Nonaqueous electrolyte, and nonaqueous electrolyte battery using the nonaqueous electrolyte

A non-aqueous electrolyte containing a thiophene compound with a cyano group and specific anion-containing compounds forms a protective film on the positive electrode, addressing capacity deterioration and resistance issues in high-temperature cycles, thereby improving battery performance.

JP2024132532AActive Publication Date: 2024-10-01MU IONIC SOLUTIONS CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023043335
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

Existing non-aqueous electrolyte batteries face issues with capacity deterioration and resistance increase during high-temperature cycle charging and discharging, as highlighted in Patent Documents 1, 2, and 3.

Method used

Incorporation of a thiophene compound with a cyano group represented by a specific formula and at least two types of anion-containing compounds, including those with S=O bonds, P-F bonds, and P=O bonds, into the non-aqueous electrolyte to form a protective film on the positive electrode, minimizing side reactions and resistance.

Benefits of technology

The solution effectively improves capacity retention and suppresses resistance increase during high-temperature cycles, enhancing the performance of non-aqueous electrolyte batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132532000001
    Figure 2024132532000001
  • Figure 2024132532000002
    Figure 2024132532000002
  • Figure 2024132532000003
    Figure 2024132532000003
Patent Text Reader

Abstract

To provide a nonaqueous electrolyte capable of achieving both an improvement in capacity retention rate and a suppression in resistance increase after high-temperature cycle charging and discharging.SOLUTION: There is provided a nonaqueous electrolyte which contains a compound represented by formula (I) and at least two anion-containing compounds, and which contains, as at least one of the anion-containing compounds, a compound selected from the group consisting of an anion-containing compound having a S=O bond, a phosphate anion-containing compound having a P-F bond and a P=O bond, and an oxalate complex anion-containing compound. (In the formula (I), R1, R2 each independently represent hydrogen, a cyano group, a halogen atom, or an organic group with a carbon number of 1 or more and 10 or less, the organic group may be substituted by at least one of a cyano group and a halogen atom, and at least one of R1 and R2 includes a cyano group.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nonaqueous electrolyte and a nonaqueous electrolyte battery containing the nonaqueous electrolyte. [Background technology]

[0002] Non-aqueous electrolyte batteries such as lithium secondary batteries are being put to practical use in a wide range of applications, from so-called consumer power sources for mobile phones, notebook computers, etc., to on-board power sources for driving automobiles, etc. However, in recent years, there has been an increasing demand for higher performance for non-aqueous electrolyte batteries, and in particular, there has been a demand for improvements in various battery characteristics such as high capacity, low-temperature usage characteristics, high-temperature storage characteristics, cycle characteristics, and safety during overcharge. To date, numerous technologies have been investigated for various battery components, including positive and negative electrode active materials and nonaqueous electrolytes, as means for improving the high-temperature storage characteristics and cycle charge / discharge characteristics of nonaqueous electrolyte secondary batteries. Patent Document 1 describes that in a nonaqueous electrolyte lithium secondary battery having a positive electrode containing a lithium-containing composite oxide as a positive electrode active material, a nonaqueous electrolyte lithium secondary battery having excellent storage characteristics can be obtained by using an electrolyte containing a compound that forms a conductive polymer by polymerization reaction. Patent Document 2 describes that the cycle characteristics and swelling characteristics of a secondary battery are improved by including in the electrolyte solution at least one of a first heterocyclic compound and a second heterocyclic compound. Patent Document 3 describes that adding a specific thiophene compound and a specific nitrile compound to the electrolyte of a lithium ion battery is effective in improving stability and lifespan and suppressing swelling. However, Patent Documents 1 and 2 have the problem of large capacity degradation and large resistance increase after high-temperature charge-discharge cycles, and Patent Document 3 has the problem of large resistance increase during charge-discharge cycles. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-90970 A [Patent Document 2] JP 2018-41588 A [Patent Document 3] U.S. Patent Publication No. 2014 / 0342242 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a non-aqueous electrolyte solution which can solve the above problems and simultaneously improve the capacity retention rate and suppress the increase in resistance after high-temperature cycle charge / discharge. [Means for solving the problem]

[0005] In view of the above-mentioned circumstances, the present inventors conducted intensive research and found that the above-mentioned problems can be solved by using a thiophene compound represented by a specific formula (I) having a cyano group and at least two kinds of anion-containing compounds including a specific anion-containing compound, thereby completing the present invention.

[0006] That is, the gist of the present invention lies in the following. [1] A composition comprising a compound represented by formula (I) and at least two anion-containing compounds, The nonaqueous electrolyte solution contains, as at least one of the anion-containing compounds, a compound selected from the group consisting of an anion-containing compound having an S=O bond, a phosphate anion-containing compound having a PF bond and a P=O bond, and an oxalate complex anion-containing compound. [ka] (In the above formula (I), R 1 , R 2 each independently represents a hydrogen atom, a cyano group, a halogen atom, or an organic group having from 1 to 10 carbon atoms, The organic group may be substituted with at least one of a cyano group and a halogen atom, and R 1 and R2 At least one of them contains a cyano group. [2] The nonaqueous electrolyte solution according to [1], wherein the compound represented by formula (I) contains one cyano group. [3] R 1 The nonaqueous electrolyte solution according to [1] or [2], wherein the number of cyano groups therein is 1. [4] R 2 is a hydrogen atom or a saturated hydrocarbon group having 1 to 3 carbon atoms. [5] R 2 is a hydrogen atom. [6] The nonaqueous electrolyte solution according to any one of [1] to [4], wherein the content of the compound represented by formula (I) is 0.001 to 5 mass %. [7] One of the anion-containing compounds is PF6 - The nonaqueous electrolyte solution according to any one of [1] to [6], wherein the nonaqueous electrolyte solution is an anion-containing compound. [8] The nonaqueous electrolyte solution according to any one of [1] to [7], wherein the total content of the anion-containing compound having an S=O bond, the phosphate anion-containing compound having a PF bond and a P=O bond, and the oxalate complex anion-containing compound is 0.001 to 5 mass%. [9] The nonaqueous electrolyte solution according to any one of [1] to [8], wherein the mass ratio (A / B) of the content (A) of the compound represented by formula (I) to the total content (B) of the anion-containing compound having an S=O bond, and the phosphate anion-containing compound having a PF bond and a P=O bond is 0.01 / 99.99 or more and 99.99 / 0.01 or less.

[10] The nonaqueous electrolyte solution according to any one of [1] to [9], further comprising a cyclic carbonate having a carbon-carbon unsaturated bond.

[11] A nonaqueous electrolyte battery comprising a positive electrode, a negative electrode, and the nonaqueous electrolyte according to any one of [1] to

[10] .

[12] The nonaqueous electrolyte battery according to

[11] , wherein the positive electrode contains a lithium transition metal compound represented by the following composition formula (2): Li 1+x MO2···(2) (In the composition formula (2), x is −0.1≦x≦0.5, and M includes at least one element including a transition metal.)

[13] The nonaqueous electrolyte battery according to

[11] , wherein the positive electrode contains a lithium transition metal compound represented by the following composition formula (3): Li a1 Ni b1 M c1 O2···(3) (In the composition formula (3), a1, b1, and c1 satisfy 0.90≦a1≦1.10, 0.30≦b1≦0.98, and 0.01≦c1≦0.5, respectively. M includes at least one element selected from the group consisting of Co, Mn, Al, Mg, Zr, Fe, Ti, V, Cr, La, Ce, Mo, Sc, Y, and Sr.) Effect of the Invention

[0007] According to the present invention, it is possible to provide a nonaqueous electrolyte solution that can simultaneously improve the capacity retention rate and suppress the increase in resistance after high-temperature cycle charge / discharge, and also to provide a nonaqueous electrolyte battery including the nonaqueous electrolyte solution.

[0008] The present inventor speculates as follows as to the reason why the non-aqueous electrolyte having the configuration of the present invention has such excellent effects. The non-aqueous electrolyte of the present invention has at least two kinds of anion-containing compounds including a specific anion-containing compound, and a specific thiophene compound having a cyano group. It is speculated that the thiophene compound acts on the positive electrode by having a cyano group at a position relatively far from the CS bond in the general formula (1), and the formation of a polymerized protective film on the positive electrode surface is initiated from the C of the CS bond in the general formula (1). It is also speculated that the positive electrode protective film sufficiently suppresses the decrease in resistance and the side reaction on the electrode by incorporating at least two kinds of anions including a specific anion-containing compound into the positive electrode protective film. As a result, it is speculated that the capacity retention rate can be improved while suppressing the increase in resistance after high-temperature charge-discharge cycles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following describes in detail the embodiment of the present invention. However, the following description is an example (representative example) of the embodiment of the present invention, and the present invention is not limited to these contents. Furthermore, the present invention can be modified and implemented as desired without departing from the gist of the present invention.

[0010] [1. Non-aqueous electrolyte] [1-1. Compound represented by formula (I)] The nonaqueous electrolyte solution according to the embodiment of the present invention contains a compound represented by the following formula (I) in addition to at least two kinds of anion-containing compounds including a specific anion-containing compound. [ka] (In the above formula (I), R 1 , R 2 each independently represents a hydrogen atom, a cyano group, a halogen atom, or an organic group having from 1 to 10 carbon atoms, The organic group may be substituted with at least one of a cyano group and a halogen atom, and R 1 and R 2 At least one of them contains a cyano group.

[0011] R 1 , R 2 is a hydrogen atom, a cyano group, a halogen atom, or an organic group having 1 to 10 carbon atoms, and R 1 and R 2 It is presumed that the C--S bond in general formula (I) effectively contributes to the effects of the invention by containing a cyano group on at least one side. The organic group may, for example, be an alkyl group, an alkenyl group, an alkynyl group, an aryl group, or an alkoxy group. In addition, the hydrogen atoms of the organic group may be substituted with halogen atoms, a portion of the carbon atoms forming the skeleton of the organic group may be substituted with oxygen atoms (specifically, the skeleton may have an ether bond or an ester bond), and a portion of the carbon atoms forming the skeleton of the organic group may be substituted with nitrogen atoms. Examples of the halogen atom include a chlorine atom and a fluorine atom, and a fluorine atom is preferable.

[0012] Specific examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups. Among them, preferred are methyl, ethyl, n-propyl, n-butyl, tert-butyl, n-pentyl, and hexyl groups, more preferred are methyl, ethyl, n-propyl, n-butyl, tert-butyl, and n-pentyl groups, and particularly preferred are methyl, ethyl, n-butyl, and tert-butyl groups. The above-mentioned alkyl groups are preferred because the compound represented by formula (I) tends to be localized near the surface of the positive electrode active material.

[0013] Specific examples of the alkenyl group include vinyl, allyl, methallyl, 2-butenyl, 3-methyl-2-butenyl, 3-butenyl, and 4-pentenyl groups. Among them, vinyl, allyl, methallyl, and 2-butenyl groups are preferred, vinyl, allyl, and methallyl groups are more preferred, and vinyl or allyl groups are particularly preferred. The above-mentioned alkenyl groups are preferred because the compound represented by formula (I) tends to be localized near the surface of the positive electrode active material.

[0014] Specific examples of the alkynyl group include ethynyl, 2-propynyl, 2-butynyl, 3-butynyl, 4-pentynyl, and 5-hexynyl groups. Among these, ethynyl, 2-propynyl, 2-butynyl, and 3-butynyl groups are preferred, 2-propynyl and 3-butynyl groups are more preferred, and 2-propynyl groups are particularly preferred. The above-mentioned alkynyl groups are preferred because the compound represented by formula (I) tends to be localized near the surface of the positive electrode active material.

[0015] Above R 1 It is preferable that the compound has a cyano group. Above R 1is an organic group having 1 to 10 carbon atoms, the hydrogen atoms of the organic group may be substituted with halogen atoms, but it is preferable that the organic group does not contain halogen atoms. In addition, a part of the carbon atoms forming the skeleton of the organic group may be substituted with oxygen atoms, for example, it may have an ether bond or an ester bond, but it is preferable that the organic group does not contain oxygen atoms. In addition, a part of the carbon atoms forming the skeleton of the organic group may be substituted with nitrogen atoms, but it is preferable that the organic group does not contain nitrogen atoms. Above R 1 may have a carbon-carbon unsaturated bond, but preferably does not have a carbon-carbon unsaturated bond. For example, 1 When is a hydrocarbon group, it is preferably a saturated hydrocarbon group. Above R 1 Preferably, it has 1 to 5 carbon atoms, more preferably 1 to 3 carbon atoms, and most preferably 1 carbon atom. In addition, the above R 1 The number of cyano groups therein is preferably 3 or less, more preferably 2 or less, and even more preferably 1. Above R 1 Specifically, -R 11 A group represented by —CN (wherein R 11 is preferably a single bond or a divalent organic group having 1 to 9 carbon atoms, and -R 12 A group represented by —CN (wherein R 12 is preferably a single bond or a divalent hydrocarbon group having 1 to 9 carbon atoms, and 13 A group represented by —CN (wherein R 13 is more preferably a single bond, an alkylene group having 1 to 9 carbon atoms, a group in which one hydrogen atom has been removed from an alkenyl group having 2 to 9 carbon atoms, or a group in which one hydrogen atom has been removed from an alkynyl group having 2 to 9 carbon atoms), and -R 14 A group represented by —CN (wherein R 14 is particularly preferably a single bond or an alkylene group having 1 to 9 carbon atoms, and most preferably a cyano group (-CN). 11 , R 12 , R 13The number of carbon atoms in R14 is preferably 1 to 9, more preferably 8 or less, even more preferably 6 or less, still more preferably 4 or less, and particularly preferably 3 or less.

[0016] Above R 2 is an organic group having 1 to 10 carbon atoms, the hydrogen atoms of the organic group may be substituted with halogen atoms, but it is preferable that the organic group does not contain halogen atoms. In addition, a part of the carbon atoms forming the skeleton of the organic group may be substituted with oxygen atoms, for example, it may have an ether bond or an ester bond, but it is preferable that the organic group does not contain oxygen atoms. In addition, a part of the carbon atoms forming the skeleton of the organic group may be substituted with nitrogen atoms, but it is preferable that the organic group does not contain nitrogen atoms. Above R 2 may have a carbon-carbon unsaturated bond, but preferably does not have a carbon-carbon unsaturated bond. For example, 2 When is a hydrocarbon group, it is preferably a saturated hydrocarbon group. Above R 2 The number of carbon atoms in the group is preferably 0 to 5, more preferably 0 to 3, and is preferably 0. R 2 may or may not have a cyano group. 2 When R has a cyano group, 2 As for -R 11 A group represented by -CN is preferred, and -R 12 A group represented by -CN is more preferred, and -R 13 A group represented by -CN is more preferred, and -R 14 A group represented by --CN is particularly preferred, with a cyano group (--CN) being most preferred. Above R 2 The number of cyano groups therein is preferably 3 or less, more preferably 2 or less, and further preferably 0 or 1. Above R 2is preferably a hydrogen atom, a halogen atom, or a saturated hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a halogen atom, and more preferably a hydrogen atom, or a saturated hydrocarbon group having 1 to 10 carbon atoms which does not contain a halogen atom. Above R 2 is more preferably a hydrogen atom or an organic group having 1 to 5 carbon atoms, particularly preferably a hydrogen atom or a saturated hydrocarbon group having 1 to 3 carbon atoms, and most preferably a hydrogen atom.

[0017] The molecular weight of the compound represented by the above formula (I) is not particularly limited, but is usually 50 or more and usually 2000 or less, preferably 1000 or less, more preferably 500 or less, particularly preferably 300 or less, and most preferably 200 or less. By being in the above range, the compound is easy to handle, and the viscosity of the electrolyte solution when it is contained can be made appropriate.

[0018] The compound represented by the above formula (I) is R 1 and R 2 At least one of the above formula (I) contains a cyano group. The number of cyano groups in the compound represented by formula (I) is not particularly limited as long as it is 1 or more, but is preferably 1 to 6, more preferably 1 to 4, even more preferably 1 to 3, particularly preferably 1 to 2, and most preferably 1. In other words, it is most preferable that the compound represented by formula (I) contains only one cyano group.

[0019] Examples of the compound represented by the above formula (I) include the following compounds. [ka]

[0020] Among the above compounds, the compounds represented by 1 to 8, 23, 16 to 23, and 38 to 42 are preferred, the compounds represented by 1 to 8, 23, and 16 to 23 are more preferred, the compounds represented by 1 and 16 to 23 are further preferred, and the compounds represented by 1 and 16 to 18 are particularly preferred. The compound represented by the above formula (I) may be used alone or in combination of two or more kinds.

[0021] The content of the compound represented by the above formula (I) in the nonaqueous electrolyte solution (the total amount when two or more types are used in combination) is not particularly limited, but is usually 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and particularly preferably 0.2 mass% or more, and is usually 8 mass% or less, preferably 5 mass% or less, more preferably 4 mass% or less, even more preferably 2 mass% or less, and most preferably 1 mass% or less. The content of the compound represented by the above formula (I) is measured by using magnetic resonance spectroscopy or the like.

[0022] [1-2. Anion-containing compounds] The nonaqueous electrolyte solution of the present embodiment contains at least two kinds of anion-containing compounds, and at least one of the anion-containing compounds is a compound selected from the group consisting of an anion-containing compound having an S=O bond, a phosphate anion-containing compound having a PF bond and a P=O bond, and an oxalate complex anion-containing compound. Anion-containing compounds include PF6 - Anion-containing compounds, BF4 - Examples of the anion-containing compound include an anion-containing compound having an S=O bond, a phosphate anion-containing compound having a PF bond and a P=O bond, and an oxalate complex anion-containing compound. The nonaqueous electrolyte of this embodiment contains PF6 as the first anion-containing compound. - It is preferred that the composition contains an anion-containing compound. The nonaqueous electrolyte solution of the present embodiment preferably contains, as the second anion-containing compound, at least one anion-containing compound selected from the group consisting of an anion-containing compound having an S=O bond, a phosphate anion-containing compound having a PF bond and a P=O bond, and an oxalate complex anion-containing compound, more preferably contains an anion-containing compound selected from the group consisting of an anion-containing compound having an S=O bond, and a phosphate anion-containing compound having a PF bond and a P=O bond, and particularly preferably contains a phosphate anion-containing compound having a PF bond and a P=O bond. The nonaqueous electrolyte of the present embodiment preferably contains a combination of the first anion-containing compound and the second anion-containing compound, and PF6 - It is more preferable that the composition contains an anion-containing compound (first anion-containing compound) and at least one anion-containing compound (second anion-containing compound) selected from the group consisting of an anion-containing compound having an S=O bond, a phosphate anion-containing compound having a PF bond and a P=O bond, and an oxalate complex anion-containing compound.

[0023] The anion-containing compound is usually an acid or a salt, and preferably a salt, and the counter cation is preferably an alkali metal cation such as lithium, sodium, or potassium, and more preferably a lithium cation.

[0024] [1-2-1.PF6 - Anion-containing compounds Non-aqueous electrolyte is PF6 - When an anion-containing compound is contained, PF6 in the total amount of non-aqueous electrolyte - The content of the anion-containing compound is not particularly limited, but is usually 0.5% by mass or more, preferably 1% by mass or more, more preferably 4% by mass or more, even more preferably 8% by mass or more, particularly preferably 8.5% by mass or more, and most preferably 9% by mass or more, based on the total amount of the nonaqueous electrolyte solution. Also, it is usually 17% by mass or less, preferably 16% by mass or less.

[0025] [1-2-2.BF4 - Anion-containing compounds The non-aqueous electrolyte is BF4 - When an anion-containing compound is contained, the total amount of BF4 in the non-aqueous electrolyte is - The content of the anion-containing compound is not particularly limited, but is preferably 0.001 mass% or more, more preferably 0.01 mass% or more, and even more preferably 0.1 mass% or more, relative to the total amount of the nonaqueous electrolyte solution, and is usually less than 8 mass, preferably 5 mass% or less, more preferably 4 mass% or less, and even more preferably 3 mass% or less.

[0026] [1-2-3. Anion-containing compounds with S=O bonds] An example of an anion-containing compound having an S=O bond is FSO3 - Fluorosulfonate anion such as (FSO2)2N - , (FSO2)(CF3SO2)N - Fluorosulfonylimide anions such as (FSO2)3C - Compounds containing fluorosulfonylmethide anion such as CH3SO4 - Examples of the compound include compounds containing alkyl sulfate anions such as those mentioned above. Among these, from the viewpoint of the balance between the output characteristics of the battery and the protection of the electrode interface, compounds containing a fluorosulfonate anion or a fluorosulfonylimide anion are preferred, and compounds containing a fluorosulfonate anion are more preferred. When the nonaqueous electrolyte solution contains an anion-containing compound having an S=O bond, the content of the anion-containing compound having an S=O bond in the total amount of the nonaqueous electrolyte solution (the total amount when two or more types are used) is preferably 0.001 mass% or more, more preferably 0.01 mass% or more, even more preferably 0.1 mass% or more, and is usually less than 8 mass%, preferably 5 mass% or less, more preferably 4 mass% or less, even more preferably 3 mass% or less. If the content of the anion-containing compound having an S=O bond is within the above range, the capacity retention rate and the resistance increase rate after a high-temperature charge-discharge cycle test can be significantly improved. Although the reason for this is unclear, it is thought that the content of the anion-containing compound having an S=O bond within the above mass ratio range can minimize side reactions of the components of the nonaqueous electrolyte on the electrode surface. The identification and content of anion-containing compounds with S=O bonds is carried out by nuclear magnetic resonance (NMR) spectroscopy.

[0027] [1-2-4. Phosphate anion-containing compounds with PF and P=O bonds] Examples of phosphate anion-containing compounds having FP bonds and P=O bonds include PO3F2 - Monofluorophosphate anion, such as PO2F2 - and the like. Among these, compounds containing a difluorophosphate anion are preferred from the viewpoint of further improving the capacity retention rate and the resistance increase rate after high-temperature cycle charge / discharge of the battery. When the non-aqueous electrolyte solution contains a phosphate anion-containing compound having an FP bond and a P=O bond, the content of the phosphate anion-containing compound having a PF bond and a P=O bond (the total amount when two or more types are used) in the total amount of the non-aqueous electrolyte solution is preferably 0.001 mass% or more, more preferably 0.01 mass% or more, even more preferably 0.1 mass% or more, and is usually less than 8 mass%, preferably 5 mass% or less, more preferably 4 mass% or less, even more preferably 3 mass% or less. If the content of the phosphate anion-containing compound having PF bonds and P=O bonds is within the above range, the capacity retention rate and the resistance increase rate after a high-temperature charge-discharge cycle test can be significantly improved. Although the reason for this is unclear, it is thought that the side reaction of the components of the nonaqueous electrolyte on the electrode surface can be minimized when the content of the phosphate anion-containing compound having PF bonds and P=O bonds is within the above mass ratio range. The identification and content of phosphate anion-containing compounds having PF bonds and P=O bonds are determined by nuclear magnetic resonance (NMR) spectroscopy.

[0028] [1-2-5. Compounds containing oxalate complex anions] The oxalate complex anion-containing compound is not particularly limited as long as it contains an anion having an oxalate complex in the molecule.The oxalate complex anion-containing compound is a compound containing an anion of an acid that forms a complex by coordinating or bonding with oxalic acid to a central atom, and can be exemplified by a compound containing a boron oxalate complex anion in which oxalic acid is coordinated or bonded to a boron atom, and a phosphorus oxalate complex anion in which oxalic acid is coordinated or bonded to a phosphorus atom. Examples of the boron oxalate complex anion include a bis(oxalate)borate anion and a difluorooxalateborate anion. Examples of the phosphorus oxalate complex anion include a tetrafluorooxalate phosphate anion, a difluorobis(oxalate)phosphate anion and a tris(oxalate)phosphate anion. Among these, from the viewpoint of forming a stable composite coating on the surface of the electrode, a compound containing a boron oxalate complex anion is preferred, and a compound containing a bis(oxalate)borate anion is more preferred. When the non-aqueous electrolyte solution contains an oxalate complex anion-containing compound, the content of the oxalate complex anion-containing compound (the total amount when two or more types are used) in the total amount of the non-aqueous electrolyte solution is preferably 0.001 mass% or more, more preferably 0.01 mass% or more, and even more preferably 0.1 mass% or more, and is usually less than 8 mass%, preferably 5 mass% or less, more preferably 4 mass% or less, and even more preferably 3 mass% or less. If the content of the oxalate complex anion-containing compound is within the above range, the capacity retention rate and the resistance increase rate after the high-temperature charge-discharge cycle test can be significantly improved. Although the reason for this is unclear, it is believed that the content of the oxalate complex anion-containing compound within the above mass ratio range can minimize the side reaction of the components of the non-aqueous electrolyte on the electrode surface. The identification and content of the oxalate complex anion-containing compound is carried out by nuclear magnetic resonance (NMR) spectroscopy.

[0029] The total content of the anion-containing compound having an S=O bond, the phosphate anion-containing compound having a PF bond and a P=O bond, and the oxalate complex anion-containing compound in the total amount of the aqueous electrolyte is preferably 0.001 mass% or more, more preferably 0.01 mass% or more, even more preferably 0.1 mass% or more, and is usually less than 8 mass%, preferably 5 mass% or less, more preferably 4 mass% or less, even more preferably 3 mass% or less.

[0030] The mass ratio (A / B) of the content (A) of the compound represented by formula (I) to the content (B) of at least one compound selected from the group consisting of an anion-containing compound having an S=O bond, a phosphate anion-containing compound having a PF bond and a P=O bond, and an oxalate complex anion-containing compound is usually 0.01 / 99.99 or more, preferably 1 / 99 or more, more preferably 10 / 90 or more, even more preferably 20 / 80 or more, particularly preferably 30 / 70 or more, most preferably 40 / 60 or more, usually 99.99 / 0.01 or less, preferably 99 / 1 or less, more preferably 90 / 10 or less, even more preferably 80 / 20 or less, particularly preferably 70 / 30 or less, and most preferably 60 / 40 or less. If the mass ratio is within this range, the battery characteristics, particularly the capacity retention rate after high-temperature charge / discharge cycles or the resistance increase rate can be significantly improved. Although the principle behind this is unclear, it is believed that by mixing them in this ratio, a low-resistance, strong protective coating is formed on the positive electrode, making it possible to more effectively suppress side reactions on the electrode while also suppressing an increase in resistance.

[0031] (PF6 - (mass ratio of the compound represented by formula (I) to the anion-containing compound) Non-aqueous electrolyte is PF6 - When an anion-containing compound is included, PF6 in non-aqueous electrolyte -The mass ratio of the content of the compound represented by formula (I) (the total amount when there are two or more kinds) to the content of the anion-containing compound (compound represented by formula (I) [g] / PF6 - The anion-containing compound [g]) is usually 0.00005 or more, preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.02 or more, and even more preferably 0.025 or more, and is usually 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, and even more preferably 0.35 or less. When the mass ratio is within the above range, the battery characteristics, particularly the capacity retention rate after high-temperature charge-discharge cycles, can be significantly improved, and the resistance increase after high-temperature charge-discharge cycles can be significantly suppressed. Although the reason for this is unclear, it is believed that when the mass ratio is within the above range, the compound represented by formula (I) and PF6 - By including an anion-containing compound, PF6 in the battery system - This is believed to be because side reactions of the anion-containing compound are minimized.

[0032] (PF6 - (mass ratio of anion-containing compound having S=O bond to anion-containing compound) Non-aqueous electrolyte is PF6 - When an anion-containing compound or an anion-containing compound having an S=O bond is contained, PF6 in a non-aqueous electrolyte - The mass ratio of the content of anion-containing compounds having S=O bonds (total amount if there are two or more types) to the content of anion-containing compounds (anion-containing compounds having S=O bonds [g] / PF6 - The anion-containing compound [g]) is usually 0.00005 or more, preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.02 or more, and even more preferably 0.025 or more, and is usually 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, and even more preferably 0.35 or less. If the mass ratio is within the above range, the battery characteristics, particularly the capacity retention rate after high-temperature charge-discharge cycles, can be significantly improved, and the resistance increase after high-temperature charge-discharge cycles can be significantly suppressed. Although the reason for this is unclear, within the above range of mass ratio, PF6 -By containing an anion-containing compound and an anion-containing compound having an S=O bond, PF6 in the battery system - This is believed to be because side reactions of the anion-containing compound are minimized.

[0033] (PF6 - Mass ratio of phosphate anion-containing compound having PF bonds and P=O bonds to anion-containing compound Non-aqueous electrolyte is PF6 - When an anion-containing compound and a phosphate anion-containing compound having a PF bond and a P=O bond are contained, PF6 in a non-aqueous electrolyte solution - The mass ratio of the content of phosphate anion-containing compounds having PF bonds and P=O bonds (total amount if two or more types are used) to the content of anion-containing compounds (PF6 - The anion-containing compound [g]) is usually 0.00005 or more, preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.02 or more, and even more preferably 0.025 or more, and is usually 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, and even more preferably 0.35 or less. If the mass ratio is within the above range, the battery characteristics, particularly the capacity retention rate after high-temperature charge-discharge cycles, can be significantly improved, and the resistance increase after high-temperature charge-discharge cycles can be significantly suppressed. Although the reason for this is unclear, within the above range of mass ratio, PF6 - By containing an anion-containing compound and a phosphate anion-containing compound having a PF bond and a P=O bond, the PF6 - This is believed to be because side reactions of the anion-containing compound are minimized.

[0034] (PF6 - (mass ratio of oxalate complex anion-containing compound to anion-containing compound) Non-aqueous electrolyte is PF6 - When an anion-containing compound and an oxalate complex anion-containing compound are included, PF6 in non-aqueous electrolyte -The mass ratio of the content of the oxalate complex anion-containing compound (total amount if two or more kinds) to the content of the anion-containing compound (oxalate complex anion-containing compound [g] / PF6 - The anion-containing compound [g]) is usually 0.00005 or more, preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.02 or more, and even more preferably 0.025 or more, and is usually 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, and even more preferably 0.35 or less. If the mass ratio is within the above range, the battery characteristics, particularly the capacity retention rate after high-temperature charge-discharge cycles, can be significantly improved, and the resistance increase after high-temperature charge-discharge cycles can be significantly suppressed. Although the reason for this is unclear, within the above range of mass ratio, PF6 - By containing an anion-containing compound and an oxalate complex anion-containing compound, PF6 in the battery system - This is believed to be because side reactions of the anion-containing compound are minimized.

[0035] [1-3. Non-aqueous solvents] The non-aqueous electrolyte according to one embodiment of the present invention, like a general non-aqueous electrolyte, usually contains a non-aqueous solvent that dissolves the above-mentioned anion-containing compound as its main component. The non-aqueous solvent used is not particularly limited as long as it dissolves the above-mentioned anion-containing compound, and a known organic solvent can be used. Examples of the organic solvent include, but are not limited to, saturated cyclic carbonates, chain carbonates, chain carboxylates, cyclic carboxylates, ether compounds, and sulfone compounds. The organic solvent can be used alone or in combination of two or more kinds. The combination of two or more organic solvents is not particularly limited, and examples thereof include saturated cyclic carbonates and chain carbonates, saturated cyclic carbonates and chain carboxylates, cyclic carboxylates or chain carbonates, and saturated cyclic carbonates, chain carbonates and chain carboxylates. Among these, saturated cyclic carbonates and chain carbonates, and saturated cyclic carbonates, chain carbonates and chain carboxylates are preferred.

[0036] [1-3-1. Saturated cyclic carbonates] Examples of saturated cyclic carbonates include those having an alkylene group having 2 to 4 carbon atoms, and from the viewpoint of improving battery characteristics resulting from an improvement in the degree of dissociation of lithium ions, saturated cyclic carbonates having 2 to 3 carbon atoms are preferably used. Specific examples of the saturated cyclic carbonate include ethylene carbonate, propylene carbonate, butylene carbonate, etc. Among them, ethylene carbonate or propylene carbonate is preferred, and ethylene carbonate, which is less susceptible to oxidation and reduction, is more preferred. The saturated cyclic carbonate may be used alone or in any combination and ratio of two or more. The content of the saturated cyclic carbonate is not particularly limited and may be any content as long as it does not significantly impair the effects of the present invention, but is usually 3% by volume or more, preferably 5% by volume or more, and is usually 90% by volume or less, preferably 85% by volume or less, and more preferably 80% by volume or less, based on the total amount of the nonaqueous solvent in the nonaqueous electrolyte. By setting the content of the saturated cyclic carbonate within this range, it is possible to avoid a decrease in electrical conductivity due to a decrease in the dielectric constant of the nonaqueous electrolyte, and it is easy to make the large current discharge characteristics and cycle characteristics of the nonaqueous electrolyte secondary battery into a good range, and the oxidation / reduction resistance of the nonaqueous electrolyte is improved, and the stability to the negative electrode and stability during high-temperature storage tend to be improved. In the present embodiment, the volume % refers to the volume at 25° C. and 1 atmospheric pressure.

[0037] [1-3-2. Chain carbonate] As the chain carbonate, for example, one having 3 to 7 carbon atoms is used, and in order to adjust the viscosity of the electrolyte solution within an appropriate range, a chain carbonate having 3 to 5 carbon atoms is preferably used. Specific examples of the chain carbonate include dimethyl carbonate, diethyl carbonate, di-n-propyl carbonate, diisopropyl carbonate, n-propyl isopropyl carbonate, ethyl methyl carbonate, and methyl-n-propyl carbonate. Dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate are particularly preferred. In addition, chain carbonates having fluorine atoms (hereinafter, sometimes abbreviated as "fluorinated chain carbonate") can also be suitably used. The number of fluorine atoms in the fluorinated chain carbonate is not particularly limited as long as it is 1 or more, but is usually 6 or less, and preferably 4 or less. When the fluorinated chain carbonate has multiple fluorine atoms, the multiple fluorine atoms may be bonded to the same carbon or different carbons. Examples of the fluorinated chain carbonate include fluorinated dimethyl carbonate derivatives such as fluoromethyl methyl carbonate; fluorinated ethyl methyl carbonate derivatives such as 2-fluoroethyl methyl carbonate; and fluorinated diethyl carbonate derivatives such as ethyl-(2-fluoroethyl) carbonate. The chain carbonate may be used alone or as a mixture of two or more kinds in any combination and in any ratio. The content of the chain carbonate is not particularly limited, but is usually 15% by volume or more, preferably 20% by volume or more, more preferably 25% by volume or more, and usually 90% by volume or less, preferably 85% by volume or less, more preferably 80% by volume or less, based on the total amount of the nonaqueous solvent in the nonaqueous electrolyte. By setting the content of the chain carbonate within the above range, the viscosity of the nonaqueous electrolyte can be set to an appropriate range, the decrease in ion conductivity can be suppressed, and the output characteristics of the nonaqueous electrolyte secondary battery can be easily set to a good range. Furthermore, by combining a specific chain carbonate with ethylene carbonate in a specific content, the battery performance can be significantly improved. For example, when dimethyl carbonate and ethyl methyl carbonate are selected as specific chain carbonates, the content of ethylene carbonate is not particularly limited and is arbitrary as long as it does not significantly impair the effects of the present invention according to this embodiment, but it is usually 15% by volume or more, preferably 20% by volume or more, and usually 45% by volume or less, preferably 40% by volume or less, based on the total amount of non-aqueous solvent in the non-aqueous electrolyte solution, the content of dimethyl carbonate is usually 20% by volume or more, preferably 30% by volume or more, and usually 50% by volume or less, preferably 45% by volume or less, based on the total amount of non-aqueous solvent in the non-aqueous electrolyte solution, the content of ethyl methyl carbonate is usually 20% by volume or more, preferably 30% by volume or more, and usually 50% by volume or less, preferably 45% by volume or less, based on the total amount of non-aqueous solvent in the non-aqueous electrolyte solution. By setting the content within the above range, there is a tendency for excellent high-temperature stability and suppression of gas generation.

[0038] [1-3-3. Chain carboxylate esters] Examples of the chain carboxylate include methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, methyl valerate, methyl isobutyrate, ethyl isobutyrate, and methyl pivalate. Among them, methyl acetate, ethyl acetate, propyl acetate, or butyl acetate is preferred from the viewpoint of improving battery characteristics. Chain carboxylates in which a portion of the hydrogen of the above-mentioned compounds is replaced with fluorine (e.g., methyl trifluoroacetate, ethyl trifluoroacetate, etc.) can also be used suitably. The content of the chain carboxylate is usually 1% by volume or more, preferably 5% by volume or more, more preferably 15% by volume or more, based on the total amount of the nonaqueous solvent in the nonaqueous electrolyte. In this range, the electrical conductivity of the nonaqueous electrolyte is improved, and the large-current discharge characteristics of the nonaqueous electrolyte battery are easily improved. In addition, the content of the chain carboxylate is usually 70% by volume or less, preferably 50% by volume or less, more preferably 40% by volume or less. By setting the upper limit in this way, the viscosity of the nonaqueous electrolyte is in an appropriate range, the decrease in electrical conductivity is avoided, the increase in the negative electrode resistance is suppressed, and the large-current discharge characteristics of the nonaqueous electrolyte secondary battery are easily in a good range.

[0039] [1-3-4. Cyclic carboxylate esters] Examples of the cyclic carboxylate include γ-butyrolactone and γ-valerolactone. Among these, γ-butyrolactone is more preferable. Cyclic carboxylates in which some of the hydrogen atoms of the above-mentioned compounds are replaced with fluorine can also be used suitably. The content of the cyclic carboxylate is usually 1% by volume or more, preferably 5% by volume or more, more preferably 15% by volume or more, based on the total amount of the nonaqueous solvent in the nonaqueous electrolyte. In this range, the electrical conductivity of the nonaqueous electrolyte is improved, and the large-current discharge characteristics of the nonaqueous electrolyte secondary battery are easily improved. In addition, the content of the cyclic carboxylate is usually 70% by volume or less, preferably 50% by volume or less, more preferably 40% by volume or less. By setting the upper limit in this way, the viscosity of the nonaqueous electrolyte is in an appropriate range, the decrease in electrical conductivity is avoided, the increase in the negative electrode resistance is suppressed, and the large-current discharge characteristics of the nonaqueous electrolyte secondary battery are easily in a good range.

[0040] [1-3-5. Ether compounds] Preferred ether compounds include chain ethers having 3 to 10 carbon atoms, such as dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether, and diethylene glycol dimethyl ether, and cyclic ethers having 3 to 6 carbon atoms, such as tetrahydrofuran, 2-methyltetrahydrofuran, 3-methyltetrahydrofuran, 1,3-dioxane, 2-methyl-1,3-dioxane, 4-methyl-1,3-dioxane, and 1,4-dioxane. Some of the hydrogen atoms in the above-mentioned ether compounds may be substituted with fluorine. Among these, as the chain ethers having 3 to 10 carbon atoms, dimethoxymethane, diethoxymethane, and ethoxymethoxymethane are preferred because they have a high solvation ability for lithium ions, improve ionic dissociation, have low viscosity, and provide high ionic conductivity, and as the cyclic ethers having 3 to 6 carbon atoms, tetrahydrofuran, 1,3-dioxane, 1,4-dioxane, and the like are preferred because they provide high ionic conductivity. The content of the ether-based compound is not particularly limited, and may be any content as long as it does not significantly impair the effects of the present invention according to this embodiment. However, it is usually 1% by volume or more, preferably 2% by volume or more, more preferably 3% by volume or more, and usually 30% by volume or less, preferably 25% by volume or less, more preferably 20% by volume or less, based on the total amount of the nonaqueous solvent in the nonaqueous electrolyte. If the content of the ether-based compound is within the above range, it is easy to ensure the effect of improving the degree of lithium ion dissociation by the ether-based compound and improving the ion conductivity due to the decrease in viscosity of the nonaqueous electrolyte. In addition, when the negative electrode active material is a carbon-based material, the phenomenon in which the chain ether is co-inserted with the lithium ion can be suppressed, so that the input / output characteristics and the charge / discharge rate characteristics can be set to an appropriate range.

[0041] [1-3-6. Sulfone compounds] The sulfone compound is not particularly limited, and may be a cyclic sulfone or a chain sulfone. In the case of a cyclic sulfone, the carbon number is usually 3 to 6, preferably 3 to 5, and in the case of a chain sulfone, the carbon number is usually 2 to 6, preferably 2 to 5. In addition, the number of sulfonyl groups in one molecule of the sulfone compound is not particularly limited, but is usually 1 or 2. Examples of cyclic sulfones include monosulfone compounds such as trimethylene sulfones, tetramethylene sulfones, and hexamethylene sulfones, and disulfone compounds such as trimethylene disulfones, tetramethylene disulfones, and hexamethylene disulfones. Among these, from the viewpoint of dielectric constant and viscosity, tetramethylene sulfones, tetramethylene disulfones, hexamethylene sulfones, and hexamethylene disulfones are more preferred, and tetramethylene sulfones (sulfolanes) are particularly preferred. As the sulfolanes, sulfolane and sulfolane derivatives are preferred, and as the sulfolane derivatives, those in which one or more hydrogen atoms bonded to the carbon atoms constituting the sulfolane ring are substituted with a fluorine atom, an alkyl group, or a fluorine-substituted alkyl group are preferred. Among these, 2-methylsulfolane, 3-methylsulfolane, 2-fluorosulfolane, 3-fluorosulfolane, 2,3-difluorosulfolane, 2-trifluoromethylsulfolane, 3-trifluoromethylsulfolane, and the like are preferred because they have high ionic conductivity and high input / output. Examples of the chain sulfone include dimethyl sulfone, ethyl methyl sulfone, diethyl sulfone, monofluoromethyl methyl sulfone, difluoromethyl methyl sulfone, trifluoromethyl methyl sulfone, pentafluoroethyl methyl sulfone, etc. Among these, dimethyl sulfone, ethyl methyl sulfone, or monofluoromethyl methyl sulfone is preferred in terms of improving the high-temperature storage stability of the electrolyte. The content of the sulfone-based compound is not particularly limited, and may be any as long as it does not significantly impair the effect of the present invention according to this embodiment, but is usually 0.3% by volume or more, preferably 0.5% by volume or more, more preferably 1% by volume or more, and is usually 40% by volume or less, preferably 35% by volume or less, more preferably 30% by volume or less, based on the total amount of the non-aqueous solvent in the non-aqueous electrolyte. If the content of the sulfone-based compound is within the above range, an electrolyte having excellent high-temperature storage stability tends to be obtained.

[0042] [1-4. Auxiliaries] The non-aqueous electrolyte of the present invention may contain various auxiliary agents within the range that does not significantly impair the effects of the present invention. As the auxiliary agent, any conventionally known one may be used. In addition, the auxiliary agent may be used alone, or two or more kinds may be used in any combination and ratio. Examples of auxiliary agents that may be contained in the non-aqueous electrolyte solution include cyclic carbonates having carbon-carbon unsaturated bonds, fluorine-containing cyclic carbonates, compounds having an isocyanate group, organic compounds having an isocyanuric acid skeleton, sulfur-containing organic compounds, phosphorus-containing organic compounds, organic compounds having a cyano group, silicon-containing compounds, aromatic compounds, non-fluorine-containing carboxylic acid esters, cyclic compounds having an ether bond, carboxylic acid anhydrides, etc. For example, compounds described in International Publication No. 2015 / 111676 can be mentioned. Among these, at least one carbonate compound selected from cyclic carbonates having a carbon-carbon unsaturated bond and fluorine-containing cyclic carbonates (hereinafter also referred to as "specific carbonate compound") is preferable. The content of the auxiliary is not particularly limited and may be any amount as long as it does not significantly impair the effects of the present invention; however, it is usually 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and usually 10 mass% or less, preferably 5 mass% or less, more preferably 3 mass% or less, even more preferably 1 mass% or less, and particularly preferably less than 1 mass%, based on the total amount of the nonaqueous electrolyte solution. The cyclic compound having an ether bond can be used as an auxiliary agent in the non-aqueous electrolyte, and also includes those that can be used as a non-aqueous solvent as described in "1-3. Non-aqueous Solvent". When the cyclic compound having an ether bond is used as an auxiliary agent, it is used in an amount of less than 4 mass%.

[0043] [1-4-1. Specific carbonate compounds] The non-aqueous electrolyte preferably contains at least one carbonate compound selected from the group consisting of cyclic carbonates having carbon-carbon unsaturated bonds and cyclic carbonates having fluorine atoms. Among these, it is preferable to contain a cyclic carbonate having carbon-carbon unsaturated bonds, and it is more preferable to contain vinylene carbonate. These can be used alone or in combination of two or more in any ratio, and it is preferable to combine an unsaturated cyclic carbonate and a fluorinated cyclic carbonate, and it is more preferable to combine a vinylene carbonate and a fluorinated cyclic carbonate, and it is more preferable to combine an unsaturated cyclic carbonate and a monofluoroethylene carbonate, and it is even more preferable to combine vinylene carbonate and a monofluoroethylene carbonate.

[0044] (Content of specific carbonate compounds) The content of the specific carbonate compound (the total amount when two or more types are used) in the total amount of the nonaqueous electrolyte solution is usually 0.001 mass% or more, preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.5 mass% or more, and is usually 10 mass% or less, preferably 5 mass% or less, more preferably 4 mass% or less, and even more preferably 3 mass% or less. If the content of the specific carbonate compound is within the above range, the battery characteristics, particularly the durability, can be improved. Although the reason for this is unclear, it is believed that the inclusion of the carbonate compound at this ratio forms a coating on the electrode, minimizing the side reaction of the components of the non-aqueous electrolyte. The identification and content of specific carbonate compounds is determined by nuclear magnetic resonance (NMR) spectroscopy.

[0045] (Mass ratio of specific carbonate compound to compound represented by formula (I)) The mass ratio of the content of the specific carbonate compound (total amount when two or more kinds are used) to the content of the compound represented by formula (I) (specific carbonate compound [g] / compound represented by formula (I) [g]) is usually 0.01 or more, preferably 0.05 or more, more preferably 0.3 or more, and even more preferably 0.5 or more, and is usually 100 or less, preferably 10 or less, more preferably 5 or less, and even more preferably 4 or less. If the mass ratio is within the above range, the battery characteristics, especially durability, can be improved. The reason for this is unclear, but it is thought that by containing the specific carbonate compound within the above mass ratio range, a coating is formed on the electrode, and side reactions of the components of the non-aqueous electrolyte can be minimized.

[0046] (PF6 - (the mass ratio of a specific carbonate compound to an anion-containing compound) In non-aqueous electrolyte, PF6 - The mass ratio of the content of specific carbonate compounds (total amount if two or more types are present) to the content of anion-containing compounds (specific carbonate compounds [g] / PF6 - The anion-containing compound [g]) is usually 0.00005 or more, preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.02 or more, even more preferably 0.025 or more, and is usually 0.5 or less, preferably 0.45 or less, more preferably 0.4 or less, even more preferably 0.35 or less. If the mass ratio is within the above range, the battery characteristics, especially durability, can be improved. Although the reason for this is unclear, it is believed that the carbonate compound and PF6 are mixed within the above mass ratio range. - By including an anion-containing compound, a coating is formed on the electrode, and PF6 in the battery system is - This is believed to be because side reactions of the anion-containing compound are minimized.

[0047] [1-4-1-1. Cyclic carbonates having carbon-carbon unsaturated bonds] The cyclic carbonate having a carbon-carbon unsaturated bond (hereinafter also referred to as "unsaturated cyclic carbonate") is not particularly limited as long as it is a cyclic carbonate having a carbon-carbon double bond or a carbon-carbon triple bond. Cyclic carbonates having an aromatic ring are also included in the unsaturated cyclic carbonate. Examples of the unsaturated cyclic carbonate include vinylene carbonates, ethylene carbonates substituted with a substituent having an aromatic ring, a carbon-carbon double bond or a carbon-carbon triple bond, phenyl carbonates, vinyl carbonates, allyl carbonates, catechol carbonates, etc. Among these, vinylene carbonates and ethylene carbonates substituted with a substituent having an aromatic ring, a carbon-carbon double bond or a carbon-carbon triple bond are preferred. Examples of vinylene carbonates include vinylene carbonate, methylvinylene carbonate, 4,5-dimethylvinylene carbonate, phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylvinylene carbonate, 4,5-vinylvinylene carbonate, allylvinylene carbonate, and 4,5-diallylvinylene carbonate. Examples of ethylene carbonates substituted with a substituent having an aromatic ring or a carbon-carbon double bond or a carbon-carbon triple bond include vinyl ethylene carbonate, 4,5-divinyl ethylene carbonate, 4-methyl-5-vinyl ethylene carbonate, 4-allyl-5-vinyl ethylene carbonate, ethynyl ethylene carbonate, 4,5-diethynyl ethylene carbonate, 4-methyl-5-ethynyl ethylene carbonate, 4-vinyl-5-ethynyl ethylene carbonate, 4-allyl-5-ethynyl ethylene carbonate, phenyl ethylene carbonate, 4,5-diphenyl ethylene carbonate, 4-phenyl-5-vinyl ethylene carbonate, 4-allyl-5-phenyl ethylene carbonate, allyl ethylene carbonate, 4,5-diallyl ethylene carbonate, and 4-methyl-5-allyl ethylene carbonate. Among these, vinylene carbonate, vinyl ethylene carbonate, and ethynyl ethylene carbonate are preferred since they form a more stable composite coating on the electrode, and one or more selected from vinylene carbonate and vinyl ethylene carbonate are more preferred, with vinylene carbonate being even more preferred. The unsaturated cyclic carbonates can be used alone or in combination of two or more kinds in any ratio.

[0048] [1-4-1-2. Cyclic carbonates containing fluorine atoms] The fluorine atom-containing cyclic carbonate is not particularly limited as long as it has a cyclic carbonate structure and contains a fluorine atom. Examples of cyclic carbonates having fluorine atoms include fluorinated cyclic carbonates having an alkylene group with 2 to 6 carbon atoms, and derivatives thereof, such as fluorinated ethylene carbonate (fluoroethylene carbonate) and derivatives thereof, and ethylene carbonate having a fluorine-containing group. Examples of derivatives of fluorinated ethylene carbonate include fluorinated ethylene carbonate substituted with an alkyl group (e.g., an alkyl group with 1 to 4 carbon atoms). Among these, fluoroethylene carbonate having 1 to 8 fluorine atoms and derivatives thereof are preferred. Examples of fluoroethylene carbonate and derivatives thereof having 1 to 8 fluorine atoms, as well as ethylene carbonate having a fluorine-containing group, include monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, 4-fluoro-4-methylethylene carbonate, 4,5-difluoro-4-methylethylene carbonate, 4-fluoro-5-methylethylene carbonate, 4,4-difluoro-5-methylethylene carbonate, 4-(fluoromethyl)-ethylene carbonate, 4-(difluoromethyl)-ethylene carbonate, 4-(trifluoromethyl)-ethylene carbonate, 4-(fluoromethyl)-4-fluoroethylene carbonate, 4-(fluoromethyl)-5-fluoroethylene carbonate, 4-fluoro-4,5-dimethylethylene carbonate, 4,5-difluoro-4,5-dimethylethylene carbonate, and 4,4-difluoro-5,5-dimethylethylene carbonate. Among these, from the viewpoints of imparting high ionic conductivity to the electrolyte and facilitating the formation of a stable interface protective film, one or more selected from monofluoroethylene carbonate, 4,4-difluoroethylene carbonate, and 4,5-difluoroethylene carbonate are preferred. The fluorine atom-containing cyclic carbonates can be used alone or in combination of two or more kinds in any ratio.

[0049] [2. Non-aqueous electrolyte secondary battery] A nonaqueous electrolyte secondary battery according to one embodiment of the present invention is a nonaqueous electrolyte secondary battery comprising a positive electrode having a positive electrode active material capable of absorbing and releasing metal ions, and a negative electrode having a negative electrode active material capable of absorbing and releasing metal ions, and comprising a nonaqueous electrolyte.

[0050] [2-1.Non-aqueous electrolyte] As the non-aqueous electrolyte solution, the above-mentioned non-aqueous electrolyte solution is used. Note that, within the scope of the present invention, it is also possible to mix the above-mentioned non-aqueous electrolyte solution with other non-aqueous electrolyte solutions.

[0051] [2-2. Positive electrode] The positive electrode has a positive electrode active material on at least a portion of the surface of a current collector.

[0052] [2-2-1. Positive electrode active material] The positive electrode active material (lithium transition metal compound) used in the positive electrode will be described below.

[0053] [2-2-1-1. Lithium transition metal compounds] The lithium transition metal compound is a compound having a structure capable of desorbing and inserting lithium ions, and examples thereof include sulfides, phosphate compounds, silicate compounds, borate compounds, lithium transition metal composite oxides, etc. Among these, phosphate compounds and lithium transition metal composite oxides are preferred, and lithium transition metal composite oxides are more preferred. Examples of lithium transition metal composite oxides include those having a spinel structure that allows three-dimensional diffusion, and those having a layered structure that allows two-dimensional diffusion of lithium ions.

[0054] Those having a spinel structure are generally represented by the following composition formula (1). Li x’ M'2O4···(1) (In formula (1), x' is 1≦x'≦1.5, and M' includes an element including at least one transition metal element.) M' is preferably one or more transition metal elements. The lithium transition metal oxide represented by the composition formula (1) is specifically LiMn2O4, LiCoMnO4, LiNi 0.5 Mn 1.5 O4, LiCoVO4, etc.

[0055] Those having a layered structure are generally represented by the following composition formula (2). Li 1+x MO2···(2) (In formula (2), x is −0.1≦x≦0.5, and M includes at least one element including a transition metal element.) Specifically, LiNi 0.7 Mn0.15 Co 0.15 O2, LiCoO2, LiNiO2, LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.80 Co 0.15 Al 0.05 O2, LiNi 0.33 Co 0.33 Mn 0.33 O2, Li 1.05 Ni 0.33 Co 0.33 Mn 0.33 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, Li 1.05 Ni 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 Examples include O2.

[0056] Among these, from the viewpoint of improving the battery capacity, a lithium transition metal composite oxide having a layered structure is preferred, and a transition metal composite oxide represented by the following composition formula (3) is more preferred. Li a1 Ni b1 M c1 O2···(3) (In the composition formula (3), a1, b1, and c1 satisfy 0.90≦a1≦1.10, 0.30≦b1≦0.98, and 0.01≦c1≦0.5, respectively. M includes at least one element selected from the group consisting of Co, Mn, Al, Mg, Zr, Fe, Ti, V, Cr, La, Ce, Mo, Sc, Y, and Sr.) It is preferable that b1 and c1 satisfy 0.50≦b1+c1≦1, and it is more preferable that b1+c1=1. It is preferable that b1 satisfies 0.30≦b1≦0.99, and it is more preferable that b1 satisfies 0.50≦b1≦0.98. It is preferable that c1 satisfies 0.01≦c1≦0.7, and it is more preferable that c1 satisfies 0.02≦c1≦0.5.

[0057] In particular, from the viewpoint of the structural stability of the lithium transition metal composite oxide, a transition metal oxide represented by the following composition formula (4) is preferable. Li a2 Ni b2 Co c2 M d2 O2···(4) (In the composition formula (4), a2, b2, and c2 are numerical values ​​that satisfy 0.90≦a2≦1.10, 0.50≦b2≦0.98, and 0.01≦c2<0.50, respectively, and b2+c2=1 is satisfied. M includes at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, V, Cr, La, Ce, Mo, Sc, Y, and Sr.) A specific example of the lithium transition metal oxide represented by the composition formula (4) is LiNi 0.7 Mn 0.15 Co 0.15 O2, LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.80 Co 0.15 Al 0.05 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, Li 1.05 Ni 0.50 Co 0.20 Mn 0.30 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, etc. In particular, from the viewpoint of improving the battery capacity, b2 is preferably 0.55 or more, more preferably 0.60 or more, further preferably 0.65 or more, and particularly preferably 0.70 or more.

[0058] In each composition formula, M preferably contains Mn or Al, more preferably Mn or Al, and further preferably contains Mn, because this increases the structural stability of the lithium transition metal oxide and suppresses structural deterioration during repeated charging and discharging.

[0059] [2-2-1-2. Introduction of different elements] Furthermore, elements (foreign elements) other than the elements contained in the above composition formula may be incorporated into the lithium transition metal composite oxide.

[0060] [2-2-1-3. Surface coating] The positive electrode active material may have a surface-attached substance having a different composition from the positive electrode active material. Examples of the surface-attached substance include oxides such as aluminum oxide, sulfates such as lithium sulfate, and carbonates such as lithium carbonate. These surface-adhering substances can be attached to the surface of the positive electrode active material, for example, by dissolving or suspending them in a solvent, adding them to the positive electrode active material by impregnation, and drying them. The amount of the surface-attaching substance is preferably 1 μmol / g or more, and more preferably 10 μmol / g or more, and is usually 1 mmol / g or less, relative to the positive electrode active material. In this specification, a positive electrode active material having the above-mentioned surface-adhering substance attached to the surface thereof is also referred to as a "positive electrode active material".

[0061] [2-2-1-4. Blend] These positive electrode active materials may be used alone or in any combination of two or more in any ratio.

[0062] [2-2-2. Positive electrode composition and manufacturing method] The configuration and manufacturing method of the positive electrode are described below. In this embodiment, the positive electrode using the positive electrode active material can be manufactured by a conventional method. That is, the positive electrode active material and the binder, and if necessary, the conductive material and the thickener, etc. are mixed in a dry state to form a sheet, which is then pressed onto the positive electrode current collector, or these materials are dissolved or dispersed in a liquid medium such as an aqueous solvent or an organic solvent to form a slurry, which is then applied to the positive electrode current collector and dried to form a positive electrode active material layer on the current collector, thereby obtaining a positive electrode. In addition, for example, the above-mentioned positive electrode active material may be roll-formed into a sheet electrode, or may be compression-formed into a pellet electrode. Hereinafter, the case where the slurry is successively applied to the positive electrode current collector and then dried will be described.

[0063] [2-2-2-1. Active material content] The content of the positive electrode active material in the positive electrode active material layer is usually 80% by mass or more and 99.5% by mass or less.

[0064] [2-2-2-2.Conductive materials] Any known conductive material can be used as the conductive material. Specific examples include metal materials such as copper and nickel; graphite such as natural graphite and artificial graphite; carbon black such as acetylene black; and carbon-based materials such as amorphous carbon such as needle coke. The conductive material may be used alone or in any combination and ratio of two or more. The conductive material is used so that it is usually contained in the positive electrode active material layer in an amount of 0.01% by mass or more and 50% by mass or less.

[0065] [2-2-2-3. Binder] The binder used in producing the positive electrode active material layer is not particularly limited as long as it is a material that is dissolved or dispersed in a liquid medium for a slurry, for example, when the positive electrode active material layer is formed by a coating method. In view of weather resistance, chemical resistance, heat resistance, flame retardancy, and the like, preferred are fluorine-based resins such as polyvinyl fluoride, polyvinylidene fluoride, and polytetrafluoroethylene; and CN group-containing polymers such as polyacrylonitrile and polyvinylidene cyanide. In addition, mixtures, modified products, derivatives, random copolymers, alternating copolymers, graft copolymers, block copolymers, etc. of the above polymers can also be used. The binder may be used alone or in any combination and ratio of two or more kinds. When a resin is used as a binder, the weight average molecular weight of the resin is optional as long as it does not significantly impair the effects of the present invention, but is usually at least 10,000, preferably at least 50,000, and particularly preferably at least 100,000, and is usually at most 3,000,000, preferably at most 950,000, and particularly preferably at most 900,000. If the molecular weight is within this range, the strength of the electrode is improved, and the electrode can be suitably formed. The proportion of the binder in the positive electrode active material layer is usually 0.1% by mass or more and 80% by mass or less.

[0066] [2-2-2-4. Current collector] The material of the positive electrode current collector is not particularly limited, and any known material can be used. Specific examples include metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum. Among them, aluminum is preferable. The shape of the current collector may be metal foil, metal cylinder, metal coil, metal plate, metal thin film, expanded metal, punched metal, foamed metal, etc. Among these, metal foil or metal thin film is preferable. The metal thin film may be appropriately formed into a mesh shape. When the positive electrode current collector has a plate or film shape, the thickness of the current collector is not limited. It is greater than 1 μm and less than 1 mm.

[0067] [2-2-2-5. Thickness of positive electrode plate] The thickness of the positive electrode plate is not particularly limited, but from the viewpoint of high capacity and high output, the thickness of the positive electrode active material layer obtained by subtracting the thickness of the current collector from the thickness of the positive electrode plate is usually 10 μm or more on one side of the current collector. It is less than 500 μm.

[0068] [2-2-2-6. Electrode density] The positive electrode active material layer obtained by coating and drying is preferably compressed by a hand press, a roller press, or the like in order to increase the packing density of the positive electrode active material. The density of the positive electrode active material layer present on the current collector is usually 1.5 g / cm 3 More than 4.5g / cm 3 The following is the result.

[0069] [2-2-2-7. Surface coating of positive electrode plate] In addition, the positive electrode plate may have a substance having a different composition from that of the positive electrode plate attached to its surface, and the substance in question may be the same as the surface-attached substance that may be attached to the surface of the positive electrode active material.

[0070] [2-3. Negative electrode] The negative electrode has a negative electrode active material on at least a portion of the surface of a current collector.

[0071] [2-3-1. Negative electrode active material] The negative electrode active material used in the negative electrode is not particularly limited as long as it can electrochemically absorb and release metal ions. Specific examples include carbon-based materials, materials containing metal elements and / or metalloid elements that can be alloyed with Li, lithium-containing metal composite oxide materials, and mixtures thereof. Among these, it is preferable to use carbon-based materials, materials containing metal elements and / or metalloid elements that can be alloyed with Li, and mixtures of materials containing metal elements and / or metalloid elements that can be alloyed with Li and carbon-based materials, in terms of good cycle characteristics and safety, and excellent continuous charging characteristics. These may be used alone or in any combination of two or more.

[0072] [2-3-1-1. Carbon-based materials] Examples of carbonaceous materials include natural graphite, artificial graphite, amorphous carbon, carbon-coated graphite, graphite-coated graphite, and resin-coated graphite. Of these, natural graphite is preferred. The carbonaceous materials may be used alone or in any combination and ratio of two or more. Examples of natural graphite include scaly graphite, scaly graphite, and / or graphite particles obtained by subjecting such graphite to treatment such as spheroidization or densification. Among these, from the viewpoint of particle packing property or charge / discharge rate characteristics, spherical or ellipsoidal graphite particles that have been subjected to spheroidization treatment are particularly preferred. The average particle size (d50) of the graphite particles is usually 1 μm or more and 100 μm or less.

[0073] [2-3-1-2. Properties of carbon-based materials] The carbonaceous material as the negative electrode active material preferably satisfies at least one of the characteristics such as the physical properties and shape shown in the following (1) to (4), and particularly preferably satisfies several of them at the same time. (1) X-ray diffraction parameters The d value (interlayer distance) of the lattice plane (002 plane) of carbon-based materials determined by X-ray diffraction using the Gakushin method is usually 0.335 nm to 0.360 nm. Also, the crystallite size (Lc) of carbon-based materials determined by X-ray diffraction using the Gakushin method is usually 1.0 nm or more. (2) Volume-based average particle size The volume-based average particle size of a carbon-based material is the volume-based average particle size (median diameter) determined by a laser diffraction / scattering method, and is usually 1 μm or more and 100 μm or less. (3) Raman R value, Raman half-width The Raman R value of a carbon-based material is a value measured using argon ion laser Raman spectroscopy, and is usually 0.01 or more and 1.5 or less. In addition, the 1580 cm -1 The Raman half-width in the vicinity is not particularly limited, but is usually 10 cm -1 More than 100cm -1 The following is the result. (4) BET specific surface area The BET specific surface area of ​​a carbon-based material is the value of the specific surface area measured using the BET method, and is usually 0.1 m 2 ·g -1 More than 100m 2 ·g -1 The following is the result. The negative electrode active material may contain two or more types of carbon-based materials having different properties. Here, the properties mean X-ray diffraction parameters, volume-based average particle size, Raman R value, Raman half-width, and BET specific surface area. Preferable examples include the case where the volume-based particle size distribution is not symmetric when centered on the median diameter, the case of containing two or more types of carbon-based materials having different Raman R values, and the case of containing two or more types of carbon-based materials having different X-ray parameters.

[0074] [2-3-1-3. Material containing a metal element and / or a metalloid element alloyable with Li] Any conventionally known material containing a metal element and / or a metalloid element alloyable with Li can be used, but from the viewpoints of capacity and cycle life, for example, it is preferably a single substance or a compound of a metal and / or a metalloid element that may be coated with carbon and is selected from the group consisting of Sb, Si, Sn, Al, As, and Zn. Further, when the material containing a metal element and / or a metalloid element alloyable with Li contains two or more types of elements, the material may be an alloy material composed of an alloy of these metals. In addition, examples of the material containing a metal element and / or a metalloid element alloyable with Li include oxides, nitrides, carbides, etc. These may contain two or more types of metal elements and / or metalloid elements alloyable with Li. Among them, metallic Si (hereinafter, may be referred to as Si in some cases) or a Si-containing inorganic compound is preferable in terms of increasing the capacity. Further, the material containing a metal element and / or a metalloid element alloyable with Li may already be alloyed with Li at the time of manufacturing the negative electrode described later. In this specification, Si or a Si-containing inorganic compound is collectively referred to as a Si compound. Specific examples of the Si compound include SiO x (0 ≦ x ≦ 2), etc. Specific examples of the metal compound alloyed with Li include Li y Si (0 < y ≦ 4.4), Li2SiO 2+z (0 < z ≦ 2), etc. As the Si compound, a Si oxide (SiO x1When 0 < x1 ≤ 2), it is preferable in terms of having a larger theoretical capacity compared to graphite, or amorphous Si or nano-sized Si crystals are preferable in that alkali ions such as lithium ions can easily enter and exit, enabling high capacity to be obtained. When the material containing a metal element and / or a metalloid element capable of alloying with Li is in the form of particles, its average particle diameter (d50) is usually 0.01 μm or more and 10 μm or less from the viewpoint of cycle life.

[0075] [2-3-1-4. Mixture of particles of a material containing a metal element and / or a metalloid element capable of alloying with Li and graphite particles] The mixture of particles of a material containing a metal element and / or a metalloid element capable of alloying with Li and graphite particles used as the negative electrode active material may be a mixture in which the particles of the material containing a metal element and / or a metalloid element capable of alloying with Li and the aforementioned graphite particles are mixed in a state of particles of independent materials, or may be a composite in which the particles of the material containing a metal element and / or a metalloid element capable of alloying with Li are present on the surface or inside of the graphite particles. The content ratio of the particles of the material containing a metal element and / or a metalloid element capable of alloying with Li to the total of the particles of the material containing a metal element and / or a metalloid element capable of alloying with Li and graphite particles is usually 1 mass% or more and 99 mass% or less.

[0076] [2-3-1-5. Lithium-containing metal composite oxide material] The lithium-containing metal composite oxide material used as the negative electrode active material is not particularly limited as long as it can occlude and release lithium ions, but a lithium-containing metal composite oxide material containing titanium is preferable from the viewpoint of high current density charge-discharge characteristics, a composite oxide of lithium and titanium (hereinafter, may be abbreviated as "lithium titanium composite oxide") is more preferable, and a lithium titanium composite oxide having a spinel structure is particularly preferable because it greatly reduces the output resistance. Furthermore, the lithium and / or titanium of the lithium titanium composite oxide may be substituted with another metal element, for example, at least one element selected from the group consisting of Al, Ga, Cu and Zn. Lithium titanium composite oxide, Li 4 / 3 Ti 5 / 3 O4, Li1Ti2O4 and Li 4 / 5 Ti 11 / 5 O4 is preferred. In addition, examples of lithium titanium composite oxides in which part of lithium and / or titanium is replaced with other elements include Li 4 / 3 Ti 4 / 3 Al 1 / 3 O4 is preferred.

[0077] [2-3-2. Negative electrode composition and manufacturing method] The negative electrode may be produced by any known method as long as it does not significantly impair the effects of the present invention. For example, the negative electrode may be produced by adding a binder, a liquid medium such as an aqueous solvent or an organic solvent, and if necessary, a thickener, a conductive material, a filler, etc. to the negative electrode active material to form a slurry, which is applied to a current collector, dried, and then pressed to form a negative electrode active material layer.

[0078] [2-3-2-1. Active material content] The content of the negative electrode active material in the negative electrode active material layer is usually 80% by mass or more and 99.5% by mass or less.

[0079] [2-3-2-2. Electrode density] The negative electrode active material layer obtained by coating and drying is preferably compacted by hand press, roller press, etc. to increase the packing density of the negative electrode active material. There are no particular restrictions on the electrode structure when the negative electrode active material is made into an electrode, but the density of the negative electrode active material layer present on the current collector is usually 1 g cm -3 More than 2.2g cm -3 The following is the result.

[0080] [2-3-2-3. Thickener] The thickener is usually used to adjust the viscosity of the slurry. The thickener is not particularly limited, but specifically includes carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, etc. These may be used alone or in any combination and ratio of two or more. When a thickener is used, the ratio of the thickener to the negative electrode active material is usually 0.1 mass % or more and 5 mass % or less.

[0081] [2-3-2-4. Binder] There are no particular limitations on the binder that binds the negative electrode active material, so long as it is a material that is stable in the nonaqueous electrolyte solution and the liquid medium used in the production of the electrode. Specific examples include rubber-like polymers such as SBR (styrene-butadiene rubber), isoprene rubber, butadiene rubber, fluororubber, NBR (acrylonitrile-butadiene rubber), and ethylene-propylene rubber; fluorine-based polymers such as polyvinylidene fluoride, polytetrafluoroethylene, and tetrafluoroethylene-ethylene copolymers. These may be used alone or in any combination and ratio of two or more. The ratio of the binder to the negative electrode active material is usually 0.1% by mass or more and 20% by mass or less. In particular, when the binder contains a rubber-like polymer such as SBR as a main component, the ratio of the binder to the negative electrode active material is preferably 0.1% by mass or more and 5% by mass or less. Also, when the binder contains a fluorine-based polymer such as polyvinylidene fluoride as a main component, the ratio of the binder to the negative electrode active material is preferably 1% by mass or more and 15% by mass or less.

[0082] [2-3-2-5. Current collector] Any known current collector can be used to hold the negative electrode active material. Examples of the current collector for the negative electrode include metal materials such as aluminum, copper, nickel, stainless steel, and nickel-plated steel, and copper is particularly preferred from the standpoints of ease of processing and cost. The shape of the current collector may be metal foil, metal cylinder, metal coil, metal plate, metal thin film, expanded metal, punched metal, foamed metal, etc. Among these, metal foil or metal thin film is preferable. The metal foil and metal thin film may be appropriately formed into a mesh shape. When the negative electrode current collector has a plate or film shape, the current collector may have any thickness, but it is usually 1 μm or more and 1 mm or less.

[0083] [2-3-2-6. Thickness of negative electrode plate] The thickness of the negative electrode (also called "negative electrode plate") is designed to match the positive electrode used and is not particularly limited, but the thickness of the negative electrode active material layer, calculated by subtracting the thickness of the current collector from the thickness of the negative electrode material, is usually 15 μm or more and 300 μm or less.

[0084] [2-3-2-7. Surface coating of negative electrode plate] The negative electrode plate may have a surface to which a substance having a different composition from the negative electrode active material (surface-attached substance) is attached. Examples of the surface-attached substance include oxides such as aluminum oxide, sulfates such as lithium sulfate, and carbonates such as lithium carbonate.

[0085] [2-4. Separator] A separator is usually interposed between the positive electrode and the negative electrode to prevent short circuiting. In this case, the non-aqueous electrolyte is usually impregnated into the separator before use. There are no particular limitations on the material and shape of the separator, and any known material can be used as long as it does not significantly impair the effects of the present invention.

[0086] [2-5.Battery design] [2-5-1. Electrode group] The electrode group may be either a laminated structure of the positive electrode plate and the negative electrode plate with the separator interposed therebetween, or a structure of the positive electrode plate and the negative electrode plate wound in a spiral shape with the separator interposed therebetween. The ratio of the volume of the electrode group to the internal volume of the battery is usually 40% or more and 90% or less.

[0087] [2-5-2. Current collection structure] In the case where the electrode group has the above-mentioned laminated structure, a structure in which the metal core parts of the electrode layers are bundled and welded to a terminal is preferably used. A structure in which multiple terminals are provided in the electrode to reduce resistance is also preferably used. In the case where the electrode group has the above-mentioned wound structure, the internal resistance can be reduced by providing multiple lead structures on each of the positive electrode and the negative electrode and bundling them to a terminal.

[0088] [2-5-3.Protection elements] The protective element may be a PTC (Positive Temperature Coefficient) element whose resistance increases with heat generation due to excessive current, a thermal fuse, a thermistor, a valve (current cutoff valve) that cuts off the current flowing through the circuit due to a sudden increase in the battery's internal pressure or temperature during abnormal heat generation, etc. It is preferable to select the above protective element so that it will not operate under normal use at high current, and it is even more preferable to design it so that abnormal heat generation or thermal runaway does not occur even without the protective element.

[0089] [2-5-4. Exterior body] A non-aqueous electrolyte secondary battery is usually constructed by housing the above-mentioned non-aqueous electrolyte, negative electrode, positive electrode, separator, etc. in an exterior body (exterior case). There are no limitations on this exterior body, and any known exterior body can be used as long as it does not significantly impair the effects of the present invention. The material of the exterior case is not particularly limited as long as it is a substance that is stable to the non-aqueous electrolyte solution used, but from the viewpoint of weight reduction, metal such as aluminum or an aluminum alloy, or a laminate film is preferably used. Examples of exterior cases using the above metals include those in which the metals are welded together by laser welding, resistance welding, or ultrasonic welding to form a sealed, airtight structure, and those in which the above metals are used with a resin gasket in between to form a crimped structure.

[0090] [2-5-5. Shape] The shape of the exterior case is also arbitrary, and may be, for example, cylindrical, rectangular, laminated, coin-shaped, large, or the like. EXAMPLES

[0091] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. The compounds used in this example are shown below. [ka]

[0092] <Examples 1 to 7 and Comparative Examples 1 to 5> [Preparation of non-aqueous electrolyte] In a dry argon atmosphere, thoroughly dried LiPF6 was dissolved in a mixture of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate (volume ratio 3:4:3) at 1.2 mol / L (as the concentration in the non-aqueous electrolyte), and vinylene carbonate was dissolved at 1 mass % to prepare a reference non-aqueous electrolyte. The additives shown in Table 1 were further added to 100 parts by weight of the prepared reference non-aqueous electrolyte. The amount of each additive added was set so that the content of each additive in the obtained non-aqueous electrolyte was the amount shown in Table 1.

[0093] [Preparation of positive electrode] LiNi as the positive electrode active material 0.7 Mn 0.15 Co 0.15 90 parts by mass of O2, 7 parts by mass of acetylene black as a conductive material, and 3 parts by mass of polyvinylidene fluoride (PVdF) as a binder were mixed in N-methyl-2-pyrrolidone to form a slurry. The obtained slurry was uniformly applied to an aluminum foil having a thickness of 15 μm, dried, and then roll-pressed to form a positive electrode. The density of the positive electrode active material layer was 3.3 g / cm. 3 It was.

[0094] [Preparation of negative electrode] 49 parts by mass of graphite powder was mixed with 50 parts by mass of an aqueous dispersion of sodium carboxymethylcellulose (concentration of sodium carboxymethylcellulose: 1% by mass) as a thickener and 1 part by mass of an aqueous dispersion of styrene-butadiene rubber (concentration of styrene-butadiene rubber: 50% by mass) as a binder, and mixed in a disperser to form a slurry. The obtained slurry was uniformly applied to a copper foil with a thickness of 10 μm, dried, and roll-pressed to form a negative electrode.

[0095] [Manufacturing non-aqueous electrolyte batteries] The positive electrode, the negative electrode, and the polyolefin separator were laminated in this order, and the battery element thus obtained was wrapped in an aluminum laminate film, and the nonaqueous electrolyte was injected and then vacuum sealed to prepare a sheet-shaped nonaqueous electrolyte secondary battery.

[0096] <Evaluation of non-aqueous electrolyte secondary batteries> The nonaqueous electrolyte secondary batteries prepared in the examples were evaluated as follows.

[0097] Initial charge / discharge and internal resistance evaluation In a thermostatic bath at 25°C, a sheet-shaped nonaqueous electrolyte secondary battery was charged at a constant current of 0.05C (the current value at which the rated capacity based on the discharge capacity at a 1-hour rate is discharged in 1 hour is defined as 1C; the same applies below) to 3.7V, then charged at a constant current / constant voltage of 0.2C to a voltage of 4.25V, and then discharged at a constant current of 0.2C to 2.8V. Furthermore, the nonaqueous electrolyte secondary battery was stabilized by charging at a constant current and constant voltage at 0.2 C to 4.1 V, and then storing at 60° C. for 24 hours. Thereafter, the battery was discharged at a constant current to 2.8 V at 25° C., and then charged at a constant current and constant voltage at 0.2 C to a voltage of 4.25 V. Thereafter, the battery was discharged at a constant current of 0.2 C to 2.5 V, and the discharge capacity at this time was designated as the “initial capacity”. Thereafter, constant current / constant voltage charging was performed at 0.2 C at 25° C. up to a voltage of 3.7 V. Each was discharged at 0.25 C, 0.5 C, 0.75 C, and 1 C, and the voltage was measured after 10 seconds. The internal resistance was calculated from the current-voltage line and used as the "initial resistance." Next, constant current / constant voltage charging was carried out at 0.2 C up to a voltage of 4.25 V, and the initial charge / discharge was completed.

[0098] Cycle testing In a thermostatic chamber at 45° C., the sheet-shaped non-aqueous electrolyte secondary battery was charged at a constant current and constant voltage of 1 C to a voltage of 4.25 V, and then discharged at a constant current of 1 C to a voltage of 2.8 V. This was repeated 200 times. Thereafter, constant current-constant voltage charging was performed at 0.2 C to a voltage of 4.25 V at 25° C., and then constant current discharging was performed at 0.2 C to 2.8 V, and the discharge capacity at this time was defined as the “capacity after 200 cycles.” The ratio of the initial capacity to the capacity after 200 cycles was defined as the “high temperature cycle capacity retention rate.” Thereafter, constant current-constant voltage charging was performed at 0.2C at 25°C up to a voltage of 3.7V. Each was discharged at 0.25C, 0.5C, 0.75C, and 1C, and the voltage was measured 10 seconds later. The internal resistance was calculated from this current-voltage line and recorded as the "resistance after 200 cycles." The ratio of the initial resistance to the resistance after 200 cycles was recorded as the "high temperature cycle resistance increase rate." The higher the high-temperature cycle capacity retention rate, the better, and the lower the high-temperature cycle resistance increase rate, the better.

[0099] Table 1 shows the high temperature cycle capacity retention rate and the high temperature cycle resistance increase rate (relative value assuming that Comparative Example 1 is 100) of the examples and comparative examples. [Table 1]

[0100] As is clear from Table 1, the nonaqueous electrolyte secondary battery comprising a nonaqueous electrolyte solution (Examples 1 to 7) containing a compound represented by formula (I) and at least two kinds of anion-containing compounds can achieve both an improvement in capacity retention rate and suppression of resistance increase after high-temperature cycle charge / discharge, as confirmed by comparison with a nonaqueous electrolyte secondary battery comprising a nonaqueous electrolyte solution containing only one kind of anion-containing compound (Comparative Example 1), a nonaqueous electrolyte solution containing two kinds of anion compounds but not containing the compound represented by formula (I) (Comparative Example 2), and a nonaqueous electrolyte solution containing one kind of anion-containing compound and the compound represented by formula (I) (Comparative Example 3). Furthermore, the nonaqueous electrolyte secondary batteries equipped with nonaqueous electrolyte solutions containing the compounds 2 and 3 used in the prior art and two kinds of anion-containing compounds (Comparative Examples 4 and 5) had a worse high-temperature cycle capacity retention rate than the nonaqueous electrolyte secondary batteries equipped with nonaqueous electrolyte solutions containing the compound represented by formula (I) and two kinds of anion-containing compounds (Examples 1 to 7). It is believed that the above results are due to the fact that the compound represented by formula (I) forms an excellent protective coating on the positive electrode, and that the two types of anions act on the negative and positive electrodes to suppress side reactions on the electrodes while suppressing an increase in resistance, thereby achieving the effects of the present invention.

Claims

1. Contains a compound represented by formula (I) and at least two anion-containing compounds, The nonaqueous electrolyte solution contains, as at least one of the anion-containing compounds, a compound selected from the group consisting of an anion-containing compound having an S═O bond, a phosphate anion-containing compound having a P-F bond and a P═O bond, and an oxalate complex anion-containing compound. [C5] (In the above formula (I), R 1 , R 2 each independently represents a hydrogen atom, a cyano group, a halogen atom, or an organic group having from 1 to 10 carbon atoms, The organic group may be substituted with at least one of a cyano group and a halogen atom, and R 1 and R 2 At least one of them contains a cyano group.)

2. The nonaqueous electrolyte solution according to claim 1 , wherein the compound represented by formula (I) contains one cyano group.

3. R 1 The nonaqueous electrolyte solution according to claim 1 or 2, wherein the number of cyano groups therein is 1.

4. R 2 The nonaqueous electrolyte according to claim 1 or 2, wherein is a hydrogen atom or a saturated hydrocarbon group having 1 to 3 carbon atoms.

5. R 2 The nonaqueous electrolyte solution according to claim 4 , wherein is a hydrogen atom.

6. The nonaqueous electrolyte solution according to claim 1 or 2, wherein the content of the compound represented by formula (I) is 0.001 to 5 mass %.

7. One of the anion-containing compounds is PF 6 - The nonaqueous electrolyte according to claim 1 or 2, which is an anion-containing compound.

8. 3. The nonaqueous electrolyte solution according to claim 1, wherein the total content of the anion-containing compound having an S═O bond, the phosphate anion-containing compound having a P-F bond and a P═O bond, and the oxalate complex anion-containing compound is 0.001 to 5 mass %.

9. 3. The nonaqueous electrolyte solution according to claim 1, wherein a mass ratio (A / B) of a content (A) of the compound represented by formula (I) to a total content (B) of an anion-containing compound having an S═O bond, and a phosphate anion-containing compound having a P-F bond and a P═O bond is 0.01 / 99.99 or more and 99.99 / 0.01 or less.

10. 3. The nonaqueous electrolyte solution according to claim 1, further comprising a cyclic carbonate having a carbon-carbon unsaturated bond.

11. A non-aqueous electrolyte battery comprising a positive electrode, a negative electrode, and the non-aqueous electrolyte according to claim 1 or 2.

12. The nonaqueous electrolyte battery according to claim 11 , wherein the positive electrode contains a lithium transition metal compound represented by the following composition formula (2): Li 1+x M.O. 2 ...(2) (In the composition formula (2), x is −0.1≦x≦0.5, and M includes at least one element including a transition metal.)

13. The nonaqueous electrolyte battery according to claim 11 , wherein the positive electrode contains a lithium transition metal compound represented by the following composition formula (3): Li a1 Ni b1 M c1 O 2 ...(3) (In the composition formula (3), a1, b1, and c1 satisfy 0.90≦a1≦1.10, 0.30≦b1≦0.98, and 0.01≦c1≦0.5, respectively. M contains at least one element selected from the group consisting of Co, Mn, Al, Mg, Zr, Fe, Ti, V, Cr, La, Ce, Mo, Sc, Y, and Sr.)

Citation Information

Patent Citations

  • High-voltage electrolyte and lithium ion battery using same

    CN105226324A

  • Lithium ion battery electrolyte additive and lithium ion battery electrolyte

    CN110931872A

  • Electrolytic solution for secondary battery, secondary battery, battery pack, electric motor vehicle, electric power storage system, electric motor-driven tool and electronic equipment

    JP2018041588A

  • Organic electrolytic solution and and Lithium battery comprising the solution

    KR1020140135038A

  • Nonaqueous liquid electrolyte for use in secondary battery, and lithium-ion secondary battery

    WO2015046175A1