METHOD FOR WELDING POROUS MEMBRANES AND PRODUCT
Patent Information
- Application Number
- DE502018015216
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-09-01
- Filing Date
- 2018-08-30
- Publication Date
- 2024-11-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for connecting breathable and waterproof materials, such as those used in clothing and footwear, often require sewing, which compromises the water resistance of the functional layer, and alternative methods like flat bonding can lead to loss of breathability and detachment issues over time.
A method involving the welding of porous membranes made from thermoplastic elastomers like polyurethane at temperatures between 100 to 250 °C to create a welded composite with a weld seam, maintaining the breathability and water resistance of the materials without the need for stitches.
The welded composite retains the same high water vapor permeability and liquid inlet pressure as the unwelded membranes, ensuring continued breathability and water resistance, even in the weld seam area, and can be used in various applications like clothing, shoes, and protective gear.
Description
[0001] The present invention relates to a method for welding porous membranes, comprising providing a first porous membrane and a second porous membrane; at least partially overlaying the first and second porous membranes to obtain an at least partially overlay region; and welding the first and second porous membranes at least in part of the overlay region at a temperature in the range of 100 to 250 °C to obtain an at least partially welded composite of the first and second porous membranes, wherein the material of the first and second porous membranes comprises a thermoplastic elastomer selected from the group consisting of polyurethane, polyester, polyetherester, polyesterester, polyamide, polyetheramide, polystyrene, ethylene-vinyl acetate elastomers, and mixtures of two or more of these elastomers,wherein the first and second porous membranes have pores with an average pore diameter of less than 2000 nm, determined by Hg porosimetry according to DIN 66133, wherein the first and second porous membranes are connected to one another in the form of a welded seam at least in part of the overlapping region. Furthermore, the invention relates to a welded composite of a first and second porous membrane, obtained or obtainable by the method according to the invention, wherein the first and second porous membranes are connected to one another in the form of a welded seam at least in part of the overlapping region, and to the use of a welded composite for producing an article selected from the group consisting of clothing, shoes, boots, protective suits, tents, and tarpaulins.
[0002] Waterproof, breathable clothing and shoes typically contain expanded polytetrafluoroethylene (ePTFE) (US 3,953,566, US 3,962,153) or polyester (Sympatex) (US 5,562,977) as a functional layer in the form of membranes or thin films. Non-porous coatings of thermoplastic polyurethane on textiles are also known (JP 5005276). Furthermore, EP 3100849 A1 relates to a method for producing a textile composite element in which a fabric layer (11) and a membrane (12) are stacked on top of one another and bonded together using pressure and heat. The fabric layer (11) consists of a thermoplastic elastomer or polymer, but this is in the form of interwoven threads. GB 2496244 A discloses a fabric laminate comprising a calendered hot air drawn layer 22 and at least one spunbonded layer 24, 26.WO 2016 / 061321 A1 discloses a laminating machine and a laminating process for laminating a membrane to a three-dimensional (3D) target surface of an article, such as a footwear article, glove, article of clothing, backpack, or other article. The membrane and the target surface can be arranged on the former, with a heat-activatable adhesive disposed between the membrane and the target surface. EP 2476324 A1 describes a sanitary article—waterproof, moisture-permeable underwear—in which two membranes are directly superimposed and welded together. A problem with this is that it is usually necessary to sew the functional layer to the carrier material, whereby the seams render the material of the functional layer water-permeable (US 2015 / 0230563).Therefore, water resistance must usually be achieved by subsequently sealing the seam with an overlying adhesive or sealing tape, with the closure being achieved by bonding or welding. Alternatives to sewing are currently unknown, and methods such as surface bonding have disadvantages. For example, the functional materials lose their breathability due to surface bonding, leading to detachment over time, etc.
[0003] The object of the invention was therefore to provide a method which allows the joining of breathable but waterproof materials without these materials losing these advantageous properties. In particular, a method should be provided which allows the joining of these materials without the use of seams, again while retaining the advantageous properties of the materials.
[0004] According to the invention, this object is achieved by a method for welding porous membranes, comprising: i) providing a first porous membrane and a second porous membrane; ii) at least partially overlaying the first and second porous membranes according to i) to obtain an at least partially overlay region; iii) welding the first and second porous membranes at least in a part of the overlay region according to ii) at a temperature in the range of 100 to 250 °C to obtain an at least partially welded composite of the first and second porous membranes, wherein the material of the first and second porous membranes comprises a thermoplastic elastomer selected from the group consisting of polyurethane, polyester, polyetherester, polyesterester, polyamide, polyetheramide, polystyrene, ethylene vinyl acetate elastomer and mixtures of two or more of these elastomers, wherein the first and second porous membranes have pores with an average pore diameter of less than 2000 nm, determined by means of Hg porosimetry according to DIN 66133, and wherein the first and second porous membranes are connected to one another in the form of a weld seam at least in part of the overlay region.
[0005] According to DIN ISO 857-1 (formerly DIN 1910-1), welding is the permanent joining of components using heat or pressure (with or without filler metals). Depending on the welding process, the connection is made in a weld seam or weld point. The energy required for welding is always supplied externally. In the sense of the present invention, welding is understood to mean the permanent joining or the creation of a non-detachable connection between the first and second porous membranes. This means that, according to DIN ISO 527-3, in the area of the weld (weld seam), the weld seam has a breaking stress in the range of 0.2 to 10 MPa, preferably in the range of 0.5 to 5 MPa, more preferably in the range of 1 to 2 MPa, before separation of the first and second porous membranes occurs.The corresponding elongation at break of the porous membrane is in the range of 5 to 200%, more preferably in the range of 5 to 100%.
[0006] Surprisingly, a welded composite produced in this way has the same good water vapor permeability and the same high liquid entry pressure as the unwelded first porous membrane itself, especially in the direct area of the weld (weld seam).
[0007] A preferred embodiment therefore relates to a method for welding porous membranes to obtain an at least partially welded composite of first and second porous membrane having a weld seam, wherein the weld seam has a breaking stress in the range of 0.2 to 10 MPa, preferably in the range of 0.5 to 5 MPa, more preferably in the range of 1 to 2 MPa, and preferably the first porous membrane has an elongation at break in the range of 5 to 200%, preferably in the range of 5 to 100%. Welding according to iii)
[0008] According to iii) of the present method, the first and second porous membranes are welded together at least in part of the overlapping region according to ii) at a temperature in the range of 100 to 250°C, thereby obtaining an at least partially welded composite of the first and second porous membranes. The welding according to iii) preferably takes place for a period of time in the range of 0.1 second to 10 minutes, more preferably in the range of 0.5 seconds to 60 seconds, more preferably in the range of 1 to 10 seconds.
[0009] Welding according to iii) preferably takes place under an atmosphere selected from protective gas, in particular argon or nitrogen, air, or lean air, more preferably under air. Welding according to iii) preferably takes place at a pressure in the range of 1 to 10 bar, more preferably in the range of 2 to 8 bar, more preferably in the range of 3 to 5 bar. Welding according to iii) takes place at a temperature in the range of 100 to 300°C, preferably in the range of 150 to 250°C.
[0010] For welding, any welding equipment known to those skilled in the art that is suitable for welding porous membranes can be used. Examples include common film sealing devices, such as automatic or semi-automatic impulse sealers.
[0011] As mentioned above, a welded composite produced in this way exhibits the same good water vapor permeability and the same high liquid entry pressure as the unwelded first porous membrane itself, particularly in the direct area of the weld (weld seam). In the context of the present invention, the term "the same good water vapor permeability" means that the water vapor permeability of the at least partially welded composite obtained according to (iii) is in the range of 75 to 100%, preferably in the range of 80 to 100%, more preferably in the range of 90 to 100%, based on the water vapor permeability of the first porous membrane provided according to (i). This applies to the entire at least partially welded composite obtained according to (iii), and in particular in the area of the weld seam.In the context of the present invention, the expression "the same high liquid inlet pressure" means that the liquid inlet pressure of the at least partially welded composite obtained according to (iii) is in the range of 75 to 100%, preferably in the range of 80 to 100%, more preferably in the range of 90 to 100%, based on the liquid inlet pressure of the first porous membrane provided according to (i). This applies to the entire at least partially welded composite obtained according to (iii), and in particular in the region of the weld seam. Porous membrane
[0012] According to i), a first and a second porous membrane are provided. The glass transition temperature Tg of the first porous membrane is preferably in the range of -40 to 120°C.
[0013] The first porous membrane preferably has an average thickness in the range of 5 to 150 µm, more preferably in the range of 50 to 100 µm, more preferably in the range of 70 to 90 µm.
[0014] A preferred embodiment therefore relates to a method for welding porous membranes comprising: i) providing a first porous membrane and a second porous membrane; ii) at least partially overlaying the first and second porous membranes according to i) to obtain an at least partially overlay region; iii) welding the first and second porous membranes at least in a part of the overlay region according to ii) at a temperature in the range of 100 to 250°C, preferably in the range of 150 to 250°C, to obtain an at least partially welded composite of the first and second porous membranes; wherein the first porous membrane has an average thickness in the range of 5 to 150 µm, more preferably in the range of 50 to 100 µm, more preferably in the range of 70 to 90 µm.
[0015] The first porous membrane has pores with an average pore diameter of less than 2000 nm, preferably in the range of 0.001 µm to 0.8 µm, determined by Hg porosimetry according to DIN 66133.
[0016] A preferred embodiment therefore relates to a method for welding porous membranes comprising: iii) welding the first and second porous membranes together at least in part of the overlapping region according to ii) at a temperature in the range of 150 to 250°C, to obtain an at least partially welded composite of the first and second porous membranes; wherein the first porous membrane has pores with an average pore diameter of less than 2000 nm, preferably in the range of 0.001 µm to 0.8 µm, determined by means of Hg porosimetry according to DIN 66133.
[0017] A particularly preferred embodiment relates to a method for welding porous membranes, wherein the first porous membrane has an average thickness in the range of 5 to 150 µm, more preferably in the range of 50 to 100 µm, more preferably in the range of 70 to 90 µm; and wherein the first porous membrane has pores with an average pore diameter of less than 2000 nm, preferably in the range of 0.001 µm to 0.8 µm, determined by means of Hg porosimetry according to DIN 66133.
[0018] The material of the first porous membrane comprises a thermoplastic elastomer selected from the group consisting of polyurethane, polyester, polyetherester, polyesterester, polyamide, polyetheramide, polystyrene, ethylene vinyl acetate elastomer and mixtures of two or more of these elastomers, preferably a polyurethane elastomer.
[0019] A preferred embodiment therefore relates to a method for welding porous membranes, wherein the material of the first porous membrane comprises a polyurethane elastomer.
[0020] A particularly preferred embodiment relates to a method for welding porous membranes, wherein the material of the first porous membrane comprises a polyurethane elastomer; wherein the first porous membrane has an average thickness in the range of 5 to 150 µm, more preferably in the range of 50 to 100 µm, more preferably in the range of 70 to 90 µm; and / or, preferably and, wherein the first porous membrane has pores with an average pore diameter of less than 2000 nm, preferably in the range of 0.001 µm to 0.8 µm, determined by means of Hg porosimetry according to DIN 66133.
[0021] Preferably, the material of the first porous membrane comprises a polyurethane elastomer based on the following components: 80 to 100% by weight of a mixture of at least one diol (D1) and at least one isocyanate (II), 0 to 20% by weight of at least one compound (C1) having at least two isocyanate-reactive groups; wherein the first porous membrane preferably has pores with an average pore diameter in the range of 0.001 µm to 0.8 µm, determined by Hg porosimetry according to DIN 66133.
[0022] In the context of the present invention, the sum of the weight percent of the components on which the polyurethane elastomer is based equals 100 weight percent. Additionally, the polyurethane elastomer may comprise other additives.
[0023] In the context of the present invention, a membrane is understood to be a thin, semipermeable structure capable of separating two liquids or molecular and / or ionic components or particles from one liquid. A membrane acts as a selective barrier, allowing some particles, substances, or chemicals to pass through while retaining others. For example, a membrane can be a reverse osmosis (RO) membrane, a forward osmosis (FO) membrane, a nanofiltration (NF) membrane, an ultrafiltration (UF) membrane, or a microfiltration (MF) membrane.
[0024] The pore size distribution within the first membrane is preferably not homogeneous; the first membrane preferably comprises pores with different pore sizes. The pore size distribution preferably has a gradient across the diameter of the first membrane, wherein a gradient in the context of the invention is understood to mean that pores on a first surface of the first membrane or close to this surface have an average pore diameter that differs from the average pore diameter of a second surface or close to this second surface.In the context of the present invention, it is possible, for example, for the pores on or near the first surface to have an average pore diameter in the range from 0.001 µm to 0.01 µm, determined by means of Hg porosimetry according to DIN 66133, and for the pores on or near the second surface to have an average pore diameter in the range from 0.1 µm to 0.8 µm, determined by means of Hg porosimetry according to DIN 66133. The degree of the gradient of the pore diameter within the first membrane can vary within wide ranges. The ratio of the pore diameter of pores on or near the first surface of the first membrane to that of the pores on or near the second surface can, for example, be in the range from 1:5 to 1:10,000, preferably in the range from 1:10 to 1:1,000, more preferably in the range from 1:100 to 1:500. According to a preferred embodiment, the pore size distribution of the first porous membrane has a gradient across the diameter of the membrane.
[0025] According to a preferred embodiment explained above, the material of the first porous membrane comprises a polyurethane elastomer (P1) based on the following components: 80 to 100% by weight of a mixture of at least one diol (D1) and at least one isocyanate (II), 0 to 20% by weight of at least one compound (C1) having at least two isocyanate-reactive groups; wherein the first porous membrane preferably has pores with an average pore diameter in the range of 0.001 µm to 0.8 µm, determined by Hg porosimetry according to DIN 66133.
[0026] The polyurethane therefore comprises no or only small amounts of the compound (C1) and consists largely of a mixture of diol (D1) and polyisocyanate (I1). The polyurethane (PU1) is preferably based on 85 to 100% by weight of a mixture of at least one diol (D1) and at least one polyisocyanate (I1), and 0 to 15% by weight of at least one compound (C1) having at least two isocyanate-reactive groups, more preferably 90 to 99.9% by weight of a mixture of at least one diol (D1) and at least one polyisocyanate (I1), and 0.1 to 10% by weight of at least one compound (C1) having at least two isocyanate-reactive groups.
[0027] The molar ratio of the at least one diol (D1) and the at least one polyisocyanate (II) is typically in the range from 95:100 to 100:95. Preferably, the molar ratio of the at least one diol (D1) and the at least one polyisocyanate (II) is in the range from 98:100 to 100:98, more preferably in the range from 99:100 to 100:99.
[0028] The first membrane may comprise further compounds, such as further polyurethanes. For example, the first membrane may comprise another polyurethane (PU2), which may be a thermoplastic polyurethane. According to a preferred embodiment, the first porous membrane therefore comprises another polyurethane (PU2) based on at least one polyol (P2), at least one diol (D2), and at least one polyisocyanate (I2).
[0029] Generally, the first membrane comprises at least 80% by weight of polyurethane (PU1), preferably at least 85% by weight of polyurethane (PU1), more preferably at least 90% by weight of polyurethane (PU1). For example, the first membrane may comprise polyurethane (PU1) in an amount ranging from 80 to 100% by weight, more preferably from 85 to 99% by weight, more preferably from 90 to 95% by weight.
[0030] The polyurethane (PU1) is based on 80 to 100% by weight of a mixture of at least one diol (D1) and at least one polyisocyanate (I1), as well as 0 to 20% by weight of at least one compound (C1) having at least two isocyanate-reactive groups.
[0031] The compound (C1) can be any compound having at least two isocyanate-reactive groups. Preferably, the isocyanate-reactive groups are hydroxyl or amino groups. The compound (C1) can be added to modify the properties of the polyurethane (PU1). Any compound can be used as long as it is suitable for producing a polyurethane (PU1) with the mixture of the at least one diol (D1) and the at least one polyisocyanate (II). For example, the compound (C1) can be a polyol, but also a polymer having at least two hydroxyl groups or at least two amino groups other than a polyol, for example a hydrophobic polymer or oligomer comprising silicon.
[0032] The compound (C1) is preferably a polyol, more preferably selected from the group of divalent radicals of an oligo- or polysiloxane of the general formula I -[Ak-O] q -Ak-Si(R 2 )-[O-Si(R 2 )] p -O-Si(R 2 )-Ak-[O-Ak] q' - (I) where Ak is C 2 -C 4 alkylene and R C 1 -C 4 alkyl and each of p, q and q' is independently a number in the range 0-50, where p is more preferably a number in the range 1 to 50, more preferably in the range 2 to 50. Ak can denote identical alkylene units in each (C1), but Ak can also denote different alkylene units in the same radical (C1). Ak can denote, for example, ethylene or propylene in the same radical (C1).
[0033] In one embodiment, (C1) is a polydimethylsiloxane of the general formula (II) where m is in the range from 5 to 80. In a further embodiment, (C1) is a polydimethylsiloxane of the general formula (III) where n and m are each in the range from 5 to 80.
[0034] According to a further embodiment, the compound (C1) is a polyol. All suitable polyols can be used here, for example, polyetherdiols or polyesterdiols, or mixtures of two or more thereof. Suitable polyether polyols or diols are, for example, polyetherdiols based on ethylene oxide or propylene oxide or mixtures thereof, for example, copolymers such as block copolymers. Furthermore, any suitable polyesterdiol can be used, whereby polyesterdiol here also includes polycarbonatediols.
[0035] The composition and properties of the first porous membrane can be varied depending on the application. For example, the thickness of the first membrane can be varied within a wide range.
[0036] The first porous membrane has a liquid inlet pressure (LEP) determined according to DIN EN 20811 in the range of 1 to 5 bar, preferably in the range of 3 to 4 bar. The water vapor permeability (WDD) determined according to DIN 53122 at 38 °C and 90% relative humidity is more than 1000 [g / m 2 < *d].
[0037] The polyurethane (PU1) is based on 80 to 100% by weight of a mixture of at least one diol (D1) and at least one polyisocyanate (II). Polyurethane (PU2), which may also be present in the first porous membrane, is based on at least one polyol (P2), at least one diol (D2), and at least one polyisocyanate (I2).
[0038] Polyisocyanate (II) and polyisocyanate (I2) may be the same or different. Aliphatic, cycloaliphatic, araliphatic, and / or aromatic diisocyanates can be used as polyisocyanates (II) and (I2). Examples include the following aromatic isocyanates: 2,4-toluene diisocyanate, mixtures of 2,4- and 2,6-toluene diisocyanate, 4,4'-, 2,4'- and / or 2,2'-diphenylmethane diisocyanate (MDI), mixtures of 2,4'- and 4,4'-diphenylmethane diisocyanate, urethane-modified liquid 4,4'- and / or 2,4-diphenylmethane diisocyanate, 4,4'-diisocyanatodiphenylethane, mixtures of monomeric methanediphenyl diisocyanates and other highly polycyclic homologues of methanediphenyl diisocyanate (polymeric MDI), 1,2- and 1,5-naphthylene diisocyanate.
[0039] Aliphatic diisocyanates are common aliphatic and / or cycloaliphatic diisocyanates, for example tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2-methylpentamethylene-1,5-diisocyanate, 2-ethylbutylene-1,4-diisocyanate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), 1,4-cyclohexane diisocyanate, 1-methyl-2,4- and / or -2,6-cyclohexane diisocyanate, 4,4'-, 2,4'- and / or 2,2'-dicyclohexylmethane diisocyanate.
[0040] Polyisocyanate prepolymers are obtainable by reacting the above-described polyisocyanates in excess, for example at temperatures in the range of 30 to 100°C, preferably at more than 80°C, with polyols to obtain the prepolymer. Polyisocyanates and commercially available polyols based on polyesters, for example, starting from adipic acid, or on polyethers, for example, starting from ethylene oxide and / or propylene oxide, are preferably used to produce the prepolymer.
[0041] Polyols are known to those skilled in the art and are described, for example, in "Kunststoffhandbuch, 7, Polyurethane," Carl Hanser Verlag, 3rd edition 1993, Section 3.1. Polyols that are preferably used are polymeric compounds containing hydrogen atoms that are reactive toward isocyanates. Particularly preferred polyols are polyetherols.
[0042] During the preparation of the polyisocyanate prepolymers, conventional chain extenders or crosslinking agents can optionally be added to the polyols. Preferred chain extenders are 1,4-butanediol, dipropylene glycol, and / or tripropylene glycol. In this case, the ratio of organic polyisocyanates to polyols and chain extender is preferably selected such that the isocyanate prepolymer has an NCO content in the range of 2% to 30%, more preferably in the range of 6% to 28%, and even more preferably in the range of 10% to 24%.
[0043] The at least one polyisocyanate (II), (II) is preferably selected from the group consisting of aromatic, araliphatic, and aliphatic polyisocyanates, preferably from the group consisting of diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), and hexamethylene diisocyanate (HDI). The polyisocyanate can be used pure or in the form of a composition, for example, as an isocyanate prepolymer. Furthermore, a mixture comprising polyisocyanate and at least one solvent can be used, with suitable solvents being known to the person skilled in the art.
[0044] Diol (D1) and diol (D2) can be the same or different. Generally, any diol can be used. Diol (D1) and diol (D2) are preferably selected from the group consisting of aliphatic, araliphatic, aromatic, and / or cycloaliphatic compounds having a molecular weight in the range from 0.05 kg / mol to 0.499 kg / mol, preferably difunctional compounds, for example diamines and / or alkanediols having 2 to 10 carbon atoms in the alkylene moiety, di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona-, and / or decaalkylene glycols having 3 to 8 carbon atoms, in particular ethylene-1,2-glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, and preferably corresponding oligo- and / or polypropylene glycols such as diethylene glycol, dipropylene glycol, 1,4-cyclohexanediol, 1,4-dimethanolcyclohexane, and neopentyl glycol, and it is therefore possible to use mixtures.The diols preferably contain only primary hydroxyl groups, with ethanediol, butanediol, and hexanediol being particularly preferred. Diol (D1) or diol (D2) is therefore preferably selected from the group consisting of ethanediol, butanediol, and hexanediol.
[0045] In the production of polyurethane (PU1) and / or polyurethane (PU2), other compounds such as catalysts and / or conventional auxiliaries and / or additives can be used.
[0046] Common additives include surfactants, fillers, flame retardants, nucleating agents, oxidation stabilizers, lubricants and mold release agents, dyes, pigments, and optional stabilizers, e.g., for protection against hydrolysis, light, heat, or discoloration, inorganic and / or organic fillers, reinforcing agents, and plasticizers. Examples of common additives and auxiliaries can be found in the "Kunststoffhandbuch" (Plastics Handbook), Volume 7, edited by Vieweg and Höchtlen, Carl Hanser Verlag, Munich 1966 (pages 103-113).
[0047] To produce the polyurethane (PU2), a polyol (P2) is used as an additional component. Polyol (P2) is preferably a diol. Any suitable diol can be used, for example, polyetherdiols or polyesterdiols, or mixtures of two or more thereof.
[0048] Suitable polyetherdiols are, for example, polyetherdiols based on ethylene oxide or propylene oxide or mixtures thereof, for example copolymers such as block copolymers. The ratio of ethylene oxide units to propylene units can be varied within a wider range and can be, for example, in the range from 50:50 to 95:5, preferably in the range from 60:40 to 90:10, more preferably in the range from 70:30 to 85:15, more preferably in the range from 75:25 to 80:20. The molecular weight of the polyetherdiols is, for example, in the range from 1000 to 4000 Daltons, preferably in the range from 1500 to 3000 Daltons, more preferably in the range from 2000 to 2500 Daltons.
[0049] Furthermore, any suitable polyesterdiol can be used, whereby polyesterdiol here also includes polycarbonatediols.
[0050] Suitable polyesterdiols can be produced from organic dicarboxylic acids having 2 to 12 carbon atoms, preferably aromatic dicarboxylic acids having 8 to 12 carbon atoms, and from polyhydric alcohols, preferably diols having 2 to 12 carbon atoms, preferably 2 to 6 carbon atoms. Examples of dicarboxylic acids are: succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, maleic acid, fumaric acid, phthalic acid, isophthalic acid, terephthalic acid, and the isomeric naphthalenedicarboxylic acids. The dicarboxylic acid can be used alone or in a mixture. Instead of the free dicarboxylic acid, a corresponding dicarboxylic acid derivative can also be used, for example, dicarboxylic acid esters of alcohols having 1 to 4 carbon atoms, or dicarboxylic acid anhydrides.Examples of di- and polyhydric alcohols, especially diols, are ethanediol, diethylene glycol, 1,2- and 1,3-propanediol, dipropylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,10-decanediol, glycerol, and trimethylolpropane, preferably ethylene glycol, 1,3-propanediol, methyl-1,3-propanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, or 1,6-hexanediol. Examples of other suitable compounds are polyesterdiols derived from lactones such as epsilon-caprolactone, or hydroxycarboxylic acids, e.g., omega-hydroxycaproic acid and hydroxybenzoic acids. Production of the first and second porous membrane
[0051] The first porous membrane is produced by a process comprising (a) Providing a solution (L1) comprising at least one polyurethane (PU1); (b) producing the first membrane from the solution (L1) according to (a) according to phase inversion.
[0052] The porous membrane has pores with an average pore diameter in the range of 0.001 µm to 0.8 µm, determined by Hg porosimetry according to DIN 66133.
[0053] Preferably, the first porous membrane receives a gradient in pore size distribution across the diameter of the membrane.
[0054] According to (a), the solution (L1) comprising at least one polyurethane (PU1) is provided. The solution (L1) comprises polyurethane (PU1) and at least one suitable solvent or solvent mixture. Suitable solvents are selected, for example, from the group of organic, especially aprotic, polar solvents. Suitable solvents have a boiling point in the range from 80 to 320°C, preferably from 100 to 280°C, more preferably from 150 to 250°C.Suitable aprotic polar solvents include, for example, high-boiling esters, ketones, asymmetrically halogenated hydrocarbons, anisole, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, sulfolane, N,N-dimethyl-2-hydroxypropanoamide, N,N-diethyl-2-hydroxypropanoamide, N,N-dimethyl-2-methoxypropanoamide, N,N-diethyl-2-methoxypropanoamide, N-formylpyrrolidine, N-acetylpyrrolidine, N-formylpiperidine, N-acetylpiperidine, N-formylmorpholine, N-acetylmorpholine, N-methyl-2-pyrrolidone, and / or N-ethyl-2-pyrrolidone. Mixtures of two or more of these solvents can also be used.
[0055] N-methylpyrrolidone is particularly preferred as the solvent for solution (L1). Solution (L1) may contain polyurethane (PU1) in an amount sufficient to form a film from the solution. Solution (L1) comprises, for example, from 10 to 35% by weight of polyurethane (PU1), preferably from 15 to 25% by weight.
[0056] The solution (L1) can be produced at elevated temperatures.
[0057] According to (b), the porous membrane is produced from solution (L1) by phase inversion. Suitable methods are known to those skilled in the art. Preferably, a non-solvent-induced phase inversion is carried out. Step (b) can, for example, comprise steps (ba) and (bb): (ba) forming a film from the solution (L1); (bb) contacting the film according to (ba) with a mixture (L2).
[0058] According to (ba), a film is produced from the solution (L1) using methods known to those skilled in the art. This film is then brought into contact with a mixture (L2) according to (bb).
[0059] Step (b) causes coagulation, and membranes are obtained. The mixture (L2) can contain any compound capable of causing coagulation. The mixture (L2) has a lower solubility for polyurethane (PU1) than the solvent used to prepare (L1). In particular, non-solvents such as water or mixtures containing water are used. Suitable coagulants include, for example, liquid water, steam, alcohols, or mixtures thereof. Preferred alcohols as coagulants in (L2) are mono-, di-, or tri-alkanols that do not contain any further functional groups, such as isopropanol, ethylene glycol, or propylene glycol.
[0060] Step (b), in particular steps (ba) and / or (bb) may be carried out at elevated temperatures.
[0061] Solution (L1) comprises at least one polyurethane (PU1) but may also comprise other compounds or additives. According to one embodiment, (L1) further comprises polyurethane (PU2). The solution (L1) may also contain additives such as polyhydroxy compounds, such as diols or triols. For example, additives can be selected from the group consisting of mono-, di-, or tri-alkanols that do not contain any other functional groups, such as isopropanol, ethylene glycol, propylene glycol, or propylenetriol (glycerol). Glycerol is preferably used as an additive in the solution (L1).
[0062] Second porous membrane The material of the second porous membrane comprises a thermoplastic elastomer selected from the group consisting of polyurethane, polyester, polyetherester, polyesterester, polyamide, polyetheramide, polystyrene, ethylene vinyl acetate elastomer and mixtures of two or more of these elastomers, preferably polyurethane elastomer.
[0063] The second porous membrane preferably has an average thickness in the range of 5 to 150 µm, more preferably in the range of 50 to 100 µm, and more preferably in the range of 70 to 90 µm. The second porous membrane preferably has pores with an average pore diameter of less than 2000 nm, preferably in the range of 0.001 µm to 0.8 µm, determined by mercury porosimetry according to DIN 66133.
[0064] In a preferred embodiment, the material of the first porous membrane according to i) and that of the second porous membrane comprises the same thermoplastic elastomer.
[0065] According to a preferred embodiment, the invention therefore relates to a method for welding porous membranes, comprising: iii) welding the first and second porous membranes at least in part of the overlay region according to ii) at a temperature in the range of 150 to 250°C, to obtain an at least partially welded composite of the first and second porous membranes.
[0066] The second porous membrane is preferably produced by the same method as described above for the first porous membrane. Welded composite
[0067] The invention further relates to a welded composite of a first and a second porous membrane, obtained or obtainable by the method described above, wherein the first and second porous membranes are connected to one another in the form of a weld seam at least in a part of the overlay region.
[0068] A "welded composite of a first and second porous membrane" is understood to mean a composite in which the first and second porous membranes at least partially overlap, and wherein the first and second porous membranes are connected to one another in the form of a weld seam, at least in part of the overlapping region. Surprisingly, such a welded composite exhibits the same good water vapor permeability and the same high liquid ingress pressure as the unwelded first porous membrane itself, particularly in the direct region of the weld seam. The "weld seam" in the context of the present invention refers to the region in which the welding of the first and second porous membranes has taken place, i.e., the region in which the first and second porous membranes are permanently connected to one another.Inseparable (synonym: non-separable) means that, according to DIN ISO 527-3, the weld seam has a fracture stress in the range of 0.2 to 10 MPa, preferably in the range of 0.5 to 5 MPa, more preferably in the range of 1 to 2 MPa, before separation of the first and second porous membranes occurs. The corresponding elongation at break of the first and second porous membranes is in the range of 5 to 200%, more preferably in the range of 5 to 100%.
[0069] In the context of the present invention, the expression "equally good water vapor permeability" means that the water vapor permeability of the at least partially welded composite obtained according to (iii) is in the range of 75 to 100%, preferably in the range of 80 to 100%, more preferably in the range of 90 to 100%, relative to the water vapor permeability of the first porous membrane provided according to (i). This applies to the entire at least partially welded composite obtained according to (iii), and in particular in the region of the weld seam. The expression "the same high liquid inlet pressure" in the context of the present invention means that the liquid inlet pressure of the at least partially welded composite obtained according to (iii) is in the range of 75 to 100%, preferably in the range of 80 to 100%, more preferably in the range of 90 to 100%, based on the liquid inlet pressure of the first porous membrane provided according to (i).This applies to the entire, at least partially welded, composite obtained according to (iii), and in particular in the area of the weld seam.
[0070] Preferably, the obtained or obtainable welded composite, particularly in the region of the weld seam, has a water vapor permeability (WP) of more than 1000 [g / m 2 < *d] at 38 °C and 90% relative humidity according to DIN 53122. Likewise, the obtained or obtainable welded composite preferably has, particularly in the region of the weld seam, a watertightness (LTP) of greater than 2 bar and preferably in the range of 2 to 5 bar, more preferably in the range of 3 to 4 bar, determined according to DIN EN 20811.
[0071] Furthermore, a welded composite of a first and second porous membrane is disclosed, wherein the first porous membrane has an average thickness in the range of 5 to 150 µm, preferably in the range of 50 to 100 µm, more preferably in the range of 70 to 90 µm. According to one embodiment, the first porous membrane has pores with an average pore diameter of less than 2000 nm, preferably in the range of 0.001 µm to 0.8 µm, determined by Hg porosimetry according to DIN 66133. A "welded composite of a first and second porous membrane" is also understood here to mean a composite in which the first and second porous membranes at least partially overlap, and wherein the first and second porous membranes are connected to one another in the form of a weld seam, at least in part of the overlapping area. The "weld seam" in the context of the present invention means the area in which the welding of the first and second porous membrane has taken place, ieThe area in which the first and second porous membranes are permanently bonded to one another. "Permanently bonded" (synonym: non-detachable) means that, according to DIN ISO 527-3, the weld seam has a fracture stress in the range of 0.2 to 10 MPa, preferably in the range of 0.5 to 5 MPa, more preferably in the range of 1 to 2 MPa, before separation of the first and second porous membranes occurs. The corresponding elongation at break of the first porous membrane is in the range of 5 to 200%, more preferably in the range of 5 to 100%.
[0072] The material of the first porous membrane preferably comprises a thermoplastic elastomer, more preferably selected from the group consisting of polyurethane, polyester, polyetherester, polyesterester, polyamide, polyetheramide, polystyrene, ethylene-vinyl acetate elastomers, and mixtures of two or more of these elastomers, more preferably polyurethane elastomer. The material of the first porous membrane preferably comprises a polyurethane elastomer (PU1) based on the following components: 80 to 100% by weight of a mixture of at least one diol (D1) and at least one isocyanate (II), 0 to 20% by weight of at least one compound (C1) having at least two isocyanate-reactive groups; and wherein the first porous membrane has pores with an average pore diameter in the range of 0.001 µm to 0.8 µm, determined by Hg porosimetry according to DIN 66133.
[0073] Preferably, the polyurethane elastomer (PU1) comprises a further polyurethane (PU2) based on at least one polyol (P2), at least one diol (D2) and at least one polyisocyanate (I2).
[0074] For details on PU1, PU2, P2, D1, D2, I1 and I2, please refer to the above explanations.
[0075] The welded composite exhibits the same good water vapor permeability and the same high liquid entry pressure as the unwelded first porous membrane itself, particularly in the direct area of the weld (weld seam). In the context of the present invention, the term "the same good water vapor permeability" means that the water vapor permeability of the welded composite is in the range of 75 to 100%, preferably in the range of 80 to 100%, more preferably in the range of 90 to 100%, based on the water vapor permeability of the first porous membrane. This applies to the entire welded composite, and especially in the area of the weld seam.The term "the same high liquid inlet pressure" in the context of the present invention means that the liquid inlet pressure of the welded composite is in the range of 75 to 100%, preferably in the range of 80 to 100%, more preferably in the range of 90 to 100%, relative to the liquid inlet pressure of the first porous membrane. This applies to the entire welded composite, and especially in the area of the weld seam.
[0076] Preferably, the welded composite also has, particularly in the area of the weld seam, a water vapor permeability (WP) of more than 1000 [g / m 2 < *d] at 38 °C and 90% relative humidity according to DIN 53122. Likewise, the welded composite preferably has, particularly in the area of the weld seam, a watertightness (LTP) of greater than 2 bar and preferably in the range of 2 to 5 bar, more preferably in the range of 3 to 4 bar, determined according to DIN EN 20811.
[0077] According to a preferred embodiment, the welded composite is used to produce an article selected from the group consisting of clothing, shoes, boots, protective suits, tents, and tarpaulins. The welded composite according to the present invention is used, for example, in clothing, such as outdoor clothing, sportswear such as sailing, climbing, or skiing clothing, rainwear, protective clothing, headwear such as hats, caps, or for shoes or boots. Furthermore, the welded composite is used in tent tarpaulins and protective films / tarpaulins. Description of the figure
[0078] Fig. 1 shows an SEM image of the cross-sectional area of the welded composite (membrane composite) in the area of the weld seam.
[0079] The present invention is further illustrated by the following embodiments and combinations of embodiments as indicated by the corresponding references and backreferences. In particular, it should be emphasized that whenever a range of embodiments is specified, for example, in the context of an expression such as "A preferred embodiment (5) which concretizes any of the embodiments (1) to (4)," each embodiment in the range is intended to be explicitly disclosed to one skilled in the art, i.e., the meaning of this expression is to be understood by one skilled in the art as synonymous with "A preferred embodiment (5) which concretizes any of the embodiments (1), (2), (3), and (4)."
[0080] In one embodiment (1), the invention relates to a method for welding porous membranes, comprising: i) providing a first porous membrane and a second porous membrane; ii) at least partially overlaying the first and second porous membranes according to i) to obtain an at least partially overlay region;iii) welding the first and second porous membranes at least in part of the overlapping region according to ii) at a temperature in the range from 100 to 250°C, preferably in the range from 150 to 250°C, to obtain an at least partially welded composite of the first and second porous membranes, wherein the material of the first and second porous membranes comprises a thermoplastic elastomer selected from the group consisting of polyurethane, polyester, polyetherester, polyesterester, polyamide, polyetheramide, polystyrene, ethylene vinyl acetate elastomer and mixtures of two or more of these elastomers, wherein the first and second porous membranes have pores with an average pore diameter of less than 2000 nm, determined by means of Hg porosimetry according to DIN 66133, wherein the first and second porous membranes are connected to one another in the form of a weld seam at least in part of the overlapping region.
[0081] A preferred embodiment (2), which concretizes embodiment (1), relates to a method wherein the welding according to iii) is carried out for a period of time in the range from 0.1 second to 10 minutes, more preferably in the range from 0.5 seconds to 60 seconds, more preferably in the range from 1 to 10 seconds.
[0082] A preferred embodiment (3), which specifies embodiment (1) or (2), relates to a method wherein the welding according to iii) is carried out under an atmosphere selected from protective gas, in particular argon or nitrogen, air or lean air, more preferably under air.
[0083] A preferred embodiment (4), which specifies one of the embodiments (1) to (3), relates to a method wherein the welding according to iii) is carried out at a pressure in the range from 1 to 10 bar, more preferably in the range from 2 to 8 bar, more preferably in the range from 3 to 5 bar.
[0084] A preferred embodiment (5), which specifies one of the embodiments (1) to (4), relates to a method wherein the welding according to iii) takes place at a temperature in the range of 150 to 250 °C.
[0085] A preferred embodiment (6), which concretizes one of the embodiments (1) to (5), relates to a method wherein the first porous membrane has an average thickness in the range of 5 to 150 µm, more preferably in the range of 50 to 100 µm, more preferably in the range of 70 to 90 µm.
[0086] A preferred embodiment (7), which specifies one of the embodiments (1) to (6), relates to a method wherein the first porous membrane has pores with an average pore diameter in the range of 0.001 µm to 0.8 µm, determined by means of Hg porosimetry according to DIN 66133.
[0087] A preferred embodiment (8), which concretizes one of the embodiments (1) to (7), relates to a method wherein the material of the first porous membrane comprises a polyurethane elastomer.
[0088] A preferred embodiment (9), which concretizes embodiment (8), relates to a method wherein the material of the first porous membrane comprises a polyurethane elastomer based on the following components: 80 to 100% by weight of a mixture of at least one diol (D1) and at least one isocyanate (II), 0 to 20% by weight of at least one compound (C1) having at least two isocyanate-reactive groups; and wherein the first porous membrane has pores with an average pore diameter in the range of 0.001 µm to 0.8 µm, determined by Hg porosimetry according to DIN 66133.
[0089] A preferred embodiment (10), which concretizes embodiment (9), relates to a method wherein the material of the first porous membrane comprises a further polyurethane (PU2) based on at least one polyol (P2), at least one diol (D2) and at least one polyisocyanate (I2).
[0090] A preferred embodiment (11), which specifies embodiment (9) or (10), relates to a process wherein the compound (C1) is a polyol, preferably selected from the group of divalent radicals of an oligo- or polysiloxane of the general formula I -[Ak-O] q -Ak-Si(R 2 )-[O-Si(R 2 )] p -O-Si(R 2 )-Ak-[O-Ak] q' - (I) wherein Ak is C 2 -C 4 alkylene and R C 1 -C 4 alkyl and each of p, q and q' is independently a number in the range of 0-50, wherein p is more preferably a number in the range of 1 to 50, more preferably in the range of 2 to 50.
[0091] A preferred embodiment (12), which specifies one of the embodiments (9) to (11), relates to a process wherein the diol (D1) is selected from the group consisting of ethanediol, butanediol and hexanediol.
[0092] A preferred embodiment (13), which specifies one of the embodiments (9) to (12), relates to a process wherein the polyisocyanate is selected from the group consisting of diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI) and hexamethylene diisocyanate (HDI).
[0093] A preferred embodiment (14), which concretizes one of the embodiments (1) to (13), relates to a method wherein the material of the second porous membrane comprises a polyurethane elastomer.
[0094] A preferred embodiment (15), which concretizes embodiment (14), relates to a method wherein the second porous membrane has an average thickness in the range of 5 to 150 µm, more preferably in the range of 50 to 100 µm, more preferably in the range of 70 to 90 µm.
[0095] A preferred embodiment (16), which specifies embodiment (14) or (15), relates to a method wherein the second porous membrane has pores with an average pore diameter in the range of 0.001 µm to 0.8 µm, determined by means of Hg porosimetry according to DIN 66133.
[0096] A preferred embodiment (17), which concretizes one of the embodiments (14) to (16), relates to a method wherein the material of the porous membrane according to i) and that of the second porous membrane comprise the same thermoplastic elastomer, preferably the same polyurethane elastomer.
[0097] An embodiment (18) of the invention relates to a welded composite of a first and a second porous membrane, obtained or obtainable by the process according to one of the embodiments (1) to (17), wherein the first and second porous membranes are connected to one another in the form of a weld seam at least in a part of the overlay region.
[0098] A preferred embodiment (19), which specifies embodiment (18), relates to a welded composite, wherein the water vapor permeability (WDP) of the welded composite at 38 °C and 90% relative humidity according to DIN 53122 is more than 1000 [g / m 2< *d].
[0099] A preferred embodiment (20), which specifies embodiment (18) or (19), relates to a welded composite, wherein the watertightness (LEP) is greater than 2 bar and preferably in the range of 2 to 5 bar, more preferably in the range of 3 to 4 bar, determined according to DIN EN 20811.
[0100] Furthermore, an embodiment (21) relating to a welded composite of a first and a second porous membrane is disclosed, wherein the first porous membrane has an average thickness in the range from 5 to 150 µm, preferably in the range from 50 to 100 µm, more preferably in the range from 70 to 90 µm.
[0101] Furthermore, an embodiment (22) is disclosed, which specifies embodiment (21), relates to a welded composite, wherein the first porous membrane has pores with an average pore diameter of less than 2000 nm, more preferably in the range from 0.001 µm to 0.8 µm, determined by means of Hg porosimetry according to DIN 66133.
[0102] Furthermore, a (23) is disclosed, which specifies embodiment (21) or (22), relates to a welded composite, wherein the material of the first porous membrane comprises a thermoplastic elastomer, more preferably selected from the group consisting of polyurethane, polyester, polyetherester, polyesterester, polyamide, polyetheramide, polystyrene, ethylene vinyl acetate elastomer and mixtures of two or more of these elastomers, preferably polyurethane elastomer.
[0103] Furthermore, a (24) is disclosed, which concretizes one of the embodiments (21) to (23), relates to a welded composite, wherein the material of the first porous membrane is a polyurethane elastomer based on the following components: 80 to 100% by weight of a mixture of at least one diol (D1) and at least one isocyanate (II), 0 to 20% by weight of at least one compound (C1) having at least two isocyanate-reactive groups; and wherein the first porous membrane has pores with an average pore diameter in the range of 0.001 µm to 0.8 µm, determined by Hg porosimetry according to DIN 66133.
[0104] Furthermore, an embodiment (25) is disclosed, which specifies embodiment (24), relates to a welded composite, wherein the material of the first porous membrane comprises a further polyurethane (PU2) based on at least one polyol (P2), at least one diol (D2) and at least one polyisocyanate (I2).
[0105] Furthermore, an embodiment (26) is disclosed, which specifies embodiment (24) or (25), and relates to a welded composite, wherein the compound (C1) is a polyol, preferably selected from the group of divalent radicals of an oligo- or polysiloxane of the general formula I -[Ak-O] q -Ak-Si(R 2 )-[O-Si(R 2 )] p -O-Si(R 2 )-Ak-[O-Ak] q' - (I) wherein Ak is C 2 -C 4 alkylene and R C 1 -C 4 alkyl and each of p, q and q' is independently a number in the range from 0 to 50, wherein p is more preferably a number in the range from 1 to 50, more preferably in the range from 2 to 50.
[0106] Furthermore, an embodiment (27) which specifies one of the embodiments (24) to (26) is disclosed, relates to a welded composite, wherein the diol (D1) is selected from the group consisting of ethanediol, butanediol and hexanediol.
[0107] Furthermore, an embodiment (28) is disclosed, which specifies one of the embodiments (24) to (27), relates to a welded composite, wherein the polyisocyanate is selected from the group consisting of diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI) and hexamethylene diisocyanate (HDI).
[0108] Furthermore, an embodiment (29) is disclosed, which specifies one of the embodiments (24) to (28), relates to a welded composite, wherein the carrier material comprises a second porous membrane, wherein the material of the second porous membrane comprises a thermoplastic elastomer selected from the group consisting of polyurethane, polyester, polyetherester, polyesterester, polyamide, polyetheramide, polystyrene, ethylene vinyl acetate elastomer and mixtures of two or more of these elastomers, preferably polyurethane elastomer.
[0109] Furthermore, an embodiment (30) is disclosed, which specifies embodiment (29), relates to a welded composite, wherein the second porous membrane has an average thickness in the range from 5 to 150 µm, more preferably in the range from 50 to 100 µm, more preferably in the range from 70 to 90 µm.
[0110] Furthermore, an embodiment (31) is disclosed, which specifies embodiment (29) or (30), relates to a welded composite, wherein the second porous membrane has pores with an average pore diameter of less than 2000 nm, more preferably in the range of 0.001 µm to 0.8 µm, determined by means of Hg porosimetry according to DIN 66133.
[0111] Furthermore, an embodiment (32) is disclosed, which concretizes one of the embodiments (29) to (31), relates to a welded composite, wherein the material of the first porous membrane according to i) and that of the second porous membrane comprise the same thermoplastic elastomer, preferably the same polyurethane elastomer.
[0112] Furthermore, an embodiment (33) is disclosed, which specifies one of the embodiments (21) to (32), relates to a welded composite, wherein the water vapor permeability (WDP) at 38 °C and 90% relative humidity according to DIN 53122 is more than 1000 [g / m 2< *d].
[0113] Furthermore, an embodiment (34) is disclosed, which concretizes one of the embodiments (21) to (33), relates to a welded composite, wherein the watertightness (LEP) is greater than 2 bar and preferably in the range of 2 to 5 bar, more preferably in the range of 3 to 4 bar, determined according to DIN EN 20811.
[0114] An embodiment (35) of the invention relates to the use of a welded composite according to one of the embodiments (18) to (20) for producing an article selected from the group consisting of clothing, shoes, boots, protective suits, tents and tarpaulins. References
[0115] US 3,953,566, US 3,962,153 US 5,562,977 JP 5005276 US 2015 / 0230563 "Kunststoffhandbuch, 7, Polyurethane", Carl Hanser Verlag, 3rd edition 1993, Section 3.1. "Kunststoffhandbuch" 7, Carl Hanser Verlag, 1966, pages 103-113. EP 3100849 A1 GB 2496244 A WO 2016 / 061321 A1 EP 2476324 A1 Examples
[0116] The following examples serve to illustrate the invention, but are not limiting with regard to the subject matter of the invention. 1. Production of the polyurethane (hard phase) 1.1 Substances
[0117] The following substances were used: abbreviation Connection Molecular weight [g / mol] ISO 1 4,4'-Methylenediphenylene diisocyanate 250.26 g / mol KV 2 1,4-Butanediol 90.12 g / mol 1.2 Synthesis of polyurethane (hard phase type 1)
[0118] The chain extender KV2 was distributed in a 2-liter can. Isocyanate Iso1 was then added with gentle stirring, and the reaction was gently heated to 70°C in air. The mixture was then stirred until a temperature of 90°C was reached. The reaction mixture was poured into a shallow dish and heated on a hotplate at 125°C for 10 minutes. The resulting rind was annealed in a heating oven at 80°C for 15 minutes.
[0119] The resulting material was cut into pieces and ground into granules. 1.3 Composition of the produced material
[0120] Isocyanate (Iso) Amount of Iso [g] Diol (KV) Quantity KV [g] Total amount [g] ISO 1 441,1 KV 2 158,9 600 2. Production of the membranes 2.1 Abbreviations and connections:
[0121] NMPN-Methylpyrrolidone GLYGlycerin LEPLiquid inlet pressure WDDWater vapor permeability 2.2 Test methods
[0122] The membranes' liquid inlet pressure was determined according to DIN EN 20811 using a 60 mm diameter pressure cell filled with ultrapure water (salt-free water filtered through a Millipore UF system) up to 4.0 bar (40,000 mm water column). The liquid inlet pressure (LEP) is defined as the pressure at which liquid water begins to permeate the membrane. A high LEP allows the membrane to withstand a high liquid water column.
[0123] Water vapor permeability (WDP) was determined using a cup method at 38 °C and 90% relative humidity according to DIN 53122. High WDP values were desired and allowed high water vapor flow rates. Tensile tests for Young's modulus and elongation at break were conducted according to DIN 53455 / ISO 527.
[0124] Tensile properties were characterized according to ISO 527-3. 2.3 Preparation of porous membranes using N-methylpyrrolidone as polymer solvent
[0125] In a three-necked flask equipped with a magnetic stirrer, 81 ml of N-methylpyrrolidone (1), 10 g of glycerol as a second additive, and 19 g of the TPU polymer according to 1. were combined. The mixture was heated to 60°C with gentle stirring until a homogeneous, clear, viscous solution was obtained, which was degassed overnight at room temperature. Clear and transparent polymer solutions were obtained.
[0126] The polymer solution was then heated to 60°C for 2 h and then coated onto a glass plate with a 150 micron coating knife at 60°C using an Erichsen coating machine at a speed of 5 mm / min. The membrane film was allowed to rest for 30 seconds, followed by immersion in a water bath at 25°C for 10 minutes. After detaching the membrane from the glass plate, it was transferred to a water bath for 12 hours. After several water washes, the membrane was stored in a humidified state until characterization for LEP and WDD. Table 1 summarizes the membrane properties. Table 1: Compositions and properties of the produced membranes; thickness in [µm], LEP in [bar], WDD in [g / m 2< *d], Young's modulus [MPa], elongation at break [%], Tg in [°C]. TPU Tg thickness LEP WDD Example 1 BUMDI 106 80 4 1220 3. Welding
[0127] Two membranes according to Section 1, Example 1 were welded in air at 120°C and a pressure of 3 bar for a period of three seconds using a semi-automatic impulse welding machine (film welding device) of the type HPL 630 A from Hawo Gerätebau GmbH, D-74847 Obrigheim. A welded membrane composite with a weld seam 3.5 mm wide was obtained. The welded membrane composite had a thickness of 120 µm in the weld seam area and was characterized in this area with regard to LEP and WDD. Table 3 shows the characterization results in comparison for the membrane according to Example 1 from Section 2 and the welded membrane composite. Table 3: Composition and properties of the membrane according to Example 1 and the welded membrane composite; thickness in [µm], LEP in [bar], WDD in [g / m 2< *d] Tg in [°C]. TPU Tg thickness LEP WDD Example 1 BUMDI 106 80 4 1220 welded membrane composite BUMDI 106 120 4 1220
[0128] The welded membrane composite exhibited the same good water vapor permeability and the same high liquid inlet pressure as the unwelded membrane according to Example 1. When determining the tensile properties, the seam of the welded membrane composite exhibited a fracture stress of 1.5 MPa with a fracture elongation of 8%.
[0129] The welded membrane composite was also examined using scanning electron microscopy (SEM). Fig. 1 is an SEM image of the cross-sectional area of the membrane composite in the area of the weld seam.
Claims
1. A process for welding porous membranes, comprising: i) providing a first porous membrane and a second porous membrane; ii) at least partially superimposing first and second porous membrane as per i) to obtain an at least partial superimposition region; iii) welding first and second porous membrane at least in a portion of the superimposition region as per ii) at a temperature in the range from 100 to 250°C to obtain an at least partially welded composite of first and second porous membrane; wherein the material of the first and the second porous membrane comprises a thermoplastic elastomer selected from the group consisting of polyurethane elastomer, polyester elastomer, polyetherester elastomer, polyesterester elastomer, polyamide elastomer, polyetheramide elastomer, polystyrene elastomer, ethylene-vinyl acetate elastomer and mixtures of two or more of these elastomers, wherein first and second porous membrane have pores having an average pore diameter of less than 2000 nm, determined by means of Hg porosimetry in accordance with DIN 66133, wherein first and second porous membrane are bonded together in the form of a weld seam at least in a portion of the superimposition region.
2. The process according to claim 1, wherein the welding as per iii) is effected for a period of time in the range from 0.1 seconds to 10 minutes, preferably in the range from 0.5 seconds to 60 seconds, more preferably in the range from 1 to 10 seconds.
3. The process according to either of claims 1 and 2, wherein the welding as per iii) is effected under an atmosphere selected from protective gas, especially argon or nitrogen, air or lean air, preferably under air.
4. The process according to any of claims 1 to 3, wherein the welding as per iii) is effected at a pressure in the range from 1 to 10 bar, preferably in the range from 2 to 8 bar, more preferably in the range from 3 to 5 bar.
5. The process according to any of claims 1 to 4, wherein the welding as per iii) is effected at a temperature in the range from 150 to 250°C.
6. The process according to any of claims 1 to 5, wherein the first porous membrane has an average thickness in the range from 5 to 150 µm, preferably in the range from 50 to 100 µm, more preferably in the range from 70 to 90 µm.
7. The process according to any of claims 1 to 6, wherein the first porous membrane has pores having an average pore diameter in the range from 0.001 µm to 0.8 µm, determined by means of Hg porosimetry in accordance with DIN 66133.
8. The process according to claim 1, wherein the material of the first porous membrane comprises a polyurethane elastomer based on the following components: - 80% to 100% by weight of a mixture of at least one diol (D1) and at least one isocyanate (11), - 0 to 20% by weight of at least one compound (C1) having at least two isocyanate-reactive groups; and wherein the porous membrane has pores having an average pore diameter in the range from 0.001 µm to 0.8 µm, determined by means of Hg porosimetry in accordance with DIN 66133.
9. The process according to claim 1, wherein the second porous membrane has an average thickness in the range from 5 to 150 µm, preferably in the range from 50 to 100 µm, more preferably in the range from 70 to 90 µm, and / or has pores having an average pore diameter t in the range from 0.001 µm to 0.8 µm, determined by means of Hg porosimetry in accordance with DIN 66133.
10. The process according to claim 9, wherein the material of the first porous membrane as per i) and that of the second porous membrane comprise the same thermoplastic elastomer, preferably the same polyurethane elastomer.
11. A welded composite of a first and a second porous membrane, obtained or obtainable by the process according to any of claims 1 to 10, wherein first and second porous membrane are bonded together in the form of a weld seam at least in a portion of the superimposition region.
12. The welded composite according to claim 11, wherein the water vapor permeability (WVP) at 38°C and 90% relative humidity according to DIN 53122 is more than 1000 [g / m2*d] and / or the watertightness (LEP) is greater than 2 bar and preferably is in the range from 2 to 5 bar, more preferably in the range from 3 to 4 bar, determined according to DIN EN 20811.