Reinforced cellulose nanofibrils (CNF)
Patent Information
- Application Number
- JP2023527461
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-11-05
- Filing Date
- 2021-11-05
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-11-05
AI Technical Summary
Cellulose materials face challenges in maintaining hydrophobic and oleophobic properties without using environmentally harmful fluorocarbons, which are persistent and costly, and conventional coatings fail to provide uniform resistance to water and grease, especially at creases and folds.
Incorporating reinforced cellulose nanofibrils (CNFs) with a blend of sugar fatty acid esters (SFAEs), glycerides, fatty acid salts, and natural waxes to enhance water and grease resistance, while maintaining biodegradability and recyclability, by using them in the wet-end papermaking process to form a stable aqueous mixture and applying mechanical shear forces.
The method improves drainage rates, prevents agglomeration, and provides uniform hydrophobic and oleophobic properties without the use of fluorocarbons, resulting in cost-effective, biodegradable, and recyclable cellulose-based materials with enhanced water and grease resistance.
Abstract
Description
[Technical Field]
[0001] The present disclosure relates to reinforced cellulose nanofibrils (CNFs) (or reinforced CNF binders), methods of making the reinforced CNF binders, methods of making wet-laid, dry-laid, or molded articles having the reinforced CNF binders by incorporating the reinforced CNFs into a furnish in the wet end of the papermaking process, methods of coating cellulose-based materials, intermediate formed fibrous articles, and / or molded articles with the reinforced CNF binders, and cellulose-based articles obtained by these methods, wherein the reinforced CNFs comprise sugar fatty acid esters, glycerides, fatty acid salts, natural waxes, and / or cellulose crosslinker (SGF) blends bonded to the CNFs. [Background technology]
[0002] Cellulosic materials have a wide range of industrial applications as bulking agents, absorbents, and printing components. Their use is preferred over other material sources due to their high thermal stability, good oxygen barrier properties, and chemical / mechanical resilience (see, e.g., Aulin et al., Cellulose (2010) 17:559-574, incorporated herein by reference in its entirety). Also of great importance are the fact that these materials are completely biodegradable once dispersed in the environment and that they are completely non-toxic. Cellulose and its derivatives are the materials of choice for environmentally friendly solutions in applications such as food and disposable packaging.
[0003] On the other hand, many of the advantages of cellulose are offset by the hydrophilic / oleophilic nature of cellulose materials, which exhibit a high affinity for water / fat and are easily hydrated (see, e.g., Aulin et al., Langmuir (2009) 25(13):7675-7685, incorporated herein by reference in its entirety). While this is beneficial for applications such as absorbents and tissues, it becomes problematic when safe packaging of moisture / lipid-containing materials (e.g., food) is required. Long-term storage of food, especially cooked foods containing large amounts of water and / or fat, is problematic for cellulose trays, for example, because the trays can first become mushy and then eventually fail. Furthermore, due to the high relative porosity of the material, multiple coatings are required to offset the inefficiency of maintaining a sufficient coating on the cellulosic surface, increasing costs.
[0004] Such problems are typically addressed industrially by coating cellulose fibers with certain hydrophobic organic materials / fluorocarbons (e.g., per- and polyfluoroalkyl substances (PFAS)), waxes, synthetic polymers (e.g., polyethylene), or silicones to physically shield the underlying hydrophilic cellulose from the water / lipids in the contents. This includes wicking between the fibers, i.e., preventing grease from flowing into the folds, or allowing the release of attached materials. For example, materials such as PVC / PEI / PE are routinely used for this purpose and are physically attached (i.e., spray-coated or extruded) to the surface to be treated.
[0005] Industrially, compounds based on fluorocarbon chemistry have long been used to produce articles with improved resistance to penetration by oil and grease due to fluorocarbons' ability to reduce the surface energy of articles. One emerging problem with the use of perfluorinated hydrocarbons is that they are highly persistent in the environment. The EPA and FDA have recently begun reviewing the sources, environmental fate, and toxicity of these compounds. A recent study reported a very high occurrence (over 90%) of perfluorooctanesulfonate in blood samples taken from schoolchildren. The cost and potential environmental liability of these compounds have led manufacturers to seek alternative means of producing articles that are resistant to penetration by oil and grease.
[0006] Although lowering surface energy improves an article's penetration resistance, lowering surface energy also has several drawbacks. For example, textile fabrics treated with fluorocarbons exhibit good stain resistance, but once soiled, the ability of cleaning compositions to penetrate and release the stain from the fabric can be affected, potentially resulting in reduced service life and permanently soiled fabrics. Another example is grease-resistant paper that is subsequently printed and / or coated with an adhesive. In this case, the necessary grease resistance is achieved by treating with fluorocarbons, but the low surface energy of the paper can cause problems related to the acceptance of printing inks or adhesives, including scuffing, backtrap mottling, poor adhesion, and registration. If the grease-resistant paper is to be used as a pressure-sensitive label with adhesive coated on one side, low surface energy can reduce adhesive strength. To improve their printability, coatability, or adhesion, low surface energy articles can be treated with post-formation processes such as corona discharge, chemical treatment, and flame treatment. However, these processes increase the manufacturing cost of the article and have other drawbacks.
[0007] It would be desirable to design a "green" bio-based coating that is hydrophobic, oleophobic, and compostable, including base paper / film, that could maintain the coating on the surface of the paper and prevent wicking into the interstices of the fibers or reduce the adhesion of materials to cellulosic surfaces, at a reduced cost, without sacrificing biodegradability and / or recyclability.
[0008] Another problem is that conventional coatings for imparting hydrophobic and / or oleophobic barrier properties, including the fluorocarbon and petrochemical coatings referred to herein, tend to perform poorly in the folds, creases, and the like of the articles to which the materials are coated. Specifically, these articles typically have poor water and / or grease resistance in these areas. This "grease creasing effect" can be defined as the sorption of grease in a paper structure caused by folding, pressing, or crushing the paper structure. A conventional solution to the grease creasing effect is to add latex, polyvinyl alcohol, or similar resins to the coating to achieve improved coating coverage in these areas. However, with such conventional solutions, the water and / or oil and grease resistance in these areas may still be poorer than in flat areas of the article, the addition of resin components increases costs, and the materials are not completely biobased because latex and polyvinyl alcohol are synthetic and / or not easily recyclable.
[0009] U.S. Patent Application Publication No. 2018 / 0066073 (hereinafter the "'073 Publication"), which is incorporated herein by reference in its entirety, discloses a tunable method for treating cellulosic materials with compositions that provide increased water resistance and / or barrier properties, such as oil and grease resistance (OGR), without sacrificing their biodegradability. In particular, the '073 application discloses methods for attaching sugar fatty acid esters ("SFAEs") onto cellulosic materials to provide treated materials that exhibit increased water resistance, lipid resistance, barrier function, and other mechanical properties.
[0010] U.S. Provisional Patent Application Publication No. 63 / 022,097, filed May 8, 2020 (hereinafter the "'097 Application"), which is incorporated herein by reference in its entirety, discloses a tunable method of treating cellulosic materials with compositions that provide increased barrier properties, such as water resistance and / or OGR resistance, without sacrificing their biodegradability. In particular, the '097 Application discloses a method of incorporating a blend of glycerides and / or fatty acid salts. The '097 Application discloses that barrier formulations including a blend of glycerides and / or fatty acid salts can further include an SFAE to impart water resistance and / or OGR resistance and / or to provide emulsifier functionality.
[0011] PCT / US2020 / 014923 (hereinafter, the "'923 Application"), the entire contents of which are incorporated herein by reference, discloses a method for treating fibrous cellulosic materials with sucrose fatty acid ester-containing particles (carrier systems) that enables surface modification, including producing such surface water resistance and / or oil / grease resistance. The disclosed method provides for combining at least one SFAE with a polymer (e.g., latex) to form micellar particles, and applying such particles to a substrate comprising a fibrous cellulose-based material (e.g., pulp) to form, among other things, a molded product. Also disclosed are compositions comprising a combination of an SFAE, latex, and optionally a mineral or other additive.
[0012] U.S. 16 / 568,953 (hereinafter the "'953 Application"), the entire contents of which are incorporated herein by reference, discloses a tunable method for treating cellulosic materials with a barrier coating comprising a prolamine and at least one polyol fatty acid ester that provides increased oil and / or grease resistance to such materials without sacrificing their biodegradability. The disclosed method provides for adhesion of the barrier coating to articles, including articles comprising cellulosic materials and articles made by such methods. Materials so treated exhibit increased oleophobicity and can be used in any application where such characteristics are desired.
[0013] U.S. 16 / 456,499 (hereinafter the "'499 Application"), the entire contents of which are incorporated herein by reference, discloses a tunable method for treating cellulosic materials with a barrier coating comprising at least two polyols and / or sugar fatty acid esters that provides increased water, oil, and grease resistance to such materials without sacrificing their biodegradability. The disclosed method provides for adhesion of the barrier coating to articles, including articles comprising cellulosic materials and articles made by such methods. Materials so treated exhibit increased hydrophobicity and oleophobicity and can be used in any application where such characteristics are desirable.
[0014] U.S. 16 / 456,433 (hereinafter the "'433 Application"), the entire contents of which are incorporated herein by reference, discloses a method for treating cellulosic materials with a composition that allows for increased retention of inorganic particles on the cellulosic substrate. The disclosed method provides for combining an SFAE with such inorganic particles and applying such a combination to the cellulosic material to eliminate or reduce the use of retention aids or binders for fillers in the papermaking process. Compositions including such combinations of SFAE and inorganic particles are also disclosed.
[0015] The use of binders obtained from natural sources is also becoming increasingly important in order to provide "green" bio-based products.
[0016] Nanocellulose is a term that refers to nanostructured cellulose, which can be cellulose nanocrystals (CNC or NCC), cellulose nanofibrils (CNF) (also referred to in the art as cellulose nanofibers and nanofibrillated cellulose), or bacterial nanocellulose.
[0017] CNFs are materials composed of nano-sized cellulose fibrils that typically have a high aspect ratio (length to width). CNFs are typically obtained from wood pulp or another natural cellulose fiber source by a process that typically involves subjecting the pulp / fibers to mechanical shear forces.
[0018] CNFs have been used as binders in papermaking processes. The inventors have determined that the use of CNFs as additives in wet-end and coating applications can result in improved OGR. However, the use of CNFs presents certain problems. One problem is that when CNFs are used as a wet-end additive to papermaking furnishes, they tend to slow the drainage rate (or dewatering) of the fiber mat from the slurry. This is a disadvantage because, for example, the rate of water removal affects the production rate of cellulose-based products. Another problem is that CNFs tend to agglomerate when used as an additive in a slurry or spray, which can adversely affect their efficiency and / or their functional properties.
[0019] Thus, there remains a need for "green" bio-based coatings for cellulose-based materials that provide improved water and / or OGR resistance, as well as "green" cellulose-based molded articles with improved water and / or OGR resistance. Summary of the Invention
[0020] While the present disclosure provides methods that address one or more of the limitations and / or concerns in the prior art discussed above and / or provide one or more improvements thereon, the present disclosure does not necessarily address every one of the limitations and / or concerns.
[0021] In one embodiment, the present disclosure is directed to a reinforced cellulose nanofibril binder comprising cellulose nanofibrils (CNFs) and an SGF blend bound to the CNFs, wherein the SGF blend comprises one or more selected from the group consisting of sugar fatty acid esters (SFAEs), glycerides, fatty acid salts ("FAS"), natural waxes, and cellulose crosslinkers.
[0022] As used herein, "SGF blend" refers to one or more sugar fatty acid esters (SFAEs), and / or one or more glycerides, and / or one or more fatty acid salts (FASs), and / or one or more natural waxes, and / or one or more cellulose cross-linking agents. In some embodiments, the SGF blend used in this disclosure does not contain SFAEs, in some embodiments, the SGF blend does not contain glycerides, in some embodiments, the SGF blend does not contain FASs, in some embodiments, the SGF blend does not contain natural waxes, and in some embodiments, the SGF blend does not contain cellulose cross-linking agents. In some embodiments, the SGF blend consists essentially of SFAEs, glycerides, and / or FASs. In some embodiments, the SGF blend consists of SFAEs, glycerides, and / or FASs.
[0023] The reinforced cellulose nanofibril binders (or reinforced CNFs) according to the present disclosure can provide certain benefits. For example, when used in the wet end of the papermaking process, the reinforced CNFs maintain or increase the drainage rate of the fiber mat from the slurry. Also, the reinforced CNFs do not have the same agglomeration problems as conventional CNFs.
[0024] In one embodiment of the present disclosure, the reinforced cellulose nanofibril binder consists essentially of a CNF and SGF blend.
[0025] In another embodiment of the reinforced cellulose nanofibril binder, the weight ratio of CNF to SGF blend is from about 1:99 to about 99:1, or from about 5:95 to about 95:5, or from about 10:90 to about 90:10, or from about 15:85 to about 85:15, or from about 20:80 to about 80:20, or from about 25:75 to about 75:25, or from about 30:70 to about 70:30, or from about 35:65 to about 65:35, or from about 40:60 to about 60:40, or from about 45:55 to about 55:45, or about 50:50.
[0026] In one embodiment, the reinforced cellulose nanofibril binder is obtained by a method including the steps of obtaining an aqueous mixture of cellulose nanofibrils (CNFs), obtaining an aqueous SGF blend, and mixing the aqueous CNF mixture with the aqueous SGF blend to obtain a CNF / SGF mixture. Mixing the CNFs with the SGF blend (thereby contacting the CNFs with the SGF blend) may be sufficient to bond the SGF blend to the CNFs. Alternatively, the SGF blend can be bonded to the CNFs by exposing the CNF / SGF mixture to heat, radiation, a catalyst, or a combination thereof for a sufficient period of time. The method may further include reducing the moisture content of the CNF / SGF mixture, for example, by draining the water.
[0027] In one embodiment, the reinforced cellulose nanofibril binder according to the present disclosure is obtained by a method comprising the steps of obtaining an aqueous mixture of cellulose pulp (wood pulp), obtaining an aqueous SGF blend, mixing the aqueous mixture of cellulose pulp with the aqueous SGF blend to obtain a cellulose / SGF mixture, and subjecting the cellulose / SGF mixture to mechanical shear forces to obtain the reinforced cellulose nanofibril binder.
[0028] In one aspect, the method for obtaining reinforced CNF may further include a step of reducing the water content of the cellulose / SGF mixture, such as by draining the water.
[0029] In one aspect, the method for obtaining reinforced CNFs may further include a step of subjecting the cellulose pulp to a pretreatment before obtaining the cellulose / SGF mixture and / or before subjecting the cellulose / SGF mixture to mechanical shear forces.
[0030] In one embodiment, the pretreatment may include lowering the pH of the aqueous mixture of cellulose pulp by adding an acid.
[0031] In one embodiment, the present disclosure provides a barrier formulation comprising reinforced CNFs according to the present disclosure. The composition of the barrier formulation can be selected to controllably derivatize the cellulose-based material by methods known in the art, such as the '073 publication or the '097 application.
[0032] In one embodiment, the present disclosure provides a method of making a cellulose-based article, the method comprising adding a reinforced cellulose nanofibril binder according to the present disclosure to an aqueous papermaking furnish and draining water from the furnish to obtain a fibrous web.
[0033] In one aspect, such a method further comprises forming the fibrous web into a shaped article having a three-dimensional shape.
[0034] In one embodiment, there is provided a method for imparting barrier properties to a cellulose-based material, the method comprising the steps of contacting the cellulose-based material with an aqueous barrier formulation to impart barrier properties, the barrier formulation comprising a reinforced cellulose nanofibril binder according to the present disclosure, and binding the barrier formulation to a surface of the cellulose-based material to obtain a bound cellulose-based material having barrier properties, wherein the barrier properties are one or more selected from the group consisting of water resistance, lipid resistance, and gas resistance.
[0035] In one embodiment, a barrier formulation is provided comprising a reinforced cellulose nanofibril binder according to the present disclosure, a second SGF blend comprising one or more sugar fatty acid esters (SFAEs), one or more glycerides, and / or one or more fatty acid salts, and water.
[0036] In one embodiment, the second SGF blend of the barrier formulation can be selected to controllably derivatize the cellulose-based material by methods known in the art, such as the '073 publication or the '097 application.
[0037] In one aspect, the barrier formulations of the present disclosure may include pigments traditionally used in the paper industry.
[0038] In one embodiment, a method for imparting barrier properties to a cellulose-based material comprises the steps of contacting the cellulose-based material with a barrier formulation to impart the barrier properties, the barrier formulation comprising a (a) cellulose nanofibril (CNF) and (b) SGF blend, and binding the barrier formulation to a surface of the cellulose-based material to obtain a bound cellulose-based material having barrier properties, wherein the barrier properties are one or more selected from the group consisting of water resistance, lipid resistance, and gas resistance.
[0039] The method for imparting barrier properties according to the present disclosure may provide similar benefits mentioned above, including maintaining or increasing drainage rates and preventing agglomeration of CNFs when the method is applied to wet-end processes.
[0040] In one embodiment, when the total weight of the barrier formulation used in the method for imparting barrier properties according to the present disclosure is considered as 100 wt%, the barrier formulation comprises from about 4 wt% to about 96 wt% CNF and from about 4 wt% to about 96 wt% SGF blend.
[0041] In one aspect, the cellulose-based material used in the method for imparting barrier properties according to the present disclosure comprises cellulose fibers, and the contacting step comprises forming an aqueous mixture of the barrier formulation and the cellulose fibers.
[0042] In one embodiment, the SGF blend can be present in the aqueous mixture or dispersion at a total concentration of at least 0.025% (wt / wt) of the total cellulosic fiber present in the aqueous mixture.
[0043] In one embodiment, the aqueous mixture includes one or more pigments conventionally used in the paper industry.
[0044] In one embodiment, the aqueous mixture is in the form of a slurry having a solids content of about 0.1-10.0 wt. %, 0.1-6.0 wt. %, or about 0.1-2.0 wt. %, or about 0.2-1.5 wt. %.
[0045] In one aspect, such a method further comprises reducing the water content of the aqueous mixture, such as by draining the water.
[0046] In another aspect, the contacting step in the method for imparting barrier properties according to the present disclosure comprises coating the surface of the cellulose-based substrate with the formulation by dipping, spraying, painting, printing, or any optional combination of any of these processes.
[0047] In one embodiment, the SGF blend is applied to the surface of the substrate in an amount of at least about 0.05 g / m 2 is present in a weight amount of
[0048] The cellulose-based substrate is not particularly limited. In one embodiment, examples of the cellulose-based substrate include paper, paperboard, bacon board, insulating materials, paper pulp, food storage cartons, compost bags, food storage bags, release paper, shipping bags, weed blocking / barrier fabric or film, mulching film, flower pots, packing beads, bubble wrap, oil absorbing materials, laminates, envelopes, gift cards, credit cards, gloves, raincoats, OGR paper, shopping bags, diapers, membranes, tableware, tea bags, coffee or tea containers, containers for holding hot or cold beverages, cups, plates, carbonated beverages, and the like. Included are surfaces of articles selected from bottles for storing liquids, bottles for storing non-carbonated liquids, lids, food packaging films, garbage disposal containers, food handling equipment, fabric fibers, water storage and transport equipment, storage and transport equipment for alcoholic or non-alcoholic beverages, outer casings or screens for electronic products, interior or exterior parts of furniture, curtains, upholstery, fabrics, films, boxes, sheets, trays, pipes, water conduits, clothing, medical devices, pharmaceutical packaging, contraceptives, camping equipment, molded cellulosic materials, and combinations thereof.
[0049] In one aspect, the method for imparting barrier properties according to the present disclosure provides a bound cellulose-based material that exhibits a water contact angle of 90° or greater.
[0050] In one aspect, the method for imparting barrier properties according to the present disclosure provides a bound cellulose-based material that exhibits a TAPPI T 559 KIT test value of 3-12.
[0051] In one aspect, the method for imparting barrier properties according to the present disclosure provides a bound cellulose-based material that exhibits a water contact angle of 90° or greater and / or a TAPPI T 559 KIT test value of 3-12 in the absence of a secondary hydrophobe.
[0052] In one embodiment, a method for making a reinforced cellulose nanofibril binder is provided, the method comprising the steps of obtaining an aqueous mixture of cellulose nanofibrils (CNFs), obtaining an aqueous SGF blend, and mixing the aqueous mixture of CNFs with the aqueous SGF blend to obtain a CNF / SGF mixture, and bonding the SGF blend to the CNFs.
[0053] In one embodiment, the method of making reinforced CNF further comprises reducing the moisture content of the CNF / SGF mixture.
[0054] In one embodiment, a method of making a reinforced cellulose nanofibril binder is provided, the method comprising the steps of obtaining an aqueous mixture of cellulose pulp, obtaining an aqueous SGF blend, mixing the aqueous mixture of cellulose pulp with the aqueous SGF blend to obtain a cellulose / SGF mixture, and subjecting the cellulose / SGF mixture to mechanical shear forces to obtain the reinforced cellulose nanofibril binder.
[0055] In one aspect, such a method comprises subjecting the cellulose pulp to a pretreatment prior to obtaining the cellulose / SGF mixture and / or prior to subjecting the cellulose / SGF mixture to mechanical shear forces.
[0056] In one embodiment, a method of making a shaped article is disclosed, comprising the steps of providing a forming tool having a three-dimensional shape with a forming portion; contacting the forming portion with a cellulose composition such that the forming portion is covered with a wet layer of pulp; and dewatering the layer of pulp on the forming tool to obtain the shaped article, wherein the cellulose composition comprises cellulose pulp and a reinforced cellulose nanofibril binder according to the present disclosure.
[0057] In one embodiment, another method of making a shaped article is disclosed, comprising the steps of providing a forming tool having a three-dimensional shape with a forming portion; contacting the forming portion with a cellulose composition such that the forming portion is covered with a wet layer of pulp; and dewatering the layer of pulp on the forming tool to obtain the shaped article, wherein the cellulose composition comprises cellulose pulp and a barrier formulation according to the present disclosure.
[0058] In one embodiment, another method of making a molded article is disclosed, the method including the steps of providing a forming tool having a three-dimensional shape with a forming portion; contacting the forming portion with a cellulose composition such that the forming portion is covered with a wet layer of pulp; dewatering the layer of pulp on the forming tool to obtain an intermediate molded article; and coating a surface of the intermediate molded article with a barrier formulation according to the present disclosure by dipping, spraying, painting, printing, or any optional combination of these processes to obtain the molded article.
[0059] In one embodiment, the method of making the molded article includes dehydrating at a temperature above 100° C. to achieve a dry content of at least about 70% by weight, preferably at least about 80% by weight.
[0060] In one embodiment, the layer of pulp present on the forming tool is dewatered by press drying carried out at a temperature above 100°C, preferably at a temperature of about 120-250°C, or more preferably at a temperature of about 150-220°C.
[0061] In one embodiment, the cellulosic composition for the method of making a molded article comprises a fiber mixture consisting essentially of chemi-thermomechanical pulp (CTMP), thermo-mechanical pulp (TMP), chemical pulp, or semi-chemical pulp, or a combination thereof. The pulp may be bleached or unbleached.
[0062] In one aspect, the forming tool is porous or perforated so that water can be removed during forming during the dewatering / drying step.
[0063] In one embodiment, the method of making the molded article further comprises coating the surface of the molded article with a barrier formulation comprising the SGF blend by dipping, spraying, painting, printing, or any optional combination of these processes.
[0064] In one embodiment, the coating of the surface of the molded article with the barrier formulation is carried out while the molded article is an intermediate molded article having a relatively high moisture content and a fiber content of about 20-50% by weight, preferably about 30-40% by weight.
[0065] In one embodiment, the present disclosure provides a cellulose-based product obtained by any of the methods described herein, wherein the cellulose-based product is a three-dimensional molded product, such as a molded food packaging product, made from cellulose fibers.
[0066] In one embodiment, the three-dimensional shape obtained by the method for producing the molded article is not particularly limited.
[0067] In one aspect, the three-dimensional shape is, for example, the shape of a bowl, cup, plate, fork, spoon, or knife.
[0068] In some embodiments, the barrier formulation consists essentially of a CNF and SGF blend.
[0069] In some embodiments, the weight ratio of CNF to SGF blend in the barrier formulation is from about 20:1 to about 1:5. In some embodiments, the weight ratio can be from about 5:1 to about 1:5.
[0070] In some embodiments, when the total weight of the barrier formulation is considered to be 100% by weight, the barrier formulation comprises about 4% to about 96% by weight of CNF and about 4% to about 96% by weight of the SGF blend. In some embodiments, the amount of CNF can be about 10% to about 70% by weight. In some embodiments, the amount of SGF blend can be about 30% to about 90% by weight.
[0071] In some embodiments, the barrier formulation further comprises one or more prolamines.
[0072] In some embodiments, the one or more prolamines are selected from wheat (gliadin), barley (hordein), rye (secalin), corn (zein), sorghum (kafirin), and / or oat (avenin).
[0073] In some embodiments, the cellulose-based material comprises cellulose fibers suitable for papermaking, and the aqueous mixture or dispersion is a papermaking furnish or raw material.
[0074] In some embodiments, the molded article exhibits a water contact angle of 90° or greater, 100° or greater, 110° or greater, or 120° or greater.
[0075] In some embodiments, the molded article exhibits a TAPPI T 559 KIT test value of 3-12.
[0076] In some embodiments, the molded article exhibits reduced permeability to gases (also referred to as "gas resistance") (e.g., resistance to oxygen, nitrogen, and carbon dioxide). In some aspects, the gas resistance is reduced permeability to oxygen.
[0077] In some embodiments, the molded article exhibits a water contact angle of 90° or greater and / or a TAPPI T 559 KIT test value of 3-12 in the absence of a secondary hydrophobe.
[0078] In some embodiments, the barrier formulation is in the form of an emulsion.
[0079] In some embodiments, the barrier formulation is a stable aqueous composition.
[0080] In another embodiment, a method of making a cellulose-based product with barrier properties is provided, the method comprising the steps of obtaining a furnish comprising an aqueous mixture of cellulose fibers, adding an SGF blend to the furnish, adding CNF to the furnish, and adding a retention aid to the furnish to aid in retention of the SGF blend on the cellulose fibers.
[0081] In some embodiments, one or more charged polymers can be added to the wet end to aid in the retention of the SFAE on the cellulose-based material. The one or more charged polymers can include one or more cationic polymers, anionic polymers, nonionic polymers, and / or zwitterionic polymers. In some embodiments, the charged polymer includes a combination of a relatively low molecular weight cationic polymer and a relatively high molecular weight anionic polymer.
[0082] In some embodiments, the charged polymer comprises one or more cationic polymers. The one or more cationic polymers may include polyacrylamide. The polyacrylamide may include polyDADMAC (polydiallyldimethylammonium chloride) or alum (aluminum sulfate).
[0083] In some embodiments, one or more prolamines can be added to the wet end to aid in the retention of the SGF blend, CNFs, and / or reinforced CNFs on the cellulose-based material. DETAILED DESCRIPTION OF THE INVENTION
[0084] Before the present compositions, methods, and methodologies are described in more detail, it is to be understood that this disclosure is not limited to the particular compositions, methods, and experimental conditions described, as these may vary. It is also to be understood that the scope of the present invention will be limited only by the appended claims, and that the terminology used herein is for the purpose of describing particular embodiments only, and is not intended to be limiting.
[0085] As used herein and in the appended claims, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Thus, for example, reference to "sugar fatty acid esters" includes one or more sugar fatty acid esters and / or compositions of the type described herein that will become apparent to one of ordinary skill in the art, such as by reading this disclosure.
[0086] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. Any methods and materials similar or equivalent to those described herein can be used in the practice or testing of this disclosure, since modifications and variations are understood to be encompassed within the spirit and scope of the disclosure.
[0087] The present disclosure provides a reinforced cellulose nanofibril binder.
[0088] Cellulose nanofibrils (also referred to herein as CNFs) and methods for their production are well known in the art.
[0089] CNFs for use in embodiments of the present disclosure are not particularly limited. CNFs can be commercially obtained or can be made by known methods that typically involve subjecting a cellulose fiber source (e.g., wood pulp) to mechanical shear forces.
[0090] The properties of the CNF are not particularly limited. The CNF may have a typical fibril width of about 5 to 20 nanometers and a length of several micrometers.
[0091] In some embodiments, the reinforced CNFs are obtained by contacting conventionally produced CNFs with an SGF blend and bonding the SGF blend to the CNFs. In another embodiment, the reinforced CNFs are obtained by subjecting a cellulose fiber source (e.g., wood pulp) to mechanical shear stress while the CNFs are mixed with the SGF blend.
[0092] As discussed above, the reinforced CNFs provide benefits compared to traditionally used CNFs, such as maintaining or increasing the drainage rate of the fiber mat from the slurry and reducing agglomeration of the CNFs.
[0093] The present disclosure provides methods for imparting barrier properties to cellulose-based materials. These methods include contacting the cellulose-based material with a barrier formulation to impart the barrier properties, and bonding the barrier formulation to the surface of the cellulose-based material to obtain a bound cellulose-based material having barrier properties, the barrier properties being one or more selected from the group consisting of water resistance, gas resistance, and lipid resistance. The barrier formulation may include reinforced CNF, or the barrier formulation may include a blend of reinforced CNF and SGF.
[0094] The methods of the present disclosure can provide a solvent-free, bio-based, high-temperature resistant barrier (or barrier coating) against oil and grease (OGR), water, and / or gases (e.g., oxygen, nitrogen, and carbon dioxide), and / or formed fibrous (e.g., molded) products having these properties.
[0095] Another aspect of the present disclosure is that barrier coatings can be configured to provide improved water and lipid (oil / grease) resistance without the use of PFAS. These barrier properties can be provided by SGF blends (see, e.g., the '073 publication, the '953 publication, the '923 application, the '499 application, the '433 application, and the '097 application, all of which are incorporated herein by reference).
[0096] In some embodiments, the reinforced CNFs can be used in the wet end of the papermaking process by adding them directly to the papermaking furnish. Alternatively, in another embodiment, a combination of CNFs and SGF blends can be added directly to the papermaking furnish to achieve similar benefits.
[0097] One or more charged polymers, such as polyDADMAC or polyacrylamide, can also be added to the furnish as retention aids to promote absorption of the SGF blend and / or CNF onto the cellulose surface. In some embodiments, charged polymers can be used to control the static charge of formulations containing SGF blends.
[0098] In another embodiment, prolamines can be used as binders, as described, for example, in U.S. Provisional Application No. 63 / 044,820, filed June 26, 2020 (hereinafter, the "'820 Application"), which is incorporated herein by reference in its entirety.
[0099] Prolamins can be used not only as binders for SGF blends and / or CNFs, but also as binders for conventional pigments added to papermaking furnishes. Pigments are typically relatively small and electrically charged on their surfaces, including their edges. Therefore, pigments can be easily trapped (and thereby selectively retained) within the prolamin matrix.
[0100] In addition to being added directly to the papermaking furnish, the barrier formulation can be coated onto a cellulose-based material or substrate (e.g., an already formed paper product) by dipping, spraying, painting, printing, extrusion coating, metering, or any combination of any of these processes. The barrier formulation may contain a sufficient amount of reinforced CNF to impart the desired water resistance and / or OGR to the cellulose-based material.
[0101] Alternatively, the barrier formulation may contain a CNF and SGF blend in an amount suitable to impart the desired water resistance and / or OGR to the cellulose-based material.
[0102] Alternatively, the barrier formulation may contain a reinforced CNF and SGF blend in an amount suitable to impart the desired water resistance and / or OGR to the cellulose-based material.
[0103] In this disclosure, the interaction between the SGF blend and the CNF can be ionic, hydrophobic, van der Waals interactions, covalent bonds, or a combination thereof. As used herein, "binding," including grammatical variations thereof, means to aggregate or cause aggregation into essentially a single mass and can refer to ionic, hydrophobic, van der Waals interactions, or covalent bonds, or a combination thereof.
[0104] In the present disclosure, the interaction between the SGF blend and the cellulose-based material can be through ionic, hydrophobic, van der Waals interactions, covalent bonds, or a combination thereof.
[0105] In the present disclosure, the interaction between the reinforced CNF and the cellulose-based material can be through ionic, hydrophobic, van der Waals interactions, covalent bonds, or a combination thereof.
[0106] In some embodiments, the barrier formulation may also contain one or more traditional binders used in papermaking, such as latex, PvOH, and starch.
[0107] As used herein, "cellulosic" refers to a natural, synthetic, or semi-synthetic material that can be molded or extruded into objects (e.g., bags, sheets) or films or filaments that can be used to make such objects or films or filaments that are structurally and functionally similar to cellulose, e.g., coatings and adhesives (e.g., carboxymethyl cellulose). As another example, the complex carbohydrate (CH) composed of glucose units that forms the major component of the cell walls of most plants. 10 O5) n The cellulose is cellulosic.
[0108] The cellulosic materials (or cellulose-based materials) described herein can be, for example, cellulose fibers conventionally used in the paper industry, microfibrillated cellulose (MFC), nanofibrillated cellulose (or CNF), or cellulose nanocrystals.
[0109] As used herein, "coating weight" is the weight of material (wet or dry) to be applied to a substrate. It is expressed in pounds per specified ream or grams per square meter.
[0110] As used herein, "effect," including grammatical variations thereof, means imparting a particular property to a particular material.
[0111] As used herein, "hydrophobic material" refers to a material that does not attract water. For example, waxes, rosins, resins, sugar fatty acid esters, fatty acid salts, glycerides, diglycerides and triglycerides with long fatty acid chains, diketene, shellac, vinyl acetate, PLA, PEI, oils, fats, lipids, other water-repellent chemicals, or combinations thereof are hydrophobic materials.
[0112] As used herein, "hydrophobic" refers to the property of being water repellent and tending to repel and not absorb water.
[0113] As used herein, "lipid resistance" or "oleophobicity" refers to the property of being lipid repellent and tending to repel and not absorb lipids, grease, fats, etc. In related embodiments, grease resistance can be measured by the "3M KIT" test, the TAPPI T559 Kit test, or the Cobb Oil Test.
[0114] As used herein, "cellulose-containing material" or "cellulose-based material" refers to a composition consisting essentially of cellulose. For example, such materials may include, but are not limited to, paper, paper sheets, paperboard, paper pulp, food storage cartons, parchment paper, cake board, butcher paper, release paper / liner for pressure-sensitive adhesives, food storage bags, shopping bags, shipping bags, bacon boards, insulating materials, tea bags, coffee or tea containers, compost bags, tableware, containers for holding hot or cold beverages, cups, lids, plates, bottles for storing carbonated liquids, gift cards, bottles for storing non-carbonated liquids, food packaging films, garbage disposal containers, food handling equipment, fabric fibers (e.g., cotton or cotton blends), water storage and transport equipment, alcoholic or non-alcoholic drinks, outer casings or screens for electronic products, interior or exterior parts of furniture, curtains, and upholstery.
[0115] As used herein, "fibers in solution" or "pulp" refers to lignocellulosic fibrous material prepared by chemically or mechanically separating cellulose fibers from wood, fiber crops, or waste paper. In related aspects, when cellulose fibers are treated by methods as described herein, the cellulose fibers themselves contain bound SFAEs, glycerides, and / or FASs as separate entities, and the bound cellulose fibers have distinct and different properties from free fibers (e.g., pulp fibers or cellulose fibers or nanocellulose or microfibrillated cellulose SFAE blend bound materials will not form hydrogen bonds between fibers as readily as unbound fibers).
[0116] As used herein, "repulpable" means producing a paper or paperboard product suitable for being broken down into a soft, shapeless mass for reuse in the manufacture of paper or paperboard.
[0117] As used herein, "adjustable," including grammatical variations thereof, means adjusting or adapting a method to achieve a particular result.
[0118] As used herein, "water contact angle" refers to the angle, measured through a liquid, at which a liquid / vapor interface meets a solid surface. It quantifies the wettability of a solid surface by a liquid. The contact angle reflects the strength with which liquid and solid molecules interact with each other compared to the strength with which each interacts with its own molecules. On many highly hydrophilic surfaces, a drop of water exhibits a contact angle between 0° and 30°. Generally, a solid surface is considered hydrophobic if the water contact angle is greater than 90°. Water contact angles are readily obtained using an optical tensiometer (see, e.g., Dyne Testing, Staffordshire, United Kingdom).
[0119] As used herein, "water vapor permeability" refers to breathability, or the ability of a textile to transport moisture. There are at least two different measurement methods. One of them, the MVTR test (Water Vapor Transmission Rate) according to ISO 15496, describes the water vapor transmission rate (WVP) of a fabric and therefore its ability to transport sweat to the outside air. The measurement determines the number of grams of moisture (water vapor) that pass through one square meter of fabric in 24 hours (the higher the level, the more breathable it is).
[0120] In one embodiment, waterfastness can be determined using the TAPPI T 530 Hercules sizing test (i.e., paper sizing test by ink fastness). Ink fastness by the Hercules method is best classified as a test that directly measures penetration. Alternatively, it is classified as a speed of penetration test. There is no single best test for "measuring sizing." The choice of test depends on the end use and mill control needs. This method is particularly suitable for use as a mill control sizing test to accurately detect changes in sizing levels. It offers the sensitivity of the ink float test while providing reproducible results, shorter test times, and automatic endpoint determination.
[0121] Sizing, measured by the resistance to penetration or absorption of aqueous liquids into the paper, is an important property of many papers, typical of which are bags, container board, meat wrap, documents, and some printing grades.
[0122] This method can be used to monitor the production of paper or paperboard for a specific end use, provided an acceptable correlation is established between the test value and the paper's end-use performance. Due to the nature of the test and the penetrant, it may not correlate well enough to be applicable to all end-use requirements. This method measures sizing by penetration rate. Other methods measure sizing by surface contact, surface penetration, or absorption. Sizing tests are selected based on their ability to simulate the means of water contact or absorption in the end use. This method can also be used to optimize sizing chemical usage costs.
[0123] As used herein, "oxygen permeability" refers to the degree to which a polymer allows the passage of a gas or fluid. The oxygen permeability (Dk) of a material is a function of the diffusivity (D) (i.e., how quickly oxygen molecules move through the material) and the solubility (k) (or the amount of oxygen molecules absorbed per volume in the material). Oxygen permeability (Dk) values are typically between 10 and 150 x 10 -11 (cm2 The relationship between hydrogel water content and oxygen permeability (units: barrers) is semi-logarithmic. The International Organization for Standardization (ISO) specifies permeability using the SI unit of hectopascal (hPa) for pressure. Therefore, Dk = 10 -11 (cm 2 ml O2) / (s ml hPa). Barrer units can be converted to hPa by multiplying them by the constant 0.75.
[0124] As used herein, "biodegradable," including grammatical variations thereof, means capable of being broken down by the action of living organisms (eg, by microorganisms), especially into harmless products.
[0125] As used herein, "recyclable," including grammatical variations thereof, means a material that can be treated or processed (post-consumer and / or scrap) to create a material suitable for reuse.
[0126] As used herein, "Gurley seconds" or "Gurley number" is a unit of measurement that describes the number of seconds required for 100 cubic centimeters (deciliters) of air to pass through 1.0 square inch of a given material at a pressure differential of 4.88 inches (0.176 psi) of water (ISO 5636-5:2003) (porosity). Additionally, for stiffness, "Gurley number" is a unit of measurement for a piece of material that measures the force required to deflect the material by a given amount (1 milligram force) when held vertically. Such values can be measured with a Gurley Precision Instruments device (Troy, New York).
[0127] HLB - The hydrophilic-lipophilic balance of a surfactant is a measure of how hydrophilic or lipophilic it is and is determined by calculating values for different regions of the molecule.
[0128] Griffin's method for nonionic surfactants, described in 1954, HLB=20* M h / M [In the formula, M h where M is the molecular weight of the hydrophilic portion of the molecule, and M is the molecular weight of the entire molecule. The results are reported on a scale of 0 to 20. An HLB value of 0 corresponds to a completely lipophilic / hydrophobic molecule, and a value of 20 corresponds to a completely hydrophilic / lipophobic molecule.
[0129] The HLB value can be used to predict the surfactant properties of a molecule. Less than 10: Fat-soluble (water-insoluble) Over 10: Water soluble (lipid insoluble) 1.5~3: Defoamer 3-6: W / O (water-in-oil) emulsifier 7-9: Wetting agent 13-15: Cleaning agent 12-16: O / W (oil-in-water) emulsifier 15-18: Solubilizers or hydrotropes.
[0130] In some embodiments, the HLB value of an SFAE / glyceride / FAS blend as described herein (or an overall formulation including said blend) may be in the lower range, hi some embodiments, the HLB value of an SFAE / glyceride / FAS blend as described herein (or an overall formulation including said blend) may be in the medium to higher range.
[0131] As used herein, "SEFOSE®" refers to a sucrose fatty acid ester (soyate) made from soybean oil containing one or more fatty acids that are unsaturated, which is commercially available from Procter & Gamble Chemicals (Cincinnati, Ohio) under the trade name SEFOSE 1618U (see Sucrose Polysoyate below). SEFOSE® is an exemplary SFAE for use in the methods and barrier formulations of the present disclosure.
[0132] As used herein, "soyate" refers to a mixture of salts of fatty acids from soybean oil. The SFAEs for use in the methods and barrier formulations of the present disclosure may include or be derived from "soyate."
[0133] As used herein, "oilseed fatty acids" refers to fatty acids from plants including, but not limited to, soybean, peanut, rapeseed, barley, canola, sesame seed, cottonseed, palm kernel, grape seed, olive, safflower, sunflower, copra, corn, coconut, flaxseed, hazelnut, wheat, rice, potato, cassava, legumes, camelina seed, mustard seed, and combinations thereof. The fatty acid chains of the SFAE / glyceride / FAS blend can be oilseed fatty acids.
[0134] As used herein, "wet strength" refers to a measure of how well the web of fibers holding paper (or other three-dimensional solid cellulose-based product) together can resist breaking forces when the paper is wet. Wet strength can be measured using a Finch Wet Strength Device from Thwing-Albert Instrument Company (West Berlin, NJ). In that case, wet strength is typically provided by wet strength additives such as kymenes, cationic glyoxylated resins, polyamidoamine-epichlorohydrin resins, polyamine-epichlorohydrin resins, including epoxide resins. In embodiments, cellulose-based materials coated with barrier formulations as described herein provide such wet strength in the absence of such additives.
[0135] As used herein, "wet" means covered or saturated with water or another liquid.
[0136] The methods described herein can include the further step of exposing the contacted cellulose-based material to heat, radiation, a catalyst, or a combination thereof for a time sufficient to bond the SGF blend, CNF, and / or reinforced CNF to the cellulose-based material. In related embodiments, such radiation can include, but is not limited to, UV, IR, visible light, or a combination thereof. In another related embodiment, the reaction can be carried out at room temperature (i.e., 25°C) to about 150°C, about 50°C to about 100°C, or about 60°C to about 80°C.
[0137] As used herein, "natural wax" refers to a relatively high molecular weight / high melting point material. "Natural wax" includes, for example, biowaxes obtained from renewable resources such as vegetable oils, fatty acids, and fatty acid esters (see, for example, https: / / www.researchgate.net / publication / 318385619_High_Quality_Biowaxes_from_Fatty_Acids_and_Fatty_Esters_Catalyst_and_Reaction_Mechanism_for_Accompanying_Reactions and https: / / www.researchgate.net / figure / a-Preparation-of-canola-PFFA-18-biowax-b-Preparation-of-nanocellulose-from-canola_fig1_306527797).
[0138] As used herein, "cellulose crosslinker" refers to known cellulose crosslinkers, such as glyoxal and less reactive dialdehydes or anhydrides.
[0139] As used herein, "glyceride" has its conventional meaning and refers to acylglycerols, which are esters formed from glycerol and fatty acids. Glycerol has three hydroxyl functional groups, which can be esterified with one, two, or three fatty acids to form mono-, di-, and triglycerides. These structures can vary in their aliphatic chains, as they can contain different carbon numbers, different degrees of unsaturation, and different configurations and positions of olefins.
[0140] Glycerides are obtained by esterification with substantially pure fatty acids by known esterification processes. Glycerides can also be extracted from vegetable oils and animal fats by known extraction methods.
[0141] As used herein, "fatty acid" has its ordinary meaning and refers to a carboxylic acid having an aliphatic chain that may be saturated or unsaturated. As used herein, fatty acid may refer to a fatty acid group attached to a glycerol residue of a glyceride.
[0142] The fatty acid group of the glyceride can be any known fatty acid. In a preferred embodiment, the fatty acid is known to be present in food, is edible, and / or is FDA approved. In some embodiments, the fatty acid is obtained from oilseeds. In another embodiment, the fatty acid is obtained from other sources of natural edible fats and oils.
[0143] The fatty acids of the glycerides can be independently selected from one or more saturated fatty acids, one or more monounsaturated fatty acids, and / or one or more polyunsaturated fatty acids, meaning, for example, that a triglyceride can contain three different fatty acid groups attached to a glycerol residue.
[0144] Exemplary saturated fatty acids for use in the formulations / compositions of the present disclosure may be selected from butyric acid (butanoic acid), caproic acid (hexanoic acid), caprylic acid (octanoic acid), capric acid (decanoic acid), lauric acid (dodecanoic acid), myristic acid (tetradecanoic acid), palmitic acid (hexadecanoic acid), stearic acid (octadecanoic acid), arachidic acid (icosanoic acid), behenic acid (docosanoic acid), or lignoceric acid (tetracosanoic acid).
[0145] Exemplary monounsaturated fatty acids for use in the formulations / compositions of the present disclosure may be selected from caproleic acid (dec-9-enoic acid), lauroleic acid ((Z)-dodec-9-enoic acid), myristoleic acid ((Z)-tetradec-9-enoic acid), palmitoleic acid ((Z)-hexadec-9-enoic acid), oleic acid ((Z)-octadec-9-enoic acid), elaidic acid ((E)-octadec-9-enoic acid), vaccenic acid ((E)-octadec-11-enoic acid), gadoleic acid ((Z)-icosa-9-enoic acid), erucic acid ((Z)-docosa-13-enoic acid), brassidic acid ((E)-docosa-13-enoic acid), or nervonic acid ((Z)-tetracos-15-enoic acid).
[0146] Exemplary polyunsaturated fatty acids for use in the formulations / compositions of the present disclosure are linoleic acid (LA) ((9Z,12Z)-octadeca-9,12-dienoic acid), alpha-linolenic acid (ALA) ((9Z,12Z,15Z)-octadeca-9,12,15-trienoic acid), gamma-linolenic acid (GLA) ((6Z,9Z,12Z)-octadeca-6,9,12-trienoic acid), columbic acid ((5E,9E,12E)-octadeca-5,9,12-trienoic acid), stearidonic acid ((6Z,9Z,12Z,15Z)-octadeca-6,9,12,15-tetraenoic acid), mead acid ((5Z,8Z,11Z)-icosa-5,8,11-trienoic acid), dihomo-gamma ... -linolenic acid (DGLA) ((8Z,11Z,14Z)-icosa-8,11,14-trienoic acid), arachidonic acid ((5Z,8Z,11Z,14Z)-icosa-5,8,11,14-tetraenoic acid), eicosapentaenoic acid (EPA) ((5Z,8Z,11Z,14Z,17Z)-icosa-5,8,11,14,17-pentaenoic acid), docosapentaenoic acid (DPA) ((7Z,10Z,13Z,16Z,19Z)-docosa-7,10,13,16,19-pentaenoic acid), and docosahexaenoic acid (DHA) ((4Z,7Z,10Z,13Z,16Z,19Z)-docosa-4,7,10,13,16,19-hexaenoic acid).
[0147] In some embodiments, the one or more glycerides can comprise a blend of one or more monoglycerides, one or more diglycerides, and / or one or more triglycerides. In this regard, the mono-, di-, and triglycerides can be blended in any weight ratio. That is, any one of the mono-, di-, or triglycerides can be the predominant glyceride component of the blend by weight (i.e., greater than 50% by weight, when the total weight of glycerides is considered to be 100% by weight). In another embodiment, the blend does not contain monoglycerides, does not contain diglycerides, or does not contain triglycerides.
[0148] The one or more glycerides may differ in their fatty acid alkyl groups. For example, the one or more glycerides may contain fatty acid groups with different carbon numbers, different degrees of unsaturation, and / or different olefin configurations and positions. The glycerides may include tripalmitin and / or tristearin.
[0149] In some embodiments, the glycerides may include one or more water-insoluble glycerides (e.g., as noted above, triglycerides are typically strongly non-polar and hydrophobic) in combination with one or more water-soluble glycerides (in any weight ratio from 0.1:99.9 to 99.9:0.1), or only insoluble glycerides. The solubility of a glyceride can be determined, for example, by its HLB value.
[0150] Those skilled in the art will appreciate that the HLB value of one or more glycerides can be selected by varying one or more of the above glyceride parameters. In this regard, when multiple glycerides are used, each glyceride can be selected to have similar or different HLB values (e.g., a lower range is used in combination with a higher range).
[0151] As used herein, "fatty acid salt" (or "FAS") has its ordinary meaning and refers to any one or more salts of fatty acids disclosed hereinabove. Exemplary cations of fatty acid salts include, but are not limited to, calcium, potassium, and sodium salts. Fatty acid salts can be synthesized by known methods or extracted from vegetable oils or animal fats by known methods. One exemplary method involves adding sodium hydroxide to fatty acids found in animal fats or vegetable oils (such as from oilseeds). For example, sodium palmitate is obtained from palm oil.
[0152] The one or more fatty acid salts may include one or more calcium, potassium, or sodium salts. The calcium, potassium, or sodium salts of fatty acids are obtained from naturally occurring sources such as oilseeds. The one or more fatty acid salts may include one or more selected from sodium oleate, sodium stearate, sodium palmitate, calcium oleate, calcium stearate, or calcium palmitate.
[0153] In some embodiments, the SGF blend may contain only one or more glycerides, only one or more fatty acid salts, or both one or more glycerides and one or more fatty acid salts. When the SGF blend contains both one or more glycerides and one or more fatty acid groups, the weight ratio of glycerides to fatty acid salts can be about 0.1:99.9 to about 99:0.1, about 10:90 to about 90:10, about 20:80 to about 80:20, about 35:65 to about 65:35, about 40:60 to about 60:40, about 45:55 to about 55:45, or about 50:50.
[0154] The weight ratio of SFAE in the SGF blend can be 0:100 to 100:0 or any weight ratio therebetween (e.g., 1:99, 5:95, 10:90, 20:80, 30:70, 40:60, 50:50, 60:50, 70:30, 80:20, 90:10, 95:5, 99:1).
[0155] The weight ratio of glycerides in the SGF blend can be 0:100 to 100:0 or any weight ratio therebetween (e.g., 1:99, 5:95, 10:90, 20:80, 30:70, 40:60, 50:50, 60:50, 70:30, 80:20, 90:10, 95:5, 99:1).
[0156] The weight ratio of fatty acid salts in the SGF blend can be 0:100 to 100:0 or any weight ratio therebetween (e.g., 1:99, 5:95, 10:90, 20:80, 30:70, 40:60, 50:50, 60:50, 70:30, 80:20, 90:10, 95:5, 99:1).
[0157] The weight ratio of natural waxes in the SGF blend can be 0:100 to 100:0 or any weight ratio therebetween (e.g., 1:99, 5:95, 10:90, 20:80, 30:70, 40:60, 50:50, 60:50, 70:30, 80:20, 90:10, 95:5, 99:1).
[0158] The weight ratio of cellulose crosslinker in the SGF blend can be 0:100 to 100:0 or any weight ratio therebetween (e.g., 1:99, 5:95, 10:90, 20:80, 30:70, 40:60, 50:50, 60:50, 70:30, 80:20, 90:10, 95:5, 99:1).
[0159] At sufficient concentrations and based on the blend selection, the binding of the SGF blend alone is sufficient to render the contacted substrate hydrophobic, i.e., hydrophobicity is achieved without the addition of waxes, rosins, resins, diketenes, shellacs, vinyl acetates, PLA, PEI, oils, other water-repellent chemicals, or combinations thereof (i.e., secondary hydrophobes), including, among other things, that other properties such as strengthening, stiffening, and bulking of cellulose-based materials are achieved by the binding of the glycerides / fatty acid salts alone.
[0160] The use of CNF alone as a binder has also been shown to increase the hydrophobicity of contacted substrates.
[0161] Saturated SFAEs, glycerides, and fatty acid salts are typically solid at nominal processing temperatures, while unsaturated SFAEs, glycerides, and fatty acid salts are typically liquid. This allows for the formation of a uniform and stable dispersion of saturated glycerides and fatty acid salts in the aqueous coating without significant interaction or incompatibility with other coating components, which are typically hydrophilic. Furthermore, this dispersion allows for the preparation of high concentrations of saturated glycerides and fatty acid salts without adversely affecting coating rheology, uniform coating application, or coating performance properties. If the saturated glyceride and fatty acid salt particles are melted and spread after heating, drying, and solidifying the coating layer, the coating surface becomes hydrophobic. The natural waxes of the present disclosure are also solid at nominal processing temperatures.
[0162] Sugar fatty acid esters of all sugars, including mono-, di-, and trisaccharides, are suitable for use in connection with aspects of the present disclosure. The sugar fatty acid esters may be mono-, di-, tri-, tetra-, penta-, hexa-, hepta-, or octaesters, and combinations thereof, including whether the fatty acid moiety may be saturated, unsaturated, or a combination thereof.
[0163] The SFAE may comprise or consist essentially of sucrose esters of fatty acids.
[0164] Many methods are known and available for making or otherwise providing the SFAEs of the present disclosure, and all such methods are believed to be available for use within the broad scope of the present disclosure. For example, in certain embodiments, fatty acid esters are preferably synthesized by esterifying sugars with one or more fatty acid moieties obtained from oilseeds, including, but not limited to, soybean oil, sunflower oil, olive oil, canola oil, peanut oil, and mixtures thereof.
[0165] The SFAE may comprise a sugar moiety, including but not limited to a sucrose moiety, substituted at one or more of its hydroxyl hydrogens with an ester moiety. In a related aspect, a disaccharide ester for use in the present disclosure may have the structure of Formula I of the '073 publication, which is incorporated herein by reference in its entirety.
[0166] Suitable disaccharides for SFAE may also include xylose, glucose, raffinose, maltodextrose, galactose, combinations of glucose, combinations of fructose, combinations of maltose, lactose, mannose, combinations of erythrose, isomaltose, isomaltulose, trehalose, trehalulose, cellobiose, laminaribiose, chitobiose, and combinations thereof.
[0167] In another embodiment, starch fatty acid esters can be used, where the starch can be from any suitable source, such as dent corn starch, waxy corn starch, potato starch, wheat starch, rice starch, sago starch, tapioca starch, sorghum starch, sweet potato starch, and mixtures thereof.
[0168] For use in the compositions of the present disclosure, the SFAE compound may have a high degree of substitution. In some embodiments, the sugar fatty acid ester is sucrose polysoyate.
[0169] [ka]
[0170] SFAEs can be produced by the techniques disclosed in the '073 application. For example, sugar fatty acid esters can be made by esterification with substantially pure fatty acids using known esterification processes. They can also be prepared by transesterification using saccharides and fatty acid esters in the form of fatty acid glycerides derived from natural sources, such as those found in oils extracted from oilseeds, such as soybean oil. Transesterification reactions using fatty acid glycerides to provide sucrose fatty acid esters are described, for example, in U.S. Pat. Nos. 3,963,699, 4,517,360, 4,518,772, 4,611,055, 5,767,257, 6,504,003, 6,121,440, and 6,995,232, and International Publication No. WO1992004361, all of which are incorporated herein by reference.
[0171] The cellulose-based products produced by the methods described herein can be configured to exhibit greater hydrophobicity (or water resistance) compared to similar cellulose-containing materials without treatment. In related embodiments, the treated cellulose-containing materials exhibit greater oleophobicity (or OGR) compared to similar cellulose-containing materials without treatment. In further related embodiments, the treated cellulose-containing materials can be biodegradable, compostable, and / or recyclable. In one embodiment, the treated cellulose-containing materials are both hydrophobic (water resistant) and oleophobic (oil resistant) (OGR).
[0172] The cellulose-based products of the present disclosure may have improved mechanical properties compared to similar untreated materials. For example, paper bags treated by the methods described herein exhibit increased burst strength, Gurley number, tensile strength, and / or maximum load energy. In one embodiment, the burst strength is increased by about 0.5 to 1.0 times, about 1.0 to 1.1 times, about 1.1 to 1.3 times, or about 1.3 to 1.5 times. In another embodiment, the Gurley number is increased by about 3 to 4 times, about 4 to 5 times, about 5 to 6 times, or about 6 to 7 times. In yet another embodiment, the tensile strain is increased by about 0.5 to 1.0 times, about 1.0 to 1.1 times, about 1.1 to 1.2 times, or about 1.2 to 1.3 times. In yet another embodiment, the maximum load energy is increased by about 1.0 to 1.1 times, about 1.1 to 1.2 times, about 1.2 to 1.3 times, and about 1.3 to 1.4 times.
[0173] The cellulose-containing material can be a base paper containing microfibrillated cellulose (MFC) or cellulose nanofibers (CNF), for example, as described in U.S. Publication No. 2015 / 0167243 (incorporated herein by reference in its entirety), where the MFC or CNF is added during the forming and papermaking process and / or added to a previous forming layer as a coating or secondary layer to reduce the porosity of the base paper. In embodiments, the resulting contacted base paper is controllably water- and oil-resistant. In related aspects, the resulting base paper can exhibit a Gurley value of at least about 10 to 15 (i.e., Gurley air resistance (sec / 100 cc, 20 oz.cyl.)), or at least about 100, at least about 200 to about 350. In one aspect, the barrier coatings described herein may be laminates for one or more layers, or may provide one or more layers as laminates, or may reduce the amount of coating for one or more layers to achieve similar performance benefits (e.g., water resistance, grease resistance, etc.) In a related aspect, the laminate may include a biodegradable and / or composable heat seal or adhesive.
[0174] In one embodiment, the SGF blend may be combined with one or more coating ingredients for internal and surface sizing (single or in combination), including, but not limited to, pigments (e.g., clay, calcium carbonate, titanium dioxide, plastic pigments), binders (e.g., starch, soy protein, polymer emulsions, PvOH, casein), and additives (e.g., glyoxal, glyoxalated resins, zirconium salts, polyethylene emulsions, carboxymethyl cellulose, acrylic polymers, alginates, polyacrylate gums, polyacrylates, biocides, oil-based defoamers, silicone-based defoamers, stilbenes, direct dyes, and acid dyes). In related aspects, such components can provide one or more properties, including, but not limited to, building a fine porous structure, forming a light-scattering surface, improving ink receptivity, improving gloss, binding pigment particles, binding the coating to the paper, reinforcing the base sheet, filling the pores of the pigment structure, reducing water sensitivity, resisting wet pick in offset printing, preventing blade scratching, improving gloss in supercalendering, reducing dusting, adjusting coating viscosity, providing water retention, dispersing pigments, maintaining coating dispersion, preventing coating / coating color deterioration, controlling foaming, reducing entrapped air and coating craters, increasing whiteness and brightness, and controlling color and shade. It will be apparent to one skilled in the art that combinations can vary depending on the property(ies) desired in the final product.
[0175] For wet-end applications, the SGF blend can be present in the aqueous mixture or dispersion at a concentration of at least 0.025% (wt / wt) of the total cellulosic fiber present in the dispersion. In related embodiments, the SGF can be present in a concentration of from about 0.05% (wt / wt) to about 0.1% (wt / wt), from about 0.1% (wt / wt) to about 0.5% (wt / wt), from about 0.5% (wt / wt) to about 1.0% (wt / wt), from about 1.0% (wt / wt) to about 2.0% (wt / wt), or from about 2.0% (wt / wt) to about 3.0% (wt / wt). % (wt / wt) to about 3.0% (wt / wt), about 3.0% (wt / wt) to about 4.0% (wt / wt), about 4.0% (wt / wt) to about 5.0% (wt / wt), about 5.0% (wt / wt) to about 10% (wt / wt), or about 10% (wt / wt) to about 50% (wt / wt).
[0176] In wet-end applications, the CNFs can be present in the aqueous mixture or dispersion at a concentration of at least 0.025% (wt / wt) of the total cellulose fiber present in the dispersion. In related embodiments, the CNFs can be present in a concentration of from about 0.05% (wt / wt) to about 0.1% (wt / wt), from about 0.1% (wt / wt) to about 0.5% (wt / wt), from about 0.5% (wt / wt) to about 1.0% (wt / wt), from about 1.0% (wt / wt) to about 2.0% (wt / wt), from about 2.0% (wt / wt) to about 3.0% (wt / wt), from about 3.0% (wt / wt) to about 4.0% (wt / wt), or from about 4.0% (wt / wt) to about 5.0% (wt / wt) of the total fiber present. ), about 5.0% (wt / wt) to about 10% (wt / wt), about 10% (wt / wt) to about 20% (wt / wt), about 20% (wt / wt) to about 30% (wt / wt), about 30% (wt / wt) to about 40% (wt / wt), about 40% (wt / wt) to about 50% (wt / wt), about 60% (wt / wt) to about 70% (wt / wt), about 70% (wt / wt) to about 80% (wt / wt), or about 80% (wt / wt) to about 90% (wt / wt).
[0177] In wet-end applications, the reinforcing CNFs can be present in the aqueous mixture or dispersion at a concentration of at least 0.025% (wt / wt) of the total cellulose fiber present in the dispersion. In related embodiments, the reinforcing CNFs are present in a concentration of from about 0.05% (wt / wt) to about 0.1% (wt / wt), from about 0.1% (wt / wt) to about 0.5% (wt / wt), from about 0.5% (wt / wt) to about 1.0% (wt / wt), from about 1.0% (wt / wt) to about 2.0% (wt / wt), from about 2.0% (wt / wt) to about 3.0% (wt / wt), from about 3.0% (wt / wt) to about 4.0% (wt / wt), or from about 4.0% (wt / wt) to about 5.0% (wt / wt) of the total fiber present. t), about 5.0% (wt / wt) to about 10% (wt / wt), about 10% (wt / wt) to about 20% (wt / wt), about 20% (wt / wt) to about 30% (wt / wt), about 30% (wt / wt) to about 40% (wt / wt), about 40% (wt / wt) to about 50% (wt / wt), about 60% (wt / wt) to about 70% (wt / wt), about 70% (wt / wt) to about 80% (wt / wt), or about 80% (wt / wt) to about 90% (wt / wt).
[0178] As used herein, "coating weight" is the weight of material (wet or dry) to be applied to a substrate, expressed in pounds per specified ream or grams per square meter.
[0179] In the coating application, the reinforced CNF is applied to the surface of the substrate in an amount of at least about 0.05 g / m 2 In a related embodiment, the SGF blend can be present on the surface of the cellulose-based material at a coating weight of about 0.05 g / m 2 ~Approx. 1.0g / m 2 , about 1.0g / m 2 ~about 2.0g / m 2 , about 2g / m 2 ~about 3g / m 2 , 3g / m 2 ~approx. 4g / m 2 , approximately 4 g / m 2 ~about 5g / m 2 , about 5g / m 2 ~about 10g / m 2 , or approximately 10 g / m2 ~about 20g / m 2 The coating weight may be
[0180] In a coating application, the SGF blend is applied to the surface of the substrate at a concentration of at least about 0.05 g / m 2 In a related embodiment, the SGF blend can be present on the surface of the cellulose-based material at a coating weight of about 0.05 g / m 2 ~Approx. 1.0g / m 2 , about 1.0g / m 2 ~about 2.0g / m 2 , about 2g / m 2 ~about 3g / m 2 , 3g / m 2 ~approx. 4g / m 2 , approximately 4 g / m 2 ~about 5g / m 2 , about 5g / m 2 ~about 10g / m 2 , or approximately 10 g / m 2 ~about 20g / m 2 The coating weight may be
[0181] In a coating application, the CNFs are applied to the surface of the cellulose-based material (or substrate) at a concentration of at least about 0.05 g / m 2 (gsm). In a related embodiment, the CNFs can be present on the surface of the cellulose-based material at a coating weight of about 0.05 g / m 2 ~Approx. 1.0g / m 2 , about 1.0g / m 2 ~about 2.0g / m 2 , about 2g / m 2 ~about 3g / m 2 , 3g / m 2 ~approx. 4g / m 2 , approximately 4 g / m 2 ~about 5g / m 2 , about 5g / m 2 ~about 10g / m 2 , about 10g / m 2 ~about 20g / m 2 , or approximately 20 g / m 2 ~about 30g / m 2 The coating weight may be
[0182] Hydrophobic barrier properties can be imparted to the substrate by the SGF blend and / or reinforced CNF in the absence of a secondary hydrophobe.
[0183] The barrier formulation may include one or more emulsifiers or emulsifying agents in concentrations sufficient to form an emulsion of the SGF blend with water and / or to form an emulsion of the reinforced CNF with water. Suitable emulsifiers or emulsifying agents include buffers, polyvinyl alcohol (PvOH), carboxymethylcellulose (CMC), milk proteins, gelatin, starch, acetylated polysaccharides, alginates, carrageenan, chitosan, inulin, long chain fatty acids, waxes, agar, alginates, glycerol, gums, lecithin, poloxamer, monoglycerol, diglycerol, monosodium phosphate, monostearate, propylene glycol, detergents, cetyl alcohol, glycerol esters, (saturated) ((poly)unsaturated) fatty acid methyl esters, and combinations thereof.
[0184] The methods described herein may include a step of predetermining the content of the SGF blend and / or the components of the SGF blend to be included in the reinforced CNF. In some embodiments, this predetermining step can be performed before preparing the reinforced CNF. The predetermining step can be performed to achieve a desired effect. When the reinforced CNF is used in a barrier formulation and / or added to a papermaking furnish at the wet end, the predetermining step can be performed to achieve a desired level of water resistance and / or a desired level of oil and grease resistance. In some embodiments, the predetermining step can be performed to increase the dewatering rate of the furnish or fiber slurry. Increasing the dewatering rate improves, for example, the production rate of cellulose-based articles. As mentioned above, dewatering of slurries containing CNFs is one of the greatest challenges facing the use of CNFs. Increased dewatering rate applies, for example, to both the creation of reinforced CNF binders and the use of reinforced CNF binders in barrier formulations. Dewatering is well known in the paper industry and is described elsewhere in this disclosure in Smook, which is incorporated herein by reference in its entirety.
[0185] The methods described herein can include a step of predetermining the content of the SGF blend to be included in the barrier formulation and / or a step of predetermining the components of the SGF blend. In some embodiments, this predetermining step can be performed before preparing the barrier formulation or before contacting the cellulose-based material with the formulation. The predetermining step can be performed to achieve a desired effect. The predetermining step can be performed to achieve a desired level of water resistance and / or a desired level of oil and grease resistance.
[0186] As mentioned above, the barrier formulation may include one or more pigments commonly used in the paper industry. The one or more pigments may be present in the formulation at a concentration of about 0.1% to about 90% by weight, based on the total weight of the formulation. In another embodiment, the pigment concentration may be about 1% to 10%, about 11% to 20%, about 21% to 30%, about 31% to 40%, about 41% to 50%, 51% to 60%, 61% to 70%, 71% to 80%, 81% to 90%, or any other range within the range of 0.1% to 90% by weight. The use of pigments is well known in the paper industry, and the pigment concentration can be selected to vary the properties of the final product. Exemplary pigments include clay, calcium carbonate, titanium dioxide, kaolin, talc, plastic pigments, silica, silicates, metal oxides, alumina, aluminates, and diatomaceous earth.
[0187] As described above, the barrier formulation may include one or more charged polymers to aid in the retention of the reinforced CNF and / or SGF blend on the cellulose-based substrate. The one or more charged polymers may include one or more cationic, anionic, nonionic, and / or zwitterionic polymers. The charged polymer may include a combination of a relatively low molecular weight cationic polymer and a relatively high molecular weight anionic polymer.
[0188] The charged polymer may be comprised of one or more cationic polymers. The one or more cationic polymers may include polyacrylamide. The polyacrylamide may include polyDADMAC (polydiallyldimethylammonium chloride).
[0189] The cationic polymer can have a weight average molecular weight of 500,000 to 10,000,000. In some embodiments, the weight average MW is 500,000 to 1,000,000, 1,000,001 to 2,000,000, 2,000,001 to 3,000,000, 3,000,001 to 4,000,000, 4,000,001 to 5,000,000, 5,000,001 to 6,000,000, 6,000,001 to 7,000,000, 7,000,001 to 8,000,000, 8,000,001 to 9,000,000, or 9,000,001 to 10,0000. In some aspects, blends of charged polymers are used to achieve a "bimodal" type weight-average MW using combinations of charged polymers with optional MWs within the above ranges (e.g., a first charged polymer having a weight-average MW of less than 1,000,000 is used in combination with a second charged polymer having a weight-average MW of greater than 2,000,000; the weight ratio of the first charged polymer to the second charged polymer is 10:90 to 90:10). In some embodiments, the concentration of the cationic polymer in the formulation is about 0.01% to about 5%, about 0.01% to about 3%, 0.05% to about 0.1%, or about 0.1% to about 1%, or about 1% to about 3% by weight, when the total weight of the formulation is considered to be 100%. In some embodiments, the weight ratio of cationic polymer to reinforcing CNF in the formulation is about 0.1:99.9 to about 20:80, 0.5:99.5 to about 15:85, about 1:99 to about 10:90, or about 2.5:97.5 to about 7.5:92.5. In some embodiments, the weight ratio of cationic polymer to SGF blend in the formulation is about 0.1:99.9 to about 20:80, 0.5:99.5 to about 15:85, about 1:99 to about 10:90, or about 2.5:97.5 to about 7.5:92.5.
[0190] In some embodiments, as described above, prolamines can be used as retention aids in barrier formulations containing reinforced CNF and / or SGF blends in place of charged polymers.
[0191] The barrier formulation may also include one or more conventional papermaking binders. Exemplary binders include CNF, the reinforced CNF of the present disclosure, starch, polymers, polymer emulsions, PvOH, prolamines, or combinations thereof. In some embodiments, the formulation may contain no binders other than the reinforced CNF.
[0192] The barrier formulation can be provided in the form of an emulsion. The emulsion can be used as the barrier formulation in the methods of the present disclosure. In some embodiments, the emulsion can contain no emulsifiers other than the SGF blend. Alternatively, the emulsion can contain from about 0.01% to about 80% by weight of one or more emulsifiers. The emulsion can also include materials to stabilize the emulsion for a period of time (e.g., weeks, months, etc.), such as nano- or microfibrillated cellulose, gums, or thickeners. A list of exemplary emulsifiers is provided above.
[0193] Cellulose-based materials or substrates, which can be dried (e.g., at about 80-150°C) before application, can be treated with the modifying formulation, for example, by immersion and exposing the surface to the composition for less than 1 second. The substrate can be heated to dry the surface, after which the modified material is ready for use. In one aspect, according to the methods described herein, the substrate can be treated with any suitable coating / sizing process typically performed in a paper mill (see, for example, Smook, G., Surface Treatments in Handbook for Pulp & Paper Technologists, (2016), 4th Ed., Cpt. 18, pp. 293-309, TAPPI Press, Peachtree Corners, GA USA, incorporated herein by reference in its entirety).
[0194] In some applications, the cellulose-based material may be dried before treatment, but no special preparation of the material is required to practice the present disclosure. In one embodiment, the disclosed method can be used on any cellulose-based surface, including, but not limited to, films, rigid containers, fibers, pulp, fabrics, etc. In one aspect, the barrier formulation can be applied by conventional size presses (vertical, inclined, horizontal), gate roll size presses, metering size presses, calendar size application, tube sizing, on-machine, off-machine, single-sided coaters, double-sided coaters, short dwell, simultaneous two-sided coaters, blade or rod coaters, gravure coaters, gravure printing, flexographic printing, inkjet printing, laser printing, water containers on calendar machines, and combinations thereof.
[0195] Depending on the source, the cellulose treated in the methods herein can be paper, paperboard, pulp, softwood fiber, hardwood fiber, or combinations thereof, nanocellulose, cellulose nanofibers, whiskers or microfibrils, microfibrillated cotton or cotton blends, cellulose nanocrystals, or nanofibrillated cellulose.
[0196] Additionally, modified fibers and cellulose-based materials as described herein can be repulped, and further, for example, water cannot be easily "pushed" across a low surface energy barrier into the sheet.
[0197] In one embodiment, the amount of barrier formulation applied is sufficient to completely cover at least one surface of the substrate, e.g., at least one surface of the cellulose-containing material. For example, in one embodiment, the barrier formulation may be applied to the entire outer surface of the container, the entire inner surface of the container, or a combination thereof, or to one or both sides of the base paper. In another embodiment, the entire upper surface of the film may be covered with the barrier formulation, the entire lower surface of the film may be covered with the barrier formulation, or a combination thereof. In some embodiments, the inner lumen of the device / instrument may be covered with the barrier formulation, the outer surface of the device / instrument may be covered with the barrier formulation, or a combination thereof.
[0198] In one embodiment, the amount of barrier formulation applied is sufficient to partially cover at least one surface of the cellulose-based material. For example, only the surface exposed to the ambient atmosphere is covered by the barrier formulation, or only the surface not exposed to the ambient atmosphere is covered by the barrier formulation (e.g., masked). As will be apparent to one skilled in the art, the amount of barrier formulation applied can depend on the use of the material to be covered. In one aspect, one surface can be coated with the barrier formulation, and the opposite surface can be coated with an agent including, but not limited to, proteins, wheat gluten, gelatin, prolamin, soy protein isolate, starch, modified starch, acetylated polysaccharides, alginate, carrageenan, chitosan, inulin, long-chain fatty acids, waxes, and combinations thereof. In a related aspect, the barrier formulation can be added to the furnish, and the resulting material on the web can be coated with an additional coating of the barrier formulation (having a composition similar to or different from that added to the wet end).
[0199] Any suitable coating process can be used to deliver any of the various barrier formulations in the course of practicing this method, hi one embodiment, the coating process includes dipping, spraying, painting, printing, and any combination of any of these processes, alone or in conjunction with other coating processes adapted to practice the methods of the present disclosure.
[0200] The permeability of a surface to various gases, such as water vapor and gases (e.g., oxygen, nitrogen, and carbon dioxide), can also be modified by the barrier formulation as the material's barrier function increases. The standard unit for measuring permeability is the barrer, and protocols for measuring these parameters are also available in the public domain (see ASTM std F2476-05 for water vapor, ASTM std F2622-8 for oxygen, and https: / / www.ametekmocon.com / products / searchbybrand / mocon for general gas testing). MOCON permeation test analyzers have been recognized as industry-leading solutions for over 50 years and are the basis for many global permeation test standards, such as ASTM D3985 and ASTM F1249. The extensive line of MOCON analyzers represents decades of technical leadership and continuous innovation in partnership with our customers, distributors, and institutions. Our MOCON permeation analyzers offer broad testing capabilities across a highly diverse range of products and materials. In some embodiments, permeability to vapors and gases can be further reduced by adding one or more prolamines to the barrier formulation.
[0201] In one embodiment, materials treated according to the disclosed methods exhibit complete biodegradability as measured by degradation in an environment under microbial challenge.
[0202] Various methods are available for defining and testing biodegradability, including the shake flask method (ASTM E1279-89(2008)) and the Zahn-Wellens test (OECD TG 302B).
[0203] A variety of methods are available for defining and testing compostability, including but not limited to ASTM D6400.
[0204] Barrier coated products of the present disclosure may have a TAPPI T 559 KIT test value of from about 3 to about 12, greater than 4, greater than 5, greater than 6, greater than 7, greater than 8, greater than 9, greater than 10, greater than 11, etc.
[0205] Barrier coated products of the present disclosure may have HST values of at least about 65 seconds, at least about 120 seconds, at least about 240 seconds, at least about 480 seconds, etc.
[0206] The surface of a barrier coated article of the present disclosure may exhibit a water contact angle of about 60 to 120 degrees, at least about 90 degrees, at least about 100 degrees, at least about 110 degrees, at least about 120 degrees, etc.
[0207] In some embodiments, the barrier formulations of the present disclosure form stable aqueous compositions, where a "stable aqueous composition" is defined as an aqueous composition that is substantially resistant to viscosity change, solidification, and settling for a period of at least 8 hours when contained in a sealed container and stored at a temperature ranging from about 0 degrees Celsius to about 60 degrees Celsius. Some embodiments of the barrier formulations are stable for a period of at least 24 hours, and often for a period of at least 6 months.
[0208] In some embodiments, the barrier coated products obtained by the methods of the present disclosure are PFAS-free. In some embodiments, the barrier coated products of the present disclosure are PFAS-free in the barrier coating.
[0209] In some embodiments, the barrier-coated product obtained by the method of the present disclosure is folded into a three-dimensional shape and contained in a sealed package. In these embodiments, the barrier layer can be the inner, exposed layer (or outer layer) of the package. The material of the package can be any conventional material for storing, transporting, selling, etc., food or beverage products. In these embodiments, the sealed package can also contain a food or beverage product therein. In these embodiments, the food or beverage product can be in contact with the barrier paper layer. The seal of the sealed package can be a hermetic seal.
[0210] In some embodiments, the barrier-coated products obtained by the methods of the present disclosure are compatible with conventional paper recycling programs, i.e., do not pose any adverse impact to recycling operations as occurs with polyethylene, polylactic acid, or wax-coated papers.
[0211] In some embodiments, the barrier-coated products obtained by the methods of the present disclosure are biobased. As used herein, "biobased" (or "biobased") refers to materials intentionally made from substances derived from living (or formerly living) organisms. In related aspects, materials containing at least about 50% of such substances are considered biobased. In some aspects, the barrier-coated products obtained by the methods of the present disclosure can be entirely biobased. In some aspects, the barrier formulations of the present disclosure can be entirely biobased.
[0212] In some embodiments, the barrier-coated products obtained by the methods of the present disclosure are recyclable. As used herein, "recyclable," including grammatical variations thereof, means that said material can be treated or processed (post-consumer and / or scrap) to make the material suitable for reuse.
[0213] In some embodiments, the barrier-coated products of the present disclosure are biodegradable. As used herein, "biodegradable," including grammatical variations thereof, means capable of being broken down by the action of living organisms (e.g., by microorganisms), especially into harmless products. [Example]
[0214] Hereinafter, the embodiments of the present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to these.
[0215] [Example 1] Example 1 was a laboratory study on the use of CNF in molded pulp products with barrier properties.
[0216] The equipment used in Example 1 is as follows: Buchner funnel - large (think about 8 inches in diameter) ·thermos Laboratory Vacuum Pump Spray bottle Stopwatch
[0217] The materials that can be used in Example 1 are as follows: Bleached kraft pulp slurried at 1% solids (50% SWK, 50% HWK) CNF slurry - 0.5% solids 10% SE-15 * CNF slurry with 0.5% solids SE-9 ** / SE30 *** Emulsion, 1% solids C-PAM (cationic polyacrylamide), 0.1% solids Cationic coagulant, 0.1% solids Pigment, IMERYS Capim DG Clay Slurry, 1% Solids
[0218] *SE-15 was obtained from HANGZHOU UNION BIOTECHNOLOGY CO., LTD. SE-15 is sold as sucrose fatty acid ester. Analysis of SE-15 revealed that it contained approximately 15-30% by weight of sugar fatty acid ester, approximately 40-60% by weight of glyceride, and the remainder fatty acid salts plus minor components.
[0219] ** SE-9 was obtained from ZHEJIANG SYNOSE TECH. SE-9 is sold as sucrose fatty acid esters. Analysis of SE-9 revealed that its composition was similar to SE-15, except for a higher glyceride content and approximately 10-20% less sucrose esters.
[0220] *** SE-30 was obtained from EAST CHEMSOURCES LIMITED. SE-30 is sold as a sucrose fatty acid ester. Analysis of SE-30 revealed it to contain over 80% sucrose esters with various substituents. The remainder of the product was glycerides with relatively little (less than 5% by weight) salt.
[0221] The test procedure for Example 1 was as follows:
[0222] <Blank or control> (1) Add a sufficient amount of bleached kraft slurry to a Buchner funnel to produce a fibrous pad having a basis weight of 150 gsm. Record the volume of furnish to be used in future runs. (2) Once the slurry is added to the Buchner funnel, start the vacuum pump. (3) Record the time to drain the furnish to the "wet line," which is the point during the draining process when the surface of the fiber slurry goes from a shiny or "wet" appearance to a dull, textured surface. (4) Continue applying vacuum to the wet sample for 10 seconds. (5) Remove the wet mat from the Buchner funnel and place the wet mat between two pieces of blotter paper. Roll a standard handsheet roller twice over the blotter paper to press the test sample. (6) The pressed sample is removed and placed in an oven at 100°C until dry.
[0223] <Internal treatment (wet end application)> (1) Add one or more additives to an aliquot of the furnish slurry (volume determined during the manufacture of the control sample) and mix. See Table 1 below. (2) A sufficient amount of the blended slurry is added to a Buchner funnel to produce a fibrous pad having a basis weight of 150 gsm. (3) Once the slurry is added to the Buchner funnel, start the vacuum pump. (4) Record the time it takes for the furnish to drain to the "wet line." (5) Continue applying vacuum to the wet sample for 10 seconds. (6) Remove the wet mat from the Buchner funnel and place the wet mat between two pieces of blotter paper. Roll a standard handsheet roller twice over the blotter paper to press the test sample. (7) The pressed sample is removed and placed in an oven at 100°C until dry.
[0224] <Spray treatment (coated articles)> (1) A sufficient amount of bleached kraft slurry is added to a Buchner funnel to produce a fibrous pad having a basis weight of 150 gsm. (2) Once the slurry is added to the Buchner funnel, start the vacuum pump. (3) Record the time it takes for the furnish to drain to the "wet line." (4) A known amount of diluted suspension of additive is sprayed onto the surface of the wet mat. See Table 2 below. (5) Continue applying vacuum to the wet sample for 10 seconds. (6) Remove the wet mat from the Buchner funnel and place the wet mat between two pieces of blotter paper. Roll a standard handsheet roller twice over the blotter paper to press the test sample. (7) The pressed sample is removed and placed in an oven at 100°C until dry.
[0225] [Table 1]
[0226] Table 1 lists the additives by their weight percentage on a dry basis.
[0227] [Table 2]
[0228] Table 2 lists the additives by their weight percentage on a dry basis.
[0229] Based on experimental testing of exemplary embodiments, the data in Table 3 demonstrates the improvements achieved in water resistance and / or oil and grease resistance. Water resistance was tested using an adapted water Cobb test from Tappi Standard Test Method T441 om-20, "Water Absorptiveness of Paper." Oil and grease resistance was tested using the 3M KIT test (Tappi Standard Test Method T559, "Grease Resistance") and an adapted oil Cobb test using vegetable oil from Tappi Standard Test Method T441 om-20.
[0230] [Table 3]
[0231] While the basic novel features of the present disclosure have been described as applicable to preferred exemplary embodiments thereof, it should be understood that those skilled in the art may make omissions, substitutions, and changes in the form and details of the present disclosure without departing from the spirit of the disclosure. Moreover, as will be readily apparent, numerous variations and modifications may readily occur to those skilled in the art. For example, any feature(s) in one or more embodiments may be applicable and combined with one or more other embodiments. It is not desired to limit the disclosure to the exact construction and operation shown and described, but all suitable equivalent modifications may be resorted to as falling within the scope of the disclosure as claimed. In other words, although embodiments of the present disclosure have been described with reference to examples, it is understood that modifications and variations are encompassed within the spirit and scope of the disclosure. The present invention is limited only by the following claims.
[0232] All references cited herein are incorporated by reference in their entirety.
Claims
1. 1. A method of making a cellulose-based article, comprising: adding a reinforced cellulose nanofibril binder comprising cellulose nanofibrils (CNF) and an SGF blend bound to the CNF to an aqueous papermaking furnish, the SGF blend comprising sugar fatty acid esters (SFAEs), glycerides, and fatty acid salts; draining water from the furnish to obtain a fibrous web; forming the fibrous web into a shaped article having a three-dimensional shape; A method comprising:
2. The method of claim 1, wherein the weight ratio of said CNF to said SGF blend is from 10:90 to 90:
10.
3. The reinforced cellulose nanofibril binder is Obtaining an aqueous mixture of cellulose nanofibrils (CNF); Obtaining an aqueous SGF blend, said aqueous SGF blend comprising sugar fatty acid esters (SFAEs), glycerides, and fatty acid salts; mixing the aqueous mixture of CNF with the aqueous SGF blend to bind the CNF to the SGF blend to obtain the reinforced cellulose nanofibril binder; Optionally, reducing the moisture content of the CNF mixed with the aqueous SGF blend. The method of claim 1 , obtained by
4. The reinforced cellulose nanofibril binder is Obtaining an aqueous mixture of cellulose pulp; Obtaining an aqueous SGF blend, said aqueous SGF blend comprising sugar fatty acid esters (SFAEs), glycerides, and fatty acid salts; mixing the mixture of cellulose pulp with the aqueous SGF blend to obtain a cellulose / SGF mixture; subjecting the cellulose / SGF mixture to mechanical shear forces to obtain the reinforced cellulose nanofibril binder; Optionally, subjecting the cellulose pulp to a pretreatment prior to obtaining the cellulose / SGF mixture and / or prior to subjecting the cellulose / SGF mixture to the mechanical shear force. The method of claim 1 , obtained by
5. 5. The method of claim 4, further comprising subjecting the cellulose pulp to a pretreatment prior to obtaining the cellulose / SGF mixture and / or prior to subjecting the cellulose / SGF mixture to the mechanical shear force.
6. 2. The method of claim 1, wherein the reinforced cellulose nanofibril binder is provided as a barrier formulation comprising the reinforced cellulose nanofibril binder and further comprising one or more pigments, one or more prolamines, one or more binders, one or more emulsifiers or substances, or one or more charged polymers.
7. 1. A method for imparting barrier properties to a cellulose-based material, comprising: contacting the cellulose-based material comprising cellulose fibers with an aqueous barrier formulation to impart the barrier properties, the barrier formulation comprising a reinforced cellulose nanofibril binder comprising cellulose nanofibrils (CNF) and an SGF blend bound to the CNF, the SGF blend comprising sugar fatty acid esters (SFAEs), glycerides, and fatty acid salts, the barrier formulation comprising about 4% to about 96% by weight of the CNF and about 4% to about 96% by weight of the SGF blend; binding said barrier formulation to a surface of said cellulose-based material to obtain a bound cellulose-based material having said barrier properties; Including, The method, wherein the barrier property is one or more selected from the group consisting of water resistance, lipid resistance, and gas resistance.
8. 8. The method of claim 7, wherein the contacting step comprises coating a surface of a cellulose-based substrate with the formulation by dipping, spraying, painting, printing, or any combination of these processes.
9. The SGF blend is at least about 0.05 g / m2 on the surface of the substrate. 2 The method of claim 8, wherein the component (A) is present in an amount of from about 1 to about 100 parts by weight.
10. The cellulose based substrate may be any of the following: paper, paperboard, bacon board, insulating materials, paper pulp, food storage cartons, compost bags, food storage bags, release paper, shipping bags, weed blocking / barrier fabrics or films, mulching films, flower pots, packing beads, bubble wrap, oil absorbing materials, laminates, envelopes, gift cards, credit cards, gloves, raincoats, OGR paper, shopping bags, diapers, membranes, tableware, tea bags, containers for holding coffee or tea, containers for holding hot or cold beverages, cups, dishes, bottles for storing carbonated liquids, non-carbonated 9. The method of claim 8, wherein the surface of an article is selected from the group consisting of bottles for storing acid liquids, lids, films for food packaging, trash disposal containers, food handling equipment, fabric fibers, water storage and transport equipment, storage and transport equipment for alcoholic or non-alcoholic beverages, outer casings or screens for electronic products, interior or exterior parts of furniture, curtains, upholstery, fabrics, films, boxes, sheets, trays, pipes, water conduits, clothing, medical devices, pharmaceutical packaging, contraceptives, camping equipment, molded cellulosic materials, and combinations thereof.
11. The method of claim 7 , wherein the bound cellulose-based material exhibits a water contact angle of 90° or greater.
12. 8. The method of claim 7, wherein the bound cellulose-based material exhibits a TAPPI T 559 KIT test value of 3 to 12 in the absence of a secondary hydrophobe.
13. 1. A method of making a molded article, comprising the steps of: providing a forming tool having a three-dimensional shape including a forming portion; contacting the forming portion with a cellulose composition such that the forming portion is covered with a wet layer of pulp; and dewatering the layer of pulp on the forming tool to obtain the molded article; The cellulose composition comprises: Cellulose pulp, as well as A reinforced cellulose nanofibril binder comprising cellulose nanofibrils (CNF) and an SGF blend bound to the CNF, the SGF blend comprising sugar fatty acid esters (SFAEs), glycerides, and fatty acid salts; A method comprising:
14. 14. The method of making a molded article according to claim 13, wherein the dehydration is carried out at a temperature above 100°C to achieve a dry content of at least 70% by weight.
15. 14. The method of making a molded article according to claim 13, further comprising coating a surface of the molded article with a barrier formulation comprising a second SGF blend comprising sugar fatty acid esters (SFAEs), glycerides, and fatty acid salts by dipping, spraying, painting, printing, or a combination of any of these processes.
16. A molded article obtainable by the method according to claim 13.
17. 17. The molded article of claim 16, wherein the three-dimensional shape is selected from the group consisting of a bowl, a cup, a plate, a fork, a spoon, and a knife.