AI Technical Summary
Existing methods for welding coated steel sheets, particularly those with aluminum-silicon coatings, face challenges in achieving stable and reproducible weld seams with consistent mechanical properties, often resulting in differences in final strength and quality due to complex system technologies and insufficient homogenization effects.
A method utilizing two laser beams that rotate around the weld pool to create a defined stirring effect, with specific parameters such as rotation frequency, welding speed, spot diameter, and spot distance, to ensure homogeneous distribution of filler wire and coating materials, thereby improving weld seam quality and mechanical properties.
This approach enables the production of reliably homogeneous weld seams with reproducible mechanical properties, addressing the issues of inconsistent strength and quality in previous methods by optimizing the interaction between laser beams and the weld pool.
Description
[0001] The invention relates to a method for welding coated steel sheets according to the preamble of claim 1.
[0002] In automotive engineering, it is common practice to manufacture body parts from highly hardenable steel sheets to ensure sufficient stability of the passenger compartment. High-strength steels have the advantage that, due to their high load-bearing capacity, dimensions and thus weight can be reduced, thus saving fuel.
[0003] High-strength steel grades formed in this way include manganese-boron alloyed steels, such as the most commonly used steel 22MnB5.
[0004] Such high-strength steel grades are processed using the so-called press hardening process, in which these steel grades are heated to such a high temperature that the originally ferritic-pearlitic steel structure is transformed into an austenitic microstructure. This austenitic high-temperature structure of the iron allows it to be transformed into a martensitic microstructure by quenching at a rate exceeding the critical hardening rate. Due to the different carbon solubility of austenite and martensite, a lattice distortion occurs, which enables high hardness of up to over 1500 MPa. This hardening process has been known for some time and is therefore widely used.
[0005] When it comes to press hardening, there are basically two different ways to produce such components: the direct and the indirect process.
[0006] In the direct process, a flat blank is austenitized and then formed and quenched in a press-hardening tool in one or more strokes. This process is comparatively inexpensive, but does not always allow for highly complex geometries.
[0007] In the indirect process, a component is first cold-formed from a flat blank, which also allows for complex geometries. The formed component is then austenitized and subsequently quenched in a press tool, usually without further major deformation. The forming tool thus has a contour corresponding to the already formed component and serves only for hardening.
[0008] Such steel sheets used for press hardening can already be provided as blanks with a corrosion protection coating. The usual corrosion protection coatings are a zinc coating or zinc alloy coating, or an aluminum or aluminum alloy coating.
[0009] It is also known to use composite blanks, so-called tailored blanks, in which either different steel grades are welded together or the same steel grades but with different thicknesses are welded together.
[0010] Here, too, coated output boards are of course possible, so that, for example, two sheets of 22MnB5 with different thicknesses and an aluminum-silicon coating are welded together.
[0011] However, particularly when welding aluminum-silicon-coated sheets, it was observed that aluminum from the coating apparently migrated into the weld seam. The aluminum in the weld seam has an adverse effect on martensite transformation or martensite formation. Furthermore, aluminum causes the formation of intermetallic phases, which are relatively hard in themselves but also very brittle and can therefore serve as crack initiators.
[0012] To avoid the problem when welding tailored blanks, it is known to partially remove aluminum layers on both sides of a planned weld butt joint before welding in order to prevent aluminum-silicon from penetrating the weld seam.
[0013] The disadvantage here is that in this case there is no corrosion protection in the area of the weld seam and, in particular, when heated for the purpose of hardening, the weld seam and the edges bordering the weld seam can become scalded and decarburized later.
[0014] Another disadvantage is that these processes for removing the aluminum-silicon coatings represent an additional process step that is not easy to master.
[0015] DE 10 2012 111 118 B3 discloses a method for laser welding one or more workpieces made of press-hardenable steel, in particular manganese-boron steel, in which butt welding is carried out and in which the workpiece or workpieces have a thickness of at least 1.8 mm and / or a thickness jump of at least 0.4 mm occurs at the butt joint, wherein filler wire is fed into the molten pool created with a laser beam during laser welding. In order to ensure that the weld seam can be reliably hardened into a martensitic structure during hot forming, this document provides for the addition of at least one alloying element from the group comprising manganese, chromium, molybdenum, silicon and / or nickel to the filler wire, which promotes the formation of austenite in the molten pool created with the laser beam, wherein this alloying element contains at least one alloying element with a thickness of at least0.1 percent greater mass fraction is present in the filler wire than in the press-hardenable steel of the workpiece or workpieces.
[0016] DE 10 2014 001 979 A1 discloses a method for laser welding one or more workpieces made of hardenable steel in a butt joint, wherein the steel is in particular a manganese-boron steel and the workpieces have a thickness between 0.5 and 1.8 mm and / or a thickness jump of between 0.2 and 0.4 mm occurs at the butt joint. During laser welding, a filler wire is introduced into the molten pool, the molten pool being generated exclusively by the single laser beam. To ensure that the weld seam can be reliably hardened into a martenstic structure during hot forming, the document stipulates that the filler wire contains at least one alloying element from the group comprising manganese, chromium, molybdenum, silicon, and / or nickel, thus promoting the formation of austenite.
[0017] EP 2 737 971 A1 discloses a tailor-welded blank and a method for its production. The sheet is produced by joining sheets of different thicknesses or compositions, with the aim of reducing quality problems in the weld zone. A filler wire is also used here, which is designed so that no ferrite is formed in the temperature range from 800 to 950°C. This process is said to be particularly suitable for AlSi-coated sheets, and this wire is also said to have a higher content of austenite-stabilizing elements, which consist in particular of carbon or manganese.
[0018] EP 1 878 531 B1 discloses a method for hybrid laser-arc welding of surface-coated metallic workpieces, wherein the surface coating is to contain aluminum. The laser beam is to be combined with at least one arc to melt the metal and weld the part(s), and at least one of the parts has deposits of the aluminum-silicon coating on the surface of one of its lateral cut surfaces to be welded prior to welding.
[0019] From EP 2 942 143 B1 a method for joining two blanks is known, wherein the blanks are steel sheets with a coating comprising a layer of aluminum or an aluminum alloy, wherein the two parts are welded together using a laser beam and an arc, wherein the arc torch comprises a filler wire electrode and the filler wire electrode is made of a steel alloy comprising stabilizing elements, wherein the laser and arc are moved in a welding direction, wherein the arc welding torch and the laser beam are arranged subsequently in the welding direction.
[0020] From EP 2 883 646 B1 a method for joining two blanks is known, wherein at least one of the blanks comprises a layer of aluminum or an aluminum alloy, wherein during the welding process a metal powder is fed into the welding zone and the metal powder is an iron-based powder comprising gamma-stabilizing elements and the laser beam welding is a two-point laser beam welding.
[0021] EP 2 007 545 B1 discloses a method for producing a welded part with very good mechanical properties, wherein a steel sheet has a coating consisting of an intermetallic layer and a metal alloy layer located on the intermetallic layer. For the purpose of welding the sheets, the metal alloy layer on the intermetallic layer is to be removed from the periphery of the sheet, i.e. the areas to be welded, wherein this layer is an aluminum alloy layer. This coating is to be removed using a laser beam, so that this layer, which is in the form of an aluminum-silicon layer, is evaporated off before welding in order to prevent harmful effects of the aluminum in the weld seam. At the same time, the intermetallic layer is to remain in place in order to potentially exert corrosion-inhibiting effects.
[0022] WO 2017 / 103149 A1 discloses a welding method in which two separately generated laser beams are guided along a planned weld seam. The first laser beam serves to melt a filler wire, while the second laser is intended to ensure mixing of the molten pool through a rotating movement. This is intended to ensure melting on the one hand and mixing of the filler material on the other. Furthermore, a method is disclosed in which a leading laser beam is generated that melts the filler wire, while a trailing laser beam is split into two laser beams that are guided one behind the other along the weld seam. It is stated that in this case, movement of these laser beams is not required.
[0023] WO 2019 / 030249 A1 discloses a welding process in which two aluminum-silicon coated sheets are joined together by means of a laser, whereby this laser rotates to mix a weld pool during the welding process.
[0024] The disadvantage of WO 2017 / 103149 A1 is that the system technology is extremely complex, and it has been found that the specified serial double focus with wire does not provide a sufficient homogenization effect.
[0025] DE 10 2017 120 051 A1 discloses a method for laser beam welding one or more steel sheets made of press-hardenable manganese-boron steel, in which at least one of the steel sheets has an aluminum coating. Laser beam welding is carried out by feeding a filler wire into the molten pool created exclusively by a laser beam. The filler wire should contain at least one austenite-stabilizing alloying element. The goal of the method is to achieve, with relatively low energy consumption and high productivity, a weld seam after hot forming that has a strength comparable to that of the base material. For this purpose, it is proposed that the laser beam be oscillated in such a way that it oscillates transversely to the welding direction, with the oscillation frequency of the laser beam being at least 200 Hz, preferably at least 500 Hz.In particular, this is intended to eliminate the need to remove the aluminum coating on the edge of the sheet metal edges to be welded.
[0026] From JP 2004 000 1084 a welding process is known in which a laser welding process and an arc welding process are combined to improve the gap bridging ability and to improve the depth welding, it being possible to design the laser as a laser with two beams, the welding device being designed to rotate the two beams around each other.
[0027] From DE 10 2014 107 716 B3 a welding process is known in which, in order to reduce welding spatter, the laser beam which carries out the welding is superimposed with a spatially oscillating movement during the feed movement, wherein the oscillating movement is carried out parallel or perpendicular to the joint.
[0028] The disadvantage of the above-mentioned methods is that stable, load-bearing welds cannot be reliably achieved in practice and, for inexplicable reasons, large differences in the final strength of the welds must be determined time and again.
[0029] The object of the invention is to make a welding process more reliable and to produce weld seams with reproducible mechanical properties.
[0030] The problem is solved by a method having the features of claim 1.
[0031] Advantageous further training is indicated in the dependent subclaims.
[0032] According to the invention, it was discovered that in processes in which one laser beam melts the wire while two trailing laser beams introduce additional energy into the molten pool, the weld seams repeatedly exhibit very different properties for inexplicable reasons.
[0033] In a process in which a single laser stirs but wire is used, the invention has shown that even with optimal mixing of the aluminum from the coating in the molten pool, the available aluminum is mathematically so high that the weld seams cannot be sufficiently hardened, especially with thin sheet thicknesses. Furthermore, it has been determined that oscillating single-spot lasers are clearly not capable of ensuring consistent weld seam quality.
[0034] According to the invention, the naturally existing melt pool flow is superimposed by an additional forced flow, which is generated by the rotation of a double laser beam, in order to distribute the filler wire and the aluminum from the coating homogeneously in the weld seam.
[0035] According to the invention, it was recognized that there is a relationship between the rotation frequency and the welding speed, without which a desired stirring effect cannot be achieved.
[0036] It has also been found that it is advantageous to adjust both the spot diameter and the spot distance in a defined manner in order to further improve the desired effects.
[0037] According to the invention, at least two laser beams, in particular two partial laser beams, are present that rotate in the weld pool. The welding lasers can, for example, rotate symmetrically around the weld pool center or asymmetrically around the weld pool center, with one welding beam or laser beam rotating in a smaller radius around the weld pool center, while a second welding beam or laser beam rotates with a larger radius around the weld pool center.
[0038] In another possible embodiment, a laser beam moves along the center of the weld pool, while a second welding beam or laser beam oscillates or rotates orbitally around the first welding beam. According to the invention, it was discovered that the feed rate and the stirring effect, in particular, must be coordinated. The stirring effect is defined as the number of revolutions due to the feed rate. An incorrect combination of feed rate and stirring effect can lead to negative effects such as humping, heavy spatter formation, and even weld seam penetration. A feed rate that is too low can negatively impact the cost-effectiveness of the process.
[0039] The invention thus relates to a method for welding coated steel sheets, in particular steel sheets coated with an aluminum-silicon metallic coating layer, wherein a configuration of two laser beams is present, wherein the laser beams act on a weld pool to be formed, wherein at least one laser beam rotates about a rotation axis so that the laser beams move relative to each other, wherein the laser beams are guided along a welding axis, wherein for the purpose of mixing the weld pool, a defined stirring effect and a defined welding speed are maintained in dependence on each other, wherein the stirring effect applies: η = f rot V w , where f rot is the rotation frequency and v W is the welding speed and where: 4 ≤ η ≤ 120 V w 1 mm 4 ≤ Vw ≤ 14 m min
[0040] In one embodiment of the invention, the laser beams are arranged symmetrically about a rotation axis and rotate diametrically opposite each other about the rotation axis or one laser beam is guided along a welding axis and the other laser beam rotates about the first laser beam or a first laser beam rotates with a first smaller radius about the rotation axis while the second laser beam rotates with a larger radius about the rotation axis or a mixture of these forms of movement.
[0041] In one embodiment, with a symmetrical rotation of the laser beams or their projection surfaces or spots, the laser beams are each spaced from the center by the spot distance X df, wherein the spot diameter or diameter of the laser beam df is 0.1 mm to 1 mm, wherein the total coverage width of the laser beams is the distance between the spot centers plus a spot diameter, wherein the amount is between 0.5 mm and 2.5 mm.
[0042] In this embodiment, it is particularly advantageous that the spot distance X df is: x df = 0,8 ∗ d f
[0043] In a next embodiment, in a laser beam configuration, two laser beams are arranged orbitally, wherein a first laser beam remains along the welding progress direction on a central axis of the weld pool, namely the welding axis, while the second laser beam or second spot rotates about an axis of rotation, wherein the axis of rotation lies on the welding axis or oscillates about the welding axis and represents the center of the first spot.
[0044] In this embodiment, it is particularly advantageous if the spot diameter is between 0.1 and 1 mm, where: x df = 0,8 ∗ d f and 0,45 mm ≤ x df + d f 2 ≤ 1,5 mm
[0045] In yet another embodiment, in a laser beam configuration, two laser beams or two laser spots rotate around a rotation axis, wherein a first laser beam or first laser spot rotates with a first radius around the rotation axis and the second laser beam or second laser spot rotates with a second radius around the rotation axis, wherein one of the radii is larger than the other, wherein the following conditions apply: 0,45 mm ≤ x df − x off + d f 2 ≤ 1,5 mm x df = 0,8 ∗ d f 0 < x off < x df 2
[0046] Where X off corresponds to the distance of the first laser beam from the rotation axis and therefore defines the eccentricity of the laser beams to each other.
[0047] In the aforementioned embodiments, it is advantageous if welding is carried out with a laser power between 2 and 10 kW, in particular 3 to 8 kW, preferably 4 to 7 kW.
[0048] It is also advantageous if the stirring effect η in mm -1< is between 4 and 30 mm -1<.
[0049] In a further embodiment, the welding speed v W is between 5 and 12 m / min, in particular 6 and 10 m / min.
[0050] The optimal process window for the stirring effect also depends on the welding speed v W .
[0051] Advantageously, the base material used is a steel which is a boron-manganese steel which can be hardened by an austenitizing and quenching process to a tensile strength of more than 900 MPa, and in particular a steel from the group of CMnB steels such as 22MnB5 or 20MnB8 is used.
[0052] It is particularly advantageous if the base material is a steel with the general alloy composition (in mass%) Carbon (C) 0,03-0,6 Manganese (Mn) 0,3-3,0 Aluminum (Al) 0,01-0,07 Silicon (Si) 0,01-0,8 Chromium (Cr) 0,02-0,6 Nickel (Ni) <0,5 Titanium (Ti) 0,01-0,08 Niobium (Nb) <0,1 Nitrogen (N) < 0,02 Boron (B) < 0,02 Phosphorus (P) < 0,01 Sulfur (S) < 0,01 Molybdenum (Mo) < 1
[0053] Rest iron and melting-related impurities are used.
[0054] Further advantageously, the base material can be a steel of the general alloy composition (in mass%) Carbon (C) 0,03-0,36 Manganese (Mn) 0,3-2,00 Aluminum (Al) 0,03-0,06 Silicon (Si) 0,01-0,20 Chromium (Cr) 0,02-0,4 Nickel (Ni) <0,5 Titanium (Ti) 0,03-0,04 Niobium (Nb) <0,1 Nitrogen (N) < 0,007 Boron (B) < 0,006 Phosphorus (P) < 0,01 Sulfur (S) < 0,01 Molybdenum (Mo) < 1
[0055] Rest iron and melting-related impurities are used.
[0056] The invention is explained by way of example with reference to a drawing. It shows: Figure 1: schematically shows the symmetrical, asymmetrical and orbital rotation of the welding laser beams; Figure 2: the process window according to the invention with regard to the stirring effect; Figure 3: the representation according to Figure 2with the significance of the outer regions; Figure 4: a table showing 16 different tests comparing embodiments according to the invention and those not according to the invention; Figure 5: a representation of a symmetrical stirring arrangement with the functions of the spot spacing and the spot diameter relative to one another; Figure 6: the process window for a symmetrical stirring arrangement; Figure 7: a schematic representation of an orbital stirring arrangement with the functions of the spot spacing and the spot diameter; Figure 8: the process window of the orbital stirring arrangement; Figure 9: the representation of an asymmetrical stirring arrangement with the functions of the spot spacing, the spot diameter, and the eccentricity; Figure 10: a hardened weld seam in a cross-section according to test V1 in the table; Figure 11: a cross-section according to test V2 in the table; Figure 12: a cross-section of the weld seam according to test V4 in the table;Figure 13: a weld seam in cross-section in micrograph according to test V16 in the table.
[0057] In Figure 1 Three different laser beam configurations are shown, which are in principle possible and can also be combined with each other. In the laser beam configurations shown, a symmetrical configuration ( Fig. 1a ), the laser beams are arranged symmetrically to a rotation axis and are rotated diametrically opposite each other around the rotation axis.
[0058] The symmetrical configuration can advantageously achieve the highest stirring efficiency. In an asymmetrical arrangement ( Fig. 1b ), one laser beam is positioned closer to the rotation axis than the other, creating eccentricity. The asymmetrical arrangement can advantageously influence the desired weld geometry.
[0059] In the orbital arrangement ( Fig. 1c) there is a central laser beam which is moved along a welding progress direction, while the second laser beam, which is distant from it, rotates around it and around the rotation axis.
[0060] The orbital arrangement can advantageously compensate for any differences in sheet thickness.
[0061] In Figure 5 the symmetrical stirring arrangement is shown in more detail.
[0062] In this laser beam configuration 1, two laser beams 2, 3 are present, each approximately equally spaced from an idealized weld pool center 4. The rotation axis 5, around which the two laser beams 2, 3 rotate according to the rotation directions 6, 7, is preferably located in the ideal weld pool center 4. Accordingly, exemplary subsequent positions 2', 3' offset by 90° are shown. The laser beams 2, 3, or their projection area (spot), have a given diameter df, corresponding to the expansion arrows 8, 9.
[0063] The two laser beams 2, 3, or their projection surfaces (spots), are each spaced apart from the center by the spot spacing X df. The theoretical weld pool width is therefore the spot spacing plus half a spot diameter. Welding progresses according to arrow 10, along the idealized weld pool center 4, at a welding progress speed v W.
[0064] In this configuration of a symmetric rotating arrangement, the spot diameter df is preferably within a range of 0.1 to 1 mm.
[0065] The distance between the spot centers, plus the spot diameter, is preferably between 0.5 mm and 3 mm, in particular 0.9 mm to 2.5 mm, whereby the spot distance x df preferably applies x df ≥ 0.8 * df .
[0066] A suitable process window for the symmetrical stirring arrangement, concerning the relationship between spot distance and diameter, can be seen in Figure 6 As already explained, the rule of thumb is that the spot diameter df is between 0.1 and 1 mm.
[0067] In a further advantageous laser beam configuration 11 ( Figure 7 ), two laser beams 2, 3 are arranged orbitally, which means that a first spot 2 remains on the welding axis 4 according to the welding progress direction 10, while a second spot 3 rotates about a rotation axis 5 which lies on the welding axis 4 and represents the center of the first spot 2.
[0068] The rotation of the second spot 3 takes place accordingly along the rotation direction 7, which is arranged in a certain radius around the rotation axis 5. The different positions of the second laser spot 3 are in Figure 7Shown as an example rotated by 180° with the position 3'. However, complete rotations are performed during welding along the welding progress 10.
[0069] The welding axis 4 is also the idealized weld pool center 4.
[0070] In this advantageous embodiment, the spot diameter is also between 0.1 and 1 mm, whereby 0,45 mm ≤ x df + d f 2 ≤ 1,5 mm .
[0071] Here too, x df = 0.8 * df is. In Figure 8 the process window applicable to the orbital stirring arrangement according to the framework conditions just mentioned is specified, wherein the function of the spot distance over the spot diameter is specified in the process window and the corresponding area according to the invention is located within the closed area.
[0072] In a further advantageous embodiment of a laser beam configuration 1 (shown in Figure 9), two laser spots 2, 3 rotate about a rotation axis 5, whereby, however, a first rotation direction 6 of a first laser beam 2 or first laser spot 2 is arranged closer to the rotation axis than the second rotation direction 7 of the second laser beam 3. The spot distance center is thus arranged away from the weld pool center 4 or offset therefrom.
[0073] In this advantageous embodiment, the spot diameter df is again between 0.1 and 1 mm, whereby the following condition is also observed: 0,45 mm ≤ x df − x off + d f 2 ≤ 1,5 mm x df = 0,8 ∗ d f 0 < x off < x df 2
[0074] In Figure 2 The process window according to the invention is shown with regard to the stirring effect. Figure 3 the respective effects when carrying out the process with unsuitable parameters, i.e. parameters that lie outside the process window.
[0075] Choosing too high a stirring effect in combination with a high welding speed can lead to humping (unstable welding process), increased occurrence of spatter and even laser weld seam breakthrough.
[0076] Surprisingly, even if the stirring effect is too low, the tendency to splash can increase significantly.
[0077] A laser welding speed (v W ) of less than 4 m / min is technically possible but no longer economically viable.
[0078] In the table according to Figure 4Sixteen welding tests are presented, with the welding tests being conducted at different welding progress rates, different stirring effects, and different power levels. After hardening, the welds were inspected and classified according to weld homogeneity and process stability. Nb stands for "not assessable," as no stable weld could be achieved in these tests.
[0079] In Figure 10 a weld seam structure after hardening is shown (example V1 from the table from Fig. 4) in which the parameters of the invention were not adhered to. The weld structure is visually inhomogeneous even after hardening, with the welding progress rate being 6 m per minute. The spot diameter is 0.3 mm, but with a spot spacing of 0, meaning that only a single laser was used. It is clear that a qualitatively satisfactory result cannot be achieved with this conventional process.
[0080] In Figure 11 is the result of an inventive design (Example Experiment 2 from the table in Fig. 4 ), with the surface being homogeneous after curing. The spot diameter here was 0.3 mm, and a symmetrical stirring arrangement with a spot spacing of 0.9 mm was used.
[0081] The laser power was 4.3 kW, and the welding progress rate was 6 m per minute. The stirring efficiency η was 4.125 mm -1< , where the stirring efficiency is the quotient of the rotation frequency and the welding speed or welding progress.
[0082] The distance of the spot center to the rotation axis was 0.45 mm, which means that the spots orbited the rotation axis on a radius.
[0083] In Figure 12 Test 4 is shown, which is not in accordance with the invention. While the spot diameter and spot spacing are within a range consistent with the invention, as is the welding progress rate, which at 6 m per minute corresponds to that of Test 2, and the distance from the spot center to the rotation axis is also the same, the stirring effect, as the quotient of the rotation frequency and welding progress rate, is too low, so that the ground section shows significant inhomogeneity after hardening.
[0084] In Figure 13 The result of test 16 according to the invention is shown. It can be seen that a homogeneous weld seam structure is present. The spot spacing is 0.4 mm with a spot diameter of 0.3 mm, and the progress rate was the same as in the other tests. The stirring effect η, at 4.125 mm -1<, is within the range of the invention, with the distance from the spot center to the rotation axis being 0.2 mm.
[0085] The advantage of the invention is that through a targeted selection of parameters and appropriate process control, reliably homogeneous weld seams can be achieved when welding aluminum-silicon coated sheets.
Claims
1. A method for welding coated steel sheets, particularly steel sheets that are coated with an aluminum-silicon metallic coating layer, wherein a configuration (1, 11, 12) of two laser beams (2, 3) is provided, wherein the laser beams act on a weld pool that is to be formed, wherein at least one laser beam (3) rotates around a rotation axis (5) so that the laser beams (2, 3) execute a movement relative to each other, wherein the laser beams (2, 3) are guided along a welding axis (4), wherein in order to achieve a mixing of the weld pool, a defined stirring effect and a defined welding speed in relation to each other are adhered to, wherein the following condition applies to the stirring effect: η = f rot v w where frot is the rotation frequency and vW is the welding speed and wherein the following conditions apply: 4 ≤ η ≤ 120 v w 1 mm and 4 ≤ v w ≤ 14 m min .
2. The method according to claim 1, characterized in that the laser beams (2, 3) are positioned symmetrically around a rotation axis (5) and rotate around the rotation axis (5) in diametrically opposed positions or one laser beam (2) is guided along a welding axis and the other laser beam (3) rotates around the first laser beam (2) or a first laser beam (2) rotates with a first smaller radius around the rotation axis (5) while the second laser beam (3) rotates with a larger radius around the rotation axis (5) or a mixture of these forms of movement.
3. The method according to one of the preceding claims, characterized in that with a symmetrical rotation of the laser beams (2, 3) or more precisely of their projected areas or spots, the laser beams (2, 3) are each spaced apart from the center by the spot spacing xdf, wherein the spot diameter or the diameter of the laser beam df is 0.1 mm to 1 mm, wherein the total coverage width of the laser beams (2, 3) is the sum of the spacing of the spot centers from each other plus one spot diameter, wherein the total is between 0.5 mm and 2.5 mm.
4. The method according to claim 3, characterized in that for the spot spacing xdf, the following condition applies: xdf ≥ 0.8 * df.
5. The method according to claim 2, characterized in that in a laser beam configuration (11), two laser beams (2, 3) are positioned orbitally, wherein a first laser beam (3) remains along the weld advancing direction (10) on a central axis of the weld pool, namely the welding axis (4), while the second laser beam (3) or second spot (3) rotates around a rotation axis (5), wherein the rotation axis (5) lies on the welding axis (4) or oscillates around the welding axis (4) and constitutes the center point of the first spot (2).
6. The method according to claim 5, characterized in that the spot diameter is between 0.1 and 1 mm, wherein the following conditions apply: x df ≥ 0.8 * d f and 0.45 mm ≤ x df + d f 2 ≤ 1.5 mm .
7. The method according to claim 2, characterized in that in a laser beam configuration (12), two laser beams (2, 3) or two laser spots (2, 3) rotate around a rotation axis (5), wherein a first laser beam (2) or first laser spot (2) rotates with a first radius around the rotation axis (5) and the second laser beam (3) or second laser spot (3) rotates with a second radius around the rotation axis (5), wherein one of the radii is greater than the other, wherein the following conditions apply: 0.45 mm ≤ x df − x off + d f 2 ≤ 1.5 mm x df ≥ 0.8 * d f 0 < x off < x df 2 8. The method according to one of the preceding claims, characterized in that the welding is performed with a laser power of between 2 and 10 kW, in particular from 3 to 8 kW, and preferably from 4 to 7 kW.
9. The method according to one of the preceding claims, characterized in that the stirring effect η in mm-1 is between 4 and 30 mm-1.
10. The method according to one of the preceding claims, characterized in that the welding speed vw is between 5 and 12 m / min, in particular between 6 and 10 m / min.
11. The method according to one of the preceding claims, characterized in that a steel that is a boron-manganese steel is used as the base material, which can be hardened by means of an austenitization and quenching process, particularly preferably to a tensile strength of greater than 900 MPa and in particular, a steel is used that belongs to the group of CMnB steels, for example a 22MnB5 or 20MnB8 steel.
12. The method according to one of the preceding claims, characterized in that a steel of the following general alloy composition (in % by mass) is used as the base material: carbon (C)0.03-0.6manganese (Mn)0.3-3.0aluminum (Al)0.01-0.07silicon (Si)0.01-0.8chromium (Cr)0.02-0.6nickel (Ni)< 0.5titanium (Ti)0.01-0.08niobium (Nb)< 0.1nitrogen (N)< 0.02boron (B)< 0.02phosphorus (P)< 0.01sulfur (S)< 0.01molybdenum (Mo)< 1 residual iron and smelting-related impurities.
13. The method according to one of the preceding claims, characterized in that a steel of the following general alloy composition (in % by mass) is used as the base material: carbon (C)0.03-0.36manganese (Mn)0.3-2.00aluminum (Al)0.03-0.06silicon (Si)0.01-0.20chromium (Cr)0.02-0.4nickel (Ni)< 0.5titanium (Ti)0.03-0.04niobium (Nb)< 0.1nitrogen (N)< 0.007boron (B)< 0.006phosphorus (P)< 0.01sulfur (S)< 0.01molybdenum (Mo)< 1 residual iron and smelting-related impurities.