Lens portion, laminate, display body, method for manufacturing display body, and display method

The lens unit with polarizing and λ/4 members optimizes light transmission and reflection, addressing the heaviness and definition issues in VR goggles, resulting in lightweight and high-definition display systems.

JP2024133081AActive Publication Date: 2024-10-01NITTO DENKO CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024107181
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-01
Estimated Expiration
2042-05-10

AI Technical Summary

Technical Problem

Existing VR goggles are heavy and lack high definition, necessitating the development of lightweight and high-definition optical members for display systems.

Method used

A lens unit comprising a polarizing member, reflective section, and λ/4 members with specific angular arrangements and thicknesses, integrated with a half mirror and lens sections, to optimize light transmission and reflection for improved image display.

Benefits of technology

The solution achieves lightweight VR goggles with high definition by optimizing light polarization and reflection, enhancing image quality and reducing weight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133081000001_ABST
    Figure 2024133081000001_ABST
Patent Text Reader

Abstract

To provide a lens portion capable of achieving weight reduction and high definition of a VR goggle.SOLUTION: A lens portion is used for a display system that displays an image to a user. The lens portion comprises: a reflection portion that reflects light, which is emitted forward from a display surface of a display element representing the image and passes through a polarization member and a first λ / 4 member, and that includes a reflection type polarization member and an absorption type polarization member disposed in front of the reflection type polarization member; a first lens portion disposed on an optical path between the display element and the reflection portion; a half mirror that is disposed between the display element and the first lens portion, transmits the light emitted from the display element, and reflects the light reflected by the reflection portion toward the reflection portion; and a second λ / 4 member disposed on an optical path between the half mirror and the reflection portion. A thickness of an absorption type polarizing film constituting the absorption type polarization member is 8 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lens portion, a laminate, a display, a manufacturing method for a display, and a display method. [Background technology]

[0002] Image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices), are rapidly becoming widespread. In image display devices, optical members such as polarizing members and phase difference members are generally used to realize image display and to improve the performance of the image display (see, for example, Patent Document 1).

[0003] In recent years, new applications for image display devices have been developed. For example, goggles with displays (VR goggles) for realizing virtual reality (VR) have begun to be commercialized. Since the use of VR goggles in various situations is being considered, there is a demand for them to be lightweight, high-definition, and the like. Weight reduction can be achieved, for example, by thinning the lenses used in the VR goggles. On the other hand, there is also a demand for the development of optical members suitable for display systems using thin lenses. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2021-103286 A Summary of the Invention [Problem to be solved by the invention]

[0005] In view of the above, a primary object of the present invention is to provide a lens portion that can realize lightweight, high-definition VR goggles. [Means for solving the problem]

[0006] 1. A lens unit according to an embodiment of the present invention is a lens unit used in a display system that displays an image to a user, and comprises: a reflecting unit that reflects light that is emitted forward from a display surface of a display element that displays an image and passes through a polarizing element and a first λ / 4 element, and includes a reflective polarizing element and an absorptive polarizing element arranged in front of the reflective polarizing element; a first lens unit that is arranged on an optical path between the display element and the reflecting unit; a half mirror that is arranged between the display element and the first lens unit, transmits light emitted from the display element and reflects light reflected by the reflecting unit towards the reflecting unit; and a second λ / 4 element that is arranged on the optical path between the half mirror and the reflecting unit, and the thickness of the absorptive polarizing film that constitutes the absorptive polarizing element is 8 μm or less. 2. In the lens portion as described in 1 above, the reflection axis of the reflective polarizing member and the absorption axis of the absorptive polarizing member may be arranged parallel to each other. 3. In the lens portion according to the above 1 or 2, the first lens portion and the half mirror may be integral with each other. 4. In the lens portion described in any one of 1 to 3 above, the lens portion may include a second lens portion disposed in front of the reflecting portion. 5. In the lens portion described in any one of 1 to 4 above, the angle between the absorption axis of the polarizing member included in the display element and the slow axis of the first λ / 4 member may be 40° to 50°, and the angle between the absorption axis of the polarizing member included in the display element and the slow axis of the second λ / 4 member may be 40° to 50°. 6. In the lens portion according to any one of the above items 1 to 5, the ratio of the thickness of the absorptive polarizing film to the thickness of the reflective polarizing member may be 15% or less.

[0007] 7. A laminate according to an embodiment of the present invention is used in the reflective portion of the lens unit described in any one of 1 to 6 above, and has the reflective polarizing member and the absorptive polarizing member. 8. In the laminate according to the above item 7, the reflective polarizing member and the absorptive polarizing member may be laminated via an adhesive layer.

[0008] 9. A display according to an embodiment of the present invention has a lens portion as described in any one of 1 to 6 above. 10. A method for manufacturing a display according to an embodiment of the present invention, which is a method for manufacturing a display having a lens portion as described in any one of 1 to 6 above.

[0009] 11. A display method according to an embodiment of the present invention includes the steps of: passing light representing an image emitted through a polarizing element and a first λ / 4 element through a half mirror and a first lens unit; passing the light that has passed through the half mirror and the first lens unit through a second λ / 4 element; reflecting the light that has passed through the second λ / 4 element toward the half mirror with a reflecting unit including a reflective polarizing element; making the light reflected by the reflecting unit and the half mirror transmittance through the reflective polarizing element of the reflecting unit by the second λ / 4 element; and transmitting the light that has transmitted through the reflective polarizing element through an absorbing polarizing element, wherein the thickness of the absorbing polarizing film that constitutes the absorbing polarizing element is 8 μm or less.

[0010] 12. A manufacturing method for an absorptive polarizing film in a lens portion according to an embodiment of the present invention includes forming a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin on one side of a long thermoplastic resin substrate to form a laminate, and subjecting the laminate to an auxiliary air-stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order, in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. 13. In the method according to the above 12, the content of the halide in the polyvinyl alcohol-based resin layer is 5 to 20 parts by weight based on 100 parts by weight of the polyvinyl alcohol-based resin. 14. In the method according to 12 or 13 above, the stretching ratio in the auxiliary in-air stretching treatment is 2.0 times or more. 15. In the manufacturing method according to any one of the above 12 to 14, the drying shrinkage treatment step is a step of heating using a heating roll. 16. In the manufacturing method according to the above item 15, the temperature of the heating roll is 60° C. to 120° C., and the shrinkage rate in the width direction of the laminate due to the drying shrinkage treatment is 2% or more. Effect of the Invention

[0011] The lens portion according to the embodiment of the present invention can achieve lighter weight and higher definition VR goggles. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram showing a general configuration of a display system according to an embodiment of the present invention. [Diagram 2] 2 is a schematic cross-sectional view showing an example of a laminate used in a reflector of the display system shown in FIG. 1. [Diagram 3] FIG. 2 is a schematic perspective view showing an example of a multilayer structure included in a reflective polarizing film. [Figure 4] FIG. 2 is a schematic diagram showing an example of a drying shrinkage treatment using a heating roll. [Diagram 5] 1 is an observation photograph showing optical unevenness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the width, thickness, shape, etc. of each part may be shown more diagrammatically than in the embodiment, but these are merely examples and do not limit the interpretation of the present invention.

[0014] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When angles are referred to herein, the angles include both clockwise and counterclockwise angles relative to a reference direction, so for example, "45°" means ±45°.

[0015] FIG. 1 is a schematic diagram showing a schematic configuration of a display system according to one embodiment of the present invention. In FIG. 1, the arrangement and shape of each component of a display system 2 are illustrated. The display system 2 includes a display element 12, a reflecting section 14, a first lens section 16, a half mirror 18, a first phase difference member 20, a second phase difference member 22, and a second lens section 24. The reflecting section 14 is disposed in front of the display surface 12a side of the display element 12, and can reflect light emitted from the display element 12. The first lens section 16 is disposed on the optical path between the display element 12 and the reflecting section 14, and the half mirror 18 is disposed between the display element 12 and the first lens section 16. The first phase difference member 20 is disposed on the optical path between the display element 12 and the half mirror 18, and the second phase difference member 22 is disposed on the optical path between the half mirror 18 and the reflecting section 14.

[0016] The components arranged in front of the half mirror (in the illustrated example, the half mirror 18, the first lens portion 16, the second phase difference member 22, the reflecting portion 14 and the second lens portion 24) may be collectively referred to as the lens portion (lens portion 4).

[0017] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12a for displaying an image. The light emitted from the display surface 12a passes through, for example, a polarizing member (typically, a polarizing film) that may be included in the display element 12, and is converted into a first linearly polarized light.

[0018] The first phase difference member 20 is a λ / 4 member that can convert a first linearly polarized light incident on the first phase difference member 20 into a first circularly polarized light (hereinafter, the first phase difference member may be referred to as a first λ / 4 member). The first phase difference member 20 may be provided integrally with the display element 12.

[0019] The half mirror 18 transmits the light emitted from the display element 12 and reflects the light reflected by the reflecting portion 14 toward the reflecting portion 14. The half mirror 18 is provided integrally with the first lens portion 16.

[0020] The second phase difference member 22 is a λ / 4 member that can transmit the light reflected by the reflecting unit 14 and the half mirror 18 through the reflecting unit 14 including a reflective polarizing member (hereinafter, the second phase difference member may be referred to as a second λ / 4 member). The second phase difference member 22 may be provided integrally with the first lens unit 16, or may be provided integrally with the reflective polarizing member included in the reflecting unit 14.

[0021] The first circularly polarized light output from the first λ / 4 member 20 passes through the half mirror 18 and the first lens unit 16, and is converted into the second linearly polarized light by the second λ / 4 member 22. The second linearly polarized light output from the second λ / 4 member 22 is reflected toward the half mirror 18 without passing through the reflective polarizing member included in the reflecting unit 14. At this time, the polarization direction of the second linearly polarized light that is incident on the reflective polarizing member included in the reflecting unit 14 is the same as the reflection axis of the reflective polarizing member. Therefore, the second linearly polarized light that is incident on the reflecting unit is reflected by the reflective polarizing member.

[0022] The second linearly polarized light reflected by the reflecting unit 14 is converted into the second circularly polarized light by the second λ / 4 member 22, and the second circularly polarized light emitted from the second λ / 4 member 22 passes through the first lens unit 16 and is reflected by the half mirror 18. The second circularly polarized light reflected by the half mirror 18 passes through the first lens unit 16 and is converted into the third linearly polarized light by the second λ / 4 member 22. The third linearly polarized light passes through the reflective polarizing member included in the reflecting unit 14. At this time, the polarization direction of the third linearly polarized light incident on the reflective polarizing member included in the reflecting unit 14 is the same as the transmission axis of the reflective polarizing member. Therefore, the third linearly polarized light incident on the reflecting unit 14 passes through the reflective polarizing member.

[0023] The light transmitted through the reflecting portion 14 passes through the second lens portion 24 and enters the user's eye 26.

[0024] For example, the absorption axis of the polarizing member included in the display element 12 and the reflection axis of the reflective polarizing member included in the reflector 14 may be disposed approximately parallel to each other or approximately perpendicular to each other. The angle between the absorption axis of the polarizing member included in the display element 12 and the slow axis of the first phase difference member 20 is, for example, 40° to 50°, may be 42° to 48°, or may be about 45°. The angle between the absorption axis of the polarizing member included in the display element 12 and the slow axis of the second phase difference member 22 is, for example, 40° to 50°, may be 42° to 48°, or may be about 45°.

[0025] The in-plane retardation Re(550) of the first retardation member 20 is, for example, 100 nm to 190 nm, may be 110 nm to 180 nm, may be 130 nm to 160 nm, or may be 135 nm to 155 nm.

[0026] The first phase difference member 20 preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases according to the wavelength of the measurement light. The Re(450) / Re(550) of the first phase difference member 20 is, for example, 0.75 or more and less than 1, and may be 0.8 or more and 0.95 or less.

[0027] The in-plane retardation Re(550) of the second retardation member 22 is, for example, 100 nm to 190 nm, may be 110 nm to 180 nm, may be 130 nm to 160 nm, or may be 135 nm to 155 nm.

[0028] The second phase difference member 22 preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases according to the wavelength of the measurement light. Re(450) / Re(550) of the second phase difference member 22 is, for example, 0.75 or more and less than 1, and may be 0.8 or more and 0.95 or less.

[0029] Each retardation member is made of any appropriate material. For example, it may be a resin film (typically, a stretched film) or may be made of a liquid crystal compound. When the retardation member is a resin film, its thickness is, for example, 10 μm to 100 μm.

[0030] Examples of the resin contained in the resin film include polycarbonate-based resins, polyester carbonate-based resins, polyester-based resins, polyvinyl acetal-based resins, polyarylate-based resins, cyclic olefin-based resins, cellulose-based resins, polyvinyl alcohol-based resins, polyamide-based resins, polyimide-based resins, polyether-based resins, polystyrene-based resins, and acrylic-based resins. These resins may be used alone or in combination (for example, blended or copolymerized). For example, a resin film containing a polycarbonate-based resin or a polyester carbonate-based resin (hereinafter sometimes simply referred to as a polycarbonate-based resin) can be suitably used. By using such a resin, for example, the above-mentioned reverse dispersion wavelength characteristic can be exhibited.

[0031] Any suitable polycarbonate-based resin can be used as the polycarbonate-based resin. For example, the polycarbonate-based resin contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, and a structural unit derived from at least one dihydroxy compound selected from the group consisting of alicyclic diol, alicyclic dimethanol, di-, tri- or polyethylene glycol, and alkylene glycol or spiro glycol. Preferably, the polycarbonate-based resin contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, a structural unit derived from an alicyclic dimethanol and / or a structural unit derived from a di-, tri- or polyethylene glycol; more preferably, it contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, and a structural unit derived from a di-, tri- or polyethylene glycol. The polycarbonate-based resin may contain a structural unit derived from another dihydroxy compound as necessary. Details of polycarbonate-based resins that can be suitably used for phase difference members and methods for forming phase difference members are described, for example, in JP-A-2014-10291, JP-A-2014-26266, JP-A-2015-212816, JP-A-2015-212817, and JP-A-2015-212818, and the descriptions in these publications are incorporated herein by reference.

[0032] An absorptive polarizing member may be provided in front of the reflective polarizing member. Typically, the absorptive polarizing member may be provided between the reflective polarizing member and the second lens portion 24. The reflection axis of the reflective polarizing member and the absorption axis of the absorptive polarizing member may be arranged substantially parallel to each other, and the transmission axis of the reflective polarizing member and the transmission axis of the absorptive polarizing member may be arranged substantially parallel to each other. The absorptive polarizing member may be included in the reflecting portion 14. When the reflecting portion 14 includes an absorptive polarizing member, the reflecting portion 14 may include a laminate having a reflective polarizing member and an absorptive polarizing member.

[0033] FIG. 2 is a schematic cross-sectional view showing an example of a laminate used in the reflector of the display system shown in FIG. 1. The laminate 30 has a reflective polarizing member 32 and an absorptive polarizing member 34, and the reflective polarizing member 32 and the absorptive polarizing member 34 are laminated via an adhesive layer 36. By using the adhesive layer, the reflective polarizing member 32 and the absorptive polarizing member 34 are fixed, and it is possible to prevent the axial arrangement of the reflection axis and the absorption axis (the transmission axis and the transmission axis) from being misaligned. In addition, it is possible to suppress the adverse effect of an air layer that may be formed between the reflective polarizing member 32 and the absorptive polarizing member 34. The adhesive layer 36 may be formed of an adhesive or a pressure-sensitive adhesive. The thickness of the adhesive layer 36 is, for example, 0.05 μm to 30 μm, preferably 3 μm to 20 μm, and more preferably 5 μm to 15 μm. Although not shown, the second phase difference member 22 may be provided integrally with the reflective polarizing member 32, and therefore the laminate 30 may have the second phase difference member 22. In this case, the second phase difference member 22 can be laminated to the reflective polarizing member 32 via an adhesive layer.

[0034] The reflective polarizing element transmits polarized light (typically, linearly polarized light) parallel to its transmission axis while maintaining its polarization state, and can reflect light in other polarization states. The reflective polarizing element is typically composed of a film having a multilayer structure (sometimes referred to as a reflective polarizing film). In this case, the thickness of the reflective polarizing element is, for example, 10 μm to 150 μm, preferably 20 μm to 100 μm, and more preferably 30 μm to 60 μm.

[0035] FIG. 3 is a schematic perspective view showing an example of a multilayer structure included in a reflective polarizing film. The multilayer structure 32a has a layer A having birefringence and a layer B having substantially no birefringence alternately. The total number of layers constituting the multilayer structure may be 50 to 1000. For example, the refractive index nx in the x-axis direction of the A layer is larger than the refractive index ny in the y-axis direction, and the refractive index nx in the x-axis direction and the refractive index ny in the y-axis direction of the B layer are substantially the same, and the refractive index difference between the A layer and the B layer is large in the x-axis direction and substantially zero in the y-axis direction. As a result, the x-axis direction can be the reflection axis, and the y-axis direction can be the transmission axis. The refractive index difference between the A layer and the B layer in the x-axis direction is preferably 0.2 to 0.3.

[0036] The A layer is typically made of a material that develops birefringence through stretching. Examples of such materials include naphthalene dicarboxylic acid polyesters (e.g., polyethylene naphthalate), polycarbonates, and acrylic resins (e.g., polymethyl methacrylate). The B layer is typically made of a material that does not substantially develop birefringence even when stretched. Examples of such materials include copolyesters of naphthalene dicarboxylic acid and terephthalic acid. The multilayer structure can be formed by combining coextrusion and stretching. For example, the material constituting the A layer and the material constituting the B layer are extruded, and then multilayered (e.g., using a multiplier). The resulting multilayer laminate is then stretched. The x-axis direction in the illustrated example can correspond to the stretching direction.

[0037] Commercially available reflective polarizing films include, for example, products manufactured by 3M under the trade names "DBEF" and "APF" and products manufactured by Nitto Denko Corporation under the trade name "APCF."

[0038] The crossed transmittance (Tc) of the reflective polarizing member (reflective polarizing film) may be, for example, 0.01% to 3%. The single transmittance (Ts) of the reflective polarizing member (reflective polarizing film) may be, for example, 43% to 49%, and preferably 45% to 47%. The degree of polarization (P) of the reflective polarizing member (reflective polarizing film) may be, for example, 92% to 99.99%.

[0039] The single transmittance (Ts) is typically measured by an ultraviolet-visible spectrophotometer. The polarization degree (P) is typically measured by an ultraviolet-visible spectrophotometer and calculated by the following formula based on the parallel transmittance (Tp) and crossed transmittance (Tc) obtained by performing luminosity correction. Ts, Tp, and Tc are Y values ​​measured by a 2-degree visual field (C light source) according to JIS Z8701 and performing luminosity correction. Polarization degree (P)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0040] The absorptive polarizing member may typically include a resin film (sometimes referred to as an absorptive polarizing film or simply a polarizing film) containing a dichroic material. Preferably, it includes a polyvinyl alcohol (PVA)-based film containing iodine. The thickness of the absorptive polarizing film is preferably 1 μm or more and 8 μm or less, more preferably 7 μm or less, and even more preferably 5 μm or less. By using an absorptive polarizing film of such a thickness, it is possible to suppress shrinkage that may occur due to environmental changes (e.g., temperature changes) and maintain excellent display characteristics. Specifically, in the above display system, since slight shrinkage of a member can cause image distortion, by using an absorptive polarizing film of such a thickness, it is possible to extremely effectively suppress distortion of the displayed image.

[0041] The ratio of the thickness of the absorptive polarizing film to the thickness of the reflective polarizing member is preferably 15% or less, more preferably 10% or less. The ratio of the thickness of the absorptive polarizing film to the total thickness of the second retardation member, the reflective polarizing member, and the absorptive polarizing member is preferably 10% or less, more preferably 5% or less.

[0042] The crossed transmittance (Tc) of the absorptive polarizing member (absorptive polarizing film) is preferably 0.5% or less, more preferably 0.1% or less, and further preferably 0.05% or less. The single transmittance (Ts) of the absorptive polarizing member (absorptive polarizing film) is, for example, 41.0% to 45.0%, and preferably 42.0% or more. The polarization degree (P) of the absorptive polarizing member (absorptive polarizing film) is, for example, 99.0% to 99.997%, and preferably 99.9% or more. By combining the reflective polarizing member with the absorptive polarizing member, excellent display characteristics can be achieved. For example, the user's perception of an afterimage (ghost) can be suppressed.

[0043] A method for producing the absorptive polarizing film according to one embodiment includes forming a polyvinyl alcohol-based resin layer (PVA-based resin layer) containing a halide and a polyvinyl alcohol-based resin (PVA-based resin) on one side of a long thermoplastic resin substrate to form a laminate, and subjecting the laminate to an auxiliary air-stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order, in which the laminate is heated while being transported in the longitudinal direction to shrink the laminate by 2% or more in the width direction. The content of the halide in the PVA-based resin layer is preferably 5 parts by weight to 20 parts by weight with respect to 100 parts by weight of the PVA-based resin. The stretching ratio in the auxiliary air-stretching treatment is preferably 2.0 times or more. The drying shrinkage treatment is preferably performed using a heating roll, and the temperature of the heating roll is preferably 60° C. to 120° C. The shrinkage rate in the width direction of the laminate due to the drying shrinkage treatment is preferably 2% or more. A laminate including a PVA-based resin layer containing a halide is prepared, the laminate is stretched in multiple stages including auxiliary air stretching and underwater stretching, and the stretched laminate is heated with a heating roll to obtain a polarizing film having excellent optical properties (typically, single transmittance and polarization degree) and suppressed variations in optical properties. Specifically, by using a heating roll in the drying shrinkage treatment step, the laminate can be uniformly shrunk over the entire laminate while being transported. This not only improves the optical properties of the obtained polarizing film, but also allows stable production of polarizing films with excellent optical properties and suppresses variations in the optical properties (particularly, single transmittance) of the polarizing film.

[0044] Any suitable method can be adopted as a method for producing a laminate of a thermoplastic resin substrate and a PVA-based resin layer. Preferably, a coating liquid containing a halide and a PVA-based resin is applied to the surface of the thermoplastic resin substrate, and then dried to form a PVA-based resin layer on the thermoplastic resin substrate. As described above, the content of the halide in the PVA-based resin layer is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA-based resin.

[0045] Any appropriate method can be used as the coating method of the coating liquid. For example, roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, knife coating (comma coating, etc.), etc. are listed. The coating and drying temperature of the coating liquid is preferably 50° C. or higher.

[0046] The thickness of the PVA-based resin layer is preferably 3 μm to 40 μm, and more preferably 3 μm to 20 μm.

[0047] Before forming the PVA-based resin layer, the thermoplastic resin substrate may be subjected to a surface treatment (e.g., corona treatment, etc.), or an easy-adhesion layer may be formed on the thermoplastic resin substrate. By carrying out such treatment, the adhesion between the thermoplastic resin substrate and the PVA-based resin layer can be improved.

[0048] The thickness of the thermoplastic resin substrate is preferably 20 μm to 300 μm, more preferably 50 μm to 200 μm. If it is less than 20 μm, it may be difficult to form a PVA-based resin layer. If it exceeds 300 μm, for example, in the underwater stretching treatment described below, it may take a long time for the thermoplastic resin substrate to absorb water, and an excessive load may be required for stretching.

[0049] The thermoplastic resin substrate preferably has a water absorption rate of 0.2% or more, more preferably 0.3% or more. The thermoplastic resin substrate can absorb water, and the water can act as a plasticizer to plasticize the substrate. As a result, the stretching stress can be significantly reduced, and the substrate can be stretched at a high ratio. On the other hand, the water absorption rate of the thermoplastic resin substrate is preferably 3.0% or less, more preferably 1.0% or less. By using such a thermoplastic resin substrate, it is possible to prevent problems such as a significant decrease in the dimensional stability of the thermoplastic resin substrate during production, which leads to a deterioration in the appearance of the resulting polarizing film. It is also possible to prevent the substrate from breaking during underwater stretching, and the PVA-based resin layer from peeling off from the thermoplastic resin substrate. The water absorption rate of the thermoplastic resin substrate can be adjusted, for example, by introducing a modifying group into the constituent material. The water absorption rate is a value determined in accordance with JIS K 7209.

[0050] The glass transition temperature (Tg) of the thermoplastic resin substrate is preferably 120°C or lower. By using such a thermoplastic resin substrate, the stretchability of the laminate can be sufficiently ensured while suppressing the crystallization of the PVA-based resin layer. Furthermore, in consideration of the plasticization of the thermoplastic resin substrate by water and the underwater stretching, it is more preferable that the temperature is 100°C or lower, and further 90°C or lower. On the other hand, the glass transition temperature of the thermoplastic resin substrate is preferably 60°C or higher. By using such a thermoplastic resin substrate, defects such as deformation of the thermoplastic resin substrate (e.g., generation of unevenness, sagging, wrinkles, etc.) during the application and drying of the coating liquid containing the PVA-based resin can be prevented, and a laminate can be produced satisfactorily. In addition, the stretching of the PVA-based resin layer can be satisfactorily performed at a suitable temperature (e.g., about 60°C). The glass transition temperature of the thermoplastic resin substrate can be adjusted, for example, by introducing a modifying group into the constituent material and heating using a crystallizing material. The glass transition temperature (Tg) is a value obtained in accordance with JIS K 7121.

[0051] Any suitable thermoplastic resin may be used as the material for the thermoplastic resin substrate. Examples of the thermoplastic resin include ester resins such as polyethylene terephthalate resins, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, polyamide resins, polycarbonate resins, and copolymer resins thereof. Among these, norbornene resins and amorphous polyethylene terephthalate resins are preferred.

[0052] In one embodiment, amorphous (uncrystallized) polyethylene terephthalate resins are preferably used. Among them, amorphous (hard to crystallize) polyethylene terephthalate resins are particularly preferably used. Specific examples of amorphous polyethylene terephthalate resins include copolymers further containing isophthalic acid and / or cyclohexanedicarboxylic acid as dicarboxylic acids, and copolymers further containing cyclohexanedimethanol or diethylene glycol as glycols.

[0053] In a preferred embodiment, the thermoplastic resin substrate is made of a polyethylene terephthalate resin having an isophthalic acid unit. This is because such a thermoplastic resin substrate has excellent stretchability and can suppress crystallization during stretching. This is believed to be due to the introduction of an isophthalic acid unit to impart a large bend to the main chain. The polyethylene terephthalate resin has a terephthalic acid unit and an ethylene glycol unit. The content ratio of the isophthalic acid unit is preferably 0.1 mol% or more, more preferably 1.0 mol% or more, based on the total of all repeating units. This is because a thermoplastic resin substrate with extremely excellent stretchability can be obtained. On the other hand, the content ratio of the isophthalic acid unit is preferably 20 mol% or less, more preferably 10 mol% or less, based on the total of all repeating units. By setting such a content ratio, the crystallinity can be favorably increased in the drying shrinkage treatment described below.

[0054] The thermoplastic resin substrate may be stretched in advance (before the PVA-based resin layer is formed). In one embodiment, the long thermoplastic resin substrate is stretched in the transverse direction. The transverse direction is preferably a direction perpendicular to the stretching direction of the laminate described below. In this specification, "perpendicular" also includes the case where the direction is substantially perpendicular. Here, "substantially perpendicular" includes the case where the direction is 90°±5.0°, preferably 90°±3.0°, and more preferably 90°±1.0°.

[0055] The stretching temperature of the thermoplastic resin substrate is preferably from the glass transition temperature (Tg) of Tg-10° C. to Tg+50° C. The stretching ratio of the thermoplastic resin substrate is preferably from 1.5 times to 3.0 times.

[0056] Any appropriate method may be adopted as the stretching method of the thermoplastic resin substrate. Specifically, it may be fixed end stretching or free end stretching. The stretching method may be dry or wet. The stretching of the thermoplastic resin substrate may be performed in one stage or multiple stages. When it is performed in multiple stages, the above-mentioned stretching ratio is the product of the stretching ratios of each stage.

[0057] The coating liquid contains a halide and a PVA resin as described above. The coating liquid is typically a solution in which the halide and the PVA resin are dissolved in a solvent. Examples of the solvent include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyhydric alcohols such as trimethylolpropane, and amines such as ethylenediamine and diethylenetriamine. These can be used alone or in combination of two or more. Among these, water is preferred. The concentration of the PVA resin in the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. With such a resin concentration, a uniform coating film that is in close contact with the thermoplastic resin substrate can be formed. The content of the halide in the coating liquid is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA resin.

[0058] Additives may be added to the coating liquid. Examples of additives include plasticizers and surfactants. Examples of plasticizers include polyhydric alcohols such as ethylene glycol and glycerin. Examples of surfactants include nonionic surfactants. These can be used to further improve the uniformity, dyeability, and stretchability of the resulting PVA-based resin layer.

[0059] Any suitable resin can be used as the PVA resin. Examples include polyvinyl alcohol and ethylene-vinyl alcohol copolymer. Polyvinyl alcohol is obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymer is obtained by saponifying ethylene-vinyl acetate copolymer. The saponification degree of the PVA resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, and more preferably 99.0 mol% to 99.93 mol%. The saponification degree can be determined in accordance with JIS K 6726-1994. By using a PVA resin with such a saponification degree, a polarizing film with excellent durability can be obtained. If the saponification degree is too high, gelation may occur.

[0060] The average degree of polymerization of the PVA resin can be appropriately selected depending on the purpose. The average degree of polymerization is usually 1000 to 10000, preferably 1200 to 4500, and more preferably 1500 to 4300. The average degree of polymerization can be determined in accordance with JIS K 6726-1994.

[0061] Any suitable halide may be used as the halide. For example, iodide and sodium chloride may be used. For example, iodide may be potassium iodide, sodium iodide, and lithium iodide. Among these, potassium iodide is preferred.

[0062] The amount of the halide in the coating solution is preferably 5 to 20 parts by weight per 100 parts by weight of the PVA-based resin, and more preferably 10 to 15 parts by weight per 100 parts by weight of the PVA-based resin. If the amount of the halide exceeds 20 parts by weight per 100 parts by weight of the PVA-based resin, the halide may bleed out, causing the final polarizing film to become cloudy.

[0063] Generally, the orientation of polyvinyl alcohol molecules in the PVA-based resin increases when the PVA-based resin layer is stretched, but when the stretched PVA-based resin layer is immersed in a liquid containing water, the orientation of the polyvinyl alcohol molecules may become disordered, and the orientation may decrease. In particular, when a laminate of a thermoplastic resin and a PVA-based resin layer is stretched in boric acid water, the tendency of the orientation degree to decrease is remarkable when the laminate is stretched in boric acid water at a relatively high temperature to stabilize the stretching of the thermoplastic resin. For example, the stretching of a PVA film alone in boric acid water is generally performed at 60°C, whereas the stretching of a laminate of A-PET (thermoplastic resin substrate) and a PVA-based resin layer is performed at a high temperature of about 70°C, and in this case, the orientation of PVA at the initial stage of stretching may decrease before it increases due to underwater stretching. In response to this, a laminate of a PVA-based resin layer containing a halide and a thermoplastic resin substrate is prepared, and the laminate is stretched at high temperature (auxiliary stretching) in air before being stretched in boric acid water, so that the crystallization of the PVA-based resin in the PVA-based resin layer of the laminate after the auxiliary stretching can be promoted. As a result, when the PVA-based resin layer is immersed in a liquid, the orientation of the polyvinyl alcohol molecules is disturbed and the orientation is reduced, compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of the polarizing film obtained through a process in which the laminate is immersed in a liquid, such as a dyeing process and an underwater stretching process.

[0064] In particular, in order to obtain high optical properties, a two-stage stretching method is selected, which combines dry stretching (auxiliary stretching) and stretching in boric acid water. By introducing auxiliary stretching like two-stage stretching, it is possible to stretch while suppressing the crystallization of the thermoplastic resin substrate, which solves the problem of the thermoplastic resin substrate being excessively crystallized and reduced in stretchability in the subsequent stretching in boric acid water, and the laminate can be stretched at a higher magnification. Furthermore, when applying a PVA-based resin onto a thermoplastic resin substrate, in order to suppress the influence of the glass transition temperature of the thermoplastic resin substrate, it is necessary to lower the application temperature compared to when applying a PVA-based resin onto a normal metal drum, which may result in a problem that the crystallization of the PVA-based resin is relatively low and sufficient optical properties cannot be obtained. In contrast, by introducing auxiliary stretching, it is possible to increase the crystallinity of the PVA-based resin even when applying a PVA-based resin onto a thermoplastic resin, and it is possible to achieve high optical properties. At the same time, by increasing the orientation of the PVA-based resin in advance, problems such as a decrease in the orientation of the PVA-based resin or dissolution when the resin is immersed in water in the subsequent dyeing and stretching processes can be prevented, making it possible to achieve high optical properties.

[0065] The stretching method of the auxiliary air stretching may be fixed end stretching (for example, a method of stretching using a tenter stretching machine) or free end stretching (for example, a method of uniaxially stretching the laminate by passing it between rolls with different peripheral speeds), but in order to obtain high optical properties, free end stretching may be actively adopted. In one embodiment, the air stretching process includes a heated roll stretching step in which the laminate is stretched by the difference in peripheral speed between heated rolls while being transported in its longitudinal direction. The air stretching process typically includes a zone stretching step and a heated roll stretching step. The order of the zone stretching step and the heated roll stretching step is not limited, and the zone stretching step may be performed first, or the heated roll stretching step may be performed first. The zone stretching step may be omitted. In one embodiment, the zone stretching step and the heated roll stretching step are performed in this order. In another embodiment, the film is stretched in a tenter stretching machine by gripping the film ends and widening the distance between the tenters in the machine direction (the increase in the distance between the tenters is the stretching ratio). At this time, the distance between the tenters in the width direction (perpendicular to the machine direction) is set to be arbitrarily close. Preferably, it can be set to be closer to the free end stretching ratio than the machine direction stretching ratio. In the case of free end stretching, the shrinkage ratio in the width direction = (1 / stretching ratio) 1 / 2 It is calculated as follows.

[0066] The auxiliary air-drawing may be performed in one step or in multiple steps. When the auxiliary air-drawing is performed in multiple steps, the draw ratio is the product of the draw ratios in each step. The draw direction in the auxiliary air-drawing is preferably approximately the same as the draw direction in the underwater drawing.

[0067] The stretching ratio in the auxiliary air-stretching is preferably 2.0 to 3.5 times. The maximum stretching ratio in the case of combining the auxiliary air-stretching and the underwater stretching is preferably 5.0 times or more, more preferably 5.5 times or more, and even more preferably 6.0 times or more, based on the original length of the laminate. In this specification, the "maximum stretching ratio" refers to the stretching ratio just before the laminate breaks, and refers to a value 0.2 lower than the stretching ratio at which the laminate breaks, which is determined separately.

[0068] The stretching temperature of the auxiliary air stretching can be set to any appropriate value depending on the material of the thermoplastic resin substrate, the stretching method, etc. The stretching temperature is preferably equal to or higher than the glass transition temperature (Tg) of the thermoplastic resin substrate, more preferably equal to or higher than the glass transition temperature (Tg) of the thermoplastic resin substrate + 10°C, and particularly preferably equal to or higher than Tg + 15°C. On the other hand, the upper limit of the stretching temperature is preferably 170°C. By stretching at such a temperature, the crystallization of the PVA resin can be suppressed from progressing rapidly, and defects due to the crystallization (for example, the orientation of the PVA resin layer due to stretching can be suppressed). The crystallization index of the PVA resin after the auxiliary air stretching is preferably 1.3 to 1.8, more preferably 1.4 to 1.7. The crystallization index of the PVA resin can be measured by the ATR method using a Fourier transform infrared spectrophotometer. Specifically, the measurement is performed using polarized light as the measurement light, and the crystallization index at 1141 cm of the obtained spectrum is suppressed. -1 and 1440cm -1 The crystallization index is calculated according to the following formula using the intensity of Crystallization index=(I C / I R ) however, I C : 1141cm when measuring with incident measuring light -1 Intensity I R : 1440cm when measuring with incident measuring light -1 Intensity It is.

[0069] If necessary, an insolubilization treatment is carried out after the auxiliary air stretching treatment and before the underwater stretching treatment or the dyeing treatment. The insolubilization treatment is typically carried out by immersing the PVA-based resin layer in an aqueous boric acid solution. By carrying out the insolubilization treatment, water resistance is imparted to the PVA-based resin layer, and it is possible to prevent a decrease in the orientation of PVA when immersed in water. The concentration of the aqueous boric acid solution is preferably 1 part by weight to 4 parts by weight with respect to 100 parts by weight of water. The liquid temperature of the insolubilization bath (aqueous boric acid solution) is preferably 20°C to 50°C.

[0070] The dyeing treatment is typically performed by dyeing the PVA-based resin layer with iodine. Specifically, the dyeing treatment is performed by adsorbing iodine to the PVA-based resin layer. Examples of the adsorption method include a method of immersing the PVA-based resin layer (laminate) in a dyeing solution containing iodine, a method of applying the dyeing solution to the PVA-based resin layer, and a method of spraying the dyeing solution onto the PVA-based resin layer. A preferred method is a method of immersing the laminate in a dyeing solution (dye bath), because iodine can be well adsorbed.

[0071] The dyeing solution is preferably an aqueous iodine solution. The amount of iodine to be mixed is preferably 0.05 to 0.5 parts by weight relative to 100 parts by weight of water. In order to increase the solubility of iodine in water, it is preferable to mix an iodide in the aqueous iodine solution. Examples of iodides include potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, and titanium iodide. Among these, potassium iodide is preferable. The amount of iodide to be mixed is preferably 0.1 to 10 parts by weight, more preferably 0.3 to 5 parts by weight, relative to 100 parts by weight of water. The temperature of the dyeing solution during dyeing is preferably 20°C to 50°C in order to suppress dissolution of the PVA resin. When the PVA-based resin layer is immersed in the dye solution, the immersion time is preferably 5 seconds to 5 minutes, and more preferably 30 seconds to 90 seconds, in order to ensure the transmittance of the PVA-based resin layer.

[0072] The dyeing conditions (concentration, liquid temperature, immersion time) can be set so that the single transmittance and polarization degree of the finally obtained polarizing film are within the above-mentioned ranges. As such dyeing conditions, preferably, an iodine aqueous solution is used as the dyeing solution, and the content ratio of iodine and potassium iodide in the iodine aqueous solution is 1:5 to 1:20. The content ratio of iodine and potassium iodide in the iodine aqueous solution is preferably 1:5 to 1:10. This makes it possible to obtain a polarizing film having the above-mentioned optical properties.

[0073] When a dyeing process is performed continuously after a process (typically, an insolubilization process) in which the laminate is immersed in a treatment bath containing boric acid, the boric acid concentration of the dyeing bath may change over time due to the boric acid contained in the treatment bath being mixed into the dyeing bath, resulting in unstable dyeability. In order to suppress the above-mentioned instability of dyeability, the upper limit of the boric acid concentration of the dyeing bath is adjusted to be preferably 4 parts by weight, more preferably 2 parts by weight, relative to 100 parts by weight of water. On the other hand, the lower limit of the boric acid concentration of the dyeing bath is preferably 0.1 parts by weight, more preferably 0.2 parts by weight, and even more preferably 0.5 parts by weight, relative to 100 parts by weight of water. In one embodiment, the dyeing process is performed using a dyeing bath in which boric acid has been blended in advance. This can reduce the rate of change in the boric acid concentration when the boric acid of the treatment bath is mixed into the dyeing bath. The amount of boric acid preliminarily mixed into the dye bath (i.e., the content of boric acid not derived from the treatment bath) is preferably 0.1 to 2 parts by weight, and more preferably 0.5 to 1.5 parts by weight, per 100 parts by weight of water.

[0074] If necessary, a crosslinking treatment is carried out after the dyeing treatment and before the underwater stretching treatment. The crosslinking treatment is typically carried out by immersing the PVA-based resin layer in an aqueous boric acid solution. The crosslinking treatment imparts water resistance to the PVA-based resin layer, and prevents the orientation of the PVA from decreasing when the layer is immersed in high-temperature water in the subsequent underwater stretching. The concentration of the aqueous boric acid solution is preferably 1 to 5 parts by weight per 100 parts by weight of water. In addition, when the crosslinking treatment is carried out after the dyeing treatment, it is preferable to further add an iodide. By adding an iodide, it is possible to suppress the elution of iodine adsorbed to the PVA-based resin layer. The amount of the iodide to be added is preferably 1 to 5 parts by weight per 100 parts by weight of water. Specific examples of the iodide are as described above. The liquid temperature of the crosslinking bath (aqueous boric acid solution) is preferably 20°C to 50°C.

[0075] The underwater stretching treatment is performed by immersing the laminate in a stretching bath. The underwater stretching treatment allows stretching at a temperature lower than the glass transition temperature (typically about 80° C.) of the thermoplastic resin substrate or the PVA-based resin layer, and allows the PVA-based resin layer to be stretched at a high magnification while suppressing crystallization. As a result, a polarizing film having excellent optical properties can be produced.

[0076] The stretching method of the laminate can be any appropriate method. Specifically, it may be fixed end stretching or free end stretching (for example, a method of uniaxially stretching the laminate by passing it between rolls having different peripheral speeds). Preferably, free end stretching is selected. The stretching of the laminate may be performed in one stage or multiple stages. When performing the stretching in multiple stages, the stretching ratio (maximum stretching ratio) of the laminate described below is the product of the stretching ratios in each stage.

[0077] The underwater stretching is preferably performed by immersing the laminate in an aqueous solution of boric acid (stretching in boric acid water). By using an aqueous solution of boric acid as a stretching bath, it is possible to impart to the PVA-based resin layer rigidity that can withstand the tension applied during stretching and water resistance that does not dissolve in water. Specifically, boric acid can generate tetrahydroxyborate anions in the aqueous solution and crosslink with the PVA-based resin through hydrogen bonds. As a result, it is possible to impart rigidity and water resistance to the PVA-based resin layer and stretch it well, and a polarizing film having excellent optical properties can be produced.

[0078] The boric acid aqueous solution is preferably obtained by dissolving boric acid and / or a borate in water as a solvent. The boric acid concentration is preferably 1 to 10 parts by weight, more preferably 3.5 to 7 parts by weight, and particularly preferably 4 to 6 parts by weight, relative to 100 parts by weight of water. By setting the boric acid concentration to 1 part by weight or more, dissolution of the PVA-based resin layer can be effectively suppressed, and a polarizing film with higher characteristics can be produced. In addition to boric acid or a borate, an aqueous solution obtained by dissolving a boron compound such as borax, glyoxal, glutaraldehyde, or the like in a solvent can also be used.

[0079] Preferably, an iodide is added to the stretching bath (boric acid aqueous solution). By adding an iodide, it is possible to suppress the elution of iodine adsorbed in the PVA resin layer. Specific examples of the iodide are as described above. The concentration of the iodide is preferably 0.05 to 15 parts by weight, more preferably 0.5 to 8 parts by weight, relative to 100 parts by weight of water.

[0080] The stretching temperature (liquid temperature of the stretching bath) is preferably 40°C to 85°C, more preferably 60°C to 75°C. At such a temperature, the laminate can be stretched at a high ratio while suppressing dissolution of the PVA-based resin layer. Specifically, as described above, the glass transition temperature (Tg) of the thermoplastic resin substrate is preferably 60°C or higher in relation to the formation of the PVA-based resin layer. In this case, if the stretching temperature is lower than 40°C, there is a risk that the substrate cannot be stretched well even when the plasticization of the thermoplastic resin substrate by water is taken into consideration. On the other hand, the higher the temperature of the stretching bath, the higher the solubility of the PVA-based resin layer, and there is a risk that excellent optical properties cannot be obtained. The immersion time of the laminate in the stretching bath is preferably 15 seconds to 5 minutes.

[0081] The stretching ratio in the underwater stretching is preferably 1.5 times or more, more preferably 3.0 times or more. The total stretching ratio of the laminate is preferably 5.0 times or more, more preferably 5.5 times or more, based on the original length of the laminate. By achieving such a high stretching ratio, a polarizing film with extremely excellent optical properties can be produced. Such a high stretching ratio can be achieved by employing an underwater stretching method (stretching in boric acid water).

[0082] The drying shrinkage treatment may be performed by zone heating, which heats the entire zone, or by heating the transport roll (using a so-called heating roll) (heat roll drying method). Preferably, both are used. By drying using a heating roll, it is possible to efficiently suppress the heat curl of the laminate and produce a polarizing film with excellent appearance. Specifically, by drying the laminate in a state where it is aligned with the heating roll, it is possible to efficiently promote the crystallization of the thermoplastic resin substrate and increase the crystallinity, and even at a relatively low drying temperature, it is possible to satisfactorily increase the crystallinity of the thermoplastic resin substrate. As a result, the rigidity of the thermoplastic resin substrate increases and it becomes in a state where it can withstand the shrinkage of the PVA-based resin layer due to drying, and curling is suppressed. In addition, by using a heating roll, it is possible to dry the laminate while maintaining it in a flat state, so that it is possible to suppress not only curling but also wrinkles. At this time, the optical properties of the laminate can be improved by shrinking it in the width direction by the drying shrinkage treatment. This is because the orientation of the PVA and the PVA / iodine complex can be effectively increased. The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment is preferably 1% to 10%, more preferably 2% to 8%, and particularly preferably 4% to 6%. By using a heating roll, the laminate can be continuously shrunk in the width direction while being transported, thereby achieving high productivity.

[0083] 4 is a schematic diagram showing an example of the drying shrinkage treatment. In the drying shrinkage treatment, the laminate 200 is dried while being transported by transport rolls R1 to R6 heated to a predetermined temperature and guide rolls G1 to G4. In the illustrated example, the transport rolls R1 to R6 are arranged so as to alternately and continuously heat the surface of the PVA resin layer and the surface of the thermoplastic resin substrate, but, for example, the transport rolls R1 to R6 may be arranged so as to continuously heat only one surface of the laminate 200 (for example, the thermoplastic resin substrate surface).

[0084] Drying conditions can be controlled by adjusting the heating temperature of the transport rolls (temperature of the heating rolls), the number of heating rolls, the contact time with the heating rolls, etc. The temperature of the heating rolls is preferably 60°C to 120°C, more preferably 65°C to 100°C, and particularly preferably 70°C to 80°C. The crystallinity of the thermoplastic resin can be favorably increased, curling can be favorably suppressed, and the laminate can be given extremely excellent durability. The temperature of the heating rolls can be measured by a contact thermometer. In the illustrated example, six transport rolls are provided, but there is no particular restriction as long as there are multiple transport rolls. The number of transport rolls is usually 2 to 40, preferably 4 to 30. The contact time (total contact time) between the laminate and the heating rolls is preferably 1 to 300 seconds, more preferably 1 to 20 seconds, and even more preferably 1 to 10 seconds.

[0085] The heating roll may be provided in a heating furnace (for example, an oven) or in a normal production line (under room temperature environment). It is preferably provided in a heating furnace equipped with a blowing means. By using drying with a heating roll in combination with hot air drying, it is possible to suppress abrupt temperature changes between the heating rolls, and it is possible to easily control shrinkage in the width direction. The hot air drying temperature is preferably 30°C to 100°C. The hot air drying time is preferably 1 second to 300 seconds. The hot air speed is preferably about 10 m / s to 30 m / s. The wind speed is the wind speed in the heating furnace, and can be measured by a mini-vane type digital anemometer.

[0086] Preferably, after the underwater stretching treatment and before the drying shrinkage treatment, a washing treatment is carried out. The washing treatment is typically carried out by immersing the PVA-based resin layer in an aqueous potassium iodide solution. EXAMPLES

[0087] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The thicknesses are values ​​measured by the following measuring method. <Thickness> The thickness of 10 μm or less was measured using a scanning electron microscope (manufactured by JEOL, product name "JSM-7100F"), and the thickness of more than 10 μm was measured using a digital micrometer (manufactured by Anritsu, product name "KC-351C").

[0088] [Example 1] The thermoplastic resin substrate was a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a water absorption rate of 0.75% and a Tg of about 75° C. One side of the resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating liquid) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin made by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Mitsubishi Chemical Corporation, product name "GOHSENEX Z410") in a ratio of 9:1, and dissolving the mixture in water. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched at its free end to 2.4 times its original size in the machine direction (longitudinal direction) between rolls with different peripheral speeds in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the final polarizing film would be 43.0% (dyeing process). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4% by weight, potassium iodide concentration: 5% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, while drying in an oven maintained at 90°C, the laminate was brought into contact with a SUS heated roll whose surface temperature was maintained at 75°C for approximately 2 seconds (drying shrinkage treatment). The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment was 5.2%. In this manner, a polarizing film (absorption type polarizing film) having a thickness of 5 μm was formed on the resin substrate.

[0089] A cycloolefin resin film having a thickness of 25 μm was attached as a protective layer to the surface of the obtained polarizing film (the surface of the laminate on the polarizing film side) via an ultraviolet-curing adhesive. Specifically, the adhesive was applied so that the thickness of the adhesive layer after curing was about 1 μm, and the two films were attached using a rolling machine. Thereafter, the adhesive was cured by irradiating it with UV light from the cycloolefin resin film side. Next, the resin substrate was peeled off to obtain a polarizing film (absorption type polarizing film) having a configuration of cycloolefin resin film / absorption type polarizing film.

[0090] [Example 2] A polarizing film including a polarizing membrane having a thickness of 7 μm was obtained in the same manner as in Example 1, except that a PVA-based resin layer having a thickness of 18 μm was formed on the resin substrate.

[0091] [Comparative Example 1] A long roll of a 30 μm-thick polyvinyl alcohol (PVA) resin film (manufactured by Kuraray, product name "PE3000") was uniaxially stretched in the longitudinal direction to 5.9 times its original size using a roll stretching machine while simultaneously undergoing swelling, dyeing, crosslinking, and washing treatments in that order, and finally a drying treatment to produce a 12 μm-thick polarizing film (absorptive polarizing film). The above swelling treatment was performed by stretching the film 2.2 times while treating with pure water at 20°C. Next, the dyeing treatment was performed by stretching the film 1.4 times while treating it in an aqueous solution at 30°C in which the weight ratio of iodine to potassium iodide was 1:7, and the iodine concentration was adjusted so that the single transmittance of the resulting polarizing film was 45.0%. Next, the crosslinking treatment was performed in two stages, and the first stage was stretched 1.2 times while treating it in an aqueous solution at 40°C in which boric acid and potassium iodide were dissolved. The aqueous solution for the first stage crosslinking treatment had a boric acid content of 5.0% by weight and a potassium iodide content of 3.0% by weight. The second stage was stretched 1.6 times while treating it in an aqueous solution at 65°C in which boric acid and potassium iodide were dissolved. The aqueous solution for the second stage crosslinking treatment had a boric acid content of 4.3% by weight and a potassium iodide content of 5.0% by weight. Next, the film was washed with an aqueous potassium iodide solution at 20° C. The aqueous solution used for the washing treatment had a potassium iodide content of 2.6% by weight. Finally, the film was dried at 70° C. for 5 minutes to obtain a polarizing film.

[0092] A cycloolefin resin film having a thickness of 25 μm was attached as a protective layer to the obtained polarizing film using a 3% aqueous solution of a PVA adhesive (manufactured by Mitsubishi Chemical Corporation, product name "GOHSENOL Z200") to obtain a polarizing film.

[0093] [Comparative Example 2] A polarizing film including a polarizing membrane having a thickness of 17 μm was obtained in the same manner as in Comparative Example 1, except that a PVA-based resin film having a thickness of 45 μm was used.

[0094] [Comparative Example 3] A polarizing film including a polarizing membrane having a thickness of 23 μm was obtained in the same manner as in Comparative Example 1, except that a PVA-based resin film having a thickness of 60 μm was used.

[0095] [Comparative Example 4] A polarizing film including a polarizing membrane having a thickness of 30 μm was obtained in the same manner as in Comparative Example 1, except that a PVA-based resin film having a thickness of 75 μm was used.

[0096] The following evaluations were carried out for the Examples and Comparative Examples. The evaluation results are summarized in Table 1. <Evaluation> 1. Dimensional change rate (%) From the obtained polarizing film, test pieces of 100 mm x 100 mm in size were cut out along the stretching direction and the direction perpendicular thereto, and were attached to a glass plate via a 20 μm thick acrylic adhesive layer. This was heated in an oven at 80° C. for 500 hours, and the size before and after heating was measured, and the dimensional change rate before and after heating was calculated. 2. Contraction stress (N / 4mm) From the obtained polarizing film (before laminating the protective film), test pieces with a size of 20 mm x 4 mm were cut out along the stretching direction and the direction perpendicular thereto, and were set in a TMA analyzer (Hitachi High-Tech Science Corporation, "TMA7100E") While maintaining this state, the specimen was heated at 50°C for 30 minutes, and the shrinkage stress generated by the specimen was measured. 3. Optical Unevenness The obtained polarizing film was cut into a size of 200 mm x 150 mm, and attached to a glass plate via a 20 μm acrylic adhesive layer to obtain a sample, which was then placed in a heating tester at 80° C. for 120 hours. After that, another standard polarizing plate (manufactured by Nitto Denko Corporation, "CRT1794") was placed on the removed sample so that their absorption axes were perpendicular to each other, and this was placed on a backlight, and in this state, in-plane unevenness was confirmed.

[0097] [Table 1]

[0098] In the comparative example, optical unevenness (particularly at the corners) was observed as shown in FIG.

[0099] The present invention is not limited to the above-described embodiment, and various modifications are possible. For example, the above-described embodiment may be replaced with a configuration that is substantially the same as the configuration shown in the above-described embodiment, a configuration that provides the same action and effect, or a configuration that can achieve the same purpose. [Industrial Applicability]

[0100] The lens portion according to the embodiment of the present invention can be used in a display such as VR goggles. [Explanation of symbols]

[0101] 2. Display System 4 Lens section 12 Display element 14 Reflector 16 First lens section 18 Half Mirror 20 First phase difference member 22 Second phase difference member 24 Second lens section 30 Laminate 32 Reflective polarizing element 34 Absorption type polarizing element 36 Adhesive layer

Claims

1. An optical member set including a polarizing member, a first λ / 4 member, a second λ / 4 member, a reflective polarizing member, and an absorptive polarizing member, The optical members included in the optical member set are arranged such that light emitted forward from a display element passes through the polarizing member and the first λ / 4 member, is reflected by the reflective polarizing member, passes through the second λ / 4 member, is reflected forward, and passes through the reflective polarizing member and the absorptive polarizing member; The thickness of the absorptive polarizing film constituting the absorptive polarizing member is 8 μm or less. Optical component set.

2. The optical member set according to claim 1 , wherein a reflection axis of the reflective polarizing member and an absorption axis of the absorptive polarizing member are arranged parallel to each other.

3. The polarizing member, the first λ / 4 member, and the second λ / 4 member are arranged such that an angle between the absorption axis of the polarizing member and the slow axis of the first λ / 4 member is 40° to 50°, and an angle between the absorption axis of the polarizing member and the slow axis of the second λ / 4 member is 40° to 50°. The optical member set according to claim 1.

4. 2. The optical member set according to claim 1, wherein a ratio of a thickness of the absorptive polarizing film to a thickness of the reflective polarizing member is 15% or less.

5. The optical member set according to any one of claims 1 to 4, A laminate having the reflective polarizing member and the absorptive polarizing member. The laminate for an optical member set.

6. The laminate for an optical member set according to claim 5 , wherein the reflective polarizing member and the absorptive polarizing member are laminated via an adhesive layer.

Citation Information

Patent Citations

  • Optical module and head-mounted display device

    CN113448101A

  • Video display device

    JP2002107655A

  • Liquid crystal display device

    JP2006251095A

  • Polarizer, polarization plate, optical film and image display apparatus

    JP2008102274A

  • Set of polarizing plates for IPS mode and IPS mode liquid crystal display using the same

    JP2018060151A