Electrostatic charge image developer, developer cartridge, process cartridge, image forming apparatus, and image forming method
By employing toner particles with controlled viscoelastic properties and a carrier with defined surface characteristics, the electrostatic image developer ensures consistent glossiness and reduces fogging across varying fixing conditions, addressing the inconsistencies in existing technologies.
Patent Information
- Application Number
- JP2023043886
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Existing electrostatic image developers exhibit significant differences in glossiness and are prone to fogging when images are fixed under varying temperature and pressure conditions, leading to inconsistent image quality.
The developer includes toner particles with specific viscoelastic properties and a carrier with controlled surface roughness, ensuring consistent glossiness and reduced fogging across different fixing conditions by using toner particles with controlled loss tangent values and a carrier with defined unevenness and roughness parameters.
The solution achieves a small difference in glossiness and suppresses fogging, providing consistent image quality under both low and high temperature and pressure fixing conditions.
Smart Images

Figure 2024133884000006 
Figure 2024133884000007 
Figure 2024133884000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrostatic image developer, a developer cartridge, a process cartridge, an image forming apparatus, and an image forming method. [Background technology]
[0002] Patent Document 1 discloses a developer using a toner for developing electrostatic latent images, which contains toner particles containing a binder resin, the binder resin containing an amorphous resin and a crystalline resin, and which is obtained by performing a strain dispersion measurement of dynamic viscoelasticity under conditions of a temperature of 130° C., a frequency of 1 Hz, and a strain amplitude of 1.0 to 500%, and in which, when the integral value of the stress in a stress-strain curve at a strain amplitude of 100% is S130 and the slope of the major axis is θ130, the S130 is more than 0 Pa and 350,000 Pa or less, and the θ130 is more than 22° and less than 90°.
[0003] Patent Document 2 discloses a developer using a toner for developing electrostatic images, which contains at least a binder resin and a release agent, the binder resin containing at least a crystalline resin, and whose storage modulus, measured at a frequency of 1 Hz and at 150° C. while changing the strain from 0.01% to 1000%, satisfies a specific relationship.
[0004] Patent Document 3 discloses a developer using a toner for developing electrostatic latent images, which contains toner particles containing a binder resin, the binder resin containing an amorphous vinyl resin and a crystalline resin, and which is obtained by performing a strain dispersion measurement of dynamic viscoelasticity under conditions of a temperature of 130° C., a frequency of 1 Hz, and a strain amplitude of 1.0 to 500%, where S130 is the integral value of the stress in a stress-strain curve at a strain amplitude of 100%, and θ130 is the slope of the major axis, and S130 is more than 0 Pa and 350,000 Pa or less, and θ130 is 0° or more and less than 10°.
[0005] Patent Document 4 discloses a developer using a toner for developing electrostatic images, which contains toner base particles containing at least a binder resin and a release agent, and an external additive, wherein the binder resin contains at least a crystalline resin, and the peak top value of the loss tangent, tan δ6°C / min, when measured from 25°C to 100°C under conditions of a frequency of 1 Hz and a temperature rise rate of 6°C / min, and the peak top value of the loss tangent, tan δ3°C / min, when measured from 25°C to 100°C under conditions of a frequency of 1 Hz and a temperature rise rate of 3°C / min, satisfy a specific relationship.
[0006] Patent Document 5 describes a polymer film containing at least a binder resin, a colorant, and a release agent, in which the rate of change γG' of storage modulus G' is 50%<γG'<86%, and the rate of change γG" of loss modulus G" is greater than 50%, and the storage modulus G' in the range of 1 to 50% strain at a temperature of 150°C is 5×10 2 ~3.5×10 3 The binder resin is a toner for developing electrostatic images, the binder resin containing a non-crystalline resin and a crystalline resin.
[0007] Patent Documents 6 and 7 disclose a developer using a toner for developing electrostatic images, which is composed of toner particles containing a binder resin, and which is characterized in that, in an elasticity image of a cross section of the toner particle taken with an atomic force microscope (AFM), the binder resin has a domain-matrix structure composed of a high elasticity resin constituting the domains and a low elasticity resin constituting the matrix, the arithmetic mean value of the ratio (L / W) of the major axis L to the minor axis W of each domain is within the range of 1.5 to 5.0, 80% or more of the domains have a major axis L within the range of 60 to 500 nm, and 80% or more of the domains have a minor axis W within the range of 45 to 100 nm. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2020-042122 A [Patent Document 2] JP 2020-106685 A [Patent Document 3] JP 2020-042121 A [Patent Document 4] JP 2019-144368 A [Patent Document 5] JP 2013-160886 A [Patent Document 6] JP 2011-237793 A [Patent Document 7] JP 2011-237792 A Summary of the Invention [Problem to be solved by the invention]
[0009] In image formation using an electrostatic image developer containing a toner, for example, a toner image transferred to a recording medium is fixed to the recording medium by heating and pressurization. When an electrostatic image developer containing a toner that is easily melted by heating is used to obtain good fixability, the difference in glossiness between a fixed image fixed under high temperature and high pressure conditions and a fixed image fixed under low temperature and low pressure conditions may become large. In addition, when an electrostatic image developer containing a toner that is easily melted by heating is used, fogging may occur on the image.
[0010] The object of the present invention is to provide an electrostatic image developer in which the difference in gloss between an image fixed under low-temperature and low-pressure conditions and an image fixed under high-temperature and high-pressure conditions is smaller and image fog is suppressed, as compared with cases in which any of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of 50(90)-D1(90) is 1.0 or more, the average irregularity spacing Sm is less than 0.5 μm or exceeds 2.5 μm, or the arithmetic mean roughness Ra is less than 0.3 μm or exceeds 1.2 μm. [Means for solving the problem]
[0011] The above problems are solved by the following means:
[0012] <1> a toner including toner particles containing a binder resin, wherein, in a dynamic viscoelasticity measurement of the toner, when a loss tangent tanδ at a temperature of 90°C and a distortion of 1% is D1(90), a loss tangent tanδ at a temperature of 90°C and a distortion of 50% is D50(90), a loss tangent tanδ at a temperature of 150°C and a distortion of 1% is D1(150), and a loss tangent tanδ at a temperature of 150°C and a distortion of 50% is D50(150), D1(90), D50(90), D1(150), and D50(150) are each 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0; a carrier including magnetic particles having a mean irregularity distance Sm and an arithmetic mean roughness Ra on the surface that satisfy the conditions of 0.5 μm≦Sm≦2.5 μm and 0.3 μm≦Ra≦1.2 μm, and a resin layer adhered to the surface of the magnetic particles; An electrostatic image developer comprising:
[0013] <2> The relationship between the D1(90) and the average irregularity spacing Sm satisfies the following formula (1): <1> Electrostatic image developer according to claim 1. Formula (1): D1(90)≦Sm≦D1(90)+1.1 <3> The relationship between the D1(90) and the arithmetic average roughness Ra satisfies the following formula (2): <1> or <2> Electrostatic image developer according to claim 1. Formula (2): 1.05-0.3×D1(90)≦Ra≦1.36-0.3×D1(90) <4> The relationship between the D50(150) and the arithmetic average roughness Ra satisfies the following formula (3): <3> Electrostatic image developer according to claim 1. Formula (3): 1.05-0.3×D50(150)≦Ra≦1.36-0.3×D50(150) <5> an exposed area ratio of the magnetic particles on the surface of the carrier is 4% or more and 20% or less; <1> ~ <4> 13. The electrostatic image developer according to claim 12,
[0014] <6> The toner particles further contain resin particles. <1> ~ <5> 13. The electrostatic image developer according to claim 12, <7> The resin particles are crosslinked resin particles. <6> Electrostatic image developer according to claim 1. <8> The crosslinked resin particles are styrene (meth)acrylic resin particles. <7> Electrostatic image developer according to claim 1. <9> the number average molecular weight of the tetrahydrofuran soluble matter in the toner particles is 5,000 or more and 15,000 or less; <1> ~ <8> 13. The electrostatic image developer according to claim 12,
[0015] <10> <1> ~ <9> The electrostatic image developer according to any one of claims 1 to 5 is contained as a replenishment developer, A developer cartridge that is detachably attached to an image forming apparatus. <11> <10> a developer cartridge according to claim 1, a developing device that contains an electrostatic image developer including a replenishment developer replenished from the developer cartridge and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer; The process cartridge is detachably mounted to the image forming apparatus. <12> <10> a developer cartridge according to claim 1, An image carrier; a charging device for charging the surface of the image carrier; an electrostatic image forming device for forming an electrostatic image on the charged surface of the image carrier; a developing device that contains an electrostatic image developer including a replenishment developer replenished from the developer cartridge and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer device for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing device for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: <13> a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; <10> a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using an electrostatic image developer containing a replenishment developer replenished from the developer cartridge described in claim 1; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,
[0016] <14> <1> ~ <9> and a developing device that contains the electrostatic image developer according to any one of claims 1 to 5 and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer, A process cartridge that is detachably attached to an image forming apparatus. <15> An image carrier; a charging device for charging the surface of the image carrier; an electrostatic image forming device for forming an electrostatic image on the charged surface of the image carrier; <1> ~ <9> a developing device that contains the electrostatic image developer according to any one of claims 1 to 5 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer device for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing device for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: <16> a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; <1> ~ <9> a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to any one of the above items; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1, Effect of the Invention
[0017] <1> or <6> According to the invention relating to the above, there is provided an electrostatic image developer in which the difference in gloss between an image fixed under low-temperature and low-pressure conditions and an image fixed under high-temperature and high-pressure conditions is smaller and image fog is suppressed, as compared with a case in which any of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of 50(90)-D1(90) is 1.0 or more, the average irregularity spacing Sm is less than 0.5 μm or exceeds 2.5 μm, or the arithmetic mean roughness Ra is less than 0.3 μm or exceeds 1.2 μm.
[0018] <2> According to the present invention, there is provided an electrostatic image developer in which image fogging is suppressed compared to a case in which the relationship between D1(90) and the average irregularity spacing Sm does not satisfy formula (1). <3> According to the present invention, there is provided an electrostatic image developer in which image fogging is suppressed compared to a case in which the relationship between D1(90) and the arithmetic mean roughness Ra does not satisfy formula (2). <4> According to the present invention, there is provided an electrostatic image developer in which image fogging is suppressed compared to a case in which the relationship between D50(150) and the arithmetic mean roughness Ra does not satisfy formula (3). <5> According to the present invention, there is provided an electrostatic image developer in which image fogging is suppressed compared to when the exposed area ratio of the magnetic particles on the carrier surface is less than 4% or exceeds 20%.
[0019] <7> According to the invention, there is provided a toner for developing electrostatic images which has a smaller difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions, as compared with a case in which the resin particles are non-crosslinked resin particles. <8> According to the invention, there is provided a toner for developing electrostatic images which has a smaller difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions, as compared with a case in which the crosslinked resin particles are polyester resin particles. <9> According to the invention, an electrostatic image developer is provided in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller than when the number average molecular weight of the tetrahydrofuran soluble matter is less than 5,000 or exceeds 15,000.
[0020] <10> , <11> , <12> or <13> According to the invention, any one of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of D50(90)-D1(90) is 1.0 or more, the average irregularity spacing Sm is less than 0.5 μm or exceeds 2.5 μm, the arithmetic mean roughness Ra is less than 0.3 μm or exceeds 1.2 μm, and the BET specific surface area of the carrier is 0.12 m 2 / g or less than 0.20m 2 The present invention provides a developer cartridge, process cartridge, image forming apparatus, or image forming method in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is small and image fogging is suppressed, as compared with the case where an electrostatic image developer having a carrier volume average particle size of more than 26 μm or more than 34 μm is used.
[0021] <14> , <15> or <16> According to the invention, any one of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of D50(90)-D1(90) is 1.0 or more, the average irregularity spacing Sm is less than 0.5 μm or exceeds 2.5 μm, the arithmetic mean roughness Ra is less than 0.3 μm or exceeds 1.2 μm, and the BET specific surface area of the carrier is 0.12 m 2 / g or less than 0.20m 2The present invention provides a process cartridge, an image forming apparatus, or an image forming method in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller and image fogging is suppressed, as compared to the case in which an electrostatic charge image developer having a viscosity of more than 1000 saturation voltage Vp-value ... [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic configuration diagram illustrating another example of an image forming apparatus according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present invention will be described as an example. The description and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the present invention. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. In this specification, (meth)acrylic means both acrylic and methacrylic.
[0024] In this specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.
[0025] [Electrostatic image developer] The electrostatic image developer (hereinafter also referred to as "developer") according to the present embodiment is a toner including toner particles containing a binder resin, and in a dynamic viscoelasticity measurement of the toner, when the loss tangent tanδ at a temperature of 90°C and a distortion of 1% is D1(90), the loss tangent tanδ at a temperature of 90°C and a distortion of 50% is D50(90), the loss tangent tanδ at a temperature of 150°C and a distortion of 1% is D1(150), and the loss tangent tanδ at a temperature of 150°C and a distortion of 50% is D50(150), and a toner having a D50(90), D50(90), D1(150), and D50(150) of 0.5 or more and 2.5 or less, with the value of D50(150)-D1(150) being less than 1.5 and the value of D50(90)-D1(90) being less than 1.0; and a carrier including magnetic particles having a mean irregularity spacing Sm and an arithmetic mean roughness Ra on the surface that satisfy 0.5 μm≦Sm≦2.5 μm and 0.3 μm≦Ra≦1.2 μm, and a resin layer adhered to the surfaces of the magnetic particles. Hereinafter, a toner having D1(90), D50(90), D1(150), and D50(150) each being 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) being less than 1.5, and the value of D50(90)-D1(90) being less than 1.0 will be referred to as a "specific toner", magnetic particles having a mean irregularity spacing Sm and an arithmetic mean roughness Ra on the surface that satisfy 0.5 μm≦Sm≦2.5 μm and 0.3 μm≦Ra≦1.2 μm will be referred to as a "specific magnetic particle", and a carrier containing specific magnetic particles and a resin layer will be referred to as a "specific carrier".
[0026] The developer according to the present embodiment has the above-mentioned configuration, which reduces the difference in glossiness between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions, and suppresses image fogging. The reason for this is presumed to be as follows. Hereinafter, the difference in glossiness between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is also referred to as the "glossiness condition difference."
[0027] As described above, in order to obtain good fixing properties, it is considered to use a developer containing a toner that is easily melted by heating. On the other hand, when an image is formed using a developer containing a toner that is easily melted by heating, the gloss condition difference may become large. This is presumably because the deformation amount of toner particles at high temperature and high strain amount is larger than the deformation amount of toner particles at low temperature and low strain amount.
[0028] In addition, when an image is formed using a developer containing a toner that is easily melted by heating, fogging may occur on the image. For example, if vibration is applied during transportation of a developer containing toner and a carrier, the carrier sinks under its own weight, which puts pressure on the toner, causing the toner particles to deform and reducing the chargeability of the toner, which may lead to fogging. In particular, if a developer cartridge containing a refill developer containing toner and a carrier is placed vertically with the developer outlet facing down and is subjected to vibration during transportation, the carrier sinks under its own weight and tends to gather near the developer outlet. Then, when the collected carrier and toner are supplied to the developing device at once, the toner cannot be charged quickly enough, which may lead to fogging.
[0029] In contrast, in this embodiment, a specific toner is used, that is, a toner in which D1(90), D50(90), D1(150), and D50(150) are each 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0. Here, a strain of 1% in dynamic viscoelasticity measurement means that a displacement of 1% is applied relative to the height of the sample (i.e., the gap). In other words, a strain of 1% is the application of a small amount of displacement, and corresponds to a case where the fixing device pressure is low in the toner fixing process. On the other hand, a strain of 50% corresponds to a case where the fixing device pressure is high in the toner fixing process. A temperature of 90°C and a strain of 1% correspond to fixing conditions at low temperature and low pressure, and a temperature of 150°C and a strain of 50% correspond to fixing conditions at high temperature and high pressure, and each loss tangent tan δ corresponds to the amount of toner deformation under each fixing condition. In the specific toner, the change in loss tangent relative to the change in the amount of distortion is small both at 90° C. and 150° C. Therefore, it is presumed that the toner has similar viscoelasticity at high temperature and high distortion and at low temperature and low distortion, so that even when an image is fixed under high temperature and high pressure conditions, a fixed image having a small difference in gloss compared to an image fixed under low temperature and low pressure conditions can be obtained.
[0030] In this embodiment, a specific toner having D1(90), D50(90), D1(150), and D50(150) all being 0.5 or more and 2.5 or less is used in combination with a specific carrier using specific magnetic particles that satisfy 0.5 μm≦Sm≦2.5 μm and 0.3 μm≦Ra≦1.2 μm. The combination of this carrier having appropriate unevenness and a toner having appropriate viscoelasticity makes it easier for the fine unevenness on the carrier surface to be appropriately caught by the toner surface. Therefore, it is presumed that even if the developer is vibrated, the carrier is prevented from sinking under its own weight, making it less likely for image fogging to occur.
[0031] For the above reasons, it is presumed that in this embodiment, the difference in gloss condition is small and image fog is suppressed.
[0032] The loss tangent of the toner is determined as follows. Specifically, a measurement sample is prepared by molding the toner to be measured into a tablet shape at room temperature (25° C.) using a press molding machine. Then, using this measurement sample, dynamic viscoelasticity measurement is performed using a rheometer under the following conditions, and the loss tangent tanδ at a temperature of 90° C. or 150° C. and a strain of 1% or 50% is obtained from each of the obtained curves of the storage modulus and loss modulus, to obtain D1(90), D50(90), D1(150), and D50(150). -Measurement conditions- Measurement device: Rheometer ARES-G2 (manufactured by TA Instruments) Measurement jig: 8mm parallel plate Gap: Adjusted to 3mm Frequency: 1Hz
[0033] The method for obtaining the specific toner is not particularly limited. As a method for obtaining the specific toner, for example, a toner having a storage modulus G' of 1×10 in the range of 90° C. to 150° C. in dynamic viscoelasticity measurement at a temperature rise of 2° C. / min is 4 Pa or more 1×10 6 One method is to incorporate resin particles having a surface roughness of not more than 1 Pa evenly into both the region close to the surface and the region close to the center of the toner particle. The storage modulus G' in the range of 90°C to 150°C is 1×10 4 Pa or more 1×10 6 Resin particles having a viscosity of 0.1 Pa or less are also referred to as "specific resin particles". The reason why the specific toner can be easily obtained by dispersing the specific resin particles evenly in both the region close to the surface of the toner particle and the region close to the center of the toner particle is not clear, but is presumed to be as follows.
[0034] As mentioned above, the specific resin particles have a storage modulus G' of 1×10 4 The specific resin particles are particles having a high elastic modulus at high temperatures. Therefore, it is presumed that the toner particles contain the specific resin particles, so that the loss tangent of the toner as a whole at high temperature and high strain is unlikely to be high, and the difference with the loss tangent of the toner as a whole at low temperature and low strain is small. In particular, it is presumed that by dispersing specific resin particles evenly in both the region close to the surface of the toner particle and the region close to the center of the toner particle, the loss tangent of the toner at both low temperature, low distortion and high temperature, high distortion is reduced, and the difference between the two is also reduced, making it easier to obtain a specific toner.
[0035] The storage modulus G' of the resin particles, as well as the loss tangent tan δ and the glass transition temperature Tg, which will be described later, are determined as follows. Specifically, a disk-shaped sample with a thickness of 2 mm and a diameter of 8 mm is prepared by applying pressure to the resin particles to be measured, and used as the measurement sample. When measuring the resin particles contained in the toner particles, the resin particles are removed from the toner particles before preparing the measurement sample. Examples of methods for removing the resin particles from the toner particles include a method in which the toner particles are immersed in a solvent that dissolves the binder resin but not the resin particles, and the binder resin is dissolved in the solvent to remove the resin particles. The obtained disk-shaped sample is sandwiched between parallel plates with a diameter of 8 mm, and the measurement temperature is raised from 10°C to 150°C at a rate of 2°C / min with a strain of 0.1 to 100%, to perform dynamic viscoelasticity measurement under the following conditions. The storage modulus G' and loss tangent tanδ are obtained from the curves of the storage modulus and loss modulus obtained by the measurement. The peak temperature of the loss tangent tanδ is defined as the glass transition temperature Tg. -Measurement conditions- Measurement device: Rheometer ARES-G2 (manufactured by TA Instruments) Gap: Adjusted to 3mm Frequency: 1Hz
[0036] The specific method for measuring the average irregularity spacing Sm and the arithmetic mean roughness Ra of the magnetic particle surface of the above carrier is to use an ultra-depth color 3D shape measuring microscope (VK-9500, manufactured by Keyence Corporation) to measure the surface of 50 magnetic particles at a magnification of 3,000 times. The average irregularity spacing Sm is calculated by calculating a roughness curve from the three-dimensional shape of the observed magnetic particle surface, and calculating the average value of the spacing of one period of peaks and valleys from the intersection point where the roughness curve intersects with the average line. The reference length for calculating the Sm value is 10 μm, and the cutoff value is 0.08 mm. The arithmetic mean roughness Ra is calculated by obtaining a roughness curve, adding up and averaging the absolute values of the deviations from the measured values of the roughness curve to the average value, and then calculating the Ra value. The reference length for calculating the Ra value is 10 μm, and the cutoff value is 0.08 mm. The Sm and Ra values are measured in accordance with JIS B0601 (1994 edition).
[0037] A suitable method for separating the magnetic particles from the carrier is to dissolve the resin coating layer with an organic solvent and separate the magnetic particles. As a more specific example of a method for separating magnetic particles from a carrier, for example, 20 g of resin-coated carrier is placed in 100 mL of toluene. Ultrasonic waves are applied at 40 kHz for 30 seconds. The magnetic particles and resin solution are separated using any filter paper according to the particle size. 20 mL of toluene is poured over the magnetic particles remaining on the filter paper to wash them. Next, the magnetic particles remaining on the filter paper are collected. The collected magnetic particles are similarly placed in 100 mL of toluene and ultrasonic waves are applied at 40 kHz for 30 seconds. Filter in the same manner, wash with 20 mL of toluene, and then collect. This is repeated a total of 10 times. Finally, the collected magnetic particles are dried.
[0038] The method for controlling the mean spacing Sm and the arithmetic mean roughness Ra of the magnetic particles is not particularly limited. The mean spacing Sm of the magnetic particles and the arithmetic mean roughness Ra are controlled, for example, by adjusting the temperature during the main sintering, adjusting the oxygen concentration during the main sintering, the amount of SiO2 added, and adding at least one component selected from the group consisting of a Ca component and a Sr component.
[0039] In this embodiment, in order to reduce the difference in glossiness conditions and suppress fogging in an image, the BET specific surface area of the magnetic particles is set to 0.12 m 2 / g or more 0.20m 2 / g or less. In this embodiment, from the viewpoint of reducing the gloss condition difference and suppressing image fogging, it is preferable that the volume average particle size of the magnetic particles is 26 μm or more and 34 μm or less.
[0040] The BET specific surface area of the magnetic particles is measured using a SA3100 specific surface area measuring device (manufactured by Beckman Coulter) with nitrogen substitution and a three-point method. Specifically, 5 g of magnetic particles are placed in a cell, degassed at 60°C for 120 minutes, and then a mixed gas of nitrogen and helium (30:70) is used. The volume average particle diameter of the magnetic particles and the carrier described later is a value measured by a laser diffraction particle size distribution measuring device LA-700 (manufactured by Horiba, Ltd.). Specifically, for the particle size ranges (channels) into which the particle size distribution obtained by the measuring device is divided, the particle diameter at which the cumulative volume distribution is subtracted from the small particle size side and the cumulative 50% is defined as the volume average particle diameter.
[0041] The method for controlling the BET specific surface area and volume average particle size of the magnetic particles is not particularly limited. The BET specific surface area of the magnetic particles is controlled, for example, by adjusting the temperature during sintering, adjusting the oxygen concentration during sintering, the amount of SiO2 added, adding at least one component selected from the group consisting of a Ca component and a Sr component, post-heating after sintering, etc. The volume average particle size of the magnetic particles is controlled, for example, by controlling the particle size during granulation such as spray drying, crushing and classification after sintering, etc.
[0042] The toner and carrier contained in the developer according to this embodiment will be described in detail below.
[0043] <Toner> The toner according to the present embodiment is configured to contain toner particles and, if necessary, an external additive.
[0044] (Toner particles) The toner particles contain at least a binder resin, and may contain other components as necessary. The toner particles preferably further contain resin particles in addition to the binder resin. Furthermore, it is presumed that the toner particles contain resin particles, so that the amount of deformation of the toner fixed image due to the fixing pressure is suppressed, and a fixed image with a small difference in glossiness can be obtained.
[0045] The resin particles are preferably crosslinked resin particles. The term "crosslinked resin particles" as used herein refers to resin particles having a bridge structure between specific atoms in the polymer structure contained in the resin particles. By using crosslinked resin particles as the resin particles, the specific resin particles tend to have a storage modulus G' within the above range at temperatures of 90° C. or higher and 150° C. or lower, and the specific toner tends to be obtained.
[0046] The crosslinked resin particles are preferably styrene (meth)acrylic resin particles. When the crosslinked resin particles are styrene (meth)acrylic resin particles, the specific resin particles tend to have a storage modulus G' within the above range at 90° C. or higher and 150° C. or lower, and the specific toner tends to be obtained.
[0047] As described above, from the viewpoint of obtaining a specific toner, the toner particles preferably contain specific resin particles as the resin particles. Hereinafter, as an example of the toner particles contained in the specific toner, toner particles containing a binder resin and specific resin particles will be described. The toner particles are composed of, for example, a binder resin, specific resin particles, and, if necessary, a colorant, a release agent, and other additives.
[0048] -Binding resin- Examples of the binder resin include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers. Examples of the binder resin include non-vinyl resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.
[0049] The binder resin preferably contains a polyester resin. By including a polyester resin as the binder resin, when styrene (meth)acrylic resin particles are used as the specific resin particles, the difference (SP value (S)-SP value (R)) between the solubility parameter SP value (S) of the specific resin particles described later and the solubility parameter SP value (R) of the binder resin tends to be within a preferred numerical range. This makes it easier for the specific resin particles to disperse in the toner particles, and as a result, the gloss condition difference is reduced. By having the difference (SP value (S)-SP value (R)) in the above range, the affinity between the binder resin and the specific resin particles is high, which prevents partial compatibility and a decrease in dispersibility, compared to when the difference is too small. Also, by having the difference (SP value (S)-SP value (R)) in the above range, the affinity between the binder resin and the specific resin particles is low, which prevents the specific resin particles from being encapsulated within the toner particles and being discharged to the surface of the toner particles or outside the toner particles, compared to when the difference is too large.
[0050] The binder resin preferably contains a crystalline resin and an amorphous resin. Here, the crystalline resin refers to a resin that has a clear endothermic peak rather than a stepwise change in endothermic amount in differential scanning calorimetry (DSC). On the other hand, an amorphous resin is one that, in thermal analysis measurement using differential scanning calorimetry (DSC), has only a step-like endothermic change rather than a clear endothermic peak, is a solid at room temperature, and becomes thermoplastic at a temperature equal to or higher than the glass transition temperature. Specifically, for example, a crystalline resin means a resin whose half-width of an endothermic peak is within 10°C when measured at a heating rate of 10°C / min, and an amorphous resin means a resin whose half-width exceeds 10°C or a resin in which no clear endothermic peak is observed.
[0051] The crystalline resin will now be described. The crystalline resin may be a crystalline polyester resin, a crystalline vinyl resin (e.g., polyal Examples of the crystalline resin include known crystalline resins such as xylene resins and long-chain alkyl (meth)acrylate resins. Among these, crystalline polyester resins are preferred from the viewpoints of the mechanical strength and low-temperature fixability of the toner.
[0052] Crystalline polyester resin The crystalline polyester resin may be, for example, a polycondensate of a polyvalent carboxylic acid and a polyhydric alcohol. The crystalline polyester resin may be a commercially available product or a synthesized product. Here, the crystalline polyester resin is preferably a polycondensate using a polymerizable monomer having a linear aliphatic group rather than a polymerizable monomer having an aromatic group, since the crystalline polyester resin can easily form a crystalline structure.
[0053] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids (e.g., 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, etc.), their anhydrides, and their lower alkyl esters (e.g., carbon number 1 to 5). As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0054] Examples of polyhydric alcohols include aliphatic diols (for example, straight-chain aliphatic diols having 7 to 20 carbon atoms in the main chain). Examples of aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred as aliphatic diols. The polyhydric alcohol may be a trihydric or higher alcohol having a crosslinked or branched structure in combination with the diol. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0055] Here, the polyhydric alcohol has an aliphatic diol content of 80 mol % or more, preferably 90 mol % or more.
[0056] The melting temperature of the crystalline polyester resin is preferably 50°C or higher and 100°C or lower, more preferably 55°C or higher and 90°C or lower, and even more preferably 60°C or higher and 85°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."
[0057] The weight average molecular weight (Mw) of the crystalline polyester resin is preferably 6,000 or more and 35,000 or less.
[0058] The crystalline polyester resin can be obtained by a known manufacturing method, for example, in the same manner as the amorphous polyester.
[0059] When the toner particles contain a crystalline resin, the content of the crystalline resin relative to the total binder resin is preferably 4% by mass or more and 50% by mass or less, more preferably 6% by mass or more and 30% by mass or less, and even more preferably 8% by mass or more and 20% by mass or less. By having the crystalline resin content in the above range, better fixability is easily obtained compared to when the content is less than the above range. Also, by having the crystalline resin content in the above range, compared to when the content is more than the above range, the glossiness of the fixed image fixed under high temperature and high pressure conditions is prevented from excessively increasing due to the relatively low elasticity crystalline resin being too much. As a result, the glossiness condition difference is reduced.
[0060] The amorphous resin will now be described. Examples of the amorphous resin include known amorphous resins such as amorphous polyester resin, amorphous vinyl resin (e.g., styrene-acrylic resin, etc.), epoxy resin, polycarbonate resin, polyurethane resin, etc. Among these, amorphous polyester resin and amorphous vinyl resin (particularly styrene-acrylic resin) are preferred, and amorphous polyester resin is more preferred.
[0061] Amorphous polyester resin The amorphous polyester resin may be, for example, a condensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol. The amorphous polyester resin may be a commercially available product or a synthesized product.
[0062] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). Among these, aromatic dicarboxylic acids are preferable as polyvalent carboxylic acids. The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower (e.g., carbon number 1 to 5) alkyl esters thereof. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0063] Examples of polyhydric alcohols include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, examples of polyhydric alcohols include aromatic diols and alicyclic diols, and more preferably aromatic diols. As the polyhydric alcohol, a polyhydric alcohol having a crosslinked or branched structure of three or more may be used in combination with the diol. Examples of the polyhydric alcohol having a trihydric or higher valence include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0064] The glass transition temperature (Tg) of the amorphous polyester resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower. The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), more specifically, from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."
[0065] The weight average molecular weight (Mw) of the amorphous polyester resin is preferably 5,000 or more and 1,000,000 or less, and more preferably 7,000 or more and 500,000 or less. The number average molecular weight (Mn) of the amorphous polyester resin is preferably 2,000 or more and 100,000 or less. The molecular weight distribution Mw / Mn of the amorphous polyester resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less. The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.
[0066] The amorphous polyester resin can be obtained by a known manufacturing method, for example, by carrying out the reaction while removing water and alcohol generated during condensation by setting the polymerization temperature to 180° C. or higher and 230° C. or lower, and reducing the pressure in the reaction system as necessary. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a solubilizing agent to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.
[0067] The binder resin preferably contains a polyester resin having an aliphatic dicarboxylic acid unit (i.e., a structural unit derived from an aliphatic dicarboxylic acid). When the polyester resin, which is the binder resin, has an aliphatic dicarboxylic acid unit, the flexibility of the binder resin is increased compared to when the binder resin has only an aromatic dicarboxylic acid unit, so that the specific resin particles can be dispersed in a state closer to uniformity, and the variation range of the loss tangent tanδ can be reduced.
[0068] In addition, the binder resin preferably contains an amorphous polyester resin having an aliphatic dicarboxylic acid unit and a crystalline polyester resin having an aliphatic dicarboxylic acid unit. When the binder resin contains an amorphous polyester resin and a crystalline polyester resin, the specific resin particles can be more uniformly dispersed by both of them having an aliphatic dicarboxylic acid unit.
[0069] In addition, examples of the aliphatic dicarboxylic acid include the dicarboxylic acid represented by the general formula "HOOC-(CH2) n In the above general formula, n is preferably 4 to 20, and more preferably 4 to 12.
[0070] The content of the binder resin is, for example, preferably from 40% by mass to 95% by mass, more preferably from 50% by mass to 90% by mass, and even more preferably from 60% by mass to 85% by mass, based on the total amount of the toner particles.
[0071] The ratio of the content of the crystalline resin to the content of the specific resin particles is preferably 0.2 or more and 10 or less, and more preferably 1 or more and 5 or less, assuming that the content of the specific resin particles is 1. By keeping the ratio of the crystalline resin content to the specific resin particle content within the above range, compared to when the ratio is less than 0.2, the amount of low-viscosity components in the toner at temperatures between 90°C and 150°C and the contribution of the specific resin particles, which are highly elastic components, is increased, thereby suppressing the decrease in the melting property of the toner and improving the fixing property. In addition, by keeping the ratio of the crystalline resin content to the specific resin particle content within the above range, the amount of reduced components is prevented from becoming excessive, which would result in an increase in the amount of deformation of the toner due to the heat and pressure applied by the fixing device, compared to when the ratio exceeds 10, and the difference in glossiness due to fixing conditions is reduced. The ratio of the content of the amorphous resin to the content of the specific resin particles is preferably 1.3 or more and 45 or less, and more preferably 3 or more and 15 or less, assuming that the content of the specific resin particles is 1.
[0072] -Specific resin particles- The specific resin particles have a storage modulus G' of 1 x 10 in the range of 90°C to 150°C in dynamic viscoelasticity measurement at a temperature rise of 2°C / min. 4 Pa or more 1×10 6 There are no particular limitations on the resin particles as long as they have a modulus of 0.1 Pa or less. The storage modulus G' of the specific resin particles in the range of 90°C to 150°C is 1×10 5 Pa or more 8×10 5 Pa or less, and 1×10 5 Pa or more 6×10 5 It is more preferable that the pressure is 0.1 Pa or less. By using resin particles having a storage modulus G' in the range of 90°C to 150°C in the above range, excessive increase in glossiness of the fixed image fixed under high temperature and high pressure conditions is suppressed compared to the case where resin particles having a lower storage modulus G' than the above range are used. This reduces the glossiness condition difference. In addition, by using resin particles having a storage modulus G' in the range of 90°C to 150°C in the above range, deterioration of fixability caused by the elasticity of the toner particles being too high is suppressed compared to the case where resin particles having a higher storage modulus G' than the above range are used, and good fixability is easily obtained.
[0073] The specific resin particles preferably have a loss tangent tanδ of 0.01 to 2.5 in the range of 30° C. to 150° C. in dynamic viscoelasticity measurement at a temperature rise rate of 2° C. / min. The specific resin particles more preferably have a loss tangent tanδ of 0.01 to 1.0 in the range of 65° C. to 150° C., and even more preferably have a loss tangent tanδ of 0.01 to 0.5 in the range of 65° C. to 150° C. By setting the loss tangent tanδ of the specific resin particles in the above range in the range of 30° C. to 150° C., the toner particles are more likely to deform during fixing, and good fixing properties are more likely to be obtained, compared to when the temperature is lower than the above range. Furthermore, by setting the loss tangent tanδ of the specific resin particles in the above range in the range of 65° C. to 150° C., which is the temperature at which the toner particles are more likely to deform, the glossiness of the fixed image fixed under high temperature and high pressure conditions is suppressed from increasing excessively, compared to when the temperature is higher than the above range. This reduces the difference in glossiness conditions.
[0074] ·Crosslinked resin particles The specific resin particles are preferably crosslinked resin particles. Here, in order to include the specific resin particles in the toner particles, it is preferable that the specific resin particles have a high affinity with the binder resin.Specific methods for increasing the affinity include controlling the SP value and using a surfactant as a dispersant for the specific resin particles.However, when using specific resin particles having a high affinity with the binder resin, the specific resin particles are composed of organic polymers, unlike inorganic fillers, carbon black, metal particles, etc., and therefore tend to be compatible with the binder resin, and dispersibility may decrease. On the other hand, when specific resin particles having low affinity with the binder resin are used, they are difficult to be included in the toner particles and may be discharged onto the surface of the toner particles or outside the toner particles.
[0075] By using specific resin particles having an intermediate affinity between specific resin particles having a high affinity with the binder resin and specific resin particles having a low affinity, it is possible to include the specific resin particles in the toner particles to a certain extent, but regardless of the toner manufacturing method such as the emulsion aggregation method or the kneading and grinding method, when the specific resin particles come into contact with each other, they have a high affinity because they are made of the same type of material, and they may maintain a state of contact and be unevenly distributed, making it difficult to evenly distribute the specific resin particles in the toner particles. One of the reasons why the specific resin particles maintain a state of contact with each other is thought to be that the polymer chains of the polymer component that constitutes the specific resin particles become entangled when they come into contact. Therefore, by using crosslinked resin particles as the specific resin particles, it becomes possible to suppress entanglement of polymer chains, to prevent the polymer chains from remaining in contact with each other, and to distribute the polymer chains evenly throughout the toner particles.
[0076] Examples of the crosslinked resin particles include crosslinked resin particles crosslinked by ionic bonds (ionically crosslinked resin particles), crosslinked resin particles crosslinked by covalent bonds (covalently crosslinked resin particles), etc. Among these, the crosslinked resin particles are preferably crosslinked resin particles crosslinked by covalent bonds.
[0077] The types of resins used in the crosslinked resin particles include polyolefin resins (polyethylene, polypropylene, etc.), styrene resins (polystyrene, α-polymethylstyrene, etc.), (meth)acrylic resins (polymethyl methacrylate, polyacrylonitrile, etc.), epoxy resins, polyurethane resins, polyurea resins, polyamide resins, polycarbonate resins, polyether resins, polyester resins, and copolymer resins thereof. These resins may be used alone or in combination of two or more types, as necessary.
[0078] Of the above resins, the resin used for the crosslinked resin particles is preferably a styrene (meth)acrylic resin, which is a copolymer resin of a styrene-based resin and a (meth)acrylic resin. That is, the crosslinked resin particles are preferably styrene (meth)acrylic resin particles. The styrene (meth)acrylic resin may be, for example, a resin obtained by radical polymerization of the following styrene-based monomer and (meth)acrylic acid-based monomer.
[0079] Examples of styrene monomers include styrene, α-methylstyrene, vinylnaphthalene, alkyl-substituted styrenes having alkyl chains such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene, halogen-substituted styrenes such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene, and fluorine-substituted styrenes such as 4-fluorostyrene and 2,5-difluorostyrene, etc. Among these, styrene and α-methylstyrene are preferred.
[0080] Examples of (meth)acrylic acid monomers include (meth)acrylic acid, n-methyl (meth)acrylate, n-ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, n-hexadecyl (meth)acrylate, n-octadecyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, amyl (meth)acrylate, Examples of such acrylates include neopentyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, phenyl (meth)acrylate, biphenyl (meth)acrylate, diphenylethyl (meth)acrylate, t-butylphenyl (meth)acrylate, terphenyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-carboxyethyl (meth)acrylate, (meth)acrylonitrile, and (meth)acrylamide. Among these, n-butyl (meth)acrylate and 2-carboxyethyl (meth)acrylate are preferred.
[0081] Examples of crosslinking agents for crosslinking the resin in the crosslinked resin particles include aromatic polyvinyl compounds such as divinylbenzene and divinylnaphthalene; polyvinyl esters of aromatic polyvalent carboxylic acids such as divinyl phthalate, divinyl isophthalate, divinyl terephthalate, divinyl homophthalate, divinyl trimesate, trivinyl trimesate, divinyl naphthalenedicarboxylate, and divinyl biphenylcarboxylate; divinyl esters of nitrogen-containing aromatic compounds such as divinyl pyridinedicarboxylate; vinyl esters of unsaturated heterocyclic compound carboxylic acids such as vinyl pyrromucate, vinyl furancarboxylate, vinyl pyrrole-2-carboxylate, and vinyl thiophenecarboxylate; butanediol diacrylate, butanediol dimethacrylate, hexanediol diacrylate, hexanediol dimethacrylate, octanediol diacrylate, octanediol dimethacrylate, nonanediol diacrylate, nonanediol dimethacrylate, decanediol diacrylate, decanedi ... (Meth)acrylic acid esters of linear polyhydric alcohols such as diol dimethacrylate, dodecane diol diacrylate, and dodecane diol dimethacrylate; (meth)acrylic acid esters of branched or substituted polyhydric alcohols such as neopentyl glycol dimethacrylate and 2-hydroxy, 1,3-diacryloxypropane; polyethylene glycol di(meth)acrylate, polypropylene polyethylene glycol di(meth)acrylates, divinyl succinate, divinyl fumarate, and maleic acid Examples of the crosslinking agent include polyvinyl esters of polyvalent carboxylic acids such as vinyl, divinyl maleate, divinyl diglycolate, vinyl itaconate, divinyl itaconate, divinyl acetonedicarboxylate, divinyl glutarate, divinyl 3,3'-thiodipropionate, divinyl trans-aconitate, trivinyl trans-aconitate, divinyl adipate, divinyl pimelate, divinyl suberate, divinyl azelaate, divinyl sebacate, divinyl dodecanedioate, and divinyl brassylate. The crosslinking agent may be used alone or in combination of two or more.
[0082] Among these, it is preferable to use a bifunctional alkyl acrylate having an alkylene chain with 6 or more carbon atoms as a crosslinking agent for crosslinking the resin. In other words, it is preferable that the crosslinked resin particles have a bifunctional alkyl acrylate as a constituent unit, and the alkylene chain in the bifunctional alkyl acrylate has 6 or more carbon atoms. The specific toner can be obtained more easily by using crosslinked resin particles having a bifunctional alkyl acrylate as a constituent unit and having 6 or more carbon atoms in the alkylene chain. In the specific toner, it is important to suppress the deformation amount of the toner particles to a certain range even under high pressure fixing conditions in order to suppress the gloss difference. If the difference in elasticity between the specific resin particles, which are crosslinked resin particles, and the binder resin is too large, it may be difficult to obtain the effect of suppressing the change in the loss tangent tan δ by the specific resin particles. For this reason, it is preferable to control the elasticity of the specific resin particles so that it does not become too high. If the crosslink density of the specific resin particles is high (i.e., the distance between the crosslinking points is short), the elasticity becomes too high, whereas if a bifunctional acrylate having a long alkylene chain is used as a crosslinking agent, the crosslink density becomes low (i.e., the distance between the crosslinking points is long), and the elasticity of the specific resin particles can be suppressed from becoming too high. As a result, the gloss difference can be further suppressed.
[0083] From the viewpoint of adjusting the crosslink density to an appropriate range, the number of carbon atoms in the alkylene chain in the bifunctional alkyl acrylate is preferably 6 or more, more preferably 6 to 12, and even more preferably 8 to 12. More specific examples of the bifunctional alkyl acrylate include 1,6-hexanediol acrylate, 1,6-hexanediol methacrylate, 1,8-octanediol diacrylate, 1,8-octanediol dimethacrylate, 1,9-nonanediol diacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol diacrylate, 1,10-decanediol dimethacrylate, 1,12-dodecanediol diacrylate, and 1,12-dodecanediol dimethacrylate, and among these, 1,10-decanediol diacrylate and 1,10-decanediol dimethacrylate are preferred.
[0084] In addition, when the specific resin particles are polymers of a composition for forming specific resin particles containing a styrene-based monomer, a (meth)acrylic acid-based monomer, and a crosslinking agent, the amount of the crosslinking agent contained in the composition may be adjusted to control the viscoelasticity of the specific resin particles. For example, by increasing the amount of the crosslinking agent contained in the composition, resin particles having a high storage modulus G' are easily obtained. The content of the crosslinking agent in the composition for forming specific resin particles is, for example, preferably 0.3 parts by mass or more and 5.0 parts by mass or less, more preferably 0.5 parts by mass or more and 2.5 parts by mass or less, and even more preferably 1.0 parts by mass or more and 2.0 parts by mass or less, relative to 100 parts by mass of the total of the styrene-based monomer, the (meth)acrylic acid-based monomer, and the crosslinking agent.
[0085] The glass transition temperature Tg of the specific resin particles determined by dynamic viscoelasticity measurement is preferably 10° C. or more and 45° C. or less. When the glass transition temperature Tg of the specific resin particles is 10° C. or more and 45° C. or less, the toner has better fixing properties and reduces the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions. Furthermore, the glass transition temperature Tg of the specific resin particles is preferably 15°C or higher and 40°C or lower, and more preferably 20°C or higher and 35°C or lower. When the glass transition temperature Tg of the specific resin particles is within the above range, the difference with the Tg of the binder resin becomes large, and the resin particles are prevented from being easily unevenly distributed in the toner particles, and the specific resin particles are easily maintained in a nearly uniform dispersion state, and the effect of suppressing deformation due to pressure during fixing is easily obtained, and the gloss difference is small. Also, when the glass transition temperature Tg of the specific resin particles is within the above range, the deterioration of low-temperature fixing property caused by the deterioration of the melting property of the binder resin is suppressed, compared to when the Tg is too high.
[0086] The number average particle diameter of the specific resin particles is preferably 60 nm or more and 300 nm or less, more preferably 100 nm or more and 200 nm or less, and even more preferably 130 nm or more and 170 nm or less. By having the number-average particle diameter of the specific resin particles in the above range, the toner particles are more susceptible to the effect of the high elasticity of the specific resin particles, and the toner particles are less susceptible to the effect of the high elasticity of the specific resin particles, and good fixability is obtained. Also, by having the number-average particle diameter of the specific resin particles in the above range, the specific resin particles are more likely to be dispersed in a nearly uniform state within the toner particles, compared to when the number-average particle diameter is larger than the above range, and the toner is more likely to have similar viscoelasticity at high temperature and low temperature. This reduces the gloss condition difference.
[0087] The number average particle size of the specific resin particles is a value measured using a transmission electron microscope (TEM). As a transmission electron microscope, for example, JEM-1010 manufactured by JEOL Datum Co., Ltd. can be used. Hereinafter, a method for measuring the number average particle diameter of the specific resin particles will be specifically described. The toner particles are cut into pieces with a thickness of about 0.3 μm using a microtome. The cross sections of the toner particles are photographed at 4,500 times magnification using a transmission electron microscope, and the circular equivalent diameters of 1,000 resin particles dispersed in the toner particles are calculated from the individual cross-sectional areas, and the arithmetic average of these is taken as the number-average particle diameter. The number average particle diameter of the specific resin particles may be a value obtained by measuring a dispersion of the specific resin particles using a laser diffraction particle size distribution measuring device (for example, LA-700 manufactured by Horiba, Ltd.).
[0088] The specific resin particles are preferably contained evenly in both a region close to the surface of the toner particle (hereinafter also referred to as the "surface region") and a region close to the center of the toner particle (hereinafter also referred to as the "center region"). By containing the specific resin particles in both the surface region and the center region, the gloss condition difference is reduced compared to the case where the specific resin particles are contained only in either the surface region or the center region. For example, when the specific resin particles are contained only in the surface region, the deformation amount of the toner particles is small under low temperature and low pressure conditions due to the influence of viscoelasticity in the surface region, whereas the deformation amount of the toner particles is large under high temperature and high pressure conditions due to the influence of viscoelasticity in the center region. Therefore, the gloss condition difference may become large. Also, when the specific resin particles are contained only in the center region, the deformation amount of the toner particles is small under low temperature and low pressure conditions, and the dispersion state of the specific resin particles in the fixed image is poor (unevenly distributed), whereas the deformation amount of the toner particles is large under high temperature and high pressure conditions, and the dispersion state of the specific resin particles in the fixed image is likely to be good (close to uniform). When the dispersion state of the specific resin particles in the fixed image is poor, the part where the specific resin particles are present is easily deformed and becomes a convex part, whereas the part where the specific resin particles are not present is easily deformed and becomes a concave part, thereby reducing the gloss. When the dispersion state is good, the above-mentioned state is suppressed, and the gloss increases. Therefore, the gloss condition difference may become large. In contrast, when specific resin particles are contained in both the surface region and the central region, it is presumed that the difference in gloss conditions is reduced, unlike when the particles are contained only in the surface region or only in the central region.
[0089] The content of the specific resin particles is preferably from 2% by mass to 30% by mass, more preferably from 5% by mass to 25% by mass, and even more preferably from 8% by mass to 20% by mass, based on the total mass of the toner particles. By the content of the specific resin particles being within the above range, the toner tends to have a similar viscoelasticity at high temperature and low temperature, and the gloss condition difference is reduced, compared with the case where the content is less than the above range. Also, by the content of the specific resin particles being within the above range, the deterioration of fixability due to the toner particles having too high elasticity is suppressed, and good fixability is obtained, compared with the case where the content is more than the above range.
[0090] -Coloring agent- Examples of colorants include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, ultramarine blue, and tetrahydrofuran. Examples of the dyes include various pigments such as phosphorus blue, chalcoil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate, and various dyes such as acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based dyes. The colorant may be used alone or in combination of two or more kinds.
[0091] The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of types of colorants may be used in combination.
[0092] The content of the colorant is, for example, preferably from 1% by mass to 30% by mass, and more preferably from 3% by mass to 15% by mass, based on the total mass of the toner particles.
[0093] -Release agent- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these.
[0094] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."
[0095] The content of the release agent is, for example, preferably from 1% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the total amount of the toner particles.
[0096] -Other additives- Examples of other additives include well-known additives such as magnetic materials, charge control agents, inorganic powders, etc. These additives are contained in the toner particles as internal additives.
[0097] -Relationship between the composition of toner particles- Difference (SP value (S) - SP value (R)) The difference between the solubility parameter SP (S) of the specific resin particles and the solubility parameter SP (R) of the binder resin (SP (S)-SP (R)) is preferably -0.32 or more and -0.12 or less.
[0098] When the difference (SP value (S)-SP value (R)) is within the above range, the affinity between the binder resin constituting the majority of the toner particles and the specific resin particles is maintained at a moderate level, and the specific resin particles are more likely to disperse uniformly within the toner particles than when the difference is smaller than the above range. This makes it easier to obtain a toner having similar viscoelasticity at high temperature and high distortion and at low temperature and low distortion, reducing the difference in gloss conditions. In other words, compared to when the difference (SP value (S)-SP value (R)) is smaller than the above range, it is less likely that the affinity between the binder resin and the specific resin particles is too high, causing the specific resin particles to move easily within the toner particles, causing some of the specific resin particles to aggregate, and reducing the effect of the specific resin particles. In addition, when the difference (SP value (S) - SP value (R)) is within the above range, the increase in melt viscosity of the entire toner caused by excessive mixing and compatibility of the specific resin particles and the binder resin during toner melting is suppressed, compared to when the difference is greater than the above range. This has the advantage of suppressing the decrease in fixability caused by too high viscoelasticity, and obtaining good fixability. When the binder resin is a mixed resin, the solubility parameter of the resin having the largest content in the binder resin is defined as the SP value (R).
[0099] The difference (SP value (S) - SP value (R)) is more preferably -0.32 or more and -0.12 or less, and further preferably -0.29 or more and -0.18 or less.
[0100] The solubility parameter SP value (S) of the specific resin particles is preferably 9.00 or more and 9.15 or less, more preferably 9.03 or more and 9.12 or less, and even more preferably 9.06 or more and 9.10 or less.
[0101] Here, the solubility parameter SP value (S) of the specific resin particles and the solubility parameter SP value (R) of the binder resin (unit: (cal / cm 3 ) 1 / 2 ) is calculated by the Okitsu method. The Okitsu method is described in detail in the Journal of the Adhesion Society of Japan, Vol. 29, No. 5 (1993).
[0102] Viscoelasticity of components excluding specific resin particles (excluded components) The storage modulus G' of the toner particles excluding the specific resin particles in the range of 30°C to 50°C is 1 x 10 8 Pa or more, and the storage modulus G' is 1×10 5 Less than Pa It is preferable that the temperature at which the toner reaches the storage elastic modulus G' is 65° C. or more and 90° C. or less. Hereinafter, the components excluding the specific resin particles from the toner particles are also referred to as "excluded components", and the storage elastic modulus G' is 1×10 5The temperature at which the storage modulus G' of an excluded component satisfies the above condition is called the "specific elastic modulus reaching temperature". The storage modulus G' of an excluded component satisfies the above condition, and the elastic modulus is high at low temperatures and low at temperatures between 65°C and 90°C. Therefore, when the storage modulus G' of an excluded component satisfies the above condition, the storage modulus G' is 1×10 5 When the temperature reaches less than 1 Pa, the toner particles are more easily melted by heating than when the temperature exceeds 90° C., resulting in good fixability.
[0103] The storage modulus G' of the excluded components at temperatures between 30°C and 50°C is 1×10 8 Pa or more, and 1×10 8 Pa or more 1×10 9 Pa or less is more preferable, and 2×10 8 Pa or more 6×10 8 It is more preferable that the pressure is 0.1 Pa or less. When the storage modulus G' of the excluded component at 30°C or higher and 50°C or lower is within the above range, the toner has better storage stability than when the storage modulus G' is lower than the above range, and better fixing properties are more likely to be obtained than when the storage modulus G' is higher than the above range.
[0104] The specific elastic modulus attainment temperature of the excluded components is preferably 65°C or higher and 90°C or lower, more preferably 68°C or higher and 80°C or lower, and even more preferably 70°C or higher and 75°C or lower. When the specific elastic modulus reaching temperature of the excluded component is within the above range, the storage stability of the toner is better than when the specific elastic modulus reaching temperature is lower than the above range, and better fixability is more easily obtained than when the specific elastic modulus reaching temperature is higher than the above range.
[0105] The loss tangent tan δ of the excluded component at the specific elastic modulus reaching temperature is preferably 0.8 or more and 1.6 or less, more preferably 0.9 or more and 1.5 or less, and even more preferably 1.0 or more and 1.4 or less. By setting the loss tangent tanδ of the excluded component at the specific elastic modulus reaching temperature within the above range, better fixability is obtained than when the loss tangent tanδ is lower than the above range. Also, by setting the loss tangent tanδ of the excluded component at the specific elastic modulus reaching temperature within the above range, the gloss condition difference is reduced compared to when the loss tangent tanδ is higher than the above range.
[0106] The storage modulus G' and loss tangent tan δ of the excluded component are determined as follows. Specifically, first, the resin particles are removed from the toner particles to extract only the removed components, and the removed components are molded into a tablet shape at 25° C. using a press molding machine to prepare a measurement sample. Examples of a method for removing the resin particles from the toner particles to extract only the removed components include a method in which the toner particles are immersed in a solvent that dissolves the binder resin but does not dissolve the resin particles, and the removed components are extracted and extracted. The obtained measurement sample is then sandwiched between parallel plates with a diameter of 8 mm, and the measurement temperature is raised from 30°C to 150°C at a rate of 2°C / min with a strain of 0.1 to 100%, to perform dynamic viscoelasticity measurement under the following conditions: The storage modulus G' and loss tangent tanδ are determined from the respective curves of the storage modulus and loss modulus obtained by the measurement. -Measurement conditions- Measurement device: Rheometer ARES-G2 (manufactured by TA Instruments) Measurement jig: 8mm parallel plate Gap: Adjusted to 3mm Frequency: 1Hz
[0107] Relationship between specific resin particles, toner particles, and excluded components In the range of 90°C to 150°C, the storage modulus of the specific resin particles is G'(p90-150), the storage modulus of the toner particles is G'(t90-150), and the storage modulus of the components excluding the specific resin particles from the toner particles is G'(r90-150). 50) is 1 x 10 4 Pa or more 1×10 6Pa or less, and logG'(t90-150)-logG'(r90-150) is preferably 1.0 or more and 4.0 or less. Furthermore, the value of logG'(t90-150)-logG'(r90-150) is more preferably 1.0 or more and 3.5 or less, further preferably 1.1 or more and 3.4 or less, and particularly preferably 1.2 or more and 3.3 or less. The value of logG'(t90-150)-logG'(r90-150) means the difference in viscoelasticity of toner particles depending on whether or not the specific resin particles are added. By dispersing and containing the specific resin particles in a nearly uniform state in the toner particles, the effect of the viscoelasticity of the specific resin particles on the viscoelasticity of the entire toner particles is suppressed, and by controlling the value of logG'(t90-150)-logG'(r90-150) to the above range, both good fixability and reduced gloss condition difference are achieved compared to when the value is smaller or larger than the above range.
[0108] -Characteristics of toner particles, etc.- The toner particles may be toner particles having a single layer structure, or may be toner particles having a so-called core-shell structure composed of a core portion (core particle) and a coating layer (shell layer) that coats the core portion. Here, the toner particles having a core-shell structure may be composed of, for example, a core portion containing a binder resin, specific resin particles, and, if necessary, other additives such as a colorant and a release agent, and a coating layer containing a binder resin and specific resin particles.
[0109] When the toner particles have a core-shell structure, it is preferable that the specific resin particles are contained in both the core particles and the shell layer. By containing the specific resin particles in both the core particles and the shell layer, the specific resin particles are contained in both the surface region and the central region of the toner particles, so that the gloss condition difference is further reduced.
[0110] The volume average particle size (D50v) of the toner particles is preferably from 2 μm to 10 μm, more preferably from 4 μm to 8 μm, and even more preferably from 4 μm to 6 μm.
[0111] The various average particle sizes and particle size distribution indexes of the toner particles are measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is then added to 100 ml to 150 ml of the electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture diameter of 100 μm. The number of particles sampled is 50,000. Based on the measured particle size distribution, cumulative distributions of volume and number are drawn for each divided particle size range (channel) from the smallest diameter side, and the particle size at 16% of the cumulative size is defined as the volume particle size D16v, the number particle size D16p, the particle size at 50% of the cumulative size as the volume average particle size D50v, the cumulative number average particle size D50p, and the particle size at 84% of the cumulative size as the volume particle size D84v and number particle size D84p. Using these, the volumetric particle size distribution index (GSDv) is (D84v / D16v) 1 / 2 The number size distribution index (GSDp) is (D84p / D16p) 1 / 2 It is calculated as:
[0112] The average circularity of the toner particles is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less.
[0113] The average circularity of toner particles is calculated by (circular equivalent perimeter) / (perimeter) [(perimeter of a circle having the same projected area as the particle image) / (perimeter of the particle projected image)]. Specifically, it is a value measured by the following method. First, the toner particles to be measured are sucked and collected, flattened, and a still image of the particles is captured by instantaneous strobe light emission, and the particle image is analyzed by a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation). The number of samples to be taken in order to calculate the average circularity is 3,500. When the toner contains an external additive, the toner (developer) to be measured is dispersed in water containing a surfactant, and then ultrasonic treatment is performed to obtain toner particles from which the external additive has been removed.
[0114] Number average molecular weight of tetrahydrofuran solubles The number average molecular weight of the tetrahydrofuran soluble matter in the toner particles is preferably from 5000 to 15000. Hereinafter, the tetrahydrofuran soluble matter is also referred to as "THF soluble matter". By having the number average molecular weight of the THF soluble matter in the toner particles be 5000 or more and 15000 or less, the change in loss tangent with respect to the change in the amount of strain is small, and even if the toner has high viscoelasticity and the amount of deformation is suppressed, high fixability can be obtained. Specifically, by having the number average molecular weight of the THF soluble matter in the above range, the amount of deformation of the toner particles is increased under high-temperature and high-pressure fixing conditions due to the presence of a large amount of low-molecular-weight components in the toner particles, and the gloss difference is suppressed compared to when the number average molecular weight is too small. In addition, by having the number average molecular weight of the THF soluble matter in the above range, the amount of deformation of the toner particles is suppressed due to the presence of a large amount of high-molecular-weight components in the toner particles, and low-temperature fixability is suppressed compared to when the number average molecular weight is too large. It is more preferable that the number average molecular weight of the THF soluble matter is 7000 or more and 10000 or less.
[0115] The number average molecular weight of the THF-soluble portion of the toner particles is measured using two "HLC-8120GPC, SC-8020 (6.0 mm ID x 15 cm, manufactured by Tosoh Corporation)" and tetrahydrofuran (THF) as an eluent to prepare the THF-soluble portion of the toner particles. Specifically, 0.5 mg of toner particles to be measured is dissolved in 1 g of THF, and the solution is subjected to ultrasonic dispersion, and then the concentration is adjusted to 0.5% by mass. Measurements are performed using an RI detector under conditions of a sample concentration of 0.5% by mass, a flow rate of 0.6 ml / min, a sample injection amount of 10 μl, and a measurement temperature of 40°C. In addition, the calibration curve is prepared from 10 samples of "Polystyrene standard sample TSK standard" manufactured by Tosoh Corporation: "A-500", "F-1", "F-10", "F-80", "F-380", "A-2500", "F-4", "F-40", "F-128", and "F-700".
[0116] When obtaining toner particles from toner containing external additives, for example, the toner is dispersed in an aqueous solution of 0.2% by mass of polyoxyethylene (10) octylphenyl ether to a concentration of 10% by mass, and the external additives are liberated by applying ultrasonic vibration (frequency 20 kHz, output 30 W) for 60 minutes while maintaining a temperature of 30° C. or less. The toner particles are filtered and washed from the resulting dispersion to obtain toner particles from which the external additives have been removed.
[0117] (External additives) Examples of the external additive include inorganic particles, such as SiO2, TiO2, Al2O3, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, K2O·(TiO2)n, Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, and MgSO4.
[0118] The surface of the inorganic particles as an external additive may be subjected to a hydrophobic treatment. The hydrophobic treatment may be performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the inorganic particles.
[0119] Examples of external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate (PMMA), and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles).
[0120] The amount of the external additive added is, for example, preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the toner particles.
[0121] (Toner characteristics) - Viscoelasticity of toner - As described above, the toner according to the present embodiment is a specified toner, in other words, D1(90), D50(90), D1(150), and D50(150) are all 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0.
[0122] D1(90) in the specific toner is 0.5 or more and 2.5 or less, preferably 0.5 or more and 2.0 or less, more preferably 0.6 or more and 1.8 or less, even more preferably 0.8 or more and 1.6 or less, and particularly preferably 1.0 or more and 1.5 or less. The D50(90) of the specific toner is from 0.5 to 2.5, preferably from 0.5 to 2.0, more preferably from 0.6 to 1.8, even more preferably from 0.8 to 1.6, and particularly preferably from 1.1 to 1.6. D1(150) in the specific toner is 0.5 or more and 2.5 or less, preferably 0.5 or more and 2.0 or less, more preferably 0.5 or more and 1.5 or less, even more preferably 0.55 or more and 1.0 or less, and particularly preferably 0.55 or more and 0.8 or less. The D50(150) of the specific toner is from 0.5 to 2.5, preferably from 0.8 to 2.2, more preferably from 1.0 to 2.0, even more preferably from 1.2 to 1.9, and particularly preferably from 1.4 to 1.7. When D1(90), D50(90), D1(150), and D50(150) are all within the above ranges, image fog is suppressed compared to when they are smaller or larger than the above ranges. Also, when D1(90), D50(90), D1(150), and D50(150) are all within the above ranges, better fixability is obtained compared to when they are smaller than the above ranges, and gloss condition differences are reduced compared to when they are larger than the above ranges.
[0123] The value of D50(150)-D1(150) in the specific toner is less than 1.5, preferably 1.2 or less, and more preferably 1.0 or less. When the value of D50(150)-D1(150) is within the above range, the gloss condition difference is reduced compared to when the value is greater than the above range. From the viewpoint of reducing the gloss condition difference, the smaller the value of D50(150)-D1(150), the more preferable. The lower limit of the value of D50(150)-D1(150) is not particularly limited.
[0124] The value of D50(90)-D1(90) in the specific toner is less than 1.0, preferably less than 0.5, more preferably 0.4 or less, and even more preferably 0.3 or less. By having the value of D50(90)-D1(90) in the above range, the gloss condition difference is reduced compared to when the value is greater than the above range. From the viewpoint of reducing the gloss condition difference, the smaller the value of D50(90)-D1(90), the more preferable. The lower limit of the value of D50(90)-D1(90) is not particularly limited.
[0125] The storage modulus G' of the toner in the range of 30°C to 50°C is 1×10 8 Pa or more, and the storage modulus G' is 1×10 5The temperature at which the storage elastic modulus G' reaches less than 1×10 Pa (i.e., the specific elastic modulus reaching temperature) is preferably 65° C. or higher and 90° C. or lower. A toner whose storage elastic modulus G' satisfies the above condition has a high elastic modulus at low temperatures and a low elastic modulus at temperatures from 65° C. to 90° C. Therefore, when the storage elastic modulus G' of a toner satisfies the above condition, the storage elastic modulus G' is 1×10 5 When the temperature reaches less than 1 Pa, the toner is more easily melted by heating than when the temperature exceeds 90° C., resulting in good fixability.
[0126] The storage modulus G' of the toner at 30°C to 50°C is 1×10 8 Pa or more, and 1×10 8 Pa or more 1×10 9 Pa is more preferable, and 2×10 8 Pa or more 6×10 8 It is more preferable that the pressure is 0.1 Pa or less. When the storage modulus G' of the toner at 30°C or higher and 50°C or lower is in the above range, the toner has better storage stability than when the storage modulus G' is lower than the above range, and better fixability is more likely to be obtained than when the storage modulus G' is higher than the above range.
[0127] The specific elastic modulus reaching temperature of the toner is preferably 65° C. or more and 90° C. or less, more preferably 70° C. or more and 87° C. or less, and even more preferably 75° C. or more and 84° C. or less. When the specific elastic modulus reaching temperature of the toner is within the above range, the toner has better storage stability than when it is lower than the above range, and better fixability is more likely to be obtained than when it is higher than the above range.
[0128] The storage elastic modulus G' and the specific elastic modulus reaching temperature of the toner are determined as follows. Specifically, the toner to be measured is molded into a tablet shape at room temperature (25°C) using a press molding machine to prepare a measurement sample. The obtained measurement sample is then sandwiched between parallel plates with a diameter of 8 mm, and the measurement temperature is raised from 30°C to 150°C at a rate of 2°C / min with a strain of 0.1 to 100%, to perform dynamic viscoelasticity measurement under the following conditions. The storage modulus G' is calculated from the curves of the storage modulus and loss modulus obtained by the measurement. -Measurement conditions- Measurement device: Rheometer ARES-G2 (manufactured by TA Instruments) Measurement jig: 8mm parallel plate Gap: Adjusted to 3mm Frequency: 1Hz
[0129] (Toner manufacturing method) Next, a method for producing the toner according to the present embodiment will be described. The toner according to the exemplary embodiment can be obtained by producing toner particles and then adding an external additive to the toner particles, if necessary.
[0130] The toner particles may be produced by any of a dry production method (e.g., a kneading and pulverizing method, etc.) and a wet production method (e.g., an aggregation-coalescence method, a suspension polymerization method, a dissolution suspension method, etc.). The method for producing the toner particles is not particularly limited, and a well-known production method is adopted. Among these, it is preferable to obtain toner particles by the aggregation and coalescence method.
[0131] Specifically, for example, when toner particles are produced by the aggregation and coalescence method, The toner particles are manufactured through a process including a step of preparing a resin particle dispersion in which resin particles to be the binder resin are dispersed, and a specific resin particle dispersion in which the specific resin particles are to be dispersed (resin particle dispersion preparation process), a step of aggregating the resin particles (or other particles, if necessary) in the resin particle dispersion (in a dispersion after mixing other particle dispersions, if necessary) to form aggregated particles (aggregated particle formation process), and a step of heating the aggregated particle dispersion in which the aggregated particles are dispersed, to fuse and coalesce the aggregated particles, thereby forming toner particles (fusion and coalescence process).
[0132] Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant and a release agent will be described, but the colorant and the release agent are used as necessary. Of course, additives other than the colorant and the release agent may be used.
[0133] -Resin particle dispersion preparation process- First, a resin particle dispersion in which resin particles serving as a binder resin are dispersed, as well as a colorant particle dispersion in which colorant particles are dispersed and a release agent particle dispersion in which release agent particles are dispersed are prepared.
[0134] Here, the resin particle dispersion liquid is prepared, for example, by dispersing resin particles in a dispersion medium with the aid of a surfactant.
[0135] The dispersion medium used in the resin particle dispersion liquid is, for example, an aqueous medium. Examples of the aqueous medium include water such as distilled water and ion-exchanged water, alcohols, etc. These may be used alone or in combination of two or more.
[0136] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. Among these, anionic surfactants and cationic surfactants are particularly preferred. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. The surfactant may be used alone or in combination of two or more kinds.
[0137] In the resin particle dispersion, examples of the method for dispersing the resin particles in the dispersion medium include general dispersion methods using, for example, a rotary shear type homogenizer, a ball mill having a media, a sand mill, a dyno mill, etc. Depending on the type of resin particles, the resin particles may be dispersed in the resin particle dispersion using, for example, a phase inversion emulsification method. The phase inversion emulsification method is a method in which the resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, a base is added to the organic continuous phase (O phase) to neutralize it, and then an aqueous medium (W phase) is added to effect conversion of the resin from W / O to O / W (so-called phase inversion), resulting in a discontinuous phase, and the resin is dispersed in particulate form in the aqueous medium.
[0138] The volume average particle size of the resin particles dispersed in the resin particle dispersion is, for example, preferably from 0.01 μm to 1 μm, more preferably from 0.08 μm to 0.8 μm, and even more preferably from 0.1 μm to 0.6 μm. The volume average particle size of the resin particles is calculated by using the particle size distribution obtained by measurement using a laser diffraction particle size distribution measuring device (e.g., LA-700 manufactured by Horiba, Ltd.), subtracting the cumulative distribution for the volume from the small particle size side for the divided particle size range (channel), and calculating the cumulative distribution for all particles by 5. The particle size at which the particle size becomes 0% is measured as the volume average particle size D50v. The volume average particle sizes of particles in other dispersions are also measured in the same manner.
[0139] The content of the resin particles in the resin particle dispersion is, for example, preferably from 5% by mass to 50% by mass, and more preferably from 10% by mass to 40% by mass.
[0140] In addition, for example, a colorant particle dispersion and a release agent particle dispersion are also prepared in the same manner as the resin particle dispersion. That is, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the resin particle dispersion are the same for the colorant particles dispersed in the colorant particle dispersion and the release agent particles dispersed in the release agent particle dispersion.
[0141] Preparation of specific resin particle dispersion The specific resin particle dispersion can be prepared by any known method, such as emulsion polymerization, melt kneading using a Banbury mixer or kneader, suspension polymerization, spray drying, etc., with emulsion polymerization being preferred.
[0142] From the viewpoint of setting the storage modulus G' and loss tangent tan δ of the specific resin particles within a preferred range, it is preferable to use a styrene-based monomer and a (meth)acrylic acid-based monomer as the monomers and polymerize them in the presence of a crosslinking agent. In the production of the specific resin particles, it is preferable to carry out emulsion polymerization a number of times. The method for producing the specific resin particles will be described in more detail below.
[0143] The method for preparing the specific resin particle dispersion liquid is as follows: A step of obtaining an emulsion containing a monomer, a crosslinking agent, a surfactant, and water (an emulsion preparation step); a step of adding a polymerization initiator to the emulsion and polymerizing the monomers by heating (first emulsion polymerization step); a step of adding an emulsion containing a monomer and a crosslinking agent to the reaction solution after the first emulsion polymerization step and polymerizing the monomer by heating (second emulsion polymerization step); It is preferred that the compound contains
[0144] (Emulsion preparation process) This is a process for obtaining an emulsion containing a monomer, a crosslinking agent, a surfactant, and water. It is preferable to obtain an emulsion by emulsifying a monomer, a crosslinking agent, a surfactant, and water using an emulsifier. Examples of emulsifiers include rotary mixers equipped with propeller-type, anchor-type, paddle-type, or turbine-type stirring blades, static mixers such as static mixers, rotor-stator type emulsifiers such as homogenizers and Clearmix, mill-type emulsifiers equipped with a grinding function, high-pressure emulsifiers such as Manton-Gaulin pressure emulsifiers, high-pressure nozzle type emulsifiers that generate cavitation under high pressure, high-pressure collision type emulsifiers such as microfluidizers that apply shear force by colliding liquids together under high pressure, ultrasonic emulsifiers that generate cavitation using ultrasound, and membrane emulsifiers that perform uniform emulsification through fine pores.
[0145] As the monomer, it is preferable to use a styrene-based monomer and a (meth)acrylic acid-based monomer. As the crosslinking agent, those already mentioned are applicable.
[0146] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. Among these, anionic surfactants are preferred. The surfactants may be used alone or in combination with two or more.
[0147] The emulsion may contain a chain transfer agent. There is no particular limitation on the chain transfer agent, but a compound having a thiol component can be used. Specifically, alkyl mercaptans such as hexyl mercaptan, heptyl mercaptan, octyl mercaptan, nonyl mercaptan, decyl mercaptan, and dodecyl mercaptan are preferred.
[0148] From the viewpoint of setting the storage modulus G' and loss tangent tanδ of the specific resin particles within a preferred range, the mass ratio of the styrene-based monomer and the (meth)acrylic acid-based monomer in the emulsion (styrene-based monomer / (meth)acrylic acid-based monomer) is preferably 0.2 or more and 1.1 or less. In order to set the storage modulus G' and loss tangent tan δ of the specific resin particles within preferred ranges, the content of the crosslinking agent in the entire emulsion is preferably 0.5% by mass or more and 3% by mass or less.
[0149] (First emulsion polymerization step) This is a process in which a polymerization initiator is added to the emulsion and then heated to polymerize the monomers. During polymerization, it is preferable to stir the emulsion (reaction solution) containing the polymerization initiator with a stirrer. The agitator may be a rotary agitator equipped with a propeller-type, anchor-type, paddle-type, or turbine-type agitator blade. As the polymerization initiator, ammonium persulfate is preferably used. In addition, when a polymerization initiator is used, the viscoelasticity of the obtained specific resin particles may be controlled by adjusting the amount of the polymerization initiator added. For example, by reducing the amount of the polymerization initiator added, resin particles having a high storage modulus G' are easily obtained.
[0150] (Second emulsion polymerization step) This is a step in which an emulsion containing a monomer is added to the reaction solution after the first emulsion polymerization step, and the monomer is polymerized by heating. During the polymerization, it is preferable to stir the reaction solution in the same manner as in the first emulsion polymerization step. In this step, the viscoelasticity of the specific resin particles obtained may be controlled by adjusting the time taken to add the emulsion containing the monomer. For example, by increasing the time taken to add the emulsion containing the monomer, resin particles having a high storage modulus G' are more likely to be obtained. The time taken to add the emulsion containing the monomer may be, for example, in the range of 2 hours to 5 hours. In addition, in this process, the viscoelasticity of the specific resin particles obtained may be controlled by adjusting the temperature when the reaction solution is stirred. For example, by lowering the temperature when the reaction solution is stirred, resin particles with a high storage modulus G' are easily obtained. The temperature when the reaction solution is stirred may be, for example, in the range of 55°C or more and 75°C or less. The emulsion containing the monomer is preferably obtained by emulsifying the monomer, a surfactant, and water using an emulsifier.
[0151] -Agglomerated particle formation process- Next, the colorant particle dispersion, the release agent particle dispersion, and the specific resin particle dispersion are mixed with the resin particle dispersion. Then, in the mixed dispersion, the resin particles, the colorant particles, the release agent particles, and the specific resin particles are hetero-aggregated to form aggregated particles containing the resin particles, the colorant particles, the release agent particles, and the specific resin particles and having a diameter close to the diameter of the target toner particles.
[0152] Specifically, for example, an aggregating agent is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic (e.g., pH 2 or more and 5 or less), a dispersion stabilizer is added as necessary, and then the mixed dispersion is heated to a temperature of the glass transition temperature of the resin particles (specifically, for example, a temperature of the glass transition temperature of the resin particles -30°C or more and the glass transition temperature -10°C or less), and the particles dispersed in the mixed dispersion are aggregated to form aggregated particles. In the aggregated particle formation process, for example, the above-mentioned aggregating agent may be added to the mixed dispersion at room temperature (e.g., 25°C) while stirring the mixed dispersion with a rotary shear homogenizer, the pH of the mixed dispersion may be adjusted to an acidic state (e.g., pH 2 or more and 5 or less), and a dispersion stabilizer may be added as necessary, followed by the above-mentioned heating.
[0153] In this step, the temperature of the mixed dispersion liquid when the aggregating agent is added may be adjusted to control the dispersion state of the specific resin particles in the toner particles obtained. For example, the dispersibility of the specific resin particles is improved by lowering the temperature of the mixed dispersion liquid. The temperature of the mixed dispersion liquid may be, for example, in the range of 5°C to 40°C. In this step, the stirring speed after the addition of the aggregating agent may be adjusted to control the dispersion state of the specific resin particles in the toner particles obtained. For example, by increasing the stirring speed after the addition of the aggregating agent, the dispersibility of the specific resin particles becomes good.
[0154] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant used as the dispersant added to the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. In particular, when a metal complex is used as the flocculant, the amount of surfactant used is reduced and the charging characteristics are improved. If necessary, an additive that forms a complex or a similar bond with the metal ions of the flocculant may be used, and a chelating agent is preferably used as this additive.
[0155] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. The chelating agent may be a water-soluble chelating agent, for example, oxycarboxylic acid such as tartaric acid, citric acid, gluconic acid, iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), ethylenediaminetetraacetic acid (EDTA), etc. The amount of the chelating agent added is, for example, preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, relative to 100 parts by mass of the resin particles.
[0156] -Fusion / coalescence process- Next, the aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition temperature of the resin particles (for example, a temperature 10 to 30° C. higher than the glass transition temperature of the resin particles) to fuse and coalesce the aggregated particles, thereby forming toner particles.
[0157] Through the above steps, toner particles are obtained. Note that, after obtaining an aggregated particle dispersion liquid in which the aggregated particles are dispersed, the toner particles may be manufactured through a process of further mixing the aggregated particle dispersion liquid, a resin particle dispersion liquid in which resin particles are dispersed, and a specific resin particle dispersion liquid in which specific resin particles are dispersed, and aggregating the aggregated particles so that the resin particles and the specific resin particles are further attached to the surfaces of the aggregated particles to form second aggregated particles, and a process of heating the second aggregated particle dispersion liquid in which the second aggregated particles are dispersed, to fuse and coalesce the second aggregated particles to form toner particles having a core / shell structure.
[0158] In the step of forming the second aggregated particles, the addition of the resin particle dispersion and the specific resin particle dispersion and the adhesion of the resin particles and the specific resin particles to the surfaces of the aggregated particles may be repeated multiple times, whereby toner particles in which the specific resin particles are evenly contained in both the surface region and the center region of the toner particles are obtained.
[0159] After the fusion and coalescence process, the toner particles formed in the solution are subjected to a known washing process, solid-liquid separation process, and drying process to obtain toner particles in a dried state. In the washing step, it is preferable to carry out sufficient replacement washing with ion-exchanged water from the viewpoint of electrostatic charge. In addition, the solid-liquid separation step is not particularly limited, but it is preferable to carry out suction filtration, pressure filtration, etc. from the viewpoint of productivity. In addition, in the drying step, there is no particular limit to the method, but it is preferable to carry out freeze drying, air flow drying, fluidized drying, vibration type fluidized drying, etc. from the viewpoint of productivity.
[0160] The toner according to the present embodiment is produced, for example, by adding an external additive to the obtained toner particles in a dry state and mixing them. The mixing may be performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.
[0161] <Career> The carrier includes magnetic particles and a resin layer attached to the surfaces of the magnetic particles.
[0162] (magnetic particles) In this embodiment, the average spacing Sm of projections and recesses on the surface of the magnetic particles satisfies 0.5 μm≦Sm≦2.5 μm. It is presumed that by having the mean irregularity spacing Sm of the magnetic particle surface in the above range, the irregularities of the carrier surface are more easily caught by the toner than when the mean irregularity spacing Sm is smaller than the above range, and image fog is suppressed. It is also presumed that by having the mean irregularity spacing Sm in the above range, the irregularities of the carrier surface are more easily caught by the toner than when the mean irregularity spacing Sm is larger than the above range, and image fog is suppressed. From the viewpoint of suppressing image fogging, the Sm of the magnetic particles is preferably from 0.8 μm to 2.5 μm, and more preferably from 1.0 μm to 2.0 μm.
[0163] From the viewpoint of suppressing image fog, the relationship between the average irregularity spacing Sm on the surface of the magnetic particle and D1(90) in the toner preferably satisfies the following formula (1'), more preferably satisfies the following formula (1), and even more preferably satisfies the following formula (1''). Formula (1') :D1(90)-0.5≦Sm≦D1(90)+1.25 Formula (1) :D1(90)≦Sm≦D1(90)+1.1 Formula (1''): D1(90)+0.05≦Sm≦D1(90)+1.05 The value of Sm-D1(90) is preferably −0.5 or more and +1.3 or less, more preferably −0.5 or more and +1.25 or less, even more preferably 0 or more and +1.1 or less, particularly preferably +0.05 or more and +1.05 or less, and most preferably +0.4 or more and +0.6 or less.
[0164] The reason why fog is suppressed when the relationship between D1(90) in the toner and the average irregularity spacing Sm in the magnetic particles of the carrier satisfies the above formula is not clear, but is presumed to be as follows. Specifically, a toner with a large D1(90) has a higher viscosity on the toner surface than a toner with a small D1(90). Therefore, by combining a carrier containing magnetic particles with a large average irregularity spacing Sm, the irregularities on the carrier surface are prevented from penetrating too much into the toner surface. If the irregularities on the carrier surface penetrate too much into the toner surface, it is thought that the developer as a whole becomes less likely to flow, making the toner more likely to deform. Therefore, it is presumed that by preventing the irregularities on the carrier surface from penetrating too much into the toner surface, image fogging caused by toner deformation is suppressed. In addition, a toner with a small D1(90) has a higher elasticity of the toner surface than a toner with a large D1(90). Therefore, it is presumed that by combining a carrier containing magnetic particles with a small average irregularity spacing Sm, the irregularities on the carrier surface are more likely to be caught by the toner surface, suppressing fogging.
[0165] In this embodiment, the arithmetic mean roughness Ra of the surface of the magnetic particles satisfies 0.3 μm≦Ra≦1.2 μm. It is presumed that by having the arithmetic surface roughness Ra of the magnetic particle surface within the above range, the unevenness of the carrier surface is more likely to be caught by the toner than when the arithmetic surface roughness Ra is smaller than the above range, and image fogging is suppressed. Also, it is presumed that by having the arithmetic mean roughness Ra within the above range, the unevenness of the carrier surface is prevented from excessively cutting into the toner surface, and image fogging caused by deformation of the toner due to the cutting in is suppressed, compared to when the arithmetic mean roughness Ra is larger than the above range. From the viewpoint of suppressing image fogging, the Ra of the magnetic particles is preferably from 0.5 μm to 1.1 μm, and more preferably from 0.7 μm to 1.0 μm.
[0166] From the viewpoint of suppressing image fog, the relationship between the arithmetic mean roughness Ra of the surface of the magnetic particles and D1(90) in the toner preferably satisfies the following formula (2'), more preferably satisfies the following formula (2), and even more preferably satisfies the following formula (2''). Formula (2'): 1.03-0.3×D1(90)≦Ra≦1.45-0.3×D1(90) Formula (2): 1.05-0.3×D1(90)≦Ra≦1.36-0.3×D1(90) Formula (2''): 1.10-0.3×D1(90)≦Ra≦1.25-0.3×D1(90) The value of Ra+0.3×D1(90) is preferably 0.75 or more and 1.55 or less, more preferably 1.03 or more and 1.45 or less, even more preferably 1.05 or more and 1.36 or less, particularly preferably 1.10 or more and 1.25 or less, and most preferably 1.10 or more and 1.20 or less.
[0167] Furthermore, from the viewpoint of further suppressing image fog, the relationship between the arithmetic mean roughness Ra of the surface of the magnetic particles and the D50(150) of the toner preferably satisfies the following formula (3'), more preferably satisfies the following formula (3), and even more preferably satisfies the following formula (3''). Formula (3'): 0.90-0.3×D50(150)≦Ra≦1.45-0.3×D50(150) Formula (3): 1.05-0.3×D50(150)≦Ra≦1.36-0.3×D50(150) Formula (3''): 1.10-0.3×D50(150)≦Ra≦1.25-0.3×D50(150) The value of Ra+0.3×D50(150) is preferably 0.75 or more and 1.56 or less, more preferably 0.90 or more and 1.45 or less, even more preferably 1.05 or more and 1.36 or less, and particularly preferably 1.10 or more and 1.25 or less.
[0168] The reason why fogging is suppressed by satisfying the above formula is not clear, but is presumed to be as follows. Specifically, as described above, a toner with a large D1(90) has a higher viscosity on the toner surface than a toner with a small D1(90). Also, a toner with a large D5(150) has a higher viscosity inside the toner than a toner with a small D50(150). Therefore, by combining a carrier containing magnetic particles with a small arithmetic mean roughness Ra, the unevenness on the carrier surface is prevented from penetrating too much into the toner. It is presumed that by preventing the unevenness on the carrier surface from penetrating too much into the toner, image fog caused by deformation of the toner is prevented. In addition, a toner with a small D1(90) has a higher elasticity on the toner surface than a toner with a large D1(90). In addition, a toner with a small D50(150) has a higher elasticity inside the toner than a toner with a large D50(150). Therefore, it is presumed that by combining a carrier containing magnetic particles with a large arithmetic mean roughness Ra, the unevenness of the carrier surface becomes more easily caught by the toner, suppressing image fog.
[0169] In this embodiment, the volume average particle size of the magnetic particles is preferably 26 μm or more and 34 μm or less. It is presumed that by having the volume average particle size of the magnetic particles in the above range, the developer has good fluidity and the toner is more easily caught by the carrier surface than when the volume average particle size is smaller than the above range, thereby suppressing image fogging. Also, by having the volume average particle size in the above range, it is presumed that by having the volume average particle size in the above range, the toner is less likely to deform or deteriorate, and the toner is more easily caught by the carrier surface than when the volume average particle size is larger than the above range, thereby suppressing image fogging. From the viewpoint of suppressing image fogging, the volume average particle size of the magnetic particles is more preferably from 26 μm to 34 μm, and even more preferably from 28 μm to 32 μm.
[0170] In this embodiment, the BET specific surface area of the magnetic particles is 0.12 m 2 / g or more 0.20m 2 It is preferable that the molecular weight is not more than 1 / g. It is presumed that, by having the BET specific surface area of the magnetic particles in the above range, the unevenness of the carrier surface is more likely to be caught by the toner than when the BET specific surface area is smaller than the above range, and image fogging is suppressed. Also, by having the BET specific surface area in the above range, it is presumed that, by having the BET specific surface area in the above range, the unevenness of the carrier surface is prevented from being excessively embedded in the toner surface, and image fogging caused by deformation of the toner due to the embedding is suppressed, compared to when the BET specific surface area is larger than the above range. The volume average particle size of the magnetic particles is set to 0.14 μm from the viewpoint of suppressing image fogging. 2 / g or more 0.19m 2 / g or less is more preferable, and 0.15m 2 / g or more 0.18m 2 It is more preferable that the molecular weight is not more than 1 / g.
[0171] As the material of the magnetic particles, a known material used as the core material of the carrier is applied. Specific examples of magnetic particles include particles of magnetic metals such as iron, nickel, and cobalt, particles of magnetic oxides such as ferrite and magnetite, resin-impregnated magnetic particles in which porous magnetic powder is impregnated with resin, and magnetic powder-dispersed resin particles in which magnetic powder is dispersed in resin. In this embodiment, ferrite particles are preferred as the magnetic particles.
[0172] The magnetic particles may contain Si element. In particular, when the magnetic particles are ferrite particles, the mean irregularity spacing Sm and the arithmetic mean roughness Ra of the magnetic particle surface can be easily controlled within the above-mentioned ranges by adding a Si-containing component such as SiO2 during the manufacturing process of the magnetic particles, as described below. The content of Si element in the entire magnetic particle is, for example, in the range of 0 mass % to 1 mass %, or may be in the range of 0.1 mass % to 0.5 mass %, or may be in the range of 0.1 mass % to 0.3 mass %.
[0173] The magnetic particles may contain at least one of Ca and Sr. In particular, when the magnetic particles are ferrite particles, the average irregularity spacing Sm and the arithmetic mean roughness Ra of the magnetic particle surface can be easily controlled within the above-mentioned ranges by adding at least one selected from the group consisting of Ca-containing components such as CaCO3 and Sr-containing components such as SrCO3 in the manufacturing process of the magnetic particles, as described below. The Ca element content relative to the entire magnetic particle is, for example, in the range of 0 mass% to 5 mass%, or may be in the range of 0.1 mass% to 2 mass%, or may be in the range of 0.5 mass% to 1.5 mass%. The content of Sr element in the entire magnetic particle is, for example, in the range of 0 mass% to 5 mass% or less, or may be in the range of 0.1 mass% to 2 mass% or less, or may be in the range of 0.5 mass% to 1.5 mass%.
[0174] The magnetic force of the magnetic particles is preferably 50 emu / g or more, more preferably 60 emu / g or more, in terms of saturation magnetization in a magnetic field of 3,000 oersteds. The saturation magnetization is measured using a vibrating sample magnetic measuring device VSMP10-15 (manufactured by Toei Kogyo Co., Ltd.). The measurement sample is packed in a cell with an inner diameter of 7 mm and a height of 5 mm and set in the device. The measurement is performed by applying a magnetic field and sweeping up to a maximum of 3,000 oersteds. The applied magnetic field is then reduced, and a hysteresis curve is prepared on a recording paper. The saturation magnetization, residual magnetization, and retentivity are determined from the curve data.
[0175] The volume resistivity of magnetic particles is 1×10 5 Ω cm or more 1×10 9 Ω cm or less is preferable, and 1×10 7 Ω cm or more 1×10 9 Ω·cm or less is more preferable. The volume resistivity (Ω·cm) of magnetic particles is measured as follows: 2 The object to be measured is placed flat on the surface of the circular jig on which the electrode plate is arranged, with a thickness of 1 mm to 3 mm, to form a layer. 2The layer is sandwiched between two electrode plates. In order to eliminate any gaps between the objects being measured, a 4 kg load is placed on the electrode plate placed on the layer, and then the thickness of the layer (cm) is measured. Both the top and bottom electrodes of the layer are connected to an electrometer and a high-voltage power supply generator. A high voltage is applied to both electrodes so that the electric field is 103.8 V / cm, and the current value (A) that flows at this time is read. The measurement environment is a temperature of 20°C and a relative humidity of 50%. The formula for calculating the volumetric electrical resistivity (Ω·cm) of the object being measured is as shown below. R=E×20 / (I-I0) / L In the above formula, R is the volume resistivity (Ω cm) of the object to be measured, E is the applied voltage (V), I is the current value (A), I0 is the current value (A) at an applied voltage of 0 V, and L is the layer thickness (cm). The coefficient 20 is the area of the electrode plate (cm 2 )
[0176] The volume resistivity of the magnetic particles is not particularly limited, but should be less than 1×10 6 Ω or more 1×10 8 It is preferably Ω or less.
[0177] The method for producing the magnetic particles in this embodiment is not particularly limited, but they can be produced, for example, as follows.
[0178] The surface properties of the magnetic particles (i.e., the mean irregularity spacing Sm, the arithmetic surface roughness Ra, and the BET specific surface area, etc.) can be adjusted to some extent by the temperature and oxygen concentration during sintering. However, the main purpose of sintering is to change the magnetic particles into a structure that has magnetization, and it is difficult to control each of the above Sm, Ra, and BET specific surface area, which are all correlated with each other.
[0179] Therefore, the magnetic particles constituting the carrier according to this embodiment can be suitably manufactured by the combination of the following (A) to (E). (A) Pre-firing is performed before the main firing. (B) The mixture is further pulverized, and granulation is carried out from the slurry with the pulverized particle size adjusted. (C) As a surface property adjuster, a Si-containing component such as SiO2, a Sr-containing component such as SrCO3, a Ca-containing component such as CaCO3, etc. are used. (D) Adjust the temperature and oxygen concentration during the final firing (E) The magnetic particles obtained by main sintering are heated while being fluidized (post-heating).
[0180] After pre-firing, the powder is pulverized to control the particle size. The powder is granulated to the desired particle size, and the volume average particle size is determined. The size of the grain boundaries, which are the basis of the magnetic particles, is controlled by the pulverized particle size after pre-firing. In addition, by adding additives such as SiO2, SrCO3, CaCO3, etc. before calcination, the surface irregularities can be controlled. Adding Si-containing components such as SiO2 increases the grain boundary area, allowing adjustments to be made so that Sm is larger. Adding Sr-containing components such as SrCO3 has the effect of increasing Ra. Adding Ca-containing components such as CaCO3 has the effect of increasing Sm. The additive may be a combination of a Si-containing component and at least one selected from the group consisting of a Sr-containing component and a Ca-containing component. The surface properties of the magnetic particles may be roughly controlled by the amount of the Si-containing component added, while the surface properties of the magnetic particles may be finely adjusted by adding at least one selected from the group consisting of a Sr-containing component and a Ca-containing component.
[0181] Next, the final sintering is performed, adjusting the sintering temperature and oxygen concentration, and magnetization to produce ferrite. The size of the entire grain boundary is adjusted by the sintering temperature and oxygen concentration. If the sintering temperature is high in the final sintering, Sm tends to be large, and if the oxygen concentration is high, Ra tends to be large. In addition, the sintering temperature and oxygen concentration in the final sintering strongly affect the resistance and magnetization. The higher the temperature and the lower the oxygen concentration, the higher the magnetization and the lower the resistance.
[0182] After the main sintering is completed and ferrite formation is completed, the internal voids are reduced (post-heating) at a temperature that does not cause the ferrite reaction. This results in the desired magnetic particles. If heat is applied while flowing, the gaps between the grain boundaries become smaller, so the BET specific surface area can be reduced with little change in Sm and Ra.
[0183] Below, an example of a method for producing magnetic particles according to this embodiment is described, showing specific materials and conditions, but the magnetic particles according to this embodiment are not limited to the materials and values described below.
[0184] For example, Fe2O3, Mn(OH)2, and Mg(OH)2 are mixed in a molar ratio of 2:0.8:0.2, respectively, and 0.1 mass % of SiO2 is added to the mixture, followed by further mixing. Next, a dispersant and water are added, and the mixture is mixed and crushed using zirconia beads with a media diameter of 1 mm. After drying the water, the mixture is pre-fired at a temperature of 900°C. The temperature for the pre-baking is not limited to the above temperatures, and may be, for example, in the range of 800° C. to 1200° C. The time for the pre-baking may be, for example, in the range of 60 minutes to 180 minutes.
[0185] The calcined product is mixed and pulverized in a wet ball mill together with a dispersant, water, and polyvinyl alcohol as a binder resin. The pulverization is stopped when the volume average particle size of the pulverized particles reaches 1.2 μm. Next, the mixture is granulated and dried using a spray dryer to produce particles with a volume average particle size of 28 μm. The dried particles are then fired in an electric furnace at 1240°C in an oxygen and nitrogen gas mixture, with the oxygen concentration adjusted to 1%. The firing temperature is not limited to the above, and may be in the range of 1200° C. to 1500° C., for example. The oxygen concentration in the firing is not limited to the above, and may be in the range of 0.1% to 5%. The firing time is, for example, in the range of 60 minutes to 300 minutes.
[0186] After the firing, the mixture is crushed and classified to obtain ferrite particles with a volume average particle size of 35μm.Then, the mixture is post-heated at 900℃ in a rotary kiln under the condition of 15ppm. The temperature for post-heating after the main firing is not limited to the above temperatures, and may be, for example, in the range of 500° C. to 1000° C. The time for post-heating after the main firing may be, for example, in the range of 30 minutes to 120 minutes. The resulting particles are then subjected to a crushing and classification process again to obtain the desired magnetic particles of 26 μm.
[0187] (Resin layer) The resin layer is a layer that is attached to the surface of the magnetic particle and contains a resin. The resin layer may be a layer that covers at least a part of the surface of the magnetic particle. Hereinafter, the resin layer is also referred to as a "resin coating layer."
[0188] Examples of resins that make up the resin coating layer include styrene-acrylic acid copolymers; polyolefin resins such as polyethylene and polypropylene; polyvinyl or polyvinylidene resins such as polystyrene, acrylic resin, polyacrylonitrile, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl carbazole, polyvinyl ether, and polyvinyl ketone; vinyl chloride-vinyl acetate copolymers; straight silicone resins or modified products thereof consisting of organosiloxane bonds; fluororesins such as polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, and polychlorotrifluoroethylene; polyesters; polyurethanes; polycarbonates; amino resins such as urea-formaldehyde resins; and epoxy resins. In particular, from the viewpoints of electrostatic charge and controllability of external additive adhesion, it is preferable that the resin constituting the resin coating layer contains an acrylic resin, it is more preferable that the acrylic resin is contained in an amount of 50 mass% or more based on the total mass of the resin in the resin coating layer, and it is particularly preferable that the acrylic resin is contained in an amount of 80 mass% or more based on the total mass of the resin in the resin coating layer.
[0189] From the viewpoint of suppressing charge fluctuations due to temperature and humidity, the resin coating layer preferably contains an acrylic resin having an alicyclic structure. As a polymerization component of the acrylic resin having an alicyclic structure, a lower alkyl ester of (meth)acrylic acid (for example, an alkyl (meth)acrylate ester having an alkyl group with 1 to 9 carbon atoms) is preferable, and specific examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. These monomers may be used alone or in combination of two or more. The acrylic resin having an alicyclic structure preferably contains cyclohexyl (meth)acrylate as a polymerization component. The content of the monomer unit derived from cyclohexyl (meth)acrylate contained in the acrylic resin having an alicyclic structure is preferably 75% by mass or more and 100% by mass or less, more preferably 85% by mass or more and 100% by mass or less, and even more preferably 95% by mass or more and 100% by mass or less, based on the total mass of the acrylic resin having an alicyclic structure.
[0190] The weight average molecular weight of the resin contained in the resin coating layer is preferably less than 300,000, more preferably less than 250,000, even more preferably from 5,000 to less than 250,000, and particularly preferably from 10,000 to 200,000. If the weight average molecular weight is within the above range, there is an advantage that the resin coating layer has good wetting to the magnetic particles and has a uniform thickness.
[0191] The resin coating layer may contain conductive particles for the purpose of controlling electrostatic charge and resistance. Examples of the conductive particles include carbon black, metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate.
[0192] Methods for forming a resin coating layer on the surface of magnetic particles include, for example, a wet method and a dry method. The wet method is a method that uses a solvent to dissolve or disperse the resin that constitutes the resin coating layer. On the other hand, the dry method is a method that does not use the above solvent.
[0193] Examples of wet manufacturing methods include an immersion method in which magnetic particles are immersed in a resin liquid for forming a resin coating layer to coat them, a spray method in which a resin liquid for forming a resin coating layer is sprayed onto the surfaces of magnetic particles, a fluidized bed method in which magnetic particles are fluidized in a fluidized bed and then sprayed with a resin liquid for forming a resin coating layer, and a kneader coater method in which magnetic particles are mixed with a resin liquid for forming a resin coating layer in a kneader coater and the solvent is removed. These manufacturing methods may be repeated or combined. The resin liquid for forming the resin coating layer used in the wet manufacturing method is prepared by dissolving or dispersing the resin and other components in a solvent. The solvent is not particularly limited, and examples of the solvent that can be used include aromatic hydrocarbons such as toluene and xylene, ketones such as acetone and methyl ethyl ketone, and ethers such as tetrahydrofuran and dioxane.
[0194] An example of the dry manufacturing method is a method in which a mixture of magnetic particles and a resin for forming a resin coating layer is heated in a dry state to form a resin coating layer. Specifically, for example, the magnetic particles and the resin for forming the resin coating layer are mixed in a gas phase and heated to melt, thereby forming a resin coating layer.
[0195] From the viewpoint of suppressing resistance changes due to temperature and humidity, the average thickness of the resin coating layer is preferably 0.6 μm or more and 1.4 μm or less, more preferably 0.8 μm or more and 1.2 μm or less, and particularly preferably 0.8 μm or more and 1.1 μm or less. The average thickness of the resin coating layer is determined by the following method. The carrier is embedded in epoxy resin and cut with a microtome to prepare a cross section of the carrier. The SEM images of the carrier cross section taken with a scanning electron microscope (SEM) are imported into an image processing analyzer and analyzed. The thickness (μm) of the resin coating layer is measured at 10 randomly selected locations per carrier particle, and then measurements are taken for 100 carriers, and the arithmetic average of all measurements is calculated to obtain the average thickness (μm) of the resin coating layer.
[0196] (Carrier characteristics) From the viewpoint of fluidity of the developer, the volume average particle size of the carrier is preferably from 25 μm to 36 μm, more preferably from 26 μm to 35 μm, and particularly preferably from 28 μm to 34 μm.
[0197] The exposed area ratio of the magnetic particles on the carrier surface is preferably 4% or more and 20% or less, more preferably 5% or more and 18% or less, and even more preferably 8% or more and 12% or less. When the exposed area ratio of the magnetic particles on the carrier surface is in the above range, image fogging is suppressed compared to when it is lower than the above range. Although the reason is not clear, it is assumed that this is because the charge of the toner is less likely to leak. In addition, when the exposed area ratio of the magnetic particles on the carrier surface is in the above range, image fogging is suppressed compared to when it is higher than the above range. Although the reason is not clear, it is assumed that this is because the fluidity of the developer is good. The exposed area ratio of the magnetic particles in the carrier can be controlled by the amount of resin used to form the resin coating layer, and the greater the amount of resin relative to the amount of magnetic particles, the smaller the exposed area ratio. The content of the resin coating layer per 100 parts by mass of the magnetic particles is preferably in the range of 1.5 parts by mass to 5 parts by mass, more preferably in the range of 2 parts by mass to 4 parts by mass, and even more preferably in the range of 2.5 parts by mass to 3.5 parts by mass.
[0198] The exposed area ratio of the magnetic particles on the carrier surface is a value determined by the following method. A target carrier and magnetic particles from which the resin coating layer has been removed from the target carrier are prepared. Methods for removing the resin coating layer from the carrier include, for example, a method for removing the resin coating layer by dissolving the resin component with an organic solvent, and a method for removing the resin coating layer by eliminating the resin component by heating at about 800°C. The carrier and magnetic particles are each used as measurement samples, and the Fe concentration (atomic%) on the sample surface is quantified by XPS, and the exposed area ratio (%) of the magnetic particles is calculated by (Fe concentration of the carrier)÷(Fe concentration of the magnetic particles)×100.
[0199] <Mixing ratio of toner and carrier> The mixture ratio (mass ratio) of toner and carrier in the initial filling developer, which is the developer contained in the developing device, is, for example, in the range of 1 part by mass to 30 parts by mass of toner per 100 parts by mass of carrier. In addition, the mixture ratio (mass ratio) of toner and carrier in a replenishment developer, which is a developer contained in a developer cartridge and replenished to a developing device, can be, for example, in a range of more than 0 parts by mass and not more than 20 parts by mass of carrier per 100 parts by mass of toner.
[0200] <Developer cartridge, process cartridge, image forming apparatus, and image forming method> A developer cartridge, a process cartridge, an image forming apparatus, and an image forming method using the above-mentioned developer will be described below. The developer cartridge according to the present embodiment is not particularly limited as long as it contains the above-mentioned developer as a replenishment developer and is detachably attached to an image forming apparatus.
[0201] The process cartridge according to this embodiment may be a first process cartridge including a developer cartridge containing the aforementioned developer as a replenishment developer, or may be a second process cartridge including a developing device containing the aforementioned developer as an initial filling developer. An example of a first process cartridge is a process cartridge that is detachably attached to an image forming apparatus and includes a developer cartridge that contains the above-mentioned developer as a replenishment developer, and a developing device that contains developer including the replenishment developer replenished from the developer cartridge and develops an electrostatic charge image formed on the surface of an image carrier using the developer into a toner image. An example of a second process cartridge is a process cartridge that is detachably attached to an image forming apparatus and that contains the above-mentioned developer as an initial filling developer and is equipped with a developing device that uses the developer to develop an electrostatic charge image formed on the surface of an image carrier into a toner image.
[0202] The image forming apparatus according to this embodiment may be a first image forming apparatus including a developer cartridge that contains the above-mentioned developer as a replenishment developer, or may be a second image forming apparatus including a developing device that contains the above-mentioned developer as an initial filling developer. An example of a first image forming apparatus is an image forming apparatus including a developer cartridge containing the above-mentioned developer as a replenishment developer, an image holder, a charging device that charges the surface of the image holder, an electrostatic image forming device that forms an electrostatic image on the surface of the charged image holder, a developing device that contains developer including the replenishment developer replenished from the developer cartridge and develops the electrostatic image formed on the surface of the image holder as a toner image using the developer, a transfer device that transfers the toner image formed on the surface of the image holder to the surface of a recording medium, and a fixing device that fixes the toner image transferred to the surface of the recording medium. An example of a second image forming apparatus is an image forming apparatus including an image carrier, a charging device that charges the surface of the image carrier, an electrostatic image forming device that forms an electrostatic image on the surface of the charged image carrier, a developing device that contains the above-mentioned developer as an initial filling developer and develops the electrostatic image formed on the surface of the image carrier into a toner image using the developer, a transfer device that transfers the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing device that fixes the toner image transferred to the surface of the recording medium.
[0203] The image forming method according to this embodiment may be a first image forming method using the above-mentioned developer as a replenishment developer, or a second image forming method using the above-mentioned developer as an initial filling developer. The first image forming method includes an image forming method having a charging step of charging the surface of an image holder, an electrostatic image forming step of forming an electrostatic image on the charged surface of the image holder, a developing step of developing the electrostatic image formed on the surface of the image holder as a toner image using a developer including a replenishment developer, which is the aforementioned developer, replenished from a developer cartridge, a transfer step of transferring the toner image formed on the surface of the image holder to the surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium. An example of a second image forming method is an image forming method having a charging step of charging the surface of an image holder, an electrostatic image forming step of forming an electrostatic image on the charged surface of the image holder, a developing step of developing the electrostatic image formed on the surface of the image holder as a toner image using the initial filling developer, which is the aforementioned developer contained in a developing device, a transfer step of transferring the toner image formed on the surface of the image holder to the surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.
[0204] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.
[0205] (First image forming apparatus and first image forming method) An example of a first image forming apparatus and a first image forming method will be described with reference to the drawings. The image forming apparatus shown in FIG. 1 is configured to employ a trickle development method in which the aforementioned developer contained in a developer cartridge as a replenishment developer is supplied to a developer storage container in the developing device by a developer supplying means, and at least a portion of the developer contained in the developer storage container is discharged by a developer discharging means. The image forming apparatus shown in FIG. 1 is configured to employ a reclaim system in which residual toner remaining on the surface of the image carrier is collected by a cleaning device and returned to the developing device for reuse.
[0206] The image forming apparatus 100 includes an image carrier 110 that rotates in a clockwise direction indicated by an arrow a in FIG. 1 , a charging device 120 that is provided above the image carrier 110 and facing the image carrier 110 and that negatively charges the surface of the image carrier 110, an electrostatic image forming device 130 that writes an image to be formed with a developer (toner) on the surface of the image carrier 110 charged by the charging device 120 to form an electrostatic image, a developing device 140 that is provided downstream of the electrostatic image forming device 130 and that applies toner to the electrostatic image formed by the electrostatic image forming device 130 to form a toner image on the surface of the image carrier 110, and an image developing device 140 that is provided downstream of the electrostatic image forming device 130 and that forms a toner image on the surface of the image carrier 110 by applying toner to the electrostatic image formed by the electrostatic image forming device 130, and an image developing device 150 that develops the image. The image forming apparatus includes an endless belt-like intermediate transfer belt 150 that travels in the direction indicated by arrow b while in contact with the holder 110 and transfers a toner image formed on the surface of the image holder 110, a discharge device 160 that discharges the surface of the image holder 110 after the toner image has been transferred to the intermediate transfer belt 150 to make it easier to remove the residual toner remaining on the surface, a cleaning device 170 that serves as residual toner recovery means for removing and recovering the residual toner on the surface of the image holder 110, and residual toner transport means 174 that transports the residual toner removed and recovered by the cleaning device 170 and supplies it to the developing device 140.
[0207] The charging device 120, the electrostatic image forming device 130, the developing device 140, the intermediate transfer belt 150, the charge removing device 160, and the cleaning device 170 are arranged in a clockwise direction on a circumference surrounding the image carrier 110.
[0208] The intermediate transfer belt 150 is held in a tensioned state by support rolls 150A and 150B, a back roll 150C, and a drive roll 150D from the inside, and is driven in the direction of arrow b with the rotation of the drive roll 150D. A primary transfer roll 151 is provided at a position facing the image carrier 110 on the inside of the intermediate transfer belt 150, which positively charges the intermediate transfer belt 150 and causes the toner on the image carrier 110 to be attracted to the outer surface of the intermediate transfer belt 150. A secondary transfer roll 152 is provided on the outside below the intermediate transfer belt 150, facing the back roll 150C, which positively charges the recording paper P and presses it against the intermediate transfer belt 150, thereby transferring the toner image formed on the intermediate transfer belt 150 onto the recording paper P.
[0209] Further provided below the intermediate transfer belt 150 are a recording medium supplying device 153 that supplies recording paper P to the secondary transfer roll 152, and a fixing device 180 that fixes the toner image while transporting the recording paper P on which the toner image has been formed by the secondary transfer roll 152.
[0210] The recording medium supply device 153 includes a pair of transport rolls 153A and a guide slope 153B that guides the recording paper P transported by the transport rolls 153A toward the secondary transfer roll 152. On the other hand, the fixing device 180 includes fixing rolls 181, which are a pair of heat rolls that fix the toner image by heating and pressing the recording paper P onto which the toner image has been transferred by the secondary transfer roll 152, and a transport conveyor 182 that transports the recording paper P toward the fixing roll 181.
[0211] The recording paper P is transported by the recording medium supplying device 153, the secondary transfer roll 152, and the fixing device 180 in the direction indicated by the arrow c.
[0212] An intermediate transfer body cleaning device 154 having a cleaning blade that removes toner remaining on the intermediate transfer belt 150 after the toner image is transferred to the recording paper P by the secondary transfer roll 152 is provided so as to face the drive roll 150D across the intermediate transfer belt 150.
[0213] The developing device 140 will be described in detail below. The developing device 140 is disposed facing the image carrier 110 in the development area, and has a developer container 141 that contains, for example, a two-component developer containing a toner charged to a negative (-) polarity and a carrier charged to a positive (+) polarity. The developer container 141 has a developer container main body 141A and a developer container cover 141B that closes the upper end of the developer container main body 141A.
[0214] The developer storage container main body 141A has a developing roll chamber 142A that houses the developing roll 142 inside, and has a first stirring chamber 143A adjacent to the developing roll chamber 142A and a second stirring chamber 144A adjacent to the first stirring chamber 143A. Also, a layer thickness regulating member 145 is provided in the developing roll chamber 142A to regulate the layer thickness of the developer on the surface of the developing roll 142 when the developer storage container cover 141B is attached to the developer storage container main body 141A.
[0215] The first stirring chamber 143A and the second stirring chamber 144A are separated by a partition wall 141C, and although not shown, the first stirring chamber 143A and the second stirring chamber 144A are connected at both ends in the longitudinal direction (longitudinal direction of the developing device) of the partition wall 141C, and the first stirring chamber 143A and the second stirring chamber 144A form a circulating stirring chamber (143A+144A).
[0216] In the developing roll chamber 142A, the developing roll 142 is disposed so as to face the image carrier 110. The developing roll 142 is a magnetic roll (fixed magnet) having magnetism, but a sleeve is provided on the outside of the developing roll 142. The developer in the first mixing chamber 143A is attracted to the surface of the developing roll 142 by the magnetic force of the magnetic roll, and is transported to the development area. The developing roll 142 has a roll shaft supported by the developer storage container main body 141A so as to be freely rotatable. Here, the developing roll 142 and the image carrier 110 rotate in opposite directions, and the developer attracted to the surface of the developing roll 142 at the opposing portion is transported to the development area from the same direction as the moving direction of the image carrier 110.
[0217] In addition, a bias power supply (not shown) is connected to the sleeve of the developing roll 142 so that a predetermined developing bias is applied (in this embodiment, a bias in which an alternating current component (AC) is superimposed on a direct current component (DC) is applied so that an alternating electric field is applied to the developing area).
[0218] The first stirring chamber 143A and the second stirring chamber 144A are provided with a first stirring member 143 (stirring / transporting member) and a second stirring member 144 (stirring / transporting member) for stirring and transporting the developer. The first stirring member 143 is composed of a first rotating shaft extending in the axial direction of the developing roll 142 and a stirring / transporting blade (projection) fixed in a spiral shape to the outer periphery of the rotating shaft. Similarly, the second stirring member 144 is composed of a second rotating shaft and a stirring / transporting blade (projection). The stirring members are supported rotatably by the developer storage container main body 141A. The first stirring member 143 and the second stirring member 144 are arranged so that the developers in the first stirring chamber 143A and the second stirring chamber 144A are transported in opposite directions by their rotation.
[0219] One end of developer supplying means 146 for supplying replenishment developer to the second stirring chamber 144A is connected to one end of the second stirring chamber 144A in the longitudinal direction, and a developer cartridge 147 containing replenishment developer is connected to the other end of the developer supplying means 146. In addition, one end of developer discharging means 148 for discharging the contained developer is also connected to one end of the second stirring chamber 144A in the longitudinal direction, and the other end of the developer discharging means 148 is connected to a developer recovery container (not shown) for recovering the discharged developer.
[0220] In this way, the developing device 140 employs a so-called trickle development method in which replenishment developer is supplied from the developer cartridge 147 to the developing device 140 (second stirring chamber 144A) via developer supply means 146, and old developer is discharged from developer discharge means 148. Specifically, the trickle development method is a development method in which replenishment developer (trickle developer) is gradually supplied into the developing device in order to suppress deterioration of the charging performance of the developer and extend the interval between developer replacements, while development is performed while discharging excess deteriorated developer (containing a large amount of deteriorated carrier).
[0221] Next, the cleaning device 170 will be described in detail. The cleaning device 170 includes a housing 171 and a cleaning blade 172 arranged to protrude from the housing 171. The cleaning blade 172 is a plate-like member extending in the axial direction of the rotation shaft of the image carrier 110, and is provided so that a tip portion (edge portion) of the cleaning blade 172 comes into contact with the image carrier 110 downstream in the rotation direction (direction of arrow a) from a transfer position by the primary transfer roll 151 and downstream in the rotation direction from a position where the static electricity is removed by the static electricity removing device 160.
[0222] As the image carrier 110 rotates in the direction of arrow a, the cleaning blade 172 intercepts and removes foreign matter such as residual toner that has not been transferred to the intermediate transfer belt 150 by the primary transfer roll 151 and is attached to the image carrier 110 from the image carrier 110.
[0223] A transport member 173 is disposed at the bottom inside the housing 171, and one end of residual toner transport means 174 is connected to the downstream side of the transport member 173 in the transport direction in the housing 171 for transporting and supplying the residual toner (developer) removed and collected by the cleaning blade 172 to the developing device 140. The other end of the residual toner transport means 174 is connected to join the developer supply means 146.
[0224] In this manner, the cleaning device 170 transports the residual toner through the residual toner transport means 174 to the developing device 140 (second mixing chamber 144A) as the transport member 173 provided at the bottom of the housing 171 rotates, and the residual toner recovered from the surface of the image carrier 110 is stirred and transported together with the developer (toner) contained in the developing device 140 and reused.
[0225] In the reclaim type image forming apparatus according to the present embodiment, for example, a portion including the developer cartridge may be a cartridge structure (first process cartridge) that is detachably attached to the image forming apparatus. For example, a process cartridge that is detachably attached to the image forming apparatus and includes a developer cartridge that contains the above-mentioned developer as a replenishment developer, a developing device that contains a developer including the replenishment developer replenished from the developer cartridge and develops an electrostatic charge image formed on the surface of an image carrier with the developer as a toner image, a developer supplying means that supplies the replenishment developer contained in the developer cartridge to the developing device, and a developer discharging means that discharges a part of the developer contained in the developing device is preferably used.
[0226] (Second image forming apparatus and second image forming method) An example of the second image forming apparatus and the second image forming method will be described with reference to the drawings. The image forming apparatus shown in Fig. 2 includes first to fourth electrophotographic image forming units 10Y, 10M, 10C, and 10K that output images of the respective colors of yellow (Y), magenta (M), cyan (C), and black (K) based on color-separated image data. These image forming units (hereinafter sometimes simply referred to as "units") 10Y, 10M, 10C, and 10K are arranged in parallel at predetermined distances from each other in the horizontal direction. These units 10Y, 10M, 10C, and 10K may be process cartridges that are detachable from the image forming apparatus.
[0227] Above each of the units 10Y, 10M, 10C, and 10K in the drawing, an intermediate transfer belt 20 is provided as an intermediate transfer body extending through each unit. The intermediate transfer belt 20 is provided wound around a drive roll 22 and a support roll 24 that are arranged from left to right in the drawing at a distance from each other and contact the inner surface of the intermediate transfer belt 20, and is adapted to run in a direction from the first unit 10Y to the fourth unit 10K. Note that a force is applied to the support roll 24 in a direction away from the drive roll 22 by a spring or the like (not shown), and tension is applied to the intermediate transfer belt 20 wound around them. In addition, an intermediate transfer body cleaning device 30 is provided on the image carrier side of the intermediate transfer belt 20, facing the drive roll 22. Further, the developing devices 4Y, 4M, 4C, and 4K of the units 10Y, 10M, 10C, and 10K are supplied with toner including four colors of toner, yellow, magenta, cyan, and black, contained in toner cartridges 8Y, 8M, 8C, and 8K, respectively.
[0228] Since the first to fourth units 10Y, 10M, 10C, and 10K have the same configuration, the first unit 10Y that forms a yellow image and is disposed upstream in the direction in which the intermediate transfer belt travels will be described here as a representative example. Note that by assigning reference numerals of magenta (M), cyan (C), and black (K) instead of yellow (Y) to parts equivalent to those of the first unit 10Y, descriptions of the second to fourth units 10M, 10C, and 10K will be omitted.
[0229] The first unit 10Y has a photoconductor 1Y that acts as an image carrier. Around the photoconductor 1Y, a charging roll (an example of a charging device) 2Y that charges the surface of the photoconductor 1Y to a predetermined potential, an exposure device (an example of an electrostatic image forming device) 3 that exposes the charged surface to a laser beam 3Y based on a color-separated image signal to form an electrostatic image, a developing device 4Y that supplies charged toner to the electrostatic image to develop it, a primary transfer roll 5Y (an example of a primary transfer device) that transfers the developed toner image onto an intermediate transfer belt 20, and a photoconductor cleaning device (an example of a cleaning device) 6Y that removes toner remaining on the surface of the photoconductor 1Y after the primary transfer are arranged in this order. The primary transfer roll 5Y is disposed inside the intermediate transfer belt 20 and is provided at a position facing the photoconductor 1Y. Furthermore, a bias power supply (not shown) that applies a primary transfer bias is connected to each of the primary transfer rolls 5Y, 5M, 5C, and 5K. Each bias power supply varies the transfer bias applied to each primary transfer roll under the control of a control unit (not shown).
[0230] Hereinafter, an operation of forming a yellow image in first unit 10Y will be described. First, prior to operation, the surface of the photoconductor 1Y is charged to a potential of −600V to −800V by the charging roll 2Y. The photoconductor 1Y has a conductivity (for example, a volume resistivity at 20° C. of 1×10 -6 The photosensitive layer is formed by laminating a photosensitive layer on a substrate having a resistivity of Ωcm or less. This photosensitive layer is usually highly resistive (the resistance of ordinary resins), but when irradiated with a laser beam 3Y, the resistivity of the portion irradiated with the laser beam changes. A laser beam 3Y is output to the charged surface of the photoreceptor 1Y via an exposure device 3 in accordance with image data for yellow sent from a control unit (not shown). The laser beam 3Y is irradiated onto the photosensitive layer on the surface of the photoreceptor 1Y, and an electrostatic charge image of a yellow image pattern is formed on the surface of the photoreceptor 1Y.
[0231] An electrostatic image is an image formed on the surface of the photoconductor 1Y by electrostatic charging. The laser beam 3Y reduces the resistivity of the irradiated parts of the photosensitive layer, causing the charged charges on the surface of the photoconductor 1Y to flow, while the charges remain in the parts not irradiated by the laser beam 3Y. This is a so-called negative latent image. The electrostatic image formed on the photoconductor 1Y is rotated to a predetermined developing position as the photoconductor 1Y travels. Then, at this developing position, the electrostatic image on the photoconductor 1Y is made visible as a toner image (developed image) by the developing device 4Y.
[0232] The developing device 4Y contains an electrostatic image developer including at least yellow toner and a carrier, for example. The yellow toner is triboelectrically charged by being stirred inside the developing device 4Y, and is held on a developer roll (an example of a developer holder) with a charge of the same polarity (negative polarity) as the charge on the photoconductor 1Y. As the surface of the photoconductor 1Y passes through the developing device 4Y, the yellow toner electrostatically adheres to the discharged latent image portion on the surface of the photoconductor 1Y, and the latent image is developed with the yellow toner. The photoconductor 1Y on which the yellow toner image has been formed continues to travel at a predetermined speed, and the toner image developed on the photoconductor 1Y is transported to a predetermined primary transfer position.
[0233] When the yellow toner image on the photoconductor 1Y is transported to the primary transfer position, a primary transfer bias is applied to the primary transfer roll 5Y, and an electrostatic force from the photoconductor 1Y toward the primary transfer roll 5Y acts on the toner image, and the toner image on the photoconductor 1Y is transferred onto the intermediate transfer belt 20. The transfer bias applied at this time has a polarity (+) opposite to the polarity (-) of the toner, and in the first unit 10Y, for example, it is controlled to +10 μA by a control unit (not shown). On the other hand, the toner remaining on the photoconductor 1Y is removed and collected by the photoconductor cleaning device 6Y.
[0234] Further, the primary transfer bias applied to the primary transfer rolls 5M, 5C, and 5K subsequent to the second unit 10M is also controlled in accordance with the first unit. In this manner, the intermediate transfer belt 20 onto which the yellow toner image has been transferred by the first unit 10Y is conveyed successively through the second to fourth units 10M, 10C, and 10K, where the toner images of the respective colors are transferred in a superimposed manner.
[0235] The intermediate transfer belt 20 onto which the four color toner images have been transferred in multiple layers through the first to fourth units reaches a secondary transfer section that is composed of the intermediate transfer belt 20, a support roll 24 that contacts the inner surface of the intermediate transfer belt, and a secondary transfer roll (an example of a secondary transfer device) 26 arranged on the image carrying surface side of the intermediate transfer belt 20. Meanwhile, a recording paper (an example of a recording medium) P is fed at a predetermined timing into the gap between the secondary transfer roll 26 and the intermediate transfer belt 20 via a supply mechanism, and a secondary transfer bias is applied to the support roll 24. The transfer bias applied at this time has a (-) polarity that is the same as the (-) polarity of the toner, and an electrostatic force from the intermediate transfer belt 20 toward the recording paper P acts on the toner image, so that the toner image on the intermediate transfer belt 20 is transferred onto the recording paper P. The secondary transfer bias at this time is determined according to the resistance detected by a resistance detection means (not shown) that detects the resistance of the secondary transfer section, and is voltage controlled.
[0236] Thereafter, the recording paper P is sent to a pressure contact portion (nip portion) of a pair of fixing rolls in the fixing device 28, where the toner image is fixed onto the recording paper P, forming a fixed image.
[0237] The recording paper P onto which the toner image is transferred can be, for example, plain paper used in electrophotographic copying machines, printers, etc. In addition to the recording paper P, other examples of the recording medium include overhead projector sheets, etc. To further improve the smoothness of the image surface after fixing, it is preferable that the surface of the recording paper P is also smooth. For example, coated paper in which the surface of ordinary paper is coated with resin or the like, art paper for printing, or the like is preferably used.
[0238] After the color image has been fixed, the recording paper P is conveyed toward the discharge section, and the series of color image forming operations is completed. EXAMPLES
[0239] Examples will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0240] [Preparation of specific resin particle dispersion] <Preparation of specific resin particle dispersion 1> Styrene: 47.9 parts n-Butyl acrylate: 51.8 parts 2-Carboxyethyl acrylate: 0.3 parts Anionic surfactant (Dow Chemical Company, Dowfax2A1): 0.8 parts 1,10-Decanediol diacrylate: 1.65 parts The above raw materials were mixed and dissolved, and 60 parts of ion-exchanged water was added thereto, followed by dispersion and emulsification in a flask to prepare an emulsion. Next, 1.3 parts of an anionic surfactant (Dowfax2A1, manufactured by The Dow Chemical Company) The resulting material was dissolved in 90 parts of ion-exchanged water, 1 part of the emulsion was added thereto, and then 10 parts of ion-exchanged water in which 5.4 parts of ammonium persulfate had been dissolved was added. The remainder of the emulsion was then added over a period of 180 minutes, and the atmosphere in the flask was replaced with nitrogen.The solution in the flask was then heated to 65°C in an oil bath while stirring, and emulsion polymerization was continued for 500 minutes, after which a specific resin particle dispersion 1 was obtained with a solids content adjusted to 24.5% by mass. The results obtained by the above-mentioned methods for the resin particles contained in the obtained specific resin particle dispersion 1 are as follows. Glass transition temperature Tg determined from dynamic viscoelasticity measurement: 32.1℃ Minimum storage modulus G'(p90-150): 2.6×10 5 Pa Maximum value of storage modulus G'(p90-150): 5.1×10 5 Pa Minimum loss tangent tanδ in the range of 30°C to 150°C: 0.028 Maximum loss tangent tanδ in the range of 30°C to 150°C: 2.35 Minimum loss tangent tanδ in the range of 65°C to 150°C: 0.028 Maximum loss tangent tanδ in the range of 65°C to 150°C: 0.203 Number average particle size: 153 nm SP value (S): 9.07
[0241] <Preparation of specific resin particle dispersion 2> Specific resin particle dispersion liquid 2 was obtained in the same manner as specific resin particle dispersion liquid 1, except that the amount of styrene added was 54.5 parts, the amount of n-butyl acrylate added was 44.6 parts, the amount of 2-carboxyethyl acrylate added was 0.84 parts, and the total amount of anionic surfactant added was 1.26 parts. The results of the resin particles contained in the obtained specific resin particle dispersion 2 obtained by the above-mentioned methods are as follows. Glass transition temperature Tg determined from dynamic viscoelasticity measurement: 44.3℃ Minimum storage modulus G'(p90-150): 3.8×10 5 Pa Maximum value of storage modulus G'(p90-150): 5.9×10 5 Pa Minimum loss tangent tanδ in the range of 30°C to 150°C: 0.028 Maximum loss tangent tanδ in the range of 30°C to 150°C: 2.41 Minimum loss tangent tanδ in the range of 65°C to 150°C: 0.028 Maximum loss tangent tanδ in the range of 65°C to 150°C: 0.411 Number average particle size: 163 nm SP value (S): 9.09
[0242] [Toner Preparation] <Preparation of amorphous resin particle dispersion 1> Terephthalic acid: 28 parts Fumaric acid: 164 parts Adipic acid: 10 parts Bisphenol A ethylene oxide 2 mole adduct: 26 parts Bisphenol A propylene oxide 2 mole adduct: 542 parts The above materials were charged into a reaction vessel equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, the temperature was raised to 190°C over 1 hour, and 1.2 parts of dibutyltin oxide was added per 100 parts of the above materials. The temperature was raised to 240°C over 6 hours while distilling off the generated water, and the dehydration condensation reaction was continued for 3 hours while maintaining the temperature at 240°C, after which the reaction product was cooled.
[0243] The reactant was transferred to a Cavitron CD1010 (Eurotech) at a rate of 100 g per minute while remaining in a molten state. At the same time, ammonia water with a concentration of 0.37% by mass was transferred to the Cavitron CD1010 at a rate of 0.1 liters per minute while being heated to 120°C in a heat exchanger. The rotor rotation speed was 60 Hz, and the pressure was 5 kg / cm. 2 The Cavitron CD1010 was operated under the conditions above to obtain a resin particle dispersion in which resin particles of an amorphous polyester resin having a volume average particle size of 169 nm were dispersed. Ion-exchanged water was added to the resin particle dispersion to adjust the solid content to 20 mass %, thereby obtaining amorphous resin particle dispersion 1. The SP value (R) of the obtained amorphous polyester resin was 9.41.
[0244] <Preparation of Crystalline Resin Particle Dispersion> 1,10-dodecanedioic acid: 225 parts 1,6-Hexanediol: 143 parts The above materials were charged into a reaction vessel equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, the temperature was raised to 160°C over 1 hour, and 0.8 parts by mass of dibutyltin oxide was added. The temperature was raised to 180°C over 6 hours while distilling off the generated water, and the dehydration condensation reaction was continued for 5 hours while maintaining the temperature at 180°C. Thereafter, the temperature was gradually raised to 230°C under reduced pressure, and stirring was performed for 2 hours while maintaining the temperature at 230°C. The reactant was then cooled. After cooling, solid-liquid separation was performed, and the solid was dried to obtain a crystalline polyester resin.
[0245] Crystalline polyester resin: 100 parts Methyl ethyl ketone: 40 parts Isopropyl alcohol: 30 parts 10% ammonia solution: 6 parts The above materials were added to a 3-liter jacketed reaction tank (manufactured by Tokyo Rikakikai Co., Ltd.: BJ-30N) equipped with a condenser, a thermometer, a water dropping device, and an anchor blade, and the resin was dissolved while stirring and mixing at 100 rpm while maintaining the temperature at 80°C in a water circulation type thermostatic bath. Thereafter, the water circulation type thermostatic bath was set to 50°C, and a total of 400 parts of ion-exchanged water kept at 50°C was dropped at a rate of 7 parts by mass / min to cause phase inversion, thereby obtaining an emulsion. 576 parts by mass of the obtained emulsion and 500 parts by mass of ion-exchanged water were placed in a 2-liter eggplant flask, and set in an evaporator (manufactured by Tokyo Rikakikai Co., Ltd.) equipped with a vacuum control unit via a trap ball. The eggplant flask was rotated and heated in a hot water bath at 60°C, and the pressure was reduced to 7 kPa while paying attention to bumping, and the solvent was removed. The volume average particle size D50v of the resin particles in this dispersion was 185 nm. Thereafter, ion-exchanged water was added to obtain a crystalline resin particle dispersion liquid with a solid content concentration of 22.1% by mass.
[0246] <Preparation of Colorant Dispersion> Cyan pigment (Dainichi Seikagaku Co., Ltd., Pigment Blue 15:3 (copper phthalocyanine)): 98 parts Anionic surfactant (Tayca Power, manufactured by Tayca Corporation): 2 parts Ion-exchanged water: 420 parts The above ingredients were mixed and dissolved, and dispersed for 10 minutes using a homogenizer (IKA Ultra Turrax), to obtain a colorant dispersion having a median particle size of 164 nm and a solid content of 21.1% by mass.
[0247] <Preparation of release agent dispersion> Synthetic wax (Nippon Seiro Co., Ltd., FNP92, melting temperature Tw: 92℃): 50 parts Anionic surfactant (Tayca Power, manufactured by Tayca Corporation): 1 part - Ion-exchanged water: 200 parts The above materials were mixed and heated to 130°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a Manton-Gaulin high pressure homogenizer (Gaulin) to obtain a release agent dispersion (solid content 20% by mass) in which release agent particles were dispersed. The volume average particle size of the release agent particles was 214 nm.
[0248] <Preparation of Toner 1> ·Amorphous resin particle dispersion 1: 169 parts ·Specified resin particle dispersion liquid 1: 33 parts ·Crystalline resin particle dispersion: 53 parts Release agent dispersion: 25 parts Colorant dispersion: 33 parts Anionic surfactant (Dow Chemical Company, Dowfax2A1): 4.8 parts The above raw materials, the liquid temperature of which had been adjusted to 10° C., were placed in a 3 L cylindrical stainless steel container, and dispersed and mixed for 2 minutes while applying shear force at 4000 rpm using a homogenizer (IKA Ultra Turrax T50). Next, 1.75 parts of a 10% aqueous solution of aluminum sulfate in nitric acid was gradually added dropwise as a flocculant, and the homogenizer was rotated at 10,000 rpm for 10 minutes to disperse and mix, thereby obtaining a raw dispersion liquid.
[0249] The raw material dispersion was then transferred to a polymerization kettle equipped with a stirrer using two paddle stirrers and a thermometer, and the stirring speed was set to 550 rpm and heating was started with a mantle heater to promote the growth of aggregated particles at 40°C. At this time, the pH of the raw material dispersion was controlled in the range of 2.2 to 3.5 with 0.3 M nitric acid and 1 M sodium hydroxide aqueous solution. The pH was maintained in the above range for about 2 hours to form aggregated particles. Next, a dispersion liquid obtained by mixing 1:21 parts of amorphous resin particle dispersion liquid and 1:8 parts of specific resin particle dispersion liquid was added, and the mixture was held for 60 minutes to allow the binder resin and specific resin particles to adhere to the surfaces of the aggregated particles.The temperature was further increased to 53°C, and then 1:21 parts of amorphous resin particle dispersion liquid was added, and the mixture was held for 60 minutes to allow the binder resin particles to adhere to the surfaces of the aggregated particles.
[0250] The aggregated particles were adjusted while checking the particle size and morphology with an optical microscope and a Multisizer 3. Thereafter, the pH was adjusted to 7.8 using a 5% aqueous sodium hydroxide solution, and maintained for 15 minutes. Thereafter, in order to fuse the aggregated particles, the pH was increased to 8.0, and the temperature was increased to 85° C. After confirming with an optical microscope that the aggregated particles had fused, heating was stopped after 2 hours, and the mixture was cooled at a temperature decreasing rate of 1.0° C. / min. Thereafter, the mixture was sieved through a 20 μm mesh, repeatedly washed with water, and then dried in a vacuum dryer to obtain toner particles 1 having a volume average particle size of 5.3 μm.
[0251] 100 parts of the obtained toner particles and 0.7 parts of dimethyl silicone oil-treated silica particles (RY200 manufactured by Nippon Aerosil Co., Ltd.) were mixed in a Henschel mixer to obtain toner 1.
[0252] <Preparation of Toner 2> Toner 2 was obtained in the same manner as Toner 1, except that instead of specific resin particle dispersion 1, a specific resin particle dispersion of the type shown in Table 1 was used in an amount such that the content of resin particles (i.e., specific resin particles) relative to the total amount of toner particles was the value shown in Table 1.
[0253] <Preparation of Toner 3> Toner 3 was obtained in the same manner as Toner 1, except that specific resin particle dispersion 1 was used in an amount such that the content of specific resin particles relative to the total toner particles was the value shown in Table 1, and the amount of crystalline resin particle dispersion added was adjusted so that the content of crystalline resin relative to the total binder resin was the value shown in Table 1.
[0254] <Preparation of Toner 4> Toner 4 was obtained in the same manner as Toner 1, except that the rotation speed of the homogenizer was changed from 10,000 rpm to 5,000 rpm.
[0255] <Preparation of Toner 5> Toner 5 was obtained in the same manner as Toner 1, except that specific resin particle dispersion 1 was used in an amount such that the content of specific resin particles relative to the total toner particles was the value shown in Table 1, and the pH during fusion of the aggregated particles was changed from 8.0 to 6.0.
[0256] <Preparation of Toner 6> Toner 6 was obtained in the same manner as Toner 1, except that the pH during fusion of the aggregated particles was changed from 8.0 to 6.5, the temperature after heating was changed from 85°C to 75°C, and 5.2 parts of anionic surfactant (Dowfax2A1, manufactured by The Dow Chemical Company) was added when the temperature reached 75°C.
[0257] <Preparation of Toner C1> ·Amorphous resin particle dispersion 1: 169 parts ·Specified resin particle dispersion 1: 41 parts ·Crystalline resin particle dispersion: 53 parts Release agent dispersion: 25 parts Colorant dispersion: 33 parts Anionic surfactant (Dow Chemical Company, Dowfax2A1): 4.8 parts The above raw materials, the liquid temperature of which had been adjusted to 30° C., were placed in a 3 L cylindrical stainless steel container, and dispersed and mixed for 2 minutes while applying shear force at 4000 rpm using a homogenizer (IKA Ultra Turrax T50). Next, 1.75 parts of a 10% aqueous solution of aluminum sulfate in nitric acid was gradually added dropwise as a flocculant, and the mixture was dispersed and mixed for 3 minutes at a homogenizer speed of 4000 rpm to obtain a raw dispersion liquid.
[0258] The raw material dispersion was then transferred to a polymerization kettle equipped with a stirrer using two paddle stirrers and a thermometer, and the stirring speed was set to 550 rpm and heating was started with a mantle heater to promote the growth of aggregated particles at 40°C. At this time, the pH of the raw material dispersion was controlled in the range of 2.2 to 3.5 with 0.3 M nitric acid and 1 M sodium hydroxide aqueous solution. The pH was maintained in the above range for about 2 hours to form aggregated particles. Next, 1:42 parts of the amorphous resin particle dispersion liquid was further added and held for 60 minutes to allow the resin particles of the binder resin to adhere to the surfaces of the aggregated particles.
[0259] The aggregated particles were adjusted while checking the particle size and morphology with an optical microscope and a Multisizer 3. Thereafter, the pH was adjusted to 7.8 using a 5% aqueous sodium hydroxide solution, and maintained for 15 minutes. Thereafter, in order to fuse the aggregated particles, the pH was increased to 8.0, and the temperature was increased to 85° C. After confirming that the aggregated particles had fused using an optical microscope, heating was stopped after 2 hours, and the mixture was cooled at a temperature drop rate of 1.0° C. / min. Thereafter, the mixture was sieved through a 20 μm mesh, repeatedly washed with water, and then dried in a vacuum dryer to obtain toner particles C1.
[0260] 100 parts of the obtained toner particles and 0.7 parts of dimethyl silicone oil-treated silica particles (RY200 manufactured by Nippon Aerosil Co., Ltd.) were mixed in a Henschel mixer to obtain toner C1.
[0261] Table 1 shows the type of specific resin particle dispersion ("Particle type" in the table), the content of specific resin particles relative to the entire toner particles ("Particle content (%)" in the table), and the content of crystalline resin relative to the entire binder resin ("Crystalline resin content (%)" in the table). Table 1 also shows the ratio of the crystalline resin content to the specific resin particle content in the obtained toner ("Crystalline content ratio vs. particles" in the table) and the ratio of the amorphous resin content to the specific resin particle content ("Amorphous content ratio vs. particles" in the table). Table 1 also shows the volume average particle size of the toner particles in the obtained toner.
[0262] Table 1 also shows the results of the storage modulus G' of the excluded components in the range of 30°C or higher and 50°C or lower ("30-50°C G' (Pa)" in the table), the temperature at which the specific elastic modulus is reached ("Attained temperature (°C)" in the table), and the loss tangent tanδ at the specific elastic modulus reaching temperature ("Attained temperature tanδ" in the table), all determined using the methods described above. Table 2 also shows the results of determining, by the above-mentioned method, for the obtained toner, D1(90), D50(90), D1(150), D50(150), D50(150)-D1(150) values ("Difference (150)" in the table), D50(90)-D1(90) value ("Difference (90)" in the table), number average molecular weight of the THF-soluble matter in the toner particles ("Mn" in the table), storage modulus G' in the range of 30°C or higher and 50°C or lower ("30-50 G'(Pa)" in the table), specific elastic modulus attainment temperature ("Attainment temperature (°C)" in the table), logG'(t90-150)-logG'(r90-150) value ("Viscoelastic difference" in the table), and difference (SP value(S)-SP value(R)) ("SP value difference" in the table).
[0263] [Table 1]
[0264] [Table 2]
[0265] [Creating the carrier] <Preparation of magnetic particles 1> Fe2O3, Mn(OH)2, Mg(OH)2, SiO2, SrCO3, and CaCO3 were mixed in the amounts shown in Table 3, and then a dispersant, water, and zirconia beads with a media diameter of 1 mm were added and crushed and mixed in a sand mill. The zirconia beads were filtered and dried, and then pre-fired in a rotary kiln at 20 rpm and 900°C to obtain a mixed oxide. Next, a dispersant and water were added, and then 6.6 parts by mass of polyvinyl alcohol was added, and the mixture was pulverized in a wet ball mill until the volume average particle size (i.e., the crushed particle size of the slurry) reached the value shown in Table 3. The mixture was then granulated and dried in a spray dryer until the dry particle size reached the value shown in Table 3. The mixture was then sintered in an electric furnace at a temperature of 1220°C for 5 hours in an oxygen-nitrogen mixed atmosphere with an oxygen concentration of 1%. The resulting particles were subjected to a crushing process and a classification process, and then heated in a rotary kiln at 15 rpm and 900°C for 2 hours, and similarly subjected to a classification process to obtain magnetic particles 1. Table 4 shows the mean irregularity spacing Sm, arithmetic mean roughness Ra, volume average particle size ("Particle size" in the table), and BET specific surface area ("BET" in the table) of the obtained magnetic particles 1.
[0266] <Preparation of Magnetic Particles 2 to 12 and C1 to C4> Magnetic particles 2 to 12 and C1 to C4 were each produced in the same manner as magnetic particle 1, except for changing the composition and reaction conditions to those in Table 3. The average projection-recess spacing Sm, arithmetic mean roughness Ra, volume average particle size ("Particle size" in the table), and BET specific surface area ("BET" in the table) of the obtained magnetic particles 2 to 12 and C1 to C4 are respectively shown in Table 4.
[0267] [Table 3]
[0268] <Preparation of Coating Agent> Cyclohexyl methacrylate (weight average molecular weight: 50,000): 30 parts Carbon black (Cabot VXC72): 0.5 parts Toluene: 250 parts Isopropyl alcohol: 50 parts The above materials and glass beads (diameter 1 mm, same amount as toluene) were placed in a sand mill and stirred at a rotation speed of 190 rpm for 30 minutes to obtain a coating agent with a solid content of 9 mass %.
[0269] <Preparation of Carriers 1 to 14 and C1 to C4> 1,000 parts of the magnetic particles shown in Table 4 and the amount of the coating agent shown in Table 4 were put into a kneader and mixed at room temperature (25° C.) for 20 minutes. Then, the mixture was heated to 70° C. and dried under reduced pressure. The dried product was then removed from the kneader and sieved through a 75 μm mesh to remove coarse powder, yielding carriers 1 to 14 and C1 to C4. The average thickness of the resin layer and the exposed area ratio of the magnetic particles in the resulting carriers are also shown in Table 4.
[0270] [Table 4]
[0271] [Preparation and evaluation of developer] <Gloss Difference> An initial filling developer was obtained by mixing 8 parts of the toner shown in Table 5 and 100 parts of the carrier shown in Table 5. The Sm-D1(90) value, Ra+0.3×D1(90) value, and Ra+0.3×D50(150) value for the obtained developer are also shown in Table 5.
[0272] The developer obtained was filled into the developing unit of a color copier ApeosPortIV C3370 (manufactured by Fujifilm Business Innovation Co., Ltd.) from which the fixing unit had been removed, and the toner loading amount was 0.45 mg / cm 2 The unfixed image was output by adjusting the image density so that the image density was adjusted to the following value. The recording medium used was A4 size OS coated W paper (127 gsm basis weight) manufactured by Fujifilm Business Innovation Co., Ltd. The output image was a 50 mm x 50 mm image with a 100% image density.
[0273] The fixing evaluation device used was an ApeosPortIV C3370 manufactured by FUJIFILM Business Innovation Co., Ltd., whose fixing unit had been removed and modified so that the nip pressure and fixing temperature could be changed. The process speed was 175 mm / sec. Under these conditions, the unfixed image was fixed under low temperature and low pressure conditions (specifically, the temperature of the fixing unit was 120 degrees and the nip pressure was 1.6 kgf / cm 2 ) and high temperature and pressure conditions (specifically, the fixing unit temperature was 180 degrees and the nip pressure was 6.0 kgf / cm 2 The image was fixed under two conditions, and a fixed image was obtained. The gloss of the fixed image was measured at 60° gloss using a BYK Micro Trigloss glossmeter, and the gloss difference between the fixed image under low temperature and low pressure conditions and the fixed image under high temperature and high pressure conditions (i.e., gloss condition difference) was calculated. The results are shown in Table 5. In addition, when the gloss difference is less than 5, it is difficult to visually recognize the gloss difference, when the gloss difference is 5 or more but less than 10, the gloss difference is visually noticeable but is slight, when the gloss difference is 10 or more but less than 15, the gloss difference is visible but within the acceptable range, and when the gloss difference is 15 or more, the gloss difference is large and outside the acceptable range.
[0274] <Focus> A replenishment developer was obtained by mixing 300 parts of the toner shown in Table 5 and 60 parts of the carrier shown in Table 5. The Sm-D1(90) value, Ra+0.3×D1(90) value, and Ra+0.3×D50(150) value of the obtained developer are as shown in Table 5. The obtained refill developer was filled into a developer cartridge for an image forming apparatus (DC VII C7773). This was stored in an individual box as per the product, and left for one month under conditions of 30°C and 95% RH with the developer outlet facing down. After that, as a tapping process, it was dropped under its own weight from a height of 5 cm 100 times. The developer cartridge after the tapping process was placed in an image forming apparatus (DC VII C7773) in an environment of 28°C and 98% RH, and 100 A4-sized solid images were printed on a recording medium, i.e., a blank sheet (i.e., an image with 0% image density) was then printed, and the state of toner fogging on the blank sheet was confirmed and evaluated according to the following criteria. The results are shown in Table 5. G1: No toner fogging when observed with a 25x magnifying glass G2: When observed with a 25x magnifying glass, only a few particles of toner were observed. G3: When observed with a 25x magnifying glass, faint toner fogging was observed. G4: Upon visual inspection, slight toner fogging was confirmed. G5: Toner fogging is confirmed by visual inspection.
[0275] [Table 5]
[0276] From the above results, it is understood that the developer of this embodiment has a small difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions, and also suppresses image fog.
[0277] The present embodiment includes the following aspects. (((1))) a toner including toner particles containing a binder resin, wherein in a dynamic viscoelasticity measurement of the toner, when a loss tangent tanδ at a temperature of 90°C and a distortion of 1% is D1(90), a loss tangent tanδ at a temperature of 90°C and a distortion of 50% is D50(90), a loss tangent tanδ at a temperature of 150°C and a distortion of 1% is D1(150), and a loss tangent tanδ at a temperature of 150°C and a distortion of 50% is D50(150), D1(90), D50(90), D1(150), and D50(150) are each 0.5 or more and 2.5 or less, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0; a carrier including magnetic particles having a mean irregularity distance Sm and an arithmetic mean roughness Ra on the surface that satisfy the conditions of 0.5 μm≦Sm≦2.5 μm and 0.3 μm≦Ra≦1.2 μm, and a resin layer adhered to the surface of the magnetic particles; Electrostatic image developer comprising:
[0278] (((2))) The relationship between D1(90) and the average irregularity spacing Sm satisfies the following formula (1), (((1))) Electrostatic image developer according to claim 1. Formula (1): D1(90)≦Sm≦D1(90)+1.1 (((3))) The electrostatic image developer according to (((1))) or (((2))), wherein the relationship between the D1(90) and the arithmetic mean roughness Ra satisfies the following formula (2): Formula (2): 1.05-0.3×D1(90)≦Ra≦1.36-0.3×D1(90) (((4))) The electrostatic image developer according to (((3))), wherein the relationship between the D50(150) and the arithmetic mean roughness Ra satisfies the following formula (3): Formula (3): 1.05-0.3×D50(150)≦Ra≦1.36-0.3×D50(150) (((5))) The electrostatic image developer according to any one of (((1))) to (((4))), wherein an exposed area ratio of the magnetic particles on the surface of the carrier is 4% or more and 20% or less.
[0279] (((6))) The electrostatic image developer according to any one of (((1))) to (((5))), wherein the toner particles further contain resin particles. (((7))) The electrostatic image developer according to (((6))), wherein the resin particles are crosslinked resin particles. (((8))) The electrostatic image developer according to (((7))), wherein the crosslinked resin particles are styrene (meth)acrylic resin particles. (((9))) The electrostatic image developer according to any one of (((1))) to (((8))), wherein the number average molecular weight of a tetrahydrofuran-soluble portion in the toner particles is 5,000 or more and 15,000 or less.
[0280] (((10))) The electrostatic image developer according to any one of (((1))) to (((9))) is contained as a replenishment developer, A developer cartridge that is detachably attached to an image forming apparatus. (((11))) A developer cartridge according to (((10))), a developing device that contains an electrostatic image developer including a replenishment developer replenished from the developer cartridge and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer; The process cartridge is detachably mounted to the image forming apparatus. (((12))) A developer cartridge according to (((10))), An image carrier; a charging device for charging the surface of the image carrier; an electrostatic image forming device for forming an electrostatic image on the charged surface of the image carrier; a developing device that contains an electrostatic image developer including a replenishment developer replenished from the developer cartridge and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer device for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing device for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: (((13))) a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using an electrostatic image developer containing a replenishment developer replenished from the developer cartridge described in (((10))); a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,
[0281] (((14))) a developing device that contains the electrostatic image developer according to any one of (((1))) to (((9))) and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer, A process cartridge that is detachably attached to an image forming apparatus. (((15))) An image carrier; a charging device for charging the surface of the image carrier; an electrostatic image forming device for forming an electrostatic image on the charged surface of the image carrier; a developing device that contains the electrostatic image developer according to any one of (((1))) to (((9))) and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer device for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing device for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: (((16))) a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to any one of (((1))) to (((9))); a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,
[0282] The invention according to (((1))) or (((6))) provides an electrostatic image developer in which the difference in gloss between an image fixed under low-temperature and low-pressure conditions and an image fixed under high-temperature and high-pressure conditions is smaller and image fog is suppressed, as compared with a case in which any of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of 50(90)-D1(90) is 1.0 or more, the average irregularity spacing Sm is less than 0.5 μm or exceeds 2.5 μm, or the arithmetic mean roughness Ra is less than 0.3 μm or exceeds 1.2 μm.
[0283] According to the invention related to (((2))), there is provided an electrostatic image developer in which image fog is suppressed compared to a case in which the relationship between D1(90) and the average irregularity spacing Sm does not satisfy formula (1). According to the invention related to (((3))), there is provided an electrostatic image developer in which image fog is suppressed compared to the case in which the relationship between D1(90) and the arithmetic mean roughness Ra does not satisfy formula (2). According to the invention related to (((4))), there is provided an electrostatic image developer in which image fog is suppressed compared to a case in which the relationship between D50(150) and the arithmetic mean roughness Ra does not satisfy formula (3). According to the invention related to (((5))), there is provided an electrostatic image developer in which image fogging is suppressed compared to when the exposed area ratio of magnetic particles on the carrier surface is less than 4% or exceeds 20%.
[0284] According to the invention related to (((7))), there is provided a toner for developing electrostatic images in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller than when the resin particles are non-crosslinked resin particles. According to the invention related to (((8))), there is provided a toner for developing electrostatic images in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller than when the crosslinked resin particles are polyester resin particles. According to the invention related to (((9))), there is provided an electrostatic image developer in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller and image fog is suppressed, as compared with the case in which the number average molecular weight of the tetrahydrofuran soluble matter is less than 5,000 or more than 15,000.
[0285] According to the invention related to (((10))), (((11))), (((12))), or (((13))), any one of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of D50(90)-D1(90) is 1.0 or more, the mean spacing Sm is less than 0.5 μm or exceeds 2.5 μm, the arithmetic mean roughness Ra is less than 0.3 μm or exceeds 1.2 μm, and the BET specific surface area of the carrier is 0.12 m 2 / g or less than 0.20m 2The present invention provides a developer cartridge, process cartridge, image forming apparatus, or image forming method in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is small and image fogging is suppressed, as compared with the case where an electrostatic image developer having a carrier volume average particle size of more than 26 μm or more than 34 μm is used.
[0286] According to the invention related to (((14))), (((15))), or (((16))), any one of D1(90), D50(90), D1(150), and D50(150) is less than 0.5 or exceeds 2.5, the value of D50(150)-D1(150) is 1.5 or more, the value of D50(90)-D1(90) is 1.0 or more, the mean spacing Sm is less than 0.5 μm or exceeds 2.5 μm, the arithmetic mean roughness Ra is less than 0.3 μm or exceeds 1.2 μm, and the BET specific surface area of the carrier is 0.12 m 2 / g or less than 0.20m 2 The present invention provides a process cartridge, an image forming apparatus, or an image forming method in which the difference in gloss between an image fixed under low temperature and low pressure conditions and an image fixed under high temperature and high pressure conditions is smaller and image fogging is suppressed, as compared to the case in which an electrostatic charge image developer having a viscosity of more than 1000 saturation voltage Vp-value ... [Explanation of symbols]
[0287] 1Y, 1M, 1C, 1K Photoconductor (an example of an image carrier) 2Y, 2M, 2C, 2K Charging roll (example of charging device) 3 Exposure device (an example of an electrostatic image forming device) 3Y, 3M, 3C, 3K laser beam 4Y, 4M, 4C, 4K developing device 5Y, 5M, 5C, 5K Primary transfer roll (part of transfer device) 6Y, 6M, 6C, 6K Photoconductor cleaning device (example of cleaning device) 8Y, 8M, 8C, 8K toner cartridges 10Y, 10M, 10C, 10K Image forming units 20 Intermediate transfer belt (part of the transfer device) 22 Driving Roll 24 Support roll 26 Secondary transfer roll (part of the transfer device) 28 Fixing device 30 Intermediate transfer body cleaning device 100 Image forming device 110 Image holder 120 Charging device 130 Electrostatic image forming device 140 Developing device 141 Developer container 146 Developer supply means 147 Developer Cartridge 148 Developer discharge means 150 Intermediate transfer belt (part of the transfer device) 151 Primary transfer roll (part of transfer device) 152 Secondary transfer roll (part of transfer device) 170 Cleaning device 174 Residual toner transport means 180 Fixing device P Recording paper (an example of a recording medium)
Claims
1. a toner including toner particles containing a binder resin, wherein, in a dynamic viscoelasticity measurement of the toner, when a loss tangent tan δ at a temperature of 90° C. and a distortion of 1% is D1(90), a loss tangent tan δ at a temperature of 90° C. and a distortion of 50% is D50(90), a loss tangent tan δ at a temperature of 150° C. and a distortion of 1% is D1(150), and a loss tangent tan δ at a temperature of 150° C. and a distortion of 50% is D50(150), D1(90), D50(90), D1(150), and D50(150) are each 0.5 to 2.5, the value of D50(150)-D1(150) is less than 1.5, and the value of D50(90)-D1(90) is less than 1.0; a carrier including magnetic particles having a mean irregularity distance Sm and an arithmetic mean roughness Ra on the surface that satisfy 0.5 μm≦Sm≦2.5 μm and 0.3 μm≦Ra≦1.2 μm, and a resin layer adhered to the surface of the magnetic particles; Electrostatic image developer comprising:
2. 2. The electrostatic image developer according to claim 1, wherein the relationship between D1(90) and the average irregularity spacing Sm satisfies the following formula (1): Formula (1): D1(90)≦Sm≦D1(90)+1.1
3. 2. The electrostatic image developer according to claim 1, wherein the relationship between the D1(90) and the arithmetic mean roughness Ra satisfies the following formula (2): Formula (2): 1.05-0.3×D1 (90)≦Ra≦1.36-0.3×D1 (90)
4. 4. The electrostatic image developer according to claim 3, wherein the relationship between the D50(150) and the arithmetic mean roughness Ra satisfies the following formula (3): Formula (3): 1.05-0.3×D50(150)≦Ra≦1.36-0.3×D50(150)
5. 2. The electrostatic image developer according to claim 1, wherein an exposed area ratio of said magnetic particles on the surface of said carrier is 4% or more and 20% or less.
6. 2. The electrostatic image developer according to claim 1, wherein said toner particles further contain resin particles.
7. 7. The electrostatic image developer according to claim 6, wherein said resin particles are crosslinked resin particles.
8. 8. The electrostatic image developer according to claim 7, wherein said crosslinked resin particles are styrene (meth)acrylic resin particles.
9. 2. The electrostatic image developer according to claim 1, wherein the number average molecular weight of the tetrahydrofuran soluble portion in the toner particles is 5,000 or more and 15,000 or less.
10. The electrostatic image developer according to any one of claims 1 to 9 is contained as a replenishment developer, A developer cartridge that is detachably attached to an image forming apparatus.
11. A developer cartridge according to claim 10; a developing device that contains an electrostatic image developer including a replenishment developer replenished from the developer cartridge and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer; The process cartridge is detachably mounted to the image forming apparatus.
12. A developer cartridge according to claim 10; An image carrier; a charging device for charging the surface of the image carrier; an electrostatic image forming device for forming an electrostatic image on the charged surface of the image carrier; a developing device that contains an electrostatic image developer including a replenishment developer replenished from the developer cartridge and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer device for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing device for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:
13. a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using an electrostatic image developer containing a replenishment developer replenished from the developer cartridge according to claim 10; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,
14. a developing device that contains the electrostatic image developer according to any one of claims 1 to 9 and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer; A process cartridge that is detachably attached to an image forming apparatus.
15. An image carrier; a charging device for charging the surface of the image carrier; an electrostatic image forming device for forming an electrostatic image on the charged surface of the image carrier; a developing device that contains the electrostatic image developer according to any one of claims 1 to 9 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer device for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing device for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:
16. a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to any one of claims 1 to 9; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,
Citation Information
Patent Citations
Toner for electrostatic charge image development and production method of the same
JP2011237792A
Image-forming method
JP2011237793A
Toner for developing electrostatic charge image and developer
JP2013160886A
Electrostatic charge image developing toner
JP2019144368A
Electrostatic latent image development toner and method of evaluating fixability of the same
JP2020042121A