METHOD FOR MANUFACTURING A PART FROM AN HEA / CCA ALLOY
The exogenous addition of nitrided particles in the additive manufacturing of HEA/CCA alloys improves mechanical properties like tensile strength and elastic stress while maintaining elongation, addressing the limitations of existing methods by enhancing the alloy's microstructure and composition.
Patent Information
- Application Number
- FR2021012260
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-11-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-11-19
AI Technical Summary
Existing methods for manufacturing high entropy alloys (HEA) and multi-component alloys (CCA) face challenges in achieving improved mechanical properties without compromising elongation, particularly in the 3d TM HEA/CCA family, where additions like aluminum and nanoparticles can either increase hardness at the expense of elongation or introduce compositional heterogeneities.
A method involving the exogenous addition of nitrided particles, such as aluminum nitride, during the additive manufacturing process through dry mixing, which enhances mechanical properties like tensile strength and elastic stress while maintaining or improving elongation, by dissolving or forming hardening precipitates within the alloy matrix.
The process results in parts with enhanced mechanical properties, including increased tensile strength and elastic stress, without negatively affecting elongation, through the integration of nitrided particles that modify the alloy's microstructure and chemical composition.
Smart Images

Figure 00000015_0000 
Figure 00000015_0001 
Figure 00000016_0000
Abstract
Description
Title of the invention: METHOD FOR MANUFACTURING A PART FROM AN HEA / CCA ALLOY Technical field
[0001] The present invention relates to the general field of manufacturing parts made of high entropy alloy (HEA) or multi-component alloy (CCA).
[0002] The invention relates to a method of manufacturing a part from such an alloy.
[0003] The invention is particularly interesting since it makes it possible to improve the mechanical resistance of high entropy alloys and CCA alloys, in particular those of the 3d TM HEA / CCA family.
[0004] The invention finds applications in numerous industrial fields, and in particular in the fields of energy, transport, medicine and defense. STATE OF THE PRIOR ART
[0005] High entropy alloys (HEA) are composed of at least five main elements in equiatomic or equivalent proportions. The configurational entropy of these alloys is maximized and thus stabilizes a single concentrated solid solution, with a face-centered cubic (FCC), body-centered cubic (BC) or hexagonal close-packed (HCP) crystallographic structure, for example. The microstructure of HEA alloys is single-phase. This single phase makes it possible to achieve new mechanical properties.
[0006] Today, research extends to multi-component alloys which contain at least 3 major elements in equiatomic proportion (also called CCA for 'complex concentrated alloy' or MPEA for Multi-Principal Element Alloy (MPEA)). These alloys do not necessarily result in the formation of a single-phase solid solution.
[0007] High-entropy and multi-component alloys can be shaped by Additive Manufacturing (AM) processes. The processes concerned have in common the use of the raw material in powder form, and the shaping of the alloy in a liquid process. The processes concerned include, but are not limited to, powder bed fusion (PBF) processes, whether laser fusion or electron beam fusion), and concentrated energy deposition (DED) processes for Directed Energy Deposition (LENS©).
[0008] Among these HEA / CCAs alloys, the 3d substructure family containing transition metals, and in particular Ti, V, Cr, Mn, Fe, Co, Ni, Cu with which Al is often associated, is studied for its innovative mechanical properties.
[0009] Several approaches have already enabled the improvement of the mechanical properties of HEA / CCA type alloys.
[0010] For example, it is known that the Al content influences the hardness of the alloy. In the AlxCoCrFeNi alloy, the addition of aluminum increases the hardness [1,2].
[0011] Another solution consists of adding nanoparticles harder than the matrix by mechanosynthesis to the incoming powder (so-called exogenous addition process). In other words, the addition particles are integrated directly into the HEA particles.
[0012] For example, Li et al. added significant concentrations (5 - 12mass%) of TiN to a CoCrFeMnNi alloy. The use of Ti is particularly known to result in equiaxed structures for HEAs formed by additive manufacturing. According to this study, the breaking stress was increased by two. However, the elongation decreased [3].
[0013] Another solution consists of adding chemical elements during the atomization step of the incoming powder (so-called endogenous addition process). These elements can combine to form germinating particles (useful for refining the microstructure) and / or form hardening particles, or become trapped in solid solution during the cooling of the alloy printed by an additive manufacturing process.
[0014] For example, Park et al. added atomic % of C in their CoCrFeMnNi alloy obtained by FLLP. Intermetallics in the form of carbides are formed. An improvement in the mechanical properties obtained by tensile tests could be observed. However, the presence of these brittle carbides can reduce the fatigue properties and / or the elongation of the materials thus obtained [4].
[0015] Song et al. added 1.8 at% N by atomization under nitrogen (endogenous addition process) to their CoCrFeNi alloy formed by laser powder bed fusion. A significant improvement in mechanical properties such as work hardening or even the tensile strength of the alloy could be observed compared to the same alloy without nitrogen as well as an increase in elongation. However, in this method two batches of powders were atomized for comparison. However, compositional and also physical heterogeneities can preexist between the batches: for example, the nickel content can vary from one batch to another [5]. Statement of the invention
[0016] An aim of the present invention is to propose a method for the additive manufacturing of parts made of high entropy alloy (HEA) or multi-component alloy (CCA). making it possible to remedy at least in part the drawbacks of the prior art and making it possible to obtain a part having good mechanical properties.
[0017] For this purpose, the present invention proposes a method for manufacturing a part made of high-entropy alloy or multi-component alloy by additive manufacturing comprising a step during which a layer of a mixture of powders is locally melted and then solidified, the mixture of powders comprising:
[0018] - first particles in an HEA or CCA alloy, and
[0019] - second particles nitrided in a metal nitride chosen from a nitride aluminum, copper nitride, chromium nitride, silicon nitride, boron nitride, tungsten nitride, iron nitride, nickel nitride, manganese nitride or a mixture thereof.
[0020] The invention is fundamentally distinguished from the prior art by the exogenous addition of elements thanks to a dry mixing step, allowing the improvement of the mechanical properties of the final alloy, in particular good tensile properties. Moreover, against all expectations, the increase in elastic and breaking stresses is not at the expense of elongation. It is, in fact, widely known from the literature that, classically, these quantities are relatively inversely proportional.
[0021] It was not a priori obvious that the nitrided particles would remain attached to the HEA or CCA powder particles during mixing and during printing.
[0022] When HEA powders are transformed into the liquid state, the nitrided particles dissolve in the liquid bath and / or remain in the form of hardening precipitates.
[0023] In the case of dissolution of the nitrided particles, the nitrogen atoms are released and move into an interstitial position (the mesh is then distorted, thus creating clusters of dislocations at the level of these atoms in solid solution) and / or recombine to form hardening precipitates; these effects contribute to hardening the matrix. At the same time, the released atoms (other than the nitrogen atoms) cause a modification of the chemical composition of the HEA mother phase, making it possible to move on the composition isopleth and thus promote the precipitation of a structure little by little CC for example (CFC->CFC+CC->CC).
[0024] The elements forming the nitrided particles are part of the final part either in the form of precipitates or in the form of atoms in interstitial position (in solid solution).
[0025] The second particles are preferably chosen from CuxNy such as for example Cu3N, CrxNy such as for example CrN, SixNy such as for example Si3N4, BxNy such as for example BN, WxNy such as for example W2N or WN, FexNy such as for example Fe2N or Fe4N, NixNy such as Ni3N, or MnxNy such as Mn4N.
[0026] x and y are the stoichiometric quantities of atoms.
[0027] Advantageously, the second particles are made of AlxNy and the stoichiometric ratios x / y of the Al and N atoms are greater than 0 and less than or equal to 5, preferably greater than 0 and less than or equal to 2, preferably 1.
[0028] Advantageously, the first particles have a larger dimension between 10 pm and 120 pm, and preferably between 20 pm and 65 pm. The inventors have observed a significant improvement in the elastic stress in connection with the addition of nitride.
[0029] Advantageously, the alloy is an alloy of the 3d TM family.
[0030] Advantageously, the high entropy alloy contains Ai and four elements selected from Co, Cr, Fe, Ni, Ti, Cu and Mn.
[0031] Even more advantageously, the high entropy alloy is AlxCoCrFeNi, AlxCoCuFeNi, AlxCoCrFeTi, AlxCrCuFeNi, AlxCrFeCuCo AlxCrCoCuFeNi or Alx CoCrFeTi, AlxCoCrFeTiNi, or AlxCoCrFeMnNi with more preferably x between 0.1 and 3.
[0032] Advantageously, the mixture of powders comprises between 0.5% and 4% by mass of second particles, and preferably between 0.5% and 3% by mass.
[0033] Advantageously, the second particles have a larger dimension between 5 nm and 5000 nm, preferably 100 and 1000 nm, even more preferably 200 and 600 nm.
[0034] Advantageously, the second particles are made of aluminum nitride, chromium nitride or a mixture of these two nitrides.
[0035] Advantageously, the additive manufacturing process is a laser powder bed fusion process or a selective electron beam powder bed fusion process.
[0036] The Laser Powder Bed Fusion (LPBF) process can comprise the following steps:
[0037] a) providing a powder comprising HEA or CCA alloy particles,
[0038] b) depositing a layer of powder on a solid substrate or on a layer of powder underlying,
[0039] c) locally melting the layer of powder deposited by scanning with a laser beam, so as to form a molten bath,
[0040] d) cooling the molten bath so as to solidify it,
[0041] repeating several times the cycle comprising steps b), c) and d) whereby a part is formed from HEA or CCA alloy,
[0042] the second particles being added before step c), and preferably before step b).
[0043] The method can be implemented regardless of the means of adding the second nitrided particles:
[0044] - by grafting: the powder provided in step a) comprises the HEA alloy particles functionalized by second particles; which makes it possible to easily modify the volume ratio between the powders when mixing the powder.
[0045] - by inclusion: the second particles are added by mechanosynthesis.
[0046] Advantageously, the mixing of powders is carried out in a dynamic mixer. 3D.
[0047] The process has many advantages:
[0048] - be simple to implement: the mixture is produced using a dry, rapid process, and it is easy to implement,
[0049] - be inexpensive, and therefore interesting from an industrial point of view,
[0050] - be able to easily store / handle powders,
[0051] - be easily adaptable to a wide range of HEA and CCA alloys, (and second particles)
[0052] - to be able to use the parameters conventionally used in the processes of additive manufacturing,
[0053] - obtain parts with improved mechanical properties and conservation of the elongation,
[0054] - to be able to obtain new microstructural perspectives,
[0055] - to be able to investigate different close compositions, for example by incrementing the quantity of chemical elements in a controlled manner, to find the compositions leading to parts with the best mechanical properties.
[0056] The invention also relates to a part made of HEA or CCA alloy obtained by such a method. The part may comprise precipitates of metal nitrides, for example aluminum nitrides, copper nitrides, chromium nitrides, silicon nitrides, boron nitrides, tungsten nitrides, iron nitrides, nickel nitrides, manganese nitrides or a mixture thereof.
[0057] Advantageously, the metal nitrides represent between 0.5% by mass and 4% by mass of the alloy, and preferably between 0.5% and 3% by mass relative to the total mass of the alloy.
[0058] The part comprises, for example, nitrided particles having a size between 1 and 500 nm and preferably between 2 and 100 nm.
[0059] Advantageously, the maximum tensile strength of the part is between 100 and 3000 MPa, or even between 600 and 2000 MPa.
[0060] Other characteristics and advantages of the invention will emerge from the additional description which follows.
[0061] It goes without saying that this additional description is given only as an illustration of the subject of the invention and must in no case be interpreted as a limitation of this subject. Brief description of the drawings
[0062] The present invention will be better understood on reading the description of exemplary embodiments given purely for informational purposes and in no way limiting, with reference to the appended drawings in which:
[0063] [Fig-1] is a photograph obtained using a scanning electron microscope of HEA alloy particles, according to one embodiment of the invention.
[0064] [Fig.2] a snapshot obtained with a scanning electron microscope of AIN particles, according to one embodiment of the invention.
[0065] [Fig.3] is a snapshot obtained using a scanning electron microscope of particles in HEA alloy functionalized by AIN particles, according to one embodiment of the invention.
[0066] [Fig.4] is another image obtained with a scanning electron microscope of HEA alloy particles functionalized by AIN particles, according to one embodiment of the invention.
[0067] [Fig.5A] is a snapshot corresponding to the boxed area of [Fig.4],
[0068] [Fig.5B]
[0069] [Fig.5C]
[0070] [Fig.5D]
[0071] [Fig.5E]
[0072] [Fig.5F]
[0073] [Fig.5G] are elementary analyses of the area represented in [Fig.5A].
[0074] [Fig.6] is a graph representing the elastic limit (Rp0.2), the maximum limit flow rate (Rm), elongation (A%) and microhardness (HV) of a conventional HEA alloy (black) and a modified HEA alloy obtained according to the invention (grey).
[0075] DETAILED DESCRIPTION OF PARTICULAR EMBODIMENTS
[0076] The additive manufacturing process of a high entropy alloy part or a multi-component comprises the following steps:
[0077] i) providing a powder of first particles in high entropy alloy HEA (for 'high entropy alloys') or in multi-component alloy CCA (for 'complex concentrated alloys'),
[0078] ii) providing a powder of second particles,
[0079] iii) printing a HEA alloy part by additive manufacturing, from a mixture containing the first particles and the second particles,
[0080] iv) optionally carrying out a heat treatment on the printed part at a temperature lower than the melting temperature of the alloy, preferably at a temperature higher than 500°C.
[0081] The second particles preferably represent from 0.5% to 4% by mass, and even more preferably from 0.5 to 3% by mass relative to the total mass of the powder mixture.
[0082] According to an advantageous embodiment, the first particles have a larger dimension between 100 nm and 120 pm and the second particles have a larger dimension between 5 nm and 5000 nm and, preferably, between 100 nm and 1000 nm, even more preferably between 200 nm and 600 nm.
[0083] Preferably, the first particles are substantially spherical and their largest dimension is their diameter.
[0084] Preferably, the first particles are HEA or CCA particles containing aluminum.
[0085] For example, CCA particles from the 3d TM family containing aluminum or HEA particles from the 3d TM family containing aluminum will be chosen.
[0086] Preferably, the first particles are HEA particles of the 3d TM family containing Ai and four elements among Co, Cr, Fe, Ni, Ti, Cu, Mn.
[0087] For example, we will choose first particles made of AlxCoCrFeNi, AlxCoCuFeNi, AlxCrCuFeNi, AlxCrFeCuCo AlxCrCoCuFeNi, AlxCoCrFeTi, AlxCoCrFeTiNi, or AlxCoCrFeMnNi more preferably with x between 0.1 and 3. For example, we will choose Al0j3CoCrFeNi.
[0088] According to a first advantageous embodiment, the second particles are chosen from AlxNy, for example AIN, CuxNy such as for example Cu3N, CrxNy such as for example CrN, SixNy such as for example Si3N4, BxNy such as for example BN, WxNy such as for example W2N or WN, FexNy such as for example Fe2N or Fe4N, NixNy such as for example Ni3N, or MnxNy such as for example Mn4N.
[0089] It can also be a mixture of them.
[0090] According to a second advantageous embodiment, it may be a compound of formula AlxMyN, with M a metallic element, preferably a transition metal, preferably AlxCryN for example AlCrN.
[0091] These different embodiments and their combination (use of a mixture of powders of type A1XM and / or compound of type AlxMyN) make it possible to play on different composition isopleths while inserting nitrogen into the alloy by solid means.
[0092] Preferably, first particles made of aluminum nitride are chosen.
[0093] Advantageously, the HEA particles are functionalized by the nitride particles.
[0094] The mixture is preferably produced by the dry method.
[0095] The first particles and the second particles may be mixed with the 3D dynamic mixer, for example with a Turbula® mixer. Alternatively, it could be a mechanosynthesis process.
[0096] In step iii), the HEA alloy part is printed by additive manufacturing. The deposition machines used for additive manufacturing processes comprise, for example, a powder delivery system, a device for spreading and homogenizing the surface of the powder, a beam (for example, an infrared laser beam at a wavelength of approximately 1000 nm), a scanner for directing the beam, and a substrate (also called a plate) which can descend vertically (along a Z axis perpendicular to the powder bed).
[0097] According to a first embodiment variant, step iii) is advantageously carried out by laser fusion on a powder bed. It may comprise the following steps:
[0098] a) depositing the powder mixture so as to form a powder layer,
[0099] b) locally melting the powder mixture layer, by scanning with a laser beam, so as to form a molten bath,
[0100] c) cooling the molten bath to solidify it, the solidified molten bath constituting the first elements of the parts to be constructed.
[0101] According to another embodiment variant, step iii) can be carried out by selective electron beam melting. It can comprise the following steps:
[0102] a) depositing the powder mixture so as to form a powder layer,
[0103] b) locally melting the powder mixture layer, by scanning with an electron beam, so as to form a molten bath,
[0104] c) cooling the molten bath to solidify it, the solidified molten bath constituting the first elements of the parts to be constructed.
[0105] In these variants, the second particles can be added by grafting or inclusion.
[0106] A beam of sufficient energy is used to melt the first particles. This produces a molten bath comprising a first surface and a second surface. The first surface is in contact with a solid substrate or with the underlying powder layer. The second surface is a free surface interfacing with the atmosphere of the manufacturing chamber. The two surfaces delimit a volume, called the melt pool.
[0107] The deposited layer may be locally melted or completely melted. It is possible to form one melted zone or a plurality of melted zones.
[0108] The melting step makes it possible to create melted patterns in the layer of the powder mixture. One or more areas of melted particles can be made to form the desired pattern. The particles forming the pattern melt completely so as to lead, during solidification (step c), to one or more areas solidified into an HEA alloy.
[0109] Steps a), b) and c) are repeated at least once so as to form at least one other solidified zone on the first solidified zone. The process is repeated until the final shape of the part is obtained, the first layer of powder mixture being formed on a substrate (also called a plate).
[0110] By way of illustration and not limitation, the parameters of the manufacturing process of the part printed by laser fusion on a powder bed are:
[0111] - between 50 and 500W for the laser power,
[0112] - between 100 and 5000 mm / s for the laser speed,
[0113] - between 25 and 120pm for the distance between two vector spaces (“hatch” in Anglo-Saxon terminology),
[0114] - between 15 and 100 pm for the layer thickness.
[0115] By way of illustration and not limitation, the parameters of the manufacturing process of the part printed by electron beam fusion on a powder bed are:
[0116] - between 50 and 3000W for the power of the electron beam,
[0117] - between 100 and 8000 mm / s for the speed of the electron beam,
[0118] - between 25 and 150pm for the distance between two vector spaces (“hatch” in Anglo-Saxon terminology),
[0119] - between 40 and 150pm for the layer thickness.
[0120] The assembly can be confined in a thermally closed and inerted enclosure, to control the atmosphere, but also to avoid the dissemination of powders. Ideally the printing atmosphere is under argon or nitrogen.
[0121] The unsolidified powders are then removed and the final part is detached from the substrate.
[0122] The part can then advantageously be subjected to heat treatment (step iv).
[0123] Heat treatment (or possibly a suitable operating temperature) would make it possible to move along the phase diagram of the alloy, promoting for example L12B2, CC, sigma or AIN germination thanks to the induced elementary modifications.
[0124] To control this precipitation, the use of a heated bed during printing, or another heating technique, is a possible solution.
[0125] For example, the AlxCoCrFeNi system offers many perspectives, due to the multiple phases achievable using annealing (in situ or post-printing). For example, annealing and the Al content can favor the formation of the Ll2et B2 phase (ordered CC) [6].
[0126] This annealing step can reduce internal stresses and improve mechanical properties. The temperature is preferably lower than the melting temperature of the alloy, for example lower than 1400°C for Al0j3CoCrFeNi. Preferably, the heat treatment is carried out at a temperature of at least 500°C.
[0127] The part thus obtained (after the printing and heat treatment steps) has a fine microstructure and good mechanical properties, particularly for its tensile properties.
[0128] An increase in the mass percentage of elements constituting the second particles is observed within the alloy formed, confirming their integration into the part obtained by the method described above. For example, for second particles of aluminum nitride, an increase in the mass percentage of N and Al is observed within the alloy formed.
[0129] In the part obtained, a possible precipitation in the form of dispersed nitrides is possible.
[0130] The size of the nitrided precipitates (for example AIN) of the part is between 1 and 500 nm and preferably between 2 and 100 nm.
[0131] The tensile stress of a part obtained by such a method is advantageously between 100 and 3000 MPa, preferably between 600 and 2000 MPa.
[0132] The invention opens up new microstructural and structural possibilities.
[0133] Although this is in no way limiting, the invention particularly finds applications in the fields of energy, transport, medicine and even defense.
[0134] Illustrative and non-limiting example of an embodiment:
[0135] We will now describe in more detail the manufacture of HEA alloy parts. The parts are 10mm*10mm*10mm cubes and 60mm*12mm*12mm tensile specimens.
[0136] The parts are obtained from a mixture comprising a powder of HEA particles and 1% by mass of AlN particles.
[0137] The HEA particles are made of an alloy called Al0> 3CoCrFeNi formed mainly of Al, Co, Cr, Fe and Ni.
[0138] The particle size of the HEA powder used is as follows: dl0=20pm, d50=29pm and d90=43pm.
[0139] The parts are manufactured using a laser powder bed fusion printing process. Approximately 5kg of mixture was used.
[0140] The HEA particles were characterized by SEM. The particles are spherical ([Fig.l]).
[0141] The AIN powder (x=y=l) was also characterized by SEM ([Fig.2]).
[0142] The mixture is made in a nano glove box in a pot (6.5L) containing:
[0143] - 5000 g of HEA powder,
[0144] - 50 g of AIN powder (for a mixture at 1% by mass),
[0145] - 250 mL of Zirconia beads with a diameter of 5 mm.
[0146] The mixture is passed through Turbula® for 30 h.
[0147] The pot is then returned to the nano glove box in order to sieve coarsely (1mm). The aim is to recover the Zirconia beads necessary for homogenizing the mixture.
[0148] Figures 3 and 4 are SEM images of the powder mixture. These images confirm the good adhesion of the AIN particles to the HEA powders. The chemical nature of the different elements present was also studied. [Fig.5A] is the SEM-BSE image of the area studied in [Fig.4]. Figures 5B to 5G show the presence of different elements (Al, Ni, N, Cr, Co, Fe respectively) in the mixture.
[0149] When adding 1% by mass of AIN, the amount of N in the alloy increases from 0.048 ±0.006 to 0.121 ±0.008 and the amount of Al increases from 3.6 ±0.2 to 3.9 ±0.3 (mass percentages).
[0150] Once these steps are completed, the mixture is used to manufacture the parts with the 3D printing machine.
[0151] The FLLP conditions for obtaining the densest cubes are:
[0152] - Laser power: 150-250 W,
[0153] - Laser speed: 500-2000 mm / s,
[0154] - Vector space: 40-100 pm,
[0155] - Layer thickness (powder bed): 20-30 pm.
[0156] An addition of 1% by mass of AIN for this HEA powder makes it possible to improve the elastic stress by approximately 8% and the breaking stress by approximately 10% without deteriorating the elongation. REFERENCES
[0157] [1] JC Rao et al., Acta Materialia 131, 206 (2017)
[0158] [2] W.-R. Wang et al., Intermetallics 26, 44 (2012)
[0159] [3] B. Li, B. Qian et al., Materials Letters 252, 88 (2019)
[0160] [4] JM Park et al., Kim, Materials Research Letters 8, 1 (2020)
[0161] [5] M. Song et al., Applied Materials Today 18, 100498 (2020)
[0162] [6] B. Gwalani et al., Materials Research Letters 7, 267 (2019)
Claims
Claims
1. Method for manufacturing a part made of a high-entropy alloy or a multi-component alloy by additive manufacturing comprising a step during which a layer of a mixture of powders is locally melted and then solidified, characterized in that the mixture of powders comprises, relative to the total mass of the mixture of powders: - first particles made of a high-entropy alloy or a multi-component alloy, and - between 0.5% and 4% by mass of second particles made of aluminum nitride.
2. Method according to claim 1, characterized in that the mixture of powders comprises between 0.5% and 3% by mass of second particles, relative to the total mass of the mixture of powders.
3. Method according to any one of the preceding claims, characterized in that the second particles have a larger dimension between 5nm and 5000nm, preferably between 100 and 1000 nm, even more preferably between 200 and 600 nm.
4. 4. Method according to any one of the preceding claims, characterized in that the second particles are made of AlxNy and the stoichiometric ratios x / y of the Al and N atoms are greater than 0 and less than or equal to 5, preferably greater than 0 and less than or equal to 2, preferably 1.
5. 5. Method according to any one of the preceding claims, characterized in that the first particles have a largest dimension between 10pm and 120pm, and preferably between 20pm and 65pm.
6. 6. Method according to any one of the preceding claims, characterized in that the alloy is an alloy of the 3d TM family.
7. 7. A method according to any one of the preceding claims, characterized in that the high entropy alloy contains Ai and four elements selected from Co, Cr, Fe, Ni, Ti, Cu and Mn.
8. 8. A method according to any one of the preceding claims, characterized in that the high entropy alloy is AlxCoCrFeNi, AlxCoCuFeNi, AlxCoCrFeTi, AlxCrCuFeNi, AlxCrFeCuCo AlxCrCoCuFeNi or AlxCoCrFeTi, AlxCoCrFeTiNi, or AlxCoCrFeMnNi, more preferably with x between 0.1 and 3.
9. 9. Method according to any one of the preceding claims, characterized in that the manufacturing process is a laser powder bed fusion process or a selective electron beam powder bed fusion process.
10. 10. A method according to any preceding claim, characterized in that the mixing of powders is carried out in a 3D dynamic mixer.