Touch sensor

By configuring the touch sensor with a mesh-shaped conductive layer having varying line widths, the issue of uneven density in touch detection electrodes is resolved, enhancing visual appearance and conductivity.

JP2024133901AInactive Publication Date: 2024-10-03FUJIFILM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023043909
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional touch sensors experience uneven density in the mesh-like touch detection electrodes due to non-uniform line widths of the metal plating layer, which affects visual appearance and functionality.

Method used

The touch sensor is designed with a conductive layer composed of thin metal wires arranged in a mesh shape, where the average line width of the plating layer between the first and second ends is narrower than at other positions, maintaining uniformity and reducing density unevenness.

Benefits of technology

The solution ensures uniform line widths across the touch detection electrodes, minimizing visual density unevenness and improving electrical conductivity and adhesion of the metal plating layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133901000001_ABST
    Figure 2024133901000001_ABST
Patent Text Reader

Abstract

To provide a touch sensor that can suppress shading unevenness of a touch detection electrode, and a method for producing the touch sensor.SOLUTION: A touch sensor comprises conductive layers formed on a substrate. The conductive layer has a touch detection electrode (11) that is composed of a plurality of fine metal wires arranged in a mesh shape and extends from a first end part (11A) to a second end part (11B) to cover an electrode length L1. The fine metal wires each have a layer to be plated and a metal plating layer. An average line width Hm of the layers to be plated of the fine metal wires in a region (R1) between the first end part (11A) and a position (P1) apart from the first end part (11A) toward the second end part (11B) side by 1 / 10 of the electrode length L1 is narrower than an average line width Hs of the layers to be plated of the fine metal wires at a position (P2) apart from the first end part (11A) toward the second end part (11B) side by 1 / 2 of the electrode length L1.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a touch sensor that detects a touch operation. [Background technology]

[0002] 2. Description of the Related Art Conventionally, in various electronic devices including tablet computers, smartphones, and other portable information devices, touch sensors are used that detect a so-called touch operation in which a finger, a stylus pen, or the like is brought into contact with or close to a screen.

[0003] Such a touch sensor often has a mesh-like touch detection electrode formed of a plurality of thin metal wires, peripheral wiring drawn from the touch detection electrode, and an electrode pad connected to the peripheral wiring, as disclosed in Patent Document 1. In Patent Document 1, the touch detection electrode, the peripheral wiring, and the electrode pad are formed by a so-called plating method. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5876351 Summary of the Invention [Problem to be solved by the invention]

[0005] As disclosed in Patent Document 1, when the touch detection electrodes, the peripheral wiring, and the electrode pads are formed by plating, for example, a plating layer having a pattern corresponding to the touch detection electrodes, the peripheral wiring, and the electrode pads is formed on a base material, and then the base material is immersed in a plating solution to perform plating processing on the touch detection electrodes, the peripheral wiring, and the electrode pads at once. In this case, depending on the shape of these patterns, the line width of the metal plating layer formed by plating may become non-uniform. Therefore, when an observer visually recognizes the mesh-shaped touch detection electrodes, unevenness in shade may occur.

[0006] The present invention has been made to solve such problems, and has an object to provide a touch sensor capable of suppressing unevenness in shading of the touch detection electrodes, and a method for manufacturing the touch sensor. [Means for solving the problem]

[0007] The above object can be achieved by the following configuration. [1] A substrate; A conductive layer is formed on a substrate, The conductive layer includes a touch detection electrode that is configured by a plurality of thin metal wires arranged in a mesh pattern and extends along a predetermined extension direction from a first end to a second end over a predetermined electrode length L; a connection terminal electrically connected to a first end of the touch detection electrode; A peripheral wiring electrically connected to the connection terminal is provided. the plurality of thin metal wires of the touch detection electrode have a plated layer and a metal plating layer covering the plated layer; A touch sensor in which the average line width Hm of the plated layer of multiple thin metal wires in a region between a first end and a position 1 / 10 of the electrode length L away from the first end toward the second end along the extension direction is narrower than the average line width Hs of the plated layer of multiple thin metal wires at a position 1 / 2 of the electrode length L away from the first end toward the second end along the extension direction. [2] The average line width Hm and the average line width Hs in the plated layer are, Hs×0.80≦Hm <Hs×0.90 The touch sensor according to [1] satisfies the following relationship. [3] A touch sensor as described in [1] or [2], in which the ratio Ms / Hs of the average line width Ms of a plurality of thin metal wires at a position 1 / 2 of the electrode length L away from the first end toward the second end along the extension direction to the average line width Hs of the layer to be plated is 1.25 or more and 1.60 or less. [4] The touch sensor according to [3], wherein the average line width Ms of the plurality of thin metal wires is 1.50 μm or more and 2.00 μm or less. [5] The touch sensor according to [3], wherein the ratio Ms / Hs of the average line width Ms of the multiple thin metal wires to the average line width Hs of the layer to be plated is 1.25 or more and 1.45 or less. Effect of the Invention

[0008] According to this invention, a touch sensor includes a substrate and a conductive layer formed on the substrate, the conductive layer including a touch detection electrode composed of a plurality of fine metal wires arranged in a mesh pattern and extending along a predetermined extension direction from a first end to a second end over a predetermined electrode length L, a connection terminal electrically connected to the first end of the touch detection electrode, and peripheral wiring electrically connected to the connection terminal, the plurality of fine metal wires of the touch detection electrode have a plated layer and a metal plating layer covering the plated layer, and an average line width Hm of the plated layer of the plurality of fine metal wires in a region between the first end and a position 1 / 10 of the electrode length L away from the first end toward the second end along the extension direction is narrower than an average line width Hs of the plated layer of the plurality of fine metal wires at a position 1 / 2 of the electrode length L away from the first end toward the second end along the extension direction, thereby suppressing uneven shading in the touch detection electrode. [Brief description of the drawings]

[0009] [Figure 1] 1 is a partial cross-sectional view of a touch sensor according to an embodiment; [Diagram 2] FIG. 2 is a plan view of a touch sensor according to the embodiment. [Diagram 3] 3 is an enlarged cross-sectional view showing a portion of a first conductive layer in the embodiment. FIG. [Figure 4] 4 is an enlarged plan view illustrating a portion of a plurality of thin metal wires of a touch detection electrode according to the embodiment. FIG. [Diagram 5] 4 is a cross-sectional view of a thin metal wire of a touch detection electrode according to the embodiment. [Figure 6] 4 is an enlarged plan view showing a part of a touch detection electrode according to the embodiment. FIG. [Figure 7] 4 is a graph showing an example of the relationship between the distance from a first end and the average line width of a layer to be plated in the embodiment. [Figure 8] 13 is a plan view of a touch detection electrode according to a modified example of the embodiment. FIG. [Figure 9] 10 is a graph showing an example of the relationship between the distance from a first end and the average line width of a layer to be plated in a modified example of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, a conductive member for a touch panel and a touch panel according to the present invention will be described in detail based on preferred embodiments shown in the accompanying drawings. In the following, the notation "~" indicating a numerical range includes the numerical values ​​written on both sides. For example, "s is a number between t1 and t2" means that the range of s includes the numerical values ​​t1 and t2, which is expressed in mathematical notation as t1≦s≦t2. Unless otherwise specified, angles including "perpendicular" and "parallel" include a generally acceptable error range in the technical field. "Transparent" means that the light transmittance is at least 40% or more in the visible light wavelength range of 400 nm to 800 nm, preferably 75% or more, more preferably 80% or more, and even more preferably 90% or more. The light transmittance is measured according to "Plastics--Determination of total light transmittance and total light reflectance" as specified in JIS K 7375:2008.

[0011] Embodiment FIG. 1 shows a configuration of a touch sensor according to an embodiment of the present invention. The touch sensor includes a substrate 1 having a first surface 1A and a second surface 1B that form a front and a back surface of the substrate, a first conductive layer 2A disposed on the first surface 1A of the substrate 1, and a second conductive layer 2B disposed on the second surface 1B of the substrate 1. The substrate 1 has insulating properties, and the first conductive layer 2A and the second conductive layer 2B are electrically insulated from each other. The substrate 1 has flexibility, and the touch sensor has flexibility equivalent to that of the substrate 1. The substrate 1 is made of a transparent material.

[0012] The touch sensor can be used as a touch panel display device (not shown) by adhering a cover member (not shown) to the surface on the first conductive layer 2A side and a display module (not shown) to the surface on the second conductive layer 2B side. At this time, a user's finger, stylus pen, or the like in contact with or close to the cover member is detected, and a touch operation by the user is detected.

[0013] FIG. 2 shows a plan view of the touch sensor. The first conductive layer 2A has a plurality of touch detection electrodes 11 for detecting a touch operation, which extend from a first end 11A to a second end 11B over a determined electrode length L1 along a determined extension direction, the Y direction, and are arranged along an X direction perpendicular to the Y direction, a plurality of connection terminals 12 electrically connected to the first ends 11A of the plurality of touch detection electrodes 11, a plurality of peripheral wirings 13 electrically connected to the plurality of connection terminals 12, and a plurality of connection pads 14 electrically connected to the plurality of peripheral wirings 13. The plurality of connection pads 14 are used for electrical connection to an external device (not shown).

[0014] The second conductive layer 2B has a plurality of touch detection electrodes 21 for detecting a touch operation, which extend from a first end 21A to a second end 21B over a defined electrode length L1 along the X direction, which is a defined extension direction, and are arranged along the Y direction, a plurality of connection terminals 22 electrically connected to the first ends 21A of the plurality of touch detection electrodes 21, a plurality of peripheral wirings 23 electrically connected to the plurality of connection terminals 22, and a plurality of connection pads 24 electrically connected to the plurality of peripheral wirings 23. The plurality of connection pads 24 are used for electrical connection to an external device (not shown).

[0015] The region in which the multiple touch detection electrodes 11 of the first conductive layer 2A are arranged and the region in which the multiple touch detection electrodes 21 of the second conductive layer 2B are arranged overlap with each other across the substrate 1 in the Z direction perpendicular to both the X direction and the Y direction.

[0016] The first conductive layer 2A is formed by a so-called plating method. As shown in Fig. 3, the first conductive layer 2A has a plateable layer 3 formed on the first surface 1A of the base material 1 and a metal plating layer 4 formed by plating the plateable layer 3 and covering the plateable layer 3.

[0017] 4, the touch detection electrode 11 is composed of a plurality of thin metal wires A arranged in a mesh shape along a first direction D1 and a second direction D2. Although the angle between the first direction D1 and the second direction D2 is not particularly limited, in the following description, it is assumed that the first direction D1 and the second direction D2 are perpendicular to each other for the sake of simplicity.

[0018] The thin metal wires A have a line width M in a direction perpendicular to the first direction D1 or the second direction D2 in which the thin metal wires A extend, that is, in the second direction D2 or the first direction D1.

[0019] As shown in Fig. 5, the fine metal wire A has a plateable layer 3 that is formed on the first surface 1A of the substrate 1 and forms a fine wire extending along a first direction D1 or a second direction D2, and a metal plating layer 4 that covers the plateable layer 3. The fine wire-shaped plateable layer 3 has a line width H in a direction perpendicular to the first direction D1 or the second direction D2 in which the plateable layer 3 extends, i.e., in the second direction D2 or the first direction D1. Here, Fig. 5 shows a cross section of the fine metal wire A extending along the first direction D1, taken along the D2-Z plane.

[0020] When plating the layer 3 to be plated, the substrate 1 on which the layer 3 to be plated is formed is immersed in a plating solution containing the metal ions to be deposited and a reducing agent for reducing the metal ions to metal. In this case, the line width and thickness of the metal plating layer 4 are adjusted by the composition of the plating solution, the plating temperature, the plating time, etc.

[0021] When the plated layer 3 of the touch detection electrode 11 has the same line width H throughout, if a plating process is performed on a plated layer 3 having a large difference in pattern shape, such as the plated layer 3 corresponding to the touch detection electrode 11 and the plated layer 3 corresponding to the peripheral wiring 13, the line width M of the metal plating layer 4 in the touch detection electrode 11 becomes non-uniform, which may result in uneven shading when an observer visually views the touch detection electrode 11.

[0022] Here, in the touch sensor of the present invention, as shown in FIG. 6, the average line width Hm of the plated layer 3 of the multiple fine metal wires A in a region R1 between the first end 11A and a position P1 that is a length L2 that is 1 / 10 of the electrode length L1 away from the first end 11A toward the second end 11B along the Y direction is narrower than the average line width Hs of the plated layer 3 of the multiple fine metal wires A at a position P2 that is a length L3 that is 1 / 2 of the electrode length L1 away from the first end 11A toward the second end 11B along the Y direction.

[0023] The average line width Hm of the plated layer 3 of the multiple fine metal wires A in region R1 can be calculated, for example, by further dividing region R1 into multiple partial regions, for example five partial regions, along the Y direction, measuring the line width H of the plated layer 3 at multiple locations, such as two locations, in each partial region, and taking the arithmetic average of all the measured line widths H. Furthermore, the average line width Hs of the plated layer 3 of the multiple fine metal wires A at position P2 can be calculated, for example, by measuring the line width H of the plated layer 3 at multiple locations, for example at least two locations, in position P2, and taking the arithmetic average of all the measured line widths H.

[0024] The inventors have found that by making the average line width Hm of the plated layer 3 of the multiple fine metal wires A in region R1 narrower than the average line width Hs of the plated layer 3 of the multiple fine metal wires A at position P2, the line width M of the multiple fine metal wires A finally formed by the plating process becomes uniform throughout the entire touch detection electrode 11, thereby suppressing unevenness in shading when an observer visually views the touch detection electrode 11.

[0025] For example, as shown in FIG. 7, by designing the average line width of the plated layer 3 of the plurality of metal thin wires A to increase from the first end 11A toward the second end 11B, the average line width Hm of the plated layer 3 in the region R1 can be made narrower than the average line width Hs of the plated layer 3 at the position P2. Here, FIG. 7 shows an example of the relationship between the distance from the first end 11A to a position away from the second end 11B along the Y direction, which is the extension direction of the touch detection electrode 11, and the average line width of the plated layer 3 at that position. Since the line width M of the metal thin wire A tends to be wider in the vicinity of the connection terminal 12 than in the central part of the touch detection electrode 11, it is preferable to design the line width H of the plated layer 3 so that, for example, the line width H of the plated layer 3 changes sharply from the first end 11A to a position about twice the length L2, and the line width H thereafter changes gradually to the second end 11B.

[0026] Furthermore, when the average line width Hm of the layer to be plated 3 in the region R1 and the average line width Hs of the layer to be plated 3 at the position P1 satisfy the relationship of the following inequality (1), the multiple thin metal wires A can be formed more uniformly over the entire touch detection electrode 11. Hs×0.80≦Hm <Hs×0.90···(1)

[0027] Furthermore, as the amount of metal deposited on the plated layer 3 increases, the electrical resistance of the touch detection electrode 11 decreases and the touch detection sensitivity improves, but on the other hand, the stress applied to the metal plating layer 4 increases, making the metal plating layer 4 more likely to peel off from the substrate 1. From this viewpoint, the ratio Ms / Hs of the average line width Ms of the plurality of thin metal wires A at a position P2 that is separated from the first end 11A toward the second end 11B along the Y direction by a length L3 that is 1 / 2 of the electrode length L1, to the average line width Hs of the plated layer 3 at position P1 is preferably 1.25 or more and 1.60 or less, and more preferably 1.25 or more and 1.45 or less.

[0028] From the same viewpoint, the average line width Ms of the plurality of thin metal wires A is preferably 1.50 μm or more and 2.00 μm or less. The average line width of the multiple thin metal wires A at a position a specific distance away from the first end 11A can be calculated, for example, by taking the arithmetic average of the line widths M of the multiple thin metal wires A at randomly selected locations at that position, for example, 10 locations.

[0029] Although not shown, the touch detection electrode 21 in the second conductive layer 2B, like the touch detection electrode 11 in the first conductive layer 2A, is also composed of a plurality of thin metal wires A arranged in a mesh pattern, and the average line width Hm of the plated layer 3 in a region R1 to a position P1 a length L2 away from the first end 21A is narrower than the average line width Hs of the plated layer 3 at a position P2 a length L3 away from the first end 21A.

[0030] Therefore, in the same manner as the touch detection electrode 11 of the first conductive layer 2A, the line width M of the multiple thin metal wires A finally formed by the plating process in the touch detection electrode 21 of the second conductive layer 2B is uniform throughout the entire touch detection electrode 21, thereby suppressing unevenness in shading when an observer visually views the touch detection electrode 21.

[0031] From the above, according to the touch sensor of the embodiment of the present invention, the average line width Hm of the plated layer 3 of the multiple metal fine wires A in the region R1 between the first end 11A and the position P1 located 1 / 10 of the electrode length L1 away from the first end 11A toward the second end 11B along the Y direction is narrower than the average line width Hs of the plated layer 3 of the multiple metal fine wires A at the position P2 located 1 / 2 of the electrode length L1 away from the first end 11A toward the second end 11B along the Y direction. Therefore, the line width M of the metal fine wires A can be formed uniformly throughout the entire touch detection electrode 11, thereby suppressing uneven shading when an observer visually views the touch detection electrode 11.

[0032] 7, an example in which the average line width of the plated layer 3 of the plurality of thin metal wires A increases continuously and monotonically from the first end 11A to the second end 11B has been described, but for example, the average line width of the plated layer 3 of the plurality of thin metal wires A may increase in a so-called stepwise manner from the first end 11A to the second end 11B. Even in this case, the average line width Hm of the thin-line plated layer 3 in the region R1 can be made narrower than the average line width Hs of the thin-line plated layer 3 in the position P2, thereby suppressing uneven shading when an observer visually recognizes the touch detection electrode 11.

[0033] Although the connection terminal 12 is formed at the first end 11A of the touch detection electrode 11, the connection terminal 12 may be further formed at the second end 11B, for example, as shown in Fig. 8. In this case, the average line width Hm of the plated layer 3 of the multiple thin metal wires A in the region R1 between the first end 11A and the position P1 separated from the first end 11A by the length L2 toward the second end 11B along the Y direction, or in the region R2 between the second end 11B and the position P3 separated from the second end 11B by the length L2 toward the first end 11A along the Y direction, is narrower than the average line width Hs of the plated layer 3 of the multiple thin metal wires A at the position P2 separated from the first end 11A and the second end 11B by the length L3.

[0034] Even in this case, similar to the case where the connection terminal 12 is formed only at the first end 11A, the line width M of the multiple thin metal wires A finally formed by the plating process becomes uniform throughout the entire touch detection electrode 11, thereby suppressing unevenness in shading when an observer visually views the touch detection electrode 11.

[0035] For example, as shown in Figure 9, by designing the average line width of the layer to be plated 3 to monotonically increase in the range from the first end 11A to a position P2 that is a length L3 away from the first end 11A along the Y direction, and to monotonically decrease in the range from position P3 to a position that is the electrode length L1 away from the first end 11A along the Y direction, i.e., to the second end 11B, the average line width Hm of the layer to be plated 3 in region R1 can be made narrower than the average line width Hs of the layer to be plated at position P2. In addition, since the line width M of the thin metal wire A tends to be wider near the connection terminal 12 than in the central part of the touch detection electrode 11, in order to make the line width M of the thin metal wire A uniform throughout the entire touch detection electrode 11, it is preferable to design the line width H of the plated layer 3 so that, for example, the line width H of the plated layer 3 changes sharply from the first end 11A and the second end 11B to a position approximately twice the length L2, and then changes gradually from there to the central part of the touch detection electrode 11.

[0036] A method for manufacturing the touch sensor according to the embodiment will be described below.

[0037] First, a transparent base material 1 is prepared, and a plated layer 3 is formed on a first surface 1A of the base material 1 by using, for example, a photolithography method, as shown in Fig. 3 and Fig. 6. The plated layer 3 has a shape corresponding to the touch detection electrodes 11, the connection terminals 12, the peripheral wiring 13, and the connection pads 14.

[0038] 4, the average line width Hm of the plated layer 3 of the multiple fine metal wires A in a region R1 between the first end 11A and a position P1 that is a length L2 that is 1 / 10 of the electrode length L1 away from the first end 11A toward the second end 11B along the Y direction is designed to be narrower than the average line width Hs of the plated layer 3 of the multiple fine metal wires A at a position P2 that is a length L3 that is 1 / 2 of the electrode length L1 away from the first end 11A toward the second end 11B along the Y direction. Although not shown, a plated layer 3 having the same configuration as the plated layer 3 formed on the first surface 1A of the substrate 1 is formed on the second surface 1B of the substrate 1.

[0039] Next, the base material 1 having the plated layer 3 formed on each of the first surface 1A and the second surface 1B is immersed in a plating solution, and a plating process is performed on the plated layer 3. As a result, as shown in Figures 3 and 6, for example, metal is precipitated on the plated layer 3, forming a metal plating layer 4. In this manner, the touch sensor is manufactured.

[0040] Each component constituting the touch sensor of the embodiment will be described below. <Base material 1> The type of substrate 1 is not particularly limited as long as it is a member capable of supporting first conductive layer 2A and second conductive layer 2B. Examples of the substrate 1 include plastic substrates, glass substrates, and metal substrates, with plastic substrates being preferred. A flexible substrate is preferable for the substrate 1 because of its excellent foldability. Examples of the flexible substrate include the above-mentioned plastic substrates. The thickness of the substrate 1 is not particularly limited, and is often 25 μm to 500 μm.

[0041] Materials constituting the substrate 1 are preferably resins having a melting point of about 290°C or less, such as polyethylene terephthalate (PET) (258°C), polycycloolefin (134°C), polycarbonate (250°C), acrylic film (128°C), polyethylene naphthalate (269°C), polyethylene (135°C), polypropylene (163°C), polystyrene (230°C), polyvinyl chloride (180°C), polyvinylidene chloride (212°C), and triacetyl cellulose (290°C), and more preferably PET, polycycloolefin, or polycarbonate. Among them, PET is particularly preferable because of its excellent adhesion to the first conductive layer 2A and the second conductive layer 2B. The values ​​in parentheses above are melting points or glass transition temperatures. The total light transmittance of the substrate 1 is preferably 85% to 100%. The total light transmittance is measured according to "Plastics - Determination of total light transmittance and total light reflectance" defined in JIS (Japanese Industrial Standards) K 7375:2008.

[0042] One of the preferred embodiments of the substrate 1 is a treated substrate that has been subjected to at least one treatment selected from the group consisting of atmospheric plasma treatment, corona discharge treatment, and ultraviolet irradiation treatment. By performing the above-mentioned treatment, hydrophilic groups such as OH groups are introduced into the surface of the treated substrate 1, improving the adhesion between the substrate 1 and the first conductive layer 2A and between the substrate 1 and the second conductive layer 2B. Among the above-mentioned treatments, atmospheric plasma treatment is preferred in that it further improves the adhesion between the substrate 1 and the first conductive layer 2A and between the substrate 1 and the second conductive layer 2B.

[0043] <Undercoat layer> In order to improve the adhesion between the substrate 1 and the first conductive layer 2A and between the substrate 1 and the second conductive layer 2B, an undercoat layer can be disposed between the substrate 1 and the first conductive layer 2A and between the substrate 1 and the second conductive layer 2B. This undercoat layer contains a polymer, and further improves the adhesion between the substrate 1 and the first conductive layer 2A and between the substrate 1 and the second conductive layer 2B.

[0044] The method for forming the undercoat layer is not particularly limited, but for example, a method of applying a composition for forming the undercoat layer containing a polymer onto a substrate and subjecting it to a heat treatment as necessary can be mentioned. In addition, gelatin, acrylic resin, urethane resin, acrylic-styrene-based latex containing inorganic or polymeric fine particles, etc. may be used as the composition for forming the undercoat layer containing a polymer.

[0045] If necessary, the touch sensor may have a refractive index adjustment layer between the substrate 1 and the first conductive layer 2A and between the substrate 1 and the second conductive layer 2B, in addition to the undercoat layer described above. As the refractive index adjustment layer, for example, an organic layer to which particles of a metal oxide such as zirconium oxide that adjusts the refractive index are added can be used.

[0046] <First conductive layer and second conductive layer> The first conductive layer 2A and the second conductive layer 2B can be formed from a metal or alloy, for example, silver, copper, gold, aluminum, nickel, chromium, molybdenum, or tungsten. The first conductive layer 2A and the second conductive layer 2B preferably contain copper, but may contain a metal other than copper, for example, gold, silver, etc. Also, they may have a laminated structure of a metal and a metal compound, and thin metal wires with a laminated structure such as copper / copper oxide or copper / copper sulfide can be used.

[0047] Next, a method for forming the first conductive layer 2A and the second conductive layer 2B will be described. A plating method can be appropriately used as the method for forming these layers. A method for forming the first conductive layer 2A and the second conductive layer 2B by plating will be described below. Examples of such a method include a method of plating a plated layer 3 obtained by patterning a photosensitive polymer containing plating catalytic metal particles by photolithography, and a method of patterning a photosensitive polymer having functional groups by photolithography, and then treating the layer 3 with a solution containing catalytic metal ions to plate the layer 3 to which catalytic metal is supported on the functional groups. EXAMPLES

[0048] Example 1 The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents and processing procedures shown in the following examples can be appropriately changed without departing from the gist of the present invention, and the scope of the present invention should not be interpreted as being limited by the following examples.

[0049] (Preparation of composition for forming plated layer) The following components were mixed to obtain a composition for forming a plateable layer. Isopropanol 38 parts by weight Polybutadiene maleic acid (butadiene-maleic acid alternating copolymer, butadiene-derived repeating unit: maleic acid-derived repeating unit = 1:1 (molar ratio), manufactured by Polysciences Co., Ltd.) 4 parts by mass FAM-201 (bifunctional acrylamide, manufactured by Fujifilm Corporation) 1 part by mass IRGACURE-OXE02 (oxime ester polymerization initiator, manufactured by BASF) 0.05 parts by mass

[0050] (Preparation of substrate with plating layer precursor layer) A polyester film with adhesive layers on both sides and a thickness of 50 μm (Cosmoshine (registered trademark) A4360, manufactured by Toyobo Co., Ltd.) was prepared as the substrate. The above-mentioned composition for forming a plateable layer was bar-coated on one side of the substrate to a thickness of about 0.3 μm. After coating, the substrate was dried at a temperature of 120° C. for 1 minute to obtain a substrate with a plateable layer precursor layer. Then, a polypropylene protective film with a thickness of 12 μm was immediately attached to the surface of the plateable layer precursor layer.

[0051] (Preparation of substrate with plating layer) An exposure mask having an exposure pattern corresponding to a plurality of touch detection electrodes 11, a plurality of connection terminals 12, a plurality of peripheral wirings 13 and a plurality of connection pads 14 as shown in FIG. 2 was placed on the substrate with the plating layer precursor to which the protective film was attached.

[0052] The exposure pattern corresponding to the touch detection electrode 11 had a square mesh opening pattern (pitch: 300 μm). The line width of the pattern corresponding to the thin metal wires A was 1.15 μm at the first end 11A, gradually widened from the first end 11A toward the second end 11B, and was 1.35 μm at the position P1, which is half the length L3 of the touch detection electrode 11.

[0053] Next, the substrate with the plated layer precursor layer was irradiated with UV light at 30 mJ / cm2 from a high-pressure mercury lamp through an exposure mask. After irradiation with UV light, the protective film was peeled off from the substrate with the plated layer precursor layer. The substrate with the plated layer precursor layer from which the protective film had been peeled off was shower-washed with a 1% by mass aqueous solution of sodium carbonate and subjected to an alkaline development treatment to obtain a substrate with a mesh-shaped plated layer. The formed plated layer had a shape corresponding to the touch detection electrode 11, the connection terminal 12, the peripheral wiring 13, and the connection pad 14.

[0054] The average line width Hm of the plated layer of the multiple thin metal wires A in a region R1 between the portion corresponding to the first end 11A and a position P1 away from the portion corresponding to the first end 11A toward the second end 11B along the Y direction by a length L2 that is 1 / 10 of the electrode length L1 of the entire portion corresponding to the touch detection electrode 11 was 1.20 μm. Also, the average line width Hs of the plated layer of the multiple thin metal wires A at a position P2 away from the portion corresponding to the first end 11A toward the second end 11B along the Y direction by a length L3 that is 1 / 2 of the electrode length L1 was 1.40 μm.

[0055] Here, the average line width Hm was calculated by dividing the region R1 into five divided regions along the Y direction, measuring the line width H of the thin-line plated layer located in each divided region at least at two locations, and taking the arithmetic average of the line width H at a total of 10 locations or more. The average line width Hs was calculated by measuring the line width H of the thin-line plated layer at position P2 at least at two locations, and taking the arithmetic average of the line width H values.

[0056] <Preparation of substrate with copper plating layer (touch sensor)> The Pd catalyst solution Omni-Shield 1573 Activator (Rohm and Haas Electronic Materials Co., Ltd.) was diluted with pure water to 5.4% by volume, and the pH (hydrogen ion exponent) was adjusted to 4 with 0.1 N hydrochloric acid. The substrate with the plated layer was immersed in this solution at a temperature of 50°C for 10 minutes. It was then washed twice with pure water.

[0057] Next, the substrate with the plated layer was immersed in a 0.8% by volume aqueous solution of the reducing agent CIRCUPOSIT PB Oxide Converter 60C (manufactured by Rohm and Haas Electronic Materials Co., Ltd.) at a temperature of 30°C for 5 minutes. After that, it was washed twice with pure water and subjected to Pd catalyst treatment. Next, the substrate with the plated layer subjected to the Pd catalyst treatment was immersed in an electroless plating solution containing 12% by volume of M agent, 6% by volume of A agent, and 10% by volume of B agent of CIRCUPOSIT 4500 (manufactured by Rohm and Haas Electronic Materials Co., Ltd.) at a temperature of 50°C for 40 minutes. After that, it was washed with pure water to form a copper plating layer covering the plated layer as a metal plating layer, and a substrate with a copper plating layer (touch sensor) was obtained. The touch sensor obtained in this way had a first conductive layer 2A including a plurality of touch detection electrodes 11, a plurality of connection terminals 12, a plurality of peripheral wirings 13, and a plurality of connection pads 14, as shown in FIG. 2, for example.

[0058] In the obtained touch sensor, the average line width Mm of the plurality of thin metal wires A in the region R1 was 2.00 μm, and the average line width Ms of the plurality of thin metal wires A in the position P1 was 2.00 μm.

[0059] Here, the average line width Mm was calculated by dividing region R1 into five divided regions along the Y direction, measuring the line width M of the thin metal wire A located in each divided region at least at two locations, and taking the arithmetic average of the line width M at a total of 10 locations or more. Also, the average line width Ms was calculated by measuring the line width M of the thin metal wire A at position P2 at least at two locations, and taking the arithmetic average of the line width M values.

[0060] The average line width Hm of the plated layer of the multiple fine metal wires A was 1.20 μm, and the average line width Hs was 1.40 μm, so the average line width Hm was narrower than the average line width Hs. In addition, the ratio Ms / Hs of the average line width Ms of the multiple fine metal wires A to the average line width Hs of the plated layer of the multiple fine metal wires A was 1.43. In addition, the average line width Hs × 0.80 = 1.12, and the average line width Hs × 0.90 = 1.26, so the average line widths Hs and Hm satisfied inequality (1).

[0061] Example 2 In the process of producing the base material with the plated layer, the touch sensor of Example 2 was produced in the same manner as in Example 1, except that an exposure mask was used to set the average line width Hm of the thin-line plated layer in the region R1 to 1.08 μm. The average line width Mm of the multiple metal fine wires A in the region R1 was 1.80 μm. The average line width Hm of the plated layer of the multiple metal fine wires A was 1.08 μm, and the average line width Hs was 1.40 μm, so the average line width Hm was narrower than the average line width Hs. In addition, the ratio Ms / Hs of the average line width Ms of the multiple metal fine wires A to the average line width Hs of the plated layer of the multiple metal fine wires A was 1.43. In addition, the average line width Hs×0.80=1.12, the average line width Hs×0.90=1.26, and the average line widths Hs and Hm did not satisfy inequality (1).

[0062] Example 3 In the process of producing the base material with the plated layer, the touch sensor of Example 3 was produced in the same manner as in Example 1, except that an exposure mask was used to set the average line width Hm of the thin-line plated layer in the region R1 to 1.32 μm. The average line width Mm of the multiple metal thin wires A in the region R1 was 2.20 μm. The average line width Hm of the plated layer of the multiple metal thin wires A was 1.32 μm, and the average line width Hs was 1.40 μm, so the average line width Hm was narrower than the average line width Hs. In addition, the ratio Ms / Hs of the average line width Ms of the multiple metal thin wires A to the average line width Hs of the plated layer of the multiple metal thin wires A was 1.43. In addition, the average line width Hs×0.80=1.12, the average line width Hs×0.90=1.26, and the average line widths Hs and Hm did not satisfy inequality (1).

[0063] Example 4 The touch sensor of Example 4 was manufactured in the same manner as Example 1, except that in the process of preparing a substrate with a plated layer, an exposure mask was used that set the average line width Hm of the thin-line plated layer in region R1 to 0.48 μm and the average line width Hs of the thin-line plated layer at position P2 to 0.56 μm, and in the process of preparing a substrate (touch sensor) with a copper plating layer, the average line width Ms of the multiple metal thin wires A at position P2 was set to 0.80 μm.

[0064] The average line width Mm of the multiple fine metal wires A in region R1 was 0.80 μm. The average line width Hm of the plated layer of the multiple fine metal wires A was 0.48 μm, and the average line width Hs was 0.56 μm, so the average line width Hm was narrower than the average line width Hs. In addition, the ratio Ms / Hs of the average line width Ms of the multiple fine metal wires A to the average line width Hs of the plated layer of the multiple fine metal wires A was 1.43. In addition, the average line width Hs × 0.80 = 0.45, the average line width Hs × 0.90 = 0.50, and the average line widths Hs and Hm satisfied inequality (1).

[0065] Example 5 The touch sensor of Example 5 was manufactured in the same manner as Example 1, except that in the process of preparing a substrate with a plated layer, an exposure mask was used that set the average line width Hm of the thin-line plated layer in region R1 to 0.83 μm and the average line width Hs of the thin-line plated layer at position P2 to 0.93 μm, and in the process of preparing a substrate (touch sensor) with a copper plating layer, the average line width Ms of the multiple metal thin wires A at position P2 was set to 1.15 μm.

[0066] The average line width Mm of the multiple fine metal wires A in region R1 was 1.15 μm. The average line width Hm of the plated layer of the multiple fine metal wires A was 0.83 μm, and the average line width Hs was 0.93 μm, so the average line width Hm was narrower than the average line width Hs. In addition, the ratio Ms / Hs of the average line width Ms of the multiple fine metal wires A to the average line width Hs of the plated layer of the multiple fine metal wires A was 1.24. In addition, the average line width Hs × 0.80 = 0.74, and the average line width Hs × 0.90 = 0.84, so the average line widths Hs and Hm satisfied inequality (1).

[0067] Example 6 The touch sensor of Example 6 was manufactured in the same manner as Example 1, except that in the process of preparing a substrate with a plated layer, an exposure mask was used that set the average line width Hm of the thin-line plated layer in region R1 to 0.60 μm and the average line width Hs of the thin-line plated layer at position P2 to 0.70 μm, and in the process of preparing a substrate (touch sensor) with a copper plating layer, the average line width Ms of the multiple metal thin wires A at position P2 was set to 1.00 μm.

[0068] The average line width Mm of the multiple fine metal wires A in region R1 was 1.00 μm. The average line width Hm of the plated layer of the multiple fine metal wires A was 0.60 μm, and the average line width Hs was 0.70 μm, so the average line width Hm was narrower than the average line width Hs. In addition, the ratio Ms / Hs of the average line width Ms of the multiple fine metal wires A to the average line width Hs of the plated layer of the multiple fine metal wires A was 1.43. In addition, the average line width Hs × 0.80 = 0.56, and the average line width Hs × 0.90 = 0.63, so the average line widths Hs and Hm satisfied inequality (1).

[0069] Example 7 The touch sensor of Example 7 was manufactured in the same manner as Example 1, except that in the process of preparing a substrate with a plated layer, an exposure mask was used that set the average line width Hm of the thin-line plated layer in region R1 to 0.90 μm and the average line width Hs of the thin-line plated layer at position P2 to 1.05 μm, and in the process of preparing a substrate (touch sensor) with a copper plating layer, the average line width Ms of the multiple metal thin wires A at position P2 was set to 1.50 μm.

[0070] The average line width Mm of the multiple fine metal wires A in region R1 was 1.50 μm. The average line width Hm of the plated layer of the multiple fine metal wires A was 0.90 μm, and the average line width Hs was 1.05 μm, so the average line width Hm was narrower than the average line width Hs. In addition, the ratio Ms / Hs of the average line width Ms of the multiple fine metal wires A to the average line width Hs of the plated layer of the multiple fine metal wires A was 1.43. In addition, the average line width Hs × 0.80 = 0.84, and the average line width Hs × 0.90 = 0.95, so the average line widths Hs and Hm satisfied inequality (1).

[0071] Example 8 The touch sensor of Example 8 was manufactured in the same manner as Example 1, except that in the process of preparing a substrate with a plated layer, an exposure mask was used that set the average line width Hm of the thin-line plated layer in region R1 to 1.54 μm and the average line width Hs of the thin-line plated layer at position P2 to 1.80 μm, and in the process of preparing a substrate (touch sensor) with a copper plating layer, the average line width Ms of the multiple metal thin wires A at position P2 was set to 2.50 μm.

[0072] The average line width Mm of the multiple fine metal wires A in region R1 was 2.50 μm. The average line width Hm of the plated layer of the multiple fine metal wires A was 1.54 μm, and the average line width Hs was 1.80 μm, so the average line width Hm was narrower than the average line width Hs. In addition, the ratio Ms / Hs of the average line width Ms of the multiple fine metal wires A to the average line width Hs of the plated layer of the multiple fine metal wires A was 1.39. In addition, the average line width Hs × 0.80 = 1.44, and the average line width Hs × 0.90 = 1.62, so the average line widths Hs and Hm satisfied inequality (1).

[0073] Example 9 The touch sensor of Example 9 was manufactured in the same manner as Example 1, except that in the process of preparing a substrate with a plated layer, an exposure mask was used that set the average line width Hm of the thin-line plated layer in region R1 to 1.25 μm and the average line width Hs of the thin-line plated layer at position P2 to 1.54 μm, and in the process of preparing a substrate (touch sensor) with a copper plating layer, the average line width Ms of the multiple metal thin wires A at position P2 was set to 2.50 μm.

[0074] The average line width Mm of the multiple fine metal wires A in region R1 was 2.50 μm. The average line width Hm of the plated layer of the multiple fine metal wires A was 1.25 μm, and the average line width Hs was 1.54 μm, so the average line width Hm was narrower than the average line width Hs. In addition, the ratio Ms / Hs of the average line width Ms of the multiple fine metal wires A to the average line width Hs of the plated layer of the multiple fine metal wires A was 1.62. In addition, the average line width Hs × 0.80 = 1.23, and the average line width Hs × 0.90 = 1.39, so the average line widths Hs and Hm satisfied inequality (1).

[0075] Example 10 The touch sensor of Example 10 was manufactured in the same manner as Example 1, except that in the process of preparing a substrate with a plated layer, an exposure mask was used that set the average line width Hm of the thin-line plated layer in region R1 to 1.62 μm and the average line width Hs of the thin-line plated layer at position P2 to 1.89 μm, and in the process of preparing a substrate (touch sensor) with a copper plating layer, the average line width Ms of the multiple metal thin wires A at position P2 was set to 2.70 μm.

[0076] The average line width Mm of the multiple fine metal wires A in region R1 was 2.70 μm. The average line width Hm of the plated layer of the multiple fine metal wires A was 1.62 μm, and the average line width Hs was 1.89 μm, so the average line width Hm was narrower than the average line width Hs. In addition, the ratio Ms / Hs of the average line width Ms of the multiple fine metal wires A to the average line width Hs of the plated layer of the multiple fine metal wires A was 1.43. In addition, the average line width Hs × 0.80 = 1.51, and the average line width Hs × 0.90 = 1.70, so the average line widths Hs and Hm satisfied inequality (1).

[0077] Comparative Example 1 The touch sensor of Comparative Example 1 was manufactured in the same manner as in Example 1, except that in the process of producing a substrate with a plated layer, an exposure mask was used in which the line width H of the thin-line plated layer was uniform throughout the entire portion corresponding to the touch detection electrode 11, and the average line width was 1.40 μm.

[0078] The average line width Mm of the multiple fine metal wires A in region R1 was 2.33 μm. The average line width Hm of the plated layer of the multiple fine metal wires A in region R1 and the average line width Hs at position P1 were equal, each being 1.40 μm. In addition, the ratio Ms / Hs of the average line width Ms of the multiple fine metal wires A to the average line width Hs of the plated layer of the multiple fine metal wires A was 1.43. In addition, the average line width Hs × 0.80 = 1.12, the average line width Hs × 0.90 = 1.26, and the average line widths Hs and Hm do not satisfy inequality (1).

[0079] The touch sensors of Examples 1 to 10 and Comparative Example 1 thus manufactured were subjected to the following evaluations of unevenness in shading, conductivity, and adhesion. (Evaluation of uneven shading) The touch sensor was placed on black paper, and light was shone on the substrate from an angle of 10 to 30 degrees. In this state, five observers visually observed the touch detection electrode for uneven shading at a position 1 m away from the front of the substrate. The uneven shading was evaluated according to the following criteria, and the evaluation given by the most observers was taken as the final evaluation result. A rating is an excellent level, B rating is a level that does not pose any practical problems, and C rating is a level that poses problems in practical use. A: No unevenness in shading can be observed. B: Slight unevenness in shading can be observed. C: Shading unevenness can be observed.

[0080] (Conductivity evaluation) The resistance value of the touch detection electrode 11 of the touch sensor was measured by the so-called four-probe method, and the measured resistance value was divided by the distance between the measurement terminals to measure the line resistance value of the touch detection electrode 11. More specifically, any one of the metal thin wires A constituting the touch detection electrode 11 was separated from the other metal thin wires A, and four microprobes B1, B2, B3, and B4 (tungsten probes manufactured by Micro Support, diameter 0.50 μm) were brought into contact with the separated metal thin wire A. At this time, the microprobes B1 and B4 were arranged on the outermost side, and the microprobes B2 and B3 were arranged between the microprobes B1 and B4 at an interval of 250.00 μm from each other. In this state, a constant current I was applied between the outermost microprobes B1 and B4 using a source meter (a KEITHLEY source meter, a 2400-type general-purpose source meter) so that the voltage between the microprobes B2 and B3 was 5 mV.

[0081] Next, the resistance value R=V / I was measured, and the obtained resistance value R was divided by the distance between the microprobes B2 and B3 to calculate the line resistance value. The same operation was performed using the metal thin wire A at any 10 locations in the touch detection electrode 11, and the arithmetic average of the obtained line resistance values ​​was calculated to calculate the final line resistance value, and the conductivity of the touch detection electrode 11 was evaluated based on this line resistance value according to the following criteria: Grade A indicates that the conductivity of the touch detection electrode 11 is excellent, Grade B indicates that the conductivity of the touch detection electrode 11 is good, Grade C indicates that the conductivity of the touch detection electrode 11 has no practical problem, and Grade D indicates that the conductivity of the touch detection electrode 11 has a practical problem. A: Line resistance is less than 40Ω / mm. B: Wire resistance value is 40 Ω / mm or more and less than 50 Ω / mm. C: Line resistance is 50 Ω / mm or more and less than 60 Ω / mm. D: Wire resistance is 60Ω / mm or more.

[0082] (Adhesion evaluation) After the tape 610 manufactured by 3M was attached to the touch detection electrode 11, the tape was peeled off by the evaluator's hand, and it was observed whether or not the metal plating layer was attached to the tape after peeling. In addition, the line resistance value of the touch detection electrode 11 was measured by the same method as the conductivity evaluation before and after the tape attached to the touch detection electrode 11 was peeled off. Next, the resistance increase rate before and after the test was calculated based on the ratio of the line resistance value before the tape was attached to the touch detection electrode 11 and the line resistance value after the tape attached to the touch detection electrode 11 was peeled off. Based on the observation result of the tape after peeling and the resistance increase rate, the adhesion of the metal plating layer in the touch detection electrode 11 was evaluated according to the following criteria. Grade A indicates that the metal plating layer has excellent adhesion, Grade B indicates that the metal plating layer has good adhesion, Grade C indicates that the adhesion of the metal plating layer has no practical problem, and Grade D indicates that the adhesion of the metal plating layer has practical problems. A: No peeling of the metal plating layer was observed, and the resistance increase rate was 20% or less. B: No peeling of the metal plating layer was observed, and the resistance increase rate was 50% or less. C: No peeling of the metal plating layer was observed, and the resistance increase rate was 100% or less. D: Peeling of the metal plating layer was observed.

[0083] Table 1 shows the evaluation results for Examples 1 to 10 and Comparative Example 1. [Table 1]

[0084] As shown in Table 1, the touch sensors of Examples 1 to 10 were all rated A or B for uneven shading, which indicates that uneven shading does not pose a practical problem. In Examples 1 to 10, the average line width Hm of the plated layer of the multiple fine metal wires A in region R1 is narrower than the average line width Hs of the plated layer of the multiple fine metal wires A in position P1, which is thought to be why the line width M of the fine metal wires A in the touch detection electrode 11 became uniform. Thus, since the line width M of the fine metal wires A is uniform in Examples 1 to 10, it is thought that even when an observer observes the touch detection electrode 11, uneven shading that would pose a practical problem would not be observed.

[0085] On the other hand, the touch sensor of Comparative Example 1 was evaluated as having a shade unevenness of C. Since the line width H of the plated layer is uniform over the entire touch detection electrode 11 of the touch sensor of Comparative Example 1, the line width M of the finally formed multiple thin metal wires A becomes excessively wide near the connection terminal 12 and becomes non-uniform. This is thought to result in shade unevenness that is problematic in practical use when an observer observes the touch detection electrode 11.

[0086] With regard to the evaluation of unevenness in shading, Examples 1 and 4 to 10 were rated A, while Examples 2 and 3 were rated B. Examples 1 and 4 to 10 satisfy inequality (1), while Examples 2 and 3 do not. Therefore, in Examples 2 and 3, it is considered that the line width M of the thin metal wire A is relatively wider near the connection terminal 12 than at position P1, causing slight unevenness in shading.

[0087] Regarding the electrical conductivity evaluation, Examples 1 to 3 and 7 to 10 were rated A, while Examples 4 and 5 were rated C, and Example 6 was rated B. In Examples 4 to 6, the average line widths Ms of the multiple thin metal wires A were 0.80 μm, 1.15 μm, and 1.00 μm, respectively, which were relatively narrow, and it is believed that current flow was relatively difficult.

[0088] In addition, the adhesion evaluation was A in Examples 1 to 7, B in Example 8, and C in Examples 9 and 10. In Examples 8 to 10, the average line width Ms of the multiple metal fine wires A was relatively wide, at 2.50 μm and 2.70 μm, so the stress acting on the metal plating layer of the metal fine wires A was relatively large, and it is considered that the metal plating layer is easily peeled off from the plated layer. In addition, when comparing Example 8 and Example 9, the average line width Ms of the multiple metal fine wires A is the same, but the ratio Ms / Hs of the average line width Ms of the multiple metal fine wires A to the average line width Hs of the plated layer of the multiple metal fine wires A is larger in Example 9. That is, in Example 9, the amount of the metal plating layer covering the thin-line plated layer is larger than that in Example 8, and the metal plating layer is subjected to a larger stress, so it is considered that the metal plating layer is easily peeled off.

[0089] From the results of the conductivity evaluation and adhesion evaluation, in order to ensure the conductivity of the touch detection electrode 11 and the adhesion of the metal plating layer in the touch detection electrode 11, it is considered that the average line width Ms of the multiple thin metal wires A is preferably 1.50 μm or more and 2.00 μm or less, and the ratio Ms / Hs is preferably 1.25 or more and 1.60 or less, and more preferably 1.25 or more and 1.45 or less.

[0090] The present invention is basically configured as described above. Although the touch sensor of the present invention has been described in detail above, the present invention is not limited to the above-mentioned embodiment, and various improvements or modifications may be made without departing from the spirit and scope of the present invention. [Explanation of symbols]

[0091] 1 substrate, 1A first surface, 1B second surface, 2A first conductive layer, 2B second conductive layer, 3 plated layer, 4 metal plating layer, 11, 21 touch detection electrode, 12, 22 connection terminal, 13, 23 peripheral wiring, 14, 24 connection pad, A metal thin wire, D1 first direction, D2 second direction, H, M line width, Hs average line width, L1 electrode length, L2, L3 length, P1, P2, P3 positions, R1, R2 area.

Claims

1. A substrate; A conductive layer is formed on the substrate, The conductive layer includes a touch detection electrode that is configured by a plurality of thin metal wires arranged in a mesh pattern and extends along a predetermined extension direction from a first end to a second end over a predetermined electrode length L1; a connection terminal electrically connected to the first end of the touch detection electrode; a peripheral wiring electrically connected to the connection terminal; the plurality of thin metal wires of the touch detection electrode have a plated layer and a metal plating layer covering the plated layer, A touch sensor in which the average line width Hm of the plated layer of the multiple thin metal wires in the region between the first end and a position away from the first end toward the second end along the extension direction by 1 / 10 of the electrode length L1 is narrower than the average line width Hs of the plated layer of the multiple thin metal wires at a position away from the first end toward the second end along the extension direction by 1 / 2 of the electrode length L1.

2. The average line width Hm and the average line width Hs in the plated layer are, Hs×0.80≦Hm<Hs×0.90 The touch sensor according to claim 1 , which satisfies the relationship:

3. A touch sensor as described in claim 1 or 2, in which the ratio Ms / Hs of the average line width Ms of the multiple thin metal wires at a position 1 / 2 of the electrode length L1 away from the first end toward the second end along the extension direction to the average line width Hs of the plated layer is 1.25 or more and 1.60 or less.

4. The touch sensor according to claim 3 , wherein the average line width Ms of the plurality of thin metal wires is not less than 1.50 μm and not more than 2.00 μm.

5. The touch sensor according to claim 3 , wherein a ratio Ms / Hs of the average line width Ms of the plurality of thin metal wires to the average line width Hs of the plated layer is 1.25 or more and 1.45 or less.

Citation Information

Patent Citations

  • Antiskid hydraulic brake system for car

    JP1983076351A