METHOD FOR PRODUCE A DIMENSIONALLY CORRECT CONCRETE WORK AND DIMENSIONALLY CORRECT CONCRETE WORKS
Patent Information
- Application Number
- DE502016016802
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-05-18
- Filing Date
- 2016-05-18
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Concrete workpieces exhibit low dimensional stability and high geometric distortions due to hydration and thermal expansion, leading to defects and reduced strength, which limits their accuracy and usability in applications requiring precise geometry.
A method involving a predetermined temperature distribution within the mold during concrete hydration, ensuring complete surface contact and controlled heat management to prevent geometric distortions, combined with a controlled filling speed to prevent air pockets and maintain fiber alignment, results in a compressive strength of 10 MPa before demolding and dimensional tolerances of +/- 25 micrometers per meter.
This approach produces dimensionally stable concrete workpieces with high precision, enabling their use in complex geometries and applications like solar collectors, with improved strength and accuracy, allowing for the creation of series parts with tight tolerances.
Description
[0001] The invention relates to a method for producing a dimensionally stable concrete workpiece according to the preamble of claim 1, as well as concrete workpieces according to the preamble of claims 11 and 13.
[0002] Concrete is widely used, but also has unfavorable properties, such as low tensile strength, which are the subject of intensive development and are often improved in larger or smaller steps.
[0003] However, it is generally accepted that concrete workpieces are not dimensionally stable. In construction, it is normal to use concrete workpieces with a tolerance of around one millimeter per meter of length (a deviation of + / - 0.5 mm from the nominal length). This is also the case with window sills, for example, where any gaps are simply covered with metal cladding.
[0004] The progressive improvement in the strength properties of concrete opens up a broader range of applications, with the geometry of the concrete workpieces increasingly being adapted to the intended load, i.e., becoming more complex to utilize the improved strength properties. However, the low precision of the corresponding concrete workpieces is a disadvantage. US Pat. No. 4,234,534 discloses a method for producing concrete in molds with a predetermined temperature distribution, achieving tolerances in the range of 2.9 × 10 -4 < m per meter of workpiece dimension, although even smaller tolerances are desirable.
[0005] Accordingly, it is the object of the present invention to provide a method for producing dimensionally stable concrete workpieces or dimensionally stable concrete workpieces.
[0006] The object is achieved by a method having the characterizing features of claim 1 and by concrete workpieces having the characterizing features according to claims 11 and 13.
[0007] By maintaining a predetermined temperature distribution in the mold walls during the hydration of the fresh concrete, the hydration of the fresh concrete can be controlled. This can be accelerated by the heat supplied to the fresh concrete and then generated by the heat itself, but can also be slowed by heat removed from the fresh concrete. This results in volume changes and hydration-induced structural changes caused by hydration and thermal expansion being manageable. Thus, the geometric distortions constantly generated in the hydrating concrete and the associated stresses remain below the threshold above which defects develop in the hydrating concrete. These defects cannot be healed until complete hydration, reducing the dimensional stability and strength of the concrete workpiece.By completely filling a sealed mold with fresh concrete, the entire surface of the fresh concrete is in contact with the mold, allowing hydration to be controlled throughout the entire body of the concrete workpiece. A compressive strength of 10 MPa prior to demolding ensures that the concrete workpiece is not mechanically damaged during demolding, preventing previously avoided defects from occurring during demolding. Finally, limiting the diameter of the largest grain size prevents heat transfer through the hydrating fresh concrete, which would otherwise lead to a chaotic temperature distribution, which, during hydration, would cause geometric distortions, corresponding stresses, and thus disrupt dimensional stability.
[0008] If such geometric distortions can be avoided during hydration, a dimensionally accurate workpiece is produced that meets high standards and is also not reduced in strength. In particular, the invention also allows the production of dimensionally accurate series parts with a tolerance of only + / - 25 micrometers per meter of workpiece length within a predetermined geometry.
[0009] At this point, it should be noted that experimental setups have been developed for investigating the developing elastic modulus in hydrating concrete. These setups maintain the hydrating concrete at a constant temperature. However, the modulus of elasticity is continuously measured through mechanical action on the concrete. This does not leave the concrete undisturbed, but rather leads to geometric distortions of the concrete. The constant temperature facilitates the evaluation of the hydration process detected via the elastic modulus, as the equivalence calculation for the passage of time, familiar to experts, is then no longer necessary, as hydration progresses at different rates due to the inherent heat generated (Claude Boulay et al.: How to monitor the modulus of elasticity of concrete, automatically since the earliest age?, Materials and Structures (2014) 47:141-155).
[0010] Because the vessel for pouring fresh concrete is designed to vary the flow rate of the emerging fresh concrete, the filling rate of the mold into which the fresh concrete is poured can, for example, be kept constant across its cross-sectional changes, or the cross-section can be adjusted. This prevents the filling rate from becoming so high in cross-sectional constrictions that, for example, air-filled pockets remain, which in turn prevent contact between the temperature-controlled walls of the mold and the fresh concrete. In other words, in the case of air-filled pockets, the mold is not completely filled with fresh concrete, so that in addition to the faulty contour of the workpiece, hydration cannot be controlled, at least locally, in the area of the pockets, and harmful geometric distortions can arise in the hydrating concrete.Further advantageous effects of a constant or adjusted filling speed, for example in fiber-reinforced concrete, are that the (usually aleatoric) orientation of the fibers desired for the strength of the concrete is not disturbed, as can be the case when turbulence occurs in cross-sectional constrictions due to excessively high filling speed.
[0011] Because a concrete workpiece according to the invention has a tolerance of 50 micrometers per meter (deviation of + / - 25 micrometers per meter of workpiece length from the nominal dimension), it can be used in areas that could not previously be covered by concrete workpieces. Both in the sense of individual parts and in series production, all of which are precisely designed and enable corresponding designs. This includes (among countless other applications) use in the field of concentrators for solar collectors, for example for the production of a facet in a dish collector. The facet consists of a carrier with a parabolic surface and a reflective layer lying directly or indirectly on the parabolic surface, with the reflective layer taking on the contour of the parabolic surface of the carrier.According to the invention, a burning range of 10 mrad or less can be generated, down to 1 mrad or even less, which is sufficient for high concentrations of sunlight.
[0012] Formation as a parabolic support for a reflective layer for a solar collector as described below.
[0013] The invention is described in more detail below with reference to the figures. Figure 1 shows a dish collector according to the prior art with a number of facets which concentrate radiation onto an absorber, Figure 2a shows an embodiment of a concrete support produced according to the invention for a facet of a collector in a view from above, Figure 2b shows the concrete support of Figur 2a from the side and from below, Figure 3a a two-part, fully closed mold for the production of the concrete beam of Figur 2a , Figure 3bthe shape of Figur 3ain closed state in a view from above of the cooling module arranged on the upper mold half, and Figure 4 shows a vessel according to the invention for pouring fresh concrete into a mold
[0014] Figur 1 shows a dish collector 1 according to the prior art, which is designed according to WO 2011 / 072410. A paraboloidal concentrator 2 is composed of individual facets 3, each of which reflects sunlight onto an absorber 4 arranged at the focal point of the paraboloidal concentrator 2. Thus, the facets 3 themselves are not paraboloids; they form a local region of the paraboloid of the concentrator 2, whereby the geometry of the reflecting surface of the facets 3 differs depending on their distance from the vertex 5 of the paraboloidal concentrator 2. Such facets 3 are referred to as paraboloidal here; as mentioned, they collectively form a paraboloid.
[0015] The reflective surface of the facets 3 is formed by a pressure-loaded, aluminum-coated, flexible membrane arranged in a pressure chamber. Due to the oval outline of the facet 3 and its pressure load, this membrane replicates the local curvature of the paraboloid 2. Each facet 3 is thus part of the paraboloid concentrator 2 and thus part of a paraboloid, at whose focal point the absorber 4 is located. Such an arrangement allows sunlight concentrations of over 1000, up to 3000 or more, to be achieved.
[0016] Figur 2a shows a concrete support 10 according to the invention, which is disc-shaped and has a circumference 11, for a reflective layer, which has been omitted to reduce the load on the figure, wherein the concrete support 10 and the reflective layer form a facet for a dish collector according to Figur 1Such a reflective layer can be formed by a reflective foil, such as an aluminum-coated PET foil, or by another membrane, such as a thin aluminum sheet. The reflective layer is placed directly onto the paraboloidal surface 12 of the concrete support 10 and, during operation, is pressed against the surface 12, for example, by the ambient pressure, since the space between the surface 11 and the reflective layer is evacuated via a vacuum channel 13. In a specific embodiment, the major axis of the oval concrete support 10 measures 1379 mm, the minor axis 1196 mm, the location of the absorber 4 ( Figur 1 ) is located at a distance of several meters from the mouth of the vacuum channel 11.
[0017] It turns out that the paraboloidal surface 12 has high precision, ie low tolerances, otherwise the concentrations required above would not be achievable.
[0018] Figur 2b shows the concrete beam 10 of Figur 2a Once from the side and then from below, where the view from below shows the delicate rib structure with ribs 15 on the underside 16, as well as support pins 17 for arranging the concrete support 10 in a dish collector frame. The perimeter 11 is formed by the outer side of a circumferential rib 15'.
[0019] Figur 2c shows an enlarged section of the concrete beam 10, again from below, to illustrate the rib structure and the associated dimensional tolerances, in particular the dimensions of the surface 12 ( Figur 2a): The dimensional tolerances of the concrete beam produced by the method according to the invention are, as mentioned, 0.05 mm per m, which, with a height h of the ribs 15 on the outside of the concrete beam 10 of 40 mm here, results in a deviation of the surface 11 from its nominal dimension of only + / - 0.001 mm. In other words, after demoulding, the concrete beam 10, without any further processing, has a highly precise surface 12, the accuracy of which enables a geometric focal spot for reflected radiation of up to 1 mrad. "Geometric focal spot" because the concrete surface 12 itself is not sufficiently reflective and therefore must be covered with a reflective layer, see the description above.However, the surface 12 gives the reflective layer its contour - so that the reflective layer achieves a focal spot during operation which essentially corresponds to the geometric focal spot of the surface 12 with a diameter of up to only 1 mrad.
[0020] This results in a simple, robust and cost-effective design and manufacture for a component that is complex due to its difficult paraboloidal shape and that is difficult to manufacture using the state of the art and at comparatively high costs.
[0021] The one in the Figuren 2a bis 2cThe concrete support 10 shown is only one example of a concrete workpiece that can be produced using the method according to the invention. Another (among many) exemplary embodiments are concrete foundations for machine tools or machining centers that operate with high precision in the micrometer range, whereby, depending on the machining operation, considerable forces act on the tool or workpiece; moreover, the workpieces themselves can weigh several tons. Stable foundations with a high-precision surface are required here, since the machine frames must be precisely positioned in the micrometer range in order to achieve the required accuracy in machining the workpieces.
[0022] Figur 3a shows a mold 20 for carrying out the method according to the invention, which has an upper half 21 for shaping the surface 12 (for the application of the reflective layer, see Figur 2a ) and a lower half 22 for the rib structure (see Figur 2b). The wall surface 25 for the formation of the surface 12 of the concrete workpiece 10 ( Figur 2a ) is dimensionally stable, ie it has a tolerance that is equal to or preferably smaller than the tolerance achievable in the finished concrete beam 10 by the method according to the invention. The wall surfaces of the lower half 22 for the formation of the rib structure ( Figur 2b , c ) may have a larger tolerance, since the dimensional stability of the ribs 15 as such is not important for the intended use of the concrete beam 10. In other words, the shape 20 is dimensionally stable in a predetermined geometry and, according to the invention, may or may not also be dimensionally stable in the other areas.
[0023] Visible are a supply channel 23 for the fresh concrete and an outlet channel 24 for the air escaping during pouring and for the fresh concrete emerging after the mold has been completely filled. The mold 20 is fully sealed, meaning the concrete workpiece to be poured is enclosed on all sides, its entire surface in contact with the walls of the mold, with no access to ambient air.
[0024] Figur 3b shows the closed, ready-to-use mold 20, which is mounted on a metal frame 26, the lower part of which rests on the floor, however, being cut off to relieve the weight on the figure. The two mold halves 21, 22 are clamped between metal supports 27, and the mold 20 is closed. The dashed line marks a rotation axis 28 around which the mold can be tilted, allowing it to be tilted from the horizontal position shown to a vertical position.
[0025] The upper mold half 21 has an annular recess 29 into which a counter-shaped, annular temperature module 30 is inserted, which in the embodiment shown extends essentially over the dimensions of the concrete beam 10 to be cast ( Figuren 2a bis 2c ) and has an inlet 31 and an outlet 32 for a heat exchange medium, here water. Inlet 31 and outlet 32 are connected via a heat exchange channel 33 arranged in a ring in the temperature module 30, so that the upper mold half can be kept at a predetermined temperature, at least in the area of the concrete beam 10 to be cast, via water circulating in the heat exchange channel 33, either along a temperature profile or at a predetermined constant temperature. The temperature module 30 is drawn transparently to such an extent that the course of the heat exchange channel 33 is visible.
[0026] What is not apparent in the figure is that the lower mold half 22 is of course also provided with a temperature module, which corresponds in its design to the temperature module 30, so that both mold halves 21, 22 can be heated or cooled equally by circulating water.
[0027] To reduce the load on the figure, a cooling and / or heating unit for the circulating heat exchange medium connected to the inlet 31 and the outlet 32 has been omitted. This can be of conventional construction and will be designed by the person skilled in the art according to the specific case. Therefore, in the case of a heating unit, the mold 20 has a heating arrangement for the contact surfaces of the fresh concrete poured into it, which is preferably designed as a liquid heating system, particularly preferably as a water heating system.
[0028] It follows that the mold 20 can be cooled and also heated via the temperature module 30, depending on the temperature of the circulating heat exchange medium, the temperature module 30 can therefore also act as a heating arrangement,
[0029] The mold 20 is preferably made of aluminum, but can particularly preferably also be made of an aluminum-silicon alloy having substantially the same thermal expansion coefficient α T as the concrete to be poured into it. A temperature profile can then be maintained for the hydration of the concrete without thermally induced volume differences arising between the concrete and the mold, which would undesirably impair the contact of the concrete with the walls of the mold during any phase of hydration.
[0030] Since the thermal expansion coefficient α T of the concrete to be poured varies depending on its composition, the specialist can adjust the coefficients α T of the concrete and the mold in a specific case. A common range for α T for fresh concrete is between 6 × 10 -6< / K and 20 × 10 -6< / K , preferably between 6 × 10 -6< / K and 18 × 10 -6< / K , particularly preferred for fiber concretes between 6 × 10 -6< / K and 14 × 10 -6 K . Accordingly, it is advisable to provide a mould for the hydration of fresh concrete poured into it with a thermal expansion coefficient α T in the above-mentioned ranges.
[0031] Figur 4 shows a vessel 40 for pouring fresh concrete into a mold 41 for producing an object that, in the embodiment shown, has a lens-shaped cross-section. The mold 41 changes its cross-section accordingly and is preferably constructed analogously to the mold 20 ( Figuren 3aand 3b ), and is here placed in a vertical position, in which it is filled with fresh concrete 42 via a discharge channel of the boiler 40, which is designed here as a line 43. Via a symbolically represented support 44, the form 41 is analogous to the form 20 ( Figur 3b ) is stored. The vessel 41 contains at least one batch of fresh concrete 42, namely as much as is necessary to completely fill the mold 41. To relieve the figure, a temperature module 30 ( Figur 3b ) or a similar arrangement for controlling the temperature is omitted.
[0032] The vessel 40 is mounted on the symbolically represented supports 45 and has an overpressure zone 46 in which pressure can be exerted on the surface 48 of the fresh concrete 42, preferably via air pressure generated by a compressor 47, whereby the fresh concrete 42 is injected through the line 43 via its inlet 49 into the mold 41, whereby the air contained in the mold 41 and displaced by the fresh concrete 42 continuously escapes through the outlet 50. It is advantageous to further provide the compressor 47 with a programmable controller 51, by means of which the air pressure in the overpressure zone 47 can be continuously varied in a predetermined manner, with the result that the volume flow of the fresh concrete flowing through the line 43 also changes in a predetermined manner. This allows the filling speed v F (ie the speed at which the level P of the fresh concrete in the mold 41 rises) to be adjusted to its cross-sectional changes, orto those of the cavity 52 to be filled. Preferably, the filling speed v F is kept constant across the cross-sectional changes of the mold 41.
[0033] In summary, a boiler is advantageous which is designed to change the volume flow of a batch of fresh concrete in a predetermined manner during the dispensing of the batch, wherein it preferably comprises a fresh concrete container connected to a dispensing channel and an arrangement for generating overpressure in the fresh concrete container, preferably by means of air, and wherein the arrangement is designed to continuously change the overpressure during the dispensing of the batch of fresh concrete, such that the volume flow of the dispensed concrete changes according to a current target value. For the determination of the current target value for the volume flow, see below. Fig 5a bis 5c .
[0034] The diagram 55 shown next to the mold 41 in the figure shows on the vertical axis the height h of the mold 41 and on the horizontal axis the flow velocity v FB of the fresh concrete 42 flowing through the pipe 43. The curve 56 shows qualitatively the flow velocity v FB for the case of a constant filling velocity v F .
[0035] It can be seen that when the fresh concrete 42 is at a level P in the inlet 47 (height h E ), the flow velocity v FB is minimal and has a value v min . Once the level P has reached the cavity 52, ie the cross-section of the mold widens, the flow velocity v FB must continuously increase so that the filling velocity v F remains constant (has a general value vx at the height h X ), with the maximum value v max being reached at the height h D (the maximum wide cross-section of the mold 41).
[0036] Thereafter, the flow velocity v FB continuously decreases in accordance with the decreasing cross-section until it again reaches the minimum value v min at outlet 48 (height h A ), with which a portion of outlet 48 continues to be filled to ensure that mold 41 is completely filled. Thereafter (at height h S ), the flow velocity v FB is stopped because the batch of concrete has been filled into mold 41.
[0037] The boiler is thus designed to change the volume flow of a batch of fresh concrete in a predetermined manner during the dispensing process, wherein with the aid of such a boiler, the fresh concrete is preferably injected into the mold at a different flow rate v FB in such a way that the mold fills with a predetermined, preferably substantially constant flow rate v FB via cross-sectional changes in the mold, wherein further preferably the injection of the fresh concrete is carried out by overpressure and the flow rate is controlled by a change in the overpressure.
[0038] In Figur 3athe rib structure of the lower mold half 22 is visible. If the level P of fresh concrete injected into the vertically aligned mold 20 rises from the inlet 23 to the outlet 24, the cross-section of the mold 20 changes continuously, which requires a constant filling speed v F and a continuous adjustment of the flow velocity v FB . The cavity of the mold 20 can be divided into horizontal cross-sections and the filling speed v F can be determined according to the area of the cross-sections. If, for example, 500 or 1000 cross-sections are provided, a finely stepped change in the cross-section and thus in the flow velocity v FB results. This allows the control system 51 ( Figur 4) accordingly and the pressure in the overpressure zone 46 is controlled by a PID controller such that the real flow velocity v FB leads to a substantially constant real filling velocity v F of the mold 20. In the specific case, the person skilled in the art can easily determine the number of cross sections and the suitable controller model based on the cavity of the mold to be used.
[0039] Figuren 5a bis 5c show a section of a mold 60 with a cavity 61 for a rib to be cast during the filling of the mold 60 with fresh concrete 62. The cavity 61 is limited at its upper end by a rounded edge 63. The surface 64 of the fresh concrete 62 rises upwards in the direction of the arrow and falls towards the wall of the mold 60 due to the comparatively high viscosity of the fresh concrete.
[0040] Figur 5ashows the moment at which the level of the fresh concrete 62 has reached the location of the cavity 61 and fresh concrete 62 penetrates into it. With further rising water level and too high filling speed, the situation arises according to Figur 5b in which the surface 64 touches the rounded edge 63 of the mold and thus encloses an air bubble 65 in the background of the cavity 61. Figur 5c shows the situation a little later. The air pocket 65 is slightly compressed, but definitely prevents the cavity 61 from being completely filled with fresh concrete 62.
[0041] It follows that if the filling speed is too high, one flank of the rib of the concrete workpiece to be cast cannot rest against the wall of the mold 60 for hydration, resulting in a defect in the workpiece regarding its geometry and dimensional accuracy. If the concrete level rises so slowly that the cavity 61 can be completely filled with fresh concrete 62 before its surface 64 closes it in contact with the rounded edge 63, the casting defect does not occur. It follows that, in connection with the geometric structure of the mold, there is a maximum permissible filling speed v F . Depending on this geometric structure, the maximum filling speed v F is the same or different for different areas of the mold. The skilled person can easily determine the speed profile of the filling speed v F (constant or predetermined variable) based on a specific mold and the fresh concrete to be poured.The advantage of adjusting the filling speed v F is that the mold can be filled as quickly as possible with regard to a specific concrete mix, which supports an efficient production process.
[0042] According to the invention, a dimensionally stable concrete workpiece such as a concrete beam 10 ( Figuren 2a bis 2c ) for a reflective layer, ▪ by filling a fully closed, dimensionally stable form with fresh concrete in a predetermined geometry, for example form 20 or 41 according to the Figuren 3b or 4The fresh concrete can, for example, be conventional fiber concrete, as selected by a specialist depending on the intended use. As mentioned above, the fully sealed mold ensures that the fresh concrete is temperature-controlled over its entire surface and that no moisture exchange with the environment can occur, which would disrupt the desired, controlled hydration. ▪ During the subsequent, undisturbed hydration, a predetermined temperature distribution is maintained on the walls of the mold surrounding the hydrating concrete. This results in a predetermined temperature distribution inside the hydrating concrete body, which prevents permanent geometric distortions. In addition to this temperature control, the undisturbed hydration also prevents other geometric distortions, such as those caused by mechanical factors.▪ Finally, the concrete workpiece is demolded at a compressive strength of more than 10 MPa, i.e., at a compressive strength sufficient for sufficient stability during careful demolding by the specialist, thus avoiding geometric distortions. ▪ The largest grain of the fresh concrete has a diameter of less than 20% of the smallest dimension of the mold. The thermal conductivity of the grain in the concrete differs from that of the cement, resulting in zones of inhomogeneous heat distribution around the aggregates, which can disrupt the desired predetermined temperature distribution in the hydrating concrete workpiece.This effect depends on the local dimensions of the concrete workpiece to be produced: Tests carried out by the applicant have shown that undesirable geometric distortions, which reduce the dimensional stability of the concrete workpiece, do not occur during hydration if the diameter of the maximum grain does not reach 20% of the smallest dimension of the mold.
[0043] According to the invention, the temperature distribution of the mold walls is adjusted such that the temperature distribution in the hydrating concrete from the start of hydration to demolding lies within a permissible interval of 15 °C, preferably 10 °C, particularly preferably 5 °C. Fundamentally, when controlling the temperature of the hydrating concrete through the mold walls, a temperature gradient in the concrete is unavoidable. A person skilled in the art can easily determine by testing a specific concrete mix which temperature gradient is currently permissible or not. Tests by the applicant have shown that a dimensional accuracy of + / - 25 micrometers per meter of dimension of the concrete workpiece can be easily achieved if the highest and lowest temperatures in the hydrating concrete at any one time do not differ by more than 5 °C, i.e. the temperature distribution in the concrete remains within a permissible interval of 5 °C.For a lower dimensional accuracy of + / - 50 micrometers per meter, depending on the concrete mix used, a temperature interval of 10 0< C or 15 0< C may be sufficient, which can easily be determined by the expert through simple tests.
[0044] For rapid production of concrete workpieces, the invention allows the hydrating concrete workpiece to be moved along a temperature profile, i.e., its temperature can be increased, for example, to accelerate hydration. This temperature profile is naturally generated by the temperature of the contact surfaces between the mold walls and the concrete. Preferably, the above-mentioned permissible temperature intervals are maintained while moving through the temperature profile. Particularly preferred for efficient production is increasing the temperature in the concrete in such a way that the concrete heats up as quickly as possible, but its temperature distribution always remains within the permissible interval of 5°C < 10°C < 15°C < 1°C.Here, too, it is easy to determine by means of experiments what the fastest possible heating rate is for a particular concrete mixture, for example by equipping the mold with thermal sensors around which the concrete is poured.
[0045] Preferably, for example, for the production of concrete beams 10 ( Figuren 2a bis 2c ) the temperature profile provides for an increase in the temperature in the concrete from 25 °C to 45 °C within 2 hours, then maintaining this temperature and finally a reduction in the temperature from 45 °C to 25 °C again within 3 hours.
[0046] Of course, the skilled person can provide a shrinkage-compensated concrete mix; shrinkage-compensating additives are known in the art. This prevents irreversible geometric distortions from occurring in the dimensionally stable mold due to shrinkage during hydration. On the other hand, it is also in accordance with the invention to coordinate thermal expansion with shrinkage in a temperature profile: the temperature profile then provides for an increase in the temperature of the hydrating concrete such that its thermal expansion essentially compensates for the shrinkage. This implies that the mold has a lower thermal expansion coefficient α T than the concrete, and that the workpiece is then demolded at a high temperature and allowed to cool freely to avoid geometric distortions due to thermal shrinkage.In each specific case, the specialist can coordinate the material and geometry of the mold, the concrete mix and the temperature profile.
[0047] Regardless of the smallest dimension of the mold, a maximum grain with a diameter of less than 1 mm, particularly preferably less than 0.5 mm, is preferably used in order to achieve perfect dimensional stability, regardless of the concrete mix used, especially with temperature profiles used during hydration.
[0048] Instead of a form according to the Figure 3 and 4With a temperature module (or other suitable cooling or heating arrangement), a mold can also be used whose mass is more than three times, preferably more than four times, and particularly preferably more than five times the mass of the fresh concrete present when completely filled. This allows the mold to absorb the heat of the hydrating concrete without the need for active cooling during hydration, allowing it to be manufactured and operated easily and inexpensively.
[0049] Using the example of a concrete beam 10 ( Figuren 2a bis 2c) The method according to the invention is briefly described: After preparatory cleaning, a mold is heated to 25 °C, and at the same time the fresh concrete is prepared by mixing its components. The viscous mass of the fresh concrete contains air bubbles due to the mixing process, which are preferably removed from the concrete in a vacuum chamber. The residual pressure remaining in the vacuum chamber is preferably 150 mbar, particularly preferably 50 mbar. Here, too, the person skilled in the art can determine the duration of the vacuum treatment for the specific concrete mix. Air bubbles cause inhomogeneities in the temperature distribution of the hydrating concrete mix and hinder the desired, homogeneous structural transformation, which is why a bubble-free concrete mix is preferred for perfect dimensional stability of the concrete workpiece.
[0050] The bubble-reduced or bubble-free concrete mix is then injected into the mold, which, in the case of a geometry such as that of mold 20, has been placed in a vertical position for this purpose, facilitating proper filling. After the mold has been completely filled, it is preferably returned to a horizontal position, with the upper half 21 ( Figur 3a ) is located at the bottom, so that the dimensionally stable surface 25 ( Figur 3a ) is particularly well stressed by the concrete's own weight and thus reduces the probability of any defects on the surface 12 of the concrete beam ( Figur 2a ) is reduced again.
[0051] After 24 hours of hydration, the concrete beam is demolded, and the casting spigots resulting from the complete filling of the mold, which originate from the feed channel 23 and outlet channel 24 (Figure 3a), are mechanically removed. Finally, the concrete is immersed in water at 90 °C for 72 hours to ensure complete hydration.
[0052] In summary, according to the invention, a concrete workpiece has a concave surface that geometrically produces a firing range of 10 mrad or less, preferably 4 mrad or less, most preferably 1 mrad or less, wherein the surface is more preferably concavely curved in two dimensions. In other words, it is clear that not only two-dimensionally curved surfaces can be produced with the accuracy achievable according to the present invention—for every conceivable purpose.
[0053] If concrete workpieces are produced in series according to the invention, they are of the same shape, with the same geometric dimensions being within a tolerance of + / - 50 × 10 -6< , preferably + / - 25 × 10 -6< m per m of the dimension of the workpiece.
Claims
1. Method for producing a dimensionally stable concrete workpiece , characterized in that, for the production of the concrete workpiece, a fully closed mould with a predetermined geometry is completely filled with fresh concrete, during the subsequent and undisturbed hydration, a predetermined temperature distribution of the walls of the mould surrounding the hydrating concrete is maintained and the concrete workpiece is demoulded at a compressive strength of more than 10 MPa, whereby the largest grain of the fresh concrete having a diameter of less than 20% of the smallest dimension of the mould, characterized in that the temperature distribution of the walls of the mould is set in such a way that the temperature distribution in the hydrating concrete from the start of hydration to demoulding is within a permissible interval of 150 .
2. Method according to claim 1, wherein the permitted interval is 100 C, preferably 50 C.
3. Method according to claim 1, wherein the concrete is moved along a temperature profile during hydration, which is generated by a temperature change of the contact surfaces of the walls of the mold with the concrete.
4. Method according to claim 1, wherein the temperature profile includes an increase in the temperature in the concrete such that the concrete heats up as quickly as possible, but its temperature distribution always remains within the permitted interval.
5. Method according to claim 1, wherein the temperature profile provides for an increase in the temperature in the concrete from 25° C to 45° C within 2 hours, then maintaining this temperature and finally a reduction in the temperature from 45° C to 25° C again within 3 hours.
6. Method according to claim 1, wherein the temperature profile provides for an increase in the temperature of the hydrating concrete such that its thermal expansion substantially compensates for shrinkage7. Method according to claim 1, wherein the largest grain has a diameter of less than 1 mm + / - 3%, preferably less than 0.5 mm + / - 3%.
8. Method according to claim 1, wherein the mold has essentially the same coefficient of thermal expansion αT as the concrete to be poured into it.
9. Method according to claim 1, wherein the fresh concrete is placed under negative pressure, which is preferably 150 mbar, preferably 50 mbar, before pouring into the mold10. Method according to claim 1, wherein the fresh concrete is injected into the mold at different flow rates vFB such that the mold fills at a predetermined, preferably substantially constant filling rate vF via changes in the cross-section of the mold, wherein further preferably the injection of the fresh concrete is effected by overpressure and the flow rate vFB is controlled by a change in the overpressure.
11. Concrete workpiece manufactured according to the method of claim 1, having a concave surface which, without reworking after the manufacturing process, geometrically has a firing range of 10 mrad or less, preferably 4 mrad or less, most preferably 1 mrad or less12. Concrete workpiece according to claim 11, wherein the surface is further concavely curved in two dimensions.
13. Concrete workpieces manufactured according to the process of claim 1, characterized in that they are of identical shape and, without reworking after the manufacturing process, each have identical geometric dimensions within a tolerance of + / - 50 × 10-6 m per m of the dimension of the workpiece.
14. Concrete work pieces according to claim 13, wherein identical geometric dimensions are within a tolerance of + / - 25 × 10-6 m per m of the dimension of the workpiece.