AI Technical Summary
The conventional method of manufacturing metal parts from ingots and metal billets is complex, costly, and prone to delays, involving multiple processing steps and transportation, which can disrupt downstream processes.
A method involving covering metal powder with a high melting point material, followed by microwave irradiation to sinter or melt and solidify the metal, allowing for the production of bonded solids through repeated layers of high melting point material and metal powder, with optional pressure application and gas atmospheres.
Enables efficient and cost-effective production of metal solids and bonded structures with improved control over the manufacturing process, reducing complexity and potential delays.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a bonded solid. [Background technology]
[0002] Conventionally, metal solid parts used in daily necessities, home appliances, machine tools, etc. are manufactured by processing ingots, metal billets, etc. The process of processing ingots and metal billets includes various steps and is complicated. In addition, the process of processing ingots and metal billets may span various processors. Therefore, the process of processing ingots and metal billets may include transportation by logistics. Therefore, the process of processing ingots and metal billets is expensive. In addition, in the process of processing ingots and metal billets, if one step is delayed, all downstream steps may be delayed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-158790 A [Patent Document 2] JP 2017-145151 A [Patent Document 3] JP 2009-035776 A [Patent Document 4] JP 2013-216943 A [Patent Document 5] JP 2017-145151 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a method for manufacturing a metal solid by which a metal solid can be easily manufactured. Another object of the present invention is to provide a method for manufacturing a bonded solid by which a metal solid can be easily bonded to a solid, and a method for manufacturing a bonded solid by which solids can be easily connected to each other. [Means for solving the problem]
[0005] According to an aspect of the present invention, there is provided a method for producing a metal solid, comprising: covering at least a portion of a periphery of a metal powder with a high-melting point material having a melting point higher than the melting point of the metal powder; and irradiating the metal powder at least partially surrounded by the high-melting point material with microwaves to heat the metal powder and sinter or melt and solidify the metal powder.
[0006] In the above-mentioned method for producing a metal solid, the steps of covering at least a portion of the periphery of the metal powder with a high melting point material and sintering or melting and solidifying the metal powder may be repeated.
[0007] In the above-mentioned method for producing a metal solid, a layered metal solid may be formed.
[0008] In the above-mentioned method for producing a metal solid, the high melting point material may include a heat insulating material that absorbs microwaves to a lesser extent than the metal powder.
[0009] In the above-described method for producing a metal solid, the high-melting point material may include an absorbing material that absorbs microwaves in at least a part of a temperature range that is lower than the temperature range in which the metal powder absorbs microwaves.
[0010] In the above-mentioned method for producing a metal solid, the high-melting point material may include an insulating material that absorbs microwaves to a lesser extent than the metal powder, and an absorbing material that absorbs microwaves in at least a part of a temperature range that is lower than the temperature range in which the metal powder absorbs microwaves.
[0011] In the above method for producing a metal solid, the high melting point material may contain 1% to 70% by mass of an absorbing material.
[0012] In the above-mentioned method for producing a metal solid, the heat insulating material may include an oxide.
[0013] In the above-mentioned method for producing a metal solid, the heat insulating material may contain at least one selected from the group consisting of aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, and titanium oxide.
[0014] In the above-mentioned method for producing a metal solid, the absorbing material may include a carbon material.
[0015] In the above-mentioned method for producing a metal solid, the absorbing material may include at least one selected from the group consisting of carbon, graphite, silicon carbide, carbon resin, and metal carbide.
[0016] In the above-mentioned method for producing a metal solid, the metal powder may contain a metal.
[0017] In the above-mentioned method for producing a metal solid, the metal powder may contain at least one selected from the group consisting of iron, nickel, copper, gold, silver, aluminum, and cobalt.
[0018] In the above-mentioned method for producing a metal solid, the metal powder may contain a metal compound.
[0019] In the above-mentioned method for producing a metal solid, the metal powder may contain at least one compound selected from the group consisting of iron, nickel, copper, gold, silver, aluminum, and cobalt.
[0020] In the above-mentioned method for producing a metal solid, the metal powder may further contain an alloy component.
[0021] In the above-mentioned method for producing a metal solid, the alloy component may contain at least one selected from the group consisting of silicon, manganese, chromium, nickel, carbon, boron, copper, aluminum, titanium, niobium, vanadium, zinc, and sulfur.
[0022] In the above-mentioned method for producing a metal solid, the metal powder may have an average particle size of 200 μm or less.
[0023] In the above-mentioned method for producing a metal solid, the metal powder may include a metal oxide, and the metal powder may be reduced by irradiating the metal powder with microwaves.
[0024] In the above-mentioned method for producing a metal solid, the metal powder may include a metal oxide, and the metal powder may be sintered by irradiating the metal powder with microwaves.
[0025] In the above-mentioned method for producing a metal solid, the high melting point material may form a mold or a container.
[0026] In the above-mentioned method for producing a metal solid, the metal powder may be in the form of a compact.
[0027] The above-mentioned method for producing a metal solid may further include applying pressure to the metal powder before irradiating the metal powder with microwaves.
[0028] In the above method for producing a metal solid, the pressure may be from 0.1 MPa to 2000 MPa.
[0029] The method for producing a metal solid may further include applying pressure to the metal powder while irradiating the metal powder with microwaves.
[0030] In the above method for producing a metal solid, the pressure may be from 0.1 MPa to 2000 MPa.
[0031] The above-mentioned method for producing a metal solid may further include applying pressure to the metal powder after irradiating the metal powder with microwaves.
[0032] In the above method for producing a metal solid, the pressure may be from 0.1 MPa to 2000 MPa.
[0033] In the above-mentioned method for producing a metal solid, the metal powder may be irradiated with microwaves in an inert gas atmosphere.
[0034] In the above-mentioned method for producing a metal solid, the metal powder may be irradiated with microwaves in a reducing atmosphere.
[0035] In the above-mentioned method for producing a metal solid, the metal powder may contain a metal oxide, and the method may further include reducing the metal oxide before irradiating the metal powder with microwaves.
[0036] In the above-mentioned method for producing a metal solid, covering at least a portion of the periphery of the metal powder with a high-melting point material having a melting point higher than the melting point of the metal powder may include forming a layer of the high-melting point material, forming a recess in the layer of the high-melting point material, and pouring the metal powder into the recess.
[0037] In the above-mentioned method for manufacturing a metal solid, forming a recess in the layer of high melting point material may include hardening a portion of the layer of high melting point material, and removing an unhardened portion of the layer of high melting point material.
[0038] In the above method for producing a metal solid, hardening the portion of the layer of high melting point material may include including a hardenable material in the portion of the layer of high melting point material.
[0039] In the above-mentioned method for producing a metal solid, a part of the layer of high melting point material may be impregnated with a hardenable material.
[0040] In the above-mentioned method for producing a metal solid, a part of the layer of the high melting point material may be hardened by light irradiation.
[0041] According to another aspect of the present invention, there is provided an apparatus for manufacturing a metal solid, comprising: a stage for arranging a metal powder and a high-melting point material covering at least a portion of the periphery of the metal powder and having a melting point higher than that of the metal powder; and a microwave irradiation unit for irradiating microwaves to the metal powder at least partially surrounded by the high-melting point material to heat the metal powder and sinter or melt and solidify the metal powder.
[0042] The above-mentioned metal solid manufacturing apparatus may further include a high-melting point material placement section for placing a high-melting point material on the stage.
[0043] In the above-described metal solid manufacturing apparatus, the high-melting point material placement unit may apply a high-melting point material onto the stage.
[0044] In the above-described metal solid manufacturing apparatus, the high-melting point material placement unit may stack a layer of high-melting point material on the stage.
[0045] The above-mentioned metal solid manufacturing apparatus may further include a hardenable material adding section for adding a hardenable material to at least a portion of the high melting point material.
[0046] The apparatus for producing the metal solid may further include a hardening device for hardening at least a portion of the high melting point material.
[0047] The above-mentioned metal solid manufacturing apparatus may further include an unhardened material removing section for removing the unhardened high melting point material.
[0048] The above-mentioned metal solid manufacturing apparatus may further include a metal powder placement unit for placing metal powder on the stage.
[0049] In the above-described apparatus for manufacturing a metal solid, the metal powder placement unit may apply metal powder onto the stage.
[0050] In the above-described metal solid manufacturing apparatus, the metal powder placement unit may place metal powder in the recessed portion of the high melting point material.
[0051] The above-mentioned metal solid manufacturing apparatus may further include a pressure unit for applying pressure to the metal powder placed on the stage.
[0052] In the above-described apparatus for producing a metal solid, the pressurizing unit may apply pressure to the metal powder before the microwave irradiating unit irradiates the metal powder with microwaves.
[0053] In the above-described apparatus for producing a metal solid, the pressurizing unit may apply pressure to the metal powder while the microwave irradiating unit irradiates the metal powder with microwaves.
[0054] In the above-described apparatus for producing a metal solid, the pressurizing unit may apply pressure to the metal powder after the microwave irradiating unit irradiates the metal powder with microwaves.
[0055] The above-mentioned metal solid manufacturing apparatus may further include an inert gas supply unit for supplying an inert gas to the metal powder.
[0056] The above-mentioned metal solid manufacturing apparatus may further include a reducing gas supply unit for supplying a reducing gas to the metal powder.
[0057] The above-mentioned metal solid manufacturing apparatus may further include a high melting point material placement unit for placing a high melting point material on the stage, and a metal powder placement unit for placing a metal powder on the stage, (1) the high melting point material placement unit and the metal powder placement unit place the metal powder surrounded by the high melting point material on the stage, and (2) the microwave irradiation unit sinters or melts and solidifies the metal powder. The metal solid manufacturing apparatus may repeat a combination of (1) and (2).
[0058] In the above-mentioned metal solid manufacturing apparatus, the metal powder may contain a metal oxide, and the apparatus may further include a reduction device that reduces the metal oxide before the microwave irradiation unit irradiates the metal powder with microwaves.
[0059] According to an aspect of the present invention, there is provided a method for producing a bonded solid, the method including: disposing a metal powder on a solid; covering at least a portion of the periphery of the metal powder with a high melting point material having a melting point higher than the melting point of the metal powder; and irradiating the metal powder at least partially surrounded by the high melting point material with microwaves to heat the metal powder and sinter or melt and solidify the metal powder, thereby forming a metal solid on the solid.
[0060] The above-mentioned method for producing a bonded solid may further include arranging a metal powder on the metal solid, covering at least a portion of the periphery of the metal powder on the metal solid with a high melting point material, and irradiating the metal powder on the metal solid with microwaves so as to heat the metal powder and sinter or melt and solidify the metal powder, thereby forming an additional metal solid on the metal solid.
[0061] In the above method for producing a bonded solid, a laminated metal solid may be formed.
[0062] In the above-mentioned method for producing a bonded solid, the high melting point material may include a heat insulating material that absorbs microwaves to a lesser extent than the metal powder.
[0063] In the above-mentioned method for producing a bound solid, the high melting point material may include an absorbing material that absorbs microwaves in at least a part of a temperature range that is lower than the temperature range in which the metal powder absorbs microwaves.
[0064] In the above-mentioned method for producing a bonded solid, the high-melting point material may include an insulating material that absorbs microwaves to a lesser extent than the metal powder, and an absorbing material that absorbs microwaves in at least a part of a temperature range that is lower than the temperature range in which the metal powder absorbs microwaves.
[0065] In the above-mentioned method for producing a binding solid, the high melting point material may contain 1% to 70% by weight of an absorbing material.
[0066] In the above-mentioned method for producing a bonding solid, the heat insulating material may contain an oxide.
[0067] In the above-mentioned method for producing a bonding solid, the heat insulating material may contain at least one selected from the group consisting of aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, and titanium oxide.
[0068] The absorbent material may include a carbon material.
[0069] In the above-mentioned method for producing a bonded solid, the absorbing material may include at least one selected from the group consisting of carbon, graphite, silicon carbide, carbon resin, and metal carbide.
[0070] In the above-mentioned method for producing a bonded solid, the metal powder may contain a metal.
[0071] In the above-mentioned method for producing a bonded solid, the metal powder may contain at least one selected from the group consisting of iron, nickel, copper, gold, silver, aluminum, and cobalt.
[0072] In the above-mentioned method for producing a bonded solid, the metal powder may contain a metal compound.
[0073] In the above-mentioned method for producing a bonded solid, the metal powder may contain at least one compound selected from the group consisting of iron, nickel, copper, gold, silver, aluminum, and cobalt.
[0074] In the above-mentioned method for producing a bonded solid, the metal powder may further contain an alloy component.
[0075] In the above-mentioned method for producing a bonded solid, the alloy component may include at least one selected from the group consisting of silicon, manganese, chromium, nickel, carbon, boron, copper, aluminum, titanium, niobium, vanadium, zinc, and sulfur.
[0076] In the above-mentioned method for producing a bonded solid, the metal powder may have an average particle size of 200 μm or less.
[0077] In the above-mentioned method for producing a bonded solid, the metal powder may include a metal oxide, and the metal powder may be reduced by irradiating the metal powder with microwaves.
[0078] In the above-mentioned method for producing a bonded solid, the metal powder may include a metal oxide, and the metal powder may be sintered by irradiating the metal powder with microwaves.
[0079] In the above-mentioned method for producing a bound solid, the high melting point material may form a mold or a container.
[0080] In the above-mentioned method for producing a bonded solid, the metal powder may be in the form of a compact.
[0081] The method for producing the bonded solid may further include applying pressure to the metal powder before irradiating the metal powder with microwaves.
[0082] In the above method for producing a bound solid, the pressure may be from 0.1 MPa to 2000 MPa.
[0083] The above-mentioned method for producing a bonded solid may further include applying pressure to the metal powder while irradiating the metal powder with microwaves.
[0084] In the above method for producing a bound solid, the pressure may be from 0.1 MPa to 2000 MPa.
[0085] The method for producing the bonded solid may further include applying pressure to the metal powder after irradiating the metal powder with microwaves.
[0086] In the above method for producing a bound solid, the pressure may be from 0.1 MPa to 2000 MPa.
[0087] In the above-mentioned method for producing a bonded solid, the metal powder may be irradiated with microwaves in an inert gas atmosphere.
[0088] In the above-mentioned method for producing a bonded solid, the metal powder may be irradiated with microwaves in a reducing atmosphere.
[0089] In the above-mentioned method for producing a bound solid, the metal powder may contain a metal oxide, and the method may further include reducing the metal oxide before irradiating the metal powder with microwaves.
[0090] In the above-mentioned method for manufacturing a bonded solid, covering at least a portion of the periphery of the metal powder with a high-melting point material having a melting point higher than the melting point of the metal powder may include forming a layer of the high-melting point material, forming a recess in the layer of the high-melting point material, and placing the solid and the metal powder in the recess.
[0091] In the above-mentioned method for manufacturing a bonded solid, forming a recess in the layer of high melting point material may include hardening a portion of the layer of high melting point material and removing an unhardened portion of the layer of high melting point material.
[0092] In the above method of producing a bonded solid, hardening the portion of the layer of high melting point material may include including a hardenable material in the portion of the layer of high melting point material.
[0093] In the above-mentioned method for producing the bonded solid, a part of the layer of the high melting point material may be impregnated with a hardenable material.
[0094] In the above-mentioned method for producing a bonded solid, a part of the layer of the high melting point material may be hardened by light irradiation.
[0095] According to an aspect of the present invention, there is provided a method for manufacturing a bonded solid, the method including: placing a bonding metal between a first solid and a second solid; covering at least a portion of the periphery of the bonding metal with a high melting point material having a melting point higher than that of the bonding metal; and applying microwaves to the bonding metal having at least a portion of its periphery covered with the high melting point material to heat the bonding metal and sinter or melt and solidify the bonding metal, thereby bonding the first solid and the second solid.
[0096] In the above-mentioned method for producing a bonded solid, the bonding metal may be in the form of a powder.
[0097] In the above-mentioned method for producing a bonded solid, the bonding metal may be a solid.
[0098] In the above-mentioned method for producing a bonded solid, the bonding metal may be liquid.
[0099] In the above-mentioned method for producing a bonding solid, the high melting point material may include a heat insulating material that absorbs microwaves to a lesser extent than the bonding metal.
[0100] In the above-mentioned method for producing a bonding solid, the high melting point material may contain an absorbing material that absorbs microwaves in at least a part of a temperature range that is lower than the temperature range in which the bonding metal absorbs microwaves.
[0101] In the above-mentioned method for producing a bonded solid, the high-melting point material may include an insulating material that absorbs microwaves to a lesser extent than the bonding metal, and an absorbing material that absorbs microwaves in at least a part of a temperature range that is lower than the temperature range in which the bonding metal absorbs microwaves.
[0102] In the above-mentioned method for producing a binding solid, the high melting point material may contain 1% to 70% by weight of an absorbing material.
[0103] In the above-mentioned method for producing a bonding solid, the heat insulating material may contain an oxide.
[0104] In the above-mentioned method for producing a bonding solid, the heat insulating material may contain at least one selected from the group consisting of aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, and titanium oxide.
[0105] In the above-mentioned method for producing a bound solid, the absorbent material may include a carbon material.
[0106] In the above-mentioned method for producing a bonded solid, the absorbing material may include at least one selected from the group consisting of carbon, graphite, silicon carbide, carbon resin, and metal carbide.
[0107] In the above-mentioned method for producing a bonded solid, the bonding metal may contain a metal.
[0108] In the above-mentioned method for producing a bonded solid, the binding metal may contain at least one selected from the group consisting of iron, nickel, copper, gold, silver, aluminum, and cobalt.
[0109] In the above-mentioned method for producing a bonded solid, the bonding metal may include a metal compound.
[0110] In the above-mentioned method for producing a bonded solid, the binding metal may contain at least one compound selected from the group consisting of iron, nickel, copper, gold, silver, aluminum, and cobalt.
[0111] In the above-mentioned method for producing a bonded solid, the bonding metal may further contain an alloy component.
[0112] In the above-mentioned method for producing a bonded solid, the alloy component may include at least one selected from the group consisting of silicon, manganese, chromium, nickel, carbon, boron, copper, aluminum, titanium, niobium, vanadium, zinc, and sulfur.
[0113] In the above-mentioned method for producing a bonded solid, the binding metal may be in the form of a powder, and the average particle size of the binding metal may be 200 μm or less.
[0114] In the above-mentioned method for producing a bonded solid, the bonding metal may include a metal oxide, and the bonding metal may be reduced by irradiating the bonding metal with microwaves.
[0115] In the above-mentioned method for producing a bonded solid, the bonding metal may include a metal oxide, and the bonding metal may be sintered by irradiating the bonding metal with microwaves.
[0116] In the above-mentioned method for producing a bound solid, the high melting point material may form a mold or a container.
[0117] In the above-mentioned method for producing a bonded solid, the bonding metal may be in the form of a compact.
[0118] The method for producing the bonded solid may further include applying pressure to the bonding metal before irradiating the bonding metal with microwaves.
[0119] In the above method for producing a bound solid, the pressure may be from 0.1 MPa to 2000 MPa.
[0120] The method for producing the bonded solid may further include applying pressure to the metal powder while the metal powder is being irradiated with microwaves.
[0121] In the above method for producing a bound solid, the pressure may be from 0.1 MPa to 2000 MPa.
[0122] The method for producing the bonded solid may further include applying pressure to the bonding metal after irradiating the bonding metal with microwaves.
[0123] In the above method for producing a bound solid, the pressure may be from 0.1 MPa to 2000 MPa.
[0124] In the above-mentioned method for producing a bonded solid, the bonding metal may be irradiated with microwaves in an inert gas atmosphere.
[0125] In the above-mentioned method for producing a bonded solid, the bonding metal may be irradiated with microwaves in a reducing atmosphere.
[0126] In the above-mentioned method for producing a bonded solid, the bonding metal may contain a metal oxide, and the method may further include reducing the metal oxide before irradiating the bonding metal with microwaves.
[0127] In the above-mentioned method for manufacturing the bonding solid, covering at least a portion of the periphery of the bonding metal with a high-melting point material having a melting point higher than that of the bonding metal may include forming a layer of the high-melting point material, forming a recess in the layer of the high-melting point material, and placing the first and second solids and the bonding metal in the recess.
[0128] In the above-mentioned method for manufacturing a bonded solid, forming a recess in the layer of high melting point material may include hardening a portion of the layer of high melting point material and removing an unhardened portion of the layer of high melting point material.
[0129] In the above method of producing a bonded solid, hardening the portion of the layer of high melting point material may include including a hardenable material in the portion of the layer of high melting point material.
[0130] In the above-mentioned method for producing the bonded solid, a part of the layer of the high melting point material may be impregnated with a hardenable material.
[0131] In the above-mentioned method for producing a bonded solid, a part of the layer of the high melting point material may be hardened by light irradiation. Effect of the Invention
[0132] According to the present invention, it is possible to provide a method for manufacturing a metal solid, which allows a metal solid to be easily manufactured. Also, according to the present invention, it is possible to provide a method for manufacturing a bonded solid, which allows a metal solid to be easily bonded to a solid, and a method for manufacturing a bonded solid, which allows solids to be easily connected to each other. [Brief description of the drawings]
[0133] [Figure 1] FIG. 1 is a schematic perspective view of a manufacturing apparatus for a metal solid according to the first embodiment. [Diagram 2] FIG. 2 is a schematic process diagram of the method for producing a metal solid according to the first embodiment. [Diagram 3] FIG. 3 is a schematic process diagram of the method for producing a metal solid according to the first embodiment. [Figure 4] FIG. 4 is a schematic process diagram of the method for producing a metal solid according to the first embodiment. [Diagram 5] FIG. 5 is a schematic process diagram of the method for producing a metal solid according to the first embodiment. [Figure 6] FIG. 6 is a schematic process diagram of the method for producing a metal solid according to the first embodiment. [Figure 7] FIG. 7 is a schematic process diagram of the method for producing a metal solid according to the first embodiment. [Figure 8] FIG. 8 is a schematic perspective view of the manufacturing apparatus for a metal solid according to the first embodiment. [Figure 9] FIG. 9 is a schematic perspective view of the manufacturing apparatus for a metal solid according to the first embodiment. [Figure 10] FIG. 10 is a schematic perspective view of the manufacturing apparatus for a metal solid according to the first embodiment. [Figure 11] FIG. 11 is a photograph of the metal solid obtained in Example 1. [Figure 12] FIG. 12 is a photograph of the metal solid obtained in Example 2. [Figure 13] FIG. 13 is a photograph of the metal solid obtained in Example 3. [Figure 14] FIG. 14 is a photograph of the metal solid obtained in Example 4. [Figure 15] FIG. 15 is a photograph of the solid coated with the metal film obtained in Example 5. [Figure 16] FIG. 16 is a photograph of the solid coated with the metal film obtained in Example 6. [Figure 17] FIG. 17 is a photograph of the solid coated with the metal film obtained in Example 7. [Figure 18] FIG. 18 is a photograph of the bonded solid obtained in Example 8. [Figure 19] FIG. 19 is a photograph of the bonded solid obtained in Example 10. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0134] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description of the drawings, the same or similar parts are denoted by the same or similar reference numerals. However, the drawings are schematic. Therefore, specific dimensions, etc. should be judged in light of the following description. In addition, it goes without saying that the drawings include parts with different dimensional relationships and ratios.
[0135] (First embodiment) The method for producing a metal solid according to the first embodiment includes covering at least a part of the periphery of a metal powder with a high-melting-point material having a melting point higher than that of the metal powder, and irradiating microwaves to the metal powder at least partially covered with the high-melting-point material to heat the metal powder and sinter or melt and solidify the metal powder. The microwaves are, for example, electromagnetic waves with a frequency of 300 MHz or more and 30 GHz or less. It is preferable that the metal powder and the high-melting-point material are in close contact with each other in the part of the metal powder covered with the high-melting-point material.
[0136] The material of the metal powder may include a metal element or a metal compound such as an alloy. Examples of metals include iron (Fe), nickel (Ni), copper (Cu), gold (Au), silver (Ag), aluminum (Al), and cobalt (Co). The sintering temperature of iron (Fe) is, for example, 1200°C. The melting point of iron (Fe) is 1538°C. The sintering temperature of nickel (Ni) is, for example, 1200°C. The melting point of nickel (Ni) is 1495°C. The sintering temperature of copper (Cu) is, for example, 800°C. The melting point of copper (Cu) is 1085°C. The sintering temperature of gold (Au) is, for example, 800°C. The melting point of gold (Au) is 1064°C. The sintering temperature of silver (Ag) is, for example, 750°C. The melting point of silver (Ag) is 962°C. The sintering temperature of aluminum (Al) is, for example, 500°C. The melting point of aluminum (Al) is 660°C. The sintering temperature of cobalt (Co) is, for example, 1100°C. The melting point of cobalt (Co) is 1455°C.
[0137] The material of the metal powder may contain one type of metal or may contain multiple types of metals. Examples of metal compounds include, but are not limited to, alloys of multiple metal elements, alloys of metal elements and nonmetal elements, metal oxides, metal hydroxides, metal chlorides, metal carbides, metal borides, and metal sulfides. The metal powder may contain, as alloy components, for example, silicon (Si), manganese (Mn), chromium (Cr), nickel (Ni), carbon (C), boron (B), copper (Cu), aluminum (Al), titanium (Ti), niobium (Nb), vanadium (V), zinc (Zn), and sulfur (S). The material of the metal powder preferably has better microwave absorption characteristics than the surrounding high-melting point materials. This makes the metal powder more easily heated by microwaves than the surrounding high-melting point materials.
[0138] The average particle diameter of the metal powder is, for example, 200 μm or less, 190 μm or less, or 180 μm or less. The average particle diameter of the metal powder is, for example, the median diameter D 50 Preferably, the particle size distribution of the metal powder is D 10 / D 50 >0.5 and D 50 / D 90 If the average particle size of the metal powder is 200 μm or less, the metal powder tends to easily absorb microwaves.
[0139] The high melting point material may include a heat insulating material that is more microwave permeable than the metal powder and absorbs microwaves less than the metal powder. The heat insulating material has a melting point higher than that of the metal powder. Since the heat insulating material absorbs microwaves less, it generates less heat even when irradiated with microwaves, and thus exhibits a heat insulating effect. Furthermore, since the heat insulating material has a melting point higher than that of the metal powder, its shape is stable even when irradiated with microwaves. Therefore, even while the metal powder irradiated with microwaves is sintered or melted, the high melting point material including the heat insulating material can maintain its shape.
[0140] The heat insulating material may include a metal oxide or a metalloid oxide. Examples of metal and metalloid oxides include, but are not limited to, aluminum oxide (Al2O3), silicon oxide (SiO2), magnesium oxide (MgO), zirconium oxide (ZrO2), and titanium oxide (TiO2). For example, the melting point of aluminum oxide (Al2O3) is 2072°C. The melting point of silicon oxide (SiO2) is 1710°C. The melting point of magnesium oxide (MgO) is 2852°C. The heat insulating material may be a compound of these.
[0141] The high melting point material may include an absorbing material that absorbs microwaves in at least a part of a temperature range that is lower than the temperature range in which the metal powder absorbs microwaves. The absorbing material has a melting point higher than the melting point of the metal powder. At least a part of the temperature range in which the absorbing material absorbs microwaves is lower than the temperature range in which the metal powder absorbs microwaves. The temperature range in which the metal powder absorbs microwaves is, for example, 300°C to 1200°C, 450°C to 1100°C, or 600°C to 800°C. The temperature range in which the absorbing material absorbs microwaves is, for example, 100°C to 1000°C, 250°C to 900°C, or 400°C to 600°C.
[0142] It is preferable that at least a part of the temperature range in which the absorbing material absorbs microwaves overlaps with the temperature range in which the metal powder absorbs microwaves. The absorbing material absorbs microwaves in a temperature range at least partially lower than the temperature range in which the metal powder absorbs microwaves, and therefore generates heat faster than the metal powder. Therefore, the absorbing material can heat the metal powder before it reaches the temperature range in which the metal powder absorbs microwaves. Therefore, when the high-melting point material contains the absorbing material, the temperature of the metal powder reaches the temperature range in which the microwaves are absorbed more quickly, and it is possible to shorten the heating time of the metal powder. In addition, since the absorbing material absorbs microwaves in a temperature range at least partially lower than the temperature range in which the metal powder absorbs microwaves, it is possible to suppress the high-melting point material from being heated more than necessary. Therefore, even while the metal powder irradiated with microwaves is sintered or melted, the high-melting point material containing the absorbing material can have a stable shape.
[0143] The absorbing material includes, for example, a carbon material. Examples of the carbon material include, but are not limited to, carbon black, amorphous carbon, graphite, silicon carbide, carbon resin, and metal carbide. The absorbing material may be a compound of these. It is preferable that the absorbing material does not contain a volatile component. By not containing a volatile component in the absorbing material, it is possible to prevent the microwave from being absorbed by the volatile component.
[0144] The high melting point material may include a reducing material that reduces the metal powder. The reducing material has a melting point higher than the melting point of the metal powder. Examples of reducing materials include carbon and silicon carbide. Carbon materials used as absorbent materials may also function as reducing materials.
[0145] The high melting point material may be composed of only an insulating material, only an absorbing material, only a reducing material, or a combination of these. In addition, the insulating material, the absorbing material, and the reducing material may have overlapping properties and functions. For example, a carbon material functions both as an absorbing material and as a reducing material.
[0146] When the high melting point material includes a heat insulating material and an absorbent material, the mass ratio of the heat insulating material to the absorbent material is preferably 1:1, or the mass ratio of the heat insulating material is greater than the mass ratio of the absorbent material. For example, the mass ratio of the absorbent material in the high melting point material is 1 mass% or more, 2 mass% or more, or 5 mass% or more, and 70 mass% or less, 50 mass% or less, 40 mass% or less, 30 mass% or less, 20 mass% or less, or 10 mass% or less. By making the mass ratio of the absorbent material in the high melting point material 50 mass% or less, it is possible to ensure the microwave permeability of the high melting point material and to make the sintering or melting solidification speed of the metal powder appropriate.
[0147] When the metal powder irradiated with microwaves is a green compact, the high melting point material may be a solid powder or the like and have fluidity. After forming the metal powder into a green compact into a desired three-dimensional shape, at least a part of the green compact is covered with a high melting point material, and then the green compact covered with the high melting point material is irradiated with microwaves, whereby the green compact is sintered and a metal solid of the desired shape is produced by metallurgy. Alternatively, the green compact covered with the high melting point material is irradiated with microwaves, and then cooled, whereby the green compact is melted and solidified, and a metal solid of the desired shape is produced. The green compact may be entirely covered with a high melting point material. The thickness, volume, etc. of the high melting point material covering the green compact can be appropriately set based on the transmittance of microwaves.
[0148] When the metal powder is molded into a green compact, a pressure of, for example, 0.1 MPa or more, 1 MPa or more, 100 MPa or more, or 200 MPa or more, and 2000 MPa or less, 1900 MPa or less, or 1800 MPa or less may be applied to the metal powder. By applying pressure, the produced metal solid tends to become dense. Examples of the pressing method include uniaxial molding, cold isostatic pressing (CIP) molding, hot isostatic pressing (HIP) molding, and roller pressing.
[0149] When the metal powder irradiated with microwaves has fluidity, the high melting point material may be in the form of a solid such as a mold or a container. For example, the entire metal powder irradiated with microwaves may be a powder, or a part of the metal powder may be a compact. The metal powder is placed in a recess of a mold or container corresponding to a desired three-dimensional shape formed by a high melting point material, at least a part of the metal powder is covered with a mold or container formed by a high melting point material, and then microwaves are irradiated to the metal powder covered with the mold or container formed by the high melting point material, whereby the metal powder is sintered and a metal solid of a desired shape is produced. In the present disclosure, the recess includes a through hole. Alternatively, the metal powder covered with a high melting point material is irradiated with microwaves, and then cooled, whereby the compact is melted and solidified, and a metal solid of a desired shape is produced. The entire periphery of the metal powder may be covered with a mold or container formed by a high melting point material. The thickness, volume, etc. of the mold or container formed by the high melting point material that covers the compact can be appropriately set based on the permeability of microwaves. The composition of the metal powder placed in the mold or container of the high melting point material may be changed depending on the position. For example, the type of metal constituting the metal powder or the alloy composition of the metal powder may be changed depending on the position.
[0150] After placing the metal powder in a mold or container made of a high melting point material, a pressure of, for example, 0.1 MPa or more, 1 MPa or more, 100 MPa or more, or 200 MPa or more, and 2000 MPa or less, 1900 MPa or less, or 1800 MPa or less may be applied to the metal powder before irradiating with microwaves. By applying pressure, the produced metal solid tends to become dense. Examples of the pressing method include uniaxial molding, cold isostatic pressing (CIP) molding, hot isostatic pressing (HIP) molding, and roller pressing.
[0151] When the high melting point material is solidified into a mold or a container, a curable material such as a photocurable resin may be dispersed in the high melting point material, and the mixture of the high melting point material and the photocurable resin may be irradiated with light to cure the mixture of the high melting point material and the photocurable resin. When the photocurable resin is an ultraviolet curable resin, the mixture of the high melting point material and the photocurable resin is irradiated with ultraviolet light. The light irradiation time is, for example, 1 hour or more, 2 hours or more, or 3 hours or more. The mass ratio of the photocurable resin in the mixture of the high melting point material and the photocurable resin is, for example, 1% or more, 2% or more, or 3% or more, and 10% or less, 9% or less, or 8% or less. By setting the mass ratio of the photocurable resin in the mixture of the high melting point material and the photocurable resin to 1% or more and 10% or less, it may be possible to ensure hardness and microwave transparency. The curable material may be thermosetting. In this case, the mixture of the high melting point material and the thermosetting material may be heated to harden the mixture of the high melting point material and the thermosetting material.
[0152] When both the metal powder and the high melting point material to be irradiated with microwaves are powders, the metal powder and the high melting point material may be laminated, and then the laminated metal powder and the high melting point material may be irradiated with microwaves. After laminating the metal powder and the high melting point material, a pressure of, for example, 0.1 MPa or more, 1 MPa or more, 100 MPa or more, or 200 MPa or more, and 2000 MPa or less, 1900 MPa or less, or 1800 MPa or less may be applied to the laminated metal powder and the high melting point material before irradiating with microwaves. By applying pressure, the produced metal solid tends to become dense. Examples of the pressing method include uniaxial molding, cold isostatic pressing (CIP) molding, hot isostatic pressing (HIP) molding, and roller pressing.
[0153] Pressure may be applied to the metal powder during the microwave irradiation, for example, at least 0.1 MPa, at least 1 MPa, at least 100 MPa, or at least 200 MPa, and at most 2000 MPa, at most 1900 MPa, or at most 1800 MPa.
[0154] After the metal powder is sintered or melted and solidified, pressure may be applied to the formed metal solid. In this case, it is preferable to apply pressure when the metal solid has heat and before it is cooled to the ambient temperature and in a state where the temperature is higher than the ambient temperature. The pressure applied is, for example, 0.1 MPa, 1 MPa or more, 100 MPa or more, or 200 MPa or more, and 2000 MPa or less, 1900 MPa or less, or 1800 MPa or less. By applying pressure, the produced metal solid tends to become dense. Examples of the pressing method include uniaxial molding, cold isostatic pressing (CIP) molding, hot isostatic pressing (HIP) molding, and roller pressing.
[0155] When the metal powder contains a metal oxide, the metal oxide is reduced by irradiating microwaves to the metal powder covered with a high melting point material containing a reducing material. When the metal powder is heated to a temperature equal to or higher than the sintering temperature and close to the melting point, a dense sintered body is easily obtained. Therefore, the metal powder may be heated to 1400°C or higher, or 1500°C or higher, by microwaves. When the metal powder is melted and solidified, it is sufficient to heat the metal powder to a temperature equal to or higher than the melting point. Note that the oxide powder of the metal may be reduced in advance before irradiating the metal powder with microwaves. For example, the metal oxide powder can be reduced by mixing the metal oxide powder with a carbon powder and heating the mixture of the metal oxide powder and the carbon powder. The reduced metal powder can be separated from the carbon powder, for example, by a magnet.
[0156] Heating the metal powder may be performed under an inert gas atmosphere. Examples of the inert gas include argon (Ar) and helium (He). Heating the metal powder may also be performed under a neutral gas atmosphere. Examples of the neutral gas include nitrogen (N2), dry hydrogen (H2), and ammonia (NH3). Heating the metal powder may also be performed under a reducing atmosphere. Examples of the reducing gas that provides the reducing atmosphere include hydrogen (H2), carbon monoxide (CO), and hydrocarbon gases (CH4, C3H8, C4H 10When the high melting point material forms a mold or a container, an inert gas, a neutral gas, or a reducing gas may be supplied to the inside of the mold or container formed by the high melting point material.
[0157] A laminated metal solid may be formed by repeatedly covering at least a part of the periphery of the metal powder with a high melting point material and sintering or melting and solidifying the metal powder. The metal solid obtained by the above method may be polished. The metal solid obtained by the above method may be used as a core, for example, and a metal powder may be arranged around it, and a high melting point material may be arranged around the metal powder, and the microwave irradiation may be repeated. This makes it possible to scale up the metal solid. The compositions of the metal powder and the high melting point material may be changed each time microwaves are irradiated. For example, the alloy components of the metal powder may be changed each time microwaves are irradiated.
[0158] 1, the metal solid manufacturing apparatus according to the first embodiment includes a stage 10 on which a metal powder and a high-melting point material that covers at least a part of the periphery of the metal powder and has a melting point higher than that of the metal powder are disposed, and a microwave irradiation unit 20 for irradiating microwaves to the metal powder at least a part of which is covered with the high-melting point material to heat the metal powder and sinter or melt and solidify the metal powder. The metal solid manufacturing apparatus according to the first embodiment is capable of carrying out, for example, the above-described method for manufacturing a metal solid according to the first embodiment.
[0159] The stage 10 is not particularly limited as long as it is capable of arranging the metal powder and the high melting point material. The stage 10 may be movable in three mutually perpendicular axial directions. For example, the stage 10 may be movable in the gravity direction and the horizontal direction.
[0160] The manufacturing apparatus for a metal solid according to the first embodiment may further include a high melting point material arrangement unit 31 that arranges a high melting point material on the stage 10. The high melting point material arrangement unit 31 may apply a high melting point material on the stage 10. The high melting point material arrangement unit 31 may form a layer of the high melting point material on the stage 10. The high melting point material arrangement unit 31 may be movable in three axial directions perpendicular to each other. For example, the high melting point material arrangement unit 31 may be movable in the gravity direction and the horizontal direction. For example, as shown in FIG. 2(a) to FIG. 2(c), the high melting point material arrangement unit 31 may apply a powder of high melting point material on the stage 10 while moving on the stage 10, and form a layer 101 of the high melting point material on the stage 10.
[0161] As shown in FIG. 1, the manufacturing apparatus for a metal solid according to the first embodiment may further include a hardenable material adding section 32 that adds a hardenable material to at least a part of the high melting point material. The hardenable material adding section 32 adds the hardenable material to a part of the high melting point material to be hardened, and does not add the hardenable material to a part of the high melting point material not to be hardened. The hardenable material may be, for example, a liquid, and the hardenable material adding section 32 may impregnate the part of the high melting point material to be hardened with the hardenable material. The hardenable material adding section 32 may be movable in three axial directions perpendicular to each other. For example, the hardenable material adding section 32 may be movable in the gravity direction and the horizontal direction. 3(a) and 3(b), the curable material adding unit 32 may apply the curable material to the high-melting point material layer 101 while patterning it, while moving over the high-melting point material layer 101 on the stage 10, and add the curable material to the part of the high-melting point material layer 101 to be cured without adding the curable material to the part 102 of the high-melting point material layer 101 to be cured. The curable material adding unit 32 may include, for example, an inkjet nozzle, and add the curable material to the high-melting point material by a binder jetting method.
[0162] The high melting point material arrangement portion 31 and the hardenable material addition portion 32 may be integrated together.
[0163] As shown in FIG. 1, the manufacturing apparatus for the metal solid according to the first embodiment may further include a curing device 40 for curing at least a part of the high melting point material. When the high melting point material includes a photocurable material, the curing device 40 is a light source. When the high melting point material includes a thermosetting material, the curing device 40 is a heat source. The curing device 40 may be movable in three axial directions perpendicular to each other. For example, the curing device 40 may be movable in the gravity direction and the horizontal direction. As shown in FIG. 3(c), the curing device 40 irradiates the layer 101 of the high melting point material with energy required for curing the curable material to cure at least a part of the layer 101 of the high melting point material. The curing device 40 may irradiate the entire surface of the layer 101 of the high melting point material with energy at once, or may irradiate the layer 101 of the high melting point material with energy while scanning the layer 101 of the high melting point material.
[0164] As shown in Fig. 1, the manufacturing apparatus for a metal solid according to the first embodiment may further include an unhardened material removing unit 50 for removing unhardened high melting point material. For example, as shown in Fig. 4(a) and Fig. 4(b), the unhardened material removing unit 50 may apply air pressure to an unhardened, powdery portion 102 of a layer 101 of high melting point material to remove the unhardened, powdery portion 102 from the layer 101 of high melting point material, thereby forming a recess 103 in the layer 101 of high melting point material.
[0165] As shown in FIG. 1, the manufacturing apparatus for a metal solid according to the first embodiment may further include a metal powder placement unit 33 that places metal powder on the stage 10. A recoater can be used as the metal powder placement unit 33. The metal powder placement unit 33 may apply metal powder onto the stage 10. The metal powder placement unit 33 may be movable in three axial directions perpendicular to each other. For example, the metal powder placement unit 33 may be movable in the direction of gravity and in the horizontal direction. For example, as shown in FIG. 5(a) and FIG. 5(b), the metal powder placement unit 33 may place metal powder 200 in the recess 103 of the layer 101 of high melting point material on the stage 10. The metal powder placed on the surface of the part of the layer 101 of high melting point material on the stage 10 where the recess 103 is not formed may be removed by a roller, a brush, or the like.
[0166] The high melting point material arrangement section 31 and the metal powder arrangement section 33 may be integrated together. The hardenable material addition section 32 and the metal powder arrangement section 33 may be integrated together. The high melting point material arrangement section 31, the hardenable material addition section 32, and the metal powder arrangement section 33 may be integrated together.
[0167] As shown in FIG. 1, the manufacturing apparatus for a metal solid according to the first embodiment may further include a pressurizing unit 60 that applies pressure to the metal powder arranged on the stage 10. As shown in FIG. 5(c), the pressurizing unit 60 applies pressure to the metal powder 200 before it is irradiated with microwaves. Pressurizing methods include uniaxial molding, cold isostatic pressing (CIP) molding, hot isostatic pressing (HIP) molding, and roller pressurizing. In the case of roller pressurizing, a pressurizing method may be selected in which the pressurizing tip of the pressurizing unit 60 is a roller type, and the stage 10 is slid while the roller is pressed against the stage 10.
[0168] For example, as shown in FIG. 6, the microwave irradiation unit 20 irradiates microwaves to the metal powder 200 arranged in the recess 103 of the layer 101 of the high melting point material on the stage 10. The microwave irradiation unit 20 may irradiate the entire surface of the metal powder 200 with microwaves at once, or may irradiate the metal powder 200 while scanning it. The manufacturing apparatus for a metal solid according to the first embodiment may further include an inert gas supply unit that supplies an inert gas to the metal powder. The inert gas supply unit supplies an inert gas to the periphery of the metal powder 200 at least while the metal powder 200 is irradiated with microwaves. The manufacturing apparatus for a metal solid according to the first embodiment may further include a reduction gas supply unit that supplies a reduction gas to the metal powder. The reduction gas supply unit supplies a reduction gas to the periphery of the metal powder 200 at least while the metal powder 200 is irradiated with microwaves. The manufacturing apparatus for a metal solid according to the first embodiment may further include a neutral gas supply unit that supplies a reduction gas to the metal powder. The neutral gas supply unit supplies neutral gas to the surroundings of the metal powder 200 at least while the metal powder 200 is irradiated with microwaves. The inert gas supply unit and the reducing gas supply unit may be integrated together. The inert gas supply unit and the neutral gas supply unit may be integrated together. The reducing gas supply unit and the neutral gas supply unit may be integrated together.
[0169] As shown in FIG. 1, the manufacturing apparatus for a metal solid according to the first embodiment may include a thermometer 71 for measuring the temperature of the metal powder arranged on the stage 10. A radiation thermometer may be used as the thermometer 71. The radiation thermometer measures the temperature of the metal powder based on the emissivity of the material of the metal powder. The thermometer 71 may also measure the temperature of the high melting point material. The microwaves irradiated by the microwave irradiator 20 may be controlled based on the temperature of the metal powder measured by the thermometer 71. The manufacturing apparatus for a metal solid according to the first embodiment may also include a microwave detector 72 for detecting the microwaves irradiated by the microwave irradiator 20. The microwaves irradiated by the microwave irradiator 20 may be controlled based on the characteristics of the microwaves detected by the microwave detector 72.
[0170] 1 may apply pressure to the metal powder 200 after the metal powder 200 is irradiated with microwaves. Pressurizing methods include uniaxial molding, cold isostatic pressing (CIP) molding, hot isostatic pressing (HIP) molding, and roller pressing. In the case of roller pressing, a pressing method may be selected in which the pressing tip of the pressing part 60 is a roller type, and the stage 10 is slid while the roller is pressed against the stage 10.
[0171] The metal powder 200 placed in the recess 103 of the layer 101 of the high melting point material on the stage 10 shown in Fig. 6 and irradiated with microwaves is then cooled and sintered or melted and solidified into a metal solid. Note that the metal powder 200 near the edge of the recess 103 of the layer 101 of the high melting point material tends to be easily heated. Therefore, the mass ratio of the absorbing material contained in the high melting point material near the edge of the recess 103 may be lower than in other parts.
[0172] The stage 10, microwave irradiation unit 20, and the like of the metal solid manufacturing apparatus according to the first embodiment may be housed in a housing.
[0173] The metal solid manufacturing apparatus according to the first embodiment may repeatedly form a layer 101 of high melting point material surrounding a metal powder on the sintered or melted and solidified metal solid and a layer 101 of high melting point material surrounding the metal solid, and sinter or melt and solidify the metal powder. This allows the metal solids to be stacked and a thick metal solid to be manufactured, even if the thickness of the metal solid formed by one microwave irradiation is thin. By changing the shape of the recesses formed in the layer 101 of high melting point material each time the layer 101 of high melting point material surrounding the metal powder is formed, a metal solid having a complex three-dimensional shape can be manufactured.
[0174] That is, as shown in FIG. 7, a first layer of high melting point material layer 101A is formed on stage 10, and metal powder 200A is placed in the recess of high melting point material layer 101A. Next, microwaves are irradiated to metal powder 200A to make metal powder 200A into first layer of metal solid 201A. Next, a second layer of high melting point material layer 101B is formed on first layer of high melting point material layer 101A, and metal powder 200B is placed in the recess of high melting point material layer 101B. Here, first layer of metal solid 201A is exposed from the recess of high melting point material layer 101B, and metal powder 200B is in contact with the surface of first layer of metal solid 201A. Next, microwaves are irradiated to metal powder 200B to make metal powder 200B into second layer of metal solid 201B. At this time, the second layer of metal solid 201B is fixed to the first layer of metal solid 201A. Thereafter, similar steps are repeated to stack metal solids.
[0175] Second embodiment A method for producing a bonded solid according to the second embodiment includes placing a metal powder on a solid, covering at least a portion of the periphery of the metal powder with a high-melting point material having a melting point higher than that of the metal powder, and irradiating the metal powder at least partially surrounded by the high-melting point material with microwaves to heat the metal powder and sinter or melt and solidify the metal powder, thereby forming a metal solid on the solid.
[0176] The material of the solid is not particularly limited, but a material having a higher melting point than the metal powder is preferable. An example of the material of the solid is a metal having a higher melting point than the metal powder. The shape of the solid is not particularly limited. Examples of the shape of the solid are a flat plate, a rectangular parallelepiped, and a cylinder. For example, the solid may have a flat surface or a curved surface.
[0177] The metal powder and the high melting point material may be the same as those in the first embodiment. The arrangement method of the metal powder and the high melting point material may be the same as those in the first embodiment. The relative arrangement of the metal powder and the high melting point material may be the same as those in the first embodiment. In addition, the microwave irradiation conditions may be the same as those in the first embodiment.
[0178] The method of disposing the metal powder on the solid is not particularly limited. The metal powder may be disposed on the solid using a recoater. The metal powder may be disposed on at least a portion of a plurality of surfaces of the solid. The metal powder may be disposed so as to cover the entire solid. The thickness of the layer of the metal powder disposed on the solid is appropriately set according to the thickness of the metal solid to be formed. The thickness of the layer of the metal powder disposed on the solid is, for example, constant. A recess may be provided in the layer of the high melting point material disposed on the stage, the solid may be disposed in the recess of the layer of the high melting point material, and the metal powder may be disposed on the solid. Alternatively, the metal powder may be disposed on the solid, and then the high melting point material may be disposed at least around the metal powder.
[0179] Before the microwave irradiation, pressure may be applied to the metal powder on the solid. The pressurizing method may be the same as that of the first embodiment. After the metal powder is irradiated with microwaves, pressure may be applied to the metal powder.
[0180] A metal solid is formed on a solid by sintering or melting and solidifying a metal powder on the solid. This bonds the metal solid to the solid. The formed metal solid may be in the form of a film. The metal solid may be formed on a solid for the purpose of coating the solid.
[0181] A further metal solid may be repeatedly formed on the metal solid formed on the solid. The metal solid may be in the form of a film, and a multi-layer film may be formed on the solid.
[0182] The method for producing a bonded solid according to the second embodiment may be carried out by the apparatus for producing a metal solid described in the first embodiment.
[0183] Third embodiment A method for manufacturing a bonded solid according to a third embodiment includes placing a bonding metal between a first solid and a second solid, covering at least a portion of the periphery of the bonding metal with a high-melting point material having a melting point higher than that of the bonding metal, and irradiating microwaves to the bonding metal at least partially surrounded by the high-melting point material to heat the bonding metal and sinter or melt and solidify the bonding metal, thereby bonding the first solid and the second solid.
[0184] The materials of the first and second solids are not particularly limited, but are preferably materials having a higher melting point than the metal powder. Examples of materials of the first and second solids include metals having a higher melting point than the metal powder. The shapes of the first and second solids are not particularly limited. The first and second solids may have surfaces that can contact each other. The first solid may have a shape that can fit with the second solid. The first solid may have a shape that can be inserted into the second solid.
[0185] The bonding metal may be a powder, a solid, or a liquid. If the bonding metal is a solid, it may have a shape that allows it to be inserted between the faying surfaces of the first solid and the faying surfaces of the second solid. If the bonding metal is a liquid, the liquid may be viscous. The bonding metal, which may be a powder or a solid, may be heated to become a liquid.
[0186] The material of the bonding metal may be the same as the metal powder described in the first embodiment. The high melting point material may be the same as the first embodiment. The bonding metal is disposed between the bonding surface of the first solid and the bonding surface of the second solid, and the high melting point material is disposed at least around the bonding metal. The method of disposing the high melting point material may be the same as the first embodiment. The relative disposition of the bonding metal and the high melting point material may be the same as the relative disposition of the metal powder and the high melting point material in the first embodiment. Note that the first solid or the second solid may be disposed between the bonding metal and the high melting point material. The microwave irradiation conditions may be the same as the first embodiment.
[0187] The method of disposing the bonding metal between the first and second solids is not particularly limited. When the bonding metal is a powder or liquid, the bonding metal may be injected between the bonding surface of the first solid and the bonding surface of the second solid. When the bonding metal is a solid, the bonding metal may be inserted between the bonding surface of the first solid and the bonding surface of the second solid. Alternatively, whether the bonding metal is a powder, liquid, or solid, the bonding metal may be disposed on the bonding surface of the first solid, and then the bonding surface of the second solid may be brought into contact with the bonding metal.
[0188] A recess may be provided in a layer of high melting point material placed on a stage, a first solid body may be placed in the recess of the layer of high melting point material, and a bonding metal and a second solid body may be sequentially placed on the first solid body. Alternatively, a bonding metal may be placed between the first solid body and the second solid body, and then a high melting point material may be placed at least around the bonding metal.
[0189] Prior to the application of microwaves, pressure may be applied to the bonding metal disposed between the first and second solids. For example, pressure may be applied to at least one of the first and second solids to apply pressure to the bonding metal. Pressure may be applied to the bonding metal after the bonding metal is irradiated with microwaves.
[0190] The first and second solid bodies are bonded together by sintering or melting the bonding metal between the first and second solid bodies.
[0191] The method for producing a bonded solid according to the third embodiment may be carried out by the apparatus for producing a metal solid described in the first embodiment.
[0192] Although the present invention has been described above by the embodiments, the description and drawings forming a part of this disclosure should not be understood as limiting the present invention. From this disclosure, various alternative embodiments, examples, and operation techniques should be apparent to those skilled in the art. For example, the pressurizing unit 60 shown in FIG. 1 may press the entire surface of the arranged metal powder 200. Alternatively, as shown in FIG. 8, the pressurizing unit 60 having a contact area smaller than the surface area of the arranged metal powder 200 may continuously press the metal powder 200 while moving. Examples of the pressing method include uniaxial molding, cold isostatic pressing (CIP) molding, hot isostatic pressing (HIP) molding, and roller pressing. In the case of roller pressing, as shown in FIG. 9, a pressing method may be selected in which the pressurizing unit 60 includes a roller, and the roller is pressed against the stage 10 and the roller is moved on the stage 10 or the stage 10 is slid. In addition, for example, as shown in FIG. 10, the manufacturing apparatus for a metal solid according to the embodiment may include a reduction device 80 that reduces the metal powder before the metal powder is irradiated with microwaves. The reduction device 80 is, for example, a heating device, and heats the metal powder to reduce the metal powder. Thus, it should be understood that the present invention encompasses various embodiments and the like that are not described herein. EXAMPLES
[0193] Example 1 A layer of high melting point material was formed. The high melting point material was composed of 93% by mass of aluminum oxide (Al2O3) powder and 7% by mass of carbon (C) powder. The surface of the high melting point material layer where the recesses were to be formed was covered with a circular aluminum plate, and the hardening material was sprayed onto the surface of the high melting point material layer, and the hardening material was allowed to penetrate into the part of the high melting point material layer that was not covered by the aluminum plate. The hardening material contained 50% by mass of UV-curable resin (Standard Photopolymer Resin manufactured by AMZLAB GmbH) and 50% by mass of ethanol. Then, the layer of high melting point material was irradiated with UV light, and the hardening resin that had penetrated into the layer of high melting point material was hardened. The high melting point material that was covered with the aluminum plate and not hardened was removed by air shower. As a result, a cylindrical recess was formed in the layer of high melting point material. The diameter of the bottom of the cylindrical recess was 7.0 mm, and the depth was 4.0 mm.
[0194] Metal powder (average particle size 45 μm) was filled into the recesses provided in the layer of high-melting-point material. The metal powder consisted of 100% iron (Fe). A pressure of 250 MPa was applied to the metal powder and the high-melting-point material surrounding the metal powder using a press. In an air atmosphere, the high-melting-point material and metal powder were irradiated with 700 W microwaves for 180 seconds, and the metal powder was heated to 1350 °C (estimated value). A photograph of the metal solid obtained by sintering the metal powder is shown in Figure 11. The obtained metal solid was cylindrical, with a diameter of the base of 7.0 mm and a height of 4.0 mm. The density of the obtained metal solid was 4.5 g / cm 2 and the relative density (= density / true density) was 58%.
[0195] Example 2 A first layer of high melting point material was formed. The high melting point material was composed of 93% by mass of aluminum oxide (Al2O3) powder and 7% by mass of carbon (C) powder. The surface of the first layer of high melting point material where the recesses were to be formed was covered with a circular aluminum plate, and a hardening material was sprayed onto the surface of the first layer of high melting point material, and the hardening material was allowed to penetrate into the portion of the first layer of high melting point material not covered by the aluminum plate. The hardening material contained 50% by mass of UV-curable resin (Standard Photopolymer Resin manufactured by AMZLAB GmbH) and 50% by mass of ethanol. Then, the first layer of high melting point material was irradiated with UV light, and the hardening resin that had penetrated into the first layer of high melting point material was hardened. The high melting point material that was covered with the aluminum plate and not hardened was removed by air shower. As a result, a cylindrical recess was formed in the first layer of high melting point material. The diameter of the bottom of the cylindrical recess was 7.0 mm, and the depth was 4.2 mm.
[0196] Metal powder was filled into the recesses in the first layer of the high melting point material. The metal powder consisted of 100% iron (Fe). A press was used to apply a pressure of 250 MPa to the metal powder and the high melting point material surrounding it. In an air atmosphere, the high melting point material and metal powder were irradiated with 700 W microwaves for 180 seconds, heating the metal powder to 1350°C (estimated value), and a cylindrical metal solid was obtained.
[0197] A second layer of high melting point material was formed on the first layer of high melting point material. The high melting point material was composed of 93% by mass of aluminum oxide (Al2O3) and 7% by mass of carbon (C). The area of the surface of the second layer of high melting point material where the recess was to be formed, directly above the metal solid surrounded by the first layer of high melting point material, was covered with a circular aluminum plate, and a hardening material was sprayed onto the surface of the second layer of high melting point material, and the hardening material was allowed to penetrate into the area of the second layer of high melting point material not covered by the aluminum plate. The hardening material contained 50% by mass of UV-curable resin (Standard Photopolymer Resin manufactured by AMZLAB GmbH) and 50% by mass of ethanol. Then, the second layer of high melting point material was irradiated with UV light, and the hardening resin that had penetrated into the second layer of high melting point material was hardened. The high melting point material that was covered with the aluminum plate and not hardened was removed by air shower. As a result, a cylindrical recess was formed in the second layer of high melting point material. The cylindrical recess had a bottom diameter of 7.0 mm and a depth of 2.4 mm. The top surface of the metal solid surrounded by the first layer of high-melting-point material was exposed from the recess provided in the second layer of high-melting-point material.
[0198] Metal powder was filled into the recesses provided in the second layer of the high melting point material. The metal powder was composed of 100% iron (Fe). A press was used to apply a pressure of 250 MPa to the metal powder and the high melting point material surrounding the metal powder. In an air atmosphere, the high melting point material and metal powder were irradiated with 700 W microwaves for 180 seconds, heating the metal powder to 1350°C (estimated value), and a cylindrical metal solid was obtained. At this time, the metal solid surrounded by the first layer of the high melting point material and the metal solid surrounded by the second layer of the high melting point material were bonded.
[0199] A photograph of the metal solid obtained by sintering the metal powder is shown in Figure 12. The obtained metal solid was cylindrical, with a base diameter of 7.0 mm and a height of 6.6 mm. The density of the obtained metal solid was 4.1 g / cm. 2 and the relative density was 52%.
[0200] Example 3 A layer of high melting point material was formed. The high melting point material was composed of 93% by mass of aluminum oxide (Al2O3) powder and 7% by mass of carbon (C) powder. The surface of the high melting point material layer where the recesses were to be formed was covered with a triangular aluminum plate, and a hardening material was sprayed onto the surface of the high melting point material layer, and the hardening material was allowed to penetrate into the part of the high melting point material layer that was not covered by the aluminum plate. The hardening material contained 50% by mass of UV-curable resin (Standard Photopolymer Resin manufactured by AMZLAB GmbH) and 50% by mass of ethanol. Then, the layer of high melting point material was irradiated with UV light, and the hardening resin that had penetrated into the layer of high melting point material was hardened. The high melting point material that was covered with the aluminum plate and not hardened was removed by air shower. As a result, a triangular prism-shaped recess was formed in the layer of high melting point material. The length of the base of the triangular prism-shaped recess was 8.0 mm, and the depth was 1.4 mm.
[0201] Metal powder was filled into the recesses provided in the layer of high melting point material. The metal powder consisted of 100% iron (Fe). A pressure of 250 MPa was applied to the metal powder and the high melting point material surrounding the metal powder using a press. In an air atmosphere, the high melting point material and metal powder were irradiated with 500 W microwaves for 70 seconds, and the metal powder was heated to 1250 °C (estimated value). Figure 13 shows a photograph of the metal solid obtained by sintering the metal powder. The obtained metal solid was in the shape of a triangular prism, with the base side length of the bottom face being 8.0 mm and the height being 1.4 mm. The density of the obtained metal solid was 4.5 g / cm 2 and the relative density was 58%.
[0202] Example 4 A layer of high melting point material was formed. The high melting point material was composed of 93% by mass of aluminum oxide (Al2O3) powder and 7% by mass of carbon (C) powder. The surface of the high melting point material layer where the recesses were to be formed was covered with a rectangular aluminum plate, and the hardening material was sprayed onto the surface of the high melting point material layer, and the hardening material was allowed to penetrate into the part of the high melting point material layer that was not covered by the aluminum plate. The hardening material contained 50% by mass of UV-curable resin (Standard Photopolymer Resin manufactured by AMZLAB GmbH) and 50% by mass of ethanol. Then, the layer of high melting point material was irradiated with UV light, and the hardening resin that had penetrated into the layer of high melting point material was hardened. The high melting point material that was covered with the aluminum plate and not hardened was removed by air shower. As a result, a rectangular prism-shaped recess was formed in the layer of high melting point material. The length of one side of the bottom surface of the rectangular prism-shaped recess was 7.2 mm, and the depth was 1.9 mm.
[0203] Metal powder was filled into the recesses provided in the layer of high melting point material. The metal powder consisted of 100% iron (Fe). A pressure of 250 MPa was applied to the metal powder and the high melting point material surrounding the metal powder using a press. In an air atmosphere, the high melting point material and metal powder were irradiated with 500 W microwaves for 70 seconds, and the metal powder was heated to 1250 °C (estimated value). A photograph of the metal solid obtained by sintering the metal powder is shown in Figure 14. The obtained metal solid was a square pillar with a side length of the base of 7.2 mm and a height of 1.9 mm. The density of the obtained metal solid was 4.5 g / cm 2 and the relative density was 58%.
[0204] Example 5 A cylindrical solid made of 99.8% copper (Cu) was prepared. The diameter of the solid was 7 mm and the height was 10 mm. A green compact made by applying a pressure of 250 MPa to 99.8% copper (Cu) powder was placed on top of the solid. The green compact was cylindrical in shape, with a diameter of 10 mm and a height of 2 mm. The green compact was placed so that the center of the solid and the center of the green compact were aligned.
[0205] A layer of high-melting-point material was formed around the solid and the green compact. The high-melting-point material consisted of 93% by mass of aluminum oxide (Al2O3) powder and 7% by mass of carbon (C) powder. A curable material was sprayed onto the surface of the high-melting-point material layer, and the high-melting-point material was permeated with the curable material. The curable material contained 50% by mass of UV-curable resin (Standard Photopolymer Resin, manufactured by AMZLAB GmbH) and 50% by mass of ethanol. The layer of high-melting-point material was then irradiated with UV light, and the curable resin that had permeated the layer of high-melting-point material was cured.
[0206] While applying a pressure of 20 MPa to the solid and green compact, the green compact covered with the high melting point material was irradiated with 700 W microwaves for 85 seconds, heating the green compact to 800°C (estimated value). Figure 15 shows a photograph of the solid coated with a copper metal film (metallic solid) after the green compact had been sintered. The solid and the metal film were firmly bonded.
[0207] Example 6 A cylindrical solid made of tool steel (SKD61) was prepared. The diameter of the solid was 10 mm and the height was 4 mm. A green compact produced by applying a pressure of 1750 MPa to powder of tool steel (SKD61) was placed on top of the solid. The green compact had a cylindrical shape with a diameter of 10 mm and a height of 4 mm. The green compact was placed so that the center of the solid and the center of the green compact were aligned.
[0208] As in Example 5, a layer of high melting point material was formed around the solid and the green compact.
[0209] While applying a pressure of 20 MPa to the solid and green compact, the green compact covered with the high melting point material was irradiated with 400 W microwaves for 1500 seconds, heating the green compact to 1200°C (estimated value). Figure 16 shows a photograph of the solid coated with a metal film (metal solid) made of tool steel after the green compact had been sintered. The solid and the metal film were firmly bonded.
[0210] Example 7 A cylindrical solid made of carbon steel (S45C) was prepared. The diameter of the solid was 10 mm and the height was 10 mm. A green compact produced by applying a pressure of 250 MPa to aluminum alloy (A6061) powder was placed on top of the solid. The green compact had a cylindrical shape, a diameter of 10 mm and a height of 4 mm. The green compact was placed so that the center of the solid and the center of the green compact were aligned.
[0211] As in Example 5, a layer of high melting point material was formed around the solid and the green compact.
[0212] While applying a pressure of 20 MPa to the solid and powder compact, the powder compact covered with the high melting point material was irradiated with 200 W microwaves for 1,500 seconds, heating the powder compact to 400°C (estimated value). Figure 17 shows a photograph of the solid that was sintered and coated with an aluminum alloy metal film (metal solid). The solid and the metal film were firmly bonded.
[0213] Example 8 A cylindrical first solid made of 99.8% copper (Cu) was prepared. The diameter of the first solid was 10 mm and the height was 10 mm. A green compact produced by applying a pressure of 250 MPa to 99.8% copper (Cu) powder was placed on top of the first solid as a binding metal. The green compact had a cylindrical shape with a diameter of 10 mm and a height of 3 mm. The green compact was placed so that the center of the first solid and the center of the green compact coincided. A cylindrical second solid made of 99.8% copper (Cu) was placed on top of the green compact. The diameter of the second solid was 10 mm and the height was 6 mm. The second solid was placed so that the center of the green compact and the center of the second solid coincided.
[0214] As in Example 5, a layer of a high melting point material was formed around the first solid, the green compact, and the second solid.
[0215] The powder compact covered with the high melting point material was irradiated with 700W microwaves for 135 seconds, and the powder compact was heated to 800℃ (estimated value). Figure 18 shows a photograph of the bonded solid formed by sintering the powder compact and bonding the first solid and the second solid. The first solid and the second solid were firmly bonded.
[0216] Example 9 A cylindrical first solid made of tool steel (SKD61) was prepared. The diameter of the first solid was 10 mm and the height was 10 mm. A green compact produced by applying a pressure of 1750 MPa to powder of tool steel (SKD61) was placed on top of the first solid as a binding metal. The green compact had a cylindrical shape with a diameter of 10 mm and a height of 3 mm. The green compact was placed so that the center of the first solid and the center of the green compact coincided. A cylindrical second solid made of tool steel (SKD61) was placed on top of the green compact. The diameter of the second solid was 10 mm and the height was 6 mm. The second solid was placed so that the center of the green compact and the center of the second solid coincided.
[0217] As in Example 5, a layer of a high melting point material was formed around the first solid, the green compact, and the second solid.
[0218] Without applying pressure, the powder compact covered with the high melting point material was irradiated with 400 W microwaves for 2000 seconds, and the powder compact was heated to 1200 °C (estimated value). The first solid and the second solid were firmly bonded.
[0219] Example 10 A cylindrical first solid made of tool steel (SKD61) was prepared. The diameter of the first solid was 10 mm and the height was 4 mm. A solid made of tool steel (SKD61) was placed on top of the first solid as a bonding metal. The bonding metal was cylindrical in shape, with a diameter of 10 mm and a height of 4 mm. The bonding metal was placed so that the center of the first solid and the center of the bonding metal coincided. A cylindrical second solid made of tool steel (SKD61) was placed on top of the bonding metal. The diameter of the second solid was 10 mm and the height was 4 mm. The second solid was placed so that the center of the bonding metal and the center of the second solid coincided.
[0220] As in Example 5, a layer of a high melting point material was formed around the first solid, the bonding metal, and the second solid.
[0221] While applying a pressure of 20 MPa to the first solid, the bonding metal, and the second solid, the bonding metal covered with the high melting point material was irradiated with 400 W microwaves for 2000 seconds, and the bonding metal was heated to 1200°C (estimated value). Figure 19 shows a photograph of the bonded solid in which the bonding metal melted and solidified, bonding the first solid and the second solid. The first solid and the second solid were firmly bonded. [Explanation of symbols]
[0222] 10 stage, 20 microwave irradiation section, 31 high melting point material placement section, 32 hardenable material addition section, 33 metal powder placement section, 40 hardening device, 50 unhardened material removal section, 60 pressure section, 101 layer, 102 portion, 103 recess, 200 metal powder
Claims
1. disposing a metallic material on a solid; covering at least a portion of the periphery of the disposed metal material with a high melting point material having a melting point higher than the melting point of the metal material; irradiating the metal material, at least a part of which is covered with the high melting point material, with microwaves to heat the metal material, sintering or melting and solidifying the metal material, and forming a metal solid on and bonded to the solid; Including, The high melting point material is a heat insulating material that absorbs the microwaves less than the metal material, the heat insulating material including an oxide; an absorbing material that absorbs the microwaves in a temperature range at least a part of which is lower than a temperature range in which the metal material absorbs the microwaves, the absorbing material including a carbon material; including a mixture of Method for producing bonded solids.
2. disposing the metallic material on the metallic solid; covering at least a portion of the periphery of the disposed metal material on the metal solid with the high melting point material; irradiating microwaves to the metal material on the metal solid, at least a portion of which is covered with the high melting point material, to heat the metal material and sinter or melt and solidify the metal material, thereby forming an additional metal solid on the metal solid; The method for producing the bonded solid of claim 1 further comprising:
3. The method of claim 2 , wherein the metal solid is formed as a laminate.
4. The method for producing a bonded solid according to any one of claims 1 to 3, wherein the high melting point material comprises from 1% to 70% by weight of the absorbent material.
5. The method for producing a bonded solid according to any one of claims 1 to 4, wherein the heat insulating material comprises at least one selected from the group consisting of aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, and titanium oxide.
6. 6. The method for producing a bonded solid according to claim 1, wherein the absorbent material comprises at least one selected from the group consisting of carbon, graphite, silicon carbide, carbon resin, and metal carbide.
7. The method for producing a bonded solid according to claim 1 , wherein the metallic material comprises a metal.
8. The method for producing a bonded solid according to any one of claims 1 to 7, wherein the metal material comprises at least one selected from the group consisting of iron, nickel, copper, gold, silver, aluminum, and cobalt.
9. The method for producing a bonded solid according to claim 1 , wherein the metal material comprises a metal compound.
10. 10. The method for producing a bonded solid according to claim 1, wherein the metal material comprises at least one compound selected from the group consisting of iron, nickel, copper, gold, silver, aluminum, and cobalt.
11. The method for producing a bonded solid according to claim 7 , wherein the metallic material further comprises an alloy component.
12. 12. The method of claim 11, wherein the alloying component comprises at least one selected from the group consisting of silicon, manganese, chromium, nickel, carbon, boron, copper, aluminum, titanium, niobium, vanadium, zinc, and sulfur.
13. The method for producing a bonded solid according to claim 1 , wherein the metal material is a metal powder, and the average particle size of the metal powder is 200 μm or less.
14. The method for producing a bonded solid according to claim 1 , wherein the metal material includes a metal oxide, and the metal material is reduced by irradiating the metal material with microwaves.
15. The method for producing a bonded solid according to claim 1 , wherein the metal material comprises a metal oxide, and the metal material is sintered by irradiating the metal material with microwaves.
16. The method for producing a bonded solid according to any one of claims 1 to 15, wherein the high melting point material forms a mould or a container.
17. The method for producing a bonded solid according to any one of claims 1 to 16, wherein the metal material is in the form of a compact.
18. The method for producing a bonded solid according to any one of claims 1 to 17, further comprising applying pressure to the metal material before irradiating the metal material with microwaves.
19. The method for producing a bonded solid according to claim 18, wherein the pressure is from 0.1 MPa to 2000 MPa.
20. The method for producing a bonded solid according to any one of claims 1 to 19, further comprising applying pressure to the metal material while irradiating the metal material with microwaves.
21. The method for producing a bonded solid according to claim 20, wherein the pressure is from 0.1 MPa to 2000 MPa.
22. The method for producing a bonded solid according to any one of claims 1 to 21, further comprising applying pressure to the metal material after irradiating the metal material with microwaves.
23. 23. The method for producing a bonded solid according to claim 22, wherein the pressure is from 0.1 MPa to 2000 MPa.
24. The method for producing a bonded solid according to any one of claims 1 to 23, wherein the irradiating of the metal material with microwaves is carried out under an inert gas atmosphere.
25. The method for producing a bonded solid according to any one of claims 1 to 24, wherein the irradiating of the metal material with microwaves is carried out under a reducing atmosphere.
26. 26. The method for producing a bonded solid according to any one of claims 1 to 25, wherein the metal material comprises a metal oxide, and further comprising reducing the metal oxide prior to irradiating the metal material with microwaves.
27. Covering at least a portion of the periphery of the disposed metal material with a high melting point material having a melting point higher than the melting point of the metal material, forming a layer of said high melting point material; forming a recess in the layer of high melting point material; placing the solid and the metallic material in the recess; A method for producing the bonded solid according to any one of claims 1 to 26, comprising:
28. forming the recess in the layer of high melting point material; hardening a portion of the layer of high melting point material; removing uncured portions of the layer of high melting point material; 28. A method for producing the bonded solid of claim 27, comprising:
29. 30. The method of claim 28, wherein hardening the portion of the layer of high melting point material comprises including a hardenable material in the portion of the layer of high melting point material.
30. 30. The method of claim 29, further comprising impregnating said portion of said layer of high melting point material with a hardenable material.
31. 31. A method for producing a bonded solid according to any one of claims 28 to 30, wherein the part of the layer of high melting point material is hardened by light irradiation.
32. disposing a bonding metal between the first solid and the second solid; covering at least a portion of the periphery of the disposed bonding metal with a high melting point material having a melting point higher than the melting point of the bonding metal; irradiating the bonding metal, at least a part of which is covered with the high melting point material, with microwaves to heat the bonding metal, sintering or melting and solidifying the bonding metal, and bonding the first solid and the second solid; Including, The high melting point material is an insulating material that absorbs the microwaves less than the bonding metal, the insulating material including an oxide; an absorbing material that absorbs the microwaves in a temperature range at least part of which is lower than the temperature range in which the binding metal absorbs the microwaves, the absorbing material including a carbon material; including a mixture of Method for producing bonded solids.
33. 33. The method of claim 32, wherein the bonding metal is a powder.
34. 33. The method of claim 32, wherein the bonding metal is a solid.
35. 33. The method of claim 32, wherein the bonding metal is a liquid.
36. 36. A method for producing a bonded solid according to any one of claims 32 to 35, wherein the high melting point material comprises from 1% to 70% by weight of the absorbent material.
37. 37. The method for producing a bonded solid according to any one of claims 32 to 36, wherein the insulating material comprises at least one selected from the group consisting of aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, and titanium oxide.
38. 38. A method for producing a bonded solid according to any one of claims 32 to 37, wherein the absorbent material comprises at least one selected from the group consisting of carbon, graphite, silicon carbide, carbon resins, and metal carbides.
39. 39. A method for producing a bonded solid according to any one of claims 32 to 38, wherein the bonding material comprises a metal.
40. 40. The method for producing a bonded solid according to any one of claims 32 to 39, wherein the binding metal comprises at least one selected from the group consisting of iron, nickel, copper, gold, silver, aluminum, and cobalt.
41. 41. A method for producing a bonded solid according to any one of claims 32 to 40, wherein the bonding metal comprises a metal compound.
42. 42. A method for producing a bonded solid according to any one of claims 32 to 41, wherein the bonding metal comprises at least one compound selected from the group consisting of iron, nickel, copper, gold, silver, aluminum, and cobalt.
43. 43. A method for producing a bonded solid according to any one of claims 39 to 42, wherein the bonding metal further comprises an alloying component.
44. 44. The method of claim 43, wherein the alloying component comprises at least one selected from the group consisting of silicon, manganese, chromium, nickel, carbon, boron, copper, aluminum, titanium, niobium, vanadium, zinc, and sulfur.
45. 45. A method for producing a bonded solid according to any one of claims 32 to 44, wherein the binding metal is a powder and the average particle size of the binding metal is 200 μm or less.
46. 46. The method for producing a bonded solid according to any one of claims 32 to 45, wherein the bonding metal comprises a metal oxide, and the bonding metal is reduced by irradiating the bonding metal with microwaves.
47. 47. The method for producing a bonded solid according to any one of claims 32 to 46, wherein the bonding metal comprises a metal oxide, and the bonding metal is sintered by irradiating the bonding metal with microwaves.
48. 48. A method for producing a bonded solid according to any one of claims 32 to 47, wherein the high melting point material forms a mould or container.
49. 35. A method for producing a bonded solid according to claim 33 or 34, wherein the bonding metal is in the form of a compact.
50. 50. The method of claim 32, further comprising applying pressure to the bonding metal prior to irradiating the bonding metal with microwaves.
51. 51. The method for producing a bonded solid according to claim 50, wherein the pressure is from 0.1 MPa to 2000 MPa.
52. 52. A method for producing a bonded solid according to any one of claims 32 to 51, further comprising applying pressure to the bonding metal while irradiating the bonding metal with microwaves.
53. 53. The method for producing a bonded solid according to claim 52, wherein the pressure is from 0.1 MPa to 2000 MPa.
54. 54. The method for producing a bonded solid according to any one of claims 32 to 53, further comprising applying pressure to the bonding metal after irradiating the bonding metal with microwaves.
55. 55. The method for producing a bonded solid according to claim 54, wherein the pressure is from 0.1 MPa to 2000 MPa.
56. The method for producing a bonded solid according to any one of claims 32 to 55, wherein the irradiating of the bonding metal with microwaves is carried out under an inert gas atmosphere.
57. 33. The method of claim 32, wherein the step of irradiating the bonding metal with microwaves is performed in a reducing atmosphere.
57. A method for producing a bonded solid according to any one of claims 1 to 56.
58. 58. A method for producing a bonded solid according to any one of claims 32 to 57, wherein the bonding metal comprises a metal oxide, and further comprising reducing the metal oxide prior to irradiating the bonding metal with microwaves.
59. Covering at least a portion of the periphery of the disposed bonding metal with a high melting point material having a melting point higher than the melting point of the bonding metal; forming a layer of said high melting point material; forming a recess in the layer of high melting point material; placing the first and second solids and the bonding metal in the recess; A method for producing the bonded solid of any one of claims 32 to 58, comprising:
60. forming the recess in the layer of high melting point material; hardening a portion of the layer of high melting point material; removing uncured portions of the layer of high melting point material; A method for producing the bonded solid of claim 59, comprising:
61. 61. The method of claim 60, wherein hardening the portion of the layer of high melting point material comprises including a hardenable material in the portion of the layer of high melting point material.
62. 62. The method of claim 61, further comprising impregnating said portion of said layer of high melting point material with a hardenable material.
63. 63. A method for producing a bonded solid according to any one of claims 60 to 62, wherein the portion of the layer of high melting point material is hardened by light irradiation.