Method for manufacturing a multi-layer assembly having a surface recess - Patents.com

JP2023545113A5Inactive Publication Date: 2024-10-17AZDEL INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023521781
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-09
Filing Date
2021-10-08
Publication Date
2024-10-17
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing multilayer assemblies face challenges in achieving strong bonding between layers, particularly due to delamination issues, which can be exacerbated by variations in material properties and layer configurations.

Method used

The introduction of recesses in the surface of the core and skin layers, formed by applying stimuli such as molds or fluid jets with protrusions, forces the porous fiber-reinforced thermoplastic layer into these recesses, enhancing the bond strength by creating gaps and aligning the layers more effectively.

Benefits of technology

This method significantly strengthens the bond between the core and skin layers, reducing the likelihood of delamination and improving the structural integrity of the multilayer assembly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Specific configurations of the multilayer assembly are described. In certain embodiments, the multilayer assembly can include a core layer, a skin layer, and one or more recesses on the surface of the multilayer assembly. In other configurations, the multilayer assembly can include a core layer, a skin layer, one or more recesses on the surface of the multilayer assembly, and one or more additional layers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Priority Claim This application is related to U.S. Patent Application No. 63 / 090,066, filed on October 9, 2020, and claims the priority and benefit thereof. The entire disclosure of which is incorporated herein by reference for all purposes.

[0002] Technical Field The specific configuration described herein relates to a multilayer assembly having one or more recesses on a surface. More specifically, the specific configuration relates to a multilayer assembly including a skin layer and a core layer, and the recesses in the skin layer and the core layer can strengthen the bond between the skin layer and the core layer.

Background Art

[0003] Background A multilayer assembly can include two or more layers. The materials of different layers can be arranged in different ways.

Summary of the Invention

Means for Solving the Problems

[0004] Summary In one aspect, the method includes the step of disposing a first porous fiber reinforced thermoplastic layer on a first surface of a core layer to form a multilayer assembly, wherein the first porous fiber reinforced thermoplastic layer comprises a web of a continuous cellular structure formed by a plurality of reinforcing materials held with a thermoplastic material. In some configurations, the method includes the step of applying a first stimulus to the first surface of the multilayer assembly to provide a plurality of first recesses within the core layer and across the first surface of the multilayer assembly, the applied first stimulus pushing the first porous fiber reinforced thermoplastic layer into the plurality of first recesses within the core layer to strengthen the bond between the first porous fiber reinforced thermoplastic layer and the core layer.

[0005] In certain embodiments, the method includes the step of applying a first stimulus to a first surface of a multilayer assembly by placing the multilayer assembly in a mold having a plurality of surface protrusions and molding the multilayer assembly using the mold. In other embodiments, the method includes the step of applying a first stimulus to a first surface of a multilayer assembly by pressing a plate having a plurality of surface protrusions onto the first surface of the multilayer assembly. In some examples, the method includes the step of applying a first stimulus to a first surface of a multilayer assembly by using a plurality of fluid jets positioned adjacent to the first surface of the multilayer assembly.

[0006] In certain embodiments, the provided first recesses have different geometric shapes. In other embodiments, the method includes the step of applying a second stimulus to the second surface of a multilayer assembly to provide a plurality of second recesses within the core layer and across the second surface of the multilayer assembly, the applied second stimulus pressing the core layer into the first porous fiber-reinforced thermoplastic layer to strengthen the bond between the first porous fiber-reinforced thermoplastic layer and the core layer. In some examples, the method includes the steps of applying a first stimulus to the first surface of a multilayer assembly by placing the multilayer assembly in a mold having a plurality of surface protrusions and molding the multilayer assembly using the mold, and applying a second stimulus to the second surface of the placed multilayer assembly. In other embodiments, the method includes the step of applying a second stimulus to the second surface of a multilayer assembly by pressing a plate having a plurality of surface protrusions onto the second surface of the multilayer assembly. In some examples, the method includes the step of applying a second stimulus to the second surface of a multilayer assembly using a plurality of fluid jets positioned adjacent to the second surface of the multilayer assembly. In other examples, the provided plurality of second recesses have different geometric shapes.

[0007] In some configurations, the multiple first recesses have different depths. In other embodiments, the method includes the step of placing a first skin layer on a first porous fiber-reinforced thermoplastic layer that has been placed, before applying the first stimulus.

[0008] In some examples, the first porous fiber-reinforced thermoplastic layer comprises an adhesive film. In another example, the method includes the step of placing a first skin layer on a multilayer assembly after applying a first stimulus.

[0009] In some examples, the core layer comprises a porous core layer, and the first porous fiber-reinforced thermoplastic layer comprises reinforcing fibers and a polyolefin thermoplastic material. In other embodiments, the core layer comprises a honeycomb core layer.

[0010] In some embodiments, the reinforcing fibers include one or more of the following: glass fibers, aramid fibers, graphite fibers, carbon fibers, inorganic mineral fibers, metal fibers, metallated synthetic fibers, and metallated inorganic fibers, fibers, and combinations thereof.

[0011] In other embodiments, the thermoplastic material includes polyethylene, polypropylene, polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, polyvinyl chloride, polyarylene ether, polycarbonate, polyester carbonate, thermoplastic polyester, polyimide, polyetherimide, polyamide, acrylonitrile-butylacrylate-styrene polymer, amorphous nylon, polyarylene ether ketone, polyphenylene sulfide, polyaryl sulfone, polyether sulfone, liquid crystalline polymer, poly(1,4-phenylene) compound, high-temperature polycarbonate, high-temperature nylon, silicone, or one or more blends of these materials.

[0012] In certain examples, the honeycomb core layer is a paper honeycomb core layer, the reinforcing fibers include glass fibers, and the thermoplastic material includes polyolefin.

[0013] In other embodiments, the method includes the steps of: arranging a second porous fiber-reinforced thermoplastic layer on a second surface of a core layer to form a multilayer assembly, wherein the second porous fiber-reinforced thermoplastic layer comprises a web of open-cell structure formed by a plurality of reinforcing materials held together with a thermoplastic material; and applying a second stimulus to the second surface of the multilayer assembly to provide a plurality of second recesses within the core layer and across the second surface of the multilayer assembly, wherein the applied second stimulus pushes the second porous fiber-reinforced thermoplastic layer into the plurality of second recesses within the core layer, thereby strengthening the bond between the second porous fiber-reinforced thermoplastic layer and the core layer.

[0014] In certain embodiments, the method includes the step of placing a multilayer assembly in a mold having a plurality of surface protrusions, and applying a second stimulus to a second surface of the multilayer assembly by molding the multilayer assembly using the mold.

[0015] In some embodiments, the method includes the step of applying a second stimulus to a second surface of a multilayer assembly by pressing a plate having a plurality of surface protrusions onto the second surface of the multilayer assembly.

[0016] In other embodiments, the method includes the step of applying a second stimulus to the second surface of a multilayer assembly using a plurality of fluid jets positioned adjacent to the second surface of the multilayer assembly.

[0017] In certain examples, the multiple first recesses are offset vertically from the multiple second recesses. In other examples, the multiple first recesses have a different depth than the multiple second recesses.

[0018] In certain embodiments, the method includes the steps of placing a first skin layer on a first porous fiber-reinforced thermoplastic layer before applying a first stimulus, and placing a second skin layer on the first porous fiber-reinforced thermoplastic layer before applying a second stimulus.

[0019] In a particular example, the method simultaneously includes the steps of applying a first stimulus to a placed skin layer and applying a second stimulus to a placed skin layer by placing a multilayer assembly in a mold having a plurality of surface protrusions and molding the multilayer assembly using the mold.

[0020] In another example, the method includes the steps of applying a first stimulus to a first skin layer on which a multilayer assembly is placed by pressing a first plate having a plurality of surface protrusions into the first skin layer on which the assembly is placed, and applying a second stimulus to a second skin layer on which the assembly is placed by pressing a second plate having a plurality of surface protrusions into the second skin layer on which the assembly is placed.

[0021] In some examples, the method includes the steps of applying a first stimulus to a first skin layer using a plurality of air jets positioned adjacent to the first skin layer, and applying a second stimulus to a second skin layer using a plurality of air jets positioned adjacent to the second skin layer.

[0022] In certain embodiments, the method includes the step of placing a first skin layer on a multilayer assembly after applying a first stimulus and a second stimulus.

[0023] In another embodiment, the multilayer assembly comprises a core layer having a plurality of recesses extending across a first surface of the core layer, and a first porous fiber-reinforced thermoplastic layer disposed on the first surface of the core layer, comprising a web of open-cell structure formed by a plurality of reinforcing materials held together with the thermoplastic material, and bonded to the surfaces of the plurality of recesses extending across the first surface of the core layer.

[0024] In an additional aspect, the multilayer assembly comprises a core layer having a plurality of recesses extending across a first surface of the core layer. In certain embodiments, the assembly comprises a first porous fiber-reinforced thermoplastic layer disposed on the first surface of the core layer, the first porous fiber-reinforced thermoplastic layer comprising a web of a continuous cellular structure formed by a plurality of reinforcing materials held with a thermoplastic material, the first porous fiber-reinforced thermoplastic layer being bonded to the surfaces of the plurality of recesses across the first surface of the core layer. In other embodiments, the assembly comprises a second porous fiber-reinforced thermoplastic layer disposed on a second surface of the core layer, the second porous fiber-reinforced thermoplastic layer comprising a web of a continuous cellular structure formed by a plurality of reinforcing materials held with a thermoplastic material.

[0025] In another aspect, the multilayer assembly comprises a core layer having a plurality of first recesses extending across a first surface of the core layer and a plurality of second recesses extending across a second surface of the core layer. In certain embodiments, the assembly comprises a first porous fiber-reinforced thermoplastic layer disposed on the first surface of the core layer, the first porous fiber-reinforced thermoplastic layer comprising a web of a continuous cellular structure formed by a plurality of reinforcing materials held with a thermoplastic material, the first porous fiber-reinforced thermoplastic layer being bonded to the surfaces of the plurality of first recesses across the first surface of the core layer. In other embodiments, the assembly comprises a second porous fiber-reinforced thermoplastic layer disposed on the second surface of the core layer, the second porous fiber-reinforced thermoplastic layer comprising a web of a continuous cellular structure formed by a plurality of reinforcing materials held with a thermoplastic material, the second porous fiber-reinforced thermoplastic layer being bonded to the surfaces of the plurality of second recesses across the second surface of the core layer.

[0026] In an additional aspect, a bulkhead wall configured to separate a passenger compartment of a vehicle from a cargo compartment of the vehicle, the bulkhead wall comprising a core layer and a first porous fiber-reinforced thermoplastic layer disposed on a first surface of the core layer, the first porous fiber-reinforced thermoplastic layer being bonded to the surfaces of a plurality of first recesses across the first surface of the core layer.

[0027] In another aspect, a vehicle load floor is described that is disposed at the rear of a vehicle and configured to support at least 50 pounds. In certain examples, the vehicle load floor includes a core layer and a first porous fiber reinforced thermoplastic layer disposed on a first surface of the core layer, and the first porous fiber reinforced thermoplastic layer is bonded to the surfaces of a plurality of first recesses across the first surface of the core layer.

[0028] In a further aspect, a vehicle is described that includes an engine compartment and a passenger compartment. In some examples, the passenger compartment includes a load floor at the rear of the vehicle configured to support at least 50 pounds. In some examples, the load floor includes a core layer and a first porous fiber reinforced thermoplastic layer disposed on a first surface of the core layer, and the first porous fiber reinforced thermoplastic layer is bonded to the surfaces of a plurality of first recesses across the first surface of the core layer.

[0029] A further aspect, examples, and figures are described. Brief Description of Some of the Drawings Specific features, elements, attributes, configurations, and embodiments of the multilayer assembly are described.

Brief Description of the Drawings

[0030] [Figure 1A] It is a view of a core layer including one or more recesses on its surface. [Figure 1B] It is a view of a core layer including one or more recesses on its surface. [Figure 1C] It is a view of a core layer including one or more recesses on its surface. [Figure 1D] It is a view of a core layer including one or more recesses on its surface. [Figure 1E] It is a view of a core layer including one or more recesses on its surface. [Figure 1F] It is a view of a core layer including one or more recesses on its surface. [Figure 1G] It is a view of a core layer including one or more recesses on its surface. [Figure 1H] It is a view of a core layer including one or more recesses on its surface. [Figure 1I] This is a diagram of a core layer having one or more recesses on its surface. [Figure 2A] This is a diagram of a core layer with multiple recesses on its surface. [Figure 2B] This is a diagram of a core layer with multiple recesses on its surface. [Figure 2C] This is a diagram of a core layer with multiple recesses on its surface. [Figure 2D] This is a diagram of a core layer with multiple recesses on its surface. [Figure 3A] This is a diagram of a core layer containing multiple recesses on two surfaces. [Figure 3B] This is a diagram of a core layer containing multiple recesses on two surfaces. [Figure 3C] This is a diagram of a core layer containing multiple recesses on two surfaces. [Figure 3D] This is a diagram of a core layer containing multiple recesses on two surfaces. [Figure 4A] This is a diagram of a multilayer assembly that includes a core layer and a skin layer, and has one or more recesses on at least one surface. [Figure 4B] This is a diagram of a multilayer assembly that includes a core layer and a skin layer, and has one or more recesses on at least one surface. [Figure 4C] This is a diagram of a multilayer assembly that includes a core layer and a skin layer, and has one or more recesses on at least one surface. [Figure 4D] This is a diagram of a multilayer assembly that includes a core layer and a skin layer, and has one or more recesses on at least one surface. [Figure 4E] This is a diagram of a multilayer assembly that includes a core layer and a skin layer, and has one or more recesses on at least one surface. [Figure 4F] This is a diagram of a multilayer assembly that includes a core layer and a skin layer, and has one or more recesses on at least one surface. [Figure 4G] This is a diagram of a multilayer assembly that includes a core layer and a skin layer, and has one or more recesses on at least one surface. [Figure 4H]This is a diagram of a multilayer assembly that includes a core layer and a skin layer, and has one or more recesses on at least one surface. [Figure 4I] This is a diagram of a multilayer assembly that includes a core layer and a skin layer, and has one or more recesses on at least one surface. [Figure 5A] This is a diagram of a multilayer assembly with multiple recesses on its surface. [Figure 5B] This is a diagram of a multilayer assembly with multiple recesses on its surface. [Figure 6A] This is a diagram of a multilayer assembly comprising a core layer and two skin layers, with one or more recesses on one or more surfaces. [Figure 6B] This is a diagram of a multilayer assembly comprising a core layer and two skin layers, with one or more recesses on one or more surfaces. [Figure 7A] This figure shows a multilayer assembly including a core layer, a skin layer, an additional layer on the skin layer, and a recess on at least one surface. [Figure 7B] This figure shows a multilayer assembly including a core layer, a skin layer, an additional layer on the skin layer, and a recess on at least one surface. [Figure 8A] This figure shows a multilayer assembly that includes a core layer, two skin layers, an additional layer on one of the skin layers, and a recess on at least one surface. [Figure 8B] This figure shows a multilayer assembly that includes a core layer, two skin layers, an additional layer on one of the skin layers, and a recess on at least one surface. [Figure 9] This figure shows an intervening layer between the core layer and the skin layer according to a specific embodiment. [Figure 10] This figure shows spikes that can be used to create recesses, with some examples. [Figure 11] This figure shows a plate with adjustable spikes according to a specific embodiment. [Figure 12] This is a photograph of a plate having multiple protrusions according to several embodiments. [Figure 13A]This is a diagram of a load-bearing floor according to a specific embodiment. [Figure 13B] Another diagram of a load-bearing floor, using a specific example. [Figure 14] This is a diagram of a truck with bulkhead walls, illustrating several examples. [Modes for carrying out the invention]

[0031] Given the merits of this disclosure, it will be recognized by those skilled in the art that the dimensions of the various layers in the drawings are not shown to scale. Unless made apparent from the specific description relating to a particular layer or other component, the thickness or dimensions of a particular layer are not intended or implied. The exact dimensions will vary depending on the final configuration of the article and / or its intended use.

[0032] Detailed explanation Specific features of a multilayer assembly having one or more surface recesses across its surfaces are described below. In some examples, a multilayer assembly may include a core layer and one or more additional layers placed on the surface of the core layer. Surface recesses may exist on one or more surfaces of the core layer and any additional layers placed on the core layer. For example, surface recesses can be formed by pressing an additional layer into the core layer such that the recessed area or recess contains the additional layer. Pressing an additional layer into the core layer can increase the bonding and / or peel strength of the additional layer to the core layer, as will be described in more detail below. This strengthening of the bonding can reduce the likelihood of the additional layer peeling or detaching from the core layer. Surface recesses may exist on two or more surfaces of the multilayer assembly as needed. Different surface recesses do not need to have the same shape, width, or depth. Further different surfaces of the multilayer assembly may have different numbers of recesses, recesses of different shapes or geometric shapes, and otherwise do not have to contain the same number or type of recesses. In certain configurations, recesses can spread across the surface of a multilayer assembly, while in other examples, recesses can be more localized or present in specific areas of the multilayer assembly, for example, more recesses may be present at the edges of the multilayer assembly to reduce delamination at the edges.

[0033] In some configurations, a core layer having one or more surface recesses is shown in Figure 1A. Core layer 110 has a recess 115 on a first surface 112 of core layer 110. The exact shape, width, and depth of the recess 115 may vary, and exemplary shapes (when viewed in cross-section) include triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. Although the recess 115 is shown as being located on the first surface 112, it may instead be located on surface 114, or the recess may be located on both surface 112 and surface 114. Furthermore, the recess 115 may be located in many different places along surface 112. As will be described in more detail below, a skin layer or other layer may be present on surface 112 (and / or surface 114), and each recess may have a portion of the skin layer or additional layer pressed into the recess 115.

[0034] In a particular embodiment, Figure 1B shows a core layer 120 having a first recess 125 on a first surface 122 and a second recess 126 on the first surface 122. The recesses 125 and 126 do not have to be the same, and the exact shape, width, and depth of each recess 125 and 126 may be independently different, with exemplary shapes (when viewed in cross-section) including triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. In some cases, one of the recesses may instead be located on a second surface, as shown in Figure 1C, with the second recess 127 located on a second surface 124 of the core layer 121. If the two recesses are located on different surfaces of the core layer 121, the shape, width, and depth of the recesses may be the same or different. As will be described in more detail below, a skin layer or other layer may be present on the surface 122 (and / or surface 124), and each recess may have a portion of the skin layer or additional layer pressed into one or both of the recesses 125 and 126.

[0035] In other configurations, the core layer may contain three or more recesses. Referring to Figure 1D, a core layer 130 is shown with recesses 135, 136, and 137 on a first surface 132. The recesses 135, 136, and 137 do not have to be the same, and the exact shape, width, and depth of each recess 135, 136, and 137 may be independently different. Exemplary shapes (when viewed in cross-section) include triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. In some cases, one of the recesses may instead be located on a second surface, as shown in Figure 1E, and a third recess 138 may be located on the second surface 134 of the core layer 131. If necessary, multiple recesses may be present on the surface 134 of the core layer 131. When three recesses are present on different surfaces of the core layers 130 and 131, the shape, width, and depth of the recesses may be the same or different. As will be described in more detail below, a skin layer or other layer may be present on surface 132 (and / or surface 134), and each recess may have a portion of the skin layer or additional layer pressed into recesses 135, 136, and 137. However, if necessary, the skin layer may be pressed into fewer recesses than all of the recesses 135, 136, and 137.

[0036] In some embodiments, a core layer may include four or more recesses. Referring to Figure 1F, a core layer 140 is shown having recesses 145, 146, 147, and 148 on a first surface 142. The recesses 145, 146, 147, and 148 do not have to be the same, and the exact shape, width, and depth of each recess 145, 146, 147, and 148 may be independently different. Exemplary shapes (when viewed in cross-section) include triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. In some cases, one of the recesses may instead be located on a second surface, as shown in Figure 1G, and a fourth recess 149 may be located on the second surface 144 of the core layer 141. If necessary, multiple recesses may be located on the surface 144 of the core layer 141. When four recesses are located on different surfaces of the core layers 140 and 141, the shape, width, and depth of the recesses may be the same or different. As will be described in more detail below, a skin layer or other layer may be present on surface 142 (and / or surface 144), and each recess may have a portion of the skin layer or additional layer pressed into recesses 145, 146, 147, and 148. However, if necessary, the skin layer may be pressed less than all of the recesses 145, 146, 147, and 148.

[0037] In some embodiments, the core layer may include five or more recesses. Referring to Figure 1H, a core layer 150 is shown having recesses 155, 156, 157, 158, and 159 on a first surface 152. The recesses 155, 156, 157, 158, and 159 do not have to be the same, and the exact shape, width, and depth of each recess 155, 156, 157, 158, and 159 may be independently different. Exemplary shapes (in cross-sectional view) include triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. In some cases, one of the recesses may instead be located on a second surface, as shown in Figure 1I, and a fifth recess 161 may be located on the second surface 154 of the core layer 151. If necessary, two or more recesses may be located on the surface 154 of the core layer 150. When the five recesses are located on different surfaces of the core layer 150, the shape, width, and depth of the recesses may be the same or different. As will be described in more detail below, a skin layer or other layer may be present on surface 152 (and / or surface 154), and each recess may have a portion of the skin layer or additional layer pressed into recesses 155, 156, 157, 158, 159, and 160. However, if necessary, the skin layer may be pressed less than all of the recesses 155, 156, 157, 158, and 159.

[0038] The core layers shown in Figures 1A to 1I may each comprise a honeycomb core layer such as a paper honeycomb core layer, a polyurethane layer, a foamed foam, or an extruded foam; a honeycomb structure made from one or more polymer materials including but not limited to polypropylene, polyethylene, polystyrene, polyamide, copolyamide, polyethylene terephthalate, polyetherimide, polyphenylene oxide, and other polymers; or a honeycomb structure made from one or more metals and metal alloys including but not limited to aluminum, iron, steel, and other metals. In some embodiments, the core layer may be a honeycomb layer having a material other than cellulose. For example, the honeycomb layer may be porous and may contain a considerable amount of open space within the core layer. The core layers shown in Figures 1A to 1I may have a basis weight of about 200 grams / square meter (gsm) to about 4000 gsm. The overall thickness of the core layers shown in Figures 1A to 1I may vary, for example, from about 0.5 cm to about 7.5 cm. The depth of the recesses shown in the core layers in Figures 1A to 1I may vary depending on the overall thickness of the core layer, for example, from about 0.125 inches (about 3 mm) to about 1 inch (about 2.5 cm), or from about 5 mm to about 1.25 mm. As described herein, different recesses may have different depths and / or geometric shapes.

[0039] In certain configurations, multiple recesses may exist across the surface of the core layer, as shown in Figures 2A to 2C. Referring to Figure 2A, a core layer 210 is shown with multiple recesses on a first surface 212. The recesses may have the same or different shapes, widths, or depths as needed. The distribution of recesses does not need to be uniform, and if necessary, more recesses may be located in one area of ​​the core layer than in other areas of the core layer. Referring to Figure 2B, a core layer 220 is shown with increased recesses located at the edges 223, 225 of the core layer 220. Figure 2C shows a recess distribution where the recesses are located toward one side or edge 233 of the core layer 230. Figure 2D shows a recess distribution where more recesses are located toward the central area of ​​the core layer 240. As will be described in more detail below, one or more skin layers or additional layers may exist on one or more surfaces of the core layer shown in Figures 2A to 2D.

[0040] In certain embodiments, the core layers shown in Figures 2A to 2D may each comprise a honeycomb core layer such as a paper honeycomb core layer, a polyurethane layer, a foamed foam, or an extruded foam; a honeycomb structure made from one or more polymer materials including but not limited to polypropylene, polyethylene, polystyrene, polyamide, copolyamide, polyethylene terephthalate, polyetherimide, polyphenylene oxide, and other polymers; or a honeycomb structure made from one or more metals and metal alloys including but not limited to aluminum, iron, steel, and other metals. In some embodiments, the core layer may be a honeycomb layer having a material other than cellulose. For example, the honeycomb layer may be porous and may contain a considerable amount of open space within the core layer. The core layers shown in Figures 2A to 2D may have a basis weight of about 200 grams / square meter (gsm) to about 4000 gsm. The overall thickness of the core layers shown in Figures 1A to 1I may vary from about 0.5 cm to about 7.5 cm. The depth of the recesses shown in Figures 2A to 2D of the core layer may vary from approximately 0.125 inches (approximately 3 mm) to approximately 1 inch (approximately 2.5 cm), for example, from approximately 5 mm to approximately 1.25 mm, depending on the overall thickness of the core layer. As described herein, different recesses may have different depths and / or geometric shapes.

[0041] In some embodiments, two or more surfaces of the core layer may have a plurality of recesses. Referring to Figure 3A, a core layer 310 is shown having a plurality of recesses on a first surface 312 and a second surface 314. The recesses on any one surface may, as required, have the same or different shapes, widths, or depths. Furthermore, all recesses on the first surface 312 may have a first shape (cross-sectional view), and all recesses on the second surface 314 may have a second shape (cross-sectional view). The first shape may be the same as or different from the second shape. The distribution of recesses on the first surface 312 and the second surface 314 does not need to be uniform, and if required, more recesses may be located in one area of ​​the core layer than in other areas of the core layer. Also, the recess distribution does not have to be the same on the first surface 312 and the second surface 314. Referring to Figure 3B, a core layer 320 is shown with an increased number of recesses located on the edges 323, 325 of the first surface 322 of the core layer 320. Figure 3C shows a recess distribution in which the recesses are located toward one side or edge 333 of the first surface 332 of core layer 330. Figure 3D shows a recess distribution in which more recesses are located toward the central region of core layer 340. The recesses on the second surfaces of core layers 310, 320, 330, and 340 are shown as uniform for illustrative purposes, but instead, the recess distribution may be non-uniform or asymmetrical, as described in relation to the recesses on the first surfaces of core layers 310, 320, 330, and 340. As will be described in more detail below, one or more skin layers or additional layers may be present on one or more surfaces of the core layers shown in Figures 3A to 3D.

[0042] In certain embodiments, the core layers shown in Figures 3A to 3D may each comprise a honeycomb core layer such as a paper honeycomb core layer, a polyurethane layer, a foamed foam, or an extruded foam; a honeycomb structure made from one or more polymer materials, including but not limited to polypropylene, polyethylene, polystyrene, polyamide, copolyamide, polyethylene terephthalate, polyetherimide, polyphenylene oxide, and other polymers; or a honeycomb structure made from one or more metals and metal alloys, including but not limited to aluminum, iron, steel, and other metals. In some embodiments, the core layer may be a honeycomb layer having a material other than cellulose. For example, the honeycomb layer may be porous and may contain a considerable amount of open space within the core layer. The core layers shown in Figures 3A to 3D may have a basis weight of about 200 grams / square meter (gsm) to about 4000 gsm. The overall thickness of the core layers shown in Figures 1A to 1I may vary from about 0.5 cm to about 7.5 cm. The depth of the recesses shown in Figures 3A to 3D of the core layer may vary from approximately 0.125 inches (approximately 3 mm) to approximately 1 inch (approximately 2.5 cm), for example, from approximately 5 mm to approximately 1.25 mm, depending on the overall thickness of the core layer. As described herein, different recesses may have different depths and / or geometric shapes.

[0043] In certain configurations, the core layers described herein can be used to provide multilayer assemblies that include the core layers in combination with skin layers or other layers. The exact configuration of the skin layers can vary, but the skin layers can be configured as porous fiber-reinforced thermoplastic layers placed on a first surface of the core layers. The porous fiber-reinforced thermoplastic layers can include a web of open-cell structures formed by multiple reinforcing materials, such as reinforcing fibers, held together with a thermoplastic material, such as a polyolefin material or other material. The porous fiber-reinforced thermoplastic layers can be bonded to the surfaces of multiple recesses across the first surface of the core layers, for example, the skin layers can have recesses that substantially mirror the recesses of the core layers, so that each recess comprises two layers, for example, core layer components and skin layer components. Various examples of multilayer assemblies having a core layer and one or more skin layers are described in more detail below.

[0044] In some configurations, a multilayer assembly may comprise a core layer and a single skin layer having one or more surface recesses on the surface of the multilayer assembly. Referring to Figure 4A, the multilayer assembly 400 comprises a core layer 410, a skin layer 411, and a recess 415 on the first surface 412 of the multilayer assembly 400. The exact shape, width, and depth of the recess 415 may vary, and exemplary shapes (in cross-sectional view) include triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. Although the recess 415 is shown as existing on the first surface 412, it may instead be located on the surface 414, or the recess may be located on both the surface 412 and the surface 414. The recess 415 includes both the core layer 410 and the skin layer 411. The presence of the recess 415 can enhance the bond between the skin layer 411 and the core layer 410.

[0045] In a particular embodiment, a multilayer assembly 420 is shown in Figure 4B as including a core layer 421 and a skin layer 422. A first recess 425 and a second recess 426 are shown on the first surface 423. The recesses 425 and 426 do not have to be the same, and the exact shape, width, and depth of the recesses 425 and 426 may be independently different, with exemplary shapes (in cross-sectional view) including triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. In some cases, one of the recesses may instead be located on a second surface, as shown in Figure 4C, and the second recess 427 is located on a second surface 424 of the multilayer assembly. If two recesses are located on different surfaces of the multilayer assembly, the shape, width, and depth of the recesses may be the same or different. Although not shown, a skin layer or other layer may be present on surface 424 as needed.

[0046] In other configurations, a multilayer assembly containing at least one skin layer may contain three or more recesses. Referring to Figure 4D, a multilayer assembly 430 is shown containing a core layer 431 and a skin layer 432, which has recesses 435, 436, and 437 on a first surface 433. The recesses 435, 436, and 437 do not have to be the same, and the exact shape, width, and depth of each recess 435, 436, and 437 may be independently different, and exemplary shapes (in cross-sectional view) include triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. In some cases, one of the recesses may instead be located on a second surface, as shown in Figure 4E, and a third recess 438 may be located on a second surface 434 of the multilayer assembly. If necessary, two or more recesses may be located on surface 434 of the multilayer assembly. If three recesses are located on different surfaces of the multilayer assembly, the shape, width, and depth of the recesses may be the same or different. Although not shown, a skin layer or other layer may be located on surface 434, if necessary.

[0047] In some embodiments, a multilayer assembly may include four or more recesses. Referring to Figure 4F, a multilayer assembly 440 is shown, which includes a core layer 441 and a skin layer 442, and which has recesses 445, 446, 447, and 448 on a first surface 443. The recesses 445, 446, 447, and 448 do not have to be the same, and the exact shape, width, and depth of each recess 445, 446, 447, and 448 may be independently different, and exemplary shapes (in cross-sectional view) include triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. In some cases, one of the recesses may instead be located on a second surface, as shown in Figure 4G, and a fourth recess 449 may be located on the second surface 444 of the multilayer assembly. If necessary, two or more recesses may be located on the surface 444 of the multilayer assembly. If the four recesses are located on different surfaces of the multilayer assembly 440, the shape, width, and depth of the recesses may be the same or different. Although not shown in the diagram, a skin layer or other layer may be present on surface 444 as needed.

[0048] In some embodiments, the core layer may include five or more recesses. Referring to Figure 4H, a multilayer assembly 450 is shown, which includes a core layer 451, a skin layer 452, and recesses 455, 456, 457, 458, and 459 on a first surface 453. The recesses 455, 456, 457, 458, and 459 do not have to be the same, and the exact shape, width, and depth of each recess 455, 456, 457, 458, and 459 may be independently different, and exemplary shapes (in cross-sectional view) include triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. In some cases, one of the recesses may instead be located on a second surface, as shown in Figure 4I, and a fifth recess 461 may be located on a second surface 454 of the multilayer assembly. If necessary, two or more recesses may be located on a surface 454 of the multilayer assembly. If the five recesses are located on different surfaces of the multilayer assembly, the shape, width, and depth of the recesses may be the same or different. Although not shown in the diagram, a skin layer or other layer may be present on surface 454 as needed.

[0049] In certain embodiments, the core layers shown in Figures 4A to 4I may each comprise a honeycomb core layer such as a paper honeycomb core layer, a polyurethane layer, a foamed foam, or an extruded foam; a honeycomb structure made from one or more polymer materials including but not limited to polypropylene, polyethylene, polystyrene, polyamide, copolyamide, polyethylene terephthalate, polyetherimide, polyphenylene oxide, and other polymers; or a honeycomb structure made from one or more metals and metal alloys including but not limited to aluminum, iron, steel, and other metals. In some embodiments, the core layer may be a honeycomb layer having a material other than cellulose. For example, the honeycomb layer may be porous and may contain a considerable amount of open space within the core layer. The core layers shown in Figures 4A to 4I may have a basis weight of about 200 grams / square meter (gsm) to about 4000 gsm. The overall thickness of the core layers shown in Figures 4A to 4I may vary from about 0.5 cm to about 7.5 cm. The depth of the recesses shown in Figures 4A to 4I of the core layer can vary from approximately 0.125 inches (approximately 3 mm) to approximately 1 inch (approximately 2.5 cm), for example, from approximately 5 mm to approximately 1.25 mm, depending on the overall thickness of the core layer. As described herein, different recesses can have different depths and / or geometric shapes.

[0050] In certain examples, the skin layers shown in Figures 4A to 4I may each comprise a porous fiber-reinforced thermoplastic layer. For example, the porous fiber-reinforced thermoplastic layer may be composed of (or used in) a glass mat thermoplastic composite (GMT) or a lightweight reinforced thermoplastic resin (LWRT). One such LWRT is prepared by HANWHA AZDEL and marketed under the trademark SUPERLITE® material. The surface density of such a GMT or LWRT may range from about 300 grams / m² (gsm) to about 4000 gsm, but depending on the needs of the specific application, the surface density may be less than 300 gsm or more than 4000 gsm. In some embodiments, the top density may be less than about 4000 gsm. In certain examples, the GMT or LWRT may comprise one or more lofting agent materials arranged in the voids or pores of the GMT or LWRT. If two or more GMT or LWRT layers are present, the GMT or LWRT layers may be the same or different.

[0051] In specific examples where LWRT is used as a porous fiber-reinforced thermoplastic skin layer, the LWRT typically comprises a thermoplastic material and multiple reinforcing fibers that together form a web of open-cell structure. The web can be formed from a random arrangement of reinforcing fibers held in place by the thermoplastic material. For example, a porous fiber-reinforced thermoplastic layer typically has a considerable amount of open-cell structure so that void spaces exist within the layer. In some examples, the porous fiber skin layers shown in Figures 4A to 4I have concentrations of 0-30%, 10-40%, 20-50%, 30-60%, 40-70%, 50-80%, 60-90%, 0-40%, 0-50%, 0-60%, 0-70%, 0-80%, 0-90%, 10-50%, 10-60%, 10-70%, 10-80%, 10-90%, 10-95%, and 20-60%. Porosity can be %, 20-70%, 20-80%, 20-90%, 20-95%, 30-70%, 30-80%, 30-90%, 30-95%, 40-80%, 40-90%, 40-95%, 50-90%, 50-95%, 60-95%, 70-80%, 70-90%, 70-95%, 80-90%, 80-95%, or any porosity within these exemplary ranges. In some examples, the skin layers shown in Figures 4A-4I have porosity or void content greater than 0%, for example, up to about 95% that are not fully solidified. Unless otherwise specified, references to skin layers shown in Figures 4A-4I with specific void content or porosity are based on the total volume of that skin layer, and not necessarily the total volume of the multilayer assembly.

[0052] In certain cases, the skin layers shown in Figures 4A to 4I can be manufactured in the form of GMT or LWRT sheets. In certain cases, the sheets can generally be prepared using chopped glass fibers, thermoplastic materials, optionally lofting agents, and one or more arbitrary thermoplastic polymer films and / or woven or nonwoven fabrics made of glass fibers or thermoplastic resin fibers, such as polypropylene (PP), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polycarbonate (PC), PC / PBT blends, or PC / PET blends. In some embodiments, PP, PBT, PET, PC / PET blends, or PC / PBT blends can be used as resins. To manufacture the sheets, the thermoplastic materials and reinforcing materials can be added to or metered into a dispersed foam contained in an open-top mixing tank fitted with an impeller. While we do not wish to be bound by any particular theory, the presence of air-trapped pockets in the foam can help disperse the glass fibers, thermoplastic materials, and lofting agents. In some examples, a dispersed mixture of fibers and thermoplastic material can be pumped via a distribution manifold to a headbox located above the wire section of a paper machine. The dispersed mixture is then fed to a moving wire screen using vacuum, which removes foam rather than fibers and thermoplastic material, continuously producing a uniform fibrous wet web. The wet web can be passed through a dryer at a temperature suitable for reducing moisture content and melting or softening the thermoplastic material. The resulting product can be pressed or compressed to form a sheet, for example, using a nip roller or other technique, and then bonded to a core layer or another layer.

[0053] In certain embodiments, the high porosity present in the skin layers shown in Figures 4A to 4I can reduce the overall weight of the multilayer assembly and allow for the inclusion of agents within the void spaces of the skin layers. For example, lofting agents can exist non-covalently within the void spaces. The application of heat or other perturbations can act to increase the volume of the non-covalently bonded lofting agents, which increases the overall thickness of the layer, for example, as the size of the lofting agents increases and / or additional air is trapped within the layer. If necessary, flame retardants, colorants, smoke suppressants and other materials may be included in the void spaces of the skin layers shown in Figures 4A to 4I. Before lofting, the multilayer assembly can be compressed to reduce its overall thickness, for example, before or after the layers are bonded to one or more other layers.

[0054] In certain embodiments, the thermoplastic material of the skin layer shown in Figures 4A to 4I may include, at least in part, one or more of polyolefins, or polyethylene, polypropylene, polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, and polyvinyl chloride, both plasticized and nonplasticized, as well as blends of these materials with each other or other polymer materials. Other suitable thermoplastic materials include, but are not limited to, polyarylene ethers, polycarbonates, polyester carbonates, thermoplastic polyesters, polyimides, polyetherimides, polyamides, copolyamides, acrylonitrile-butyl acrylate-styrene polymers, amorphous nylons, polyarylene ether ketones, polyphenylene sulfides, polyarylsulfones, polyethersulfones, liquid crystalline polymers, poly(1,4-phenylene) compounds commercially available as PARMAX®, high-temperature polycarbonates such as Bayer's APEC® PC, high-temperature nylons and silicones, as well as copolymers, alloys and blends of these materials with each other or other polymer materials. The thermoplastic materials used to form the skin layers shown in Figures 4A to 4I can be used in powder form, resin form, rosin form, particle form, fiber form or other suitable form. Various exemplary forms of thermoplastic materials are described herein, for example, in U.S. Patent Application Publication No. 20130244528 and U.S. Patent Application Publication No. 20120065283. The exact amount of thermoplastic material present in the skin layers shown in Figures 4A to 4I may vary, with exemplary amounts ranging from about 20% by weight to about 80% by weight, for example, 30 to 70% by weight or 35 to 65% by weight. It will be recognized by those skilled in the art that the total weight percentage of all materials used in any one of the skin layers shown in Figures 4A to 4I is added to 100% by weight.

[0055] In certain examples, the reinforcing fibers of the skin layer shown in Figures 4A to 4I may comprise glass fibers, carbon fibers, graphite fibers, synthetic organic fibers, in particular high modulus organic fibers, e.g., para- and meta-aramid fibers, nylon fibers, polyester fibers, resins suitable for use as fibers or with high melt flow index, mineral fibers such as basalt, mineral wool (e.g., rock or slag wool), wollastonite, alumina silica, or mixtures thereof, metal fibers, metallized natural and / or synthetic fibers, ceramic fibers, yarn fibers, or mixtures thereof. In some embodiments, any of the aforementioned fibers may be chemically treated before use to provide desired functional groups or to impart other physical properties to the fibers, for example, by chemical treatment to enable reaction with thermoplastic materials, lofting agents or both. The fiber content in the skin layer shown in Figures 4A to 4I may independently be about 20% to about 90% of the layer's weight, more specifically about 30% to about 70% of the layer's weight. Typically, the fiber content of a multilayer assembly having the skin layers shown in Figures 4A–4I varies between about 20%–90% by weight of the assembly, more specifically between about 30%–80% by weight, for example between about 40%–70% by weight. The specific size and / or orientation of the fibers used may depend, at least in part, on the thermoplastic polymer material used and / or the desired properties of the skin layers shown in Figures 4A–4I. Appropriate additional fiber types, fiber sizes and quantities will be readily selected by those skilled in the art, taking into account the interests of this disclosure. In one non-limiting example, the fibers dispersed in the thermoplastic material and optionally in the lofting agent to provide the skin layers shown in Figures 4A–4I may generally have a diameter greater than about 5 microns, more specifically between about 5 microns and about 22 microns, and a length of about 5 mm to about 200 mm, more specifically, the fiber diameter may be about 2 microns to about 22 microns, and the fiber length may be about 5 mm to about 75 mm.

[0056] In some embodiments, the lofting ability of the skin layers shown in Figures 4A to 4I can be further adjusted by including one or more added lofting agents. The exact type of lofting agent used in the skin layers shown in Figures 4A to 4I may depend on many factors, including, for example, a desired lofting temperature and a desired degree of loft. In some cases, microsphere lofting agents that can increase in size when exposed to convective heating, such as expandable microspheres, can be used. Exemplary commercially available lofting agents are available from Kureha Corporation (Japan). In other examples, a first lofting agent having a first average particle size and a second lofting agent having a second average particle size different from the first average particle size can be used in the skin layers shown in Figures 4A to 4I. In other examples, the lofting agent may be an expandable graphite material that can also impart some flame retardancy to the multilayer assembly.

[0057] In some configurations, the skin layers shown in Figures 4A to 4I may be substantially halogen-free or halogen-free layers to meet the limitations of hazardous substance requirements for a particular application. In other examples, one or more layers may contain halogenated flame retardants, e.g., one or more of F, Cl, Br, I, and At, or compounds containing such halogens, e.g., tetrabromobisphenol-A polycarbonate or monohalo-, dihalo-, trihalo-, or tetrahalopolycarbonate. In some examples, the thermoplastic material used for the skin layers shown in Figures 4A to 4I may contain one or more halogens to impart some degree of flame retardancy without the addition of another flame retardant. Where halogenated flame retardants are present, they are preferably present in amounts that can vary depending on other components present. For example, the halogenated flame retardant may be present in amounts of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically about 1% to about 13% by weight, e.g., about 5% to about 13% by weight. If necessary, two different halogenated flame retardants may be added to the layer. In other examples, non-halogenated flame retardants may be added, such as flame retardants containing one or more of N, P, As, Sb, Bi, S, Se, and Te. In some embodiments, the non-halogenated flame retardants may contain phosphorylated materials, and as a result, the layer may be more environmentally friendly. If non-halogenated or substantially halogen-free flame retardants are present, the flame retardants are preferably present in an amount that can vary depending on other components present. For example, substantially halogen-free flame retardants may be present in an amount of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically, about 1% to about 13% by weight based on the weight of the layer, for example, about 5% to about 13% by weight. If desired, two different substantially halogen-free flame retardants may be added to one or more layers described herein.In certain cases, one or more of the skin layers shown in Figures 4A to 4I described herein may contain one or more halogenated flame retardants in combination with one or more substantially halogen-free flame retardants. If two different flame retardants are present, the combination of the two flame retardants may be present in amounts that can vary depending on other components present. For example, the total weight of the flame retardants present may be about 0.1 weight percent to about 20 weight percent (based on the weight of the layer), more specifically, about 1 weight percent to about 15 weight percent based on the weight of the layer, for example, about 2 weight percent to about 14 weight percent. The flame retardants used in the layers described herein can be added to a mixture containing thermoplastic material and fibers (before discarding the mixture onto a wire screen or other processing component), or they can be added after the layer has been formed. In some examples, the flame retardant material may include one or more of expansive graphite material, magnesium hydroxide (MDH), and aluminum hydroxide (ATH).

[0058] In certain embodiments, the skin layer shown in Figures 4A to 4I may include one or more film layers in combination with the porous fiber-reinforced thermoplastic layer. For example, the film of the skin layer shown in Figures 4A to 4I may include, or be, a thermoplastic film, a polyolefin film, an elastomer film, etc. In certain configurations, the film includes at least one of the following: polyolefin, e.g., polyethylene or polypropylene, at least one poly(etherimide), at least one poly(etherketone), at least one poly(ether-etherketone), at least one poly(phenylene sulfide), poly(arylene sulfone), at least one poly(ethersulfone), at least one poly(amideimide), poly(1,4-phenylene), at least one polycarbonate, at least one nylon, and at least one silicone. In some embodiments, there may be two or more films in combination with the porous fiber-reinforced thermoplastic layer for the skin layer shown in Figures 4A to 4I.

[0059] In some embodiments, two or more surfaces of a multilayer assembly including a core layer and a skin layer may have multiple recesses. Referring to Figure 5A, a multilayer assembly 510 is shown having multiple recesses on a first surface 513 and a second surface 514. In some cases, different surfaces may include different numbers of recesses, recesses of different depths, recesses of different shapes, etc. The first surface 513 has a skin layer 512 on a core layer 511. Recesses on any one surface may, as required, have the same or different shapes, widths, or depths. Furthermore, all recesses on the first surface 513 may have a first shape (cross-sectional view), and all recesses on the second surface 514 may have a second shape (cross-sectional view). The first shape may be the same as or different from the second shape. The distribution of recesses on the first surface 513 and the second surface 514 does not need to be uniform, and, if required, more recesses may be located in one area of ​​the core layer than in other areas of the core layer. Also, the recess distribution does not have to be the same on the first surface 513 and the second surface 514. Referring to Figure 5B, a multilayer assembly 520 is shown with a core layer 521 and a skin layer 522, and an increased number of recesses located at the edges 524, 525 on the first surface 523 of the multilayer assembly 520. The distribution of recesses may also have other arrangements. For example, the increased number of recesses may be arranged toward one side or edge 524 on the first surface 523. Alternatively, a recess distribution may be produced in which more recesses are located toward the central region of the multilayer assembly. The recesses on the second surface of the multilayer assemblies 510, 520 are shown as uniform for illustrative purposes, but instead, the recess distribution may be non-uniform or asymmetrical, as described in relation to the recesses on the first surface of the multilayer assemblies 510, 520.

[0060] In certain embodiments, the core layers shown in Figures 5A and 5B may each comprise a honeycomb core layer such as a paper honeycomb core layer, a polyurethane layer, a foamed foam, or an extruded foam; a honeycomb structure made from one or more polymer materials including but not limited to polypropylene, polyethylene, polystyrene, polyamide, copolyamide, polyethylene terephthalate, polyetherimide, polyphenylene oxide, and other polymers; or a honeycomb structure made from one or more metals and metal alloys including but not limited to aluminum, iron, steel, and other metals. In some embodiments, the core layer may be a honeycomb layer having a material other than cellulose. For example, the honeycomb layer may be porous and may contain a considerable amount of open space within the core layer. The core layers shown in Figures 5A and 5B may have a basis weight of about 200 grams / square meter (gsm) to about 4000 gsm. The overall thickness of the core layers shown in Figures 5A and 5B may vary from about 0.5 cm to about 7.5 cm. The depth of the recesses shown in the core layers of Figures 5A and 5B can vary from approximately 0.125 inches (approximately 3 mm) to approximately 1 inch (approximately 2.5 cm), for example, from approximately 5 mm to approximately 1.25 mm, depending on the overall thickness of the core layer. As described herein, different recesses can have different depths and / or geometric shapes.

[0061] In certain examples, the skin layers shown in Figures 5A and 5B may each comprise a porous fiber-reinforced thermoplastic layer. For example, the porous fiber-reinforced thermoplastic layer may be composed of (or used in) a glass mat thermoplastic composite (GMT) or a lightweight reinforced thermoplastic resin (LWRT). One such LWRT is prepared by HANWHA AZDEL and marketed under the trademark SUPERLITE® material. The surface density of such a GMT or LWRT may range from about 300 grams / square meter (gsm) to about 4000 gsm, but depending on the needs of the specific application, the surface density may be less than 300 gsm or more than 4000 gsm. In some embodiments, the top density may be less than about 4000 gsm. In certain examples, the GMT or LWRT may comprise one or more lofting agent materials arranged in the voids or pores of the GMT or LWRT. If two or more GMT or LWRT layers are present, the GMT or LWRT layers may be the same or different.

[0062] In specific examples where LWRT is used as a porous fiber-reinforced thermoplastic skin layer, the LWRT typically comprises a thermoplastic material and multiple reinforcing fibers that together form a web of open-cell structure. The web can be formed from a random arrangement of reinforcing fibers held in place by the thermoplastic material. For example, a porous fiber-reinforced thermoplastic layer typically has a considerable amount of open-cell structure so that void spaces exist within the layer. In some examples, the porous fiber skin layers shown in Figures 5A and 5B have concentrations of 0-30%, 10-40%, 20-50%, 30-60%, 40-70%, 50-80%, 60-90%, 0-40%, 0-50%, 0-60%, 0-70%, 0-80%, 0-90%, 10-50%, 10-60%, 10-70%, 10-80%, 10-90%, 10-95%, and 20-60%. Porosity can be 0%, 20-70%, 20-80%, 20-90%, 20-95%, 30-70%, 30-80%, 30-90%, 30-95%, 40-80%, 40-90%, 40-95%, 50-90%, 50-95%, 60-95%, 70-80%, 70-90%, 70-95%, 80-90%, 80-95%, or any porosity within these exemplary ranges. In some examples, the skin layers shown in Figures 5A and 5B have porosity or void content greater than 0%, for example, up to about 95% that are not fully solidified. Unless otherwise specified, references to skin layers shown in Figures 5A and 5B with specific void content or porosity are based on the total volume of that skin layer, and not necessarily the total volume of the multilayer assembly.

[0063] In certain cases, the skin layers shown in Figures 5A and 5B can be manufactured in the form of GMT or LWRT sheets. In certain cases, the sheets can generally be prepared using chopped glass fibers, thermoplastic materials, optionally lofting agents, and one or more arbitrary thermoplastic polymer films and / or woven or nonwoven fabrics made of glass fibers or thermoplastic resin fibers, such as polypropylene (PP), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polycarbonate (PC), PC / PBT blends, or PC / PET blends. In some embodiments, PP, PBT, PET, PC / PET blends, or PC / PBT blends can be used as resins. To manufacture the sheets, the thermoplastic materials and reinforcing materials can be added to or metered into a dispersed foam contained in an open-top mixing tank fitted with an impeller. While we do not wish to be bound by any particular theory, the presence of air-trapped pockets in the foam can help disperse the glass fibers, thermoplastic materials, and lofting agents. In some examples, a dispersed mixture of fibers and thermoplastic material can be pumped via a distribution manifold to a headbox located above the wire section of a paper machine. The dispersed mixture is then fed to a moving wire screen using vacuum, which removes foam rather than fibers and thermoplastic material, continuously producing a uniform fibrous wet web. The wet web can be passed through a dryer at a temperature suitable for reducing moisture content and melting or softening the thermoplastic material. The resulting product can be pressed or compressed to form a sheet, for example, using a nip roller or other technique, and then bonded to a core layer or another layer.

[0064] In certain embodiments, the high porosity present in the skin layer shown in Figures 5A and 5B can reduce the overall weight of the multilayer assembly and allow for the inclusion of agents within the void spaces of the skin layer. For example, lofting agents can be present in the void spaces non-covalently. The application of heat or other perturbations can act to increase the volume of the non-covalently bonded lofting agents, which increases the overall thickness of the layer, for example, as the size of the lofting agents increases and / or additional air is trapped in the layer. If necessary, flame retardants, colorants, smoke suppressants and other materials may be included in the void spaces of the skin layer shown in Figures 5A and 5B. Before lofting, the multilayer assembly can be compressed to reduce its overall thickness, for example, before or after a layer is bonded to one or more other layers.

[0065] In certain embodiments, the thermoplastic material of the skin layer shown in Figures 5A and 5B may, at least in part, include one or more of polyolefins, or polyethylene, polypropylene, polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, and polyvinyl chloride, both plasticized and nonplasticized, as well as blends of these materials with each other or with other polymer materials. Other suitable thermoplastic materials include, but are not limited to, polyarylene ethers, polycarbonates, polyester carbonates, thermoplastic polyesters, polyimides, polyetherimides, polyamides, copolyamides, acrylonitrile-butyl acrylate-styrene polymers, amorphous nylons, polyarylene ether ketones, polyphenylene sulfides, polyarylsulfones, polyethersulfones, liquid crystalline polymers, poly(1,4-phenylene) compounds commercially available as PARMAX®, high-temperature polycarbonates such as Bayer's APEC® PC, high-temperature nylons and silicones, as well as copolymers, alloys and blends of these materials with each other or other polymer materials. The thermoplastic materials used to form the skin layers shown in Figures 5A and 5B can be used in powder form, resin form, rosin form, particle form, fiber form or other suitable form. Various exemplary forms of thermoplastic materials are described herein, for example, in U.S. Patent Application Publication No. 20130244528 and U.S. Patent Application Publication No. 20120065283. The exact amount of thermoplastic material present in the skin layers shown in Figures 5A and 5B may vary, with exemplary amounts ranging from about 20% by weight to about 80% by weight, for example, 30-70% by weight or 35-65% by weight. It will be recognized by those skilled in the art that the total weight percentage of all materials used in either of the skin layers shown in Figures 5A and 5B is added to 100% by weight.

[0066] In certain examples, the reinforcing fibers of the skin layer shown in Figures 5A and 5B may comprise glass fibers, carbon fibers, graphite fibers, synthetic organic fibers, in particular high modulus organic fibers, e.g., para- and meta-aramid fibers, nylon fibers, polyester fibers, resins suitable for use as fibers or with high melt flow index, mineral fibers such as basalt, mineral wool (e.g., rock or slag wool), wollastonite, alumina silica, or mixtures thereof, metal fibers, metallized natural and / or synthetic fibers, ceramic fibers, yarn fibers, or mixtures thereof. In some embodiments, any of the aforementioned fibers may be chemically treated before use to provide desired functional groups or to impart other physical properties to the fibers, for example, by chemical treatment to enable reaction with thermoplastic materials, lofting agents or both. The fiber content in the skin layer shown in Figures 5A and 5B may independently be about 20% to about 90% of the layer's weight, more specifically about 30% to about 70% of the layer's weight. Typically, the fiber content of a multilayer assembly including the skin layer shown in Figures 5A and 5B varies between about 20% and about 90% by weight of the assembly, more specifically between about 30% and about 80% by weight, for example between about 40% and about 70% by weight. The specific size and / or orientation of the fibers used may depend, at least in part, on the thermoplastic polymer material used and / or the desired properties of the skin layer shown in Figures 5A and 5B. Appropriate additional fiber types, fiber sizes and quantities will be readily selected by those skilled in the art, taking into account the interests of this disclosure. In one non-limiting example, the fibers dispersed in the thermoplastic material and optionally in the lofting agent to provide the skin layer shown in Figures 5A and 5B may generally have a diameter greater than about 5 microns, more specifically between about 5 microns and about 22 microns, and a length of about 5 mm to about 200 mm, more specifically, the fiber diameter may be about 2 microns to about 22 microns, and the fiber length may be about 5 mm to about 75 mm.

[0067] In some embodiments, the lofting ability of the skin layers shown in Figures 5A and 5B can be further adjusted by including one or more added lofting agents. The exact type of lofting agent used in the skin layers shown in Figures 5A and 5B may depend on many factors, including, for example, a desired lofting temperature and a desired degree of loft. In some cases, microsphere lofting agents that can increase in size when exposed to convective heating, such as expandable microspheres, can be used. Exemplary commercially available lofting agents are available from Kureha Corporation (Japan). In other examples, a first lofting agent having a first average particle size and a second lofting agent having a second average particle size different from the first average particle size can be used in the skin layers shown in Figures 5A and 5B. In other examples, the lofting agent may be an expandable graphite material that can also impart some flame retardancy to the multilayer assembly.

[0068] In some configurations, the skin layers shown in Figures 5A and 5B may be substantially halogen-free or halogen-free to meet the limitations of hazardous substance requirements for a particular application. In other examples, one or more layers may contain halogenated flame retardants, e.g., one or more of F, Cl, Br, I, and At, or compounds containing such halogens, e.g., tetrabromobisphenol-A polycarbonate or monohalo-, dihalo-, trihalo-, or tetrahalopolycarbonate. In some cases, the thermoplastic material used for the skin layers shown in Figures 5A and 5B may contain one or more halogens to impart some degree of flame retardancy without the addition of another flame retardant. Where halogenated flame retardants are present, they are preferably present in amounts that can vary depending on other components present. For example, the halogenated flame retardant may be present in amounts of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically about 1% to about 13% by weight, e.g., about 5% to about 13% by weight. If necessary, two different halogenated flame retardants may be added to the layer. In other examples, non-halogenated flame retardants may be added, such as flame retardants containing one or more of N, P, As, Sb, Bi, S, Se, and Te. In some embodiments, the non-halogenated flame retardants may contain phosphorylated materials, and as a result, the layer may be more environmentally friendly. If non-halogenated or substantially halogen-free flame retardants are present, the flame retardants are preferably present in an amount that can vary depending on other components present. For example, substantially halogen-free flame retardants may be present in an amount of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically, about 1% to about 13% by weight based on the weight of the layer, for example, about 5% to about 13% by weight. If desired, two different substantially halogen-free flame retardants may be added to one or more layers described herein.In certain cases, one or more of the skin layers shown in Figures 5A and 5B described herein may contain one or more halogenated flame retardants in combination with one or more substantially halogen-free flame retardants. If two different flame retardants are present, the combination of the two flame retardants may be present in amounts that can vary depending on other components present. For example, the total weight of the flame retardants present may be about 0.1 weight percent to about 20 weight percent (based on the weight of the layer), more specifically, about 1 weight percent to about 15 weight percent based on the weight of the layer, for example, about 2 weight percent to about 14 weight percent. The flame retardants used in the layers described herein can be added to a mixture containing thermoplastic material and fibers (before discarding the mixture onto a wire screen or other processing component) or can be added after the layer has been formed. In some examples, the flame retardant material may include one or more of expansive graphite material, magnesium hydroxide (MDH), and aluminum hydroxide (ATH).

[0069] In certain configurations, the skin layer shown in Figures 5A and 5B may include one or more film layers in combination with the porous fiber-reinforced thermoplastic layer. For example, the film of the skin layer shown in Figures 5A and 5B may include, or be, a thermoplastic film, a polyolefin film, an elastomer film, etc. In certain configurations, the film includes at least one of the following: polyolefin, e.g., polyethylene or polypropylene, at least one poly(etherimide), at least one poly(etherketone), at least one poly(ether-etherketone), at least one poly(phenylene sulfide), poly(arylene sulfone), at least one poly(ethersulfone), at least one poly(amideimide), poly(1,4-phenylene), at least one polycarbonate, at least one nylon, and at least one silicone. In some embodiments, there may be two or more films in combination with the porous fiber-reinforced thermoplastic layer for the skin layer shown in Figures 5A and 5B.

[0070] In certain configurations, the core layers described herein can be used to provide a multilayer assembly including the core layer in combination with two skin layers. The exact configuration of the skin layers can vary, but each skin layer can be configured as a porous fiber-reinforced thermoplastic layer placed on the surface of the core layer. Each porous fiber-reinforced thermoplastic layer can include a web of open-cell structure formed by multiple reinforcing materials held together with the thermoplastic material. One or both of the porous fiber-reinforced thermoplastic layers can be bonded to the surface of multiple recesses across the first surface of the core layer, for example, a skin layer may have recesses that substantially mirror the recesses of the core layer, so that each recess comprises two layers, e.g., a core layer component and a skin layer component.

[0071] Referring to Figure 6A, the multilayer assembly 600 comprises a core layer 610, a first skin layer 611, and a second skin layer 612. A recess 616 on the first surface 615 of the multilayer assembly 600 is shown. The exact shape, width, and depth of the recess 616 may vary, and exemplary shapes (in cross-sectional view) include triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. Although the recess 616 is shown as being present on the first surface 615, it may instead be present on surface 617, or recesses may be present on both surfaces 616 and 617. The recess 617 includes both the core layer 610 and the skin layer 611. The presence of the recess 616 can enhance the bond between the skin layer 611 and the core layer 610. In Figure 6A, no recess is present on the second surface 617 of the multilayer assembly 600. Multiple recesses 616 may be present on the first surface 615, if necessary. For example, the first surface 615 may have one, two, three, four, five or more individual recesses across the surface 615.

[0072] In a particular embodiment, the multilayer assembly 620 is shown in Figure 6B as comprising a core layer 621, a first skin layer 622, and a second skin layer 623. A first recess 626 is present on the first surface 624, and a second recess 628 is present on the second surface 627. The recesses 626 and 628 do not have to be the same, and the exact shape, width, and depth of the recesses 626 and 628 may differ independently, with exemplary shapes (in cross-sectional view) including triangular, semicircular, elliptical, symmetrical, asymmetrical, and other shapes. In some examples, the surface 624 may have one, two, three, four, five, or more recesses. Similarly, the surface 627 may have one, two, three, four, five, or more recesses. The number of recesses on each surface 624, 627 does not have to be the same. By including recesses on different surfaces of the multilayer assembly 620, which includes a core layer 621 and two skin layers 622 and 623, an enhanced bond between the different skin layers 622 and 623 and the core layer 621 can be achieved.

[0073] In certain embodiments, the core layers shown in Figures 6A and 6B may each comprise a honeycomb core layer such as a paper honeycomb core layer, a polyurethane layer, a foamed foam, or an extruded foam; a honeycomb structure made from one or more polymer materials including but not limited to polypropylene, polyethylene, polystyrene, polyamide, copolyamide, polyethylene terephthalate, polyetherimide, polyphenylene oxide, and other polymers; or a honeycomb structure made from one or more metals and metal alloys including but not limited to aluminum, iron, steel, and other metals. In some embodiments, the core layer may be a honeycomb layer having a material other than cellulose. For example, the honeycomb layer may be porous and may contain a considerable amount of open space within the core layer. The core layers shown in Figures 6A and 6B may have a basis weight of about 200 grams / square meter (gsm) to about 4000 gsm. The overall thickness of the core layers shown in Figures 6A and 6B may vary from about 0.5 cm to about 7.5 cm. The depth of the recesses shown in the core layers of Figures 6A and 6B can vary from approximately 0.125 inches (approximately 3 mm) to approximately 1 inch (approximately 2.5 cm), for example, from approximately 5 mm to approximately 1.25 mm, depending on the overall thickness of the core layer. As described herein, different recesses can have different depths and / or geometric shapes.

[0074] In certain examples, the skin layers shown in Figures 6A and 6B may each comprise a porous fiber-reinforced thermoplastic layer. For example, the porous fiber-reinforced thermoplastic layer may be composed of (or used in) a glass mat thermoplastic composite (GMT) or a lightweight reinforced thermoplastic resin (LWRT). One such LWRT is prepared by HANWHA AZDEL and marketed under the trademark SUPERLITE® material. The surface density of such a GMT or LWRT may range from about 300 grams / m² (gsm) to about 4000 gsm, but depending on the needs of the specific application, the surface density may be less than 300 gsm or more than 4000 gsm. In some embodiments, the top density may be less than about 4000 gsm. In certain examples, the GMT or LWRT may comprise one or more lofting agent materials arranged in the voids or pores of the GMT or LWRT. If two or more GMT or LWRT layers are present, the GMT or LWRT layers may be the same or different.

[0075] In specific examples where LWRT is used as a porous fiber-reinforced thermoplastic skin layer, the LWRT typically comprises a thermoplastic material and multiple reinforcing fibers that together form a web of open-cell structure. The web can be formed from a random arrangement of reinforcing fibers held in place by the thermoplastic material. For example, a porous fiber-reinforced thermoplastic layer typically has a considerable amount of open-cell structure so that void spaces exist within the layer. In some examples, the porous fiber skin layers shown in Figures 6A and 6B have concentrations of 0-30%, 10-40%, 20-50%, 30-60%, 40-70%, 50-80%, 60-90%, 0-40%, 0-50%, 0-60%, 0-70%, 0-80%, 0-90%, 10-50%, 10-60%, 10-70%, 10-80%, 10-90%, 10-95%, and 20-60%. Porosity can be %, 20-70%, 20-80%, 20-90%, 20-95%, 30-70%, 30-80%, 30-90%, 30-95%, 40-80%, 40-90%, 40-95%, 50-90%, 50-95%, 60-95%, 70-80%, 70-90%, 70-95%, 80-90%, 80-95%, or any porosity within these exemplary ranges. In some examples, the skin layers shown in Figures 6A and 6B have porosity or void content greater than 0%, for example, up to about 95% that are not fully solidified. Unless otherwise specified, references to skin layers shown in Figures 6A and 6B with specific void content or porosity are based on the total volume of that skin layer, and not necessarily the total volume of the multilayer assembly.

[0076] In certain cases, the skin layers shown in Figures 6A and 6B can be manufactured in the form of GMT or LWRT sheets. In certain cases, the sheets can generally be prepared using chopped glass fibers, thermoplastic materials, optionally lofting agents, and one or more arbitrary thermoplastic polymer films and / or woven or nonwoven fabrics made of glass fibers or thermoplastic resin fibers, such as polypropylene (PP), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polycarbonate (PC), PC / PBT blends, or PC / PET blends. In some embodiments, PP, PBT, PET, PC / PET blends, or PC / PBT blends can be used as resins. To manufacture the sheets, the thermoplastic materials and reinforcing materials can be added to or metered into a dispersed foam contained in an open-top mixing tank fitted with an impeller. While we do not wish to be bound by any particular theory, the presence of air-trapped pockets in the foam can help disperse the glass fibers, thermoplastic materials, and lofting agents. In some examples, a dispersed mixture of fibers and thermoplastic material can be pumped via a distribution manifold to a headbox located above the wire section of a paper machine. The dispersed mixture is then fed to a moving wire screen using vacuum, which removes foam rather than fibers and thermoplastic material, continuously producing a uniform fibrous wet web. The wet web can be passed through a dryer at a temperature suitable for reducing moisture content and melting or softening the thermoplastic material. The resulting product can be pressed or compressed to form a sheet, for example, using a nip roller or other technique, and then bonded to a core layer or another layer.

[0077] In certain embodiments, the high porosity present in the skin layer shown in Figures 6A and 6B can reduce the overall weight of the multilayer assembly and allow for the inclusion of agents within the void spaces of the skin layer. For example, lofting agents can be present in the void spaces non-covalently. The application of heat or other perturbations can act to increase the volume of the non-covalently bonded lofting agents, which increases the overall thickness of the layer, for example, as the size of the lofting agents increases and / or additional air is trapped in the layer. If necessary, flame retardants, colorants, smoke suppressants and other materials may be included in the void spaces of the skin layer shown in Figures 6A and 6B. Before lofting, the multilayer assembly can be compressed to reduce its overall thickness, for example, before or after the layers are bonded to one or more other layers.

[0078] In certain embodiments, the thermoplastic material of the skin layer shown in Figures 6A and 6B may, at least in part, include one or more of polyolefins, or polyethylene, polypropylene, polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, and polyvinyl chloride, both plasticized and nonplasticized, as well as blends of these materials with each other or with other polymer materials. Other suitable thermoplastic materials include, but are not limited to, polyarylene ethers, polycarbonates, polyester carbonates, thermoplastic polyesters, polyimides, polyetherimides, polyamides, copolyamides, acrylonitrile-butyl acrylate-styrene polymers, amorphous nylons, polyarylene ether ketones, polyphenylene sulfides, polyarylsulfones, polyethersulfones, liquid crystalline polymers, poly(1,4-phenylene) compounds commercially available as PARMAX®, high-temperature polycarbonates such as Bayer's APEC® PC, high-temperature nylons and silicones, as well as copolymers, alloys and blends of these materials with each other or other polymer materials. The thermoplastic materials used to form the skin layers shown in Figures 6A and 6B can be used in powder form, resin form, rosin form, particle form, fiber form or other suitable form. Various exemplary forms of thermoplastic materials are described herein, for example, in U.S. Patent Application Publication No. 20130244528 and U.S. Patent Application Publication No. 20120065283. The exact amount of thermoplastic material present in the skin layers shown in Figures 6A and 6B may vary, with exemplary amounts ranging from about 20% by weight to about 80% by weight, for example, 30-70% by weight or 35-65% by weight. It will be recognized by those skilled in the art that the total weight percentage of all materials used in either of the skin layers shown in Figures 6A and 6B is added to 100% by weight.

[0079] In certain examples, the reinforcing fibers of the skin layer shown in Figures 6A and 6B may comprise glass fibers, carbon fibers, graphite fibers, synthetic organic fibers, in particular high modulus organic fibers, e.g., para- and meta-aramid fibers, nylon fibers, polyester fibers, resins suitable for use as fibers or with high melt flow index, mineral fibers such as basalt, mineral wool (e.g., rock or slag wool), wollastonite, alumina silica, or mixtures thereof, metal fibers, metallized natural and / or synthetic fibers, ceramic fibers, yarn fibers, or mixtures thereof. In some embodiments, any of the aforementioned fibers may be chemically treated before use to provide desired functional groups or to impart other physical properties to the fibers, for example, by chemical treatment to enable reaction with thermoplastic materials, lofting agents or both. The fiber content in the skin layer shown in Figures 6A and 6B may independently be about 20% to about 90% of the layer's weight, more specifically about 30% to about 70% of the layer's weight. Typically, the fiber content of a multilayer assembly including the skin layer shown in Figures 6A and 6B varies between about 20% and about 90% by weight of the assembly, more specifically between about 30% and about 80% by weight, for example, about 40% and about 70% by weight. The specific size and / or orientation of the fibers used may depend, at least in part, on the thermoplastic polymer material used and / or the desired properties of the skin layer shown in Figures 6A and 6B. Appropriate additional fiber types, fiber sizes and quantities will be readily selected by those skilled in the art, taking into account the interests of this disclosure. In one non-limiting example, the fibers dispersed in the thermoplastic material and optionally in the lofting agent to provide the skin layer shown in Figures 6A and 6B may generally have a diameter greater than about 5 microns, more specifically between about 5 microns and about 22 microns, and a length of about 5 mm to about 200 mm, more specifically, the fiber diameter may be about 2 microns to about 22 microns, and the fiber length may be about 5 mm to about 75 mm.

[0080] In some embodiments, the lofting ability of the skin layers shown in Figures 6A and 6B can be further adjusted by including one or more added lofting agents. The exact type of lofting agent used in the skin layers shown in Figures 6A and 6B may depend on many factors, including, for example, a desired lofting temperature and a desired degree of loft. In some cases, microsphere lofting agents that can increase in size when exposed to convective heating, such as expandable microspheres, can be used. Exemplary commercially available lofting agents are available from Kureha Corporation (Japan). In other examples, a first lofting agent having a first average particle size and a second lofting agent having a second average particle size different from the first average particle size can be used in the skin layers shown in Figures 6A and 6B. In other examples, the lofting agent may be an expandable graphite material that can also impart some flame retardancy to the multilayer assembly.

[0081] In some configurations, the skin layers shown in Figures 6A and 6B may be substantially halogen-free or halogen-free to meet the limitations of hazardous substance requirements for a particular application. In other examples, one or more layers may contain halogenated flame retardants, e.g., one or more of F, Cl, Br, I, and At, or compounds containing such halogens, e.g., tetrabromobisphenol-A polycarbonate or monohalo-, dihalo-, trihalo-, or tetrahalopolycarbonate. In some cases, the thermoplastic material used for the skin layers shown in Figures 6A and 6B may contain one or more halogens to impart some degree of flame retardancy without the addition of another flame retardant. Where halogenated flame retardants are present, they are preferably present in amounts that can vary depending on other components present. For example, the halogenated flame retardant may be present in amounts of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically about 1% to about 13% by weight, e.g., about 5% to about 13% by weight. If necessary, two different halogenated flame retardants may be added to the layer. In other examples, non-halogenated flame retardants may be added, such as flame retardants containing one or more of N, P, As, Sb, Bi, S, Se, and Te. In some embodiments, the non-halogenated flame retardants may contain phosphorylated materials, and as a result, the layer may be more environmentally friendly. If non-halogenated or substantially halogen-free flame retardants are present, the flame retardants are preferably present in an amount that can vary depending on other components present. For example, substantially halogen-free flame retardants may be present in an amount of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically, about 1% to about 13% by weight based on the weight of the layer, for example, about 5% to about 13% by weight. If desired, two different substantially halogen-free flame retardants may be added to one or more layers described herein.In certain cases, one or more of the skin layers shown in Figures 6A and 6B described herein may contain one or more halogenated flame retardants in combination with one or more substantially halogen-free flame retardants. If two different flame retardants are present, the combination of the two flame retardants may be present in amounts that can vary depending on other components present. For example, the total weight of the flame retardants present may be about 0.1 weight percent to about 20 weight percent (based on the weight of the layer), more specifically, about 1 weight percent to about 15 weight percent based on the weight of the layer, for example, about 2 weight percent to about 14 weight percent. The flame retardants used in the layers described herein can be added to a mixture containing thermoplastic material and fibers (before discarding the mixture onto a wire screen or other processing component) or can be added after the layer has been formed. In some examples, the flame retardant material may include one or more of expansive graphite material, magnesium hydroxide (MDH), and aluminum hydroxide (ATH).

[0082] In certain embodiments, the skin layer shown in Figures 6A and 6B may include one or more film layers in combination with the porous fiber-reinforced thermoplastic layer. For example, the film of the skin layer shown in Figures 6A and 6B may include, or be, a thermoplastic film, a polyolefin film, an elastomer film, etc. In certain configurations, the film includes at least one of the following: polyolefin, e.g., polyethylene or polypropylene, at least one poly(etherimide), at least one poly(etherketone), at least one poly(ether-etherketone), at least one poly(phenylene sulfide), poly(arylene sulfone), at least one poly(ethersulfone), at least one poly(amideimide), poly(1,4-phenylene), at least one polycarbonate, at least one nylon, and at least one silicone. In some embodiments, there may be two or more films in combination with the porous fiber-reinforced thermoplastic layer for the skin layer shown in Figures 6A and 6B.

[0083] In some embodiments, a multilayer assembly may include a core layer, a skin layer, and an additional layer. Referring to Figure 7A, a multilayer assembly 700 is shown, comprising a core layer 711, a skin layer 712, and an additional layer 713 positioned on the skin layer 712. In Figure 7A, the additional layer 713 coincides with the skin layer 712 such that a recess 715 includes the core layer 711, the skin layer 712, and the additional layer 713. In other examples, the additional layer may have sufficient structure to span any recess in the skin layer. For example, referring to Figure 7B, a multilayer assembly 720 is shown, comprising a core layer 721, a skin layer 722, and an additional layer 723 positioned on the skin layer 722. A recess 725 is shown that forms a gap between the skin layer 722 and the additional layer 723. For example, a projection or other device may be pressed into the skin layer 722 and the core layer 721 to form the recess 725, as will be described in more detail below. Next, layer 723 can be placed on the assembly such that layer 723 overlaps the recess 725. Even when viewing the multilayer assembly 720 outward, the additional layer 723 can be generally planar, so no recess is shown on the surface of the multilayer assembly 720. The presence of a skin layer 722 with a recess into the core layer 721 combined with the additional layer 723 can enhance the bond between the skin layer 722 and the core layer 721, but still provides a nearly flat or planar surface for the multilayer assembly 720. If an additional layer is present on the skin layer as shown in Figures 7A and 7B, one or more surfaces of the multilayer assembly may contain two, three, four, five or more individual recesses, each recess containing a core layer, a skin layer, and optionally an additional layer. Although not shown, one, two, three, four, five or more recesses may be present on any one surface of the assembly shown in Figures 7A and 7B.

[0084] In certain embodiments, the core layers shown in Figures 7A and 7B may each comprise a honeycomb core layer such as a paper honeycomb core layer, a polyurethane layer, a foamed foam, or an extruded foam; a honeycomb structure made from one or more polymer materials including but not limited to polypropylene, polyethylene, polystyrene, polyamide, copolyamide, polyethylene terephthalate, polyetherimide, polyphenylene oxide, and other polymers; or a honeycomb structure made from one or more metals and metal alloys including but not limited to aluminum, iron, steel, and other metals. In some embodiments, the core layer may be a honeycomb layer having a material other than cellulose. For example, the honeycomb layer may be porous and may contain a considerable amount of open space within the core layer. The core layers shown in Figures 7A and 7B may have a basis weight of about 200 grams / square meter (gsm) to about 4000 gsm. The overall thickness of the core layers shown in Figures 7A and 7B may vary from about 0.5 cm to about 7.5 cm. The depth of the recesses shown in the core layers of Figures 7A and 7B may vary from approximately 0.125 inches (approximately 3 mm) to approximately 1 inch (approximately 2.5 cm), for example, from approximately 5 mm to approximately 1.25 mm, depending on the overall thickness of the core layer. As described herein, different recesses may have different depths and / or geometric shapes.

[0085] In certain examples, the skin layers shown in Figures 7A and 7B may each comprise a porous fiber-reinforced thermoplastic layer. For example, the porous fiber-reinforced thermoplastic layer may be composed of (or used in) a glass mat thermoplastic composite (GMT) or a lightweight reinforced thermoplastic resin (LWRT). One such LWRT is prepared by HANWHA AZDEL and marketed under the trademark SUPERLITE® material. The surface density of such a GMT or LWRT may range from about 300 grams / m² (gsm) to about 4000 gsm, but depending on the needs of the specific application, the surface density may be less than 300 gsm or more than 4000 gsm. In some embodiments, the top density may be less than about 4000 gsm. In certain examples, the GMT or LWRT may comprise one or more lofting agent materials arranged in the voids or pores of the GMT or LWRT. If two or more GMT or LWRT layers are present, the GMT or LWRT layers may be the same or different.

[0086] In specific examples where LWRT is used as a porous fiber-reinforced thermoplastic skin layer, the LWRT typically comprises a thermoplastic material and multiple reinforcing fibers that together form a web of open-cell structure. The web can be formed from a random arrangement of reinforcing fibers held in place by the thermoplastic material. For example, a porous fiber-reinforced thermoplastic layer typically has a considerable amount of open-cell structure so that void spaces exist within the layer. In some examples, the porous fiber skin layers shown in Figures 7A and 7B have concentrations of 0-30%, 10-40%, 20-50%, 30-60%, 40-70%, 50-80%, 60-90%, 0-40%, 0-50%, 0-60%, 0-70%, 0-80%, 0-90%, 10-50%, 10-60%, 10-70%, 10-80%, 10-90%, 10-95%, and 20-60%. Porosity can be %, 20-70%, 20-80%, 20-90%, 20-95%, 30-70%, 30-80%, 30-90%, 30-95%, 40-80%, 40-90%, 40-95%, 50-90%, 50-95%, 60-95%, 70-80%, 70-90%, 70-95%, 80-90%, 80-95%, or any porosity within these exemplary ranges. In some examples, the skin layers shown in Figures 7A and 7B have porosity or void content greater than 0%, for example, up to about 95% that are not fully solidified. Unless otherwise specified, references to skin layers shown in Figures 7A and 7B with specific void content or porosity are based on the total volume of that skin layer, and not necessarily the total volume of the multilayer assembly.

[0087] In certain cases, the skin layers shown in Figures 7A and 7B can be manufactured in the form of GMT or LWRT sheets. In certain cases, the sheets can generally be prepared using chopped glass fibers, thermoplastic materials, optionally lofting agents, and one or more arbitrary thermoplastic polymer films and / or woven or nonwoven fabrics made of glass fibers or thermoplastic resin fibers, such as polypropylene (PP), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polycarbonate (PC), PC / PBT blends, or PC / PET blends. In some embodiments, PP, PBT, PET, PC / PET blends, or PC / PBT blends can be used as resins. To manufacture the sheets, the thermoplastic materials and reinforcing materials can be added to or metered into a dispersed foam contained in an open-top mixing tank fitted with an impeller. While we do not wish to be bound by any particular theory, the presence of air-trapped pockets in the foam can help disperse the glass fibers, thermoplastic materials, and lofting agents. In some examples, a dispersed mixture of fibers and thermoplastic material can be pumped via a distribution manifold to a headbox located above the wire section of a paper machine. The dispersed mixture is then fed to a moving wire screen using vacuum, which removes foam rather than fibers and thermoplastic material, continuously producing a uniform fibrous wet web. The wet web can be passed through a dryer at a temperature suitable for reducing moisture content and melting or softening the thermoplastic material. The resulting product can be pressed or compressed to form a sheet, for example, using a nip roller or other technique, and then bonded to a core layer or another layer.

[0088] In certain embodiments, the high porosity present in the skin layer shown in Figures 7A and 7B can reduce the overall weight of the multilayer assembly and allow for the inclusion of agents within the void spaces of the skin layer. For example, lofting agents can exist non-covalently within the void spaces. The application of heat or other perturbations can act to increase the volume of the non-covalently bonded lofting agents, which increases the overall thickness of the layer, for example, as the size of the lofting agents increases and / or additional air is trapped within the layer. If necessary, flame retardants, colorants, smoke suppressants and other materials may be included in the void spaces of the skin layer shown in Figures 7A and 7B. Before lofting, the multilayer assembly can be compressed to reduce its overall thickness, for example, before or after the layers are bonded to one or more other layers.

[0089] In certain embodiments, the thermoplastic material of the skin layer shown in Figures 7A and 7B may, at least in part, include one or more of polyolefins, or polyethylene, polypropylene, polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, and polyvinyl chloride, both plasticized and nonplasticized, as well as blends of these materials with each other or other polymer materials. Other suitable thermoplastic materials include, but are not limited to, polyarylene ethers, polycarbonates, polyester carbonates, thermoplastic polyesters, polyimides, polyetherimides, polyamides, copolyamides, acrylonitrile-butyl acrylate-styrene polymers, amorphous nylons, polyarylene ether ketones, polyphenylene sulfides, polyarylsulfones, polyethersulfones, liquid crystalline polymers, poly(1,4-phenylene) compounds commercially available as PARMAX®, high-temperature polycarbonates such as Bayer's APEC® PC, high-temperature nylons and silicones, as well as copolymers, alloys and blends of these materials with each other or other polymer materials. The thermoplastic materials used to form the skin layers shown in Figures 7A and 7B can be used in powder form, resin form, rosin form, particle form, fiber form or other suitable form. Various exemplary forms of thermoplastic materials are described herein, for example, in U.S. Patent Application Publication No. 20130244528 and U.S. Patent Application Publication No. 20120065283. The exact amount of thermoplastic material present in the skin layers shown in Figures 7A and 7B may vary, with exemplary amounts ranging from about 20% by weight to about 80% by weight, for example, 30-70% by weight or 35-65% by weight. It will be recognized by those skilled in the art that the total weight percentage of all materials used in either of the skin layers shown in Figures 7A and 7B is added to 100% by weight.

[0090] In certain examples, the reinforcing fibers of the skin layer shown in Figures 7A and 7B may comprise glass fibers, carbon fibers, graphite fibers, synthetic organic fibers, in particular high modulus organic fibers, e.g., para- and meta-aramid fibers, nylon fibers, polyester fibers, resins suitable for use as fibers or with high melt flow index, mineral fibers such as basalt, mineral wool (e.g., rock or slag wool), wollastonite, alumina silica, or mixtures thereof, metal fibers, metallized natural and / or synthetic fibers, ceramic fibers, yarn fibers, or mixtures thereof. In some embodiments, any of the aforementioned fibers may be chemically treated before use to provide desired functional groups or to impart other physical properties to the fibers, for example, by chemical treatment to enable reaction with thermoplastic materials, lofting agents or both. The fiber content in the skin layer shown in Figures 7A and 7B may independently be about 20% to about 90% of the layer's weight, more specifically about 30% to about 70% of the layer's weight. Typically, the fiber content of a multilayer assembly including the skin layer shown in Figures 7A and 7B varies between about 20% and about 90% by weight of the assembly, more specifically between about 30% and about 80% by weight, for example, about 40% and about 70% by weight. The specific size and / or orientation of the fibers used may depend, at least in part, on the thermoplastic polymer material used and / or the desired properties of the skin layer shown in Figures 7A and 7B. Appropriate additional fiber types, fiber sizes and quantities will be readily selected by those skilled in the art, taking into account the interests of this disclosure. In one non-limiting example, the fibers dispersed in the thermoplastic material and optionally in the lofting agent to provide the skin layer shown in Figures 7A and 7B may generally have a diameter greater than about 5 microns, more specifically between about 5 microns and about 22 microns, and a length of about 5 mm to about 200 mm, more specifically, the fiber diameter may be about 2 microns to about 22 microns, and the fiber length may be about 5 mm to about 75 mm.

[0091] In some embodiments, the lofting ability of the skin layers shown in Figures 7A and 7B can be further adjusted by including one or more added lofting agents. The exact type of lofting agent used in the skin layers shown in Figures 7A and 7B may depend on many factors, including, for example, a desired lofting temperature and a desired degree of loft. In some cases, microsphere lofting agents that can increase in size when exposed to convective heating, such as expandable microspheres, can be used. Exemplary commercially available lofting agents are available from Kureha Corporation (Japan). In other examples, a first lofting agent having a first average particle size and a second lofting agent having a second average particle size different from the first average particle size can be used in the skin layers shown in Figures 7A and 7B. In other examples, the lofting agent may be an expandable graphite material that can also impart some flame retardancy to the multilayer assembly.

[0092] In some configurations, the skin layers shown in Figures 7A and 7B may be substantially halogen-free or halogen-free layers to meet the limitations of hazardous substance requirements for a particular application. In other examples, one or more layers may contain halogenated flame retardants, e.g., one or more of F, Cl, Br, I, and At, or compounds containing such halogens, e.g., tetrabromobisphenol-A polycarbonate or monohalo-, dihalo-, trihalo-, or tetrahalopolycarbonate. In some cases, the thermoplastic material used for the skin layers shown in Figures 7A and 7B may contain one or more halogens to impart some degree of flame retardancy without the addition of another flame retardant. Where halogenated flame retardants are present, they are preferably present in amounts that can vary depending on other components present. For example, the halogenated flame retardant may be present in amounts of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically about 1% to about 13% by weight, e.g., about 5% to about 13% by weight. If necessary, two different halogenated flame retardants may be added to the layer. In other examples, non-halogenated flame retardants may be added, such as flame retardants containing one or more of N, P, As, Sb, Bi, S, Se, and Te. In some embodiments, the non-halogenated flame retardants may contain phosphorylated materials, and as a result, the layer may be more environmentally friendly. If non-halogenated or substantially halogen-free flame retardants are present, the flame retardants are preferably present in an amount that can vary depending on other components present. For example, substantially halogen-free flame retardants may be present in an amount of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically, about 1% to about 13% by weight based on the weight of the layer, for example, about 5% to about 13% by weight. If desired, two different substantially halogen-free flame retardants may be added to one or more layers described herein.In certain cases, one or more of the skin layers shown in Figures 7A and 7B described herein may contain one or more halogenated flame retardants in combination with one or more substantially halogen-free flame retardants. If two different flame retardants are present, the combination of the two flame retardants may be present in amounts that can vary depending on other components present. For example, the total weight of the flame retardants present may be about 0.1 weight percent to about 20 weight percent (based on the weight of the layer), more specifically, about 1 weight percent to about 15 weight percent based on the weight of the layer, for example, about 2 weight percent to about 14 weight percent. The flame retardants used in the layers described herein can be added to a mixture containing thermoplastic material and fibers (before discarding the mixture onto a wire screen or other processing component), or they can be added after the layer has been formed. In some examples, the flame retardant material may include one or more of expansive graphite material, magnesium hydroxide (MDH), and aluminum hydroxide (ATH).

[0093] In certain embodiments, the skin layer shown in Figures 7A and 7B may include one or more film layers in combination with the porous fiber-reinforced thermoplastic layer. For example, the film of the skin layer shown in Figures 7A and 7B may include, or be, a thermoplastic film, a polyolefin film, an elastomer film, etc. In certain configurations, the film includes at least one of the following: polyolefin, e.g., polyethylene or polypropylene, at least one poly(etherimide), at least one poly(etherketone), at least one poly(ether-etherketone), at least one poly(phenylene sulfide), poly(arylene sulfone), at least one poly(ethersulfone), at least one poly(amideimide), poly(1,4-phenylene), at least one polycarbonate, at least one nylon, and at least one silicone. In some embodiments, there may be two or more films in combination with the porous fiber-reinforced thermoplastic layer for the skin layer shown in Figures 7A and 7B.

[0094] In certain embodiments, the additional layers shown in Figures 7A and 7B may include films (e.g., thermoplastic films or elastomer films), frims, scrims (e.g., fibrous scrims or scrims containing hydrophilic fibers such as cellulose fibers), foils, woven fabrics, nonwoven fabrics, or exist as inorganic coatings, organic coatings, or thermosetting coatings. In other examples, the additional layers shown in Figures 7A and 7B may contain a limiting oxygen index greater than about 22, as measured according to ISO 4589 1996. When a thermoplastic film is present as (or as part of) the additional layer shown in Figures 7A and 7B, the thermoplastic film may include at least one of poly(etherimide), poly(etherketone), poly(ether-etherketone), poly(phenylene sulfide), poly(arylene sulfone), poly(ethersulfone), poly(amideimide), poly(1,4-phenylene), polycarbonate, nylon, and silicone. If a fibrous scrim is present as an additional layer (or as part thereof) as shown in Figures 7A and 7B, the fibrous scrim may include at least one of glass fibers, aramid fibers, graphite fibers, carbon fibers, inorganic mineral fibers, metal fibers, metallated synthetic fibers, and metallated inorganic fibers. If a thermosetting coating is present as an additional layer (or as part thereof) as shown in Figures 7A and 7B, the coating may include at least one of unsaturated polyurethanes, vinyl esters, phenols, and epoxy. If an inorganic coating is present as an additional layer (or as part thereof) as shown in Figures 7A and 7B, the inorganic coating may include minerals containing cations selected from Ca, Mg, Ba, Si, Zn, Ti, and Al, or it may include at least one of gypsum, calcium carbonate, and mortar. If a nonwoven fabric is present as an additional layer (or as part thereof) as shown in Figures 7A and 7B, the nonwoven fabric may include thermoplastic materials, thermosetting binders, inorganic fibers, metal fibers, metallated inorganic fibers, and metallated synthetic fibers. If necessary, the additional layers shown in Figures 7A and 7B may include expandable graphite material, flame retardant material, fibers, etc.

[0095] In certain embodiments, an additional layer may be present on the second surface of the core layer, as shown in Figures 8A and 8B. Figure 8A shows a multilayer assembly 800 including a core layer 811, skin layers 812 and 814, and an additional layer 813. The recess 815 is present on one surface of the assembly 800, but two, three, four, five or more recesses may be present on one or more surfaces of the multilayer assembly, as required. For example, multiple recesses may be present on surface 817 and / or surface 819. An additional layer may be present on surface 819, as required, although it is not shown.

[0096] In some examples, the additional layer may have sufficient structure to span any recess in the skin layer. For example, referring to Figure 8B, a multilayer assembly 820 is shown comprising a core layer 821, skin layers 822, 824, and an additional layer 823 placed on top of the skin layer 822. A recess 825 is shown that forms a gap between the skin layer 822 and the additional layer 823. For example, a protrusion or other device can be pressed into the skin layer 822 and the core layer 821 to form the recess 825. The layer 823 can then be placed on the assembly so that it overlaps the recess 825. Even when viewing the multilayer assembly 820 outward, the additional layer 823 may be generally planar, so no recess is shown on the surface of the multilayer assembly 820. The presence of the skin layer 822 having a recess into the core layer 821 in combination with the additional layer 823 can enhance the bond between the skin layer 822 and the core layer 821, but still provides a nearly flat or planar surface for the multilayer assembly 820. If necessary, two, three, four, five or more recesses may be present on one or more surfaces of the multilayer assembly. For example, multiple recesses may be present on surface 827 and / or surface 829. Although not shown, additional layers may be present on surface 829 if necessary.

[0097] In certain embodiments, the core layers shown in Figures 8A and 8B may each comprise a honeycomb core layer such as a paper honeycomb core layer, a polyurethane layer, a foamed foam, or an extruded foam; a honeycomb structure made from one or more polymer materials including but not limited to polypropylene, polyethylene, polystyrene, polyamide, copolyamide, polyethylene terephthalate, polyetherimide, polyphenylene oxide, and other polymers; or a honeycomb structure made from one or more metals and metal alloys including but not limited to aluminum, iron, steel, and other metals. In some embodiments, the core layer may be a honeycomb layer having a material other than cellulose. For example, the honeycomb layer may be porous and may contain a considerable amount of open space within the core layer. The core layers shown in Figures 8A and 8B may have a basis weight of about 200 grams / square meter (gsm) to about 4000 gsm. The overall thickness of the core layers shown in Figures 8A and 8B may vary from about 0.5 cm to about 7.5 cm. The depth of the recesses shown in the core layer in Figures 8A and 8B may vary from approximately 0.125 inches (approximately 3 mm) to approximately 1 inch (approximately 2.5 cm), for example, from approximately 5 mm to approximately 1.25 mm, depending on the overall thickness of the core layer. As described herein, different recesses may have different depths and / or geometric shapes.

[0098] In certain examples, the skin layers shown in Figures 8A and 8B may each comprise a porous fiber-reinforced thermoplastic layer. For example, the porous fiber-reinforced thermoplastic layer may be composed of (or used in) a glass mat thermoplastic composite (GMT) or a lightweight reinforced thermoplastic resin (LWRT). One such LWRT is prepared by HANWHA AZDEL and marketed under the trademark SUPERLITE® material. The surface density of such a GMT or LWRT may range from about 300 grams / m² (gsm) to about 4000 gsm, but depending on the needs of the specific application, the surface density may be less than 300 gsm or more than 4000 gsm. In some embodiments, the top density may be less than about 4000 gsm. In certain examples, the GMT or LWRT may comprise one or more lofting agent materials arranged in the voids or pores of the GMT or LWRT. If two or more GMT or LWRT layers are present, the GMT or LWRT layers may be the same or different.

[0099] In specific examples where LWRT is used as a porous fiber-reinforced thermoplastic skin layer, the LWRT typically comprises a thermoplastic material and multiple reinforcing fibers that together form a web of open-cell structure. The web can be formed from a random arrangement of reinforcing fibers held in place by the thermoplastic material. For example, a porous fiber-reinforced thermoplastic layer typically has a considerable amount of open-cell structure so that void spaces exist within the layer. In some examples, the porous fiber skin layers shown in Figures 8A and 8B have concentrations of 0-30%, 10-40%, 20-50%, 30-60%, 40-70%, 50-80%, 60-90%, 0-40%, 0-50%, 0-60%, 0-70%, 0-80%, 0-90%, 10-50%, 10-60%, 10-70%, 10-80%, 10-90%, 10-95%, and 20-60%. Porosity can be %, 20-70%, 20-80%, 20-90%, 20-95%, 30-70%, 30-80%, 30-90%, 30-95%, 40-80%, 40-90%, 40-95%, 50-90%, 50-95%, 60-95%, 70-80%, 70-90%, 70-95%, 80-90%, 80-95%, or any porosity within these exemplary ranges. In some examples, the skin layers shown in Figures 8A and 8B have porosity or void content greater than 0%, for example, up to about 95% that are not fully solidified. Unless otherwise specified, references to skin layers shown in Figures 8A and 8B with specific void content or porosity are based on the total volume of that skin layer, and not necessarily the total volume of the multilayer assembly.

[0100] In certain cases, the skin layers shown in Figures 8A and 8B can be manufactured in the form of GMT or LWRT sheets. In certain cases, the sheets can generally be prepared using chopped glass fibers, thermoplastic materials, optionally lofting agents, and one or more arbitrary thermoplastic polymer films and / or woven or nonwoven fabrics made of glass fibers or thermoplastic resin fibers, such as polypropylene (PP), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polycarbonate (PC), PC / PBT blends, or PC / PET blends. In some embodiments, PP, PBT, PET, PC / PET blends, or PC / PBT blends can be used as resins. To manufacture the sheets, the thermoplastic materials and reinforcing materials can be added to or metered into a dispersed foam contained in an open-top mixing tank fitted with an impeller. While we do not wish to be bound by any particular theory, the presence of air-trapped pockets in the foam can help disperse the glass fibers, thermoplastic materials, and lofting agents. In some examples, a dispersed mixture of fibers and thermoplastic material can be pumped via a distribution manifold to a headbox located above the wire section of a paper machine. The dispersed mixture is then fed to a moving wire screen using vacuum, which removes foam rather than fibers and thermoplastic material, continuously producing a uniform fibrous wet web. The wet web can be passed through a dryer at a temperature suitable for reducing moisture content and melting or softening the thermoplastic material. The resulting product can be pressed or compressed to form a sheet, for example, using a nip roller or other technique, and then bonded to a core layer or another layer.

[0101] In certain embodiments, the high porosity present in the skin layer shown in Figures 8A and 8B can reduce the overall weight of the multilayer assembly and allow for the inclusion of agents within the void spaces of the skin layer. For example, lofting agents can be present in the void spaces non-covalently. The application of heat or other perturbations can act to increase the volume of the non-covalently bonded lofting agents, which increases the overall thickness of the layer, for example, as the size of the lofting agents increases and / or additional air is trapped in the layer. If necessary, flame retardants, colorants, smoke suppressants and other materials may be included in the void spaces of the skin layer shown in Figures 8A and 8B. Before lofting, the multilayer assembly can be compressed to reduce its overall thickness, for example, before or after a layer is bonded to one or more other layers.

[0102] In certain embodiments, the thermoplastic material of the skin layer shown in Figures 8A and 8B may, at least in part, include one or more of polyolefins, or polyethylene, polypropylene, polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, and polyvinyl chloride, both plasticized and nonplasticized, as well as blends of these materials with each other or with other polymer materials. Other suitable thermoplastic materials include, but are not limited to, polyarylene ethers, polycarbonates, polyester carbonates, thermoplastic polyesters, polyimides, polyetherimides, polyamides, copolyamides, acrylonitrile-butyl acrylate-styrene polymers, amorphous nylons, polyarylene ether ketones, polyphenylene sulfides, polyarylsulfones, polyethersulfones, liquid crystalline polymers, poly(1,4-phenylene) compounds commercially available as PARMAX®, high-temperature polycarbonates such as Bayer's APEC® PC, high-temperature nylons and silicones, as well as copolymers, alloys and blends of these materials with each other or other polymer materials. The thermoplastic materials used to form the skin layers shown in Figures 8A and 8B can be used in powder form, resin form, rosin form, particle form, fiber form or other suitable form. Various exemplary forms of thermoplastic materials are described herein, and for example, in U.S. Patent Application Publication No. 20130244528 and U.S. Patent Application Publication No. 20120065283. The exact amount of thermoplastic material present in the skin layers shown in Figures 8A and 8B may vary, with exemplary amounts ranging from about 20% by weight to about 80% by weight, for example, 30-70% by weight or 35-65% by weight. It will be recognized by those skilled in the art that the total weight percentage of all materials used in either of the skin layers shown in Figures 8A and 8B is added to 100% by weight.

[0103] In certain examples, the reinforcing fibers of the skin layer shown in Figures 8A and 8B may comprise glass fibers, carbon fibers, graphite fibers, synthetic organic fibers, in particular high modulus organic fibers, e.g., para- and meta-aramid fibers, nylon fibers, polyester fibers, resins suitable for use as fibers or with high melt flow index, mineral fibers such as basalt, mineral wool (e.g., rock or slag wool), wollastonite, alumina silica, or mixtures thereof, metal fibers, metallized natural and / or synthetic fibers, ceramic fibers, yarn fibers, or mixtures thereof. In some embodiments, any of the aforementioned fibers may be chemically treated before use to provide desired functional groups or to impart other physical properties to the fibers, for example, by chemical treatment to enable reaction with thermoplastic materials, lofting agents or both. The fiber content in the skin layer shown in Figures 8A and 8B may independently be about 20% to about 90% of the layer's weight, more specifically about 30% to about 70% of the layer's weight. Typically, the fiber content of a multilayer assembly including the skin layer shown in Figures 8A and 8B varies between about 20% and about 90% by weight of the assembly, more specifically between about 30% and about 80% by weight, for example, about 40% and about 70% by weight. The specific size and / or orientation of the fibers used may depend, at least in part, on the thermoplastic polymer material used and / or the desired properties of the skin layer shown in Figures 8A and 8B. Appropriate additional fiber types, fiber sizes and quantities will be readily selected by those skilled in the art, taking into account the interests of this disclosure. In one non-limiting example, the fibers dispersed in the thermoplastic material and optionally in the lofting agent to provide the skin layer shown in Figures 8A and 8B may generally have a diameter greater than about 5 microns, more specifically between about 5 microns and about 22 microns, and a length of about 5 mm to about 200 mm, more specifically, the fiber diameter may be about 2 microns to about 22 microns, and the fiber length may be about 5 mm to about 75 mm.

[0104] In some embodiments, the lofting ability of the skin layers shown in Figures 8A and 8B can be further adjusted by including one or more added lofting agents. The exact type of lofting agent used in the skin layers shown in Figures 8A and 8B may depend on many factors, including, for example, a desired lofting temperature and a desired degree of loft. In some cases, microsphere lofting agents that can increase in size when exposed to convective heating, such as expandable microspheres, can be used. Exemplary commercially available lofting agents are available from Kureha Corporation (Japan). In other examples, a first lofting agent having a first average particle size and a second lofting agent having a second average particle size different from the first average particle size can be used in the skin layers shown in Figures 8A and 8B. In other examples, the lofting agent may be an expandable graphite material that can also impart some flame retardancy to the multilayer assembly.

[0105] In some configurations, the skin layers shown in Figures 8A and 8B may be substantially halogen-free or halogen-free layers to meet the limitations of hazardous substance requirements for a particular application. In other examples, one or more layers may contain halogenated flame retardants, e.g., one or more of F, Cl, Br, I, and At, or compounds containing such halogens, e.g., tetrabromobisphenol-A polycarbonate or monohalo-, dihalo-, trihalo-, or tetrahalopolycarbonate. In some cases, the thermoplastic material used for the skin layers shown in Figures 8A and 8B may contain one or more halogens to impart some degree of flame retardancy without the addition of another flame retardant. Where halogenated flame retardants are present, they are preferably present in amounts that can vary depending on other components present. For example, the halogenated flame retardant may be present in amounts of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically about 1% to about 13% by weight, e.g., about 5% to about 13% by weight. If necessary, two different halogenated flame retardants may be added to the layer. In other examples, non-halogenated flame retardants may be added, such as flame retardants containing one or more of N, P, As, Sb, Bi, S, Se, and Te. In some embodiments, the non-halogenated flame retardants may contain phosphorylated materials, and as a result, the layer may be more environmentally friendly. If non-halogenated or substantially halogen-free flame retardants are present, the flame retardants are preferably present in an amount that can vary depending on other components present. For example, substantially halogen-free flame retardants may be present in an amount of about 0.1% to about 15% by weight (based on the weight of the layer), more specifically, about 1% to about 13% by weight based on the weight of the layer, for example, about 5% to about 13% by weight. If desired, two different substantially halogen-free flame retardants may be added to one or more layers described herein.In certain cases, one or more of the skin layers shown in Figures 8A and 8B described herein may contain one or more halogenated flame retardants in combination with one or more substantially halogen-free flame retardants. If two different flame retardants are present, the combination of the two flame retardants may be present in amounts that can vary depending on other components present. For example, the total weight of the flame retardants present may be about 0.1 weight percent to about 20 weight percent (based on the weight of the layer), more specifically, about 1 weight percent to about 15 weight percent based on the weight of the layer, for example, about 2 weight percent to about 14 weight percent. The flame retardants used in the layers described herein can be added to a mixture containing thermoplastic material and fibers (before discarding the mixture onto a wire screen or other processing component) or can be added after the layer has been formed. In some examples, the flame retardant material may include one or more of expansive graphite material, magnesium hydroxide (MDH), and aluminum hydroxide (ATH).

[0106] In certain embodiments, the skin layer shown in Figures 8A and 8B may include one or more film layers in combination with the porous fiber-reinforced thermoplastic layer. For example, the film of the skin layer shown in Figures 8A and 8B may include, or be, a thermoplastic film, a polyolefin film, an elastomer film, etc. In certain configurations, the film includes at least one of the following: polyolefin, e.g., polyethylene or polypropylene, at least one poly(etherimide), at least one poly(etherketone), at least one poly(ether-etherketone), at least one poly(phenylene sulfide), poly(arylene sulfone), at least one poly(ethersulfone), at least one poly(amideimide), poly(1,4-phenylene), at least one polycarbonate, at least one nylon, and at least one silicone. In some embodiments, there may be two or more films in combination with the porous fiber-reinforced thermoplastic layer for the skin layer shown in Figures 8A and 8B.

[0107] In certain embodiments, the additional layers shown in Figures 8A and 8B may include films (e.g., thermoplastic films or elastomer films), frims, scrims (e.g., fibrous scrims or scrims containing hydrophilic fibers such as cellulose fibers), foils, woven fabrics, nonwoven fabrics, or exist as inorganic coatings, organic coatings, or thermosetting coatings. In other examples, the additional layers shown in Figures 8A and 8B may contain a limiting oxygen index greater than about 22, as measured according to ISO 4589 1996. When a thermoplastic film is present as (or as part of) the additional layer shown in Figures 8A and 8B, the thermoplastic film may include at least one of poly(etherimide), poly(etherketone), poly(ether-etherketone), poly(phenylene sulfide), poly(arylene sulfone), poly(ethersulfone), poly(amideimide), poly(1,4-phenylene), polycarbonate, nylon, and silicone. If a fibrous scrim is present as an additional layer (or as part thereof) as shown in Figures 8A and 8B, the fibrous scrim may include at least one of glass fibers, aramid fibers, graphite fibers, carbon fibers, inorganic mineral fibers, metal fibers, metallated synthetic fibers, and metallated inorganic fibers. If a thermosetting coating is present as an additional layer (or as part thereof) as shown in Figures 8A and 8B, the coating may include at least one of unsaturated polyurethanes, vinyl esters, phenols, and epoxys. If an inorganic coating is present as an additional layer (or as part thereof) as shown in Figures 8A and 8B, the inorganic coating may include minerals containing cations selected from Ca, Mg, Ba, Si, Zn, Ti, and Al, or it may include at least one of gypsum, calcium carbonate, and mortar. If a nonwoven fabric is present as an additional layer (or as part thereof) as shown in Figures 8A and 8B, the nonwoven fabric may include thermoplastic materials, thermosetting binders, inorganic fibers, metal fibers, metallated inorganic fibers, and metallated synthetic fibers. If necessary, the additional layers shown in Figures 8A and 8B may include expandable graphite material, flame retardant material, fibers, etc.

[0108] In some examples, one or more intervening layers may be present between the core layer and the skin layer. Referring to Figure 9, an intervening layer 920 is shown between the core layer 910 and the skin layer 930. The intervening layer 920 may be, for example, an adhesive layer, a powder coat layer, a film, or other material. Although not shown, one or more additional layers may also be present on the second surface 904 of the core layer 910. Furthermore, the second surface 904 may optionally have one, two, three, four, five, or more recesses. The core layer 910 and the skin layer 930 may include any of these materials described, for example, with reference to Figures 8A and 8B.

[0109] In certain cases, it may be desirable to preform a skin layer having one or more recesses. Since one or more recesses in the skin layer can mirror recesses in the core layer, the skin layer and core layer can be positioned together. For example, recesses can be formed in the skin layer using injection, pressing, or other equipment, as will be described in more detail below. These recesses can then be bonded to the recesses in the core layer by matching various recesses. By mirroring the recesses in the skin layer and core layer, the skin layer can be bonded to the core layer in a desired orientation. For example, if the skin layer has a specific arrangement of fibers, it may be desirable to orient the fibers either longitudinally or transversely. By creating an asymmetrical or unique arrangement of recesses in the skin layer and core layer, the skin layer and core layer can be bonded to each other in a specific orientation.

[0110] In certain embodiments, the recesses described herein can be generated in many different ways. For example, referring to Figure 10, a spike 1010 on a plate 1000 is shown. The spike 1010 can be pressed into a core layer, a skin layer, or both to form a recess. The exact depth to which the spike is pressed into the layer can vary from about 1 / 8 inch (about 30 mm) to 1 / 2 inch (about 1.25 cm). The depth can be adjusted as needed by pressing the spike 1010 further into the layer or by increasing the length of the spike 1010. The spike 1010 can take many different forms and shapes, and can have sharp or rounded ends, can be solid, can be hollow, can have two or more different protrusions, or can take other forms. The spike 1010 typically contains a material having a higher melting point than the material used for the skin layer. For example, the spike 1010 may include metals, high-temperature polymers, rubber, carbon fiber, diamond, or other materials having melting points above 200°C, above 250°C, or above 300°C. If necessary, the spike 1010 may be coated with materials such as adhesives, powders, dyes, flame retardants, particles, resins, rosin, fibers, or other materials. In some cases, the spike 1010 may include a non-stick coating, such as a fluoropolymer or other material, so that the core layer and skin layer do not adhere to the spike during the manufacturing of the multilayer assembly.

[0111] In certain embodiments, spikes may be present within a plate along with one or more other spikes. For example, referring to Figure 11, a plate 1100 is shown comprising several spikes (collectively 1110) each having an independently adjustable depth. The depths of the spikes 1110 may be the same or different to provide recesses of different depths. Furthermore, the dimensions and shapes of the spikes do not need to be the same. The spikes 1110 may include any of the configurations and materials described in relation to spikes 1010.

[0112] In some examples, a plate with multiple protrusions can be pressed into the surface of a multilayer assembly to create multiple recesses. Referring to Figure 12, a plate 1200 is shown with 19 individual rows, each having 9 protrusions, for a total of 171 individual protrusions. The exact number of protrusions per row may be one, two, three, or more. Similarly, the number of rows present on the plate may be one, two, three, or more. The individual protrusions in each row may be spaced symmetrically or asymmetrically from one another as needed. Furthermore, the shape, size, and / or depth of the different protrusions do not have to be the same. In using plate 1200, a skin layer can be placed on a core layer and heated to soften the skin layer and / or core layer. Then, plate 1200 can be pressed into the softened skin layer to form multiple recesses across the entire surface of the skin layer.

[0113] In certain examples, the protrusions are shown as fixed in Figure 12, but if necessary, one or more of the protrusions can be actuated, for example, by hydraulics, pneumatics, etc., to push them into the skin layer. For example, the plate may be positioned adjacent to the skin layer and remain stationary. One or more individual protrusions can be actuated to push them into the skin layer and / or core layer to form recesses.

[0114] In certain configurations, softened skin layers can be positioned adjacent to multiple air jets to form recesses on the first surface of a multilayer assembly. For example, applying air pressure from air jets, for instance, continuously or intermittently, can act to push the skin layers into the core layers, forming one or more recesses. Different air pressures can be used as needed to form recesses of different depths and / or shapes. Recesses can be formed using ambient air, an inert gas such as nitrogen or helium, or other gases. In some cases, a reactive gas can be used so that fibers and / or thermoplastic materials present in the skin layer can react with materials in the reactive gas.

[0115] In certain examples, the core layers described herein can be manufactured by extruding or expanding a foam, or by joining multiple strips of material and / or by cutting the material to a predetermined thickness and height to produce a honeycomb structure. These strips can be attached (glued / welded) at predetermined intervals, for example. When pulled open, the cells can provide a honeycomb structure. For example, in one example, a paper roll can be used to provide a series of laminated sheets that can be joined together with adhesive in certain areas. The laminated sheets can then be sliced. The slices can be expanded to provide a core having multiple cells or honeycombs. In the case of metal honeycomb structures, they can be manufactured by printing, forging, casting, or other methods.

[0116] In manufacturing the skin layers described herein, it may be desirable to use a wet process and one or more additional materials. For example, a liquid or fluid medium containing dispersed material, such as a thermoplastic material, and one or more types of reinforcing materials, such as fibers, which may optionally contain one or more additives described herein (e.g., flame retardants, lofting agents, etc.), can be agitated or stirred in the presence of a gas, such as air or other gas. The dispersion can then be placed on a moving support, such as a wire screen or other support material, to provide a substantially uniform distribution of the material in the deposited material. To enhance material dispersion and / or uniformity, the agitated dispersion may contain, for example, anionic, cationic, or nonionic activators, such as those sold by Industrial Soaps under the name ACE liquid, those sold by Glover Chemicals as TEXOFOR® FN 15 material, and those sold by Float-Ore as AMINE Fb 19 material. These agents can help disperse air in the liquid dispersion. The components can be added to a mixing tank, flotation cell, or other suitable apparatus in the presence of air to provide a dispersion. While aqueous dispersions are preferably used, one or more non-aqueous fluids may be present to assist dispersion, alter the viscosity of the fluid, or otherwise impart desired physical or chemical properties to the dispersion or prepreg, core, or article.

[0117] In certain cases, after the dispersion has been mixed for a sufficient period of time, the fluid containing the suspended material can be placed on a screen, moving wire, or other suitable support structure to provide a web of the deposited material. Suction or reduced pressure can be applied to the web to remove any liquid from the deposited material, leaving the thermoplastic material and any other materials present, such as fibers, additives, etc. The resulting web can be dried and compacted or pressed to a desired thickness before being fully formed to provide the desired skin layer. Depending on the properties of the thermoplastic and reinforcing materials, a wet process may be used, but it may be preferable to use an airlaid process, a dry blending process, a carding and needleing process, or other known processes used to manufacture nonwoven products.

[0118] In certain embodiments, the skin layers described herein can be manufactured using in-line processes and / or in-line systems. For example, a system for manufacturing a skin layer may include a headbox that can be used to mix materials and deposit a liquid containing thermoplastic material (TP) and reinforcing material (RM) onto a moving support. The moving support can be moved using pulleys or rollers that can be coupled to a motor. A vacuum device may be present to remove the liquid, rather than the TP or RM, from the deposited material on the moving support to form a web. The web can be solidified or dried for at least a certain period of time before being delivered to any set of rollers for compression. A moving belt can receive the dried web from the moving support. The gap between the moving support and the belt can be made small to prevent the dried web from falling.

[0119] In certain cases, the web can then be placed on the core layer and heated to a desired temperature, for example, 170-240 degrees Celsius, to soften it. The exact time used to heat the web can vary from a few seconds to several minutes, depending on the overall thickness of the dry web. A plate, mold, or the like with protrusions can then be pressed onto the heated web on the core layer to form one or more recesses, thereby strengthening the bond of the skin layer to the sidewalls of the core layer, which is formed by pressing the protrusions into the multilayer assembly.

[0120] In certain embodiments, a multilayer assembly can be placed in a mold along with other layers that may be bonded to the multilayer assembly. The mold walls may be provided with projections for creating recesses in the final assembly after molding. When the mold is heated, for example, to 300°C or higher, the assembly can be molded into the desired final article, and at the same time, recesses can be formed to strengthen the bond between the skin layer and the core layer.

[0121] In certain embodiments, an inflatable bladder having protrusions can be used with or without a mold to create recesses on the surface of the assembly described herein. The inflatable bladder may be made of a high-temperature material to soften one or more layers of the assembly, allowing the dimples or recesses to be pressed into the surface of the assembly.

[0122] In certain embodiments, the overall thickness, weight, etc., of the multilayer assembly may vary. In some examples, the thickness of the multilayer assembly may vary. In some examples, such as load-bearing floors for automotive applications, the load-bearing floor may have an effective basis weight such that it deflects less than 4 mm when a load of up to 125 pounds (approximately 57 kg) is placed on the floor. In other examples, the multilayer assembly may have an effective basis weight such that it deflects less than 8 mm when a load of up to 500 pounds (approximately 227 kg) is placed on the floor. Applications with higher weight-bearing requirements may have a higher basis weight as needed.

[0123] In certain embodiments, the multilayer assemblies described herein can be used in vehicles such as automobiles, trucks, trains, airplanes, recreational vehicles such as tow trucks for RVs, Class A RVs, Class B RVs, Class C RVs, truck campers, toy carriers, RV trailers or other recreational vehicles, and in building applications such as siding, ceilings, wall sills, floors, wall panels or other applications.

[0124] In a particular embodiment, a load-bearing floor 1300 is shown in Figure 13A. A side view of a load-bearing floor usable as a vehicle load-bearing floor is shown. The load-bearing floor 1300 is typically located in the rear of a vehicle, for example, in the rear storage of a sports utility vehicle or minivan, and is designed to accommodate components, gear, luggage, spare tires, etc., for storage. A lid or cover (not shown) may be present to enclose the components within the vehicle load-bearing floor 1300 and shield them from view. The load-bearing floor 1300 may comprise a multilayer assembly having one or more recesses, for example, as described herein. In some cases, the load-bearing floor 1300 provides sufficient weight-bearing capacity, for example, about 50 pounds or more (capable of withstanding a force of about 22 kg or more or at least 220 Newtons), thereby eliminating the need for any underlying support members from the vehicle to support it.

[0125] In certain examples, a load-bearing floor may have a layered structure as described herein in relation to Figures 1A to 8B. In some examples, a load-bearing floor may have a layered arrangement as shown in Figure 13B. A load-bearing floor 1350 includes a honeycomb layer 1355. An optional adhesive layer 1360 is present on the first surface of layer 1355. A first fiber-reinforced thermoplastic layer 1365 may be present on the adhesive layer 1360. A skin, decorative layer, or scrim 1370 may be present on layer 1365. Another optional adhesive layer 1375 may be present on the second surface of the honeycomb layer 1355. A second fiber-reinforced thermoplastic layer 1380 may be present on layer 1375. A skin, scrim, or decorative layer 1385 may be present on layer 1380. Recesses (not shown) may be present on or within one or more surfaces as described herein.

[0126] In other embodiments, the multilayer assemblies described herein may reside within a bulkhead wall. For example, a bulkhead wall configured to separate the passenger compartment of a vehicle from the cargo compartment of a vehicle may include one or more of the multilayer assemblies described herein. The bulkhead wall comprises a core layer and a first porous fiber-reinforced thermoplastic layer disposed on a first surface of the core layer, the first porous fiber-reinforced thermoplastic layer being bonded to the surfaces of a plurality of first recesses across the first surface of the core layer. In Figure 14, a bulkhead wall 1410 is shown separating the passenger compartment 1405 from the sleeping area 1420 within a truck driver's cab 1400. Bulkhead walls comprising the multilayer assemblies described herein may also reside in passenger cars, recreational vehicles, trains, subways, ships, airplanes, and the like.

[0127] In certain embodiments, a multilayer assembly may comprise two or more core or honeycomb layers. For example, one, two, three or more honeycomb layers may be present in any single multilayer assembly, as needed. The honeycomb layers may be arranged adjacent to one another or separated by one or more other layers. The honeycomb layers described herein may be manufactured using dimples or recesses before or after bonding to other layers.

[0128] In light of the advantages of this disclosure, it will be recognized by those skilled in the art that structures other than dimples or recesses can be provided in a similar manner. For example, channels, slots, or other structures can also be manufactured using similar methods and materials as described herein.

[0129] When introducing elements of the examples disclosed herein, the articles “a,” “an,” “the,” and “said” are intended to mean that there are one or more elements. The terms “comprising,” “including,” “with,” and “having” are intended to be open-ended, meaning that additional elements other than those enumerated may exist. In light of the merits of this disclosure, it will be recognized by those skilled in the art that various components of the examples can be interchanged or substituted with various components of other examples.

[0130] While specific aspects, examples, and embodiments have been described above, those skilled in the art will recognize that, in consideration of the interests of this disclosure, additions, substitutions, modifications, and changes are possible to the disclosed exemplary aspects, examples, and embodiments.

Claims

1. disposing a first porous fiber reinforced thermoplastic layer on a first surface of the core layer to form a multi-layer assembly, the first porous fiber reinforced thermoplastic layer comprising an open cell web formed by a plurality of reinforcing materials held together by a thermoplastic material; applying a first stimulus to the first surface of the multi-layer assembly to provide a plurality of first recesses in the core layer and across the first surface of the multi-layer assembly, the applied first stimulus forcing the first porous fiber reinforced thermoplastic layer into the plurality of first recesses in the core layer to enhance bonding between the first porous fiber reinforced thermoplastic layer and the core layer; A method comprising:

2. 2. The method of claim 1, comprising applying the first stimulus to the first surface of the multi-layer assembly by placing the multi-layer assembly in a mold comprising a plurality of surface protrusions and molding the multi-layer assembly using the mold.

3. 10. The method of claim 1, comprising applying the first stimulus to the first surface of the multi-layer assembly by pressing a plate having a plurality of surface protrusions against the first surface of the multi-layer assembly.

4. 10. The method of claim 1, comprising applying the first stimulus to the first surface of the multi-layer assembly using a plurality of fluid jets positioned adjacent to the first surface of the multi-layer assembly.

5. The method of claim 1 , wherein the provided plurality of first recesses have different geometric shapes.

6. 2. The method of claim 1, further comprising applying a second stimulus to the second surface of the multi-layer assembly to provide a plurality of second recesses in the core layer and across the second surface of the multi-layer assembly, the applied second stimulus forcing the core layer into the first porous fiber-reinforced thermoplastic layer to strengthen a bond between the first porous fiber-reinforced thermoplastic layer and the core layer.

7. 7. The method of claim 6, comprising the steps of applying the first stimulus to the first surface of the multi-layer assembly by placing the multi-layer assembly in a mold having a plurality of surface protrusions and molding the multi-layer assembly using the mold, and applying the second stimulus to the second surface of the placed multi-layer assembly.

8. 7. The method of claim 6, comprising applying the second stimulus to the second surface of the multi-layer assembly by pressing a plate comprising a plurality of surface protrusions against the second surface of the multi-layer assembly.

9. 7. The method of claim 6, comprising applying the second stimulus to the second surface of the multi-layer assembly using a plurality of fluid jets positioned adjacent to the second surface of the multi-layer assembly.

10. The method of claim 6 , wherein the provided plurality of second recesses have different geometric shapes.

11. The method of claim 1 , wherein the plurality of first recesses have different depths.

12. 10. The method of claim 1, further comprising disposing a first skin layer on the disposed first porous fiber reinforced thermoplastic layer prior to applying the first stimulus.

13. The method of claim 1 , wherein the first porous fiber reinforced thermoplastic layer comprises an adhesive film.

14. The method of claim 1 , comprising disposing a first skin layer over the multi-layer assembly after applying the first stimulus.

15. The method of claim 1 , wherein the core layer comprises a porous core layer and the first porous fiber reinforced thermoplastic layer comprises reinforcing fibers and a polyolefin thermoplastic material.

16. The method of claim 1 , wherein the core layer comprises a honeycomb core layer.

17. 17. The method of claim 16, wherein the reinforcing fibers comprise one or more of glass fibers, aramid fibers, graphite fibers, carbon fibers, inorganic mineral fibers, metal fibers, metallized synthetic fibers, and metallized inorganic fibers, fibers, and combinations thereof.

18. 17. The method of claim 16, wherein the thermoplastic material comprises one or more of polyethylene, polypropylene, polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, polyvinyl chloride, polyarylene ether, polycarbonate, polyester carbonate, thermoplastic polyester, polyimide, polyetherimide, polyamide, acrylonitrile-butyl acrylate-styrene polymer, amorphous nylon, polyarylene ether ketone, polyphenylene sulfide, polyarylsulfone, polyethersulfone, liquid crystal polymer, poly(1,4 phenylene) compound, high heat polycarbonate, high temperature nylon, silicone, or blends of these materials with each other.

19. 17. The method of claim 16, wherein the honeycomb core layer is a paper honeycomb core layer, the reinforcing fibers include glass fibers, and the thermoplastic material includes a polyolefin.

20. disposing a second porous fiber reinforced thermoplastic layer on a second surface of the core layer to form the multi-layer assembly, the second porous fiber reinforced thermoplastic layer comprising an open cell web formed by a plurality of reinforcing materials held together by a thermoplastic material; applying a second stimulus to the second surface of the multi-layer assembly to provide a plurality of second recesses in the core layer and across the second surface of the multi-layer assembly, the applied second stimulus forcing the second porous fiber reinforced thermoplastic layer into the plurality of second recesses in the core layer to enhance bonding between the second porous fiber reinforced thermoplastic layer and the core layer; The method of claim 1 further comprising: