to actual needs. In addition, the material of the conductive layer 15 is copper or aluminum, and the material of the conductive layer 15 can be designed according to actual needs.

[0035] In this embodiment, the coating area 12 and the blank area 11 are arranged on the surface of the conductive layer 15, and the thickness of the defluorination layer 13 is 10nm to 2000nm. The thickness of the defluorination layer 13 can be designed to be any value in the range of 10nm, 30nm, 30nm, 200nm, 500nm, 1000nm, 1500nm, 1700nm, 2000nm, etc. In actual design, the thickness of the defluorination layer 13 can be designed according to actual needs.

[0036] like Figure 4 As shown, in an optional embodiment, the current collector body 1 further includes a support layer 14, a primer layer 16, and a transition layer 17. The primer layer 16 can be formed on the surface of the support layer 14 by magnetron sputtering coating or vacuum evaporation coating. The primer layer 16 is used to enhance the bonding force between the subsequent transition layer 17 and the support layer 14, and can also enhance the high temperature resistance of the metal layer of the current collector body 1, so that it will not be damaged by high temperature in subsequent processes. In addition, the transition layer 17 can be formed on the surface of the primer layer 16 by magnetron sputtering coating or vacuum evaporation coating, so that the square resistance of the surface of the current collector body 1 reaches a suitable value, which is conducive to subsequent coating.

[0037] In an optional embodiment, the material of the support layer 14 can be HIPS, PCTFE, PMMA, FEP, PFA, PTFE, PMP, HDPE, LDPE, LLDPE, PMP, PP, UHMWPE, PS, HIPS, ABS, EVA, SAN, ECTFE, ETFE, PPE, PE, SMA, MABS, PPE, PBT, PSU, CP, LCP, PA6-10, PBT, PEI, PET, PETG, POM, etc. Of course, in actual design, the material of the support layer 14 can be designed according to actual needs. In addition, the material of the base layer 16 is copper, nickel, aluminum, silicon nitride, silicon carbide, aluminum oxide or polyethylene glycol. Of course, in actual design, the material of the base layer 16 can be designed according to actual needs.

[0038] In an optional embodiment, the coating area 12 and the blank area 11 are arranged on the surface of the transition layer 17, and the thickness of the defluorination layer 13 is 10nm to 2000nm. The thickness of the defluorination layer 13 can be designed to be any value in the range of 10nm, 30nm, 30nm, 200nm, 500nm, 1000nm, 1500nm, 1700nm, 2000nm, etc. In actual design, the thickness of the defluorination layer 13 can be designed according to actual needs.

[0039] like Figure 5As shown, in another optional embodiment, the current collector body 1 also includes a support layer 14, a primer layer 16, a transition layer 17, and a thickening layer 18. The primer layer 16 can be formed on the surface of the support layer 14 by magnetron sputtering coating or vacuum evaporation coating. The primer layer 16 is used to enhance the bonding force between the subsequent transition layer 17 and the support layer 14, and can also enhance the high temperature resistance of the metal layer of the current collector body 1, so that it will not be damaged by high temperature in subsequent processes. In addition, the transition layer 17 can be formed on the surface of the primer layer 16 by magnetron sputtering coating or vacuum evaporation coating, so that the square resistance of the surface of the current collector body 1 reaches a suitable value, which is conducive to subsequent coating. In addition, the thickening layer 18 is formed on the surface of the transition layer 17 by electroplating. The characteristic of electroplating is that a thicker metal layer can be formed at one time, which reduces the production cost, and the thickening layer 18 can increase the thickness of the conductive layer 15 of the current collector body 1, so that the current collector body 1 meets the square resistance requirements.

[0040] In another optional embodiment, the thickness of the support layer 14 is 3um to 8um. The thickness of the support layer 14 can be designed to be any value in the range of 3um, 4um, 5um, 6um, 7um, 8um, etc. In actual design, the thickness of the support layer 14 can be designed according to actual needs.

[0041] In another optional embodiment, the thickness of the base layer 16 is 10nm to 50nm. The thickness of the base layer 16 can be designed to be any value in the range of 10nm, 12nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 48nm, 50nm, etc. In actual design, the thickness of the base layer 16 can be designed according to actual needs.

[0042] In another optional embodiment, the thickness of the transition layer 17 is 100nm to 500nm. The thickness of the transition layer 17 can be designed to be any value in the range of 100nm, 120nm, 150nm, 200nm, 250nm, 300nm, 320nm, 350nm, 400nm, 450nm, 470nm, 500nm, etc. In actual design, the thickness of the transition layer 17 can be designed according to actual needs.

[0043] In another optional embodiment, the thickness of the thickening layer 18 is 500nm to 1000nm. The thickness of the thickening layer 18 can be designed to be any value in the range of 500nm, 520nm, 550nm, 600nm, 650nm, 700nm, 750nm, 770nm, 800nm, 850nm, 900nm, 920nm, 970nm, 1000nm, etc. In actual design, the thickness of the thickening layer 18 can be designed according to actual needs.

[0044] In another optional embodiment, the coating area 12 and the blank area 11 are arranged on the surface of the thickened layer 18, and the thickness of the defluorination layer 13 is 10nm to 2000nm. The thickness of the defluorination layer 13 can be designed to be any value in the range of 10nm, 30nm, 30nm, 200nm, 500nm, 1000nm, 1500nm, 1700nm, 2000nm, etc. In actual design, the thickness of the defluorination layer 13 can be designed according to actual needs.

[0045] like Figure 6 As shown, in another optional embodiment, the support layer 14 includes a coating area 141 and a white edge area 142. The coating area 141 is used to coat the base layer 16, and the white edge area 142 is not plated with metal, so that the roll-up is smooth without warping or burning. In addition, the width of the white edge area 142 is 1 cm to 3 cm, and the width of the white edge area 142 can be designed to be any value in the range of 1 cm, 1.1 cm, 1.3 cm, 1.5 cm, 1.7 cm, 2 cm, 2.2 cm, 2.5 cm, 2.7 cm, 3 cm, etc. In actual design, the width of the white edge area 142 can be designed according to actual needs.

[0046] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the claims attached to the utility model.

[0047] The above is an exemplary description of the utility model patent in conjunction with the accompanying drawings. It is obvious that the implementation of the utility model patent is not limited to the above-mentioned method. As long as various improvements are made by adopting the method concept and technical solution of the utility model patent, or the concept and technical solution of the utility model patent are directly applied to other occasions without improvement, they are all within the protection scope of the utility model.

Claims

1. A defluorinated composite current collector, characterized in that: The invention comprises a current collector body, wherein the current collector body comprises a coating area and a blank area, an active material is arranged on the coating area, and a defluorination layer is arranged between the active material and the coating area.

2. The defluorinated composite current collector according to claim 1, characterized in that: The thickness of the defluorination layer is 10nm~2000nm.

3. The defluorinated composite current collector according to claim 1, characterized in that: The current collector body further includes a support layer and a conductive layer disposed on the surface of the support layer, and the coating area and the blank area are disposed on the surface of the conductive layer.

4. The defluorinated composite current collector according to claim 1, characterized in that: The current collector body further includes a support layer and a primer layer disposed on the surface of the support layer. A transition layer is disposed on the surface of the primer layer. The coating area and the blank area are disposed on the surface of the transition layer.

5. The defluorinated composite current collector according to claim 1, characterized in that: The current collector body also includes a support layer, a base layer arranged on the surface of the support layer, a transition layer is arranged on the surface of the base layer, a thickening layer is arranged on the surface of the transition layer, and the coating area and the blank area are arranged on the surface of the thickening layer.

6. The defluorinated composite current collector according to any one of claims 3, 4 or 5, characterized in that: The thickness of the support layer is 3um~8um.

7. The defluorinated composite current collector according to claim 4 or 5, characterized in that: The thickness of the primer layer is 10nm-50nm.

8. The defluorinated composite current collector according to claim 4 or 5, characterized in that: The thickness of the transition layer is 100nm~500nm.

9. The defluorinated composite current collector according to any one of claims 3, 4 or 5, characterized in that: The support layer is also provided with a white edge area to ensure smooth rolling.

10. The defluorinated composite current collector according to claim 9, characterized in that: The width of the white edge area is 1 cm to 3 cm.