Cylindrical battery, preparation method thereof and power utilization device
By optimizing the electrolyte ratio and volumetric energy density, and combining the coating design of the positive and negative electrodes, the problem of poor high-rate discharge performance of traditional cylindrical batteries has been solved, achieving high energy density and safety, making it suitable for products with high-rate discharge.
Patent Information
- Application Number
- CN202411049348.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional cylindrical batteries have poor high-rate discharge performance, making them difficult to apply to product scenarios that require high-rate charging and discharging. Furthermore, the amount of electrolyte injected is limited by the space of the metal casing, affecting the gravimetric energy density.
By controlling the mass-to-electric ratio and volumetric energy density of the electrolyte within a reasonable range, the coating composition and parameters of the positive and negative electrodes are optimized, including the ratio and particle size of the positive electrode active material, conductive agent, and binder. Combined with the all-tab structure, the space utilization and electrochemical performance of the battery are improved.
It significantly improves the high-rate discharge performance and energy density of cylindrical batteries within a limited space, enhances battery safety, cycle stability and range performance, extends battery life, and is suitable for negative electrodes with different silicon contents.
Smart Images

Figure CN118983499A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a cylindrical battery and a preparation method and an electrical device thereof. Background Art
[0002] According to the packaging form, lithium batteries can be divided into three forms: square, cylindrical and soft pack. Among them, cylindrical batteries have gradually become a hot spot in lithium battery research due to their good consistency, high production efficiency, and strong heat dissipation capacity at the system level. Cylindrical batteries are usually packaged in a cylindrical metal shell. The interior of the metal shell is used to accommodate the battery core and inject electrolyte. The battery core is formed by winding the positive electrode sheet, the negative electrode sheet and the separator between the two. The positive electrode sheet and the negative electrode sheet are both provided with pole ears for connecting to the electrical connecting sheet to further connect the positive and negative terminals of the battery, so that an electrical path is formed between the positive and negative electrodes.
[0003] Traditional cylindrical battery products have poor high-rate discharge performance and are difficult to apply to product application scenarios that require high-rate charge and discharge, such as electric drills, electric planers, electric saws, handheld electric vacuum cleaners, etc. With the emergence of full-ear battery cell technology, the internal resistance of the battery cell has been significantly reduced, making high-rate charge and discharge possible. In order to achieve high-rate discharge, a sufficient quality of electrolyte is required to ensure that the battery has good dynamic performance. However, the amount of electrolyte injected is limited by the residual space of the metal shell (that is, the internal space of the metal shell minus the portion occupied by the solid material of the battery dry coil core) and the safety design of the battery cell. At the same time, too much electrolyte injection will increase the weight of the battery cell and affect the weight energy density. Therefore, the design of the electrolyte injection amount is a major difficulty in the research and development of cylindrical batteries. Summary of the invention
[0004] To solve the above problems, the first aspect of the present invention provides a cylindrical battery, including a shell, the interior of the shell accommodates a battery core and is injected with an electrolyte, the battery core is wound by a positive electrode sheet, a negative electrode sheet and a separator therebetween, at least one surface of the positive electrode sheet has a positive electrode coating, and at least one surface of the negative electrode sheet has a negative electrode coating; wherein the mass-to-electricity ratio of the electrolyte is m, the volume energy density of the cylindrical battery is n, and m and n satisfy 1.0≤m / n≤3.1.
[0005] In some embodiments, the mass-to-electricity ratio m is 1000-1800 mg / Ah.
[0006] In some embodiments, the volumetric energy density n is 440-1000 Wh / L.
[0007] In some embodiments, the cylindrical battery has a diameter of 14-50 mm, a height of 34-150 mm, and a ratio of height to diameter greater than or equal to 1.7.
[0008] In some embodiments, the space utilization coefficient σ of the cylindrical battery is 85-92%. In some embodiments, the battery AC internal resistance of the cylindrical battery is r, and r, m, and n satisfy 1≤m*r / n≤33.
[0009] In some embodiments, the AC internal resistance of the battery is 1-20 mΩ, preferably 2-10 mΩ.
[0010] In some embodiments, the positive electrode coating comprises 1.4-2.5% of positive electrode conductor, 0.8-1.2% of positive electrode binder, and the balance is positive electrode active material; the positive electrode active material is selected from a mixture of one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium nickel oxide, and lithium manganese oxide, and the average particle size Dv50 of the positive electrode active material is 5-15 μm. According to weight percentage, the negative electrode coating comprises 0.8-1.1% of negative electrode conductor, 0.7-1.2% of negative electrode slurry thickener, 1.5-2.3% of negative electrode binder, 0-45% of silicon material, and the balance is carbon material; the average particle size Dv50 of the mixed silicon material and carbon material is 8-20 μm; the silicon material is silicon oxygen material and / or silicon carbon material.
[0011] In some embodiments, the single-sided surface density of the positive electrode sheet is 0.0065-0.03 g / cm 2 ; The single-sided surface density of the negative electrode sheet is 0.005-0.012g / cm 2 .
[0012] In some embodiments, the compaction density of the positive electrode sheet is p1, and the compaction density of the negative electrode sheet is p2, satisfying the following equation (1) and / or equation (2):
[0013] Formula (1), 3.1≤m*p1 / n≤11.47,
[0014] Formula (2), 1.3≤m*p2 / n≤5.27.
[0015] In some embodiments, the compaction density p1 of the positive electrode sheet is 3.1-3.7 g / cm 3 ; The compaction density p2 of the negative electrode is 1.3-1.7g / cm 3 .
[0016] In some embodiments, the single-side surface capacity of the positive electrode is 1.4-3.75 mAh / cm 2 The single-side surface capacity of the negative electrode is 1.5-4.8 mAh / cm 2 The ratio of the single-sided surface capacity of the negative electrode sheet to the single-sided surface capacity of the positive electrode sheet is 1.01-1.18.
[0017] In some embodiments, the surface of the positive electrode sheet includes a positive electrode coated portion and a positive electrode uncoated portion, and the surface of the negative electrode sheet includes a negative electrode coated portion and a negative electrode uncoated portion; at least a portion of the positive electrode uncoated portion is used as a positive electrode lug, or the positive electrode uncoated portion is welded to the positive electrode lug; at least a portion of the negative electrode uncoated portion is used as a negative electrode lug, or the negative electrode uncoated portion is welded to the negative electrode lug.
[0018] A second aspect of the present invention provides a method for preparing the above cylindrical battery, comprising the following steps:
[0019] a. Preparing a positive electrode sheet: mixing a positive electrode slurry, coating it on at least one side of an aluminum foil, and drying it to obtain a positive electrode sheet;
[0020] b. Preparing a negative electrode sheet: mixing a negative electrode slurry, coating it on at least one side of a copper foil, and drying it to obtain a negative electrode sheet;
[0021] c. Preparation of battery roll core: rolling the positive electrode sheet and the negative electrode sheet separately, slitting and die-cutting them, and then winding them together with the separator to obtain a battery roll core;
[0022] d. Assemble cylindrical batteries: Weld the tabs of the battery core to the electrical connector, install them into the shell, inject electrolyte, seal and form them to obtain cylindrical batteries.
[0023] A third aspect of the present invention provides an electrical device, comprising the above-mentioned cylindrical battery, wherein the cylindrical battery is used to supply power to the electrical device.
[0024] The cylindrical battery provided by the present invention can fully improve the high-rate discharge performance and energy density of the cylindrical battery within the limited space of the cylindrical shell by regulating multiple parameters in the battery. In addition, the cylindrical battery provided by the present invention is suitable for negative electrodes with different silicon contents, which expands the application range of silicon-containing negative electrodes. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the description of the present application will be briefly introduced below.
[0026] Figure 1 It is a schematic diagram of the structure of the cylindrical battery in this application;
[0027] Figure 2 It is a schematic diagram of the structure of a positive electrode sheet in this application;
[0028] Figure 3 It is a schematic diagram of the structure of a negative electrode sheet in this application;
[0029] Figure 4 It is a schematic diagram of the structure of another positive electrode sheet in this application;
[0030] Figure 5It is a schematic diagram of the structure of another negative electrode sheet in this application;
[0031] Figure 6 It is a comparison chart of the change in capacity retention rate of Example 1 of the present application and Comparative Example 1 during 500 cycles.
[0032] Reference numerals: 1 - positive terminal, 2 - shell, 3 - negative terminal, 4 - positive electrode coating portion, 5 - positive electrode uncoated portion, 6 - negative electrode coating portion, 7 - negative electrode uncoated portion, 8 - positive electrode tab, 9 - negative electrode tab. DETAILED DESCRIPTION
[0033] Examples of the present embodiment are described in detail below. The examples are only used to explain the present embodiment and are not to be construed as limiting the present embodiment.
[0034] One aspect of the present application provides a cylindrical battery (see Figure 1 ), the top is the positive terminal 1, and the bottom is the negative terminal 3. The cylindrical battery includes a shell 2; the interior of the shell 2 accommodates the battery core and is injected with electrolyte; wherein the battery core is wound by a positive electrode sheet, a negative electrode sheet and a separator therebetween, at least one surface of the positive electrode sheet has a positive electrode coating, and at least one surface of the negative electrode sheet has a negative electrode coating.
[0035] In some embodiments, the mass-to-electricity ratio of the electrolyte is m (unit: mg / Ah), the volume energy density of the cylindrical battery is n (unit: Wh / L), and m and n satisfy: 1.0≤m / n≤3.1; preferably, 1.1≤m / n≤2.8.
[0036] In the present application, the mass-to-electricity ratio m of the electrolyte refers to the ratio of the mass of the electrolyte remaining in the battery after the battery is filled and formed to the battery capacity Q of the battery, wherein the mass determination of the electrolyte includes the following steps:
[0037] S11: weighing the battery to be tested to obtain a first mass w1;
[0038] S12: dismantling the battery, pouring out the electrolyte, adding dimethyl carbonate (DMC) into the shell for extraction 2-5 times, and pouring out the extract;
[0039] S13: Soaking the battery core inside the shell with dimethyl carbonate and washing it 2-5 times;
[0040] S14: putting the battery core and the shell into an oven to fully remove the dimethyl carbonate, and weighing to obtain w2;
[0041] S15: Calculate the mass of the electrolyte as w1-w2 (unit: mg).
[0042] It should be noted that the above test measures the mass of electrolyte retained by the battery after formation, rather than the mass of electrolyte injected during battery assembly.
[0043] In this application, the test method of battery capacity Q (unit: Ah) includes the following steps: place a fresh battery in a dry environment at 25±2℃ for at least 3 hours, at this temperature, charge it to 4.2V at 0.2C constant current, and then charge it to 0.02C at 4.2V constant voltage; after standing for 30 minutes, discharge it to 2.5V at 0.2C constant current, and the capacity obtained is the battery capacity Q (unit: Ah). The mass-to-electricity ratio of the electrolyte m=(w1-w2) / Q is further calculated based on the mass of the electrolyte and the battery capacity.
[0044] In the present application, the volume energy density n of a cylindrical battery refers to the energy that can be released per unit volume of the battery, which can be tested by the following method: place a fresh battery in a dry environment at 25±2°C for at least 3 hours, use a battery tester to charge the battery at 0.2C to a voltage of 4.2V, charge it to 0.02C at a constant voltage, let it stand for 30 minutes, and then discharge it to 2.5V at 0.2C, record the battery energy E (unit: Wh), and further calculate the battery volume energy density n=E / V based on the volume of the cylindrical battery.
[0045] In order to ensure the safety of the battery in abnormal conditions such as overheating, short circuit or overcharging, a current interrupt device (CID) is usually provided in the battery. When the pressure exceeds the preset threshold, the CID will automatically cut off the positive lead to form a short circuit to ensure the safety of the battery. Under normal working conditions, in order not to trigger the preset pressure threshold of the CID, a certain residual space must be retained inside the battery casing, so the amount of electrolyte added cannot be too high. On the one hand, the battery will produce gas during the formation process, and on the other hand, the battery will also produce a certain amount of gas during storage or use. If the residual space is too small, the internal gas pressure of the battery will be too high, causing the CID to be activated prematurely, causing the battery to lose its normal use function.
[0046] When the m / n ratio is too large, if it is due to the high mass-to-electricity ratio m of the electrolyte, more electrolyte may cause side reactions during storage or use and produce a large amount of gas, which cannot be absorbed by the battery itself and cannot be discharged from the battery shell, thereby causing the battery shell to deform or the CID to be actuated prematurely; if it is due to the low volume energy density n of the battery, the most cost-effective battery cannot be obtained, and the low battery energy carried in a limited space cannot meet the long-term use requirements of electrical devices.
[0047] When the m / n ratio is too small, if it is due to the low mass-to-electricity ratio m of the electrolyte, the electrolyte remaining inside the battery shell after formation will not be able to meet the requirements of ion conductivity, thereby directly reducing the battery's charge and discharge capabilities and even causing lithium deposition in the battery; if it is due to the battery's volume energy density n being too high, the battery's optimal cycle stability performance cannot be achieved and the battery life cannot be guaranteed.
[0048] Therefore, controlling the ratio of the electrolyte mass to the battery volume energy density within a reasonable range not only improves the safety of the battery, but also improves the battery's endurance performance and cycle stability, extends the battery life, and provides sufficient protection for the battery to discharge at a high rate.
[0049] In some embodiments, the mass-to-electricity ratio m is 1000-1800 mg / Ah; preferably, the mass-to-electricity ratio m is 1300-1700 mg / Ah. The mass-to-electricity ratio within the set range helps to balance the charge and discharge performance and cycle life of the battery. A high mass-to-electricity ratio will reduce the battery cycle life performance due to gas production in the electrolyte, and a low mass-to-electricity ratio will reduce the lithium ion conduction rate inside the battery and thus affect the charge and discharge performance.
[0050] In some embodiments, the volume energy density n is 440-1000Wh / L; preferably, the volume energy density n is 540-950Wh / L. The volume energy density within the set range helps to achieve a better battery cycle life in a limited battery internal space, increase battery capacity, and achieve long battery life.
[0051] In some embodiments, the battery AC internal resistance of the cylindrical battery is r (unit: mΩ), and r, m and n satisfy: 1≤m*r / n≤33; preferably, 5≤m*r / n≤10. The battery AC internal resistance in this application refers to the internal resistance of the battery at 50% SOC at 25°C, which can be obtained by testing the battery using an AC internal resistance tester (such as AT526). By limiting the battery AC internal resistance, the battery energy density and cycle life are improved while reducing invalid energy consumption, and the battery temperature rise is avoided, causing the battery management system (BMS) to alarm, thereby limiting the use of the battery.
[0052] In some embodiments, the battery AC internal resistance r is 1-20 mΩ; preferably, the battery AC internal resistance r is 2-10 mΩ. It is understandable that the smaller the battery AC internal resistance r is, the less heat is generated during high-rate discharge, and the less likely it is to trigger the temperature protection setting, which is conducive to exerting the battery capacity.
[0053] Based on the range limitation of the mutual correlation of multiple parameters, the R & D process can be significantly shortened, eliminating the need for repeated experiments on a single parameter, reducing R & D investment, and the obtained battery products fully meet the usage requirements. High energy storage, combined with excellent cycle stability and safety, provides sufficient guarantee for high-rate discharge.
[0054] In some embodiments, by weight percentage, the positive electrode coating coated on the positive electrode sheet contains 1.4 - 2.5% of positive electrode conductive agent and 0.8 - 1.2% of positive electrode binder, and the balance is positive electrode active material.
[0055] In some embodiments, the positive electrode active material is selected from one or more mixtures of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminate, lithium nickel manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium nickel oxide, and lithium manganese oxide. In this application, in order to improve the energy density of the battery, in some preferred embodiments, the positive electrode active material in the positive electrode coating is Li a Ni b Co c Mn d M e O2, where 0.9 < a < 1.1, 0.8 < b < 0.94, 0.1 ≤ c < 0.4, 0.05 ≤ d < 0.4, 0 ≤ e ≤ 0.1, and M is at least one of Al, Mg, Zr, Ti, W, Nb, Mo, and B. Exemplarily, the positive electrode active material in this application is lithium nickel cobalt manganese oxide, with the chemical formula LiNi 0.8 Co 0.1 Mn 0.1 O2, also known as the 811 positive electrode.
[0056] Preferably, the average particle size D V 50 of lithium nickel cobalt manganese oxide is 5 - 15 μm. The average particle size D V 50 in this application is the particle size corresponding to the cumulative volume distribution value of 50%. Dv50 can be measured by the laser diffraction method for particle size distribution (specifically referring to GB / T19077 - 2016) using a laser diffraction particle size distribution measuring instrument (such as Malvern 3000). By controlling the particle size of the positive electrode active material, it is beneficial to achieve a balance between process difficulty and battery performance. If the average particle size is too small, the viscosity of the positive electrode slurry will be large, the fluidity will become poor, increasing the difficulty of the coating process, and uneven coating will further affect the battery performance; if the average particle size is too large, the specific surface area available for the electrochemical reaction on the positive electrode active material will be too small, resulting in a significant reduction in battery performance.
[0057] The positive electrode conductive agent of the positive electrode coating in the present application can be any one or more mixtures known to those skilled in the art, and optional ones include carbon nanotubes, conductive carbon black, graphene, acetylene black, etc. The positive electrode binder of the positive electrode coating in the present application can be any one or more mixtures known to those skilled in the art, and optional ones include polyvinylidene fluoride (PVDF), polyacrylate, polyacrylic acid (PAA), etc.
[0058] Preferably, in terms of weight percentage, the positive electrode coating coated on the positive electrode sheet contains 0.4-0.9% carbon nanotubes, 1-1.6% conductive carbon black, 0.8-1.2% polyvinylidene fluoride, and the remainder is lithium nickel cobalt manganese oxide.
[0059] The preparation method of the positive electrode sheet comprises the following steps: weighing the positive electrode active material, the positive electrode conductive agent, and the positive electrode binder as the solid matter of the positive electrode slurry, dispersing the solid matter of the positive electrode slurry in N-methyl-2-pyrrolidone (NMP solvent), mixing in a homogenizer, coating on at least one side of the aluminum foil, and drying to obtain the positive electrode sheet. The solid content of the positive electrode slurry can be 50-70%, and the positive electrode slurry after drying is the positive electrode coating.
[0060] In some embodiments, the single-sided surface density of the positive electrode sheet is 0.0065-0.03 g / cm 2 Preferably, the single-sided surface density of the positive electrode is 0.009-0.02 g / cm 2 By adjusting the single-sided surface density of the positive electrode coating on the positive electrode sheet, it is beneficial to improve the battery's cycle performance, safety performance and battery life. If the surface density is too large, the electrode coating is thicker, the lithium ion diffusion path becomes longer, the battery kinetic performance deteriorates, the transmission of lithium ions between the positive and negative electrodes is blocked, the battery charging and discharging performance decreases, and the battery may overheat due to insufficient infiltration, shortening the service life; if the surface density is too small, the energy density is reduced and the battery life is shortened.
[0061] Taking the test of the double-sided coated pole piece as an example, the test method of the single-sided surface density in this application includes the following steps:
[0062] S21: Clean the sample electrode with dimethyl carbonate 2-5 times and put it into an oven for drying to fully remove the dimethyl carbonate;
[0063] S22: Take a disc with an area of S from the double-sided coating area on the sample electrode and weigh it to obtain the sum of the mass of the foil and the coating m1;
[0064] S23: scrape off all the powder on the surface of the disc, wipe the surface of the disc with NMP to fully remove the powder, and fully dry the disc, and weigh the disc again to obtain the foil mass m2;
[0065] S24: Calculate the single-surface density as (m1-m2) / (2S) (unit: g / cm 2 ).
[0066] To ensure the accuracy of the data, the above operation can be repeated three times to calculate the average surface density. It can be understood that if the tested pole piece is coated on one side, the calculation formula for the single-side surface density is (m1-m2) / S.
[0067] In some embodiments, the compaction density of the positive electrode sheet is p1, and the compaction density of the negative electrode sheet is p2, satisfying the following equation (1) and / or equation (2):
[0068] Formula (1), 3.1≤m*p1 / n≤11.47,
[0069] Formula (2), 1.3≤m*p2 / n≤5.27.
[0070] The compaction density of the pole piece has a great influence on the mass-to-electricity ratio of the electrolyte in the battery and the volume energy density of the battery. The greater the compaction density of the pole piece, the higher the volume energy density of the battery. However, if the compaction density of the pole piece is too large, it is difficult for the electrolyte to penetrate the pole piece, the electrochemical reaction of the pole piece is insufficient, and even battery abnormalities may occur. Therefore, the mass-to-electricity ratio of the electrolyte, the volume energy density of the battery, and the compaction density of the pole piece need to be comprehensively controlled within a reasonable range to improve the comprehensive electrochemical performance of the battery.
[0071] In some embodiments, the compaction density of the positive electrode sheet is 3.1-3.7 g / cm 3 By adjusting the compaction density, the electrolyte wetting effect and coating adhesion are balanced. If the compaction density is too large, the electrode porosity will be reduced, the electrolyte wetting effect will be poor, and the diffusion resistance of lithium ions in the pores of the positive electrode coating will also increase, which will eventually lead to a decrease in battery kinetic performance. If the compaction density is too small, the electrical contact between the positive electrode active material particles and between the particles and the current collector foil will be poor, and the electrode powder will easily fall off during processing.
[0072] The test method for compacted density in this application includes the following steps:
[0073] S31: Clean the sample electrode with dimethyl carbonate 2-5 times and put it into an oven for drying to fully remove the dimethyl carbonate;
[0074] S32: Take a disc with an area of S from the double-sided coating area on the sample pole piece, weigh it to get the sum of the mass of the foil and the coating m1, and use a spiral micrometer to measure the sum of the thickness of the foil and the coating d1;
[0075] S33: scrape off all the powder on the surface of the disc, wipe the surface of the disc with NMP to fully remove the powder, and fully dry the disc, weigh the disc again to obtain the mass m2 of the foil, and use the spiral micrometer to measure the thickness of the foil again to obtain d2;
[0076] S34: Calculate the compacted density as (m1-m2) / [S*(d1-d2)] (unit: g / cm 3 ).
[0077] To ensure the accuracy of the data, the above operation can be repeated three times to calculate the average value of the compacted density.
[0078] In some embodiments, the porosity of the positive electrode sheet is 10-50% to ensure contact between the electrolyte and the positive electrode active material particles, while improving the electrical contact between the particles of the positive electrode active material and between the positive electrode active material and the foil. The porosity in this application can be measured using a fully automatic mercury intrusion pore size tester.
[0079] In some embodiments, the single-side surface capacity of the positive electrode is 1.4-3.75 mAh / cm 2 , to ensure that the positive electrode sheet achieves a balance in terms of dynamic performance and cell energy density. . The single-sided surface capacity in this application can be obtained by testing and calculating with an Arbin battery tester. The test conditions are: at 25°C, 0.2C constant current charging to 4.2V, 4.2V constant voltage to 0.02C; then 0.2C constant current discharge to 2.5V to obtain the battery capacity; then the battery capacity is divided by the total area of the positive electrode sheet coating to obtain the single-sided surface capacity of the electrode sheet.
[0080] In some embodiments, the negative electrode coating coated on the negative electrode sheet contains, by weight percentage, 0.8-1.1% of a negative electrode conductor, 0.7-1.2% of a negative electrode slurry thickener, 1.5-2.3% of a negative electrode binder, 0-25% of a silicon material, and the remainder is a carbon material.
[0081] In some embodiments, the carbon material is artificial graphite and / or natural graphite. The silicon material in the present application is a silicon-carbon material and / or a silicon-oxygen material, wherein the silicon-carbon material may be a carbon-coated silicon material, and the coated silicon material may be crystalline silicon, amorphous silicon or a silicon-carbon composite material; the silicon-oxygen material is silicon oxide, which may be represented by the chemical formula SiO xIndicates that 0<x≤2, silicon oxide can also be further treated with carbon coating. Under the same negative electrode sheet surface capacity design, the introduction of silicon material can reduce the surface density and thickness of the negative electrode sheet and improve the high-rate charge and discharge performance of the battery. However, the change in the amount of silicon material will cause the various performances of the battery to change, which increases the difficulty of research and development. The inventors found in the study that by regulating the overall correlation between the mass-to-electricity ratio of the electrolyte, the volume energy density of the battery, the internal resistance of the battery and other parameters, the research and development efficiency can be significantly improved.
[0082] In some embodiments, the average particle size D of the mixed carbon material and silicon material is V 50 is 8-20 μm. Carbon material and silicon material together constitute the negative electrode active material in the negative electrode coating of the present application. By adjusting the average particle size of the negative electrode active material, the fluidity of the negative electrode slurry can be improved to ensure the smooth coating process, while providing as large a specific surface area as possible for the power supply chemical reaction, thereby improving the battery performance.
[0083] The negative electrode conductive agent and negative electrode binder of the negative electrode coating in the present application can be any one or more mixtures known to those skilled in the art, and can be selected as needed. The negative electrode thickener of the negative electrode coating in the present application can be any one or more mixtures known to those skilled in the art, such as a cellulose thickener.
[0084] Preferably, in terms of weight percentage, the negative electrode coating coated on the negative electrode sheet comprises 0.8-1.1% acetylene black, 0.7-1.2% carboxymethyl cellulose (CMC), 1.5-2.3% polyacrylate, 0-19.2% silicon material, and the remainder is artificial graphite.
[0085] The preparation method of the negative electrode sheet comprises the following steps: weighing carbon material, silicon material, negative electrode conductive agent, negative electrode slurry thickener, and negative electrode binder as solid substances of negative electrode slurry, dispersing the solid substances of negative electrode slurry in deionized water, mixing in a homogenizer, coating on at least one side of the copper foil, and drying to obtain a negative electrode sheet. The solid content of the negative electrode slurry can be 30-50%, and the negative electrode slurry after drying is the negative electrode coating.
[0086] In some embodiments, the single-sided surface density of the negative electrode sheet is 0.005-0.012 g / cm 2 . By adjusting the single-sided surface density of the negative electrode sheet, the battery can have the optimal NP ratio (Negative / Positive Ratio, the ratio of the negative electrode capacity per unit area of the battery to the positive electrode capacity), thereby improving the high-rate discharge performance of the battery under the premise of safety. When the single-sided surface density of the negative electrode sheet is too large, the electrode sheet coating will be too thick and the battery dynamics performance will deteriorate; when the single-sided surface density of the negative electrode sheet is too small, the battery energy density will decrease, which is not conducive to long battery life.
[0087] In some embodiments, the compaction density of the negative electrode sheet is 1.3-1.7 g / cm 3 . By limiting the compaction density of the negative electrode sheet, it helps to improve the dynamic performance and fast charging performance of the battery. When the compaction density of the negative electrode sheet is too large, the porosity of the negative electrode coating is not enough to fully infiltrate the electrolyte. At the same time, the diffusion resistance of lithium ions in the pores of the negative electrode coating will also increase, and the battery dynamic performance will deteriorate; when the compaction density of the negative electrode sheet is too small, the electronic conductivity between the particles of the negative electrode active material deteriorates, and the battery fast charging performance decreases.
[0088] In some embodiments, the porosity of the negative electrode sheet is 12-45% to ensure good contact between the electrolyte, the negative electrode active particles, and the foil, so that the electrochemical reaction can proceed smoothly and the battery cycle performance is stable.
[0089] In some embodiments, the single-side surface capacity of the negative electrode sheet is 1.5-4.8 mAh / cm 2 , to ensure that the negative electrode has better dynamic performance and the battery cell has higher energy density.
[0090] The test methods for single-surface density, compaction density, porosity, single-surface capacity and other parameters of the negative electrode sheet are the same as those for the corresponding parameters of the positive electrode sheet. By adjusting the various parameters of the positive and negative electrode sheets, it is helpful to improve the infiltration effect of the electrolyte, reduce the internal resistance of the battery, and achieve the best high-rate discharge performance and cycle performance.
[0091] In some embodiments, the surface of the positive electrode sheet includes a positive electrode coating portion 4 and a positive electrode uncoated portion 5, wherein the positive electrode uncoated portion 5 is located at the upper end of the positive electrode sheet in the width direction, and at least part of the positive electrode uncoated portion 5 is used as a positive electrode ear (see Figure 2 ); The surface of the negative electrode sheet includes a negative electrode coating portion 6 and a negative electrode uncoated portion 7, the negative electrode uncoated portion 7 is located at the lower end of the negative electrode sheet in the width direction, and at least part of itself is used as a negative electrode ear (see Figure 3 ). Preferably, the entirety of the positive electrode uncoated portion 5 is used as a positive electrode lug, and the entirety of the negative electrode uncoated portion 7 is used as a negative electrode lug. The full lug structure is used to improve the high-rate discharge performance of the cylindrical lithium-ion battery. Compared with the solution of using only part of the uncoated portion as a lug, the full lug has a higher current capacity.
[0092] In other embodiments, the positive electrode uncoated portion 5 is located between two positive electrode coated portions 4 in the length direction of the positive electrode sheet and is used for welding with the positive electrode tab 8 (see Figure 4 ); two negative electrode uncoated portions 7 are located at both ends of a negative electrode coated portion 6 in the length direction of the negative electrode sheet, and are used for welding with two negative electrode ears 9 (see Figure 5 ).
[0093] In some embodiments, the area of the positive electrode uncoated portion 5 accounts for 4-15% of the total area of the positive electrode sheet; the area of the negative electrode uncoated portion 7 accounts for 4-15% of the total area of the negative electrode sheet. In this application, when the electrode sheet has a coating on a single surface, the above-mentioned electrode sheet area refers to the single-side area; when the electrode sheet has a coating on both sides, the above-mentioned electrode sheet area refers to the double-side area. By limiting the area ratio of the uncoated portion, a balance between the battery volume energy density and the current capacity can be achieved.
[0094] The method for preparing a battery roll core using the above-mentioned positive electrode sheet and negative electrode sheet comprises the following steps: the positive electrode sheet and the negative electrode sheet are cut and die-cut according to the size requirements, and then wound together with the separator to obtain a cylindrical battery roll core. The base material of the separator in the present application can be polyethylene PE or polypropylene PP, and a ceramic coating is coated on one side or both sides of the base material.
[0095] In some embodiments, the diameter of the cylindrical battery is 14-50mm, the height is 34-150mm, and the ratio of the height to the diameter is greater than or equal to 1.7. In some preferred embodiments, the diameter of the cylindrical battery is 14-36mm, the height is 34-90mm, and the ratio of the height to the diameter is greater than or equal to 1.9. In other preferred embodiments, the diameter of the cylindrical battery is 36-50mm, the height is 80-150mm, and the ratio of the height to the diameter is greater than or equal to 1.7. By limiting the diameter and height of the cylindrical battery, the space utilization coefficient of the battery is improved and the volume energy density is increased.
[0096] In some embodiments, the space utilization factor σ of the cylindrical battery is 85-92%.
[0097] The test method of the space utilization coefficient in this application includes the following steps:
[0098] S41: Measure the volume V1 inside the battery shell. For the regular shell volume, it is calculated by measuring the diameter and height of the battery; for the irregular shell volume, it is obtained by testing with a gas displacement method true density instrument Gas pycometer;
[0099] S42: Measure the volume V2 of the winding assembly (including the positive electrode sheet, the negative electrode sheet, the separator, and the current collecting plate) inside the battery by the water displacement method according to the Archimedean principle;
[0100] S43: Calculate the space utilization coefficient of the battery as V2 / V1.
[0101] In some embodiments, the electrolyte comprises a lithium salt and a solvent. The lithium salt in the present application may be lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), etc.; preferably lithium hexafluorophosphate, which has good ionic conductivity and electrochemical stability, can form an electrolyte interface in an organic solvent that protects the aluminum current collector and the graphite negative electrode, while ensuring the conductivity of the battery, improving the safety of the battery. The solvent in the present application may be a mixture of one or more of ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl formate, ethyl acetate, and propyl propionate, preferably ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate are mixed in a volume ratio of 1:1:1.
[0102] In some embodiments, the concentration of lithium salt in the electrolyte is 0.8-1.7 mol / L; preferably, the concentration of lithium salt in the electrolyte is 1-1.6 mol / L. By controlling the lithium salt concentration within a preferred range, a balance between the battery's conductivity and energy density can be achieved. When the lithium salt concentration is too low, it is not conducive to high-rate discharge; when the lithium salt concentration is too high, the viscosity of the electrolyte increases, the battery's energy density is low, the battery's electrochemical stability decreases, and the battery life and safety are negatively affected.
[0103] The preparation method of the electrolyte comprises the following steps: dissolving lithium salt in a solvent to prepare an electrolyte.
[0104] The battery assembly method comprises the following steps: placing the battery core into a shell, injecting electrolyte, sealing, and forming the battery to obtain the battery.
[0105] According to the charge and discharge test, the continuous high current discharge rate of the cylindrical battery in this application is between 4C and 25C. Taking the battery capacity of 4Ah as an example, the cylindrical battery in this application can be used normally at a discharge current of 16A (4C) -100A (25C), achieving high rate discharge.
[0106] The cylindrical battery provided in this application needs to pass the 500-cycle cycle retention test, and the test method is as follows:
[0107] S51: Take a fresh battery cell, charge it to 4.2V at 2C constant current at 25℃, and charge it to 0.2C at 4.2V constant voltage; let it stand for 30 minutes, and discharge it to 2.5V at 7.5C. The capacity obtained is the initial capacity and is recorded as a;
[0108] S52: Then, a 2C charge / 7.5C discharge cycle test is performed, and the rest time after charging and discharging is 30 minutes. The cell capacity after 500 cycles is recorded as b;
[0109] S53: Calculate the 500-cycle capacity retention rate as b / a×100%.
[0110] The cylindrical battery provided in this application also needs hot box testing, and the testing method is as follows:
[0111] S61: Take a battery that has been cycled for 500 cycles and place it in a 25°C constant temperature box for more than 4 hours;
[0112] S62: Discharge the battery at a constant current of 0.1C to 2.5V cutoff, and let it stand for 5 minutes;
[0113] S63: The battery is charged at a constant current of 0.2C to a cutoff of 4.2V, and at a constant voltage of 0.05C to a cutoff, and allowed to stand for 5 minutes;
[0114] S64: Place the battery in a temperature box, set the heating rate to 5K / min, heat to 130°C, and keep it for 1 hour, then stop heating and cool it to below 30°C by self-heating;
[0115] S65: If the battery does not catch fire or emit smoke, it is considered passed, otherwise it is failed. At least 6 batteries are tested and the pass rate is recorded.
[0116] Another aspect of the present invention provides an electrical device, comprising the above-mentioned cylindrical battery, wherein the cylindrical battery is used to supply power to the electrical device.
[0117] The present invention will be further explained with reference to the following examples.
[0118] Example 1
[0119] Example 1 provides a cylindrical battery, which is prepared by the following method:
[0120] a. Preparation of positive electrode: According to the weight percentage, weigh 97% lithium nickel cobalt manganese oxide (chemical formula: LiNi 0.8 Co 0.1 Mn 0.1 O2, also known as 811 positive electrode), 0.4% carbon nanotubes, 1.6% conductive carbon black, and 1% polyvinylidene fluoride as the solid matter of the positive electrode slurry, the solid matter of the positive electrode slurry is dispersed in N-methyl-2-pyrrolidone, the solid content is 60%, after mixing in a homogenizer, coated on both sides of the aluminum foil, and dried to obtain a positive electrode sheet; wherein the average particle size D V 50 is 8μm, and the single-sided surface density of the positive electrode is 0.01313g / cm 2 , compaction density p1 is 3.5g / cm 3 , porosity is 21%;
[0121] b. Preparation of negative electrode sheet: According to the weight percentage, 92.64% artificial graphite, 3.36% silicon oxide material (SiO), 1% acetylene black, 1% carboxymethyl cellulose, and 2% polyacrylic acid are weighed as the solid matter of the negative electrode slurry, and the solid matter of the negative electrode slurry is dispersed in deionized water with a solid content of 40%. After mixing in a homogenizer, it is coated on both sides of the copper foil and dried to obtain a negative electrode sheet; wherein the average particle size D of the mixture of artificial graphite and silicon oxide material is V 50 is 12μm, and the single-sided surface density of the negative electrode sheet is 0.00682g / cm 2 , compaction density p2 is 1.55g / cm 3 , porosity is 32%;
[0122] c. Preparation of battery roll core: After rolling the positive electrode sheet and the negative electrode sheet separately, slitting and die-cutting according to the size requirements, and winding them together with the separator to obtain a cylindrical battery roll core;
[0123] d. Prepare an electrolyte: mix ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 1:1:1 to obtain an organic solvent, and then dissolve lithium salt LiPF6 in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L;
[0124] e. Assemble the battery: After welding the tabs of the battery core to the electrical connector, place them in the housing, inject 7000 mg of electrolyte, seal and form, and obtain a cylindrical battery with a diameter of 21 mm and a height of 70 mm. The measured space utilization coefficient σ of the battery is 87%, the battery capacity is 4050 mAh, and the single-side surface capacity of the positive electrode is 3.03 mAh / cm 2 .
[0125] Example 2
[0126] Example 2 provides a cylindrical battery, which differs from Example 1 in that the mass of the injected electrolyte is 5000 mg.
[0127] Example 3
[0128] Example 3 provides a cylindrical battery, which differs from Example 1 in that: in step a, the single-sided surface density of the positive electrode sheet is 0.01315 g / cm 2 , porosity is 20%; in step b, the weight percentage of artificial graphite is 96%, no silicon material, the average particle size of artificial graphite is D V 50 is 12μm, and the compaction density p2 of the negative electrode sheet is 1.6g / cm 3 The single-sided surface density of the negative electrode sheet is 0.00826g / cm 2The mass of the injected electrolyte is 6300 mg. The measured space utilization coefficient of the battery is 87.6%, the battery capacity is 4100 mAh, and the single-side surface capacity of the positive electrode is 3.1 mAh / cm 2 .
[0129] Example 4
[0130] Example 4 provides a cylindrical battery, which differs from Example 3 in that the mass of the injected electrolyte is 4150 mg.
[0131] Example 5
[0132] Example 5 provides a cylindrical battery, which differs from Example 1 in that: in step a, the single-sided surface density of the positive electrode sheet is 0.01718 g / cm 2 , compaction density p1 is 3.52g / cm 3 , the porosity is 20%; in step b, the weight percentage of artificial graphite is 86.4%, the mass percentage of silicon oxide material is 9.6%, and the compaction density p2 of the negative electrode sheet is 1.5g / cm 3 The single-sided surface density of the negative electrode sheet is 0.00703g / cm 2 The mass of the injected electrolyte is 6600 mg. The measured space utilization coefficient of the battery is 88.1%, the battery capacity is 5060 mAh, and the single-side surface capacity of the positive electrode is 3.3 mAh / cm 2 .
[0133] Example 6
[0134] Example 6 provides a cylindrical battery, which differs from Example 5 in that the mass of the injected electrolyte is 8600 mg.
[0135] Example 7
[0136] Example 7 provides a cylindrical battery, which differs from Example 1 in that: in step a, the single-sided surface density of the positive electrode sheet is 0.02771 g / cm 2 , compaction density p1 is 3.6g / cm 3 , the porosity is 20%; in step b, the weight percentage of artificial graphite is 76.8%, the mass percentage of silicon oxide material is 19.2%, and the single surface density of the negative electrode sheet is 0.011g / cm 2 The compaction density p2 of the negative electrode is 1.6 g / cm 3 ; The mass of the injected electrolyte is 6300 mg; the measured space utilization coefficient σ of the battery is 88.7%, the battery capacity is 5800 mAh, and the single-side surface capacity of the positive electrode is 3.6 mAh / cm 2 .
[0137] Example 8
[0138] Example 8 provides a cylindrical battery, which differs from Example 7 in that the mass of the injected electrolyte is 7500 mg.
[0139] Comparative Example 1
[0140] Comparative Example 1 provides a cylindrical battery, which differs from Example 1 in that the mass of the injected electrolyte is 9200 mg.
[0141] Comparative Example 2
[0142] Comparative Example 2 provides a cylindrical battery, which differs from Example 1 in that: in step a, the single-sided surface density of the positive electrode sheet is 0.01315 g / cm 2 In step b, the weight percentage of artificial graphite is 96%, no silicon material, and the average particle size of artificial graphite is D V 50 is 12μm, and the single-sided surface density of the negative electrode sheet is 0.00826g / cm 2 The compaction density p2 of the negative electrode is 1.6 g / cm 3 ; The mass of the injected electrolyte is 9300 mg; the measured space utilization coefficient σ of the battery is 87.6%, and the battery capacity is 4100 mAh.
[0143] Comparative Example 3
[0144] Comparative Example 3 provides a cylindrical battery, which differs from Example 1 in that: in step a, the single-sided surface density of the positive electrode sheet is 0.01718 g / cm 2 The compaction density p1 of the positive electrode is 3.52g / cm 3 In step b, the weight percentage of artificial graphite is 86.4%, the mass percentage of silicon oxide material is 9.6%, and the single surface density of the negative electrode sheet is 0.00703g / cm 2 The compaction density p2 of the negative electrode is 1.5g / cm 3 ; The mass of the injected electrolyte is 4000 mg; the measured space utilization coefficient σ of the battery is 88.1%, and the battery capacity is 5060 mAh.
[0145] Comparative Example 4
[0146] Comparative Example 4 provides a cylindrical battery, which differs from Example 1 in that: in step a, the single-sided surface density of the positive electrode sheet is 0.02771 g / cm 2 The compaction density p1 of the positive electrode is 3.6g / cm 3 In step b, the weight percentage of artificial graphite is 76.8%, the mass percentage of silicon oxide material is 19.2%, and the single surface density of the negative electrode sheet is 0.011g / cm 2 The compaction density p2 of the negative electrode is 1.6 g / cm3 ; The mass of the injected electrolyte is 4500 mg; the measured space utilization coefficient σ of the battery is 88.7%, and the battery capacity is 5800 mAh.
[0147] Comparative Example 5
[0148] Comparative Example 5 provides a cylindrical battery, which differs from Example 1 in that: in step a, the compaction density p1 of the positive electrode sheet is 3 g / cm 3 ;The battery capacity is 3900mAh.
[0149] Comparative Example 6
[0150] Comparative Example 6 provides a cylindrical battery, which differs from Example 1 in that: in step a, the compaction density p1 of the positive electrode sheet is 3.8 g / cm 3 ;The battery capacity is 4200mAh.
[0151] Comparative Example 7
[0152] Comparative Example 7 provides a cylindrical battery, which differs from Example 1 in that: in step b, the compaction density p2 of the negative electrode sheet is 1.2 g / cm 3 ;The battery capacity is 3700mAh.
[0153] Comparative Example 8
[0154] Comparative Example 8 provides a cylindrical battery, which differs from Example 1 in that: in step b, the compaction density p2 of the negative electrode sheet is 1.8 g / cm 3 ;The battery capacity is 4300mAh.
[0155] The parameters of the above embodiments are shown in Table 1 and Table 2.
[0156] Table 1
[0157]
[0158]
[0159] Table 2
[0160]
[0161]
[0162] Figure 6 A comparison chart of the change in capacity retention rate during 500 cycles of Example 1 of the present application and Comparative Example 1 is shown. As the number of cycles increases, the capacity retention rate of Comparative Example 1 rapidly drops to below 60%, while the rate of decrease in the capacity retention rate of Example 1 is significantly slower, and ultimately retains 80%.
[0163] It can be seen from Examples 1-8 and Comparative Examples 1-4 in Tables 1 and 2 that when the mass-to-electricity ratio and volume energy density of lithium-ion cylindrical batteries are within a reasonable range, the battery can obtain better cycle performance and can meet actual use requirements. If the volume energy density of the battery is increased blindly, the safety performance of the battery may deteriorate. For small-capacity lithium-ion cylindrical batteries, better hot box test results can be obtained while ensuring that the internal resistance of the battery is low, and the test pass rate is above 66.7%. For large-capacity lithium-ion cylindrical batteries, the internal resistance of the battery increases significantly, and only general hot box test results can be obtained, and the test pass rate is above 50%.
[0164] It can be seen from Example 1 and Comparative Examples 5-8 in Table 1 and Table 2 that the volume energy density of the battery can be improved by designing different compaction densities for the positive electrode sheet and different compaction densities for the negative electrode sheet, but the battery cycle performance is poor and cannot meet the actual use requirements. At the same time, the hot box test results in Comparative Examples 5-8 are poor, proving that the battery safety performance needs to be improved.
[0165] Through Table 1 and Figure 6 It can be known that the cylindrical battery provided by this application can fully improve the high-rate discharge performance and energy density of the cylindrical lithium-ion battery within the limited space of the cylindrical shell, meet the high-rate discharge performance of the battery (4-25C), and its capacity retention rate reaches more than 70% after 500 cycles under 7.5C discharge conditions. Under appropriate parameter limitations, this application can be applied to the research and development of negative electrodes with different silicon contents to expand the application range of silicon-containing negative electrodes.
[0166] In the description of this specification, reference to the terms "some embodiments", "an example", or similar descriptions means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment are included in at least one embodiment or example. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0167] Although examples of the present embodiment have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present embodiment, and the scope of the present embodiment is defined by the claims and their equivalents.
Claims
1. A cylindrical battery, comprising a shell, wherein a battery core is contained in the shell and an electrolyte is injected therein, wherein the battery core is wound by a positive electrode sheet, a negative electrode sheet and a separator therebetween, wherein at least one surface of the positive electrode sheet has a positive electrode coating, and at least one surface of the negative electrode sheet has a negative electrode coating, wherein: The mass-to-electricity ratio of the electrolyte is m, the volume energy density of the cylindrical battery is n, and m and n satisfy 1.0≤m / n≤3.
1.
2. The cylindrical battery according to claim 1, characterized in that: The mass-to-electricity ratio m is 1000-1800 mg / Ah.
3. The cylindrical battery according to claim 1, characterized in that: The volume energy density n is 440-1000Wh / L.
4. The cylindrical battery according to claim 1, characterized in that: The cylindrical battery has a diameter of 14-50 mm and a height of 34-150 mm, and a ratio of the height to the diameter is greater than or equal to 1.
7.
5. The cylindrical battery according to claim 4, characterized in that: The space utilization coefficient σ of the cylindrical battery is 85-92%.
6. The cylindrical battery according to claim 1, characterized in that: The battery AC internal resistance of the cylindrical battery is r, and r, m, and n satisfy 1≤m*r / n≤33.
7. The cylindrical battery according to claim 6, characterized in that: The battery AC internal resistance is 1-20 mΩ.
8. The cylindrical battery according to any one of claims 1 to 7, characterized in that: According to weight percentage, the positive electrode coating contains 1.4-2.5% of positive electrode conductor, 0.8-1.2% of positive electrode binder, and the balance is positive electrode active material; the positive electrode active material is selected from a mixture of one or more of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide, and the average particle size Dv50 of the positive electrode active material is 5-15 μm; According to weight percentage, the negative electrode coating contains 0.8-1.1% of negative electrode conductor, 0.7-1.2% of negative electrode slurry thickener, 1.5-2.3% of negative electrode binder, 0-45% of silicon material, and the balance is carbon material; the average particle size Dv50 of the mixed silicon material and the carbon material is 8-20μm; the silicon material is silicon-oxygen material and / or silicon-carbon material.
9. The cylindrical battery according to claim 1, characterized in that: The single surface density of the positive electrode sheet is 0.0065-0.03 g / cm 2 The single surface density of the negative electrode sheet is 0.005-0.012g / cm 2 .
10. The cylindrical battery according to claim 1, characterized in that: The compaction density of the positive electrode sheet is p1, and the compaction density of the negative electrode sheet is p2, satisfying the following relationship (1) and / or (2): Formula (1), 3.1≤m*p1 / n≤11.47, Formula (2), 1.3≤m*p2 / n≤5.
27.
11. The cylindrical battery according to claim 10, characterized in that: The compaction density p1 of the positive electrode sheet is 3.1-3.7 g / cm 3 The compaction density p2 of the negative electrode sheet is 1.3-1.7 g / cm 3 .
12. The cylindrical battery according to claim 1, characterized in that: The single-side surface capacity of the positive electrode sheet is 1.4-3.75 mAh / cm 2 The single-side surface capacity of the negative electrode sheet is 1.5-4.8 mAh / cm 2 The ratio of the single-side surface capacity of the negative electrode sheet to the single-side surface capacity of the positive electrode sheet is 1.01-1.
18.
13. The cylindrical battery according to claim 1, characterized in that: The surface of the positive electrode sheet includes a positive electrode coating portion and a positive electrode uncoated portion, and the surface of the negative electrode sheet includes a negative electrode coating portion and a negative electrode uncoated portion; At least part of the positive electrode uncoated portion is used as a positive electrode lug; or, the positive electrode uncoated portion is welded to the positive electrode lug; At least part of the negative electrode uncoated portion is used as a negative electrode tab; or, the negative electrode uncoated portion is welded to the negative electrode tab.
14. A method for preparing a cylindrical battery according to any one of claims 1 to 13, characterized in that: The following steps are involved: a. Preparing the positive electrode sheet: mixing the positive electrode slurry, coating it on at least one side of the aluminum foil, and drying it to obtain the positive electrode sheet; b. Preparing the negative electrode sheet: mixing the negative electrode slurry, coating it on at least one side of the copper foil, and drying it to obtain the negative electrode sheet; c. Preparing the battery roll core: rolling the positive electrode sheet and the negative electrode sheet separately, slitting and die-cutting them, and then winding them together with the separator to obtain the battery roll core; d. Assembling the cylindrical battery: welding the tabs of the battery core to the electrical connection sheet, placing the battery core into the housing, injecting the electrolyte, sealing, and forming the battery to obtain the cylindrical battery.
15. An electrical device, characterized in that: It comprises a cylindrical battery according to any one of claims 1 to 13, wherein the cylindrical battery is used to supply power to the electrical device.
Citation Information
Cited By
Lithium ion cylindrical battery with hot gas safety and power utilization device
CN120319905A
A heat-safe lithium-ion cylindrical battery and an electrical device
CN120319905B
Battery cell, battery and electric equipment
CN121862809A
Full-tab cylindrical lithium ion battery and preparation method thereof
CN122511966A
Method for predicting rapid charging performance of cylindrical lithium secondary battery, cylindrical lithium secondary battery and method for manufacturing the same