A cathode composition

A lithium-rich manganese oxide cathode with a single-phase rock salt structure addresses the cost and stability issues of existing compositions by utilizing manganese, achieving superior stability and capacity performance in lithium-ion batteries.

GB2589063BActive Publication Date: 2024-11-20DYSON TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
GB2019015244
Authority / Receiving Office
GB · GB
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-10-22
Publication Date
2024-11-20
Estimated Expiration
2039-10-22

AI Technical Summary

Technical Problem

Current lithium-ion battery cathode compositions based on nickel, cobalt, and aluminum offer higher capacities and energy densities but are costly and suffer from stability issues and voltage profile evolution during cycling, while manganese, an abundant alternative, requires a cost-effective and stable lithium-rich composition to achieve parity or better performance.

Method used

A lithium-rich manganese oxide cathode composition with a single-phase rock salt crystal structure, specifically Li1+xMn1-xO2, where x is between 0 and 0.3, is developed, which is synthesized using conventional ball-milling techniques and exhibits improved stability and capacity performance without spinel or layered structures, and can be used as a bulk or composite cathode.

Benefits of technology

The lithium-rich manganese oxide cathode composition demonstrates enhanced stability and electrochemical cycling performance compared to traditional layered structures, achieving improved charge capacity and reduced cost through the use of abundant manganese, while maintaining or exceeding energy density and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000002_0000
    Figure 00000002_0000
  • Figure 00000003_0000
    Figure 00000003_0000
  • Figure 00000003_0001
    Figure 00000003_0001
Patent Text Reader

Abstract

A cathode composition for a lithium-ion cell or battery of the general formula: Li1+Mn1−O2 The composition is in the form of a single phase having a rock salt crystal structure; such that an x-ray diffraction pattern of the composition using a CuKα radiation source has an absence of peaks below a 2Ɵ value of 35. The value of x is greater than 0, and equal to or less than 0.3. x may be equal to 0.1. The composition can be formed from two precursors, such as LiMnO2 and Li2MnO3, and mixed via a ball milling process. Additives and binders may also be added such as carbon black.
Need to check novelty before this filing date? Find Prior Art

Description

The present invention relates to a set of electroactive lithium-rich manganese cathode compositions having a rock salt structure. More specifically the present invention relates to a set of high capacity lithium-ri ch manganese oxide cathode compositions which can be used as a bulk composition or composite cathode composition in an electrochemical cell. The performance and cost of lithium ion batteries primarily relies on the composition of the positive electrode (cathode). Currently available lithium-based cathode compositions are graded mainly on their energy density, electrochemical performance and the price of raw materials required to formulate the composition. Manganese would be an ideal sole-transition metal centre for a lithium-based cathode composition, as the abundance of manganese in the Earth’s crust is far greater than cobalt and nickel. Although much higher capacities and energy densities can currently be achieved with compositions comprising nickel, cobalt and aluminium, the cost of these metals is far greater. In addition, these nickel, cobalt and aluminium-based composition still suffer with problems of the voltage profile evolving on cycling, costly (because of the inclusion of cobalt and nickel) and show significant stability issues, such as gas loss during cycling. There is a need for a simple, robust and cost-effective lithium-rich composition which delivers parity or better in terms of energy density and performance. In a first aspect, the present invention provides a cathode composition for a lithium-ion battery of the general formula: Li1+xMn1_xO2; wherein the composition is in the form of a single phase having a rock salt crystal structure such that an x-ray diffraction pattern of the composition using a Cu Ka radiation source has an absence of peaks below a 29 value of 35; and the value of x is greater than 0, and equal to or less than 0.3. Conventional ordered or layered lithium and manganese-rich compositions (Lii+xTmi-x02 where Tm is predominately Mn) have lithium ions sitting in both the alkali and transition metal sites. In addition to the above, x-ray diffraction pattern of these conventional compositions will have a peak at a 20 value of 18. However, in the present invention the x-ray diffraction pattern of the cathode composition has an absence of a peak at a 29 value of 18. In other words, the single phase crystal structure of the present invention is absent of any spinel or layered structures, and is considered purely as a single phase rock salt crystal structure. The single phase crystal structure does not exhibit either a R3(bar)m and / or a C2 / m space group. Where lithium and cobalt ions fully occupy alternating layers within the structure. It has been found that a cathode composition with an improved stability and capacity performance can be achieved by the lithium-rich manganese oxide compositions as defined above. The cathode compositions of the present invention also exhibit improved electrochemical cycling when compared to the traditional layered lithium manganese oxide structures of the prior art. In particular, the compositions are provided as a single phase rock salt crystal structure (i.e. face centred cubic lattice with the Fm3(bar)m space group). The specifically identified compounds can be manufactured reproducibly at a high rate using conventional ball-milling techniques by mixing LiMnO2 and I^MnCh precursors in different proportions. In addition, other conventional techniques can be used to manufacture a thin film of the cathode composition, such as PVD techniques including, but not limited to sputtering and sublimation / evaporation of target material. In specific examples, the value of x may be equal to or greater than 0.1. The value of x may be equal to or greater than 0.17. The value of x may be equal to or greater than 0.2. The value of x may be equal to or greater than 0.2 and equal to or less than 0.3. The value of x may be equal to or greater than 0.1 and equal to or less than 0.2. The value of x may be equal to 0.2. In a particular example, x is equal to 0.2. This particular composition is thus Li1.2Mno.8O2. This particular composition has demonstrated an improved capacity for charge, and stability over a number of cycles. The composition may be expressed as the general formula: (a)LiMnO2*(l-a)Li2MnO3; wherein two precursors are provided in proportions defined by a, and a has a value in the range greater than 0 and less than 1; and the precursors are mixed by a ball milling process to provide a bulk composition with a rock salt structure. In examples a has a value in the range greater than 0.05 and less than 0.95 In specific examples, the value of a may be equal or greater than 0.15 and equal to or less than 0.7. The value of a may be equal to or greater than 0.15 and equal to or less than 0.4. As shown in the Examples of the present invention below, the cathode composition may be selected from one of 0.7LiMn02-0.3Li2Mn03; 0.6LiMn02-0.4Li2Mn03; 0.5LiMn02-0.5Li2Mn03; 0.4LiMn02-0.6Li2Mn03;     0.3LiMn02-0.7Li2Mn03;     0.2LiMn02-0.8Li2Mn03; 0.15LiMnO2- 0.85Li2MnO3; 0.4LiMnO2- 0.6Li2MnO3. In a second aspect, the present invention provides a cathode (or more generally an electrode). The cathode can be made with the cathode composition as a thin film as part of a PVD technique, or alternatively the cathode can be made using the cathode composition as cathode active in a composite electrode. In examples, a composite cathode may be made from a cathode composition of the present invention comprising 3 fractions. The first is the cathode composition of the present invention as previously described (in a variety of mass percentages from 60-98%, however, typically 70, 75, 80, 90 and 95%). The second fraction of the composite cathode comprises electroactive additives such as carbon, for example, Super P and Carbon black, which comprises 60-90 % of the mass fraction remaining excluding the first fraction. The third fraction is typically a polymeric binder such as PVDF, PTFE, NaCMC and NaAlginate. In some case additional fractions maybe included and the overall percentages may change. The overall electrochemical performance of the composite cathode can be improved by the introduction of electroactive additives, and the structural properties of the resulting composite cathode can also be improved by adding material that improves cohesion of the cathode composition and adhesion of the material to particular substrates. In a third aspect, the present invention provides an electrochemical cell comprising a cathode with a cathode composition according to the description above, an electrolyte and an anode. The electrolyte may, for example, take the form of a liquid or solid, such as a gel or a ceramic. In order that the present invention may be more readily understood, an embodiment of the invention will now be described, by way of example, with reference to the accompanying Figures, in which: Figure 1 shows powder X-ray Diffraction patterns of various Li-Mn-0 compounds that exist, with their space groups and lattice parameters; Figure 2 shows powder X-ray Diffraction patterns of the synthesised cathode compositions Li1.2Mno.sO2 (or 0.4LiMn02’0.6Li2Mn03) compound in Example 1; Figures 3a and b shows first cycle galvanostatic load curves for the first cycle of Li1.2Mno.sO2 and Li1.1Mno.9O2 at 45°C at C / 10 respectively, and Figures 3c and d show evolution of the charge and discharge capacity as a function of cycle for Li1.2Mno.sO2 and Li1.1Mno.9O2 respectively; Figure 4 shows preparation of Li1.2Mno.sO2 with a conventional planetary ball mill at 400 rpm with ZrO2 balls (upper line) compared to the high energy ball mill with 700 rpm and WC balls (lower line); Figure 5 shows preparation of Li1.2Mno.sO2 with starting materials Li2MnO3, Li2O2 and Mn2O3 (upper line) compared to starting materials Li2MnO3 and LiMnO2 (lower line); Figure 6 shows Electrochemical data of Li1.2Mno.sO2 prepared from Li2MnO3, Li2O2 and Mn2O3 with C / 10 charge, and C / 5 discharge; and Figure 7 shows X-ray diffraction patterns of the precursors (lower line), ball milled for 40 min (second to lower line), ball milled for 5 h (second to higher line) and ball milled for lOh (higher line). The present invention will now be illustrated with reference to the following examples. Example 1 - Synthesis of the Lithium Rich Manganese Oxide Cathode Compositions Material comprising LiMnO2 and Li2MnO3 precursors were mixed in different molar proportions in accordance with Table 1 using WC jars and balls. All materials were handled at all times under inert atmosphere (in an Argon filled glovebox) and never exposed to ambient atmosphere, ie protected against moisture and oxygen at all times. A planetary ball milling (Fritsch Planetary Micro Mill PULVERISETTE 7 premium line which can deliver energy which are approximately 150 % above that which can be achieved through conventional milling) was employed and the milling was performed at a speed rate of 700 rpm for 10 minutes, following 30 minutes break. Phase purity was assessed after repeating this milling and resting cycle for at least 30 times, i.e. for a total milling time of at least 5 hours. However, it is possible that less milling times are necessary to achieve phase purity. The phase transformation is assessed by X-ray diffraction. If the phase transformation is not complete, the same program is repeated, and so on. LiMnO2 Li2MnO3 Resulting Composition Stoichiometry 0.7 0.3 0.7LiMnO2- 0.3Li2MnO3 Li1.1Mno.9O2 0.6 0.4 0.6LiMnO2- 0.4Li2MnO3 Li1.13Mno.87O2 0.5 0.5 0.5LiMn02-0.5Li2Mn03 Li1.17Mno.83O2 0.4 0.6 0.4LiMnO2- 0.6Li2MnO3 Li1.2Mno.8O2 0.3 0.7 0.3LiMnO2- 0.7Li2MnO3 Li1.23Mno.77O2 0.2 0.8 0.2LiMnO2- 0.8Li2MnO3 Li1.27Mno.73O2 0.15 0.85 0.15LiMnO2- 0.85Li2MnO3 Li1.28Mno.72O2 Alternate starting materials can be used here including but not limited to MmCh, Mn02, Li2O, Li2O2, Mn2O4, LiMn2O4. An addition route for the preparation of Li1.2Mno.sO2 was tried with Li2O, Mn2O3 and Mn02 which resulted in the same phase as shown in Figure 2. Alternatively a conventional planetary ball mill was used, the Retsch PM 100 mill. Here both mills were used to prepare Li1.2Mno.sO2 at a milling speed of 400 rpm with ZrO2 balls. Here it can be clearly understood that the lower density of the milling media and the rotation rate will result in significantly lower energy collisions. The conditions employed by both mills were successful in obtaining the disordered rock salt phase (Fig 4) with a composition of Li1.2Mno.sO2 indicating that preparation at high energies is not the only route to cathode composition production. Alternatively, mechanofusion or conventional Physical Vapour Deposition techniques can be considered to prepare these cathode compositions. Example 2 - Structural Analysis and Characterisation of the Lithium Rich Manganese Oxide Cathode Compositions The materials according to Example 1 were examined with Powder X-Ray Diffraction (PXRD) which was carried out utilising a Panalytical Aeris benchtop XRD with a Cu Ka Radiation. The range of measurement was 10-90 0 2 theta. Figure 2 shows a representative Powder X-ray Diffraction pattern of the synthesised compositions. These are characteristic of a cation disordered rock salt structure. All of the patterns appear to show the broad major peaks consistent with a face centred cubic lattice with the Fm3(bar)m space group, as shown in Figure 2. It should be noted that broad peaks are displayed due to the ball milling process which without wishing to be bound by theory results in a cathode composition with a small crystallite size. There is no evidence for the presence of the layered precursors which had a layered LiMnO2 or Li2MnO3 structures with the space group R3(bar)m or C2 / m, which would indicate that the ball-milling synthesis has converted the material of the precursors into the cathode composition of the present inventions. No presence of extra peaks due to impurities was observed. The example XRD in Figure 2 shown for Li1.2Mno.sO2 was indicative of all samples with a slight shifting of the peak positions in accordance with changes to the bulk lattice parameters as a result of the changing composition. It should also be noted that no crystalline phases for other common LipMniOq (database patterns shown in Figure 1 for comparison) can be seen in the final product. Figure 7 also shows how the reaction proceeds as the initial precursors are slowly removed on continual milling as the disordered rock salt phase becomes the dominant feature. Example 3 - Electrochemical Analysis of the Lithium Rich Manganese Oxide Cathode Compositions The cathode compositions according to Example 1 were characterised electrochemically through galvanostatic cycling performed with a BioLogic BCS series potentiostats. All the samples were assembled as powdered cathodes into Swagelok type cells with a metallic lithium counter / reference electrode and cycled between 2 and 4.8 V vs. Li+ / Li at a current rate of C / 10 as defined by a capacity of 300 mAh / g. The electrolyte employed was LP40 (a IM solution of LiPFe in 1:1 w / w ratio of EC;DEC). Figures 3a-d shows the potential curves during the charge and subsequent discharge of the first cycle for compositions 0.7LiMn02-0.3Li2Mn03 and 0.4LiMn02’0.6Li2Mn03 according to Example 1. Both samples present high discharge capacities above 200 mAh / g at C / 10. The values of the first discharge capacities for all materials which have been prepared are detailed in the Table below. The 0.4LiMn02’0.6Li2Mn03 cathode composition exhibits a sloping region at the beginning of charge, until ca. 4 V vs Li+ / Li and a high potential plateau centred at around 4.2 V vs Li+ / Li that appears to be irreversible on the first discharge. This general feature could be considered consistent for all the prepared materials with Li>l. 1 per formula unit with the length of the plateau correlating to the amount of lithium in the material: the more lithium is present the longer the plateau. The 0.7LiMn02’0.3Li2Mn03 composition exhibits a different first charge. A long sloping region is observed up to the high potential cut-off of 4.8 V vs Li+ / Li. No potential plateau is observed, less irreversibility on discharge is seen and therefore a higher first cycle coulombic efficiency. Phase purity First charge capacity (mAh / g) First discharge capacity (mAh / g) Coulombic efficiency at the first cycle 0.7LiMn02-0.3Li2Mn03 No crystalline phase detectable except rock-salt structure (Fm3(bar)m) 230 209 90.8% 0.6LiMn02-0.4Li2Mn03 No crystalline phase detectable except rock-salt structure (Fm3(bar)m) 279.5 249.6 89.3% 0.5LiMn02-0.5Li2Mn03 No crystalline phase detectable except rock-salt structure (Fm3(bar)m) 281 250 88.9% 0.4LiMn02-0.6Li2Mn03 No crystalline phase detectable except rock-salt structure (Fm3(bar)m) 315.9 245.3 77.7% 0.3LiMn02-0.7Li2Mn03 No crystalline phase detectable except rock-salt structure (Fm3(bar)m) 317.8 264 83.1% 0.2LiMn02-0.8Li2Mn03 No crystalline phase detectable except rock-salt structure (Fm3(bar)m) 346.2 239.6 69.2 0.15LiMn02-0.85Li2Mn03 No crystalline phase detectable except rock-salt structure (Fm3(bar)m) 376.9 242.9 64.4%

Claims

1. A cathode composition for a lithium-ion battery of the general formula:Lii+xMn1_xO2wherein the composition is in the form of a single phase having a rock salt crystal structure such that an x-ray diffraction pattern of the composition using a Cu Ka radiation source has an absence of peaks below a 29 value of 35; andthe value of x is greater than 0, and equal to or less than 0.3.

2. A cathode composition according to claim 1, wherein the x-ray diffraction pattern of the composition has an absence of a peak at a 29 value of 18.

3. A cathode composition according to claim 1 or claim 2, wherein the single phase crystal structure is absent of any spinel or layered structures.

4. A cathode composition according to claim 4, wherein the single phase crystal structure does not exhibit either a R3(bar)m and / or a C2 / m space group.

5. The cathode composition according to claim 1, wherein the value of x is equal to orgreater than 9.1.

6. The cathode composition according to claim 1, wherein the value of x is equal to orgreater than 9.17.

7. The cathode composition according to claim 1, wherein the value of x is equal to orgreater than 9.2.

8. The cathode composition according to claim 1, wherein the value of x is equal to orgreater than 9.2 and equal to or less than 9.3.

9. The cathode compound according to claim 1, wherein the value of x is equal to orgreater than 9.1 and equal to or less than 9.2.

10. The cathode composition according to any one of the previous claims, wherein the value of x is equal to 0.2.

11. The cathode composition according to any one of the previous claims, wherein the single phase crystal structure exhibits the Fm3(bar)m space group.

12. The cathode composition according to claim 1, wherein the composition is expressed as the general formula:(a)LiMnO2*(l -a)Li2MnO3wherein two precursors are provided in proportions defined by a, and a has a value in the range greater than 0, and less than 1; andthe precursors are mixed by a ball milling process.

13. The composition according to claim 12, wherein the value of a is equal or greater than 0.15 and equal to or less than 0.7.

14. The composition according to claim 12, wherein the value of a is equal or greater than 0.15 and equal to or less than 0.4.

15. The composition according to claim 12, wherein the composition is 0.4LiMn02*0.6Li2Mn03.

16. An electrode comprising the cathode composition according to any one of previous claims 1 to 15.

17. The electrode according to claim 16, wherein the electrode comprises electroactive additives and / or a binder.

18. The electrode according to claim 17, wherein the electroactive additive is selected from at least one of carbon or carbon black.

19. The electrode according to claim 17 or claim 18, wherein the polymeric binder is selected from at least one of PVDF, PTFE, NaCMC or NaAlginate.