High energy density compositional gradient electrode and method of manufacture thereof

JP2024096854A5Active Publication Date: 2024-10-2424M TECHNOLOGIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024063875
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-05-24
Filing Date
2024-04-11
Publication Date
2024-10-24
Estimated Expiration
2039-05-24

AI Technical Summary

Technical Problem

Conventional electrodes face limitations in thickness due to conductivity issues and manufacturing challenges, leading to reduced ion/electron storage capacity and increased internal resistance, which hinders the development of high-energy density batteries that can be both high capacity and high speed.

Method used

The development of electrodes with compositional gradients, including variations in porosity, active material concentration, and conductivity across the thickness, allowing for thicker electrodes with improved ion diffusion and reduced tortuosity, using semi-solid materials to enhance conductivity and reduce inert components.

Benefits of technology

This approach enables electrodes with higher energy density and superior rate capabilities, achieving faster charging and discharging without the limitations of conventional electrodes, while maintaining mechanical stability and reducing irreversible capacity loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide an electrode that can be made thicker and has superior performance characteristics such as superior rate capability and charge capacity.SOLUTION: An electrode includes a current collector 110, a first electrode material 120 disposed on the current collector 110 and having first porosity, and a second electrode material 130 disposed on the first electrode material 120 and having second porosity greater than the first porosity, and the second electrode material 130 includes a mixture of an active material and a conductive material in a liquid electrolyte.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to and the benefit of U.S. Provisional Patent Application No. 62 / 676,049, filed May 24, 2018, entitled "HIGH ENERGY DENSITY COMPOSITION GRADIENT ELECTRODE AND METHOD FOR MANUFACTURING SAME," the disclosure of which is incorporated herein by reference in its entirety. [Background technology]

[0002] Consumers want batteries that can be charged quickly and store enough energy to perform the intended application for as long as needed. To achieve the desired theoretical energy density, battery manufacturers have increased the thickness of the electrodes to increase the total ionic / electronic storage capacity of the electrodes. However, these thicker electrodes often result in some of the active material being largely unavailable for ionic / electronic storage due to the reduced conductivity across these portions of the electrodes as a function of the electrode thickness. Battery manufacturers also use high-capacity materials in the electrodes (e.g., anodes) to increase the theoretical energy density, but these materials often expand and contract volumetrically during use of the electrodes, potentially damaging the battery. Thus, reducing inactive components in the electrodes and finished batteries and improving energy density and overall performance is a persistent goal of energy storage system development. Summary of the Invention

[0003] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The embodiments described herein generally relate to devices, systems, and methods for manufacturing high energy density electrodes that include a first electrode material disposed on a current collector and having a first porosity, and a second electrode material disposed on the first electrode material and having a second porosity. In some embodiments, the second porosity is less than the first porosity. In some embodiments, the second porosity is substantially equal to the first priority. In some embodiments, the second porosity is greater than the first porosity.

[0004] In some embodiments, the second electrode material comprises a mixture of active material and conductive material in a liquid electrolyte. In some embodiments, the first electrode material may have a different composition than the second electrode material. In some embodiments, the first electrode material may comprise a high capacity material such as tin, a tin alloy such as Sn-Fe, tin monoxide, silicon, a silicon alloy such as Si-Co, silicon monoxide, aluminum, an aluminum alloy, a metal monoxide (CoO, FeO, etc.), or a titanium oxide. In some embodiments, the silicon and / or silicon alloy and / or silicon monoxide have a higher concentration (e.g., by volume percent) in the first layer than in the second layer. In some embodiments, the lithium-containing material may be disposed between the first electrode material and the second electrode material. In some embodiments, a portion of the first electrode material may be removed to expose a portion of the current collector, such that when the second electrode material is disposed on the first electrode material, a portion of the second electrode material may be disposed directly on the exposed portion of the current collector. [Brief description of the drawings]

[0005] [Figure 1] FIG. 2 is a schematic diagram of a multi-layer electrode, according to one embodiment. [Diagram 2] FIG. 2 is a schematic diagram of a multi-layer electrode, according to one embodiment. [Diagram 3] FIG. 2 is a schematic diagram of a multi-layer electrode including an extended region, according to one embodiment. [Figure 4] FIG. 2 is a schematic diagram of a multi-layer electrode, according to one embodiment. [Diagram 5] FIG. 2 is a schematic diagram of a multi-layer electrode, according to one embodiment. [Figure 6] 1 is a graphical representation of the behavior of a half-cell with a multilayer electrode. [Figure 7] 1 is a graphical representation of charge and discharge curves for a cell with a multi-layer electrode. [Figure 8] 1 is a graphical representation of charge and discharge curves for a cell with a multi-layer electrode. [Figure 9] 1 is a graphical representation of charge and discharge curves for a cell with a multi-layer electrode. [Figure 10] 1 is a graphical representation of capacity retention of cells with multi-layer electrodes. [Figure 11] 1 is a graphical representation of capacity retention of cells with multi-layer electrodes. [Figure 12] 1 is a graphical representation of capacity retention of cells with multi-layer electrodes. [Figure 13] 1 is a graphical representation of the comparison of beginning-of-life and end-of-life capacity of cells with multi-layer electrodes. [Figure 14] 1 is a graphical representation of charge and discharge curves for a cell with a multi-layer electrode. [Figure 15] 1 is a graphical representation of charge and discharge curves for a cell with a multi-layer electrode. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0006] SUMMARY OF THE DISCLOSURE The embodiments described herein generally relate to devices, systems, and methods for manufacturing high energy density electrodes having porosity that increases with distance from the current collector.

[0007] Conventional battery systems store electrochemical energy by separating an ion source and an ion sink at different ionic electrochemical potentials. The difference in electrochemical potential creates a voltage difference between the positive and negative electrodes, which generates an electric current if the electrodes are connected with a conductive element. The difference in electrochemical potential between the positive and negative electrodes can generate a higher voltage system, contributing to a higher energy density cell. In a conventional battery system, the negative and positive electrodes are connected through a parallel configuration of two conductive elements. The external element conducts only electrons, while the internal element is separated by a separator and electrolyte and conducts only ions. Since a charge imbalance cannot be maintained between the negative and positive electrodes, the external and internal flows supply ions and electrons at the same rate. The generated electric current can drive an external device. A rechargeable battery can be recharged by applying an opposite voltage difference that drives the electric and ionic current in the opposite direction to the battery being discharged. Thus, the active material of a secondary battery must have the ability to accept and donate ions. Increasing the electrochemical potential creates a larger voltage difference between the cathode and anode of the battery, increasing the electrochemically stored energy per unit mass of the battery.

[0008] Batteries in consumer electronics have been gradually increasing in energy density with advances in lithium-ion battery technology. The stored energy or charge capacity of a manufactured battery is a function of (1) the specific charge capacity of the active material (mAh / g), (2) the volume of the electrodes (cm 3 ) (i.e., the product of the electrode thickness, the electrode area, and the number of layers (stacks)), and (3) the loading of active material in the electrode medium (e.g., cm 3 Therefore, to increase commercial appeal (e.g., increasing energy density and decreasing cost), the area charge capacity (mAh / cm 2) is desirable. The areal charge capacity can be increased, for example, by utilizing active materials with higher specific charge capacity, by increasing the relative proportion of active charge storage material in the overall electrode formulation (i.e., "loading"), and / or by increasing the relative proportion of electrode material used in a particular battery form factor. In other words, increasing the ratio of active charge storage components (e.g., electrodes) to inactive components (e.g., separators and current collectors) can improve the overall performance of the battery by eliminating or reducing components that do not contribute to the overall performance of the battery. One way to achieve increased areal charge capacity and thus reduced relative proportion of inactive components is by increasing the thickness of the electrodes.

[0009] Conventional electrode compositions generally cannot be thicker than about 100 μm due to certain performance and manufacturing limitations. For example, i) conventional electrodes with thicknesses greater than 100 μm (single-sided coated thickness) typically suffer from a significant reduction in rate capability due to limitations in diffusion through the thickness of the electrode (porosity, tortuosity, impedance, etc.) that increase rapidly with increasing thickness. ii) conventional thick electrodes are difficult to fabricate due to limitations in drying and post-processing, such as solvent removal rate, capillary forces during drying leading to cracking of the electrode, poor adhesion of the electrode to the current collector leading to delamination (e.g., during the high-speed roll-to-roll calendaring process used to fabricate conventional electrodes), binder migration during the solvent removal process, and / or deformation during the subsequent compression process. iii) Without being bound to a particular theory, the binders used in conventional electrodes may impede the pore structure of the electrode, reducing the available pore volume and increasing the tortuosity (i.e., effective path length) by occupying a significant portion of the space between the functional components (i.e., active and conductive components) of the electrode, thereby increasing the resistance to diffusion of ions. It is also known that binders used in conventional electrodes can at least partially coat the surface of the electrode active material, thereby slowing or completely blocking the flow of ions to the active material, thereby increasing tortuosity.

[0010] Furthermore, known conventional batteries have either high capacity or high rate capability, but not both. A battery with a first charge capacity at a first C rate, e.g., 0.5C, generally has a second, lower charge capacity when discharged at a second, higher C rate, e.g., 2C. This is because the higher internal resistance of conventional electrodes (e.g., solid electrodes with binders) causes higher energy losses inside conventional batteries, causing the voltage to drop and the battery to reach the low-end voltage cutoff sooner. Thicker electrodes generally have higher internal resistance and therefore have lower rate capability. For example, lead acid batteries do not perform well at 1 CC rate. Often lead acid batteries are rated at 0.2 CC rate, and even at this low C rate, they cannot achieve 100% capacity. In contrast, ultracapacitors can be discharged at very high C rates and still maintain 100% capacity, but have a much lower charge capacity than conventional batteries. Thus, there is a need for electrodes that can be made thicker and still have superior performance characteristics, such as superior rate capability and charge capacity. The gradient in physical properties and composition can aid in the diffusion of electroactive species. The gradient in composition can include the active material composition.

[0011] Thus, the embodiments described herein generally relate to electrodes having a composition gradient (hereinafter "electrode thickness") in the z-direction (also referred to as the "0001" direction), i.e., perpendicular to the surface of the current collector. In other words, the electrodes can be designed to be at least partially anisotropic and / or non-uniform to tailor the electrodes for improved mechanical, chemical, and / or electrochemical performance.

[0012] As used herein, "composition" may be anisotropic and may refer to physical, chemical, or electrochemical composition or a combination thereof. For example, in some embodiments, the electrode material immediately adjacent to the surface of the current collector may be less porous than the electrode material further away from the surface of the current collector. Without wishing to be bound by a particular theory, for example, the use of a porosity gradient may result in an electrode that can be made thicker without experiencing a decrease in ionic conductivity. In some embodiments, the composition of the electrode material adjacent to the surface of the current collector may be chemically different from the electrode material further away from the surface of the current collector.

[0013] As used herein, the terms "about" and "approximately" generally mean plus or minus 10% of the stated value, for example, about 250 μm includes 225 μm to 275 μm, and about 1,000 μm includes 900 μm to 1,100 μm.

[0014] As used herein, the term "semi-solid" refers to a material that is a mixture of liquid and solid phases, such as, for example, a particle suspension, a colloidal suspension, an emulsion, a gel, or a micelle.

[0015] As used herein, the terms "activated carbon network" and "networked carbon" refer to the general qualitative state of an electrode. For example, an electrode with an activated carbon network (or networked carbon) is such that the carbon particles in the electrode assume the form of individual particles and mutual arrangement that facilitates electrical contact and electrical conductivity between the particles throughout the thickness and length of the electrode. Conversely, the terms "non-activated carbon network" and "non-networked carbon" refer to an electrode in which the carbon particles exist as individual particle islands or multi-particle agglomerate islands that may not be sufficiently connected to provide adequate electrical conduction through the electrode.

[0016] As used herein, the terms "energy density" and "volumetric energy density" refer to the amount of energy (e.g., MJ) stored in an electrochemical cell per unit volume (e.g., L) of materials, such as electrodes, separators, electrolytes, current collectors, etc., that the electrochemical cell contains to operate. Specifically, materials used for packaging the electrochemical cell are excluded from the calculation of volumetric energy density.

[0017] As used herein, the term "high capacity material" or "high capacity anode material" refers to a material with an irreversible capacity of greater than 300 mAh / g that can be incorporated into an electrode to facilitate the uptake of electroactive species. Examples include tin, tin alloys such as Sn-Fe, tin monoxide, silicon, silicon alloys such as Si-Co, silicon monoxide, aluminum, aluminum alloys, metal monoxides (CoO, FeO, etc.), or titanium oxide.

[0018] As used herein, the term "composite high capacity electrode layer" refers to an electrode layer with both high capacity materials and conventional anode materials, for example, a silicon-graphite layer.

[0019] As used herein, the term "solid high capacitance electrode layer" refers to an electrode layer with a single solid phase high capacitance material, for example, sputtered silicon, tin, tin alloys such as Sn-Fe, tin monoxide, silicon, silicon alloys such as Si-Co, silicon monoxide, aluminum, aluminum alloys, metal monoxides (CoO, FeO, etc.), or titanium oxide.

[0020] In some embodiments, the compositional gradient may include any physical, chemical, and / or electrochemical property of the electrode material. In some embodiments, the compositional gradient may include a change in porosity of the electrode material across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in active material or active material concentration across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in conductive material or conductive material concentration across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in electrolyte or electrolyte concentration across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in additive (e.g., electrolyte additive) or additive concentration across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in density (unit mass per unit volume) across the thickness of the electrode. In some embodiments, the compositional gradient may include a change between at least one of the following crystallinity structures across the thickness of the electrode: cubic, hexagonal, tetragonal, rhombohedral, orthorhombic, monoclinic, and triclinic. In some embodiments, the compositional gradient may include a change in pH across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in ionic conductivity across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in electronic conductivity across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in energy density across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in theoretical energy density across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in Young's modulus across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in yield strength across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in tensile strength across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in volume expansion / contraction potential across the thickness of the electrode during operation of the electrochemical cell. In some embodiments, the compositional gradient may include a change in the plastic deformability of the electrode material across the electrode gradient.In some embodiments, the compositional gradient may include a change in the solubility of at least one of the active material, conductive material, and additive in the electrolyte across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in the percentage of binder across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in the processability of the electrode material across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in the flowability of the electrode material across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in the ion storage potential across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in the capacity fade experienced after the first charge / discharge cycle across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in viscosity across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in density across the thickness of the electrode. In some embodiments, the compositional gradient may include a change in surface area across the thickness of the electrode. In some embodiments, the change in surface area across the thickness of the electrode may be due to a change in active material concentration (i.e., active material closer to the current collector is more concentrated than active material further away, or vice versa). In some embodiments, the change in surface area across the thickness of the electrode can be due to a change in active material composition (i.e., the active material composition closer to the current collector is different from the active material composition away from the current collector).

[0021] In some embodiments, several compositionally distinct electrode materials can be disposed on a current collector (e.g., in a laminated structure) to achieve a composition gradient through the thickness of the electrode. In some embodiments, the number of compositionally distinct electrode materials can be greater than 1, greater than about 2, greater than about 3, greater than about 4, greater than about 5, greater than about 6, greater than about 7, greater than about 8, greater than about 9, greater than about 10, or greater than about 15, including all values ​​and ranges therebetween. In some embodiments, a first layer can be disposed on the current collector, a second layer can be disposed on the first layer, and subsequent layers can be disposed on top of the previous layer until a top layer is disposed to form a completed electrode. In some embodiments, the first one or more layers can be combined with a second one or more other layers in any suitable order and using any suitable method, and the combined layers can be simultaneously disposed on the current collector to form a completed electrode. In some embodiments, a single electrode material may be formed on a current collector that has a compositional gradient (anisotropy) across the thickness of the electrode.

[0022] 1 is a schematic diagram of an electrode 100 including a first electrode material 120 disposed on a current collector 110 and a second electrode material 130 disposed on the first electrode material 120. In some embodiments, the first electrode material 120 and / or the second electrode material 130 may include at least one of a solid electrode material, a semi-solid electrode material, a high capacity material, and combinations thereof (collectively "electrode materials").

[0023] The electrode 100 can be used as a cathode, an anode, or in any other manner in an electrochemical device. In some embodiments, the electrode 100 can include a range of materials and any suitable form factor as described in U.S. Patent No. 8,993,159, entitled "Semi-Solid Electrode with High Rate Capability," filed April 29, 2013 (the "'159 Patent"), the entire disclosure of which is incorporated herein by reference.

[0024] Similarly, current collector 110 can be configured to be used as a cathode current collector, an anode current collector, or for any other purpose as desired. Examples of possible materials, electrochemical compatibility properties, form factors, and uses for current collector 110 are described in further detail in the '159 patent. Current collector 110 can be substantially similar to the current collectors described in the '159 patent and therefore will not be described in detail herein.

[0025] In some embodiments, the electrode materials may include active materials, conductive materials, electrolytes, additives, binders, and / or combinations thereof. In some embodiments, the active materials may be ion storage materials and / or any other compounds or ion complexes that can undergo faradaic or non-faradaic reactions to store energy. The active materials may also be multi-phase materials that include redox active solids mixed with non-redox active phases, including solid-liquid suspensions, or liquid-liquid multi-phase mixtures, including micelles or emulsions with liquid ion storage materials intimately mixed with a supporting liquid phase. Systems utilizing various working ions include Li + , Na + or other alkali ions are the working ions, and Ca 2+ , Mg 2+ , or Al 3+ In some embodiments, the negative electrode storage material and the positive electrode storage material can be electrochemically combined to form an electrochemical cell, where the negative electrode stores the working ion of interest at a lower absolute potential than the positive electrode. The cell voltage can be approximately determined by the difference in the ion storage potentials of the two ion storage electrode materials.

[0026] Electrochemical cells that use negative and / or positive ion storage materials that are insoluble storage hosts for working ions can absorb or release working ions while all other components of the material remain substantially insoluble in the electrolyte. In some embodiments, these cells can be particularly advantageous because the electrolyte is not contaminated with the electrochemical composition. Additionally, cells that use negative and / or positive lithium ion storage materials can be particularly advantageous when using non-aqueous electrochemical compositions.

[0027] In some embodiments, the ion-storing redox composition comprises materials proven to work in conventional lithium ion batteries. In some embodiments, the positive semi-solid electroactive material comprises a lithium positive electroactive material, where the lithium cations shuttle between the negative and positive electrodes and are intercalated into solid host particles suspended in a liquid electrolyte. In some embodiments, the lithium cations can be intercalated into the solid matrix of a solid high capacity material.

[0028] In some embodiments, the redox active compounds may be organic or inorganic and may include, but are not limited to, lithium metal, sodium metal, lithium metal alloys, gallium and indium alloys with or without dissolved lithium, molten transition metal chlorides, thionyl chloride, etc., or redox polymers and organics that may become liquid under the operating conditions of the battery. Such liquid forms may also be diluted or mixed with another non-redox active liquid that is a diluent or solvent, including mixing with such a diluent to form a lower melting point liquid phase.

[0029] In some embodiments, the redox-active electrode material may include organic redox compounds that store the working ion of interest at a potential useful for either the positive or negative electrode of the battery. Such organic redox-active storage materials include "p"-doped conductive polymers such as polyaniline or polyacetylene-based materials, polynitroxide or organic radical electrodes (such as those described in H. Nishide et al., Electrochim. Acta, 50, 827-831, (2004), and K. Nakahara et al., Chem. Phys. Lett., 359, 351-354 (2002)), carbonyl-based organics, and compounds such as Li2C6O6, Li2C8H4O4, Li2C6H4O4 (see, for example, M. Armand et al., Nature Materials, DOI:10.1038 / nmat2372), and oxocarbons and carboxylates, including organosulfur compounds. In some embodiments, the conventional active materials include cobalt, manganese, nickel-cadmium-manganese, phosphate, lithium manganese oxide, lithium iron phosphate, lithium cobalt oxide, LiNi 0.8 Co 0.15 Al 0.05 The lithium alloys and lithium alloy forming compounds may include silicon, bismuth, boron, gallium, indium, zinc, tin, tin oxide, antimony, aluminum, titanium oxide, molybdenum, germanium, manganese, niobium, vanadium, tantalum, gold, platinum, iron, copper, chromium, nickel, cobalt, zirconium, yttrium, molybdenum oxide, germanium oxide, silicon oxide, silicon carbide, and other suitable chemicals.

[0030] In some embodiments, conductive materials for the electrode materials may include, for example, graphite, carbon powder, pyrolitic carbon, carbon black, carbon fiber, carbon microfiber, carbon nanotubes (CNTs), single-walled CNTs, multi-walled CNTs, fullerene carbon including "buckyballs", graphene sheets and / or aggregates of graphene sheets, other conductive materials, metals (Cu, Al, powders, etc.), alloys, or combinations thereof.

[0031] In some embodiments, the electrolyte for the electrode material may include a non-aqueous liquid electrolyte, which may include, for example, a polar solvent such as an alcohol or an aprotic organic solvent. Many organic solvents have been proposed as components of Li-ion battery electrolytes, particularly the cyclic carbonate family and their chlorinated or fluorinated derivatives, such as ethylene carbonate, propylene carbonate, butylene carbonate, and the acyclic dialkyl carbonate family, such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, dibutyl carbonate, butyl methyl carbonate, butyl ethyl carbonate, and butyl propyl carbonate. Other solvents proposed as components of Li-ion battery electrolyte solutions include γ-butyrolactone, dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, diethyl ether, sulfolane, methyl sulfolane, acetonitrile, propiononitrile, ethyl acetate, methyl propionate, ethyl propionate, dimethyl carbonate, tetraglyme, and the like. In some embodiments, these non-aqueous solvents can be used as multi-component mixtures in which salts are dissolved to provide ionic conductivity. In some embodiments, the salt providing lithium conductivity may include LiClO4, LiPF6, LiBF4, LiFSI, LiAsF6, LiTFSI, LiBETI, LiBOB, etc. In some embodiments, the electrochemical cell may include a selectively permeable membrane configured to separate electrolyte molecules on the cathode side from electrolyte molecules on the anode side. This selectively permeable membrane may enable the use of multiple electrolytes (i.e., anolyte on the anode side and catholyte on the cathode side), as described in U.S. patent application Ser. No. 16 / 242,849, entitled "Electrochemical Cell Including a Selectively Permeable Membrane, Systems and Methods for Manufacturing Thereof," filed Jan. 8, 2019 (the "'849 Application"), the disclosure of which is incorporated herein by reference in its entirety.

[0032] In some embodiments, the binder is selected from the group consisting of starch, carboxymethylcellulose (CMC), diacetyl cellulose, hydroxypropyl cellulose, ethylene glycol, polyacrylates, poly(acrylic acid), polytetrafluoroethylene, polyimides, polyethylene oxide, poly(vinylidene fluoride), rubber, ethylene-propylene-diene monomer (EPDM), hydrophilic binders, polyvinylidene fluoride (PVDF), styrene butadiene copolymer, poly(3,4-ethylenedioxythiophene):poly(styrenesulfonate) (PEDOT:PSS), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), maleic anhydride grafted polyvinylidene fluoride (MPVDF), styrene butadiene rubber (SBR), S The polymeric material may include a mixture of BR and sodium carboxymethylcellulose (SBR+CMC), polyacrylonitrile, fluorinated polyimide, poly(3-hexylthiophene)-b-poly(ethylene oxide), poly(1-pyrene methyl methacrylate) (PPy), poly(1-pyrene methyl methacrylate-co-methacrylic acid) (PPy-MAA), poly(1-pyrene methyl methacrylate-co-triethylene glycol methyl ether) (PPyE), polyacrylic acid and its lithium salts (PAA), sodium polyacrylate, fluorinated polyacrylic acid, polyimide (PI), polyamideimide (PAI), polyetherimide (PEI), other suitable polymeric materials configured to provide sufficient mechanical support to the electrode material, and combinations thereof. In some embodiments, the electrode material can include from about 0.01% to about 30% by weight, from about 1% to about 20% by weight, from about 2% to about 19% by weight, from about 3% to about 18% by weight, from about 4% to about 17% by weight, from about 5% to about 16% by weight, from about 6% to about 15% by weight, or from about 5% to about 20% by weight (including all values ​​and ranges) of binder.

[0033] In some embodiments, the thickness of the electrode 100 can be at least about 30 μm. In some embodiments, the thickness of the semi-solid electrode can be at least about 100 μm, at least about 150 μm, at least about 200 μm, at least about 250 μm, at least about 300 μm, at least about 350 μm, at least about 400 μm, at least about 450 μm, at least about 500 μm, at least about 600 μm, at least about 700 μm, at least about 800 μm, at least about 900 μm, at least about 1,000 μm, at least about 1,500 μm, and up to about 2,000 μm (including all thicknesses therebetween). In some embodiments, the thickness of the first electrode material 120 can be less than about 50% of the total thickness of the electrode 100. In some embodiments, the thickness of the first electrode material 120 can be less than about 45%, less than about 40%, less than about 35%, less than about 30%, less than about 25%, less than about 20%, less than about 15%, less than about 10%, less than about 5%, or less than about 3% of the total thickness of the electrode 100. In some embodiments, the thickness of the first electrode material 120 can be less than about 80 μm, less than about 70 μm, less than about 60 μm, less than about 50 μm, less than about 40 μm, less than about 30 μm, less than about 20 μm, less than about 10 μm, less than about 5 μm, less than about 2 μm, or less than about 1 μm.

[0034] In some embodiments, the thickness of the second electrode material 130 may be at least about 20% of the total thickness of the electrode 100. In some embodiments, the thickness of the second electrode material 130 may be at least about 50%, at least about 60%, at least about 70%, at least about 80%, at least about 90%, at least about 95%, at least about 97%, at least about 98%, or at least about 99% of the total thickness of the electrode 100. In some embodiments, the thickness of the second electrode material 120 may be at least about 30 μm. In some embodiments, the thickness of the second electrode material 120 may be at least about 50 μm, at least about 100 μm, at least about 150 μm, at least about 200 μm, at least about 250 μm, at least about 300 μm. It can be at least about 350 μm, at least about 400 μm, at least about 450 μm, at least about 500 μm, at least about 600 μm, at least about 700 μm, at least about 800 μm, at least about 900 μm, at least about 1,000 μm, at least about 1,500 μm, and up to about 2,000 μm (including all thicknesses therebetween).

[0035] In some embodiments, the first electrode material 120 may include a solid electrode material manufactured according to a conventional solid electrode manufacturing process. In some embodiments, the solid electrode material may be manufactured by forming a slurry including an active material, a conductive additive, and a binder dissolved or dispersed in a solvent. The slurry is disposed on an electrode current collector or other suitable structure in an electrochemical cell, and then dried (e.g., by evaporating the solvent) and calendared to a specified thickness. Manufacturing of the solid electrode material may also generally include mixing, casting, calendaring, drying, cutting, and processing (bending, rolling, etc.) of the material according to the battery structure being constructed. Once the electrode material is dried and calendared, it may be wetted (e.g., under pressure) with an electrolyte.

[0036] In some embodiments, the first electrode material 120 may comprise a solid electrode material produced by a deposition process, including evaporation, electron beam deposition, electrochemical deposition, sol-gel, sputtering, and physical spray methods.

[0037] In some embodiments, the second electrode material 130 may include a pure conductive agent dispersed on the first electrode material 120. Coating a conductive slurry (without active material) on the first electrode material 120 as an electrolyte serves as an alternative method for electrolyte release in conventional cell manufacturing processes. The conductive agent, especially with a volume expansion material, can flow into the first electrode material 120 during cycling and fill voids. In other words, the use of the conductive agent can help maintain the electronic conductivity of the electrode, thereby improving the cycling stability of the first electrode material 120.

[0038] In some embodiments, the second electrode material 130 may comprise a semi-solid electrode material. In some embodiments, the semi-solid electrode materials described herein can be made (i) thicker than solid electrode materials (e.g., 250 μm up to 2,000 μm, or thicker) due to the reduced tortuosity and higher electronic conductivity of the semi-solid electrodes, (ii) with higher active material loadings than conventional electrode materials, and (iii) by simplified manufacturing processes using less equipment. These relatively thick semi-solid electrodes reduce the volume, mass, and cost contributions of inactive components to the active components, thereby enhancing the commercial appeal of electrodes that include semi-solid electrode materials. In some embodiments, the second electrode material 130 can be disposed on the first electrode material 120 without a drying step. Eliminating the drying step can potentially reduce processing time and manufacturing costs. In some embodiments, the second electrode material 130 can be disposed on a separator (not shown), and then the separator with the second electrode material 130 can be combined with the first electrode material 120 disposed on the current collector 110. In some embodiments, the second electrode material 130 can include a binder. In some embodiments, the second electrode material 130 can be substantially free of a binder.

[0039] In some embodiments, the semi-solid electrode materials described herein can be binder-free. Instead, the volume typically occupied by the binder of conventional electrodes in the semi-solid electrode materials is now occupied by 1) electrolytes, which have the effect of reducing tortuosity and increasing the total salt available for ion diffusion, thereby countering the salt depletion effect typical of conventional thick electrodes at high rates, 2) active materials, which have the effect of increasing the charge capacity of the battery, or 3) conductive additives, which have the effect of increasing the electronic conductivity of the electrode, thereby countering the high internal impedance of conventional thick electrodes. The reduced tortuosity and higher electronic conductivity of the semi-solid electrodes described herein result in superior rate capability and charge capacity of electrochemical cells formed from the semi-solid electrodes.

[0040] The semi-solid electrode materials described herein can be made substantially thicker than conventional electrode materials, allowing for a much higher ratio of active material to inactive material. In some embodiments, this increased active to inactive material ratio can increase the overall charge capacity and energy density of batteries that include the semi-solid electrode materials described herein.

[0041] As described herein, solid electrode materials are typically dense (have lower porosity), while semi-solid electrode materials are typically less dense (have higher porosity). Without wishing to be bound by a particular theory, the lower porosity of the solid electrode material may result in a lower probability of ion conduction to the available active material due to increased tortuosity of the ions throughout the thickness of the electrode. In some embodiments, the first electrode material 120 may include a solid electrode material and the second electrode material 130 may include a semi-solid electrode material such that the composition gradient throughout the thickness of the electrode includes a change in porosity. Without wishing to be bound by a particular theory, by creating a porosity gradient throughout the thickness of the electrode 100, the total theoretical energy density of the electrode 100 is higher due to the use of conventional electrode materials, and the accessibility of conventional active materials to ions remains high due to the high ion flux throughout the semi-solid electrode material.

[0042] In some embodiments, the first electrode material 120 has been described as comprising a solid electrode material and the second electrode material 130 has been described as comprising a semi-solid electrode material, although other configurations and chemistries are possible. For example, in some embodiments, the first electrode material 120 may comprise a semi-solid electrode material having a first composition, and the second electrode material 130 may comprise a semi-solid electrode material having a second composition. In some embodiments, the first electrode material 120 may comprise a semi-solid electrode material having a first porosity, and the second electrode material 130 may comprise a semi-solid electrode material having a second porosity that is greater than the first porosity. In some embodiments, the first electrode material 120 may comprise a semi-solid electrode material having a first ion storage capacity, and the second electrode material 130 may comprise a semi-solid electrode material having a second ion storage capacity that is less than the first ion storage capacity. In some embodiments, the first electrode material 120 may include a semi-solid electrode material having a first ionic conductivity, and the second electrode material 130 may include a semi-solid electrode material having a second ionic conductivity greater than the first ionic conductivity.

[0043] In some embodiments, the first electrode material 120 can have a first porosity and the second electrode material 130 can have a second porosity that is less than the first porosity. In some embodiments, the second porosity can be greater than the first porosity. In some embodiments, the second porosity can be substantially equal to the first porosity.

[0044] In some embodiments, the first porosity can be less than about 3% or less than about 5%. In some embodiments, the first porosity can be about 20% to about 25%, about 25% to about 30%, about 30% to about 35%, about 35% to about 40%, about 40% to about 45%, about 45% to about 50%, about 50% to about 55%, or about 55% to about 60%.

[0045] In some embodiments, the second porosity can be about 20% to about 25%, about 25% to about 30%, about 30% to about 35%, about 35% to about 40%, about 40% to about 45%, about 45% to about 50%, about 50% to about 55%, or about 55% to about 60%.

[0046] In some embodiments, the first electrode material 120 can have a first surface area and the second electrode material 130 can have a second surface area that is greater than the first surface area. In some embodiments, the second surface area can be less than the first surface area. In some embodiments, the second surface area can be substantially equal to the first surface area.

[0047] In some embodiments, the first electrode material 120 is about 1 m 2 / g. In some embodiments, the first electrode material 120 may include an active material with a surface area of ​​less than about 1 m 2 / g ~ approx. 2m 2 / g, approx. 2m 2 / g to about 3m 2 / g, approx. 3m 2 / g~about 4m 2 / g, approx. 4m 2 / g~about 5m 2 / g, or about 5m 2 The active material may include an active material with a surface area greater than 0.1 μm / g.

[0048] In some embodiments, the second electrode material 130 is about 1 m 2 / g. In some embodiments, the second electrode material 130 may include an active material with a surface area of ​​less than about 1 m 2 / g ~ approx. 2m 2 / g, approx. 2m 2 / g to about 3m 2 / g, approx. 3m 2 / g~about 4m 2 / g, approx. 4m 2 / g~about 5m 2 / g, or about 5m 2 The active material may include an active material with a surface area greater than 0.1 μm / g.

[0049] In some embodiments, during operation of the electrochemical cell, ions may be shuttled through the second electrode material 130 at a first rate and to the first electrode material 120 at a second rate that is less than the first rate. In some embodiments, the first electrode material 120 may have a first ion storage capacity and the second electrode material 130 may have a second ion storage capacity that is less than the first ion storage capacity. In some embodiments, the completed electrode may have a thickness substantially equal to the sum of the thicknesses of the current collector 110, the first electrode material 120, and the third electrode material 130. In some embodiments, the thickness of the completed composition gradient electrode may have a greater power density than an electrode formed from either only the first electrode material 120 or only the second electrode material 130 and having the same thickness as the completed composition gradient electrode.

[0050] In some embodiments, the first electrode material 120 may include a higher concentration of high expansion active material in charging, such as silicon-based (Si, SiO, Si alloys) and / or tin-based (Sn, SnO, Sn alloys), than the second electrode material 130.

[0051] The higher expansion active material may migrate to smaller particles after charge and discharge cycles due to the expansion-compression forces during cycling. These forces tend to reduce the electronic network during cycling, and the higher expansion material near the current collector can ensure the electronic pathway. In some embodiments, having a semi-solid electrode as the second electrode material 130 tends to absorb these expansion forces. In some embodiments, having a high porosity of the high expansion active material in the first electrode material 120 allows the semi-solid electrode with the higher electronic conductivity network and the lower expansion active material in the second layer to migrate to the porous region, thereby maintaining the electronic network.

[0052] In some embodiments, the energy density of a finished electrode 100 having a composition gradient (e.g., including a first electrode material 120 and a second electrode material 130) is about 0.2 MJ / L, about 0.25 MJ / L, about 0.3 MJ / L, about 0.35 MJ / L, about 0.4 MJ / L, about 0.45 MJ / L, about 0.5 MJ / L, about 0.55 MJ / L, about 0.6 MJ / L, about 0.65 MJ / L, about 0.7 MJ / L, or about 0.8 MJ / L. , about 0.75MJ / L, about 0.8MJ / L, about 0.85MJ / L, about 0.9MJ / L, about 0.95MJ / L, about 1.0MJ / L, about 1.05MJ / L, about 1.1MJ / L, about 1.15MJ / L, approx. 1.2MJ / L, approx. 1.25MJ / L, approx. 1.3MJ / L, approx. 1.35MJ / L, approx. 1.4MJ / L, approx. 1.45MJ / L, approx. 1.5MJ / L, approx. 1.55MJ / L, approx. 1.6MJ / L, approximately 1.65MJ / L, approximately 1.7MJ / L, approximately 1.75MJ / L, approximately 1.8MJ / L, approximately 1.85MJ / L, approximately 1.9MJ / L, approximately 1.95MJ / L, approximately 2.0MJ / L, approximately 2.05MJ / L, approx. 2.1MJ / L, approx. 2.15MJ / L, approx. 2.2MJ / L, approx. 2.25MJ / L, approx. 2.3MJ / L, approx. 2.35MJ / L, approx. 2.4MJ / L, approx. 2.45MJ / L, approx. 2.5MJ / L, about 2.55 MJ / L, about 2.6 MJ / L, about 2.65 MJ / L, about 2.7 MJ / L, about 2.75 MJ / L, about 2.8 MJ / L, about 2.85 MJ / L, about 2.9 MJ / L, about 2.95 MJ / L, about 3.0 MJ / L, about 3.5 MJ / L, about 4.0 MJ / L, about 4.5 MJ / L, or about 5.0 MJ / L (including all values ​​and ranges therebetween).

[0053] In some embodiments, the energy density of the first electrode material 120 is about 0.2 MJ / L, about 0.25 MJ / L, about 0.3 MJ / L, about 0.35 MJ / L, about 0.4 MJ / L, about 0.45 MJ / L, about 0.5 MJ / L, about 0.55 MJ / L, about 0.6 MJ / L, about 0.65 MJ / L, about 0.7 MJ / L, about 0.75 MJ / L, about 0.8 MJ / L, about 0.85 MJ / L, or about 0.9 MJ / L. / L, approx. 0.9MJ / L, approx. 0.95MJ / L, approx. 1.0MJ / L, approx. 1.05MJ / L, approx. 1.1MJ / L, approx. 1.15MJ / L, approx. 1.2MJ / L, approx. 1.25MJ / L, approx. 1.3MJ / L, approx. 1.35MJ / L, approx. 1.4MJ / L, approx. 1.45MJ / L, approx. 1.5MJ / L, approx. 1.55MJ / L, approx. 1.6MJ / L, approx. 1.65MJ / L, approx. 1.7MJ / L, approx. 1.75MJ / L, approx. 1.8MJ / L, approx. 1.85MJ / L, approx. 1.9MJ / L, approx. 1.95MJ / L, approx. 2.0MJ / L, approx. 2.05MJ / L, approx. 2.1MJ / L, approx. 2.15MJ / L, approx. 2.2MJ / L, approx. 2.25MJ / L, approx. 2.3MJ / L, approx. 2.35MJ / L, approx. 2.4MJ / L, approx. 2.45MJ / L, approx. 2.5MJ / L, approx. 2.55M J / L, can be greater than about 2.6 MJ / L, about 2.65 MJ / L, about 2.7 MJ / L, about 2.75 MJ / L, about 2.8 MJ / L, about 2.85 MJ / L, about 2.9 MJ / L, about 2.95 MJ / L, about 3.0 MJ / L, about 3.5 MJ / L, about 4.0 MJ / L, about 4.5 MJ / L, or about 5.0 MJ / L (including all values ​​and ranges therebetween).

[0054] In some embodiments, the energy density of the second electrode material 130 is about 0.2 MJ / L, about 0.25 MJ / L, about 0.3 MJ / L, about 0.35 MJ / L, about 0.4 MJ / L, about 0.45 MJ / L, about 0.5 MJ / L, about 0.55 MJ / L, about 0.6 MJ / L, about 0.65 MJ / L, about 0.7 MJ / L, about 0.75 MJ / L, about 0.8 MJ / L, about 0.85 MJ / L, or about 0.9 MJ / L. / L, approx. 0.9MJ / L, approx. 0.95MJ / L, approx. 1.0MJ / L, approx. 1.05MJ / L, approx. 1.1MJ / L, approx. 1.15MJ / L, approx. 1.2MJ / L, approx. 1.25MJ / L, approx. 1.3MJ / L, approx. 1.35MJ / L, approx. 1.4MJ / L, approx. 1.45MJ / L, approx. 1.5MJ / L, approx. 1.55MJ / L, approx. 1.6MJ / L, approx. 1.65MJ / L, approx. 1.7MJ / L, approx. 1.75MJ / L, approx. 1.8MJ / L, approx. 1.85MJ / L, approx. 1.9MJ / L, approx. 1.95MJ / L, approx. 2.0MJ / L, approx. 2.05MJ / L, approx. 2.1MJ / L, approx. 2.15MJ / L, approx. 2.2MJ / L, approx. 2.25MJ / L, approx. 2.3MJ / L, approx. 2.35MJ / L, approx. 2.4MJ / L, approx. 2.45MJ / L, approx. 2.5MJ / L, approx. 2.55M J / L, can be greater than about 2.6 MJ / L, about 2.65 MJ / L, about 2.7 MJ / L, about 2.75 MJ / L, about 2.8 MJ / L, about 2.85 MJ / L, about 2.9 MJ / L, about 2.95 MJ / L, about 3.0 MJ / L, about 3.5 MJ / L, about 4.0 MJ / L, about 4.5 MJ / L, or about 5.0 MJ / L (including all values ​​and ranges therebetween).

[0055] In some embodiments, the specific energy of a finished electrode 100 having a composition gradient (e.g., including a first electrode material 120 and a second electrode material 130) is about 0.2 MJ / kg, about 0.25 MJ / kg, about 0.3 MJ / kg, about 0.35 MJ / kg, about 0.4 MJ / kg, about 0.45 MJ / kg, about 0.5 MJ / kg, about 0.55 MJ / kg, about 0.6 J / kg, about 0.65 MJ / kg, about 0.7 MJ / kg, about 0.75 MJ / kg, about It can be greater than 0.8 MJ / kg, about 0.85 MJ / kg, about 0.9 MJ / kg, about 0.95 MJ / kg, about 1.0 MJ / kg, about 1.05 MJ / kg, about 1.1 MJ / kg, about 1.15 MJ / kg, about 1.2 MJ / kg, about 1.25 MJ / kg, about 1.3 MJ / kg, about 1.35 MJ / kg, about 1.4 MJ / kg, about 1.45 MJ / kg, or about 1.5 MJ / kg (including all values ​​and ranges therebetween).

[0056] In some embodiments, the specific energy of the first electrode material 120 is about 0.2 MJ / kg, about 0.25 MJ / kg, about 0.3 MJ / kg, about 0.35 MJ / kg, about 0.4 MJ / kg, about 0.45 MJ / kg, about 0.5 MJ / kg, about 0.55 MJ / kg, about 0.6 J / kg, about 0.65 MJ / kg, about 0.7 MJ / kg, about 0.75 MJ / kg, about 0.8 MJ / kg, about 0.85 MJ / kg, about 0.9 MJ / kg, about 10 MJ / kg, about 11 MJ / kg, about 12 MJ / kg, about 13 MJ / kg, about 14 MJ / kg, about 15 MJ / kg, about 16 MJ / kg, about 17 MJ / kg, about 18 MJ / kg, about 19 MJ / kg, about 20 MJ / kg, about 21 MJ / kg, about 22 MJ / kg, about 23 MJ / kg, about 24 MJ / kg, about 25 MJ / kg, about 26 MJ / kg, about 27 MJ / kg, about 28 MJ / kg, about 29 MJ / kg, about 30 MJ / kg, about 31 MJ / kg, about 32 MJ / kg, about 33 MJ / kg, about 34 MJ / kg, about 35 MJ / kg, about 36 MJ / kg, about 37 MJ / kg, about 38 MJ / kg, about 39 MJ / kg, about 40 MJ / kg, about 41 MJ / kg, about 42 MJ / kg, about 43 MJ / kg, about 44 MJ / kg, about 45 MJ / kg, about 46 MJ / kg, about 47 M kg, about 0.9 MJ / kg, about 0.95 MJ / kg, about 1.0 MJ / kg, about 1.05 MJ / kg, about 1.1 MJ / kg, about 1.15 MJ / kg, about 1.2 MJ / kg, about 1.25 MJ / kg, about 1.3 MJ / kg, about 1.35 MJ / kg, about 1.4 MJ / kg, about 1.45 MJ / kg, or about 1.5 MJ / kg (including all values ​​and ranges therebetween).

[0057] In some embodiments, the specific energy of the second electrode material 130 is about 0.2 MJ / kg, about 0.25 MJ / kg, about 0.3 MJ / kg, about 0.35 MJ / kg, about 0.4 MJ / kg, about 0.45 MJ / kg, about 0.5 MJ / kg, about 0.55 MJ / kg, about 0.6 J / kg, about 0.65 MJ / kg, about 0.7 MJ / kg, about 0.75 MJ / kg, about 0.8 MJ / kg, about 0.85 MJ / kg, about 0.9 MJ / kg, about 10 MJ / kg, about 11 MJ / kg, about 12 MJ / kg, about 13 MJ / kg, about 14 MJ / kg, about 15 MJ / kg, about 16 MJ / kg, about 17 MJ / kg, about 18 MJ / kg, about 19 MJ / kg, about 20 MJ / kg, about 21 MJ / kg, about 22 MJ / kg, about 23 MJ / kg, about 24 MJ / kg, about 25 MJ / kg, about 26 MJ / kg, about 27 MJ / kg, about 28 MJ / kg, about 29 MJ / kg, about 30 MJ / kg, about 31 MJ / kg, about 32 MJ / kg, about 33 MJ / kg, about 34 MJ / kg, about 35 MJ / kg, about 36 MJ / kg, about 37 MJ / kg, about 38 MJ / kg, about 39 MJ / kg, about 40 MJ / kg, about 41 MJ / kg, about 42 MJ / kg, about 43 MJ / kg, about 44 MJ / kg, about 45 MJ / kg, about 46 MJ / kg, about 47 M kg, about 0.9 MJ / kg, about 0.95 MJ / kg, about 1.0 MJ / kg, about 1.05 MJ / kg, about 1.1 MJ / kg, about 1.15 MJ / kg, about 1.2 MJ / kg, about 1.25 MJ / kg, about 1.3 MJ / kg, about 1.35 MJ / kg, about 1.4 MJ / kg, about 1.45 MJ / kg, or about 1.5 MJ / kg (including all values ​​and ranges therebetween).

[0058] In some embodiments, the first electrode material 120 may include about 10 vol%, about 20 vol%, about 30 vol%, about 40 vol%, about 50 vol%, about 60 vol%, about 70 vol%, about 80 vol%, about 90 vol%, or about 100 vol% of the high capacity anode material. In some embodiments, the second electrode material 130 may include a high capacity anode material combined with carbon, graphite, or other active materials with or without a binder. In some embodiments, the second electrode material 130 may include less than about 60 vol%, less than about 55 vol%, less than about 50 vol%, less than about 45 vol%, less than about 40 vol%, less than about 35 vol%, less than about 30% vol%, less than about 25 vol%, less than about 20 vol%, less than about 15 vol%, less than about 10 vol%, or less than about 5 vol% of the high capacity anode material. In some embodiments, the second electrode material 130 may be substantially free of high capacitance materials.

[0059] As noted above, electrode 100 includes two layers of different anode materials. In some embodiments, electrode 100 may alternatively include two or more layers of different cathode materials. In some embodiments, first electrode material 120 and / or second electrode material 130 may include any material that can be used as a cathode in a lithium-ion battery. Examples of cathode materials that can be used in electrochemical cells are described in the '159 patent incorporated by reference above.

[0060] Typically, the current collector 110 in the cathode used in lithium-ion batteries is made of aluminum coated with conductive carbon. The conductive carbon coating can improve the electrical conductivity and increase the mechanical strength of the current collector 110, thereby reducing the possibility of cracking of the current collector 110. In some embodiments, the first electrode material 120 can be disposed on the bare aluminum current collector instead of the conductive carbon layer. In some embodiments, the first electrode material 120 in the cathode can be manufactured and / or deposited via the same methods as in the anode, as described above. In some embodiments, the first electrode material 120 in the cathode can have the same or similar thickness as the first electrode material 120 in the anode, as described above. In some embodiments, the second electrode material 130 in the cathode can be a semi-solid cathode and can be deposited via the same methods as in the anode, as described above. In some embodiments, the second electrode material 130 in the cathode can have a similar thickness as the second electrode material 130 in the anode, as described above.

[0061] In some embodiments, the volume percentage of the high capacity anode material in the second electrode material 130 may be about 10-80% less than the volume percentage of the high capacity anode material in the first electrode material 120.

[0062] In some embodiments, the cycle life of a completed electrode 100 having a composition gradient (e.g., including a first electrode material 120 and a second electrode material 130) is greater than about 200 charge / discharge cycles, greater than about 250 cycles, greater than about 300 cycles, greater than about 350 cycles, greater than about 400 cycles, greater than about 450 cycles, greater than about 500 cycles, greater than about 550 cycles, greater than about 600 cycles, greater than about 650 cycles, greater than about 700 cycles, greater than about 750 cycles, greater than about 800 cycles, greater than about 850 cycles, greater than about 900 cycles, greater than about 950 cycles, greater than about 1,000 cycles, greater than about 1,050 cycles, greater than about The number of cycles may be greater than about 1,100, greater than about 1,250, greater than about 1,300, greater than about 1,350, greater than about 1,400, greater than about 1,450, greater than about 1,500, greater than about 1,550, greater than about 1,600, greater than about 1,650, greater than about 1,700, greater than about 1,750, greater than about 1,800, greater than about 1,850, greater than about 1,900, greater than about 1,950, greater than about 2,000, greater than about 2,500, greater than about 3,000, greater than about 5,000, or greater than about 10,000 cycles.

[0063] In some embodiments, the charge rate of an electrochemical cell including a finished electrode 100 having a composition gradient (e.g., including a first electrode material 120 and a second electrode material 130) can be less than about 5 hours, less than about 4.5 hours, less than about 3 hours, less than about 3 hours, less than about 2.5 hours, less than about 2 hours, less than about 1.5 hours, or less than about 1 hour (including all values ​​and ranges therebetween) per 100 g of electrode material at a rate of 1C. In some embodiments, having a semi-solid electrode second electrode material 130 and a conventional (i.e., "dry") first electrode material 120 can avoid the electrolyte filling process, which is typically the last step in a conventional battery manufacturing process. This can also lead to higher loading in the first electrode material 120 by allowing the electrolyte present in the second electrode material 130 to saturate the first electrode material 120.

[0064] Before lithiation Many electrodes, e.g., lithium-ion electrodes, especially anodes, can suffer from irreversible capacity loss during the battery formation stage (i.e., the first cycling step involving charging and discharging an electrochemical cell containing the electrode). Irreversible capacity loss can occur due to the consumption of lithium ions from the cathode active material by the anode, which uses these lithium ions to form a solid electrolyte interface (SEI) layer. This amount of consumed lithium represents an undesirable irreversible capacity loss, since it is no longer available for use in subsequent charge storage. Furthermore, this irreversible capacity loss can be accompanied by a volume expansion of the anode, as lithium ions are irreversibly trapped in the anode material. This volume expansion problem is exacerbated with semi-solid anodes that include high capacity anode materials (e.g., silicon or tin) in the semi-solid anode formulation. This is because the high capacity anode materials can incorporate larger amounts of lithium (and enable higher energy cell designs) compared to conventional materials such as graphite. For example, graphite can incorporate about one lithium atom for every six carbon atoms, while silicon can theoretically incorporate about 4.4 lithium atoms for every silicon atom.

[0065] This higher capacity allows the formation of electrochemical cells with much higher charge capacity per unit area compared to conventional electrochemical cells, but the larger number of lithium ions incorporated means that the semi-solid anodes containing high capacity materials will have a larger irreversible capacity as they consume more lithium from the cathode to form the SEI layer. Furthermore, silicon undergoes significant volume expansion as lithium ions are incorporated into silicon atoms. Repeated volume changes (i.e., expansion and / or contraction) can cause irreversible mechanical damage that can adversely affect charge capacity and shorten the life of the electrochemical cell. A detailed description of the effect of lithiation on the stress and morphology of silicon electrodes is provided in “In situ Measurements of Stress Evolution in Silicon Thin Films During Electrochemical Lithiation and Delithiation” by V. Sethuraman et al., Journal of Power Sources 195 (2010) 5062-5066, the contents of which are incorporated herein by reference in their entirety.

[0066] In some embodiments, the electrodes described herein may be prelithiated electrodes, for example, prelithiated during mixing of semi-solid electrode materials or prelithiated during assembly of the electrode. In some embodiments, such prelithiation may help form an SEI layer in the electrode before electrochemical cell formation and before the first charge / discharge cycle is completed. In some embodiments, the prelithiation of the electrode may be prelithiation of the anode. In some embodiments, the prelithiation may be performed by disposing a lithium-containing material in the anode so that lithium ions are more easily and early in the battery formation process by the anode active material.

[0067] 2 is a schematic diagram of an electrode 200 including a first electrode material 220, a second electrode material 230, and a lithium-containing material 240 disposed in any suitable order on a current collector 210. In some embodiments, the first electrode material 220 and / or the second electrode material 230 can include at least one of a solid electrode material, a semi-solid electrode material, a high capacity material, and combinations thereof (collectively "electrode materials"). In some embodiments, the electrode 200 is an anode.

[0068] In some embodiments, the electrode materials described herein can be pre-lithiated with lithium-containing material 240 during preparation of electrode 200 and prior to formation of an electrochemical cell, thereby at least partially overcoming the above-mentioned problems of irreversible capacity loss and volume expansion. The semi-solid electrode materials described herein allow for the mixing of lithium-containing materials into the semi-solid electrode material. Without wishing to be bound by a particular theory, this may be possible because the semi-solid electrode materials described herein include an electrolyte mixed into the semi-solid electrode composition. The electrolyte provides a medium for the lithium ions provided by the lithium-containing material 240 to interact with the active materials included in the semi-solid electrode material, particularly the active materials (e.g., graphite) or high-capacity materials (e.g., silicon or tin) included in the semi-solid anode material. This allows for the formation of an SEI layer during the mixing step, so that when such a pre-lithiated electrode 200 is paired with a second electrode (not shown, e.g., a cathode) in an electrochemical cell, the lithium ions from the second electrode are not used to form an SEI layer in the pre-lithiated electrode 200. In other words, due to the pre-lithiation, the lithium ions from the second electrode (e.g., cathode) do not contribute to irreversible capacity loss in the pre-lithiated electrode 200. In some embodiments, since the lithium ions from the second electrode do not contribute to irreversible capacity loss in the pre-lithiated electrode 200, it may enable the second electrode (e.g., cathode) to maintain its initial capacity after electrochemical cell formation. Furthermore, the electrolyte included in the electrode 200 may also protect the lithium-containing material 240 from the surrounding environment (e.g., moisture or humidity of the surrounding environment), thereby enabling the lithium-containing material 240 to remain stable during the mixing process.

[0069] In some embodiments, prelithiation may be performed by disposing a lithium-containing material 240 in the electrode 200 at some point during the manufacture of the electrode 200. In some embodiments, the lithium-containing material 240 may be disposed between the first electrode material 220 and the second electrode material 230. In some embodiments, the lithium-containing material 240 may be disposed between the current collector 210 and the first electrode material 220. In some embodiments, the lithium-containing material 240 may be disposed between the second electrode material 230 and a subsequently disposed electrode material layer (not shown). In some embodiments, the lithium-containing material 240 may be disposed between the second electrode material 230 and a separator (not shown) that is ionically permeable and configured to separate the electrode 200 from the second electrode.

[0070] In some embodiments, the lithium-containing material 240 can be formed according to any suitable form factor, including, but not limited to, a sheet, a slurry, a suspension, a plurality of particles, a powder, an alloy solution, and combinations thereof.

[0071] In some embodiments, the lithium-containing material 240 may include lithium metal and a binder. In some embodiments, the lithium-containing material 240 may further include a carbonaceous (e.g., graphite) material. In some embodiments, the lithium-containing material 240 may initially include a solvent that is removed during drying of the electrode material.

[0072] Another advantage provided by the prelithiation of the semi-solid electrodes described herein is that the anode may be prelithiated so that it is fully charged before being paired with the cathode. This allows for the use of a cathode that does not have lithium available to form an SEI layer in the anode. Thus, carbon-based anode materials can be used instead of lithium metal, leading to improved cycle stability and safety. Furthermore, lithium ion insertion into the high capacity material contained in the anode can also occur during the mixing step, which allows any expansion of the high capacity material to occur during the mixing step. In other words, the prelithiation can pre-expand the semi-solid anode, such that the semi-solid anode experiences less expansion during electrochemical cell formation and subsequent charge / discharge cycles. In this way, physical damage to the electrochemical cell due to the expansion of the semi-solid anode can be substantially reduced or in some cases eliminated. Thus, an electrochemical cell including such a prelithiated semi-solid anode may have substantially higher mechanical stability and longer life compared to anodes (e.g., semi-solid anodes) that are not prelithiated.

[0073] In some embodiments, additional electrolyte can be added after or during the prelithiation process, where electrolyte is consumed to generate the SEI, and electrolyte is added to reduce the electrode in the absence of electrolyte locally within the electrode.

[0074] Additional examples of devices, methods, and systems for prelithiation of electrodes can be found in U.S. Patent Application No. 2016 / 0126543, entitled “Prelithiation of Electrode Materials in Semi-Solid Electrodes,” filed November 3, 2015 (the “'543 Publication”), the entire disclosure of which is incorporated herein by reference.

[0075] high capacity material In some embodiments, higher energy density and capacity can be achieved, for example, by improving the materials used in the anode and / or cathode and / or increasing the thickness of the anode / cathode (i.e., a higher ratio of active material to inactive material). One of the latest materials used in consumer electronics anodes is silicon (Si), tin (Sn), silicon alloys, or tin alloys, for example, due to its high capacity and low voltage. Typically, this high capacity active material is mixed with graphite due to its high first charge capacity and associated first charge irreversible capacity. Silicon has an initial charge theoretical capacity of 4,200 mAh / g and an irreversible capacity of greater than 300 mAh / g. Thus, common anodes utilizing Si contain a mixture of silicon and graphite to reduce the irreversible capacity. In addition, silicon undergoes a very large volume change during lithium insertion, increasing the volume of the material by more than 300%. To limit this large volume expansion, current high capacity anodes utilize 10-20% silicon in the anode mix, resulting in an anode with an overall capacity of about 700 to about 4,200 mAh / g.

[0076] Conventional cathode compositions have a capacity of about 150-200 mAh / g and cannot be thicker than 200 μm because conventional electrodes manufactured using high-speed roll-to-roll calendaring tend to delaminate at thicknesses of about 200 μm compared to flat current collectors. Also, thicker electrodes have higher cell impedances that reduce energy efficiency (e.g., as described in Yu et al., “Effect of electrode parameters on LiFePO4 cathodes,” J. Electrochem. Soc. Vol. 153, A835-A839 (2006)). Thus, to match high-capacity anodes with conventional cathodes, current state-of-the-art batteries have focused on reducing the thickness of the anode. For example, anodes with thicknesses of about 40-50 μm and even thinner have been developed. Such thin coatings of these anode materials are beginning to approach the thickness level of a single graphite particle. Thickness and associated loading density limitations in conventional coating processes have hindered the development of batteries that take full advantage of the high capacity available in high-energy anodes.

[0077] When a high capacitance material is incorporated into, for example, electrode 100 or electrode 200, the associated swelling during operation can cause damage to the electrode and electrochemical cells constructed therefrom. However, the use of the semi-solid electrode materials described herein in conjunction with a high capacitance material in an electrode has the surprising and unexpected result of less damage to the electrode due to swelling of the high capacitance material.

[0078] FIG. 3 is a side view of an electrode 300 including a first electrode material 320 disposed on a current collector 310 and a second electrode material 330 disposed on the second electrode material 320. In some embodiments, the first electrode material 320 and / or the second electrode material 330 may include at least one of a solid electrode material, a semi-solid electrode material, a high-capacity material, and combinations thereof (collectively, "electrode materials"). In some embodiments, a portion of the first electrode material 320 may be removed (e.g., by laser ablation) to expose a portion of the current collector 310. In some embodiments, the removal of the portion of the first electrode material 320 may form a plurality of extended regions 330a, 330b, 330c. In some embodiments, when the second electrode material 330 is disposed on the first electrode material 320, at least a portion of the second electrode material 330 may be interposed within the plurality of extended regions 330a, 330b, 330c. In some embodiments, rather than removing portions of the first electrode material 320 to form the plurality of extended regions 330a, 330b, 330c, the plurality of extended regions 330a, 330b, 330c may be formed by selective deposition of the first electrode material 320 onto the current collector 310. In some embodiments, selective deposition of the first electrode material 320 onto the current collector 310 may be accomplished by first disposing a mask material onto the current collector 310, then disposing the first electrode material 320 onto the current collector 310, and removing the mask to define the plurality of extended regions 330a, 330b, 330c. In some embodiments, at least one of the first electrode material 120 and the second electrode material 130 may include a high capacitance material. In some embodiments, the high capacitance material may have any suitable form factor, such as a sheet, a bulk material, microscale particles, nanoscale particles, or a combination thereof.In some embodiments, the high capacity material may include any material capable of storing ions, including, but not limited to, silicon, bismuth, boron, gallium, indium, zinc, tin, antimony, aluminum, titanium oxide, molybdenum, germanium, manganese, niobium, vanadium, tantalum, iron, copper, gold, platinum, chromium, nickel, cobalt, zirconium, yttrium, molybdenum oxide, germanium oxide, silicon oxide, silicon carbide, other high capacity materials or alloys, and any combination thereof.

[0079] In some embodiments, the electrode 300 may include about 66% to 70% by weight Si, about 15% to 22% by weight Co, and about 4% to 12% by weight C. In some embodiments, the electrode 300 may include about 70% by weight Si, about 15% to 20% by weight Ni, and about 10% to 15% by weight C. In some embodiments, the electrode 300 may include about 70% by weight Si, about 15% by weight Fe, and about 15% by weight C. In some embodiments, the electrode 300 may include about 70% by weight Si, about 20% by weight Ti, and about 10% by weight C. In some embodiments, the electrode 300 may include about 70% by weight Si, about 15% by weight Mo, and about 15% by weight C. In some embodiments, the electrode 300 may include about 70% Si, 15% Co, 5% Ni, and about 10% C by weight. In some embodiments, the electrode 300 may include about 70% C, 10% Co, 10% Ni, and about 10% C by weight. In some embodiments, the electrode 300 may include about 70% Si, 5% Co, 15% Ni, and about 10% Si by weight. In some embodiments, the electrode 300 may include about 70% Si, 5% Fe, 10% Ni, and about 15% C by weight. In some embodiments, the electrode 300 may include about 70% Si, 10% Co, and about 5% Ni by weight. In some embodiments, the electrode 300 may include about 74% Si, 2% Sn, and about 24% Co by weight. In some embodiments, the electrode 300 may include about 73% Si, about 2% Sn, and about 25% Ni by weight. In some embodiments, the electrode 300 may include about 70% Si, 10% Fe, about 10% Ti, and about 10% Co by weight. In some embodiments, the electrode 300 may include about 70% Si, about 15% Fe, about 5% Ti, and about 10% C by weight. In some embodiments, the electrode 300 may include about 74.67% Si, 16% Fe, 5.33% Ti, and 4% C by weight. In some embodiments, the electrode 300 may include about 55% Si, 29.3% Al, and about 15.7% Fe by weight.In some embodiments, the electrode 300 may include about 70% Si, about 20% C from the precursor, and about 10% graphite by weight. In some embodiments, the electrode 300 may include about 55% Si, about 29.3% Al, and about 15.7% Fe by weight. In some embodiments, the electrode 300 may include about 60-62% Si, about 16-20% Al, about 12-14% Fe, and about 8% Ti by weight. In some embodiments, the electrode 300 may include about 50% Sn, about 27.3%-35.1% Co, about 5%-15% Ti, and about 7.7%-9.9% C by weight. In some embodiments, electrode 300 can include about 50 wt % Sn, about 39-42.3 wt % Co, and about 7.7-11 wt % C. In some embodiments, electrode 300 can include about 35-70 mol % Si, about 1-45 mol % Al, about 5-25 mol % transition metal, about 1-15 mol % Sn, about 2-15 mol % yttrium, a lanthanide element, an actinide element, or a combination thereof.

[0080] In some embodiments, the electrode 300 may include a tin metal alloy, such as, for example, Sn-Co-C, Sn-Fe-C, Sn-Mg-C, or La-Ni-Sn alloys. In some embodiments, the electrode 300 may include an amorphous oxide, such as, for example, an SnO or SiO amorphous oxide. In some embodiments, the electrode 300 may include a glassy anode, such as, for example, an Sn-Si-Al-BO, Sn-Sb-SO, SnO2-P2O5, or SnO-B2O3-P2O5-Al2O3 anode. In some embodiments, the electrode 300 may include a metal oxide, such as, for example, CoO, SnO2, or V2O5. In some embodiments, the electrode 300 may include a metal oxide, such as, for example, Li3N or Li 2.6 Co O.4 The nitrides may include metal nitrides such as N.

[0081] In some embodiments, the electrode 100 including the high capacitance material can be an anode, the first electrode material 120 can include the high capacitance material, and the second electrode material 130 can include a semi-solid electrode material. In some embodiments, the portion of the first electrode material 120 including the high capacitance material that is removed to form the plurality of expansion regions 330a, 330b, 330c can be substantially filled by the semi-solid electrode material when the second electrode material 330 is disposed on the first electrode material 320. While not wishing to be bound by a particular theory, when the electrochemical cell is operating, the high capacitance material can expand up to about 400%, expanding the first electrode material 320. In some embodiments, the second electrode material 330 can be configured to deform when the first electrode material 320 expands and / or contracts during operation of the electrochemical cell.

[0082] FIG. 4 illustrates an electrode 400 including a current collector 410, a first electrode material 420, and a second electrode material 430. The current collector 410, the first electrode material 420, and the second electrode material 430 may be substantially similar or identical to the current collector 110, the first electrode material 120, and the second electrode material 130, as described above with reference to FIG. 1, and therefore will not be described in detail herein. In some embodiments, the first electrode material 420 may include sputtered or electroplated silicon, and the second electrode material 430 may include a semi-solid electrode material. During operation, the first electrode material 420 (e.g., a sputtered silicon electrode) may develop cracks during cycling and split into multiple separate parts (e.g., 420a, 420b, 420c). These cracks may restrict the movement of electrons in the horizontal direction (e.g., in the x- or y-direction). In other words, electrons may only be able to move laterally efficiently within the second electrode material 430. This reduced electron mobility may result in lower energy density or power density performance in electrochemical cells including the first electrode material 420.

[0083] 5, in some embodiments, the electrode 500 may include a current collector 510, a first electrode material 520, a second electrode material 530, and a third electrode material 540 disposed between the first electrode material 520 and the second electrode material 530. The current collector 510, the first electrode material 520, and the second electrode material 530 may be substantially similar or identical to the current collector 110, the first electrode material 120, and the second electrode material 130, as described above with reference to FIG. 1, and therefore will not be described in detail herein. In some embodiments, the first electrode material 520 may include sputtered or electroplated silicon. In some embodiments, the third electrode material 540 may include graphite. The components of the first electrode material 520 (e.g., silicon) may continuously react with the electrolyte solution in the electrochemical cell, and it may be difficult to control the SEI on the surface of the first electrode material 520. In some embodiments where the first electrode material 520 is sputtered or electroplated, the first electrode material 520 has low porosity (i.e., less surface area for reaction with the electrolyte), but chemical reactions can still occur at the interface with the electrolyte. Thus, by coating the first electrode material 520 with a third electrode material 540, including, for example, graphite, these interfacial chemical reactions can be minimized. In other words, in some embodiments, cracks in the first electrode material 520 may occur, but by coating with the third electrode material 540, the cracks can be minimized or reduced. Furthermore, the conductive material (e.g., graphite) in the third electrode material 540 and the second electrode material 530 can migrate into the interstitial regions resulting from the cracks in the first electrode material 520. The presence of conductive material in these interstitial regions can facilitate the vertical movement of electrons (i.e., z-direction) and correct the performance degradation caused by silicon cracks.

[0084] Additional examples of electrodes and electrochemical cells including high capacity materials, and methods of making them, can be found in U.S. Pat. No. 9,437,864, entitled "Asymmetric Battery With Semi-Solid Cathode and High Energy Density Anode," filed Sep. 6, 2016, the entire disclosure of which is incorporated herein by reference.

[0085] Although various system, method and device embodiments have been described above, it should be understood that they are presented by way of example only, and not by way of limitation. Where the above methods and steps show certain events occurring in a particular order, those skilled in the art having the benefit of this disclosure will recognize that the order of certain steps can be changed and such changes are in accordance with variations of the invention. In addition, some of the steps can be performed simultaneously in a parallel process, where possible, or can be performed sequentially as described above. Although embodiments have been particularly shown and described, it will be understood that various changes in form and details can be made.

[0086] Example 1 (Si / semi-solid graphite and Li) Electrochemical cell example 1 (also referred to as "Ex1") was prepared using a semi-solid / Si anode and a Li metal anode. The semi-solid cathode was prepared by mixing 60 vol.% graphite powder and 2 vol.% carbon conductive additive with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The anode slurry was prepared using a roller mill and centrifugal mixing process. Mixing was performed at 1100 rpm for 2 minutes. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a solubility of 1.5×10 ー4 The slurry was fabricated into a 250 μm thick electrode and tested against a Li metal anode in a pouch cell configuration. The cell was tested using a Maccor battery tester and cycled over a voltage range of V=0.005V to 1V. The cell was charged using a constant current-constant voltage at a constant current rate of C / 10. The cell was discharged at C / 10. Figure 6 shows the first cycle of this bilayer anode cell.

[0087] Example 2 (LiMnPO4 / semi-solid cathode and Li) Electrochemical cell example 2 (also referred to as "Ex2") was prepared using a semi-solid NMC / conventional coating LiMnPO4 cathode and Li metal anode. A first layer of conventional coating LiMnPO4 slurry was made by mixing 80 wt% LiMnPO4, 10 wt% carbon black, and 10 wt% PVDF, then diluting with NMP in a centrifugal mixer. Mixing was performed at 1100 rpm for 30 minutes. The NMP-containing slurry was cast on bare Al and then dried to remove the NMP. The dried conventional cathode was then calendered to control the porosity to less than 30%. A semi-solid cathode was prepared by mixing 55 vol% NMC811 powder and 2 vol% carbon black with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The cathode slurry was prepared using a centrifugal mixer. Mixing was performed at 1400 rpm for 2 minutes. The semi-solid slurry has a mixing indentation of more than 0.9 kPa and a pressure of 1.5 × 10 ー4 The slurry was fabricated into a 250 μm thick electrode and tested against a Li metal anode in a pouch cell configuration.

[0088] Example 3 (SiO / Hard Carbon Semi-Solid Anode and NMC Semi-Solid Cathode) Electrochemical cell example 3 (also referred to as "Ex3") was prepared using a semi-solid / conventional anode and a Li metal anode. A first layer of conventional coating hard carbon slurry was made by mixing 80 wt% hard carbon, 10 wt% carbon black, and 10 wt% PVDF, then diluting with NMP in a centrifugal mixer. Mixing was performed at 1100 rpm for 30 minutes. The NMP-containing slurry was cast onto nickel foam and then dried to remove the NMP. The dried conventional cathode was then calendered to control the porosity to less than 20%. A semi-solid anode was prepared by mixing 40 vol% silicon monoxide powder and 10 vol% carbon black with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The anode slurry was prepared using a centrifugal mixer. Mixing was performed at 1100 rpm for 30 seconds. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a porosity of 1.5×10 ー4 The slurry was fabricated into a 250 μm thick electrode and tested against a Li metal anode in a pouch cell configuration.

[0089] Example 4 (SiO / Hard Carbon Semi-Solid Anode and Semi-Solid Cathode) Electrochemical cell example 4 (also referred to as "Ex3") was prepared using a semi-solid / conventional anode and a semi-solid nmc cathode. The first layer of conventional coating SiO slurry was made by mixing 80 wt% SiO nanowires, 10 wt% carbon black, and 20 wt% PVDF and diluting with NMP in a centrifugal mixer. Mixing was performed at 1100 rpm for 30 minutes. The NMP-containing slurry was cast on copper and then dried to remove the NMP. The dried conventional cathode was then calendered to control the porosity to less than 30%. The semi-solid anode was prepared by mixing 50 vol% graphite powder and 2 vol% carbon black with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The anode slurry was prepared using a centrifugal mixer. Mixing was performed at 1100 rpm for 30 seconds. The semi-solid slurry has a mixing indentation of more than 0.9 kPa and a pressure of 1.5 × 10 ー4 The slurry was fabricated into a 250 μm thick electrode and tested against a Li metal anode in a pouch cell configuration. The semi-solid cathode was prepared by mixing 50 vol.% NMC622 and 2 vol.% activated carbon with an ethylene carbonate / dimethyl carbonate / LiPF6 based electrolyte. The cathode slurry was prepared using a centrifugal mixer. Mixing was performed at 1400 rpm for 2 minutes. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a conductivity of 1.5×10 ー4 The cathode slurry was made into a 200 μm thick electrode. The cell was tested using a Maccor battery tester and cycled over a voltage range of V=4.2V to 2.2V. The cell was charged using a constant current constant voltage at a constant current rate of C / 10. The cell was discharged at C / 10. The formation curve for this semi-solid cell is shown in FIG. 7.

[0090] Example 5 (normal semi-solid cell) Electrochemical Cell Example 5 (also referred to as "Ex5") was prepared using a semi-solid cathode and a semi-solid graphite anode. The semi-solid cathode was prepared by mixing 50% by volume of NMC811 and 2% by volume of activated carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The cathode slurry was prepared using a centrifugal mixer. Mixing was performed at 1400 rpm for 2 minutes. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a 1.5×10 ー4 The cathode slurry was made into a 200 μm thick electrode. The cathode was then densified to achieve a solids loading of over 66 vol.%. The anode graphite semi-solid slurry was prepared by mixing 60 vol.% graphite powder and 2 vol.% conductive carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The slurry was mixed at 1100 rpm for 2 minutes using a centrifugal mixer. The anode slurry was made into a 250 μm thick electrode.

[0091] Example 6 (Semi-solid cathode and semi-solid / Si) Electrochemical cell example 6 (also referred to as "Ex6") was prepared using a semi-solid cathode and two layers of semi-solid graphite / sputtered Si anode. The semi-solid cathode was prepared by mixing 50% by volume of NMC811 and 2% by volume of activated carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The cathode slurry was prepared using a centrifugal mixer. Mixing was performed at 1400 rpm for 2 minutes. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a 1.5×10 ー4The cathode slurry was made into a 200 μm thick electrode. The cathode was then densified to achieve a solid loading of over 66% by volume. A sputtering machine was used to sputter a first layer of Si onto the copper with a controlled thickness of 2 μm. The anode's second layer of graphite in a semi-solid slurry was prepared by mixing 60% by volume of graphite powder and 2% by volume of conductive carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. A centrifugal mixer was used to mix the slurry at 1100 rpm for 2 minutes. The anode slurry was cast into a 250 μm thick sputtered Si electrode.

[0092] Example 7 (Semi-solid Si-graphite / sputtered Si) Electrochemical cell example 7 (also referred to as "Ex7") was prepared using a semi-solid cathode and two layers of semi-solid Si-graphite / sputtered Si anode. The semi-solid cathode was prepared by mixing 50% by volume of NMC811 and 2% by volume of activated carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The cathode slurry was prepared using a centrifugal mixer. Mixing was performed at 1400 rpm for 2 minutes. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a solubility of 1.5×10 ー4 The cathode slurry was made into a 200 μm thick electrode. The cathode was then densified to achieve a solid loading of over 66 vol.%. A sputtering machine was used to sputter a first layer of Si onto the copper with a controlled thickness of 2 μm. The anode second layer of graphite in a semi-solid slurry was prepared by mixing 40 vol.% graphite powder, 20 vol.% agglomerated Si, and 2 vol.% conductive carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. A centrifugal mixer was used to mix the slurry at 1100 rpm for 2 min. The anode slurry was cast into a 200 μm thick sputtered Si electrode.

[0093] In Table 1, the Ex5 cell is compared with the Ex6 and Ex7 cells. Table 1 shows the beginning of life (BOL) energy density and specific energy of cells with semi-solid graphite anode, two-layer semi-solid graphite / sputtered Si anode, and two-layer semi-solid Si-graphite / sputtered Si anode. Adding high-capacity material to the electrode significantly improves the capacity. A 6% improvement is achieved by using two-layer semi-solid graphite / sputtered Si anode, while a 21% improvement is achieved by using two-layer semi-solid Si-graphite / sputtered Si anode. [Table 1]

[0094] Example 8 (Semi-solid conventional cast silicon anode and semi-solid cathode) Electrochemical cell example 8 (also referred to as "Ex8") was prepared using a semi-solid cathode and two layers of semi-solid graphite / conventional Si anode. The semi-solid cathode was prepared by mixing 50% by volume of NMC811 and 2% by volume of activated carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The cathode slurry was prepared using a centrifugal mixer. Mixing was performed at 1400 rpm for 2 minutes. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a 1.5×10 ー4The cathode slurry was made into a 200 μm thick electrode. The first layer of conventional coating Si nanoparticle slurry was made by mixing 70 wt% Si, 5 wt% carbon black, and 15 wt% polyimide binder, then diluting with NMP in a centrifugal mixer. Mixing was done at 1100 rpm for 30 minutes. The NMP-containing slurry was cast onto copper and then dried to remove the NMP. The dried conventional cathode was then calendered to control the porosity to less than 30%. The thickness of the first layer was 40 μm. Anode second layer graphite semi-solid slurry was prepared by mixing 53 vol% graphite powder and 2 vol% conductive carbon with ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The slurry was mixed at 1100 rpm for 2 minutes using a centrifugal mixer. The anode slurry was cast into a 250 μm thick Si electrode.

[0095] Example 9 (Semi-solid graphite sputtered silicon anode and semi-solid cathode) Electrochemical cell Example 9 (also referred to as "Ex9") was prepared using a semi-solid cathode and two layers of semi-solid graphite / sputtered Si anode. The semi-solid cathode was prepared by mixing 50% by volume of NMC811 and 2% by volume of activated carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The cathode slurry was prepared using a centrifugal mixer. Mixing was performed at 1400 rpm for 2 minutes. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a 1.5×10 ー4The cathode slurry was made into a 200 μm thick electrode. A sputtering machine was used to sputter a first layer of Si onto the copper with a controlled thickness of 2 μm. Anode second layer graphite semi-solid slurry was prepared by mixing 53 vol.% graphite powder and 2 vol.% conductive carbon with an ethylene carbonate / dimethyl carbonate / LiPF6 based electrolyte. A centrifugal mixer was used to mix the slurry at 1100 rpm for 2 minutes. The anode slurry was cast into a 250 μm thick Si electrode.

[0096] Figure 8 shows a plot of the capacity vs. voltage for the first charge and discharge of the Ex8 cell. Figure 9 shows a plot of the capacity vs. voltage for the first charge and discharge of the Ex9 cell. Both cells were discharged from 4.3 V to 2.7 V. The charge rate was C / 20 and the discharge rate was C / 10.

[0097] FIG. 10 shows the capacity retention plot of the Ex8 cell at voltage discharge from 4.2V to 3.0V. Under these conditions, after 100 cycles, the cell retains about 90% of its capacity. FIG. 11 shows the capacity retention of the Ex8 cell at voltage discharge from 4.3V to 2.7V. At this greater depth of discharge, the cell retains only about 60% of its capacity after 100 cycles. FIG. 12 shows the capacity retention plot of the Ex9 cell at voltage discharge from 4.3V to 2.7V. After 100 cycles, the Ex9 cell retained about 95% of its capacity. The cells in FIG. 10 and FIG. 11 were operated at similar depth of discharge, and the Ex9 cell with sputtered silicon retained significantly more of its capacity. The cells in FIG. 10, FIG. 11, and FIG. 12 were operated at charge and discharge rates of C / 4 and C / 3, respectively.

[0098] Figure 13 shows the cell voltage versus specific capacity for the first cycle after formation and the last cycle of cycling testing of a battery constructed according to Ex9. This is similar information to that presented in Figure 12 regarding capacity retention for cells constructed according to Ex9. This plot shows minimal capacity loss associated with this battery design as the charge / discharge curves follow similar trajectories at the beginning and end of life.

[0099] Example 10 (Tin / Graphite Dual Anode vs. 811 Cathode) Electrochemical Cell Example 10 (also referred to as "Ex10") was prepared using a semi-solid cathode and a two-layer semi-solid graphite / tin metal anode. The semi-solid cathode was prepared by mixing 50% by volume of NMC811 and 2% by volume of activated carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The cathode slurry was prepared using a centrifugal mixer. Mixing was performed at 1400 rpm for 2 minutes. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a 1.5×10 ー4 The cathode slurry was made into a 200 μm thick electrode. The first layer of tin was electrochemically deposited on copper with a controlled thickness of 10 μm. Anode second layer graphite semi-solid slurry was prepared by mixing 53 vol.% graphite powder and 2 vol.% conductive carbon with an ethylene carbonate / dimethyl carbonate / LiPF6 based electrolyte. The slurry was mixed at 1100 rpm for 2 min using a centrifugal mixer. The anode slurry was cast into a 250 μm thick Sn electrode. Figure 14 shows the voltage vs. capacity plots for the first cycle of the Ex10 cell for voltages from 4.2 to 2.6 V. The characterized Li-Sn alloying voltage of 0.4 V can be assigned to the obvious plateau at 3.4 V in the charging curves of Figure 16, indicating two different anode chemistries.

[0100] Example 11 (Sn / Si / graphite anode) Electrochemical Cell Example 11 (also referred to as "Ex11") was prepared using a semi-solid cathode and a three-layer semi-solid Sn / Si / graphite anode. The semi-solid cathode was prepared by mixing 50% by volume of NMC811 and 2% by volume of activated carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The cathode slurry was prepared using a centrifugal mixer. Mixing was performed at 1400 rpm for 2 minutes. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a 1.5×10 ー4 The cathode slurry was made into a 200 μm thick electrode. The first layer Si was sputtered onto the copper with a controlled thickness of 2 μm using a sputtering machine. The second layer Sn was electrochemically deposited onto the sputtered Si with a controlled thickness of 10 μm. The anode top layer graphite semi-solid slurry was prepared by mixing 53 vol% Si-graphite mixed powder and 2 vol% conductive carbon with an ethylene carbonate / dimethyl carbonate / LiPF6 based electrolyte. The slurry was mixed at 1100 rpm for 2 minutes using a centrifugal mixer. The anode slurry was cast into a 250 μm thick Sn / Si electrode.

[0101] Example 12 (two-layer cathode and semi-solid anode) Electrochemical cell Example 12 (also referred to as "Ex12") was prepared using a bilayer cathode and a graphite semi-solid anode. The bilayer cathode consisted of a first layer of sputtered LiCoO2 and a semi-solid layer of LiMnNiCoO2. The thickness of the first layer was 500 nm. The thickness of the second layer was 200 μm. The semi-solid layer of the LiMnNiCoO2 cathode was prepared by mixing 50 vol.% NMC811 and 2 vol.% activated carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The slurry of the semi-solid layer was prepared using a centrifugal mixer. Mixing was performed at 1200 rpm for 2 minutes. The semi-solid slurry had a mixing indentation of more than 0.9 kPa and a solubility of 1.5×10 ー3The anode second layer graphite semi-solid slurry was prepared by mixing 53 vol% graphite powder and 2 vol% conductive carbon with ethylene carbonate / dimethyl carbonate / LiPF6 based electrolyte. The slurry was mixed at 900 rpm for 30 minutes using a centrifugal mixer. The anode slurry was cast onto a copper current collector with a thickness of 250 μm. Figure 15 shows the voltage vs. capacity plots for the first cycle of the Ex12 cell for voltages from 4.3 to 2.5 V.

[0102] Example 13 (Trilayer cathode with dual electrolyte) Electrochemical cell Example 13 (also referred to as "Ex13") was prepared using a tri-layer cathode with LiPON coating and a graphite semi-solid anode. The tri-layer cathode consisted of a first layer of sputtered LiCoO2, a middle semi-solid layer of LiMnNiCoO2, and sputtered LiPON to fill the surface of the cathode. The thickness of the first layer was 500 nm. The thickness of the second layer was 200 μm, and the thickness of the top layer was 20 nm. The semi-solid layer of the LiMnNiCoO2 cathode was prepared by mixing 50% by volume of NMC811 and 2% by volume of activated carbon with an ethylene carbonate / acetonitrile / LiPF6-based electrolyte. The slurry of the semi-solid layer was prepared using a centrifugal mixer. Mixing was performed at 1200 rpm for 2 minutes. Anode second layer graphite semi-solid slurry was prepared by mixing 53 vol.% graphite powder and 2 vol.% conductive carbon with ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The slurry was mixed at 900 rpm for 30 minutes using a centrifugal mixer. The anode slurry was cast onto a 250 μm thick copper current collector. The cell was assembled in a pouch cell format to allow separation of the catholyte and anolyte.

[0103] Example 14 (double-sided electrode) Electrochemical cell example 14 (also referred to as "Ex14") was prepared using a bilayer LiCoO2 / LiMnNiCoO2 cathode coating and a bilayer graphite / Si semi-solid anode. The bilayer cathode consisted of a first layer of sputtered LiCoO2 and a semi-solid layer of LiMnNiCoO2. The thickness of the first layer was 500 nm. The thickness of the second layer was 200 μm. The semi-solid layer of LiMnNiCoO2 cathode was prepared by mixing 50 vol.% NMC811 and 2 vol.% activated carbon with an ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. On the anode side, a top layer of Si was sputtered onto the copper with a controlled thickness of 2 μm using a sputtering machine. Anode second layer graphite semi-solid slurry was prepared by mixing 53 vol.% graphite powder and 2 vol.% conductive carbon with ethylene carbonate / dimethyl carbonate / LiPF6-based electrolyte. The slurry was mixed at 1100 rpm for 2 min using a centrifugal mixer. The anode slurry was cast onto a 220 μm thick Si electrode.

Claims

1. A current collector; a first electrode material disposed on the current collector and having a first surface area; a second electrode material disposed on the first electrode material, the second electrode material having a second surface area greater than the first surface area; The second electrode material comprises a mixture of an active material and a conductive material in a liquid electrolyte.

2. The electrode of claim 1 , wherein the first electrode material comprises a solid high capacity electrode layer.

3. 3. The electrode of claim 2, wherein the solid high capacity electrode layer comprises at least one of tin, silicon, antimony, aluminum, and titanium oxide.

4. The electrode of claim 1 , wherein the first electrode material and the second electrode material have a combined thickness of about 150 μm to about 2000 μm.

5. The electrode of claim 1 , wherein the first electrode material has a thickness of about 1 μm to about 80 μm.

6. The electrode of claim 1 , wherein the first electrode material has a thickness that is less than about 10% of a total thickness of the electrode.

7. The electrode of claim 1 , wherein the second electrode material has a thickness that is at least about 80% of the total thickness of the electrode.

8. 10. The electrode of claim 1, further comprising a lithium-containing material disposed between the first electrode material and the second electrode material.

9. The electrode of claim 1 , wherein the theoretical energy density varies across a thickness of the electrode.

10. The electrode of claim 1 , wherein the first electrode material comprises at least one of carbon fibers, carbon microfibers, graphene sheets, or carbon nanotubes.

11. A current collector; a first electrode layer having a solid composition, the first electrode layer including a solid high capacity electrode layer comprising at least one of carbon fibers, carbon microfibers, graphene sheets, or carbon nanotubes, the first electrode layer including a binder; a second electrode layer disposed on the first electrode material, the second electrode layer comprising a semi-solid electrode material including a mixture of an active material and a conductive material in a liquid electrolyte.

12. 12. The electrode of claim 11, wherein the anode is configured to allow for intercalation or alloying of lithium ions into each of the first and second electrode layers.

13. 12. The electrode of claim 11 , wherein the first electrode layer and the second electrode layer have a combined specific capacity of at least 200 mAh / g.

14. The electrode of claim 11 , wherein the first electrode layer and the second electrode layer have a combined thickness of about 150 μm to about 2000 μm.

15. The electrode of claim 11 , wherein the first electrode layer has a thickness of about 3% to about 50% of a total thickness of the electrode.

16. The electrode of claim 11 , wherein the second electrode layer has a thickness of about 50% to about 99% of a total thickness of the electrode.

17. 12. The electrode of claim 11, wherein during operation, ions are shuttled through the second electrode layer at a first velocity and through the first electrode layer at a second velocity, the second velocity being less than the first velocity.

18. The electrode of claim 11 , wherein the first electrode layer comprises at least one of carbon fibers, carbon microfibers, graphene sheets, or carbon nanotubes.

19. A current collector; a first electrode layer disposed on the current collector, the first electrode layer comprising a solid electrode material having a first density and including a binder; a second electrode layer disposed on the first electrode layer, the second electrode layer comprising a semi-solid electrode material including a mixture of an active material and a conductive material in a liquid electrolyte, the second electrode layer having a second density different from the first density.

20. 20. The electrode of claim 19, wherein the first electrode layer comprises a high capacitance material, the high capacitance material comprising at least one of tin, silicon, antimony, aluminum, and titanium oxide.

21. 21. The electrode of claim 20, wherein the first electrode layer comprises about 10% to about 20% by volume of a high capacity material.

22. 20. The electrode of claim 19, wherein the first electrode layer and the second electrode layer are incorporated into a lithium ion battery that operates via at least one of intercalation or alloying of lithium ions into each of the first electrode layer and the second electrode layer.

23. 20. The electrode of claim 19, wherein the first electrode layer and the second electrode layer have a combined specific capacity of at least 200 mAh / g.

24. 20. The electrode of claim 19, wherein the first electrode layer and the second electrode layer have a combined thickness of about 150 μm to about 2000 μm.

25. 20. The electrode of claim 19, wherein the first electrode layer comprises at least one of carbon fibers, carbon microfibers, graphene sheets, or carbon nanotubes.