Laminated sealant film
The laminated sealant film addresses delamination and appearance issues by optimizing layer compositions and elastic modulus, achieving effective low-temperature bag-forming and energy-efficient packaging for various products.
Patent Information
- Application Number
- PCT/JP2024/006806
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-02-26
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional sealant films suffer from delamination and lack excellent appearance and low-temperature bag-forming properties, which are essential for efficient packaging of products like foods, beverages, and pharmaceuticals.
A laminated sealant film is developed with specific layer compositions and elastic modulus control, comprising a laminate layer, intermediate layer, and sealing layer made of polypropylene resin compositions, with optimized melt flow rates and melting points, and inclusion of anti-blocking agents and organic lubricants to prevent delamination and enhance low-temperature sealing.
The laminated sealant film effectively prevents delamination, maintains excellent appearance, and exhibits improved low-temperature bag-forming properties, making it suitable for automatic formation of packaging bags, such as pillow, gusset, and three-sided seal bags, while reducing heat sealing temperatures and energy consumption.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Laminated Sealant Film
[0001] The present invention relates to a laminated sealant film that is resistant to delamination, has excellent appearance, and is easy to form into bags at low temperatures.
[0002] As disclosed in Patent Documents 1 to 5, packaging materials have been developed to suit the contents of many products, such as foods, beverages, pharmaceuticals, and chemicals. Packaging materials are used in various forms, such as pillow packaging, gusset packaging, and three-sided seal packaging, and the sealant films used in packaging materials also have functions required for their applications.
[0003] Japanese Patent No. 4731699 Japanese Patent Application Laid-Open No. 2000-272064 Japanese Patent Application Laid-Open No. 2000-272065 Japanese Patent Application Laid-Open No. 2002-241716 Japanese Patent Application Laid-Open No. 2020-192695
[0004] Sealant films are particularly suitable for automatic bag-making processes for pillow packaging bags, gusset packaging bags, and three-sided sealed packaging bags while packaging the contents. The lower the heat-sealing temperature, the lower the electricity bill and the lower the risk of burns, improving workability. Furthermore, low-temperature heat-sealing properties increase packaging and bag-making speeds, reduce packaging material waste, and produce cleaner finished packaging bags. However, conventional sealant films have been resistant to delamination and have not exhibited excellent appearance or low-temperature bag-making properties.
[0005] An object of the present invention is to provide a laminated sealant film that is resistant to delamination, has an excellent appearance, and is easy to form into a bag at low temperature.
[0006] As a result of extensive research to achieve this object, the inventors have succeeded in obtaining a laminate sealant film that is less susceptible to interlayer delamination and has excellent appearance and low-temperature bag-forming properties by controlling the raw material composition of each layer of the laminate sealant film and the elastic modulus of the entire film. The laminate sealant film according to the embodiment is as follows [1], and preferably any one of [2] to
[11] .
[0007] [1] A laminate sealant film satisfying the following requirements 1) to 7): 1) A laminate sealant film comprising at least a laminate layer, an intermediate layer, and a seal layer, in this order; 2) The laminate layer, the intermediate layer, and the seal layer are each made of a polypropylene-based resin composition; 3) The ratio of the melt flow rate of the polypropylene-based resin composition of the intermediate layer to the melt flow rate of the polypropylene-based resin composition of the laminate layer is 0.6 or more and 2.0 or less; 4) The ratio of the melt flow rate of the polypropylene-based resin composition of the seal layer to the melt flow rate of the polypropylene-based resin composition of the intermediate layer is 0.6 or more and 2.0 or less; 5) The melt flow rates of the polypropylene-based resin compositions of the laminate layer, the intermediate layer, and the seal layer are 1 g / 10 min (load 2.16 kgf) or more and 9 g / 10 min (load 2.16 kgf) or less, respectively. 6) The melting point of the polypropylene resin composition in the seal layer is 100°C or higher and 140°C or lower. 7) A laminate sealant film having a tensile modulus in the longitudinal direction of 600 MPa or lower. [2] The laminate sealant film according to [1], wherein the polypropylene resin composition contains a propylene random copolymer. [3] The laminate sealant film according to [1] or [2], wherein the laminate sealant film has a main peak of melting point of 120°C or higher and 160°C or lower. [4] The laminate sealant film according to any one of [1] to [3], wherein the static friction coefficient between the surfaces of the seal layers is 1.0 or lower. [5] The laminate sealant film according to any one of [1] to [4], wherein the dynamic friction coefficient between the surfaces of the seal layers is 1.0 or lower. [6] The laminate sealant film according to any one of [1] to [5], wherein the seal layer contains silica particles. [7] The laminate sealant film according to any one of [1] to [6], wherein the seal layer contains erucic acid amide. [8] The laminate sealant film according to any one of [1] to [7], wherein the seal layer contains organic particles. [9] The laminate sealant film according to any one of [1] to [8], wherein the tensile modulus in the longitudinal direction is 200 MPa or more and 600 MPa or less.
[10] The laminate sealant film according to any one of [1] to [9], which satisfies the following 8) and 9): 8) The difference between the melting point of the polypropylene resin composition of the laminate layer and the melting point of the polypropylene resin composition of the intermediate layer is 30°C or less. 9) The difference between the melting point of the polypropylene resin composition of the intermediate layer and the melting point of the polypropylene resin composition of the seal layer is 30°C or less.
[11] The laminate sealant film according to any one of [2] to
[10] , wherein the propylene random copolymer is a random copolymer of propylene, ethylene, and butene-1.
[0008] According to the present invention, a laminated sealant film can be provided that is resistant to delamination, has an excellent appearance, and is easy to form into bags at low temperatures. Because of its excellent low-temperature formability, the laminated sealant film is suitable as a packaging material for many products, such as food, beverages, pharmaceuticals, and chemicals. It is particularly suitable for automatic bag-forming into pillow-shaped bags, gusseted bags, three-sided sealed bags, and other bags while packaging the contents.
[0009] The laminate sealant film according to the embodiment satisfies the following requirements 1) to 7). 1) The laminate sealant film includes at least a laminate layer, an intermediate layer, and a seal layer, in this order. 2) The laminate layer, the intermediate layer, and the seal layer are each made of a polypropylene-based resin composition. 3) The ratio of the melt flow rate of the polypropylene-based resin composition of the intermediate layer to the melt flow rate of the polypropylene-based resin composition of the laminate layer is 0.6 or more and 2.0 or less. 4) The ratio of the melt flow rate of the polypropylene-based resin composition of the seal layer to the melt flow rate of the polypropylene-based resin composition of the intermediate layer is 0.6 or more and 2.0 or less. 5) The melt flow rates of the polypropylene-based resin compositions of the laminate layer, the intermediate layer, and the seal layer are 1 g / 10 min (load 2.16 kgf) or more and 9 g / 10 min (load 2.16 kgf) or less, respectively. 6) The melting point of the polypropylene-based resin composition of the seal layer is 100°C or more and 140°C or less. 7) A laminated sealant film having a tensile modulus in the longitudinal direction of 600 MPa or less.
[0010] The laminate sealant film according to the embodiment will be described in detail below. The laminate sealant film includes at least a laminate layer, an intermediate layer, and a sealing layer in this order. The laminate layer, the intermediate layer, and the sealing layer will be described in detail below.
[0011] (Laminate Layer) The laminate layer is made of a polypropylene-based resin composition. The polypropylene-based resin composition contains a polypropylene-based resin as a main component. The term "main component" means that the polypropylene-based resin accounts for 90% by mass or more of the polypropylene-based resin composition, more preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 99% by mass or more. This proportion is preferably 100% by mass or less. The laminate layer preferably contains 95% by mass or more of the polypropylene-based resin composition, more preferably 97% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass. The laminate layer may contain unavoidable impurities in addition to the polypropylene-based resin composition.
[0012] (Polypropylene-Based Resin) The polypropylene-based resin in the laminate layer is a resin containing propylene as a main component, and examples thereof include propylene homopolymers, random copolymers and block copolymers of propylene and one or more α-olefins such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, octene-1, etc. Among these, random copolymers and / or block copolymers of propylene and one or more α-olefins such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, octene-1 are preferred, propylene random copolymers, which are random copolymers of propylene and one or more α-olefins, are more preferred, and random copolymers of propylene, ethylene, and butene-1 are even more preferred. The term "main component" means that the proportion of propylene in the polypropylene-based resin is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 99% by mass or more. The proportion is preferably 100% by mass or less.
[0013] The polypropylene resin composition of the laminate layer preferably has a melt flow rate (load 2.16 kgf) of 1 g / 10 min or more and 9 g / 10 min or less, more preferably 1.5 g / 10 min or more and 8 g / 10 min or less, and even more preferably 3 g / 10 min or more and 7 g / 10 min or less. The melt flow rate can be measured in accordance with JIS K7210.
[0014] The upper limit of the melting point (JIS K7121) of the polypropylene resin composition of the laminate layer is preferably 160°C or lower, more preferably 150°C or lower, and even more preferably 140°C or lower. When the melting point (JIS K7121) of the polypropylene resin composition of the laminate layer is 160°C or lower, the tensile modulus of the laminate sealant film is easily controlled to 600 MPa or lower. The lower limit of the melting point (JIS K7121) of the polypropylene resin composition of the laminate layer is preferably 120°C or higher, more preferably 125°C or higher, and even more preferably 130°C or higher. When the melting point (JIS K7121) of the polypropylene resin composition of the laminate layer is 120°C or higher, the laminate sealant film is less likely to wrinkle, for example, when subjected to retort treatment, and transparency is easily maintained. Furthermore, when laminated with a stretched polypropylene film, it is possible to obtain packaging bags made of the same material, and the laminate sealant film can be used for applications that could not be achieved with a sealant film made of a polyethylene resin. This is useful as a so-called monomaterial film.
[0015] In addition to the polypropylene-based resin, the polypropylene-based resin composition of the laminate layer may contain, for example, at least one ethylene homopolymer selected from the group consisting of high-pressure low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, and high-density polyethylene. Furthermore, it may contain a random or block copolymer, or a mixture thereof, primarily composed of ethylene and copolymerized with other monomers, such as α-olefins such as propylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, and octene-1, vinyl acetate, (meth)acrylic acid, and (meth)acrylic acid esters. These may be crystalline, low-crystalline, or amorphous. The content of these polymers other than the polypropylene-based resin in the laminate layer is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less. This proportion may be 0.1% by mass or more.
[0016] The polyethylene resin of the laminate layer preferably has a melt flow rate (load 2.16 kgf) of 0.1 g / 10 min or more and 9 g / 10 min or less, more preferably 0.5 g / 10 min or more and 8 g / 10 min or less, and even more preferably 1 g / 10 min or more and 7 g / 10 min or less. The melt flow rate can be measured in accordance with JIS K7210. The polyethylene resin of the laminate layer preferably has a melting point (JIS K7121) of 100°C or more and 140°C or less, more preferably 105°C or more and 135°C or less, and even more preferably 110°C or more and 130°C or less. The melting point of the polyethylene resin may show two or more melting endothermic peaks, and the peak with the highest melting temperature is considered to be the main peak.
[0017] (Antiblocking Agent) The polypropylene resin composition of the laminate layer preferably contains an antiblocking agent. Examples of antiblocking agents include particles made of silica such as synthetic silica, inorganic particles such as diatomaceous earth, zeolite, talc, and mica, and organic particles such as silicone particles, acrylic particles, nylon particles, and polyethylene particles. It is more preferable to contain silica particles and / or polyethylene particles. In particular, it is preferable to contain silica particles and polyethylene particles. The average particle size of the particles is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 4 μm or more. The average particle size of the particles is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. The particle size is the volume average particle size.
[0018] The particle content of the polypropylene resin composition in the laminate layer is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.4% by mass or more. It is also preferably 2% by mass or less, more preferably 1.5% by mass or less, and even more preferably 1.0% by mass or less. When the particle content is 2% by mass or less, the number of protrusions on the surface is not too large, and poor appearance and abrasion resistance are unlikely to occur.
[0019] (Organic Lubricant) The polypropylene resin composition of the laminate layer preferably contains 0.01% by mass or more and 2.0% by mass or less of a fatty acid amide as an organic lubricant, more preferably 0.05% by mass or more and 1.5% by mass or less, and particularly preferably 0.1% by mass or more and 1.0% by mass or less. When the fatty acid amide is 0.01% by mass or more, blocking between films is not too strong, and the film handling is likely to be satisfactory. When the fatty acid amide is 2.0% by mass or less, the seal strength is unlikely to decrease. Examples of fatty acid amides include erucic acid amide, ethylene bisoleic acid amide, and behenic acid amide, and these may be used in combination.
[0020] The closer the melt flow rate of the resin composition or raw material resin of the laminate layer is to that of the resin composition or raw material resin of the intermediate layer, the better the appearance. Therefore, the ratio of the melt flow rate of the polypropylene resin composition of the intermediate layer to the melt flow rate of the polypropylene resin composition of the laminate layer is 0.6 to 2.0, preferably 0.7 to 1.6, more preferably 0.8 to 1.4, and even more preferably 0.9 to 1.2. When the melt flow rate ratio is within this range, poor appearance such as layer misalignment, blemishes, and unevenness is less likely to occur.
[0021] (Intermediate layer) The intermediate layer is made of a polypropylene-based resin composition. The polypropylene-based resin composition contains a polypropylene-based resin as a main component. The term "main component" means that the polypropylene-based resin accounts for 90% by mass or more of the polypropylene-based resin composition, and this proportion is preferably 95% by mass or more, more preferably 97% by mass or more, even more preferably 99% by mass or more. This proportion is preferably 100% by mass or less. The intermediate layer preferably contains 95% by mass or more of the polypropylene-based resin composition, more preferably 97% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass. The intermediate layer may contain unavoidable impurities in addition to the polypropylene-based resin composition.
[0022] (Polypropylene Resin) The polypropylene resin in the intermediate layer is a resin containing propylene as a main component, and examples thereof include propylene homopolymers, random copolymers and block copolymers of propylene and one or more α-olefins such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, octene-1, etc. Among these, random copolymers of propylene and one or more α-olefins such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, octene-1 are preferred, propylene random copolymers which are random copolymers of propylene and one or more α-olefins are more preferred, and random copolymers of propylene, ethylene, and butene-1 are even more preferred. The term "main component" means that the proportion of propylene in the polypropylene-based resin is 90% by mass or more, preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 99% by mass or more. The proportion is preferably 100% by mass or less.
[0023] The polypropylene resin composition of the intermediate layer preferably has a melt flow rate (load 2.16 kgf) of 1 g / 10 min or more and 9 g / 10 min or less, more preferably 1.5 g / 10 min or more and 2 g / 10 min or less, and even more preferably 3 g / 10 min or more and 7 g / 10 min or less. The melt flow rate can be measured in accordance with JIS K7210. The upper limit of the melting point (JIS K7121) of the polypropylene resin composition of the intermediate layer is preferably 150°C or less, more preferably 145°C or less, and even more preferably 140°C or less. When the melting point (JIS K7121) of the polypropylene resin composition of the intermediate layer is 150°C or less, the tensile modulus of the laminate sealant film is easily set to 600 MPa or less. The lower limit of the melting point (JIS K7121) of the polypropylene resin composition of the intermediate layer is preferably 120°C or higher, more preferably 125°C or higher, and even more preferably 130°C or higher. When the melting point (JIS K7121) of the polypropylene resin composition of the intermediate layer is 120°C or higher, the laminated sealant film is less likely to wrinkle when subjected to, for example, retort treatment, and transparency is easily maintained. Furthermore, the laminated sealant film can be used for applications that could not be achieved with sealant films made of polyethylene resins, such as laminating it with an OPP film to form a mono-material film.
[0024] In addition to the polypropylene resin, the polypropylene resin composition of the intermediate layer may contain, for example, at least one ethylene homopolymer selected from the group consisting of high-pressure low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, and high-density polyethylene. Furthermore, it may contain a random or block copolymer, or a mixture thereof, primarily composed of ethylene and copolymerized with other monomers, such as α-olefins such as propylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, and octene-1, vinyl acetate, (meth)acrylic acid, and (meth)acrylic acid esters. These may be crystalline, low-crystalline, or amorphous. The content of these polymers other than the polypropylene resin in the intermediate layer is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less. This proportion may be 0.1% by mass or more.
[0025] The polyethylene resin of the intermediate layer preferably has a melt flow rate of 0.1 g / 10 min or more and 9 g / 10 min or less, more preferably 0.5 g / 10 min or more and 8 g / 10 min or less, and even more preferably 1 g / 10 min or more and 7 g / 10 min or less. The polyethylene resin of the intermediate layer preferably has a melting point of 100°C or more and 140°C or less, more preferably 105°C or more and 135°C or less, and even more preferably 110°C or more and 130°C or less. The melting point of the polyethylene resin may show two or more melting endothermic peaks, and the peak with the highest melting temperature is defined as the main peak.
[0026] (Anti-blocking Agent) The polypropylene resin composition of the intermediate layer may contain an anti-blocking agent. Examples of anti-blocking agents include silica particles such as synthetic silica, inorganic particles such as diatomaceous earth, zeolite, talc, and mica, and organic particles such as silicone particles, acrylic particles, nylon particles, and polyethylene particles. It is particularly preferable to contain silica particles and / or polyethylene particles. It is particularly preferable to contain silica particles and polyethylene particles. The average particle size of the particles is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 5 μm or more. The average particle size of the particles is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. The particle size is the volume average particle size.
[0027] The particle content in the polypropylene resin composition of the intermediate layer is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.4% by mass or more, and is preferably 2% by mass or less, more preferably 1.5% by mass or less, and even more preferably 1.0% by mass or less.
[0028] (Organic Lubricant) The polypropylene resin composition of the intermediate layer may contain a fatty acid amide, preferably from 0.01% by mass to 2.0% by mass, more preferably from 0.05% by mass to 1.5% by mass, and particularly preferably from 0.1% by mass to 1.0% by mass. Examples of the fatty acid amide include erucic acid amide, ethylene bisoleic acid amide, and behenic acid amide, and these may be used in combination.
[0029] The closer the melt flow rate of the resin composition or raw material resin of the intermediate layer is to that of the resin composition or raw material resin of the seal layer, the better the appearance. Therefore, the ratio of the melt flow rate of the polypropylene resin composition of the intermediate layer to the melt flow rate of the polypropylene resin composition of the laminate layer is 0.6 to 2.0, preferably 0.7 to 1.6, more preferably 0.8 to 1.4, and even more preferably 0.9 to 1.2. When the melt flow rate ratio is within this range, poor appearance such as layer misalignment, blemishes, and unevenness is less likely to occur.
[0030] (Sealing layer) The sealing layer is made of a polypropylene-based resin composition. The polypropylene-based resin composition contains a polypropylene-based resin as a main component. The term "main component" means that the polypropylene-based resin accounts for 90% by mass or more of the polypropylene-based resin composition, more preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 98% by mass or more. This proportion is preferably 100% by mass or less, and even more preferably 99% by mass or less. The sealing layer preferably contains 95% by mass or more of the polypropylene-based resin composition, more preferably 97% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass. The sealing layer may contain unavoidable impurities in addition to the polypropylene-based resin composition.
[0031] (Polypropylene-based resin) The polypropylene-based resin in the seal layer is a resin containing propylene as a main component, and examples thereof include propylene homopolymers, random copolymers and block copolymers of propylene and one or more α-olefins such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, and octene-1. Among these, random copolymers of propylene and one or more α-olefins such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, and octene-1 are preferred, propylene random copolymers, which are random copolymers of propylene and one or more α-olefins, are more preferred, and random copolymers of propylene, ethylene, and butene-1 are even more preferred. The term "main component" means that propylene accounts for 90% by mass or more of the polypropylene-based resin, and the proportion is preferably 95% by mass or more, more preferably 97% by mass or more, and even more preferably 99% by mass or more. The proportion is preferably 100% by mass or less. Polypropylene-based resins have a higher melting point and better transparency than polyethylene-based resins.
[0032] The polypropylene resin composition of the seal layer preferably has a melt flow rate (load 2.16 kgf) of 1 g / 10 min or more and 9 g / 10 min or less, more preferably 1.5 g / 10 min or more and 2 g / 10 min or less, and even more preferably 3 g / 10 min or more and 7 g / 10 min or less. The melt flow rate can be measured in accordance with JIS K7112. The polypropylene resin composition of the seal layer preferably has a melting point of 140°C or less, more preferably 135°C or less. When the melting point of the polypropylene resin composition of the seal layer is 140°C or less, the low-temperature sealability (effect) is excellent. Furthermore, when the melting point of the polypropylene resin composition of the seal layer is 140°C or less, the tensile modulus of the laminate sealant film is easily reduced to 600 MPa or less. The polypropylene resin composition of the seal layer preferably has a melting point of 100°C or more, more preferably 110°C or more, even more preferably 120°C or more, and particularly preferably 125°C or more. When the melting point of the polypropylene resin composition of the seal layer is 120° C. or higher, the seal layer is excellent in heat resistance such as retort resistance and in self-supporting properties.
[0033] (Anti-blocking agent) The polypropylene resin composition of the seal layer preferably contains an anti-blocking agent. Examples of anti-blocking agents include particles made of silica such as synthetic silica, inorganic particles such as diatomaceous earth, zeolite, talc, and mica, and organic particles such as silicone particles, acrylic particles, nylon particles, and polyethylene particles. It is more preferable to contain silica particles and / or polyethylene particles. In particular, it is preferable to contain silica particles and polyethylene particles. The average particle size of the particles is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 4 μm or more. The average particle size of the particles is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. The particle size is the volume average particle size.
[0034] The particle content in the polypropylene resin composition of the sealing layer is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.4% by mass or more. Also, it is preferably 2% by mass or less, more preferably 1.5% by mass or less, and even more preferably 1.0% by mass or less. If the particle content is less than 0.1% by mass, it becomes difficult to achieve a surface roughness Ra of 0.1 μm or more on at least one surface layer, making it difficult to obtain anti-blocking properties and slip properties. Furthermore, by adding particles in an amount of 2% by mass or less, surface protrusions can be reduced, making it easier to prevent the occurrence of abrasion resistance.
[0035] (Organic Lubricant) The polypropylene resin composition of the sealing layer preferably contains 0.01% by mass or more and 2.0% by mass or less of a fatty acid amide as an organic lubricant, more preferably 0.05% by mass or more and 1.5% by mass or less, and particularly preferably 0.1% by mass or more and 1.0% by mass or less. When the fatty acid amide content is 0.01% by mass or more, blocking between films is reduced, making it easier to handle the film. When the content is 2.0% by mass or less, the seal strength is less likely to decrease. Examples of fatty acid amides include erucic acid amide, ethylene bisoleic acid amide, and behenic acid amide, and these may be used in combination. In particular, erucic acid amide has a low melting point, is easy to bleed, and is easy to impart lubricity. The sealing layer more preferably contains silica particles as an antiblocking agent and erucic acid amide as an organic lubricant. The sealing layer more preferably contains polyethylene particles as an antiblocking agent and erucic acid amide as an organic lubricant. More preferably, the sealing layer contains silica particles and polyethylene particles as an antiblocking agent in combination with erucic acid amide as an organic lubricant.
[0036] (Layer Structure) Examples of the layer structure of the laminate sealant film include laminate layer / intermediate layer / sealing layer and laminate layer / intermediate layer 1 / intermediate layer 2 / sealing layer. For example, laminate layer / intermediate layer / sealing layer indicates a structure in which a laminate layer, an intermediate layer, and a sealing layer are laminated in this order. Arranging an intermediate layer between the laminate layer and the sealing layer is preferable because it reduces peeling between the laminate layer and the sealing layer and makes it easier to use recycled raw materials. The raw material composition of the intermediate layer is preferably intermediate between the laminate layer and the sealing layer to reduce peeling between the laminate layer and the sealing layer. The thickness of the laminate layer is preferably 3 μm or more, more preferably 5 μm or more. The thickness of the sealing layer is preferably 3 μm or more, more preferably 5 μm or more. The thickness of the intermediate layer is preferably 3 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and particularly preferably 15 μm or more. The thickness of the laminate layer is preferably 12 μm or less, more preferably 10 μm or less, and even more preferably 8 μm or less. The thickness of the seal layer is preferably 12 μm or less, more preferably 10 μm or more, and even more preferably 8 μm or less. The thickness of the intermediate layer is preferably 30 μm or less, more preferably 25 μm or less, and even more preferably 20 μm or less. The ratio of the thickness of the intermediate layer to the thickness of the laminate layer is preferably 1.0 or more, more preferably 1.5 or more, and even more preferably 2.0 or more. The ratio of the thickness of the seal layer to the thickness of the laminate layer is preferably 0.3 or more and 1.5 or less, and preferably 0.5 or more and 1.2 or less. The ratio of the thickness of the intermediate layer to the thickness of the seal layer is preferably 1.0 or more, more preferably 1.5 or more, and even more preferably 2.0 or more.
[0037] The smaller the difference in melt flow rate between the raw material resins of adjacent layers and / or the smaller the difference in melt flow rate between the raw material resins mixed in each layer, the more improved the appearance. The ratio of the melt flow rates of the raw material resins of adjacent layers is preferably 0.6 or more and 2.0 or less. When the melt flow rate ratio is within this range, poor appearance such as layer misalignment, blemishes, and unevenness is less likely to occur. Furthermore, the main peak of the melting point of the laminate sealant film is preferably 120°C or more, more preferably 130°C or more, and even more preferably 140°C or more. When the main peak of the melting point of the film is 120°C or more, the suitability for high retort is further improved. The smaller the difference in the melting points of the polypropylene resin compositions of adjacent layers, the less likely poor appearance such as layer misalignment, blemishes, and unevenness is to occur. The main peak of the melting point of the laminate sealant film is preferably 160°C or less, more preferably 150°C or less. The difference between the melting point of the polypropylene resin composition of the laminate layer and the melting point of the polypropylene resin composition of the intermediate layer, and the difference between the melting point of the polypropylene resin composition of the intermediate layer and the melting point of the polypropylene resin composition of the seal layer are preferably 30°C or less, more preferably 20°C or less, and even more preferably 10°C or less.
[0038] (Method for producing laminate sealant film) The method for producing a laminate sealant film will be described in detail below, but is not limited thereto. First, the resin compositions of the laminate layer, intermediate layer, and seal layer may be prepared by blending the above-mentioned resin raw materials and various additives as necessary using a mixer such as a Henschel mixer, a Banbury mixer, or a tumbler mixer. Then, the obtained resin composition can be used to form a film.
[0039] (Melt Extrusion Process) The mixed resin composition is melted, for example, under conditions of a resin temperature of 110°C or higher and 300°C or lower, and melt-extruded into a sheet form, for example, through a T-die, cast onto a cooling roll, and cooled and solidified to obtain an unstretched sheet. A specific method for this is preferably casting onto a cooling roll. Multilayering can be achieved using a multilayering device such as a multilayer feed block, a static mixer, or a multi-manifold die. For example, resins delivered from different flow paths using two or more extruders can be laminated into multiple layers using a multilayer feed block or a multi-manifold die. Examples of methods include melt-extruding a melt-kneaded laminated resin composition sheet and forming it into a film using a T-die method or an inflation method. However, the T-die method is particularly preferred because it allows for a high resin melt temperature.
[0040] (Cooling and Solidification Process) For example, it is preferable to cast a sheet melt-extruded from a T-die onto a chill roll and cool it. The lower limit of the chill roll temperature is preferably 10°C. If the temperature is lower than this, not only may the crystallization suppression effect saturate, but problems such as condensation may also occur, which is undesirable. The upper limit of the chill roll temperature is preferably 70°C or lower. If the temperature exceeds this range, crystallization will progress and transparency will deteriorate, which is undesirable. Furthermore, when the chill roll temperature is within the above range, it is preferable to reduce the humidity of the environment near the chill roll to prevent condensation. During casting, the surface temperature of the chill roll rises because the hot resin comes into contact with the surface. Typically, chill rolls are cooled by flowing cooling water through piping inside. However, it is necessary to reduce the temperature difference across the width of the chill roll surface by ensuring a sufficient amount of cooling water, optimizing the piping arrangement, and performing maintenance to prevent sludge from adhering to the piping. In this case, the thickness of the unstretched sheet is preferably in the range of 3 μm to 200 μm. The thickness of the film is preferably in the range of 5 μm or more and 100 μm or less, more preferably 10 μm or more and 80 μm or less.
[0041] The unstretched sheet obtained may be stretched, but stretching to a ratio of 2.0 or more will result in a tensile modulus of elasticity exceeding 600 MPa, so the stretching ratio is preferably less than 2.0.
[0042] (Film characteristics) The film characteristics will be described. The "longitudinal direction" of the laminate sealant film is the direction corresponding to the flow direction in the film manufacturing process, and the "width direction" is the direction perpendicular to the flow direction in the film manufacturing process. Hereinafter, the "longitudinal direction" may be abbreviated as the "MD direction" and the "width direction" may be abbreviated as the "TD direction."
[0043] (Tensile modulus) The upper limit of the longitudinal tensile modulus of the laminate sealant film is preferably 600 MPa or less, more preferably 580 MPa or less, even more preferably 560 MPa or less, even more preferably 540 MPa or less, particularly preferably 520 MPa or less, and most preferably 500 MPa or less. When the longitudinal tensile modulus is 600 MPa or less, the low-temperature sealing effect at the sealing initiation temperature is improved. The lower limit of the longitudinal tensile modulus of the laminate sealant film is preferably 200 MPa or more, more preferably 250 MPa or more, even more preferably 300 MPa or more, and even more preferably 325 MPa or more. When the longitudinal tensile modulus is 200 MPa or more, bag-making processing is easier. The upper limit of the widthwise tensile modulus of the laminate sealant film is preferably 580 MPa or less, more preferably 530 MPa or less, even more preferably 500 MPa or less, even more preferably 480 MPa or less, and particularly preferably 440 MPa or less. When the tensile modulus in the width direction is 580 MPa or less, the low-temperature sealing effect of the sealing initiation temperature is improved. The lower limit of the tensile modulus in the width direction of the laminated sealant film is preferably 200 MPa or more, more preferably 250 MPa or more, even more preferably 300 MPa or more, and even more preferably 325 MPa or more. When the tensile modulus in the width direction is 200 MPa or more, bag-making processing is easier.
[0044] The upper limit of the sum of the longitudinal tensile modulus and the widthwise tensile modulus of the laminated sealant film is preferably 1180 MPa or less, more preferably 1130 MPa or less, even more preferably 1080 MPa or less, even more preferably 1030 MPa or less, particularly preferably 980 MPa or less, and most preferably 930 MPa or less. When the longitudinal tensile modulus is 1180 MPa or less, the low-temperature sealing effect of the sealing start temperature is improved. The lower limit of the sum of the longitudinal tensile modulus and the widthwise tensile modulus of the laminated sealant film is preferably 400 MPa or more, more preferably 500 MPa or more, even more preferably 600 MPa or more, and even more preferably 650 MPa or more. When the longitudinal tensile modulus is 400 MPa or more, bag-making processing is easier. The upper limit of the average of the longitudinal and width tensile moduli of the laminated sealant film is preferably 600 MPa or less, more preferably 580 MPa or less, even more preferably 560 MPa or less, even more preferably 540 MPa or less, and particularly preferably 520 MPa or less. When the average of the longitudinal and width tensile moduli is 600 MPa or less, the low-temperature sealing effect of the sealing start temperature is improved. The lower limit of the average of the longitudinal and width tensile moduli of the laminated sealant film is preferably 200 MPa or more, more preferably 250 MPa or more, even more preferably 300 MPa or more, and even more preferably 325 MPa or more. When the longitudinal tensile modulus is 200 MPa or more, bag-making processing is easier.
[0045] (Haze) The haze of the laminated sealant film is preferably 10% or less, more preferably 9% or less, even more preferably 8% or less, even more preferably 7% or less, and particularly preferably 5% or less. If the haze exceeds 10%, the film often has streaks or scratches, and the contents become difficult to see. The haze of the laminated sealant film is preferably 1% or more, more preferably 2% or more, and even more preferably 3% or more. If the haze is 1% or more, the coefficient of friction is less likely to increase.
[0046] (Appearance Unevenness) The closer the melt flow rates of the resin composition or raw resin of the seal layer and the resin composition or raw resin of the intermediate layer, the better the appearance of the laminated sealant film. The more the melt flow rates differ, the more likely appearance unevenness occurs.
[0047] (Delamination) The delamination of a laminated sealant film refers to the case where, for example, delamination occurs between the seal layer and the intermediate layer when measuring the flat seal initiation temperature, the hermetic seal initiation temperature, or the burst strength. If delamination occurs, it becomes difficult to remove the contents, so it is preferable that delamination does not occur. Delamination is likely to occur when the components or component ratios of the resin compositions of the seal layer and the intermediate layer and / or the intermediate layer and the laminate layer are significantly different.
[0048] (Flat seal initiation temperature) The flat seal initiation temperature of the laminated sealant film is preferably 100°C or higher and 150°C or lower, more preferably 105°C or higher and 140°C or lower, even more preferably 116°C or higher and 135°C or lower, and even more preferably 121°C or higher and 130°C or lower. The flat seal initiation temperature preferably has a lower limit of a temperature 30°C or higher than the melting point of the polypropylene-based resin of the seal layer and an upper limit of a temperature 10°C or higher than the melting point of the polypropylene-based resin of the laminate layer. The low-temperature sealing effect of the flat seal initiation temperature is evaluated based on the degree of decrease in heat seal temperature, using the heat seal temperature in Comparative Example 1 described below as a reference. The low-temperature sealability of the flat seal initiation temperature is preferably 5°C or higher, more preferably 10°C or higher, even more preferably 15°C or higher, even more preferably 20°C or higher, particularly preferably 25°C or higher, and most preferably 27°C or higher.
[0049] (Hard seal initiation temperature) The hard seal initiation temperature of the laminated sealant film is preferably 100°C or higher and 160°C or lower, more preferably 110°C or higher and 150°C or lower, and even more preferably 120°C or higher and 140°C or lower. The hard seal initiation temperature is preferably set at a lower limit of 30°C or higher than the lowest melting point of the polypropylene-based resin in the seal layer and at an upper limit of 10°C or higher than the highest melting point of the polypropylene-based resin in the laminate layer. The low-temperature sealing effect of the hard seal initiation temperature is evaluated based on the degree of reduction in the hard seal temperature, using the hard seal temperature in Comparative Example 1 described below as a reference. The low-temperature sealability of the hard seal initiation temperature is preferably above 10°C, more preferably 11°C or higher, even more preferably 12°C or higher, particularly preferably 15°C or higher, and most preferably 20°C or higher.
[0050] (Hot tack property) The hot tack property of the laminated sealant film is preferably such that the tack peel distance is 20 mm or less at a lower temperature. Here, good hot tack property means that the seal strength between sealant films is sufficient even when the resin of the sealant film is in a molten state. The low-temperature sealing effect of hot tack property is evaluated by the degree of decrease in heat sealing temperature, based on the hot tack temperature in Comparative Example 1 described below. The low-temperature sealing property of hot tack property is preferably 5°C or higher, more preferably 10°C or higher, even more preferably 15°C or higher, even more preferably 18°C or higher, and particularly preferably 20°C or higher.
[0051] The seal layer contains a polypropylene-based resin containing an ethylene component, which lowers the melting point, thereby lowering the flat seal initiation temperature and the hermetic seal initiation temperature, thereby achieving low-temperature sealability. Furthermore, the laminate layer, intermediate layer, and seal layer contain a polypropylene-based resin as their main components, which makes it easier to maintain the heat resistance of the laminate sealant film and reduces interlayer delamination.
[0052] (Burst Strength) The burst strength of a laminate sealant film is evaluated using a bag made from the laminate sealant film. When a high burst strength is required, such as for retort sterilization, it is preferably 20 kPa or more, more preferably 25 kPa or more. On the other hand, the burst strength of a laminate sealant film may be 35 kPa or less, or even 30 kPa or less. By optimizing the melting point of the sealing layer and the elastic modulus of the film, it has been confirmed that the laminate sealant film not only achieves a low-temperature sealing effect at least at the flat seal initiation temperature and the hermetic seal initiation temperature, but also improves its burst strength. This is thought to be due to the fact that the bag becomes more easily deformed by optimizing the elastic modulus in particular, thereby improving the burst strength.
[0053] (Static and dynamic friction coefficients) The static and dynamic friction coefficients of the laminated sealant film between the surfaces of the seal layers at a load of 0.5 kgf are preferably 2.0 or less, more preferably 1.0 or less, and even more preferably 0.5 or less. When the static and / or dynamic friction coefficients are 2.0 or less, the films have sufficient slip properties, improving the handling properties of the film as a packaging material.
[0054] This application claims the benefit of priority based on Japanese Patent Application No. 2023-065649, filed on April 13, 2023. The entire contents of the specification of Japanese Patent Application No. 2023-065649, filed on April 13, 2023, are incorporated herein by reference.
[0055] (Melting Point of Resin) The melting point of the resin was measured in accordance with JIS K7121 using a differential scanning calorimeter (DSC60, manufactured by Seiko Instruments Inc.). Specifically, about 5 mg of a sample was packed into an aluminum pan, heated from room temperature to 200°C at a heating / cooling rate of 10°C / min, held at 200°C for 3 minutes, cooled to 23°C, held at 23°C for 3 minutes, and then heated again to 200°C. The temperature of the highest melting endothermic peak was taken as the melting point. When there were two or more melting endothermic peaks, the highest melting endothermic peak was taken as the melting point.
[0056] (Melt Flow Rate) In accordance with JIS K7210, measurements were made using a thermal flow evaluation device (Shimadzu Corporation, capillary rheometer, CFT-500D) under a load of 2.16 kgf at a temperature of 230°C for polypropylene-based resins and at a temperature of 190°C for polyethylene-based resins such as L-LDPE.
[0057] (Average particle size of particles) Inorganic particles or polyethylene particles were dispersed in ion-exchanged water stirred at a predetermined rotation speed (about 5000 rpm) using a high-speed stirrer, and the resulting dispersion was added to Isotone (physiological saline) and further dispersed using an ultrasonic disperser. The particle size distribution was then determined using a Coulter counter method, and the volume average particle size was calculated. The refractive index used was 1.30 for physiological saline, 1.457 for synthetic silica and diatomaceous earth, and 1.54 for polyethylene.
[0058] (Flat seal initiation temperature) A laminated sealant film and a biaxially oriented polyethylene terephthalate film (Toyobo Co., Ltd., Toyobo Ester (registered trademark), E5100, 12 μm) were stacked, folded in half so that the seal layers of the laminated sealant film faced each other, and heat-sealed using a thermal gradient tester (Toyo Seiki Seisakusho Co., Ltd., model: HG-100-2) at a sealing pressure of 0.2 MPa, a sealing time of 1.0 second, and a heat-sealing temperature of 70 to 160 ° C. at 5 ° C. intervals. The heat-sealed sample was cut into strips with a heat-seal width of 15 mm and set in a universal material testing machine (Instron Japan Company Limited, 68TM-5 model). The maximum strength of the peeled seal layers at a speed of 200 mm / min was measured with n = 3, and the heat-sealing strength and heat-sealing temperature at each temperature were plotted. The heat seal temperature at which the strength reached 4.9 N / 15 mm was read from a graph connecting each plot with a straight line, and this was taken as the flat seal initiation temperature.
[0059] (Low-temperature sealing effect of flat seal initiation temperature) The low-temperature sealing effect of the flat seal initiation temperature was evaluated by the difference (°C) between the flat seal initiation temperature in Comparative Example 1 described below. Specifically, the low-temperature sealability evaluation for Example 1 and Comparative Example 1 was made as follows: (flat seal initiation temperature in Comparative Example 1: 160°C) - (flat seal initiation temperature in Example 1: 130°C) = 30°C.
[0060] (Preparation of Laminated Product) A laminated product of a laminated sealant film and a biaxially oriented polypropylene film (Pylen (registered trademark), P2161, 20 μm, manufactured by Toyobo Co., Ltd.) was prepared as follows: First, a dry laminating adhesive (TM569, CAT-10L, manufactured by Toyo-Morton Co., Ltd.) was applied to the corona surface of the biaxially oriented polypropylene film at a solid content of 3 g / m. 2 The solvent was evaporated and removed in an oven at 80° C., and then the corona surface of the laminated sealant film and the adhesive-coated surface were nipped and laminated with a temperature-controlled roll at 60° C. This laminated laminated sealant film was left standing at 40° C. for 2 days.
[0061] (Sealing Initiation Temperature) This laminated sealant film was made into bags using a horizontal pillow packaging machine (FW3301 II / B BD100, manufactured by Fujikikai Co., Ltd.). The conditions were set to a cut length of 250 mm, a height of 45 mm, and a rotation speed of 40 rpm. A sponge scrubber (Kikuron Co., Ltd., Kikuron A (size: 75 × 115 × 36 mm)) was used as the contents. The bag was made at the same temperature for the center seal and end seal portions, and the temperature was lowered in 5°C increments from 170°C. For evaluation, one bag was first cut into two so that two complete end seal portions were obtained. Next, several drops of an evaluation liquid (self-recording ink RED1812E, manufactured by Kobayashi Create Co., Ltd.) were placed in each half bag, and the bag was visually evaluated by rubbing it with a finger to determine whether the evaluation liquid penetrated through the overlapping portion between the center seal and end seal. The lowest heat seal temperature at which the test liquid did not penetrate was determined as the seal initiation temperature.
[0062] (Low-temperature sealing effect of sealing start temperature) The low-temperature sealing effect of sealing start temperature was evaluated by the difference (°C) between the sealing start temperature in Comparative Example 1 described below as a reference. Specifically, the low-temperature sealability evaluation for Example 1 and Comparative Example 1 was made as follows: (sealing start temperature in Comparative Example 1: 155°C) - (sealing start temperature in Example 1: 135°C) = 20°C.
[0063] (Hot tack temperature) The laminated sealant films were stacked with the sealant surfaces facing each other, and subjected to a pressure of 2 kgf / cm at temperatures of 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, and 170°C. 2 After heat sealing for 1 second at a pressure of 1000 kJ / s, a load of 46 g was applied and the distance the sealed portion peeled off was measured. The device used was a HEAT SEAL TESTER, TP-701-B, manufactured by Tester Sangyo Co., Ltd. The temperature at which the peeled distance of the sealed portion was 20 mm or less was defined as the hot tack temperature.
[0064] (Low-temperature sealing effect of hot tack temperature) The low-temperature sealing effect of the hot tack temperature was evaluated by the difference in hot tack temperature (°C) based on the hot tack temperature in Comparative Example 1 described below. Specifically, the low-temperature sealing effect evaluation for Example 1 and Comparative Example 1 was made as follows: (hot tack temperature in Comparative Example 1: 165°C) - (hot tack temperature in Example 1: 135°C) = 30°C.
[0065] (Burst Strength) A horizontal pillow packaging machine (manufactured by Fujikikai Co., Ltd., FW3301 II / B BD100) was used, with a cut length of 250 mm, a height of 45 mm, and a rotation speed of 40 rpm. A sponge scrubber (manufactured by Kikuron Co., Ltd., Kikuron A (size: 75 x 115 x 36 mm)) was used as the contents, and the temperatures of the center seal portion and the end seal portion were set as the sealing start temperatures. A laminated laminated sealant film was produced into a bag. Evaluation was performed using burst strength (JIS Z0238 Test method for heat-sealed flexible packaging bags and semi-rigid containers). Burst strength was measured using a seal strength / burst strength measuring instrument (manufactured by Sun Scientific Co., Ltd., SEAL TESTER, FKT-100-J).
[0066] (Tensile modulus) Measurement was performed under the following conditions in accordance with JIS K7127. First, the tensile modulus of the laminated sealant film in the machine direction (MD) and the transverse direction (TD) of the film was measured three times with a sample length of 100 mm, a sample width of 15 mm, a chuck distance of 20 mm, and a speed of 200 mm / min, and the average value was taken as the tensile modulus in each direction.
[0067] (Delamination) When the flat seal initiation temperature, hermetic seal initiation temperature, or burst strength was measured, delamination of the laminated sealant film was evaluated as occurring if delamination occurred between the seal layer and the intermediate layer and / or between the intermediate layer and the laminate layer.
[0068] (Appearance Unevenness) Appearance unevenness of the laminated sealant film was evaluated by visually inspecting the film for the presence or absence of appearance defects such as layer misalignment, spots, and unevenness.
[0069] (Haze) The haze of the laminate sealant film was measured in accordance with JIS K7105 using a turbidity meter (manufactured by Nippon Denshoku Industries Co., Ltd., model: ZE2000).
[0070] (Static and Dynamic Friction Coefficients) The static and dynamic friction coefficients were determined in accordance with JIS K7125 under the following conditions at 23°C and 65% RH. The load was 0.5 kgf and the tensile speed was 200 mm / min. The measurement surfaces were as follows, and the measurement device used was a TENSILON STM-T-50BP manufactured by Toyo Baldwin Co., Ltd. (B / B) Between the opposing seal layer surfaces of the laminate sealant film itself, i.e., between the seal layer surfaces. (F / B) Between the opposing seal layer surfaces of the laminate sealant film itself and the laminate layer surface. (CP / CP) Between the opposing seal layer surfaces of the laminate sealant film, i.e., between the seal layer surfaces. (OP / CP) Between the laminate layer surface of the laminate sealant film and the surface of the biaxially oriented polypropylene film.
[0071] (Polypropylene-based resin) The following resins were used as polypropylene-based resins: 1) WF836DG3 (manufactured by Sumitomo Chemical Co., Ltd., Noblene (registered trademark), homopropylene, melting point 158°C, melt flow rate 7.0 g / 10 min, tensile modulus 1,500 MPa) 2) FL8115A (manufactured by Sumitomo Chemical Co., Ltd., Noblene (registered trademark), propylene-ethylene-butene random copolymer, melting point 148°C, melt flow rate 7.0 g / 10 min, tensile modulus 1,000 MPa) 3) FL6632G (manufactured by Sumitomo Chemical Co., Ltd., Noblene (registered trademark), propylene-ethylene-butene random copolymer, melting point 138°C, melt flow rate 6.0 g / 10 min, tensile modulus 1,100 MPa) 4) FL6745A (manufactured by Sumitomo Chemical Co., Ltd., Noblen (registered trademark), propylene-ethylene-butene random copolymer, melting point 130°C, melt flow rate 6.0 g / 10 min, tensile modulus 700 MPa) 5) WF577PG (manufactured by Sumitomo Chemical Co., Ltd., Noblen (registered trademark), propylene-ethylene-butene random copolymer, melting point 142°C, melt flow rate 3.2 g / 10 min, tensile modulus 900 MPa) 6) S131 (manufactured by Sumitomo Chemical Co., Ltd., Noblen (registered trademark), propylene-ethylene-butene random copolymer, melting point 132°C, melt flow rate 1.5 g / 10 min, tensile modulus 650 MPa)
[0072] (Polyethylene Resin) The following resin was used as the polyethylene resin: 1) FV405 (manufactured by Sumitomo Chemical Co., Ltd., Sumikathene (registered trademark) E, linear low-density polyethylene resin, melting point 118°C, melt flow rate 3.8 g / 10 min, flexural modulus 220 MPa)
[0073] (Anti-blocking agent) The following particles were used as the anti-blocking agent: 1) Synthetic silica: KMP130-2 (average particle size 2 μm, manufactured by Shin-Etsu Chemical Co., Ltd.) 2) Synthetic silica: KMP130-4 (average particle size 4 μm, manufactured by Shin-Etsu Chemical Co., Ltd.) 3) Ultra-high molecular weight polyethylene particles: PM200 (average particle size 10 μm, manufactured by Mitsui Chemicals, Inc.)
[0074] (Organic Lubricant) The following compounds were used as organic lubricants: 1) Erucic acid amide: Brand name Diamid L-200 (melting point 81°C, manufactured by Mitsubishi Chemical Corporation) 2) Behenic acid amide: Brand name D1007 (melting point 110°C, manufactured by Tokyo Chemical Industry Co., Ltd.)
[0075] (Masterbatches) 1) Silica masterbatch: Noblen (registered trademark) FL6745A manufactured by Sumitomo Chemical Co., Ltd. was mixed with silica (KMP-130-2 manufactured by Shin-Etsu Chemical Co., Ltd., average particle size 2 μm) to prepare a masterbatch containing 15% by mass of silica. 2) Silica masterbatch: Noblen (registered trademark) FL6745A manufactured by Sumitomo Chemical Co., Ltd. was mixed with silica (KMP-130-4 manufactured by Shin-Etsu Chemical Co., Ltd., average particle size 4 μm) to prepare a masterbatch containing 12% by mass of silica. 3) Ultra-high molecular weight polyethylene particle masterbatch: Noblen (registered trademark) FL6745A manufactured by Sumitomo Chemical Co., Ltd. was mixed with ultra-high molecular weight polyethylene particles (Mipelon PM200 manufactured by Mitsui Chemicals, Inc., average particle size 10 μm) to prepare a masterbatch containing 10% by mass of ultra-high molecular weight polyethylene particles. 4) Erucamide masterbatch: A masterbatch containing 5% by mass of erucamide was prepared by mixing erucamide with Noblen (registered trademark) FL6745A manufactured by Sumitomo Chemical Co., Ltd. 5) Behenamide masterbatch: A masterbatch containing 2% by mass of behenamide was prepared by mixing behenamide with Noblen (registered trademark) FL6745A manufactured by Sumitomo Chemical Co., Ltd.
[0076] Example 1: The laminate layer was made from WF836DG3, and the intermediate layer and seal layer from FL6745A. The seal layer was made from the resins and additives listed in Table 1, using appropriate masterbatches. The resins were melted at 240°C in three extruders, filtered through a sintered filter with a filtration accuracy of 60 μm, and then co-extruded into a sheet from a T-die. The laminate layer, intermediate layer, and seal layer were melt-extruded to a thickness ratio of 20:60:20% by volume. The resulting laminate was cooled and solidified on a cooling roll at 30°C, then wound up into a roll at a speed of 20 m / min. A laminate sealant film with a thickness of 30 μm and a laminate layer wet tension of 45 mN / m was obtained.
[0077] A dry laminating adhesive (TM569, CAT-10L, manufactured by Toyo-Morton Co., Ltd.) was applied to the corona surface of a biaxially stretched polypropylene film (Pylen (registered trademark), P2161, 20 μm, manufactured by Toyobo Co., Ltd.) at a solid content of 3 g / m 2 The solvent was evaporated in an oven at 80°C, and then the corona surface of the resulting laminate sealant film and the adhesive-coated surface were nipped between temperature-controlled rolls at 60°C to laminate them. Prior to lamination, the surface of the laminate sealant film on the laminate layer side was subjected to corona treatment. The laminated laminate sealant film was left to stand at 40°C for 2 days. The evaluation results are shown in Table 2.
[0078] (Examples 2 to 10) A laminated sealant film was obtained in the same manner as in Example 1, except that a master batch was appropriately used to make the laminate layer, intermediate layer, and seal layer using the resins and additives shown in Table 1 as raw materials, and then laminated laminated sealant films were produced. The evaluation results are shown in Table 2.
[0079] The laminated sealant films of Examples 1 to 10 exhibited good appearance without delamination or uneven appearance. Furthermore, the flat seal initiation temperature and hermetic seal initiation temperature could be reduced, demonstrating good low-temperature bag-forming properties.
[0080] Comparative Examples 1 to 9 A laminated sealant film was prepared in the same manner as in Example 1, except that the laminate layer, intermediate layer, and seal layer were prepared using appropriate masterbatches made from the resins and additives shown in Table 3. In Comparative Examples in which FL6745A was not used in the seal layer, a masterbatch was prepared using the propylene-based resin or polyethylene-based resin used in the seal layer instead of FL6745A. The evaluation results are shown in Table 4.
[0081] The laminate sealant film obtained in Comparative Example 1 had high flat sealing temperatures and hermetic sealing temperatures. The laminate sealant film obtained in Comparative Example 2 had a low melting point of the seal layer, but insufficient low-temperature sealing effect at the flat sealing temperature, and a high elastic modulus, resulting in poor low-temperature sealing effect at the hermetic sealing temperature. The laminate sealant film obtained in Comparative Example 3 had a low melting point of the seal layer, but insufficient low-temperature sealing effect at the flat sealing temperature, and a low elastic modulus, but also poor low-temperature sealing effect at the hermetic sealing temperature. The laminate sealant film obtained in Comparative Example 4 had a low melting point of the seal layer, but sufficient low-temperature sealing effect at the flat sealing temperature, but a high elastic modulus, resulting in poor low-temperature sealing effect at the hermetic sealing temperature. The laminate sealant film obtained in Comparative Example 5 had a low elastic modulus, but a high melting point of the seal layer, resulting in poor low-temperature sealing effect at the flat sealing temperature and hermetic sealing temperature. The laminate sealant film obtained in Comparative Example 6 had a large melt flow rate ratio between the intermediate layer and the seal layer, resulting in uneven appearance. The laminate sealant film obtained in Comparative Example 7 had a seal layer made of polyethylene resin, resulting in interlayer delamination between the seal layer and the intermediate layer. The laminated sealant film obtained in Comparative Example 8 had a low melting point of the seal layer but an insufficient low-temperature effect at the flat sealing temperature, and also had a low elastic modulus but an insufficient low-temperature sealing effect at the hermetic sealing temperature. The laminated sealant film obtained in Comparative Example 9 had a low melting point of the seal layer but an insufficient low-temperature effect at the flat sealing temperature, and also had a low elastic modulus but an insufficient low-temperature sealing effect at the hermetic sealing temperature. Furthermore, due to the large melt flow rate ratio between the laminate layer and the intermediate layer, uneven appearance was observed.
[0082] The results are shown in Tables 1 to 4. The content of additives in Tables 1 and 3 indicates the ratio to 100% by mass of resin. In Tables 2 and 4, "resin" means "resin composition."
[0083]
[0084]
[0085]
[0086]
[0087] The laminated sealant film of the present invention has excellent low-temperature bag-forming properties and is therefore suitable as a packaging material for many products, such as foods, beverages, pharmaceuticals, and chemicals. In particular, it can be suitably used for automatically forming pillow packaging bags, gusset packaging bags, three-side seal packaging bags, and the like while packaging the contents.
Claims
1. A laminated sealant film that satisfies the following 1) to 7). 1) A laminated sealant film that includes at least a laminate layer, an intermediate layer, and a seal layer in this order. 2) The laminate layer, the intermediate layer, and the seal layer are each made of a polypropylene-based resin composition. 3) The ratio of the melt flow rate of the polypropylene-based resin composition of the intermediate layer to the melt flow rate of the polypropylene-based resin composition of the laminate layer is 0.6 or more and 2.0 or less. 4) The ratio of the melt flow rate of the polypropylene-based resin composition of the seal layer to the melt flow rate of the polypropylene-based resin composition of the intermediate layer is 0.6 or more and 2.0 or less. 5) The melt flow rates of the polypropylene-based resin compositions of the laminate layer, the intermediate layer, and the seal layer are 1 g / 10 min (load 2.16 kgf) or more and 9 g / 10 min (load 2.16 kgf) or less, respectively. 6) The melting point of the polypropylene resin composition of the seal layer is 100° C. or more and 140° C. or less. 7) A laminated sealant film having a tensile modulus in the longitudinal direction of 600 MPa or less.
2. The laminate sealant film according to claim 1, wherein the polypropylene resin composition contains a propylene random copolymer.
3. The laminate sealant film according to claim 1 or 2, wherein the main peak of the melting point of the laminate sealant film is 120°C or higher and 160°C or lower.
4. The laminated sealant film according to claim 1 or 2, wherein the static friction coefficient between the surfaces of the sealing layers is 1.0 or less.
5. The laminated sealant film according to claim 1 or 2, wherein the coefficient of dynamic friction between the surfaces of the sealing layers is 1.0 or less.
6. The laminate sealant film of claim 1 or 2, wherein the sealing layer comprises silica particles.
7. The laminate sealant film of claim 1 or 2, wherein the sealing layer comprises erucamide.
8. The laminate sealant film according to claim 1 or 2, wherein the sealing layer comprises organic particles.
9. The laminate sealant film according to claim 1 or 2, wherein the tensile modulus in the longitudinal direction is 200 MPa or more and 600 MPa or less.
10. The laminated sealant film according to claim 1 or 2, which satisfies the following requirements 8) and 9). 8) The difference between the melting point of the polypropylene resin composition of the laminate layer and the melting point of the polypropylene resin composition of the intermediate layer is 30° C. or less. 9) The difference between the melting point of the polypropylene resin composition of the intermediate layer and the melting point of the polypropylene resin composition of the seal layer is 30° C. or less.
Citation Information
Patent Citations
Laminated polypropylene non-stretched film
JP2007237641A
Impact resistant film and laminate using the same
JP2017132186A
Unstretched polypropylene-based resin film
JP2020075400A
Non-stretched multilayer film
JP2021176691A
Film for sealant
JP2022035851A
Cited By
Composite film, packaging material containing composite film, packaging mode and application of packaging material
CN119567687A
A composite film, a packaging material comprising the composite film, a packaging method thereof, and its application.
CN119567687B
Polypropylene film, packaging material, and package
JP2026065766A
Polypropylene-based unstretched film and film laminate
JP2026106137A
Polypropylene film, packaging material, and packaging body
JP7789873B1