Glass for medicine container, and glass tube for medicine container and medicine container using the same

A glass composition with controlled components and molar ratios addresses the challenge of achieving both hydrolysis resistance and processability in pharmaceutical containers, ensuring reduced delamination and contamination, suitable for pharmaceutical containers.

JP2024133712AActive Publication Date: 2024-10-02NIPPON ELECTRIC GLASS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024112254
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-08-13
Filing Date
2024-07-12
Publication Date
2024-10-02
Estimated Expiration
2040-01-20

AI Technical Summary

Technical Problem

Existing glass for pharmaceutical containers face challenges in achieving both excellent hydrolysis resistance and processability, with borosilicate glass formulations compromising on hydrolysis resistance when viscosity is reduced to improve processability, leading to issues like delamination and contamination during processing.

Method used

A glass composition with controlled components, including specific ratios of SiO2, Al2O3, B2O3, Li2O, Na2O, K2O, and limited amounts of MgO, CaO, SrO, and BaO, ensuring both hydrolysis resistance and processability by regulating molar ratios such as K2O/(Li2O+Na2O+K2O) and Al2O3/(Li2O+Na2O+K2O) to minimize delamination and evaporation of glass components during processing.

Benefits of technology

The proposed glass composition achieves high hydrolysis resistance and processability, reducing delamination and contamination risks, with controlled alkaline elution and improved chemical durability, suitable for pharmaceutical containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133712000001
    Figure 2024133712000001
  • Figure 2024133712000002
    Figure 2024133712000002
  • Figure 2024133712000003
    Figure 2024133712000003
Patent Text Reader

Abstract

To provide a glass for a medicine container that excels in both hydrolytic resistance and processability, and a glass tube and a medicine container using the same.SOLUTION: A glass for a medicine container of the present invention includes as a glass composition, in terms of mol%, SiO2 60-85%, Al2O3 3-20%, B2O3 0-5%, Li2O 0-9%, Na2O 0-12%, K2O 0-6%, Li2O+Na2O+K2O 0.1-26%, SrO 0-1%, and BaO 0-1%, with the value of molar ratio K2O / (Li2O+Na2O+K2O) being 0.60 or less, and the value of molar ratio Al2O3 / (Li2O+Na2O+K2O) being 50 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass for pharmaceutical containers having excellent processability and hydrolysis resistance, and a glass tube for pharmaceutical containers and pharmaceutical containers each using the same. Background technology Traditionally, various glass containers have been used as filling containers for storing pharmaceuticals. Pharmaceuticals are broadly divided into two types: oral and parenteral. For parenteral drugs in particular, the glass container must be of extremely high quality, since the drug is filled and stored in the glass container and administered directly into the patient's bloodstream.

[0002] Pharmaceutical containers are also required to prevent the components of the drugs filled in them from changing in quality. If glass components leach into the drugs, they may change the properties of the drugs and affect the health and even the life of the patient. For this reason, the pharmacopoeias of each country restrict the amount of glass components that can leach from glass used for pharmaceutical containers.

[0003] Therefore, borosilicate glass is used as a glass material that satisfies the standards for components eluted from glass.

[0004] In recent years, with the development of medicine and pharmacology, highly effective drugs are being developed, but when such drugs are filled and stored in glass containers that contain a lot of B2O3, the inner surface of the glass container is eroded, and the inner surface of the container peels off and floats in the drug as flakes, causing a phenomenon called delamination, which has become a problem. This is because insoluble foreign matter generated by delamination, etc., may be harmful to the human body if injected into the patient's body together with the drug, such as by forming blood clots in the blood vessels.

[0005] Furthermore, in order to be able to handle such highly effective drugs, there is a demand for glass that is less susceptible to elution of glass components in water or drugs than before and has better hydrolysis resistance.

[0006] Glass for pharmaceutical containers is required to be processed into complex shapes such as ampoules, vials, prefilled syringes, cartridges, etc., and therefore, at the same time, it is also desired that the glass has low viscosity and excellent processability. Furthermore, regarding the working temperature during processing, if the working temperature is high, the components contained in the glass are likely to evaporate during processing, which may contaminate the inner surface of the container and, ultimately, the medicine in the glass container. [Prior art documents] [Patent documents]

[0007] Patent document 1: WO2013 / 063275 publication Summary of the Invention [Problem to be solved by the invention]

[0008] In view of the above circumstances, Patent Document 1 proposes glass with a reduced B2O3 content in order to reduce delamination. However, since reducing B2O3 increases the viscosity of the glass, the glass is made to contain a large amount of Na2O in order to reduce the viscosity. This results in a problem of poor hydrolysis resistance.

[0009] The technical object of the present invention is to provide a glass for pharmaceutical containers that combines excellent hydrolysis resistance and processability, and a glass tube and pharmaceutical container using the same. [Means for solving the problem]

[0010] The present inventors have conducted extensive research into the components constituting the glass, and have found that the above problems can be solved by strictly controlling the content of each component, which they propose as the present invention.

[0011] Specifically, the glass for pharmaceutical containers of the present invention has improved hydrolysis resistance by strictly controlling the content of Na2O, which is likely to affect the hydrolysis resistance of glass. Furthermore, it is possible to achieve both excellent hydrolysis resistance and processability by strictly controlling the molar ratios of K2O / (Li2O+Na2O+K2O) and Al2O3 / (Li2O+Na2O+K2O).

[0012] That is, the glass for pharmaceutical containers of the present invention has a glass composition containing, in mole percent, 60-85% SiO2, 3-20% Al2O3, 0-5% B2O3, 0-9% Li2O, 0-12% Na2O, 0-6% K2O, 0.1-26% Li2O+Na2O+K2O, 0-1% SrO, and 0-1% BaO, and is characterized in that the molar ratio K2O / (Li2O+Na2O+K2O) is 0.60 or less, and the molar ratio Al2O3 / (Li2O+Na2O+K2O) is 50 or less. Here, "Li2O+Na2O+K2O" refers to the combined amount of Li2O, Na2O, and K2O, "K2O / (Li2O+Na2O+K2O)" refers to the value obtained by dividing the K2O content by the combined amount of Li2O, Na2O, and K2O, and "Al2O3 / (Li2O+Na2O+K2O)" refers to the value obtained by dividing the Al2O3 content by the combined amount of Li2O, Na2O, and K2O.

[0013] In this way, it becomes easier to obtain a glass for pharmaceutical containers that has both excellent hydrolysis resistance and processability.

[0014] The glass for pharmaceutical containers of the present invention preferably contains, as a glass composition, 0-7% Li2O, 0-7.9% Na2O, and 0-3% K2O.

[0015] In this way, better hydrolysis resistance can be easily obtained.

[0016] The glass for pharmaceutical containers of the present invention preferably has a total content of MgO, CaO, SrO and BaO of 0 to 5 mol %.

[0017] In this way, better hydrolysis resistance can be easily obtained.

[0018] The glass for pharmaceutical containers of the present invention preferably contains, in terms of mole percent, 0-0.5% MgO, 0-0.5% CaO, 0-0.3% SrO, and 0-0.3% BaO as a glass composition.

[0019] In this way, better hydrolysis resistance can be easily obtained.

[0020] The glass for pharmaceutical containers of the present invention preferably has a molar ratio K2O / (Li2O+Na2O+K2O) of 0.24 or less.

[0021] In this way, better processability can be easily achieved.

[0022] The glass for pharmaceutical containers of the present invention preferably has a molar ratio Al2O3 / (Li2O+Na2O+K2O) of 0.85 or less.

[0023] In this way, better processability can be easily achieved.

[0024] The glass for pharmaceutical containers of the present invention preferably has a B2O3 content of 0.01 to 1 mol %.

[0025] In this way, it is possible to obtain good workability while suppressing the occurrence of delamination.

[0026] The glass for pharmaceutical containers of the present invention preferably has a ZrO2 content of 0 to 2 mol %.

[0027] The glass for pharmaceutical containers of the present invention has a glass composition containing, in mole percent, 60-85% SiO2, 5-17.5% Al2O3, 0-4% B2O3, 0-6% Li2O, 0-8.3% Na2O, 0-5% K2O, 0.1-26% Li2O+Na2O+K2O, 0-1% SrO, 0-1% BaO, and 0-5% MgO+CaO+SrO+BaO, and is characterized in that the molar ratio K2O / (Li2O+Na2O+K2O) is 0.24 or less and the molar ratio Al2O3 / (Li2O+Na2O+K2O) is 0.67 or less.

[0028] The glass for pharmaceutical containers of the present invention has a glass composition containing, in mole percent, 60-85% SiO2, 5-17.5% Al2O3, 0-5% B2O3, 0-7% Li2O, 0-8.3% Na2O, 0-5% K2O, 0.1-26% Li2O+Na2O+K2O, 0-1% SrO, 0-1% BaO, and 0-3.7% MgO+CaO+SrO+BaO, and is characterized in that the molar ratio K2O / (Li2O+Na2O+K2O) is 0.24 or less and the molar ratio Al2O3 / (Li2O+Na2O+K2O) is 0.67 or less.

[0029] The glass for pharmaceutical containers of the present invention is characterized in that it contains, in mole percent, 60-85% SiO2, 5-20% Al2O3, 0-5% B2O3, 0.1-26% Li2O+Na2O+K2O, and 0-3% MgO+CaO+SrO+BaO.

[0030] The glass for pharmaceutical containers of the present invention has a glass composition comprising, in mole percent, 60-85% SiO2, 3-7% Al2O3, 0-5% B2O3, 0-7% Li2O, 0-8.3% Na2O, 0-5% K2O, 0.1-26% Li2O+Na2O+K2O, 0-1% SrO, 0-1% BaO, and 0-3.7% MgO+CaO+SrO+BaO, and is characterized in that the molar ratio K2O / (Li2O+Na2O+K2O) is 0.24 or less, the molar ratio Al2O3 / (Li2O+Na2O+K2O) is 0.5 or less, and the molar ratio SiO2 / Al2O3 is 16 or less.

[0031] Moreover, the glass for pharmaceutical containers of the present invention preferably has a class of at least HGA1 in a hydrolysis resistance test (acetone washing) according to ISO720.

[0032] In the present invention, the "hydrolysis resistance test in accordance with ISO720 (acetone washing)" refers to the following test. (1) The glass sample is crushed in an alumina mortar and classified into particles of 300 to 425 μm using a sieve. (2) The obtained powder sample is washed with acetone and dried in an oven at 140°C. (3) After drying, 10 g of the powder sample was placed in a quartz flask, 50 mL of purified water was added, and the flask was then sealed and processed in an autoclave under the following processing conditions: the temperature was raised from 100°C to 121°C at 1°C / min, then the flask was kept at 121°C for 30 minutes, and then the temperature was lowered to 100°C at 0.5°C / min. (4) After autoclaving, transfer the solution in the quartz flask to another beaker, and then wash the inside of the quartz flask three times with 15 mL of purified water, and add the washings to the beaker as well. (5) Add methyl red indicator to the beaker and titrate with 0.02 mol / L hydrochloric acid aqueous solution. (6) 1 mL of 0.02 mol / L hydrochloric acid solution is equivalent to 620 μg of Na2O, and converted into the amount of alkali elution per 1 g of glass.

[0033] In addition, "class of at least HGA1 in the hydrolysis resistance test (acetone washing) in accordance with ISO 720" means that the amount of alkali elution per 1 g of glass, calculated as Na2O, determined by the above test is 62 μg / g or less.

[0034] The glass for pharmaceutical containers of the present invention preferably has a working point of 1,300° C. or less. The "working point" is defined as the temperature at which the viscosity of the glass reaches 10 4.0 This refers to the temperature at which the viscosity becomes dPa s.

[0035] In this way, since there is no need to raise the processing temperature when processing into pharmaceutical containers, etc., evaporation of glass components during processing can be reduced, making it easier to suppress contamination of the inner surface of the container.

[0036] The glass tube for pharmaceutical containers of the present invention is preferably made of the above-mentioned glass for pharmaceutical containers.

[0037] The pharmaceutical container of the present invention is preferably made of the above-mentioned glass for pharmaceutical containers. The glass for pharmaceutical containers of the present invention has high hydrolysis resistance. Furthermore, since the processing temperature can be lowered, the evaporation of glass components during processing can be reduced, and contamination of the inner surface of the container can be easily suppressed. As a result, it is easy to obtain a pharmaceutical container with excellent hydrolysis resistance and therefore chemical durability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] The reasons for limiting the composition range of each component will be described below. In the following explanation, "%" means "mol %" unless otherwise specified.

[0039] SiO2 is one of the components that constitute the network structure of glass. If the SiO2 content is too low, vitrification becomes difficult, and the thermal expansion coefficient increases, making it easy for thermal shock resistance to decrease. On the other hand, if the SiO2 content is too high, the liquidus temperature increases and devitrification becomes easy. Therefore, the SiO2 content is preferably 60 to 85%, 65 to 85%, 68 to 83%, and particularly 70 to 80%.

[0040] Al2O3 is one of the components that constitute the network structure of glass, and has the effect of improving the hydrolysis resistance of glass. If the content of Al2O3 is too low, the hydrolysis resistance is likely to deteriorate. On the other hand, if the content of Al2O3 is too high, the viscosity increases. Therefore, the content of Al2O3 is preferably 3 to 20%, 4 to 20%, 4 to 17.5%, 4.5 to 17.5%, 5 to 15%, 5.3 to 14%, 5.4 to 13%, 5.5 to 12.4%, 5.6 to 12%, 5.7 to 11.5%, 5.8 to 11%, 5.9 to 10%, and particularly 6 to 9%.

[0041] B2O3 has the effect of lowering the viscosity of glass and improving melting property and processability. However, B2O3 is considered to be one of the factors that cause delamination, and if the content is too high, delamination resistance deteriorates and flakes tend to occur. Therefore, the content of B2O3 is preferably 0 to 5%, 0.01 to 4%, 0.02 to 3%, 0.03 to 2%, 0.04 to 1%, 0.04 to 0.8%, and particularly 0.05 to 0.5%.

[0042] Alkali metal oxides (R2O), Li2O, Na2O and K2O, have the effect of reducing the viscosity of glass and improving processability and meltability. The lower limit of the total content of R2O is preferably 0.1% or more, 0.5% or more, 1% or more, 2% or more, 3% or more, 4% or more, 4.5% or more, 5% or more, 5.5% or more, 6% or more, 6.5% or more, 7% or more, 7.5% or more, particularly 8% or more. When the processability of glass is particularly important, the lower limit of the total content of R2O is 8.5% or more, 9% or more, 9.5% or more, 10% or more, 10.5% or more, 11% or more. On the other hand, if the total content of these components is too high, the hydrolysis resistance of the glass deteriorates, or the thermal expansion coefficient increases, resulting in a decrease in thermal shock resistance. Therefore, the upper limit of the total content of R2O is preferably 26% or less, 23% or less, 20% or less, 18% or less, 17.5% or less, 17% or less, less than 17%, 16% or less, 15% or less, 14% or less, 13.9% or less, 13% or less, 12% or less, and particularly 11% or less.

[0043] As mentioned above, Li2O has the effect of lowering the viscosity of glass and improving the workability and meltability. Among R2O, Li2O has the highest effect of lowering the viscosity of glass, followed by Na2O and K2O in that order. However, if the content of Li2O is too high, the hydrolysis resistance is likely to deteriorate. Therefore, the content of Li2O is preferably 0 to 9%, 0 to 8%, 0 to 7%, 0 to 6.5%, 0 to 6.3%, 0 to 6.1%, 0 to 6%, 0 to 5.9%, 0 to 5.8%, 0 to 5.7%, 0 to 5.5%, 0 to 5%, 0 to 4.5%, 0 to 4%, and particularly 0 to 3.5%. In particular, with regard to the resistance to devitrification, devitrification is particularly unlikely to occur when the content of Li2O is 6% or less.

[0044] When emphasis is placed on the processability of the glass, the Li2O content is preferably 0.1 to 9%, and may be 0.5 to 8%, 1 to 7%, 2 to 6.5%, 2.5 to 6.3%, 3 to 6.1%, 3.5 to 6%, and particularly 4 to 5%.

[0045] Furthermore, when emphasis is placed on achieving both the workability and hydrolysis resistance of the glass, the Li2O content is preferably 2 to 8%, 2.5 to 7%, and particularly preferably 3 to 6.5%.

[0046] Like Li2O, Na2O has the effect of lowering the viscosity of glass and improving workability and meltability. If the content is too small, the devitrification resistance may decrease. On the other hand, as described above, if the content of Na2O is too large, the hydrolysis resistance in particular deteriorates. Therefore, the content of Na2O is preferably 0 to 12%, 0 to 10%, 0 to 9%, 0 to 8.5%, 0 to 8.3%, 0 to 8%, 0 to 7.9%, 0 to 7.5%, 0 to 7%, 0 to 6.5%, 0 to 6%, 0 to 5.5%, and particularly 0 to 5%.

[0047] When emphasis is placed on the processability of the glass, the Na2O content is preferably 0.1 to 12%, and may be 0.5 to 11%, 1 to 10%, 2 to 9%, 2.5 to 8.5%, 3 to 8%, 3.5 to 7.9%, 4 to 7.5%, or 4.5 to 7%, and particularly 5 to 6.5%.

[0048] Although K2O has a lower viscosity than Li2O and Na2O, it has the effect of lowering the viscosity of glass and improving processability and meltability. However, if the content of K2O is too high, hydrolysis resistance deteriorates. On the other hand, if the content is too low, devitrification resistance may deteriorate. Therefore, the content of K2O is preferably 0 to 6%, 0 to 5%, 0 to 4%, 0 to 3%, 0 to 2.9%, 0 to 2.8%, 0 to 2.7%, 0 to 2.6%, 0 to 2.5%, 0 to 2%, and particularly 0 to less than 2%.

[0049] When emphasis is placed on the processability of the glass, the K2O content is preferably 0.01 to 11%, and may be 0.05 to 10%, 0.1 to 8%, 0.5 to 6%, 0.8 to 5.5%, 1 to 5%, 1.2 to 4%, 1.4 to 3.5%, and particularly 1.5 to 3%.

[0050] Among the above-mentioned alkali metal oxides (R2O), Li2O has the highest effect of lowering the viscosity of glass, followed by Na2O and K2O. Therefore, from the viewpoint of lowering the viscosity of glass, the relationship of the contents of each is preferably Li2O≧Na2O≧K2O, Li2O≧Na2O>K2O or Li2O>Na2O≧K2O, and particularly preferably Li2O>Na2O>K2O. Moreover, if the proportion of K2O is too high, it becomes difficult to maintain both the viscosity and hydrolysis resistance of the glass in a good condition. Therefore, from the viewpoint of achieving both viscosity and hydrolysis resistance, it is preferable that Na2O>K2O.

[0051] If the proportion of Li2O in the alkali metal oxides (R2O) contained in the glass is too high, the devitrification resistance of the glass is reduced. Therefore, in an embodiment, from the viewpoint of devitrification resistance, the alkali metal oxides (R2O) may satisfy the relationship Na2O>Li2O. Furthermore, the effect of improving the devitrification resistance of the glass is greatest with K2O, followed by Na2O and Li2O in that order. From the viewpoint of achieving both hydrolysis resistance and devitrification resistance of the glass, it is preferable that Li2O≧Na2O≧K2O, Li2O≧K2O>Na2O, or Li2O>Na2O≧K2O, and it is particularly preferable that Li2O>K2O>Na2O.

[0052] Moreover, if the proportion of K2O in the alkali metal oxide (R2O) is too high, the effect of lowering the viscosity of the glass is reduced. Therefore, the upper limit of the molar ratio K2O / (Li2O+Na2O+K2O) is preferably 0.60 or less, 0.50 or less, 0.40 or less, 0.24 or less, 0.22 or less, 0.21 or less, 0.18 or less, particularly 0.15 or less. In this way, the viscosity of the glass is easily lowered. On the other hand, if the value of the molar ratio K2O / (Li2O+Na2O+K2O) is too small, the hydrolysis resistance of the glass may deteriorate. Therefore, the lower limit of the molar ratio K2O / (Li2O+Na2O+K2O) is preferably more than 0, 0.01 or more, particularly 0.03 or more, 0.05 or more, 0.8 or more, 0.1 or more, 0.13 or more.

[0053] Increasing the content of Al2O3 improves hydrolysis resistance while increasing the viscosity of the glass. In addition, increasing the contents of Li2O, Na2O, and K2O deteriorates hydrolysis resistance while decreasing the viscosity of the glass. In the present invention, in order to achieve both hydrolysis resistance and processability of the glass, it is necessary to strictly control the balance of the contents of the components related to these properties. Therefore, the value of the molar ratio Al2O3 / (Li2O+Na2O+K2O) is preferably 50 or less, 40 or less, 30 or less, 20 or less, 10 or less, 5 or less, 3 or less, 2 or less, 1.2 or less, 0 to 1, 0 to 0.85, 0 to 0.8, more than 0 to 0.74, 0.01 to 0.7, 0.1 to 0.67, 0.2 to 0.65, 0.3 to 0.61, 0.33 to 0.60, 0.34 to 0.59, 0.4 to 0.55, and particularly more than 0.4 to 0.5. As described above, by limiting the contents of Al2O3, Li2O, Na2O, and K2O, it becomes easy to achieve both good hydrolysis resistance and processability. In particular, when the molar ratio Al2O3 / (Li2O+Na2O+K2O) is 0.67 or less, it becomes easier to achieve both good hydrolysis resistance and processability.

[0054] If the content of Al2O3 is too low relative to SiO2, the hydrolysis resistance of the glass deteriorates, and the devitrification resistance also deteriorates. In the present invention, in order to maintain good devitrification resistance in addition to hydrolysis resistance and processability of the glass, it is desirable to strictly control the component balance of SiO2 and Al2O3. Therefore, the upper limit range of the molar ratio SiO2 / Al2O3 is preferably 30 or less, 20 or less, 18 or less, 17 or less, 16 or less, and particularly 15 or less. In addition, if the content of Al2O3 is too high relative to SiO2, it becomes difficult to achieve both hydrolysis resistance and processability. Therefore, the lower limit range of the molar ratio SiO2 / Al2O3 is preferably 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, 11 or more, and particularly 12 or more.

[0055] In order to achieve both hydrolysis resistance and processability of glass, it is preferable to regulate the balance between the content of SiO2, which is the component with the highest content in the present invention, and the content of Li2O, Na2O, and K2O, which have the function of reducing viscosity. Therefore, the value of the molar ratio SiO2 / (Li2O+Na2O+K2O) is preferably 10 or less, 8 or less, 7.9 or less, 7 or less, 6.9 or less, 6.5 or less, 6.1 or less, 6.0 or less, 5.9 or less, and particularly 5.7 or less. By limiting the contents of SiO2, Li2O, Na2O, and K2O as described above, it becomes easy to achieve both good hydrolysis resistance and processability. In particular, when the value of the molar ratio SiO2 / (Li2O+Na2O+K2O) is 6.9 or less, it becomes easier to achieve both hydrolysis resistance and processability.

[0056] Furthermore, it is preferable to appropriately regulate the value of Li2O / (Na2O+K2O) of the alkali metal oxide (R2O). In this way, the effect of Li2O, which has a high effect of reducing viscosity among alkali metal oxides, can be enjoyed while suppressing the effect of Na2O, which particularly deteriorates hydrolysis resistance. Therefore, the lower limit of Li2O / (Na2O+K2O) is 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, and particularly preferably 0.7 or more. On the other hand, if Li2O / (Na2O+K2O) is too large, the raw material cost increases. Therefore, the upper limit of the molar ratio Li2O / (Na2O+K2O) of the total content of Li2O, Na2O, and K2O is preferably 2.0 or less, 1.5 or less, 1.2 or less, 1.1 or less, 1.0 or less, less than 1.0, 0.9 or less, 0.8 or less, or less than 0.8.

[0057] Alkaline earth metal oxides (R'O), MgO, CaO, SrO and BaO, have the effect of reducing the viscosity of glass. They also affect hydrolysis resistance. If the content of these components is too high, the hydrolysis resistance and devitrification resistance of the glass will decrease, and R'O dissolved from the glass into the chemicals may precipitate as carbonate or sulfate. Therefore, the total amount of R'O is preferably 0 to 10%, and is preferably 0 to 5%, 0 to 4%, 0 to 3.7%, 0 to 3%, 0 to 2%, 0 to 1%, 0 to 0.9%, 0 to 0.8%, 0 to 0.7%, 0 to 0.6%, 0 to 0.5%, 0 to 0.4%, 0 to 0.3%, 0 to 0.2%, 0 to 0.1%, 0 to 0.01%, less than 0.01%, and particularly none. In the present invention, "not containing" means not actively adding, and does not exclude unavoidable impurities.

[0058] Here, the ease of precipitation of carbonates or sulfates of R'O depends on the solubility of each salt. Specifically, MgO has the highest solubility, followed by CaO, SrO, and BaO in that order. Therefore, MgO is the least likely to cause salt precipitation, and BaO is the most likely to cause salt precipitation. Therefore, when focusing on solubility, the content of R'O is preferably MgO≧CaO≧SrO≧BaO, and more preferably MgO>CaO>SrO>BaO.

[0059] On the other hand, BaO has the highest effect of reducing the viscosity of the glass, followed by SrO, CaO, and MgO in that order. Therefore, when emphasis is placed on processability, the content of R'O is preferably BaO≧SrO≧CaO≧MgO, and more preferably BaO>SrO>CaO>MgO.

[0060] In addition, it is preferable to restrict MgO in the glass for pharmaceutical containers of the present invention. As described above, MgO is a component that has high solubility of carbonate or sulfate and is unlikely to cause salt precipitation. However, since Mg ions are likely to react with hydrated silicic acid, when Mg ions in the glass are eluted, the hydrated silicic acid formed on the glass surface reacts with Mg ions to form an insoluble magnesium silicate hydrate film. This film may peel off due to vibration or the like and become a flaky insoluble foreign matter. In addition, if the content of MgO is too high, the hydrolysis resistance is deteriorated. Therefore, in the present invention, it is preferable to strictly restrict MgO. Therefore, the content of MgO is preferably 0 to 10%, 0 to 8%, 0 to 5%, 0 to 3%, 0 to 1%, 0 to 0.9%, 0 to 0.8%, 0 to 0.7%, 0 to 0.6%, 0 to 0.5%, 0 to 0.4%, 0 to 0.3%, 0 to 0.2%, 0 to 0.1%, 0 to 0.05%, 0 to 0.03%, less than 0 to 0.03%, 0 to 0.01%, or less than 0 to 0.01%. It is also preferable that no MgO is contained. Note that, when the workability of the glass is particularly important, 0.01% or more of MgO may be contained.

[0061] In addition, in order to improve hydrolysis resistance, it is preferable to strictly regulate CaO in the glass for pharmaceutical containers of the present invention. The CaO content is preferably 0 to 10%, 0 to 8%, 0 to 5%, 0 to 3%, 0 to 1%, 0 to 0.9%, 0 to 0.8%, 0 to 0.7%, 0 to 0.6%, 0 to 0.5%, 0 to 0.4%, 0 to 0.3%, 0 to 0.2%, 0 to 0.1%, 0 to 0.05%, 0 to 0.03%, less than 0 to 0.03%, 0 to 0.01%, and less than 0 to 0.01%. It is also preferable that CaO is not contained. Note that, when the workability of the glass is particularly important, CaO may be contained in an amount of 0.01% or more.

[0062] In addition, in the glass for pharmaceutical containers of the present invention, in order to suppress precipitation of carbonates or sulfates and improve hydrolysis resistance, it is preferable to strictly regulate the SrO content. The SrO content is preferably 0 to 1%, and more preferably 0 to 0.9%, 0 to 0.8%, 0 to 0.7%, 0 to 0.6%, 0 to 0.5%, 0 to 0.4%, 0 to 0.3%, 0 to 0.2%, 0 to 0.1%, 0 to 0.01%, less than 0 to 0.01%, and particularly none.

[0063] In addition, in the glass for pharmaceutical containers of the present invention, it is preferable to strictly regulate BaO in order to suppress precipitation of carbonates or sulfates and improve hydrolysis resistance. The content of BaO is preferably 0 to 1%, and more preferably 0 to 0.9%, 0 to 0.8%, 0 to 0.7%, 0 to 0.6%, 0 to 0.5%, 0 to 0.4%, 0 to 0.3%, 0 to 0.2%, 0 to 0.1%, 0 to 0.01%, less than 0 to 0.01%, and particularly none.

[0064] As described above, MgO is a component that has high solubility of carbonate or sulfate and is unlikely to cause salt precipitation, while Mg ions are likely to react with hydrated silicic acid, and therefore may form an insoluble magnesium silicate hydrate film. Therefore, it is preferable that the value of the molar ratio MgO / (MgO+CaO+SrO+BaO) is regulated in the glass for pharmaceutical containers of the present invention. The value of the molar ratio MgO / (MgO+CaO+SrO+BaO) is preferably 1 or less, less than 1, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, less than 0.5, 0.4 or less, 0.3 or less, 0.2 or less, 0.1 or less, and particularly 0.

[0065] Also, the value of MgO+CaO is preferably 0-10%, 0-5%, 0-4%, 0-3.7%, 0-3%, 0-2%, 0-1%, 0-0.9%, 0-0.8%, 0-0.7%, 0-0.6%, 0-0.5%, 0-0.4%, 0-0.3%, 0-0.2%, 0-0.1%, 0-0.01%, less than 0-0.01%, and particularly preferably none. In this way, precipitation of carbonates or sulfates is less likely to occur. Note that "MgO+CaO" refers to the total content of MgO and CaO.

[0066] In addition, the molar ratio MgO / CaO of the content of MgO and CaO is preferably less than 9.0, 8.0 or less, 6.0 or less, 5.0 or less, 3.0 or less, 1.0 or less, 1.0 or less, or 0.5 or less. More preferably, it is 0.9 or less, 0.7 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, or 0.1 or less. In this way, the hydrolysis resistance can be improved. As described above, in the present invention, MgO may generate an insoluble magnesium silicate hydrate film, but CaO is a component that is less likely to react with SiO2 than MgO, and is less likely to generate an insoluble film. Therefore, by regulating the molar ratio MgO / CaO, the safety of the container can be improved. In addition, the viscosity of the glass can be reduced, so that excellent processability can be obtained.

[0067] In addition, in order to achieve both hydrolysis resistance and processability, it is more preferable to regulate the balance between the CaO and Li2O contents in the glass for pharmaceutical containers of the present invention. The molar ratio of the CaO and Li2O contents, CaO / Li2O, is preferably 2.0 or less, 1.5 or less, 1.2 or less, 1.1 or less, 1.0 or less, less than 1.0, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, 0.1 or less, and particularly preferably 0.

[0068] In addition, the total content of SiO2, Al2O3, B2O3, Li2O, Na2O, K2O, MgO, CaO, SrO and BaO in the glass for pharmaceutical containers of the present invention is preferably 90% or more, 93% or more, 95% or more, 96% or more, 97% or more, 98% or more, 98.5% or more, and particularly 99% or more. By doing so, the effects of the above-mentioned components can be efficiently obtained, making it easier to achieve both excellent hydrolysis resistance and processability.

[0069] The glass for pharmaceutical containers of the present invention may contain other components as a glass composition other than those mentioned above. For example, ZrO2 may be contained in order to improve the alkali resistance of the glass. However, if the content of ZrO2 is too high, the viscosity of the glass increases and the devitrification resistance decreases. When ZrO2 is contained, the content is preferably 0 to 3%, 0 to 2.5%, 0 to 2%, 0 to 1.5%, 0.1 to 0.8%, and particularly preferably 0.2 to 0.6%.

[0070] The glass for pharmaceutical containers of the present invention may contain ZnO. While ZnO has the effect of reducing the viscosity of the glass, if the content is too high, it affects the hydrolysis resistance of the glass. In the present invention, the content of ZnO is preferably 0 to 4%, 0 to 1%, and preferably none.

[0071] Also, if it is desired to color the glass, TiO2 and Fe2O3 can be added to the batch raw materials, and in this case, the total content of standard TiO2 and Fe2O3 is preferably 7% or less, 6% or less, 5% or less, 1% or less, or even 0.5% or less.

[0072] The glass may contain one or more fining agents such as F, Cl, Sb2O3, SnO2, and SO3. In this case, the total content of standard fining agents is preferably 5% or less, more preferably 1% or less, and even more preferably 0.5% or less.

[0073] In addition, in order to improve chemical durability, high temperature viscosity, etc., P2O5, Cr2O3, PbO, La2O3, WO3, Nb2O3, Y2O3, etc. may be added at 3% or less, 2% or less, 1% or less, less than 1%, and 0.5% or less, respectively.

[0074] Impurities such as H2, CO2, CO, H2O, He, Ne, Ar, and N2 may each be contained up to 0.1%. The amount of each of precious metal elements such as Pt, Rh, and Au is preferably 500 ppm or less, and more preferably 300 ppm or less.

[0075] In addition to the above-mentioned composition range, the glass composition may contain, in mole percent, SiO2 60-85%, Al2O3 5-17.5%, B2O3 0-4%, Li2O 0-6%, Na2O 0-8.3%, K2O 0-5%, Li2O+Na2O+K2O 0.1-26%, SrO 0-1%, BaO 0-1%, MgO+CaO+SrO+BaO 0-5%, and the molar ratio K2O / (Li2O+Na2O+K2O) is 0.24 or less and the molar ratio Al2O3 / (Li2O+Na2O+K2O) is 0.67 or less. The reasons for limiting each component and the preferred range are the same as those described above, so the explanation will be omitted here.

[0076] In addition to the above-mentioned composition range, for example, the glass composition may contain, in mole percent, SiO2 60-85%, Al2O3 5-17.5%, B2O3 0-5%, Li2O 0-7%, Na2O 0-8.3%, K2O 0-5%, Li2O+Na2O+K2O 0.1-26%, SrO 0-1%, BaO 0-1%, MgO+CaO+SrO+BaO 0-3.7%, and the molar ratio K2O / (Li2O+Na2O+K2O) is 0.24 or less and the molar ratio Al2O3 / (Li2O+Na2O+K2O) is 0.67 or less. The reasons for limiting each component and the preferred range are the same as those described above, so the explanation will be omitted here.

[0077] As another embodiment of the glass for pharmaceutical containers of the present invention, in addition to the above-mentioned composition ranges, for example, glass containing, in mol %, 60-85% SiO2, 5-20% Al2O3, 0-5% B2O3, 0.1-26% Li2O+Na2O+K2O, and 0-3% MgO+CaO+SrO+BaO can be exemplified. The reasons for limiting each component and the preferred ranges are the same as those described above, so explanations will be omitted here.

[0078] Further, as another embodiment of the glass for pharmaceutical containers of the present invention, in addition to the above-mentioned composition ranges, for example, glass compositions containing, in mole percent, SiO2 60-85%, Al2O3 3-7%, B2O3 0-5%, Li2O 0-7%, Na2O 0-8.3%, K2O 0-5%, Li2O+Na2O+K2O 0.1-26%, SrO 0-1%, BaO 0-1%, MgO+CaO+SrO+BaO 0-3.7%, a molar ratio K2O / (Li2O+Na2O+K2O) of 0.24 or less, a molar ratio Al2O3 / (Li2O+Na2O+K2O) of 0.5 or less, and a molar ratio SiO2 / Al2O3 of 16 or less can be exemplified. The reasons for limiting each component and the preferred ranges are the same as those described above, so explanations will be omitted here.

[0079] Moreover, the glass for pharmaceutical containers of the present invention preferably has a class of at least HGA1 in a hydrolysis resistance test (acetone washing) according to ISO720.

[0080] Furthermore, the glass for pharmaceutical containers of the present invention preferably has an alkali elution amount calculated as Na2O in a hydrolysis resistance test (acetone washing) in accordance with ISO 720 that is less than 62 μg / g, 60 μg / g or less, 57 μg / g or less, 55 μg / g or less, 53 μg / g or less, and particularly 50 μg / g or less. If the alkali elution amount is too high, when the glass is processed into an ampule or vial and filled with a medicine and stored, the medicine component may be deteriorated by the alkali component eluted from the glass.

[0081] The alkali resistance of glass is an index for judging the resistance to delamination. The glass for pharmaceutical containers of the present invention preferably has an alkali resistance of at least Class 2 in a test conforming to ISO 695. Here, "alkali resistance test conforming to ISO 695" refers to the following test. (1) Surface area of ​​all mirror-finished surfaces: Acm 2 (However, A is 10~15cm 2 A glass sample piece (specified as 1:1) is prepared. First, as a pretreatment, the sample is mixed with a solution of hydrofluoric acid (40 wt%) and hydrochloric acid (2 mol / L) in a volume ratio of 1:9. The sample is immersed in this and stirred with a magnetic stirrer for 10 minutes. The sample is then removed and subjected to ultrasonic cleaning with purified water for 2 minutes three times, and ultrasonic cleaning with ethanol for 1 minute twice. (2) The sample is then dried in an oven at 110°C for 1 hour and allowed to cool in a desiccator for 30 minutes. (3) Measure and record the mass m1 of the sample to an accuracy of ±0.1 mg. (4) Prepare 800 mL of a solution by mixing an aqueous solution of sodium hydroxide (1 mol / L) and an aqueous solution of sodium carbonate (0.5 mol / L) in a volume ratio of 1:1. Place the solution in a stainless steel container and boil it using a mantle heater. Add a sample suspended from a platinum wire and hold for 3 hours. Remove the sample and ultrasonically clean it with purified water for 2 minutes three times, then ultrasonically clean it with ethanol for 1 minute twice. After that, dry the sample in an oven at 110°C for 1 hour and leave it to cool in a desiccator for 30 minutes. (5) Measure and record the mass m2 of the sample to an accuracy of ±0.1 mg. (6) Mass m1, m2 (mg) and surface area A (cm2) of the sample before and after immersion in the boiling alkaline solution 2 ) to calculate the mass loss per unit area using the following formula, and use this as the measured value for the alkali resistance test. (Mass loss per unit area) = 100 × (m1-m2) / A In addition, "Class 2 alkali resistance in a test conforming to ISO 695" means that the mass loss per unit area calculated as above is 175 mg / dm 2 This means that the mass loss per unit area calculated above is 75 mg / dm 2 If the glass has a mass loss per unit area of ​​130 mg / dm or less, the glass has an alkali resistance of Class 1 according to a test in accordance with ISO 695. 2 Less than 75 mg / dm 2 It is preferable that:

[0082] Delamination often occurs when a drug is filled and stored in a glass container with a solution that behaves like a strong alkali even if the pH is near neutral, such as citric acid or phosphate buffer. The mass loss per unit area determined by a test in accordance with ISO695 is 175 mg / dm 2 If the mass loss per unit area of ​​the glass for pharmaceutical containers of the present invention is larger than 130 mg / dm 2 Less than 75 mg / dm 2 It is preferable that:

[0083] Furthermore, the glass for pharmaceutical containers of the present invention preferably has a mass loss per unit area of ​​1.5 mg / dm2 or less in an acid resistance test in accordance with YBB00342004. 2 Below 0.7 mg / dm 2If the amount of mass loss is large, when a bottle container such as an ampule or vial is made and filled with a liquid medicine and stored, the amount of glass components eluted may increase significantly, causing deterioration of the liquid medicine components. Note that "acid resistance test according to YBB00342004" refers to the following test.

[0084] Here, "acid resistance test in accordance with YBB00342004" refers to the following test. (1) Surface area of ​​all mirror-finished surfaces: Acm 2 (However, A is 100±5cm 2 A glass sample piece (specified as 1:1) is prepared. First, as a pretreatment, the sample is mixed with a solution of hydrofluoric acid (40 wt%) and hydrochloric acid (2 mol / L) in a volume ratio of 1:9. The sample is immersed in this and stirred with a magnetic stirrer for 10 minutes. The sample is then removed and subjected to ultrasonic cleaning with purified water for 2 minutes three times, and ultrasonic cleaning with ethanol for 1 minute twice. (2) The sample is then dried in an oven at 110°C for 1 hour and allowed to cool in a desiccator for 30 minutes. (3) Measure and record the mass m1 of the sample to an accuracy of ±0.1 mg. (4) Prepare 800 mL of hydrochloric acid solution (6 mol / L). Place the solution in a silica glass container and boil it using an electric heater. Add a sample suspended from a platinum wire and hold for 6 hours. Remove the sample and ultrasonically clean it with purified water for 2 minutes three times, then ultrasonically clean it with ethanol for 1 minute twice. After that, dry the sample in an oven at 110°C for 1 hour and leave it to cool in a desiccator for 30 minutes. (5) Measure and record the mass m2 of the sample to an accuracy of ±0.1 mg. (6) Mass m1, m2 (mg) and surface area A (cm2) of the sample before and after immersion in the boiling acid solution 2 ) to calculate half of the mass loss per unit area using the following formula, and use this as the measured value for the acid resistance test. (Mass loss per unit area) = 1 / 2 x 100 x (m1-m2) / A The glass for pharmaceutical containers of the present invention has a working point of preferably 1350°C or less, 1300°C or less, 1260°C or less, particularly 1250°C or less. When the working point is high, the processing temperature when processing the glass tube into an ampoule or vial becomes higher, and the evaporation of the alkaline components contained in the glass increases significantly. The evaporated alkaline components adhere to the inner wall of the glass tube, and the glass tube is processed into a glass container. Such a glass container can cause the deterioration of the medicine when it is filled and stored. In addition, in glass containing a large amount of boron, when the working point becomes high, the evaporation of boron also increases, which can cause delamination.

[0085] The glass for pharmaceutical containers of the present invention can form a compressive stress layer on its surface by subjecting it to chemical strengthening treatment. Specifically, the glass for pharmaceutical containers of the present invention has a compressive stress value of 100 MPa or more, preferably 200 MPa or more, and particularly preferably 300 MPa or more, formed when chemical strengthening (ion exchange) treatment is performed by immersing it in a KNO3 molten salt at 475°C for 7 hours. The depth of the compressive stress layer is preferably 10 μm or more, more preferably 20 μm or more, and particularly preferably 30 μm or more.

[0086] The compressive stress value (CS) and the depth from the sample surface (DOL) after chemical strengthening (ion exchange) can be measured as follows. First, both surfaces of the sample are mirror-polished, and then immersed in molten KNO3 salt at 475°C for 7 hours to perform chemical strengthening (ion exchange). Next, the surface of the sample is washed, and the compressive stress value (CS) of the compressive stress layer on the surface and the depth from the sample surface (DOL) are calculated from the number and spacing of interference fringes observed using a surface stress meter (FSM-6000, manufactured by Orihara Seisakusho Co., Ltd.). In the calculation, the refractive index of the sample is set to 1.50 and the photoelastic constant is set to 29.5 [(nm / cm) / MPa]. Although the glass composition in the surface layer of the glass is microscopically different before and after chemical strengthening, the glass composition is not substantially different when viewed as a whole glass.

[0087] Next, a method for producing the glass tube for pharmaceutical containers of the present invention will be described. The following description will be given as an example using the Danna method.

[0088] First, glass raw materials are mixed to obtain a predetermined glass composition to prepare a glass batch. Next, the glass batch is continuously fed into a melting furnace at 1550 to 1700°C to melt and refine it, and the resulting molten glass is wound around a rotating refractory while air is blown out from the tip of the refractory to draw the glass into a tube shape.

[0089] The drawn tubular glass is then cut to a predetermined length to obtain a glass tube, which is then used to manufacture vials or ampoules.

[0090] The glass tube for pharmaceutical containers of the present invention may be manufactured by any conventional method, not limited to the Danna method. For example, the Vello method or the down-draw method is effective as a manufacturing method for the glass tube for pharmaceutical containers of the present invention.

[0091] Next, a method for manufacturing the pharmaceutical container of the present invention will be described. As an example, a pharmaceutical container is manufactured by processing a glass tube using a vertical processing method.

[0092] First, a glass tube is prepared. Next, while the glass tube is vertically held, one end of the glass tube is heated with a burner, and a forming tool is used to form a shoulder and a mouth. Next, the part of the glass tube above the shoulder is heated with the burner and melted.

[0093] The cut portion is then heated with a burner to form the bottom portion, thereby obtaining a pharmaceutical container.

[0094] The fused portion of the glass tube is opened by heating with a burner and is used for the next container production. By repeating the above-mentioned forming process in this manner, a plurality of pharmaceutical containers can be obtained from the glass tube.

[0095] Furthermore, by immersing pharmaceutical containers such as ampoules and vials obtained using the glass tube for pharmaceutical containers of the present invention in a KNO3 molten salt for ion exchange, a chemically strengthened pharmaceutical container can be obtained.

[0096] The glass tube for pharmaceutical containers of the present invention can be coated on its outer surface. The coating can be made of any material selected from inorganic coatings and organic coatings, such as fluorine, silicone, and surfactants.

[0097] Furthermore, the pharmaceutical containers such as ampoules and vials obtained by using the glass tube for pharmaceutical containers of the present invention can be coated on their inner and / or outer surfaces. The coating can be made of any material selected from inorganic coatings and organic coatings such as fluorine, silicone, and surfactants. EXAMPLES

[0098] The present invention will be described below with reference to examples.

[0099] Tables 1 to 5 show examples of the present invention (Nos. 1 to 15, 17 to 63) and a comparative example (No. 16).

[0100] [Table 1]

[0101] [Table 2]

[0102] [Table 3]

[0103] [Table 4]

[0104] [Table 5] Each sample was prepared as follows.

[0105] First, a 550g batch was prepared to have the composition shown in the table, and melted in a platinum crucible at 1550°C for 2.5 hours. In order to improve the homogeneity of the sample, the sample was stirred twice during the melting process. In order to further improve the homogeneity of the sample, the glass was once water-granulated and dried, and then melted again in a platinum crucible at 1550°C for 1 hour and stirred once. In order to reduce bubbles in the sample, the sample was melted at 1600°C for 2 hours. After melting, an ingot was made, and it was processed into the shape required for measurement and subjected to various evaluations. The results are shown in Tables 1 to 3.

[0106] The hydrolysis resistance test was performed according to ISO720 (washed with acetone). The detailed test procedure is as follows. The glass sample was crushed in an alumina mortar with an alumina pestle and classified into particles with a particle size of 300 to 425 μm using a sieve. The obtained powder was washed with acetone and dried in an oven at 140 °C. 10 g of the dried powder sample was placed in a quartz flask, and 50 mL of purified water was added and the flask was covered. The quartz flask containing the sample was placed in an autoclave and treated. The treatment conditions were as follows: the temperature was raised from 100 °C to 121 °C at 1 °C / min, then held at 121 °C for 30 minutes, and then cooled to 100 °C at 0.5 °C / min. The solution in the quartz flask was transferred to another beaker, and the quartz flask was washed three times with 15 mL of purified water, and the washing water was also added to the beaker. Methyl red indicator was added to the beaker and titrated with 0.02 mol / L hydrochloric acid solution. The amount of alkaline elution was calculated by converting 1 mL of 0.02 mol / L hydrochloric acid solution into equivalent to 620 μg of Na2O, and this was used as a measurement value of hydrolysis resistance.

[0107] The alkali resistance of the glass was evaluated by a test based on ISO695.

[0108] The acid resistance of the glass was evaluated by an acid resistance test in accordance with YBB00342004.

[0109] The strain point Ps was measured using a fiber drawing method based on ASTM C336, with the glass viscosity at 10 14.5 The temperature at which the viscosity becomes Pa·s was determined.

[0110] The annealing point Ta and softening point Ts were measured using the fiber drawing method based on ASTM C388, with the glass viscosity at 10 7.6 The temperature at which the viscosity becomes dPa·s was determined.

[0111] Working point (glass viscosity is 10 4.0 dPa·s) and the glass viscosity is 10 3.0 The temperature at which the viscosity reaches dPa·s was measured using the platinum sphere pulling method.

[0112] The linear thermal expansion coefficient was measured using a glass sample molded into a rod shape of about 5 mmφ×20 mm with a dilatometer in the temperature range of 20 to 300° C.

[0113] The liquidus temperature was measured by filling a crushed glass sample into a platinum boat of about 120 x 20 x 10 mm and placing it in an electric furnace with a linear temperature gradient for 24 hours. After that, the crystal precipitation points were identified by microscopic observation, and the temperature corresponding to the crystal precipitation points was calculated from the temperature gradient graph of the electric furnace, and this temperature was taken as the liquidus temperature.

[0114] The liquidus viscosity was calculated by determining a viscosity curve of the glass from the strain point, annealing point, softening point, working temperature, and Fulcher's viscosity formula, and calculating the viscosity of the glass at the liquidus temperature from this viscosity curve. This viscosity was defined as the liquidus viscosity.

[0115] The compressive stress value (CS) and depth from the sample surface (DOL) of the samples after chemical strengthening (ion exchange) were measured using a surface stress meter (FSM-6000, manufactured by Orihara Seisakusho Co., Ltd.).

[0116] As is clear from Tables 1 to 5, the examples of the present invention had a working point of 1,321° C. or less and an alkali elution amount of 58.9 μg / g or less in the hydrolysis resistance test. [Industrial Applicability]

[0117] The glass for pharmaceutical containers of the present invention is suitable as glass for producing pharmaceutical containers such as ampoules, vials, prefilled syringes, cartridges, etc. It can also be applied to pharmaceutical containers for oral drugs and beverage bottles.

Claims

1. The glass composition is, in mol%, SiO 2 70-85%, Al 2 O 3 3-20%, B 2 O 3 0-4%, Li 2 O 0-5%, Na 2 O 0-12%, K 2 O 0-6%, Li 2 O+Na 2 O+K 2 O 0.1-26%, SrO 0-1%, BaO 0-1%, molar ratio K 2 O / (Li 2 O+Na 2 O+K 2 O) is 0.24 or less, and the molar ratio of Al 2 O 3 / (Li 2 O+Na 2 O+K 2 O) is 50 or less, and the molar ratio SiO 2 / (Li 2 O+Na 2 O+K 2 1. A glass for pharmaceutical containers, characterized in that the value of MgO / (MgO+CaO+SrO+BaO) is 6.5 or less and the value of the molar ratio MgO / (MgO+CaO+SrO+BaO) is 0.8 or less.

2. 2. The glass for pharmaceutical containers according to claim 1, characterized in that the glass composition satisfies, in mol %, CaO≧MgO.

3. The glass composition is, in mole percent, Na 2 O 0-7.9%, K 2 3. The glass for pharmaceutical containers according to claim 1, further comprising 0 to 3% O.

4. 4. The glass for pharmaceutical containers according to claim 1, characterized in that it contains, in mole percent, 0-0.5% MgO, 0-0.5% CaO, 0-0.3% SrO, and 0-0.3% BaO as a glass composition.

5. B 2 O 3 5. The glass for pharmaceutical containers according to claim 1, wherein the content of is 0.01 to 1 mol %.

6. ZrO 2 6. The glass for pharmaceutical containers according to claim 1, wherein the content of is 0 to 2 mol %.

7. 7. The glass for pharmaceutical containers according to claim 1, characterized in that its class in a hydrolysis resistance test (washed with acetone) in accordance with ISO 720 is at least HGA1.

8. 8. The glass for pharmaceutical containers according to claim 1, wherein the working point is 1,300° C. or lower.

9. A glass tube for pharmaceutical containers, comprising the glass for pharmaceutical containers according to any one of claims 1 to 8.

10. A pharmaceutical container comprising the glass for pharmaceutical containers according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Alkaline earth aluminosilicate glass composition with improved chemical and mechanical durability

    JP2015501280A

  • Glass for pharmaceutical containers, glass tube for pharmaceutical containers and pharmaceutical containers using the same

    JP7530047B2