Multilayer construction suitable for use as a reflector
Patent Information
- Application Number
- DE502021005276
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-30
- Filing Date
- 2021-11-25
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-11-25
AI Technical Summary
Current materials for high-temperature components like headlight reflectors face challenges in maintaining thermal stability, surface quality, and processability due to the trade-offs between thermal conductivity, thermal expansion coefficients, and surface roughness, especially when combining thermoplastics with metals, which limits their design complexity and recyclability.
A layer structure comprising a thermoplastic polycarbonate-based substrate layer with a specific composition of aromatic polycarbonate, expanded graphite, and fired silicon dioxide, combined with a metal layer, achieved through 1-component injection molding and dynamic tool temperature control, enabling improved thermal conductivity, surface quality, and thermal expansion matching that of metals.
This solution allows for the production of high-precision, thermally stable components with enhanced surface quality and design flexibility, suitable for complex geometries in headlight reflectors and mirror optics, while simplifying the structure compared to conventional multilayer hybrids and improving recyclability.
Description
[0001] The invention relates to a layered arrangement comprising a substrate layer and a metal layer, wherein the substrate layer has a high surface quality, minimized thermal expansion coefficients, and good thermal conductivity. The thermoplastic substrate layer consists of a polycarbonate-based composition.
[0002] Due to their high heat resistance, polycarbonate-based molding compounds, and especially copolycarbonate-based ones, are particularly well-suited for components exposed to high ambient temperatures and potential hot spots. Headlight reflectors and other headlight components, as well as mirror optics in head-up displays installed in car interiors, are exposed to high temperatures due to the heat radiated by the light source (e.g., LEDs due to semiconductors, xenon, halogen) or solar radiation. They must not alter their thermomechanical properties or shape in the process.
[0003] Temperature stability primarily refers to the property of a material not to undergo significant geometric changes when exposed to temperature changes (especially hot spots caused by solar radiation). In polymers, this property is achieved by adding large amounts of filler with a low thermal expansion coefficient.
[0004] However, the use of large amounts of filler in polycarbonate leads to a significant reduction in flow properties, which in turn imposes certain limitations on the material's processability. This is particularly problematic with regard to challenging component geometries (the transition from monolithic to multi-refractor designs with increasingly smaller functional units), such as substrate layers for headlight reflectors.
[0005] Since headlight reflectors are also components with very high quality requirements for the metal surface, the underlying substrate layer must also exhibit very high surface quality, measured by the roughness of the substrate surface and the associated gloss. Compared to unfilled polymers, a very high surface quality for filler-containing materials can only be ensured through a special processing technique, dynamic mold temperature control, as described in EP 2 785 794 A1. Different qualities can be achieved depending on the filler type and filler content.
[0006] The thermal expansion of a component and the associated stability of a light-optical projection, which is essential in reflectors and head-up displays, also depends on the material's intrinsic ability to distribute / dissipate heat. This property is practically nonexistent in pure polymers (insulators). Here, too, the thermal conductivity of the entire molding compound can be significantly improved by adding suitable fillers that themselves exhibit high thermal conductivity. However, the addition of such fillers in conventional compositions comes at the expense of the maximum achievable surface quality, even when using dynamic mold temperature control. Furthermore, the flow behavior of the polymer melt, measurable by the melt viscosity of the molding compound, as well as the ductility of the molded part, are significantly reduced, depending on the amount and type of filler.
[0007] Due to ever-increasing demands on the design and performance of automotive headlights, there is a trend towards multi-layer hybrid structures. Such structures comprise a layer or body made of a metallic material, e.g., aluminum or magnesium, which acts as a heat sink, a thermoplastic material with a high surface quality applied to it, and an additional reflective layer made of metal. When combining such materials, the thermoplastic material should have a thermal expansion coefficient similar to that of the metal in order to achieve as synchronous thermally induced warpage as possible and thus ensure permanent adhesion. Currently, this can only be achieved with highly filled thermoplastics, since metal, e.g., aluminum, has an expansion coefficient of < 30 ppm / K and pure thermoplastics have a thermal expansion coefficient of > 60 ppm / K.One possible replacement for such metal-thermoplastic hybrids would be a combination of two (identical or different) thermoplastics, where one material would have to exhibit very high thermal conductivity and thus act as a heat sink. The second material would be unfilled and would thus provide the necessary surface quality for the reflective layer.
[0008] Multilayer hybrid structures for producing molded parts such as reflectors or mirror elements are already known. EP3502306 A1 relates to a multilayer body which comprises I) a substrate layer (S), II) a metal layer (M) directly bonded thereto and III) optionally a protective layer (P) lying on the metal layer, wherein the substrate layer comprises a composition obtainable by mixing components A) to D), wherein A) is a polycarbonate, B) is an unsized talc, C) at least one anhydride-modified α-olefin polymer and optionally D) a part of the amount of component B) can be replaced by at least one further filler selected from the group consisting of an expanded graphite with a particle diameter D50 of less than 800 µm or a mixture of the aforementioned expanded graphite with unexpanded graphite and a boron nitride as a further filler, wherein in the case of graphite up to 8 wt.-parts of the amount of component B) can be replaced and wherein in the case of boron nitride up to 15 parts by weight of the amount of component B) can be replaced, wherein the amounts of components B) and C) before mixing with component C) are coordinated such that 0.10 to 1.4 parts by weight of component C) are used per 10 parts by weight of component B) and wherein the composition is free from graft polymers and polyesters.
[0009] The multilayer bodies are used to manufacture molded parts such as reflectors and (housing) components for light and heat sources and displays. Examples of molded parts include lamp sockets, lamp covers, light-collecting systems, collimators, vapor-deposited displays, vapor-deposited panes, lens mounts, light guide elements, LED bases, LED reflectors, heat sinks, cooling elements, solar reflectors, and automotive parts. Automotive parts are typically bezels, headlight housings, and indicators.
[0010] However, the inventors of the present application came up with another idea for a functionally alternative component that would be significantly more attractive both in terms of component manufacturing and later recyclability. If it were possible to identify a material that possesses both the necessary thermal conductivity for use as a heat sink and simultaneously offers the required surface quality of the surface material, novel reflectors could be manufactured using a single-component injection molding process with subsequent metallization.
[0011] The challenge, however, lies in the combination of all the aforementioned properties: Maximizing light stability is a key feature for greater road safety, particularly for high-precision light optics, which are now based on LED and laser technologies. The feasibility of more complex geometries and thus innovative designs, which requires corresponding flowability of the material, also places high demands on such a material. Furthermore, surfaces with high surface quality must be achievable. The task was therefore to provide appropriate layer arrangements, also called layer structures, that meet the aforementioned requirements and are simpler in structure than the conventional multilayer hybrid structures with their three essential core layers mentioned above.It has surprisingly been shown that, using certain thermoplastic compositions, it is possible to realize the product using 1-component injection molding technology with dynamic mold temperature control and subsequent metallization.
[0012] The invention thus relates to layer structures comprising i) a substrate layer made of a thermoplastic polycarbonate-based composition containing a) 44 to 63 wt.% aromatic polycarbonate, b) 3 to 8 wt.% expanded graphite, c) 34 to 38 wt.% calcined silicon dioxide, d) 0 to 10 wt.% one or more further additives, wherein the total amount of expanded graphite and calcined silicon dioxide is at least 40 wt.%, and ii) a metal layer applied to the substrate layer i.
[0013] The total amount of expanded graphite and calcined silicon dioxide according to components b and c, ie the sum of their individual amounts, is preferably at least 42 wt.%, more preferably at least 42.5 wt.%, particularly preferably at least 44 wt.%, most preferably at least 45 wt.%.
[0014] "Substrate layer made of a thermoplastic ... composition" means that the substrate layer consists of the composition or has a portion consisting of the composition. Preferably, the substrate layer consists of the composition.
[0015] "Layer structure" in the sense of the invention means a sequence of at least layers i and ii, i.e., two layers, and could also be referred to as a "multilayer structure." In principle, additional layers are also possible, although preferred layer structures according to the invention comprise only layers i and ii.
[0016] Preferred layer structures according to the invention are those in which the thermoplastic polycarbonate-based composition of the substrate layer i a) 54 to 60 wt.% aromatic polycarbonate, b) 5 to 7.5 wt.% expanded graphite, c) 35 to 37.5 wt.% calcined silicon dioxide, d) 0 to 5 wt.% one or more further additives.
[0017] Particularly preferred layer structures according to the invention comprise i) a substrate layer made of a thermoplastic polycarbonate-based composition and ii) a metal layer applied to the substrate layer i, wherein the thermoplastic polycarbonate-based composition of the substrate layer i consists of the following components: a) 54 to 60 wt.% aromatic polycarbonate, b) 5 to 7.5 wt.% expanded graphite, most preferably with a D(0.5) of the expanded graphite of 700 µm to 1200 µm, determined by sieve analysis according to DIN 51938:2015-09, c) 35 to 37.5 wt.% calcined silicon dioxide, most preferably with a D(0.5) of the calcined silicon dioxide of 3 µm to 5 µm, determined according to ISO 13320:2009-10, d) 0 to 5 wt.% one or more further additives, wherein the total amount of expanded graphite and calcined silicon dioxide at least 40 wt.%, in particular at least 42 wt.-%, wherein very particularly preferably at least one thermal stabilizer, at least one mold release agent and carbon black are contained as additives, wherein extremely preferably no further additives are contained. .
[0018] Layer structures according to the invention can be component elements for a wide variety of applications.
[0019] Such a layered structure is preferably part of a reflector or forms the reflector. This, together with a light source and possibly a frame and possibly a housing, such as a headlight housing, is part of a lighting device, wherein the reflector is arranged such that at least part of the light emitted by the light source is reflected by the reflector. An example of such a lighting device is a headlight, as used in motor vehicles, in particular as a headlight. According to the invention, the component is also preferably a mirror element of a head-up display. In a head-up display, such a mirror element has the purpose of projecting the desired image onto the windshield.
[0020] It is understood that one or more additional layers in addition to the substrate layer and the metal layer may be part of the layered structure. Such layers are, in particular, protective layers. A layered structure according to the invention preferably comprises no further layers besides the substrate layer, the metal layer, and one or more protective layers.
[0021] Preferred embodiments of the layered structures, particularly with regard to the thermoplastic polycarbonate-based composition, are described below. It is understood that preferred embodiments can be combined with one another unless otherwise stated.
[0022] The invention also relates to a method for producing the layer structures. This method comprises the steps of a) the substrate layer is formed from the thermoplastic polycarbonate-based composition described elsewhere in this application by means of one-component injection molding with dynamic mold temperature control and then b) a metal layer is applied to this substrate layer.
[0023] The metal layer acts as a reflective layer, at least partially reflecting light in the wavelength range from 380 nm to 750 nm. In the simplest case, the metal layer is fully reflective, similar to a mirror layer.
[0024] It can be, for example, an aluminum layer or a precious metal layer. The layer can be applied by chemical processes, particularly chemical vapor deposition (CVD) or electroplating, or by physical processes, particularly physical vapor deposition (PVD) or sputtering. The processes are described in more detail, for example, in "Vacuum Coating Vol. 1 to 5," H. Frey, VDI-Verlag, Düsseldorf, 1995, or in "Surface and Thin-Film Technology," Part 1, RA Haefer, Springer, Verlag 1987.
[0025] The reflective layer, i.e., the metal layer, of the layered structure according to the invention preferably has a thickness of ≥ 10 nm to ≤ 1000 nm, more preferably ≥ 50 nm to ≤ 800 nm, particularly preferably > 60 nm to < 500 nm, and most preferably > 60 nm to < 300 nm, determined by atomic force microscopy. This is the total thickness of the metal layer. If, for example, two layers of different metal are applied to one another, the thickness of the metal layer of the layered structure is the sum of the thicknesses of these two layers.
[0026] To achieve better metal adhesion and to clean the substrate surface, the surface to be coated can be subjected to plasma pretreatment. Plasma pretreatment can potentially alter the surface properties of polymers. These methods are described, for example, by Friedrich et al. in "Metallized plastics 5 & 6: Fundamental and applied aspects" and in H. Grünwald et al. "Surface and Coatings Technology, 111 (1999), 287-296." However, plasma pretreatment is not required to produce the layered structure according to the invention.
[0027] The metal layer preferably contains at least one element selected from Ag, Al, Au, Pt, Fe, Cr, Sn, In, Ti, Pd, Nb, Cu, V, stainless steel, or their alloys. The layer is preferably an aluminum, silver, gold, palladium, or copper layer, particularly preferably a silver or aluminum layer.
[0028] The metal layer covers the substrate layer completely or partially. If the metal layer only partially covers the substrate layer, at least 60%, preferably at least 70%, more preferably at least 80%, particularly preferably at least 90% of the substrate layer is covered by the metal layer.
[0029] To protect against oxidation or other damage, the metal layer can be provided with one or more additional layers, etc., which form the protective layer(s). For this purpose, the metal layer is preferably enclosed on one or both sides by one or more metal oxide or metal nitride layers, which enable the homogeneous deposition of metal and / or protect the metal as a protective layer - also called a sacrificial layer. Suitable oxides and / or nitrides are, in particular, aluminum oxide, titanium dioxide, silicon oxide SiO x , tantalum pentoxide TazO s, zirconium oxide, zirconium dioxide, niobium oxide, hafnium oxide, zinc tin oxide, indium tin oxide, aluminum zinc oxide, silicon nitride, boron nitride, or titanium nitride. However, these layers do not count as part of the metal layer.
[0030] Alternatively or additionally, other protective layers than metal oxide or metal nitride layers can also be considered. These protect the metal layer or metal-like layers from external influences, i.e. from corrosion or other external influences such as cleaning agents, scratches, etc. Such protective layers can be applied using a PECVD (plasma enhanced chemical vapor deposition) or plasma polymerization process. In this process, low-boiling precursors, in particular those based on siloxane, are vaporized in a plasma and thereby activated so that they can form a film. Typical substances used in this case are hexamethyldisiloxane (HMDSO), tetramethyldisiloxane, decamethylcyclopentasiloxane, octamethylcyclotetrasiloxane and trimethoxymethylsilane, with hexamethyldisiloxane being particularly preferred. The protective layer is most preferably a layer containing hexamethyldisiloxane (HMDSO).The total thickness of the protective layer is preferably a maximum of 100 nm, more preferably less than 100 nm and particularly preferably less than 50 nm, most preferably less than 35 nm.
[0031] Preferably, no further layer follows the protective layer(s) or the metal layer if no protective layer is present, which is a preferred embodiment for metal layers made of gold and / or platinum. The described protective layers are also generally not absolutely necessary for the layer structure according to the invention, so that in one embodiment, no protective layer is applied to the metal layer. Preferably, the layer structure according to the invention is a structure consisting only of layers i and ii. For use in applications such as reflectors, no heat sink element is required with the intended composition; rather, several functions are fulfilled solely by the multilayer structure according to the invention.
[0032] Various modifications can be made to the above-mentioned layer structure. For example, two layers of silver can be used, or different layer thicknesses can be used.
[0033] The layered structure can be planar and thus serve as a simple mirror. According to another embodiment, however, the layered structure is not planar. In this case, the layered structure can act as a converging or diverging mirror. The layered structure can, for example, be designed as a paraboloid of revolution.
[0034] Applications of the layered structure according to the invention include headlight reflectors, but also, for example, mirror optics in head-up displays. Headlight reflectors or mirror optics in head-up displays comprising a layered structure according to the invention are thus also the subject of the present invention. Thermoplastic substrate layer
[0035] The components of the thermoplastic composition of the substrate layer are described below. It is understood that the weight percentages refer to the total weight of the respective composition.
[0036] Furthermore, it is understood that the components used may contain common impurities, for example, resulting from their manufacturing process. It is preferable to use components that are as pure as possible. It is also understood that these impurities may also be present in a closed formulation of the composition. They then contribute to the respective weight fraction of the component from which they originate and must be included in this calculation. Component a
[0037] Component a of the compositions are aromatic polycarbonates.
[0038] Aromatic polycarbonates within the meaning of the present invention include both homopolycarbonates and copolycarbonates and / or polyestercarbonates; the polycarbonates can be linear or branched in a known manner. Mixtures of polycarbonates can also be used according to the invention.
[0039] The thermoplastic polycarbonates preferably have weight-average molecular weights M w of 15,000 g / mol to 40,000 g / mol, more preferably up to 34,000 g / mol, particularly preferably from 17,000 g / mol to 33,000 g / mol, in particular from 19,000 g / mol to 32,000 g / mol, determined by gel permeation chromatography, calibrated against bisphenol A polycarbonate standards using dichloromethane as the eluent, calibration with linear polycarbonates (from bisphenol A and phosgene) of known molar mass distribution from PSS Polymer Standards Service GmbH, Germany, calibration according to method 2301-0257502-09D (from 2009 in German) from Currenta GmbH & Co. OHG, Leverkusen. The eluent is dichloromethane. Column combination made of cross-linked styrene-divinylbenzene resins. Analytical column diameter: 7.5 mm; length: 300 mm. Column material particle sizes: 3 µm to 20 µm. Solution concentration: 0.2 wt.%.Flow rate: 1.0 ml / min, solution temperature: 30°C. Use of UV and / or RI detection.
[0040] A portion, up to 80 mol%, preferably from 20 mol% to 50 mol%, of the carbonate groups in the polycarbonates used according to the invention can be replaced by aromatic dicarboxylic acid ester groups. Such polycarbonates, which contain both carbonic acid residues and acid residues of aromatic dicarboxylic acids incorporated into the molecular chain, are referred to as aromatic polyester carbonates. For the purposes of the present invention, they are subsumed under the generic term of thermoplastic aromatic polycarbonates.
[0041] The polycarbonates are produced in a known manner from dihydroxyaryl compounds, carbonic acid derivatives, optionally chain terminators and optionally branching agents, whereby to produce the polyester carbonates, some of the carbonic acid derivatives are replaced by aromatic dicarboxylic acids or derivatives of dicarboxylic acids, depending on the carbonate structural units to be replaced in the aromatic polycarbonates by aromatic dicarboxylic acid ester structural units.
[0042] Dihydroxyaryl compounds suitable for the production of polycarbonates are those of the formula (1) HO-Z-OH (1), in which Zein aromatic radical having 6 to 30 C atoms, which may contain one or more aromatic nuclei, may be substituted and may contain aliphatic or cycloaliphatic radicals or alkylaryls or heteroatoms as bridge members.
[0043] Preferably, Z in formula (1) represents a radical of formula (2) in the R 6< and R 7< independently of one another represent H, C 1 - to C 18 -alkyl-, C 1 - to C 18 -alkoxy, halogen such as Cl or Br or represent in each case optionally substituted aryl- or aralkyl, preferably H or C 1 - to C 12 -alkyl, particularly preferably H or C 1 - to C 8 -alkyl and very particularly preferably H or methyl, and X represents a single bond, -SO 2 -, -CO-, -O-, -S-, C 1 - to C 6 -alkylene, C 2 - to C 5 -alkylidene or C 5 - to C 6 -cycloalkylidene, which may be substituted by C 1 - to C 6 -alkyl, preferably methyl or ethyl, and furthermore represents C 6 - to C 12 -arylene, which may optionally be condensed with further aromatic rings containing heteroatoms.
[0044] Preferably, X represents a single bond, C 1 - to C 5 -alkylene, C 2 - to C 5 -alkylidene, C 5 - to C 6 -cycloalkylidene, -O-, -SO-, -CO-, -S-, -SO 2 - or a radical of the formula (3)
[0045] Examples of dihydroxyaryl compounds are: dihydroxybenzenes, dihydroxydiphenyls, bis-(hydroxyphenyl)-alkanes, bis-(hydroxyphenyl)-cycloalkanes, bis-(hydroxyphenyl)-aryls, bis-(hydroxyphenyl)-ethers, bis-(hydroxyphenyl)-ketones, bis-(hydroxyphenyl)-sulfides, bis-(hydroxyphenyl)-sulfones, bis-(hydroxyphenyl)-sulfoxides, 1,1'-bis-(hydroxyphenyl)-diisopropylbenzenes and their nuclear alkylated and nuclear halogenated compounds.
[0046] Dihydroxyaryl compounds suitable for the production of the polycarbonates and copolycarbonates to be used according to the invention include, for example, hydroquinone, resorcinol, dihydroxydiphenyl, bis(hydroxyphenyl)alkanes, bis(hydroxyphenyl)cycloalkanes, bis(hydroxyphenyl) sulfides, bis(hydroxyphenyl) ethers, bis(hydroxyphenyl) ketones, bis(hydroxyphenyl) sulfones, bis(hydroxyphenyl) sulfoxides, α,α'-bis(hydroxyphenyl)diisopropylbenzenes, and their alkylated, nuclear-alkylated, and nuclear-halogenated compounds. Si-containing telechelics can also be used to produce copolycarbonates, yielding so-called Si copolycarbonates.
[0047] Preferred dihydroxyaryl compounds are 4,4'-dihydroxydiphenyl, 2,2-bis-(4-hydroxyphenyl)-1-phenylpropane, 1,1-bis-(4-hydroxyphenyl)-phenylethane, 2,2-bis-(4-hydroxyphenyl)propane, 2,4-bis-(4-hydroxyphenyl)-2-methylbutane, 1,3-Bis-[2-(4-hydroxyphenyl)-2-propyl]benzene (Bisphenol M), 2,2-Bis-(3-methyl-4-hydroxyphenyl)-propane, Bis-(3,5-dimethyl-4-hydroxyphenyl)-methane, 2,2-Bis-(3,5-dimethyl-4-hydroxyphenyl)-propne, Bis-(3,5-dimethyl-4-hydroxyphenyl)-sulfone, 2,4-Bis-(3,5-dimethyl-4-hydroxyphenyl)-2-methylbutane, 1,3-bis-[2-(3,5-dimethyl-4-hydroxyphenyl)-2-propyl]-benzene and 1,1-bis-(4-hydroxyphenyl)-3,3,5-triamethylcyclohexane (bisphenol TMC) as well as the bisphenols of formulas (I) to (III) in which R' is in each case a C 1 to C 4 alkyl radical, aralkyl radical or aryl radical, preferably a methyl radical or phenyl radical, very particularly preferably a methyl radical.
[0048] Particularly preferred dihydroxyaryl compounds are 4,4'-dihydroxydiphenyl, 1,1-bis-(4-hydroxyphenyl)-phenyl-ethane, 2,2-bis-(4-hydroxyphenyl)-propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)-propane, 1,1-bis-(4-hydroxyphenyl)-cyclohexane and 1,1-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (bisphenol TMC) as well as the dihydroxyaryl compounds of the formulas (I), (II) and / or (III).
[0049] These and other suitable dihydroxyaryl compounds are described, for example, in US 2 999 835 A, 3 148 172 A, 2 991 273 A, 3 271 367 A, 4 982 014 A and 2 999 846 A, in German Offenlegungsschriften 1 570 703 A, 2 063 050 A, 2 036 052 A, 2 211 956 A and 3 832 396 A, in French patent specification 1 561 518 A1, in the monograph "H. Schnell, Chemistry and Physics of Polycarbonates, Interscience Publishers, New York 1964, p. 28 ff.; p. 102 ff.", and in "DG Legrand, JT Bendler, Handbook of Polycarbonate Science and Technology, Marcel Dekker New York 2000, p. 72ff."
[0050] In the case of homopolycarbonates, only one dihydroxyaryl compound is used; in the case of copolycarbonates, two or more dihydroxyaryl compounds are used.
[0051] Particularly preferred polycarbonates are the homopolycarbonate based on bisphenol A, the homopolycarbonate based on 1,1-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane and the copolycarbonates based on the two monomers bisphenol A and 1,1-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane or the two monomers bisphenol A and 4,4'-dihydroxydiphenyl, as well as the dihydroxyaryl compounds of the formulas (I), (II) and / or (III) in which R' is each C 1 - to C 4 -alkyl, aralkyl or aryl, preferably methyl or phenyl, most preferably methyl, derived homo- or copolycarbonates, in particular with bisphenol A.
[0052] The total proportion of the monomer units based on the formulas (I), (II), (III), 4,4'-dihydroxydiphenyl and / or bisphenol TMC in the copolycarbonate is preferably 0.1 - 88 mol%, particularly preferably 1 - 86 mol%, very particularly preferably 5 - 84 mol% and in particular 10 - 82 mol% (based on the sum of the moles of dihydroxyaryl compounds used).
[0053] The dihydroxyaryl compounds used, as well as all other chemicals and auxiliaries added to the synthesis, may be contaminated with impurities arising from their own synthesis, handling, and storage. However, it is desirable to work with raw materials that are as pure as possible.
[0054] The copolycarbonates can be present as block and random copolycarbonates. Random copolycarbonates are particularly preferred.
[0055] The ratio of the frequency of the diphenolate monomer units in the copolycarbonate results from the molar ratio of the dihydroxyaryl compounds used.
[0056] The relative solution viscosity of the copolycarbonates, determined according to ISO 1628-4:1999, is preferably in the range of 1.15 - 1.35.
[0057] The monofunctional chain terminators required to regulate the molecular weight, such as phenols or alkylphenols, in particular phenol, p-tert-butylphenol, iso-octylphenol, cumylphenol, their chlorocarbonic acid esters or acid chlorides of monocarboxylic acids or mixtures of these chain terminators, are either added to the reaction with the bisphenolate or the bisphenolates or added at any time during the synthesis as long as phosgene or chlorocarbonic acid end groups are still present in the reaction mixture, or in the case of the acid chlorides and chlorocarbonic acid esters as chain terminators as long as sufficient phenolic end groups of the polymer being formed are available.
[0058] Preferably, however, the chain terminator(s) are added after the phosgenation at a place or at a time when no more phosgene is present but the catalyst has not yet been added, or they are added before the catalyst, together with the catalyst or in parallel.
[0059] Any branching agents or branching agent mixtures that may be used are added to the synthesis in the same way, but usually before the chain terminators. Typically, trisphenols, quaternphenols, or acid chlorides of tri- or tetracarboxylic acids are used, or mixtures of polyphenols or acid chlorides.
[0060] Some of the compounds which can be used as branching agents and which have three or more than three phenolic hydroxyl groups are, for example, phloroglucinol, 4,6-dimethyl-2,4,6-tri-(4-hydroxyphenyl)-2-heptene, 4,6-dimethyl-2,4,6-tri-(4-hydroxyphenyl)-heptane, 1,3,5-tris-(4-hydroxyphenyl)-benzene, 1,1,1-tri-(4-hydroxyphenyl)-ethane, tris-(4-hydroxyphenyl)-phenylmethane, 2,2-bis-[4,4-bis-(4-hydroxyphenyl)-cyclohexyl]-propane, 2,4-bis-(4-hydroxyphenyl-isopropyl)-phenol, tetra-(4-hydroxyphenyl)-methane.
[0061] Some of the other trifunctional compounds are 2,4-dihydroxybenzoic acid, trimesic acid, cyanuric chloride and 3,3-bis-(3-methyl-4-hydroxyphenyl)-2-oxo-2,3-dihydroindole.
[0062] Preferred branching agents are 3,3-bis-(3-methyl-4-hydroxyphenyl)-2-oxo-2,3-dihydroindole and 1,1,1-tri-(4-hydroxyphenyl)ethane.
[0063] The amount of branching agents to be used, if necessary, is 0.05 mol% to 2 mol%, again based on the moles of diphenols used.
[0064] The branching agents can either be added together with the diphenols and the chain terminators in the aqueous alkaline phase or dissolved in an organic solvent before phosgenation.
[0065] All of these measures for producing polycarbonates are familiar to the person skilled in the art.
[0066] Aromatic dicarboxylic acids suitable for the production of polyester carbonates are, for example, orthophthalic acid, terephthalic acid, isophthalic acid, tert-butylisophthalic acid, 3,3'-diphenyldicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4-benzophenonedicarboxylic acid, 3,4'-benzophenonedicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 2,2-bis-(4-carboxyphenyl)-propane, trimethyl-3-phenylindane-4,5'-dicarboxylic acid.
[0067] Of the aromatic dicarboxylic acids, terephthalic acid and / or isophthalic acid are particularly preferred.
[0068] Derivatives of dicarboxylic acids are the dicarboxylic acid dihalides and the dicarboxylic acid dialkyl esters, in particular the dicarboxylic acid dichlorides and the dicarboxylic acid dimethyl esters.
[0069] The replacement of the carbonate groups by the aromatic dicarboxylic acid ester groups occurs essentially stoichiometrically and quantitatively, so that the molar ratio of the reactants is also reflected in the finished polyester carbonate. The incorporation of the aromatic dicarboxylic acid ester groups can occur both randomly and blockwise.
[0070] Preferred methods of producing the polycarbonates to be used according to the invention, including the polyester carbonates, are the known interfacial process and the known melt transesterification process (cf., for example, WO 2004 / 063249 A1, WO 2001 / 05866 A1, US 5,340,905 A, US 5,097,002 A, US-A 5,717,057 A).
[0071] In the former case, the acid derivatives used are preferably phosgene and optionally dicarboxylic acid dichlorides; in the latter case, diphenyl carbonate and optionally dicarboxylic acid diesters are preferred. Catalysts, solvents, workup, reaction conditions, etc., for polycarbonate or polyester carbonate production are sufficiently described and known in both cases.
[0072] Also preferred are copolycarbonates for the preparation of which diphenols of the general formula (1a) were used: where R 5< represents hydrogen or C 1 to C 4 alkyl, C 1 to C 3 alkoxy, preferably hydrogen; Methoxy or methyl, R 6< , R 7< , R 8< and R 9< each independently of one another represent C 1 - to C 4 -alkyl or C 6 - to C 12 -aryl, preferably methyl or phenyl, Y represents a single bond, SO 2 -, -S-, -CO-, -O-, C 1 - to C 6 -alkylene, C 2 - to C 5 -alkylidene, C 6 - to C 12 -arylene, which may optionally be condensed with further aromatic rings containing heteroatoms or represents a C 5 - to C 6 -cycloalkylidene radical which may be mono- or polysubstituted by C 1 - to C 4 -alkyl, preferably a single bond, -O-, isopropylidene or represents a C 5 - to C 6 -cycloalkylidene radical which may be mono- or polysubstituted by C 1 - to C 4 -alkyl, V represents oxygen, C 2 - to C 6 -alkylene or C 3 - to C 6 -alkylidene, preferably oxygen or C 3 -alkylene, p, q and r each independently represent 0 or 1 when q = 0,W stands for a single bond when q = 1 and r = 0, W stands for oxygen, C 2 - to C 6 -alkylene or C 3 - to C 6 -alkylidene, preferably oxygen or C 3 -alkylene when q = 1 and r = 1, W and V each independently stand for C 2 - to C 6 -alkylene or C 3 - to C 6 -alkylidene, preferably C 3 -alkylene, Z stands for a C 1 - to C 6 -alkylene, preferably C 2 -alkylene, o stands for an average number of repeating units of 10 to 500, preferably 10 to 100, and m stands for an average number of repeating units of 1 to 10, preferably 1 to 6, more preferably 1.5 to 5. It is also possible to use diphenols in which two or more siloxane blocks of the general formula (1a) are linked to one another via terephthalic acid and / or isophthalic acid to form ester groups.
[0073] Particularly preferred are (poly)siloxanes of the formulas (2) and (3) where R1 is hydrogen, C1 to C4 alkyl, preferably hydrogen or methyl and particularly preferably hydrogen, R2 independently of one another is aryl or alkyl, preferably methyl, X is a single bond, -SO2-, -CO-, -O-, -S-, C1 to C6 alkylene, C2 to C5 alkylidene or C6 to C12 arylene, which may optionally be condensed with further aromatic rings containing heteroatoms, X is preferably a single bond, C1 to C5 alkylene, C2 to C5 alkylidene, C5 to C12 cycloalkylidene, -O-, -SO- -CO-, -S-, -SO2-, particularly preferably X is a single bond, isopropylidene, C5 to C12 cycloalkylidene or oxygen, and very particularly preferably isopropylidene, n is an average number from 10 to 400, preferably 10 and 100, particularly preferably 15 to 50 and m is an average number from 1 to 10, preferably from 1 to 6 and particularly preferably from 1.5 to 5..
[0074] Likewise preferably, the siloxane block can be derived from the following structure or where a in formula (IV), (V) and (VI) represents an average number from 10 to 400, preferably 10 to 100 and particularly preferably 15 to 50.
[0075] It is also preferred that at least two identical or different siloxane blocks of the general formulas (IV), (V) or (VI) are linked to one another via terephthalic acid and / or isophthalic acid to form ester groups.
[0076] It is also preferred if in formula (1a) p = 0, V is C 3 -alkylene, r = 1, Z is C 2 -alkylene, R 8< and R 9< are methyl, q = 1, W is C 3 -alkylene, m = 1, R 5< is hydrogen or C 1 - to C 4 -alkyl, preferably hydrogen or methyl, R 6< and R 7< each independently of one another are C 1 - to C 4 -alkyl, preferably methyl and o is 10 to 500.
[0077] Copolycarbonates with monomer units of formula (1a) and in particular their preparation are described in WO 2015 / 052106 A2.
[0078] Copolycarbonates with monomer units of formula (IV) and in particular their preparation are described in WO 2015 / 052106 A2.
[0079] Compositions within the meaning of the invention are "polycarbonate-based compositions." These are compositions whose base material, i.e., predominantly present component, is a polycarbonate. "Predominantly" here means at least 44 wt. %, preferably at least 50 wt. %, more preferably at least 54 wt. %, particularly preferably up to 60 wt. %, aromatic polycarbonate, based on the total composition. Component b
[0080] Expanded graphite is used as component b of the thermoplastic compositions of the substrate layer of the multilayer structure. The graphite used can be one type of expanded graphite, but also a mixture of two or more types.
[0081] In expanded graphites, the individual basal planes of the graphite are pushed apart by a special treatment, resulting in an increase in the volume of the graphite, preferably by a factor of 200 to 400. The production of expanded graphites is described, among others, in US 1,137,373 A, US 1,191,383 A, and US 3,404,061 A.
[0082] Graphites are used in the compositions in the form of fibers, rods, spheres, hollow spheres, platelets, in powder form, both in aggregated and agglomerated form, preferably in platelet form.
[0083] In the present invention, a platelet-shaped structure refers to a particle with a flat geometry. Thus, the height of the particles is usually significantly smaller than their width or length. Such flat particles can, in turn, be agglomerated or aggregated into structures.
[0084] The height of the platelet-shaped primary particles, determined by atomic force microscopy (AFM), is less than 500 nm, preferably less than 200 nm, and particularly preferably less than 100 nm. Due to the small size of these primary particles, the shape of the particles can be bent, curved, wavy, or otherwise deformed.
[0085] The length dimensions of the particles can be determined using standard methods, such as electron microscopy.
[0086] Graphite is used in the thermoplastic compositions according to the invention in amounts of 3.0 to 8.0 wt.%, preferably 5.0 to 7.5 wt.%, in order to obtain good thermal conductivity of the thermoplastic compositions.
[0087] According to the invention, graphite with a relatively high specific surface area, determined as the BET surface area by nitrogen adsorption according to ASTM D3037:1993, is preferably used. Graphites with a BET surface area of ≥ 5 m 2 / g, particularly preferably ≥ 10 m 2 / g, and most preferably ≥ 18 m 2 / g are preferably used in the thermoplastic compositions.
[0088] The graphites preferably have a particle size distribution, determined by sieve analysis according to DIN 51938:2015-09, which is characterized by the D(0.5), of at least 400 µm, more preferably of at least 600 µm, even more preferably of at least 650 µm to 1300 µm, and particularly preferably of at least 700 µm to 1200 µm, most preferably of 720 µm to <1200 µm. In one embodiment, a particle size distribution with a D(0.5) of the expanded graphite of <1000 µm is preferred.
[0089] Preferably, at least the ranges for D(0.5) apply to the graphite used. More preferably, the following preferred ranges for D(0.1) and D(0.9) also apply, either alternatively or particularly preferably additively together: The graphites preferably have a particle size distribution, determined by sieve analysis according to DIN 51938:2015-09, which is characterized by a D(0.9), of at least 1 mm, preferably of at least 1.2 mm, more preferably of at least 1.4 mm, and even more preferably of at least 1.5 mm.
[0090] The graphites also preferably have a particle size distribution, determined by sieve analysis according to DIN 51938:2015-09, which is characterized by a D(0,1), of at least 100 µm, preferably of at least 150 µm, more preferably of at least 200 µm and even more preferably of at least 250 µm,
[0091] The graphites used preferably have a density, determined with xylene, in the range from 2.0 g / cm 3< to 2.4 g / cm 3< , preferably from 2.1 g / cm 3< to 2.3 g / cm 3< and more preferably from 2.2 g / cm 3< to 2.27 g / cm 3< .
[0092] The carbon content of the graphites used in the layer structures according to the invention, determined according to DIN 51903:2012-11 at 800 °C for 20 hours, is preferably ≥ 90%, more preferably ≥ 95% and even more preferably ≥ 98%.
[0093] The residual moisture content of the graphites used in the layer structures according to the invention, determined according to DIN 51904:2012-11 at 110 °C for 8 hours, is preferably ≤ 5%, more preferably ≤ 3% and even more preferably ≤ 2%.
[0094] The thermal conductivity of the graphites used in the layer structures according to the invention is between 250 and 400 W / (m*K) parallel to the basal planes and between 6 and 8 W(m*K) perpendicular to the basal planes before processing.
[0095] The electrical resistance of the graphites used in the layer structures according to the invention is approximately 0.001 Ω*cm parallel to the basal planes before processing and is less than 0.1 Ω*cm perpendicular to the basal planes.
[0096] The bulk density of the graphite, determined according to DIN 51705:2001-06, is usually between 50 g / l and 250 g / l, preferably between 65 g / l and 220 g / l and more preferably between 100 g / l and 200 g / l.
[0097] Graphites having a sulfur content of less than 200 ppm are preferably used in the thermoplastic compositions of the layer structures according to the invention.
[0098] Preferably, graphites are used in the thermoplastic compositions of the layer structures according to the invention which have a leachable chlorine ion content of less than 100 ppm.
[0099] Graphites which have a nitrate and nitrite content of less than 50 ppm are also preferably used in the thermoplastic compositions of the layer structures according to the invention.
[0100] Particularly preferred graphites are those which meet all of these limit values, ie for the sulfur, chlorine ion, nitrate and nitrite content.
[0101] Commercially available graphites include Ecophit GFG 5, Ecophit GFG 50, Ecophit GFG 200, Ecophit GFG 350, Ecophit GFG 500, Ecophit GFG 900, Ecophit GFG 1200 from SGL Carbon GmbH, TIMREX BNB90, TIMREX KS5-44, TIMREX KS6, TIMREX KS150, TIMREX SFG44, TIMREX SFG150, TIMREX C-THERM ™< 001 and TIMREX C-THERM ™< 011 from TIMCAL Ltd., SC 20 O, SC 4000 O / SM and SC 8000 O / SM from Graphit Kropfmühl AG, Mechano-Cond 1, Mechano-Lube 2 and Mechano-Lube 4G from HC Carbon GmbH, Nord-Min 251 and Nord-Min 560T from Nordmann Rassmann GmbH and ASBURY A99, Asbury 230U and Asbury 3806 from Asbury Carbons. Component c
[0102] Compositions suitable for use in the layer structure according to the invention contain fused silica as component c. Fused silica is quartz glass, fused and resolidified silica. It can be fused silica made from naturally occurring or synthetically produced quartz, or a mixture of both.
[0103] Component c is preferably quartz material produced from processed quartz sand by iron-free grinding followed by air separation.
[0104] Component c is present in the compositions in an amount of 34 to 38 wt.%, preferably 35 to 37.5 wt.%.
[0105] The silicon dioxide used in the compositions of the substrate layer preferably has a spherical and / or approximately spherical grain shape. Approximately spherical means the following: If the sphere is described by axes of equal length emanating from a common origin and directed into space, with the axes defining the radius of the sphere in all spatial directions, a deviation of up to 20% in the axial lengths of the spherical particles from the ideal state of the sphere is possible in order to still be considered approximately spherical.
[0106] The calcined silicon dioxide is preferably characterized by an average diameter d(0.5), determined according to ISO 13320:2009-10, of 2 to 10 µm, more preferably of 2.5 to 8.0 µm, even more preferably of 3 to 5 µm, wherein an upper diameter d(0.9), determined according to ISO 13320:2009, of 6 to 34 µm is preferred, more preferably of 6.5 to 25.0 µm, even more preferably of 7 to 15 µm, and particularly preferably of 10 µm,
[0107] Preferably, the calcined silica has a BET specific surface area, determined by nitrogen adsorption according to ISO 9277:2010-09, of 0.4 to 8.0 m 2 / g, more preferably of 2 to 7 m 2 / g, and most preferably of 4.4 to 6 m 2 / g.
[0108] Even more preferred calcined silicon dioxide has only a maximum of 3 wt.% secondary components, wherein preferably the content of Al 2 O 3 < 2.0 wt.%, Fe 2 O 3 < 0.05 wt.%, (CaO + MgO) < 0.1 wt.%, (Na2O + K2O) < 0.1 wt.%, in each case based on the total weight of the calcined silicon dioxide.
[0109] Preferably, calcined silicon dioxide having a pH value, measured according to ISO 10390:2005 in aqueous suspension, in the range 6 to 9, more preferably 6.5 to 8.0, is used.
[0110] The silicon dioxide preferably has an oil absorption number according to DIN EN ISO 787-5:1995-10 of preferably 20 to 30 g / 100 g.
[0111] Fumed silicon dioxide with a surface coating can be used, with epoxy-modified, polyurethane-modified, and unmodified silane compounds, methylsiloxane, and methacrylsilane coatings, or mixtures of the aforementioned silane compounds being preferred. An epoxysilane coating is particularly preferred. The coating of silicon dioxide is carried out according to general methods known to those skilled in the art.
[0112] However, the silicon dioxide used for compositions according to the invention preferably does not contain any size.
[0113] It is understood that calcined silicon dioxide having the properties described as preferred can form component c alone or in a mixture with one or more other calcined silicon dioxides. Component c is preferably a calcined silicon dioxide having one or more of the properties described as preferred. Component d
[0114] In addition, further additives are optionally included, up to 10 wt.%, preferably up to 6 wt.%, more preferably up to 5 wt.%, even more preferably 0.1 to 0.7 wt.%, wherein these weight percentages, here as elsewhere, relate to the total weight of the composition.
[0115] The group of other additives does not include expanded graphite and calcined silicon dioxide, as these are already described as components b and c.
[0116] Such additives, as are usually added to polycarbonate-containing compositions, are, for example, thermal stabilizers, antistatic agents, UV absorbers, IR absorbers, flame retardants, anti-drip agents, impact modifiers, antioxidants, inorganic pigments, carbon black, colorants and / or inorganic fillers such as titanium dioxide, silicates, aluminum silicates, talc, chalk, quartz powder, wollastonite, mica / clay layers, montmorillonite, aluminum oxide, magnesium oxide, silicon dioxide (unfired) and / or barium sulfate and / or mold release agents, as described, for example, in EP 0 839 623 A1, WO 96 / 15102 A2, EP 0 500 496 A1 or in the "Plastics Additives Handbook", Hans Zweifel, 5th Edition 2000, Hanser Verlag, Munich, in the amounts customary for polycarbonate. These additives can be added individually or in a mixture.
[0117] Phosphorus-based stabilizers selected from the group of phosphates, phosphites, phosphonites, phosphines, and mixtures thereof are particularly suitable as thermal stabilizers. Mixtures of different compounds from one of these subgroups, e.g., two phosphites, can also be used.
[0118] Phosphorus compounds with the oxidation number +III, in particular phosphines and / or phosphites, are preferably used as thermal stabilizers.
[0119] Particularly preferred thermal stabilizers are triphenylphosphine, tris-(2,4-di-tert-butylphenyl)phosphite (Irgafos 168), tetrakis-(2,4-di-tert-butylphenyl)-[1,1-biphenyl]-4,4'-diylbisphosphonite, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (Irganox 1076), bis-(2,4-dicumylphenyl)-pentaerythritol diphosphite (Doverphos S-9228), bis-(2,6-di-tert-butyl-4-methylphenyl)-pentaerythritol diphosphite (ADK STAB PEP-36).
[0120] They are used alone or in a mixture, e.g., Irganox B900 (a mixture of Irgafos 168 and Irganox 1076 in a ratio of 4:1) or Doverphos S-9228 with Irganox B900 or Irganox 1076.
[0121] The thermal stabilizers are preferably used in amounts of up to 1.0 wt.%, more preferably 0.003 wt.% to 1.0 wt.%, even more preferably 0.005 wt.% to 0.5 wt.%, particularly preferably 0.01 wt.% to 0.3 wt.%.
[0122] Preferred mold release agents are esters of aliphatic long-chain carboxylic acids with mono- or polyvalent aliphatic and / or aromatic hydroxy compounds. Particularly preferred are pentaerythritol tetrastearate, glycerol monostearate, stearyl stearate, and propanediol distearate, or mixtures thereof.
[0123] Preferred UV absorbers have the lowest possible transmission below 400 nm and the highest possible transmission above 400 nm. Ultraviolet absorbers particularly suitable for use in the composition according to the invention are benzotriazoles, triazines, benzophenones, and / or arylated cyanoacrylates.
[0124] Particularly suitable ultraviolet absorbers are hydroxybenzotriazoles, such as 2-(3',5'-bis-(1,1-dimethylbenzyl)-2'-hydroxy-phenyl)-benzotriazole (Tinuvin 234, Ciba Specialty Chemicals, Basel), 2-(2'-hydroxy-5'-(tert.-octyl)-phenyl)-benzotriazole (Tinuvin 329, Ciba Specialty Chemicals, Basel), 2-(2'-hydroxy-3'-(2-butyl)-5'-(tert.butyl)-phenyl)-benzotriazole (Tinuvin 350, Ciba Specialty Chemicals, Basel), bis-(3-(2H-benzotriazolyl)-2-hydroxy-5-tert.-octyl)methane, (Tinuvin ®< 360, Ciba Specialty Chemicals, Basel), (2-(4,6-Diphenyl-1,3,5-triazin-2-yl)-5-(hexyloxy)-phenol (Tinuvin 1577, Ciba Specialty Chemicals, Basel), as well as the benzophenones 2,4-Dihydroxybenzophenone (Chimasorb 22, Ciba Specialty Chemicals, Basel) and 2-Hydroxy-4-(octyloxy)-benzophenone (Chimassorb 81, Ciba, Basel), 2-Cyano-3,3-diphenyl-2-propenoic acid 2-ethylhexyl ester, 2,2-Bis[[(2-cyano-1-oxo-3,3-diphenyl-2-propenyl)oxy]-methyl]-1,3-propanediyl ester (9CI) (Uvinul 3030, BASF AG Ludwigshafen), 2-[2-Hydroxy-4-(2-ethylhexyl)oxy]phenyl-4,6-di(4-phenyl)phenyl-1,3,5-triazine (CGX UVA 006, Ciba Specialty Chemicals, Basel) or tetraethyl 2,2'-(1,4-phenylene-dimethylidene) bismalonate (Hostavin B-Cap, Clariant AG).
[0125] Particularly preferred special UV stabilizers are, for example, Tinuvin 360, Tinuvin 350, Tinuvin 329, Hostavin B-CAP, particularly preferably TIN 329 and Hostavin B-Cap. Mixtures of these ultraviolet absorbers can also be used. Particularly suitable ultraviolet absorbers are hydroxybenzotriazoles, such as 2-(3',5'-bis-(1,1-dimethylbenzyl)-2'-hydroxyphenyl)-benzotriazole (Tinuvin 234, BASF SE, Ludwigshafen), 2-(2'-hydroxy-5'-(tert.-octyl)-phenyl)-benzotriazole (Tinuvin 329, BASF SE, Ludwigshafen), bis-(3-(2H-benzotriazolyl)-2-hydroxy-5-tert.-octyl)methane (Tinuvin 360, BASF SE, Ludwigshafen), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(hexyloxy)-phenol (Tinuvin 1577, BASF SE, Ludwigshafen), 2-(5chloro-2H-benzotriazol-2-yl)-6-(1,1-dimethylethyl)-4-methyl-phenol (Tinuvin 326, BASF SE, Ludwigshafen), as well as benzophenones such as 2,4-dihydroxybenzophenone (Chimasorb 22, BASF SE, Ludwigshafen) and 2-hydroxy-4-(octyloxy)-benzophenone (Chimassorb 81, BASF SE, Ludwigshafen), 2,2-bis[[(2-cyano-1-oxo-3,3-diphenyl-2-propenyl)oxy]-methyl]-1,3-propanediyl ester (9CI) (Uvinul 3030, BASF SE, Ludwigshafen), 2-[2-Hydroxy-4-(2-ethylhexyl)oxy]phenyl-4,6-di(4-phenyl)phenyl-1,3,5-triazine (Tinuvin 1600, BASF SE, Ludwigshafen), tetraethyl 2,2'-(1,4-phenylenedimethylidene)bismalonate (Hostavin B-Cap, Clariant AG) or N-(2-Ethoxyphenyl)-N'-(2-ethylphenyl)-ethanediamide (Tinuvin 312, CAS No. 23949-66-8, BASF SE, Ludwigshafen).
[0126] Particularly preferred specific UV stabilizers are Tinuvin 360, Tinuvin 329, Tinuvin 326, Tinuvin 1600, Tinuvin 312, Uvinul 3030 and / or Hostavin B-Cap; most preferred are Tinuvin 329 and Tinuvin 360.
[0127] If UV absorbers are included, the composition preferably contains UV absorbers in an amount of up to 0.8 wt.%, preferably 0.05 wt.% to 0.5 wt.%, more preferably 0.08 wt.% to 0.4 wt.%, most preferably 0.1 wt.% to 0.35 wt.%, based on the total composition.
[0128] Suitable IR absorbers are disclosed, for example, in EP 1 559 743 A1, EP 1 865 027 A1, DE 10022037 A1, DE 10006208 A1, and in the Italian patent applications RM2010A000225, RM2010A000227, and RM2010A000228. Of the IR absorbers mentioned in the cited literature, those based on borides and tungstates, in particular cesium tungstate or zinc-doped cesium tungstate, as well as ITO- and ATO-based absorbers, and combinations thereof, are preferred.
[0129] The compositions according to the invention may also contain phosphates or sulfonic acid esters as transesterification stabilizers. Triisooctyl phosphate is preferably included as the transesterification stabilizer. Triisooctyl phosphate is preferably used in amounts of 0.003 wt.% to 0.05 wt.%, more preferably 0.005 wt.% to 0.04 wt.%, and particularly preferably 0.01 wt.% to 0.03 wt.%, based on the total composition.
[0130] Suitable colorants can be pigments, organic and inorganic pigments, carbon black and / or dyes. Colorants or pigments within the meaning of the present invention are sulfur-containing pigments such as cadmium red or cadmium yellow, iron cyanide-based pigments such as Prussian blue, oxide pigments such as zinc oxide, red iron oxide, black iron oxide, chromium oxide, titanium yellow, zinc-iron-based brown, titanium-cobalt-based green, cobalt blue, copper-chromium-based black and copper-iron-based black or chromium-based pigments such as chrome yellow, phthalocyanine-derived dyes such as copper phthalocyanine blue or copper phthalocyanine green, condensed polycyclic dyes and pigments such as azo-based (e.g. nickel azo yellow), sulfur-indigo dyes, perinone-based, perylene-based, quinacridone-derived, dioxazine-based, isoindolinone-based and quinophthalone-derived derivatives, anthraquinone-based, heterocyclic systems.
[0131] Specific examples of commercial products include MACROLEX Blue RR, MACROLEX Violet 3R, MACROLEX Violet B (Lanxess AG, Germany), Sumiplast Violet RR, Sumiplast Violet B, Sumiplast Blue OR (Sumitomo Chemical Co., Ltd.), Diaresin Violet D, Diaresin Blue G, Diaresin Blue N (Mitsubishi Chemical Corporation), Heliogen Blue, or Heliogen Green (BASF AG, Germany). Among these, cyanine derivatives, quinoline derivatives, anthraquinone derivatives, and phthalocyanine derivatives are preferred.
[0132] Fillers other than components b and c may also be added, provided their type and quantity do not impair the properties of the present invention. These can be, for example, particulate, flaky, or fibrous. Examples include chalk, barium sulfate, silicates / aluminosilicates such as mica / clay layer minerals, montmorillonite, particularly in an organophilic form modified by ion exchange, kaolin, zeolites, vermiculite, magnesium hydroxide, and aluminum hydroxide. Mixtures of various inorganic materials can also be used.
[0133] Preferably, the composition does not contain waxy stabilizers.
[0134] Preferably, the further additives are only one or more selected from the group consisting of thermal stabilizers, antistatic agents, UV absorbers, IR absorbers, antioxidants, inorganic pigments, carbon black, colorants, silicates, in particular aluminum silicates, chalk, quartz powder, mica / clay layers, montmorillonite, aluminum oxide, magnesium oxide, silicon dioxide (unfired), barium sulfate and / or mold release agents.
[0135] In addition, further components may be added which, depending on the type of component and the amount, do not adversely affect the level of properties of the present invention.
[0136] It is understood that the thermoplastic compositions of the substrate layer can, in principle, also contain blend partners. Suitable thermoplastic polymers as blend partners include, for example, polystyrene, styrene copolymers, aromatic polyesters such as polyethylene terephthalate (PET), PET-cyclohexanedimethanol copolymer (PETG), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), cyclic polyolefins, poly- or copolyacrylates, poly- or copolymethacrylates such as poly- or copolymethyl methacrylates (such as PMMA), as well as copolymers with styrene such as transparent polystyreneacrylonitrile (PSAN), thermoplastic polyurethanes, and / or polymers based on cyclic olefins (e.g., TOPAS, a commercial product from Ticona).
[0137] Particularly preferred compositions for the substrate layers according to the invention contain at least one thermal stabilizer, a mold release agent, and carbon black as additives. Very particularly preferably, no further components are present besides components a, b, and c and one or more thermal stabilizers, mold release agents, and carbon black.
[0138] Preferably, the CLTE values of the substrate layer, longitudinal and transverse, determined according to DIN 53752 method A: 1980, are ≤ 46.5 ppm / K, with their ratio (longitudinal / transverse) more preferably being ≥ 0.84, and / or the thermal conductivity of the substrate layer, in plane, determined according to ASTM E 1461:2013, is preferably ≥ 0.7 W / (m·K), more preferably ≥ 0.85 W / (m·K), particularly preferably ≥ 0.89 W / (m·K) and / or the thermal conductivity of the substrate layer, through plane, determined according to ASTM E 1461:2013, is preferably ≥ 0.45 W / (m·K).
[0139] Preferably, the gloss of the substrate layer, determined according to ASTM D 523-14, is > 90°, more preferably > 92°, even more preferably ≥ 94°.
[0140] Even more preferably, the Vicat temperature of the composition of the substrate layer, determined according to DIN ISO 306:2014-3, is ≥ 141°C, particularly preferably ≥ 142°C.
[0141] Due to the requirements, it is particularly preferred that all of these properties are met together.
[0142] The preparation of the inventive compositions of the substrate layer, comprising components a to c and optionally d, as well as any blending partners, is carried out using conventional incorporation processes by combining, mixing, and homogenizing the individual components, with homogenization preferably taking place in the melt under the action of shear forces. Optionally, the combining and mixing takes place before melt homogenization using powder premixes.
[0143] Premixes of granules or granules and powders containing components b, c and, if applicable, d can also be used.
[0144] Premixes prepared from solutions of the mixture components in suitable solvents may also be used, optionally by homogenisation in solution and subsequent removal of the solvent.
[0145] In particular, components b, c and optionally d of the composition according to the invention can be introduced into the polycarbonate, optionally into the polycarbonate with blend partner, by known methods or as a masterbatch.
[0146] The use of masterbatches is preferred for introducing components b, c and, if applicable, d, individually or in a mixture.
[0147] In this context, the composition according to the invention can be combined, mixed, homogenized, and then extruded in conventional devices such as screw extruders (e.g., twin-screw extruders, ZSK), kneaders, Brabender or Banbury mills. After extrusion, the extrudate can be cooled and comminuted. Individual components can also be premixed, and then the remaining starting materials can be added individually and / or in a mixed form.
[0148] The merging and mixing of a premix in the melt can also take place in the plasticizing unit of an injection molding machine. In this case, the melt is transferred directly into a molded body in the subsequent step.
[0149] The compositions according to the invention can be processed into any desired shaped articles in the usual way on conventional machines, for example on extruders or injection molding machines. In the production of the substrate layer of the layer structure according to the invention, dynamic mold temperature control is used during injection molding. The conditions for this are typically determined by the machine operator within the scope of their specialist knowledge. In the case of dynamic mold temperature control for the production of a substrate layer of a layer structure according to the invention, a melt temperature of 300 to 340°C, a mold temperature of 140 to 170°C, an injection speed of 40 to 80 mm / s and a holding pressure of 700 to 900 bar are typically selected conditions, for example a melt temperature of 330°C, a mold temperature of 160°C, an injection speed of 40 mm / s and a holding pressure of 900 bar. Examples 1. Description of raw materials and test methods
[0150] The polycarbonate compositions described in the following examples were compounded on a BUSS MX58 co-kneader with a throughput of 80 kg / h. The melt temperature was between 250 and 310 °C, with the kneader housing, kneader shaft, discharge housing, and discharge screw shaft at a defined temperature of 260 °C. The die plate temperature was 300 °C. Component b was added via a side extruder along with a powder premix (polycarbonate powder + additives). Component c was added directly via the main feed. Component a: Linear polycarbonate based on bisphenol A with a melt volume flow rate MVR of 19 cm 3 < / (10 min) (according to ISO 1133:2012-03, at a test temperature of 300°C and a load of 1.2 kg). Component b-1: Expanded graphite Ecophit ®< GFG 900 from SGL Carbon GmbH with a D(0.5) of approx. 900 µm according to DIN 51938:2015-09. Component b-2: Expanded graphite SC 4000 O / SM with a D(0.5) of approx. 1000 µm according to DIN 51938:2015-09 from Graphit Kropfmühl GmbH. Component c: Calcined silicon dioxide Amosil FW 600 from Quarzwerke GmbH in Frechen, uncoated, with an average particle size D(0.5) of approx. 4 µm, D(0.98) of approx. 13 µm, a D(0.1) / D(0.9) ratio of approx. 1.5 / 10 and a specific surface area of approx. 6 m² / g, determined according to DIN-ISO 9277:2014-01. Component c*: Compacted talc with a talc content of 98 wt.%, an iron oxide content of 1.9 wt.%, an aluminum oxide content of 0.2 wt.%, a loss on ignition (DIN 51081 / 1000 °C) of 5.4 wt.%, a pH value (according to EN ISO 787-9:1995) of 9.15, a D(0.5) (sedimentation analysis) of 2.2 µm; a BET surface area according to ISO 4652:2012-06 of 10 m 2 < / g, type: Finntalc M05SLC, manufacturer: Mondo Minerals BV Component d-1: "Wax." A maleic anhydride-modified polypropylene copolymer from Honeywell (AC907P) with an average molecular weight (gel permeation chromatography in ortho-dichlorobenzene at 150 °C with polystyrene calibration) of M w = 20,700 g / mol, M n = 1,460 g / mol, and an acid number of 78 mg KOH / g (ASTM D-1386:2015).
[0151] The Vicat softening temperatureVST / B50 or B120 as a measure of heat resistance was determined according to DIN ISO 306:2014-3 on test specimens measuring 8 mm x 10 mm x 4 mm with a stamp load of 50 N and a heating rate of 50°C / h or 120°C / h using the Coesfeld Eco 2920 device from Coesfeld Materialtest.
[0152] The thermal expansion coefficients ( CLTE ) were measured according to DIN 53752:1980-12 (linear thermal expansion coefficient, parallel / vertical, at 23-60°C (with a heating rate of 3K / min).
[0153] The Thermal conductivity TC in injection molding direction (in-plane) at 23°C was determined according to ASTM E 1461:2013 on samples with dimensions of 60 mm x 60 mm x 2 mm.
[0154] The Thermal conductivity TC in injection molding direction (through-plane) at 23°C was determined according to ASTM E 1461:2013 on samples with dimensions of 60 mm x 60 mm x 2 mm.
[0155] The determination of Melt viscosities was carried out according to ISO 11443:2014-04 using the Visco-Robo 45.00 device from Göttfert (cone-plate arrangement).
[0156] The density was determined according to ISO 1183-1:2012.
[0157] The Shine was determined according to ASTM D 523-14.
[0158] The test specimens used to determine surface quality were manufactured using dynamic mold temperature control in the injection molding process. The materials were processed at a melt temperature of 330°C and a mold temperature of 166°C (heating) and 85°C (cooling). The injection speed was 40 mm / s, and the holding pressure was 900 bar.
[0159] Following the examinations, a metal layerapplied to the substrate layer using the following procedure: The coating system consisted of a vacuum chamber in which the samples were positioned on a rotating sample holder. The sample holder rotated at approximately 20 rpm. Before being placed in the vacuum chamber, the test specimens were blown with ionized air to remove dust. For metallization, Ar gas was introduced at a pressure of 5 1 10 -3 mbar. Using a DC magnetron, an aluminum layer approximately 200 nm thick was applied to the samples with a power density of 6.4 W / cm 2 . 2. Recipes and results
[0160] Table 1: Compositions according to the invention E1 to E4 and comparative examples V1 to V7 Recipe V1 V2 V3 E1 E2 E3 V4 E4 V5 V6 V7 a % by weight 59,37 59,37 54,37 59,37 56,87 54,37 60,00 60,00 59,60 74,75 74,00 b-1 % by weight 1 1 5 7,5 7,5 10 5 b-2 % by weight 5 10 5 c % by weight 40 39 44 35 35 37,5 30 35 30 c* % by weight 20 20 d-1 % by weight 1 further additives d-2, d-3, d-4: (thermostabilizer / deformer / carbon black) % by weight 0,075 / 0,4 / 0,16 0,075 / 0,4 / 0,16 0,075 / 0,4 / 0,16 0,075 / 0,4 / 0,16 0,075 / 0,4 / 0,16 0,075 / 0,4 / 0,16 0,1 / 0,3 / 0,25 / - / - Examinations Melt viscosity at 300°C Pa·s 286 320 330 358 406 438 395 296 357 145 223 TC (in plane) W / (m·K) 0,32 0,49 0,47 0,96 1,58 1,71 1,88 0,89 1,87 1,7 1,57 TC (through plane) W / (m·K) 0,26 0,36 0,38 0,47 0,59 0,61 ng ng ng 0,4 ng VST / B50 [°C] 142 142 142 142 142 142 148 147 148 139 147 CLTE parallel (RT-60°C) ppm / K 44 43 43 40 36 35 36 42 36 37 40 CLTE vertical (RT-60°C) ppm / K 45 46 44 46 43 41 45 46 43 49 55 Ratio CLTE parallel / CLTE vertical 0,98 0,93 0,96 0,87 0,84 0,84 0,81 0,90 0,84 0,76 0,72 density g / cm 3< 1,46 1,46 1,50 1,46 1,48 1,50 1,44 1,43 1,46 1,38 1,37 Gloss (at 20°) ° 102 ng 100 100 97 94 73 103 90 ng 103 ng: not measured
[0161] The thermal conductivity of a composition is determined by the fillers incorporated and their weight or volume fraction. The filler-specific thermal conductivity largely determines the degree of thermal conductivity of the overall composition. The use of a low-thermally conductive filler such as quartz at a concentration of 40 wt.% (V1) results in a total thermal conductivity (in-plane) of 0.32 W / mK, which is too low for the intended purpose. A major advantage of quartz as a spherical filler is the high dimensional stability of the composition (expressed by the ratio of parallel to perpendicular CLTE, here 0.98). The addition or partial substitution of the filler with graphite enables an increase in thermal conductivity, but reduces the dimensional stability of the overall composition due to its platelet-shaped particle geometry.At low graphite concentrations (V2 and V3), the CLTE ratio (and thus the degree of isotropy) is still very close to the ideal value (CLTE parallel = CLTE perpendicular = 1.0), but the thermal conductivity is only minimally increased, even at a total filler content of 45%. The addition of 5-7.5 wt% graphite (E1-E3) offers an optimal balance between in-plane thermal conductivity (> 0.85 W / mK) and isotropy (≥ 0.84).
[0162] The choice of graphite also influences these properties due to particle size distributions. For example, graphite b2, at least in low concentrations, achieves a lower thermal conductivity (cf. E4 and E1). Although compositions E3 and V5 have the same CLTE ratio, the higher filler content of E3 (45%) is preferred, as it results in a lower CLTE and thus lower shrinkage behavior.
[0163] Another disadvantage of high graphite contents is the surface quality (measured by the gloss level). This is evident in V4 and V5, whose gloss level is significantly lower than the other compositions with less graphite. The combination of graphite and talc as filler (V6 and V7) leads to high thermal conductivities even at lower total filler contents, but has the major disadvantage of reduced dimensional stability (see CLTE quotient) due to the platelet-shaped particle geometry as with graphite. Furthermore, talc can only be incorporated into polycarbonate with the help of a waxy stabilizer (d). However, this stabilizer leads to the formation of streaks on the surface during processing, which has a negative impact on metal adhesion and the thermal stability of a reflector structure.
[0164] The examples shown show that only a balanced ratio of quartz and graphite (E1-E3, E4) leads to a good property combination profile of CLTE, CLTE quotient, thermal conductivity and surface quality (gloss).
Claims
1. Layer structure, comprising i) a substrate layer made of a thermoplastic polycarbonate-based composition and ii) a metal layer applied to the substrate layer i, characterized in that the thermoplastic polycarbonate-based composition of substrate layer i contains the following components: a) 44% to 63% by weight of aromatic polycarbonate, b) 3% to 8% by weight of expanded graphite, c) 34% to 38% by weight of fired silicon dioxide, d) 0% to 10% by weight of one or more further additives, wherein the total amount of expanded graphite and fired silicon dioxide is at least 40% by weight.
2. Layer structure according to Claim 1, wherein the thermoplastic polycarbonate-based composition of substrate layer i contains a) 54% to 60% by weight of aromatic polycarbonate, b) 5% to 7.5% by weight of expanded graphite, c) 35% to 37.5% by weight of fired silicon dioxide, d) 0% to 5% by weight of one or more further additives.
3. Layer structure according to Claim 1 or 2, wherein the substrate layer has been produced by injection moulding with dynamic temperature control of the mould.
4. Layer structure according to any of the preceding claims, wherein the layer structure comprises no further layers other than optionally one or more protective layers.
5. Layer structure according to any of the preceding claims, wherein the thermoplastic polycarbonate-based composition of substrate layer i consists of components a to c and optionally d.
6. Layer structure according to any of the preceding claims, wherein the group of the further additives consists of the group of flame retardants, heat stabilizers, antistats, UV absorbers, IR absorbers, anti-dripping agents, impact modifiers, antioxidants, inorganic pigments, carbon black, organic colourants, inorganic fillers and / or mould-release agents.
7. Layer structure according to any of the preceding claims, wherein the D(0.5) of the expanded graphite is 700 µm to 1200 µm, determined by sieve analysis in accordance with DIN 51938:2015-09.
8. Layer structure according to any of the preceding claims, wherein the D(0.5) of the fired silicon dioxide is 2.5 µm to 8.0 µm, determined in accordance with ISO 13320:2009-10.
9. Layer structure according to any of the preceding claims, wherein the D(0.5) of the fired silicon dioxide is 3 µm to 5 µm, determined in accordance with ISO 13320:2009-10.
10. Layer structure according to any of the preceding claims, wherein for the substrate layer the ratio of the longitudinal and transversal CLTE value (longitudinal:transversal), determined in accordance with DIN 53752-Method A:1980, is ≥ 0.84 and the in-plane thermal conductivity, determined in accordance with ASTM E 1461:2013, is ≥ 0.7 W / (m·K) and the Vicat temperature, determined in accordance with DIN ISO 306:2014-3, is ≥ 141°C and the gloss, determined in accordance with ASTM D 523-14, is > 90°.
11. Layer structure according to any of the preceding claims, wherein the metal layer ii has a thickness of ≥ 60 nm to ≤ 300 nm, determined by atomic force microscopy.
12. Component comprising a layer structure according to any of the preceding claims.
13. Component according to Claim 12, wherein the component is a reflector or a mirror element of a head-up display.
14. Component according to Claim 13, wherein the component is a headlamp reflector.
15. Method for producing a layer structure according to any of Claims 1 to 11, wherein a) the substrate layer is formed from the thermoplastic polycarbonate-based composition by one-component injection moulding with dynamic temperature control of the mould and then b) a metal layer is applied to this substrate layer.