Active material, electrode, secondary battery, battery pack, and vehicle
A composite metal oxide with an aperiodic crystal structure addresses the limitations of carbon-based electrodes by increasing Li insertion capacity and stability, resulting in higher energy density and longer battery life.
Patent Information
- Application Number
- JP2023044358
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Existing lithium-ion secondary batteries face challenges in achieving high energy density, rapid charging, and long-term reliability, particularly with carbon-based negative electrodes that risk heat generation and ignition due to metallic lithium dendrite formation, and alternative materials like monoclinic niobium titanium oxide have limitations in capacity and energy density.
A composite metal oxide with an aperiodic crystal structure, containing Mo, Nb, and optionally Ti, V, Ta, Fe, Co, Mn, Ni, Bi, Sb, As, P, Cr, W, B, Na, K, Mg, Al, Ca, or Si, is used as an active material, forming spherical particles with controlled particle sizes and compositions to enhance Li insertion capacity and stability, reducing side reactions and improving life performance.
The composite metal oxide achieves higher reversible capacity and longer lifespan by allowing more Li insertion with reduced structural strain and improved conductivity, enhancing battery performance in terms of capacity and life span.
Smart Images

Figure 2024134180000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE Embodiments of the present invention relate to an active material, an electrode, a secondary battery, a battery pack, and a vehicle. [Background technology]
[0002] In recent years, research and development of secondary batteries such as lithium ion secondary batteries and nonaqueous electrolyte secondary batteries as high energy density batteries has been actively promoted. Secondary batteries are expected to be used as power sources for vehicles such as hybrid cars and electric cars, or as uninterruptible power sources for mobile phone base stations. Therefore, in addition to energy density, secondary batteries are also required to have other excellent performances such as rapid charge and discharge performance and long-term reliability.
[0003] A typical negative electrode for lithium-ion batteries is a carbon-based negative electrode that uses carbonaceous materials such as graphite as the active material. When a battery using a carbon-based negative electrode is repeatedly charged and discharged rapidly, dendrites of metallic lithium are deposited on the electrode, which may cause an internal short circuit and lead to heat generation or fire. Therefore, a battery has been developed that uses a metal composite oxide instead of a carbonaceous material for the negative electrode, thereby increasing the negative electrode operating potential. For example, the spinel-type lithium titanium composite oxide Li4Ti5O 12 The battery using this as the negative electrode has an average operating potential of 1.55 V (vs. Li / Li + ) is high, which means that Li dendrite precipitation does not progress, making stable rapid charging and discharging possible, and since it operates at a potential where reduction side reactions in the electrolyte are unlikely to occur, it has a longer life than batteries using carbon-based anodes. However, Li4Ti5O 12 In batteries using this material in the negative electrode, the theoretical capacity of the active material was low at 175 mAh / g, and the energy density was low compared to batteries equipped with a carbon-based negative electrode.
[0004] Therefore, monoclinic niobium titanium oxide TiNb2O7 is being considered. +) while exhibiting high capacity. For this reason, it is expected that the volumetric energy density will exceed that of carbon-based negative electrodes. However, in order to fully popularize electric vehicles, it is desirable to further increase the energy density of lithium-ion secondary batteries from the viewpoint of improving driving range, and it is desirable to develop a high-capacity rapid charging battery. Of course, it is undesirable that other battery performances, such as life performance, will deteriorate as the capacity is increased. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-99287 A [Patent Document 2] Patent Publication No. 2021-61223 [Patent Document 3] International Publication No. 2019 / 234248 [Non-patent literature]
[0006] [Non-Patent Document 1] Nature, 559, 556-563(2018) [Non-Patent Document 2] J. Mater. Chem. A, 2019, 7, 6522-6532 [Non-Patent Document 3] International Tables for Crystallography (2006). 1st online ed. Chester: International Union of Crystallography. [Non-Patent Document 4] "Practice of Powder X-ray Analysis" First Edition (2002) Edited by the X-ray Analysis Research Roundtable of the Japan Society for Analytical Chemistry, edited by Izumi Nakai and Fujio Izumi (Asakura Publishing) [Non-Patent Document 5] Dr. Michael et al., Image Processing with ImageJ, Reprinted from the July 2004 issue of Biophotonics International copyrighted by Laurin Publishing Co. INC. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the embodiments is to provide an active material and an electrode capable of realizing a high-capacity, long-life secondary battery, a high-capacity, long-life secondary battery and a battery pack, and a vehicle equipped with the battery pack. [Means for solving the problem]
[0008] According to an embodiment, an active material is provided that includes a composite metal oxide containing Mo, Nb, and at least one element M selected from the group consisting of Ti, V, Ta, Fe, Co, Mn, Ni, Bi, Sb, As, P, Cr, W, B, Na, K, Mg, Al, Ca, Y, and Si. The composite metal oxide has a non-periodic crystal structure. The active material includes the composite metal oxide as spherical particles. The spherical particles include primary particles of the composite metal oxide having an average particle size of 10 nm or more and 300 nm or less, and are secondary particles having an average particle size of 1 μm or more and 10 μm or less.
[0009] According to another embodiment, there is provided an electrode comprising the active material described above.
[0010] According to yet another embodiment, there is provided a secondary battery comprising a positive electrode, a negative electrode, and an electrolyte. The positive electrode or the negative electrode is the electrode described above.
[0011] According to still another embodiment, there is provided a battery pack including the above-mentioned secondary battery.
[0012] According to an embodiment, a vehicle including the above battery pack is provided. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic diagram showing an example of a crystal structure contained in a composite metal oxide contained in an active material according to an embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a crystal structure that may be contained in a composite metal oxide contained in the active material according to the embodiment. [Diagram 3] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Figure 4] 4 is an enlarged cross-sectional view of a portion A of the secondary battery shown in FIG. 3. [Diagram 5] FIG. 4 is a partially cutaway perspective view illustrating a schematic diagram of another example of a secondary battery according to an embodiment. [Figure 6] 6 is an enlarged cross-sectional view of a portion B of the secondary battery shown in FIG. 5. [Figure 7] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 8] FIG. 1 is an exploded perspective view illustrating an example of a battery pack according to an embodiment. [Figure 9] 9 is a block diagram showing an example of an electric circuit of the battery pack shown in FIG. 8. [Figure 10] 1 is a partially see-through view illustrating an example of a vehicle according to an embodiment. [Figure 11] 1 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to an embodiment. [Figure 12] 5 is a scanning electron microscope image at a magnification of 50,000 times of the composite metal oxide powder obtained in Example 1. [Figure 13] 1 is a scanning electron microscope image at a magnification of 10,000 times of the composite metal oxide powder obtained in Example 1. [Figure 14] 5 is a scanning electron microscope image at a magnification of 50,000 times of the composite metal oxide powder obtained in Comparative Example 1. [Figure 15] 1 is a scanning electron microscope image at a magnification of 10,000 times of the composite metal oxide powder obtained in Comparative Example 1. [Figure 16] 2 is a scanning electron microscope image at a magnification of 20,000 times of the composite metal oxide powder obtained in Comparative Example 2. [Figure 17]1 is a scanning electron microscope image at a magnification of 10,000 times of the composite metal oxide powder obtained in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In order to obtain a high-capacity material, it is desirable to select a material that has a large amount of charge compensation when carrier ions (e.g., lithium ions) are inserted. For this purpose, a composite oxide containing molybdenum (Mo), a hexavalent element, can be used as a compound with even higher capacity.
[0015] There are various factors that are known to limit the lifespan of a battery. One of them is cracking of the electrode active material particles and the resulting interruption of the conductive path. Another is the deterioration of the active material or electrolyte due to a side reaction between the electrolyte (e.g., liquid electrolyte) and the electrode active material.
[0016] Hereinafter, the embodiments will be described with reference to the drawings. In the following description, components that perform the same or similar functions are given the same reference numerals throughout the drawings, and duplicated descriptions will be omitted. Note that each figure is a schematic diagram for explaining the embodiment and facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from the actual device, but these can be appropriately modified in design by taking into consideration the following description and known techniques.
[0017] (First embodiment) According to a first embodiment, an active material is provided that includes a composite metal oxide having a non-periodic crystal structure. The composite metal oxide includes Mo, Nb, and element M. Element M is at least one selected from the group consisting of Ti, V, Ta, Fe, Co, Mn, Ni, Bi, Sb, As, P, Cr, W, B, Na, K, Mg, Al, Ca, Y, and Si. The composite metal oxide is included in the active material as spherical particles. The spherical particles are secondary particles that include primary particles of the composite metal oxide, and the average particle diameter of the primary particles is 10 nm or more and 300 nm or less, and the average particle diameter of the secondary particles is 1 μm or more and 10 μm or less.
[0018] The above composite metal oxide is, for example, represented by the general formula Li a M b NbMo c O d and may be a compound represented thereby. In the general formula, M is at least one of the above elements M and is selected from the group consisting of Ti, V, Ta, Fe, Co, Mn, Ni, Bi, Sb, As, P, Cr, W, B, Na, K, Mg, Al, Ca, Y, and Si. Each subscript in the formula satisfies 0 ≦ a ≦ b + 2 + 3c, 0 < b ≦ 1.5, 0 ≦ c ≦ 0.5, and 2.33 ≦ d / (1 + b + c) ≦ 2.50, respectively.
[0019] Such an active material may be an active material for a battery. The active material may be, for example, an electrode active material used for an electrode of a secondary battery such as a lithium-ion battery or a non-aqueous electrolyte battery. More specifically, the active material may be, for example, a negative electrode active material used for a negative electrode of a secondary battery.
[0020] By using, as an electrode active material, a composite oxide having an amorphous crystal structure composed of an Mo element, an Nb element, and at least one of the above elements M, a secondary battery with high capacity and long life can be realized.
[0021] <Crystal Structure> The composite metal oxide included in the active material according to the first embodiment corresponds to a part of an oxide material having a structure of the Wadsley-Roth phase, which is a crystal phase in an oxide material containing niobium. It has been reported that the Wadsley-Roth phase takes a crystal structure in the range of 2.33 ≦ A O and A Me where A O / A Me ≦ 2.65, with respect to the ratio of oxygen O to metal element Me in the composition. For example, in the case of TiNb2O7, it has a crystal structure on the reducing side where A O / A Me = 2.33.
[0022] Here, reduction means that the ratio of oxygen in the structure is low. In the Wadsley-Roth phase, the vertex-sharing structure of oxygen-metal octahedra forms a rhenium oxide type block structure, and the blocks share the rhenium oxide rhombohedrons, or tetrahedra are inserted between them and share the vertices, forming a crystal structure in which the rhenium oxide type blocks (ReO3 type blocks) are connected in a two-dimensional direction. The reduced side crystal structure has a structure in which the rhenium oxide type blocks are small in size. Although the rhenium oxide type crystal structure has voids that can accommodate a large amount of Li, it is a highly symmetrical crystal structure, and therefore it is difficult to change the bond length between the metal element and the oxygen element to eliminate the charge repulsion when Li is inserted. For this reason, the rhenium oxide type crystal structure can be said to be a structure in which Li insertion is restricted by the charge repulsion that occurs when Li is inserted. Here, the reduced side crystal structure is A O / A Me Since the number of oxygen atoms in the structure decreases as the size of the rhenium oxide block decreases. As a result, when Li is inserted, the crystal structure can expand in volume due to the change in the bond length between the metal element and the oxygen element. Therefore, by including a rhenium oxide crystal structure, it is possible to achieve a large amount of Li insertion, since there is no restriction on the structural change when Li is inserted, while having a large gap.
[0023] The composite metal oxide contained in the active material according to the first embodiment also has a crystal structure on the reduction side like TiNb2O7, which allows more lithium (Li) to be inserted into the crystal structure, resulting in a crystal structure with a large reversible capacity. In other words, the crystal structure of the composite oxide is a crystal structure on the reduction side that belongs to the Wadsley-Roth phase consisting of three elements including niobium, molybdenum, and element M.
[0024] FIG. 1 shows a schematic diagram of an example of a crystal structure that may be included in such a composite metal oxide. The crystal structure 10 includes an octahedron 10a and a tetrahedron 10b each composed of a metal element 18 and an oxygen element 19. The octahedrons 10a are connected to each other by sharing corners to form a rhenium oxide type block (ReO3 block). FIG. 1 shows the crystal structure 10 viewed from the stacking direction of the ReO3 block. The ReO3 block surrounded by a thick line (e.g., block 15a) and the ReO3 block shown only by a thin line (e.g., block 15d) have different planes on which the metal elements 18 are arranged. This example is characterized by having no periodicity of the structure. Blocks of different sizes are connected and exist according to the arrangement method of the Wadsley-Roth phase. The smallest block has two sides and the largest block has six sides. For example, block 15a is made up of 3×3 octahedrons 10a, block 15b is made up of 2×3 octahedrons 10a, block 15c is made up of 2×4 octahedrons 10a, block 15d is made up of 2×2 octahedrons 10a, block 15e is made up of 3×6 octahedrons 10a, block 15f is made up of 5×3 octahedrons 10a, and block 15g is made up of 4×4 octahedrons 10a. These sizes can be freely adjusted according to the metal / oxygen ratio due to the mixed state of Nb, Mo, and element M, and are not limited. The majority are connected by octahedral edge sharing 17, but some may also include tetrahedral vertex sharing by tetrahedrons 10b.
[0025] Another example of the crystal structure that may be included in the composite metal oxide is shown in FIG. 2. In this example, the number of atoms of the metal element Me included as a constituent element is A Me The number of oxygen atoms A O The ratio of A O / A Me = 2.50. This crystal structure has periodicity. Figure 2 shows the unit cell of the crystal structure in the
[0001] direction as viewed along the c-axis. The space group of the crystal structure is I -It belongs to space group 4 and is assigned the space group number 82. The space group referred to here corresponds to the International Tables for Crystallography (Non-Patent Document 3), specifically, the contents of Vol. A: Space-group symmetry of the said material (2nd online edition (2016); ISBN: 978-0-470-97423-0, doi: 10.1107 / 97809553602060000114). However, the space groups are P4 (space group number 75), I4 (space group number 79), P - 4 (space group number 81), P42 / n (space group number 86), I4 / m (space group number 87), P4nc (space group number 104), P - 421c (space group number 114), P - 4n2 (space group number 118) - It can also be explained by the attribution of a simple cubic lattice having a four-fold symmetry axis or a four-fold anti-axis similar to 4 (space group number 82), and it may change if the composition ratio is deviated from the stoichiometric composition ratio by adjusting the composition ratio, or if the structure is distorted due to the presence of a different phase. The crystal structure 11 includes octahedra 11a and tetrahedra 11b each composed of a metal element 18 and an oxygen element 19. The octahedra 11a are connected to each other by sharing vertices to form a rhenium oxide type block (ReO3 type block). The size of the block is 3 x 3 = 9 octahedra 11a. The nine-unit rhenium oxide type block forms planes in the a-axis direction and b-axis direction by sharing the edges of the octahedrons 11a or sharing the vertices of the tetrahedrons 11b. The planes including the nine octahedra 11a are connected to each other by sharing octahedral edges or tetrahedral vertices on the c-axis side, forming a crystal structure.
[0026] Comparing the crystal structure 10 shown in FIG. 1 with the crystal structure 11 shown in FIG. 2, the number of octahedral edge sharing is large in FIG. 1 compared to FIG. 2 because the vertex connections of the tetrahedrons are replaced by edge connections of the octahedrons, and the octahedral lattice distortion is increased. Therefore, in the crystal structure 10 in FIG. 1, the lattice distortion of the octahedrons is large, which facilitates structural relaxation due to the change in bond length during Li insertion, making it possible to increase the amount of Li insertion. Furthermore, since the crystal structure 10 in FIG. 1 contains octahedral edge sharing without having a periodic structure, the asymmetry of the framework is maintained even when the amount of Li insertion is increased. Therefore, the reversible capacity of the crystal structure 10 in FIG. 1 is further improved compared to the crystal structure 11 in FIG. 2. Therefore, by including the crystal structure in FIG. 1, which has a non-periodic crystal structure, in the active material, it is possible to improve the capacity.
[0027] In the above non-periodic crystal structure, the metal / oxygen ratio, which changes with the composition ratio, can be adjusted by changing the size of the ReO3 type block and the number of octahedral edge-sharing or tetrahedral vertex-sharing connections. Therefore, the oxygen / metal ratio can be changed by the composition ratio and can be freely adjusted.
[0028] Molybdenum element (Mo) can be incorporated into the crystal structure not only in a hexavalent state but also in a tetravalent or pentavalent state. The valence of Mo is determined by adjusting the charge balance according to the amount of niobium and element M mixed in the crystal structure shown in FIG. 1 or FIG. 2 and the amount of oxygen. In the case of a hexavalent element, charge compensation during Li insertion with element M such as Ti is a three-electron reaction, so that the theoretical capacity of Li that can be inserted can be increased. An element in a tetravalent or pentavalent state is arranged in the crystal structure in a form in which electrons are supplied to the d band of the Mo element. Therefore, by including a tetravalent or pentavalent Mo element, the conductivity can be changed and the battery performance can be improved. It is known that the Wadsley-Roth phase containing molybdenum has a high operating potential (becomes noble). If oxides containing titanium and niobium are compared, for example, the titanium-niobium-molybdenum composite oxide, which is one aspect of the first embodiment, has a crystal structure containing a high concentration of molybdenum element, and therefore the operating potential can be increased more than TiNb2O7. As a result, the operating potential falls within a potential region in which there is little reduction side reaction of the electrolyte, and a long life performance can be achieved.
[0029] The valence of Mo may be higher than the valence estimated from the crystal structure of FIG. 1 or FIG. 2 and the balance between the amount of oxygen and the metal element. In this case, it is presumed that cation vacancies are formed in the crystal structure and included in the structure to adjust the charge balance. By including cation vacancies in the structure, the electronic conductivity of the active material is improved, thereby improving the battery performance. On the other hand, since cation vacancies have the effect of locally capturing Li in the structure, too many cation vacancies are not preferable from the viewpoint of inhibiting Li movement in the solid.
[0030] In addition, in this active material, it is also possible to form oxygen vacancies by setting the amount of Mo element to be less than the ideal composition. By forming oxygen vacancies, the electronic conductivity of the active material is improved, and thus the battery performance can be improved. On the other hand, too much oxygen vacancy causes charge repulsion of Li. Therefore, too much oxygen vacancy is not preferable because it inhibits the movement of Li.
[0031] The non-periodic crystal structure as shown in FIG. 1 can be confirmed by observation using a scanning transmission electron microscope with a high-angle annular dark-field method, which will be described later.
[0032] The composite oxide further contains at least one of the above-mentioned elements M in addition to Nb and Mo as metal elements. In the non-periodic crystal structure in FIG. 1, the change in the oxygen / metal composition ratio due to charge compensation can be maintained by changing the size of the ReO3 type block and changing the octahedral edge sharing and tetrahedral vertex sharing at the connection part. The Mo element can be included in the structure by adjusting the valence in the structure in the range of 4 to 6. In addition, as described above, the active material can easily create oxygen deficiencies and cation vacancies in the structure. Therefore, the charge balance in the structure can be adjusted with a high degree of freedom, and the element M can be freely selected. As the element M, at least one can be selected from the group consisting of Ti, V, Ta, Fe, Co, Mn, Ni, Bi, Sb, As, P, Cr, W, B, Na, K, Mg, Al, Ca, Y, and Si.
[0033] The element M may be included in the crystal structure as a metal element forming the above-mentioned tetrahedron or octahedron, for example. Alternatively, the element M may be present in the active material in a form not included in the crystal structure of the composite oxide.
[0034] For example, vanadium (V) and phosphorus (P) elements can be included in the crystal structure as pentavalent elements. Titanium (Ti), zirconia (Zr), and silicon (Si) can be included in the structure as tetravalent elements. Iron (Fe), chromium (Cr), aluminum (Al), bismuth (Bi), antimony (Sb), boron (B), arsenic (As), cobalt (Co), manganese (Mn), nickel (Ni), and yttrium (Y) can be incorporated into the crystal structure as trivalent elements. Magnesium (Mg) and calcium (Ca) can be incorporated into the crystal structure as divalent elements. Potassium (K) and sodium (Na) can be incorporated into the crystal structure as monovalent elements. Of these elements, tetravalent elements have a higher charge than elements with a valence of 3 or less, so they can be included in large amounts without decreasing the oxygen / metal ratio in the structure, and are therefore preferred because they can increase the Mo ratio in the structure. In particular, titanium (Ti) is the most preferable of the M elements because it is the element that can be contained in the largest amount in the structure and has an ionic radius close to that of pentavalent Nb, making it easy to incorporate into the structure.
[0035] Tantalum (Ta) is a pentavalent element that can replace Nb. Ta and Nb are in the same group on the periodic table, so they have similar physical and chemical properties. Therefore, it is possible to obtain the same battery performance even if Nb is replaced with Ta.
[0036] Tungsten (W) is a hexavalent element that can replace part of the Mo element. It is generally known that the Wadsley-Roth phase containing W has high rate performance due to the fast Li diffusion rate in the solid. Therefore, the inclusion of W can further improve the rate performance of the active material.
[0037] <Active material particles> The active material according to the first embodiment is in the form of spherical particles. For example, the active material may be composed of secondary particles having a spherical shape of a composite oxide containing Mo, Nb, and the element M and having a non-periodic crystal structure.
[0038] By granulating the secondary particles into a spherical shape, the difference between particles at the contact points between the electrolyte and the active material is reduced. This makes it possible to make the Li insertion and desorption reaction during charging and discharging uniform in an electrode that uses spherical secondary particles as the active material. This makes it possible to suppress side reactions. Furthermore, since the changes due to volume expansion and contraction during Li insertion and desorption are isotropic, destruction of the conductive path is suppressed. As a result, this leads to improved life performance.
[0039] The spherical secondary particles referred to here are those with a coefficient of form unevenness FU of 0.8 or more. The coefficient of form unevenness FU is a parameter devised by noting that the circumferential length l in a projected cross section becomes larger compared to the cross-sectional area a as the degree of unevenness around the particle increases. The dimensionless quantity f that expresses the relationship between the circumferential length l and the cross-sectional area a is expressed as f = a / l 2 The value of f is maximum when the cross-sectional shape is a circle, and the value f when the radius of the circle is r is c f c = πr 2 / (2πr) 2 The value f assuming a circle c The ratio of f to the above value is defined as the roughness coefficient FU and is expressed by the following formula 1.
[0040]
number
[0041] In the above formula 1, as described above, l is the perimeter of the particle in the projected cross section, a is the cross-sectional area of the particle in the projected cross section, and π is the circular constant. When the target particle is a perfect sphere (projected cross section is a circle), the roughness coefficient FU is 1.00. The method of calculating the roughness coefficient FU from the projected cross section of a secondary particle will be described in detail later.
[0042] The average primary particle diameter of the spherical particles is 10 nm or more and 300 nm or less. From the viewpoint of the appropriate range of Li diffusivity and diffusion distance of the material in the embodiment, by adjusting the primary particle diameter within the above range, it is possible to operate the battery with low resistance and stability. Furthermore, it is possible to suppress cracking of the primary particles due to the volume expansion and contraction of the composite metal oxide during insertion and desorption of Li.
[0043] The average secondary particle diameter of the spherical particles is 1 μm or more and 10 μm or less. On the one hand, if the secondary particle diameter is moderately large, the particle contact points can be kept small, making it easier to build good conductive paths between particles. On the other hand, since the secondary particle diameter is not unnecessarily large, it is easier to ensure conductive paths inside the particles. By adjusting the diameter within the above range, it is possible to keep the conductive paths of the particles in the electrode stable, and it is possible to improve the life performance. This average secondary particle diameter means the particle diameter at which the volume cumulative value is 50% in the particle size distribution determined by a laser diffraction type particle size distribution measuring device.
[0044] The BET specific surface area of the active material is 5m 2 / g or more 40m 2 / g or less is desirable, and 10m 2 / g or more is more preferable. By reducing the specific surface area, the amount of side reactions of the active material is reduced, and the life performance is improved. In the embodiment, the specific surface area is within the above range when the secondary particles (spherical particles) are assumed to be ideal spheres from the viewpoint of the appropriate primary particle size and the true density of the material. In other words, if it is within the above range, it can be said that the specific surface area is sufficiently reduced.
[0045] The BET specific surface area refers to the specific surface area determined by the nitrogen BET (Brunauer, Emmet and Teller) method. The method for determining the specific surface area based on the nitrogen BET method will be described in detail later.
[0046] <Manufacturing method> The active material according to the first embodiment can be produced as follows.
[0047] (liquid phase synthesis) The method for producing the composite metal oxide is not particularly limited, but it can be synthesized by, for example, a solid-phase reaction method, a sol-gel method, a hydrothermal synthesis method, etc. As an example, a method for producing a titanium-niobium-molybdenum composite oxide (i.e., element M=Ti) using the sol-gel method will be described.
[0048] As the starting material, a titanium compound, a niobium compound, and a molybdenum compound are used. Examples of titanium compounds include titanium tetraisopropoxide, titanyl sulfate, titanium chloride, titanium ammonium oxalate and its hydrate, titanium hydroxide, and titanium oxide. Examples of niobium compounds include niobium chloride, ammonium niobium oxalate and its hydrate, niobium hydroxide, and niobium oxide. Examples of molybdenum compounds include molybdenum chloride, ammonium molybdate and its hydrate, molybdenum hydroxide, and molybdenum oxide. When an element other than Ti is selected as the element M or another element is selected together with Ti, the titanium compound is appropriately replaced with or used in combination with the selected element M.
[0049] It is preferable to dissolve the starting materials in pure water or acid in advance to prepare a solution. By dissolving the materials, it is possible to obtain a dry gel in which each element is homogeneously mixed, thereby increasing reactivity. If the materials cannot be dissolved in pure water, they are dissolved using acid.
[0050] Examples of acids used to dissolve the raw materials include citric acid and oxalic acid, but it is preferable to use oxalic acid from the viewpoint of solubility. For example, when using oxalic acid, it is preferable to use a concentration of 0.5 M or more and 1 M or less. When dissolving, it is preferable to use a temperature of 70° C. or more in order to shorten the reaction time.
[0051] If it is difficult to dissolve the raw materials, the reaction can be carried out as a dispersion. In this case, the average particle size of the raw materials contained in the dispersion is preferably 3 μm or less, more preferably 1 μm. After preparing a solution (or dispersion) in which the composition ratio of each compound is adjusted to a predetermined ratio, the solution is heated and stirred while being neutralized with an aqueous ammonia solution to adjust the pH. A gel solution is obtained by adjusting the pH. By setting the pH to 5 or more and 8 or less, it is possible to form a gel that contains each raw material homogeneously, and this makes it possible to obtain a dry gel that has good reactivity when fired.
[0052] Next, the gel liquid is heated to near the boiling point to evaporate the water and proceed with gelation. After gelation, the water is further evaporated and drying is performed to obtain a dry gel. During gelation and drying, for example, the entire amount of the solution can be evaporated and concentrated to obtain a dry gel. The dry gel produced by evaporating and concentrating the entire amount of the solution is preferably pulverized before firing to reduce the average particle size to 10 μm or less, more preferably 5 μm or less. This allows the particle size after firing to be reduced. The obtained dry gel is fired.
[0053] In the step of evaporating the solvent to gel and obtain a dried gel, it is more preferable to use a spray dryer. By spraying, it is possible to form fine droplets of the sol solution. By drying in the form of fine droplets, it is possible to prevent particle aggregation that progresses during solvent drying, and therefore it is possible to make the particle size smaller after drying and reduce the number of coarse particles. This makes it possible to increase the homogeneity of the reaction during the firing of the precursor and also to suppress the aggregation of particles during firing. The drying temperature during spray drying is preferably 100°C or higher and 200°C or lower.
[0054] The dried gel is pre-baked at 200°C to 500°C for 1 hour to 10 hours. This makes it possible to burn off excess organic components, thereby increasing the reactivity during the main baking.
[0055] The firing is preferably performed at a temperature of 600° C. to 800° C. for a time period of 1 hour to 10 hours. By performing firing within such a temperature range, it is possible to obtain the desired phase while suppressing the sublimation of molybdenum.
[0056] In the powder after sintering, secondary particles are formed in which the particles aggregate into irregular shapes. When an electrode is constructed using an active material containing irregular particles, the irregular particles are unable to maintain a good conductive path between the particles. Furthermore, in areas where the irregular particles have few particle contacts, the conductive path is destroyed by collapse during charging and discharging. Because the use of irregular particles leads to a decrease in charging and discharging performance, particle molding is carried out.
[0057] For particle molding, the amorphous aggregates are first crushed, which can be achieved by wet dispersion. It is preferable to prepare a slurry containing the powder after firing, and crush the aggregated particles to the vicinity of the primary particles using a wet bead mill. For the slurry containing the powder after firing, it is preferable to select water as the solvent and to include a dispersant in a mass ratio of 5 or less to the mass of the active material.
[0058] Examples of dispersants that can be used include surfactants, polyacrylic acid, polyethylene glycol, polyethyleneimine, polyvinylpyrrolidone, styrene-maleic acid polymers, ethylene-maleic acid polymers, hydroxyethyl cellulose, carboxymethyl cellulose, ethyl cellulose, and polyvinyl alcohol. The diameter of the media in the bead mill is selected to be 1 mm or less, preferably 0.2 mm or less, from the viewpoint of dispersing the particles to the vicinity of the above-mentioned primary particle diameter. The media material is preferably zirconia from the viewpoint of preventing contamination. The use of small-diameter beads increases the frequency of contact between the particles and the beads. This allows the fine particle dispersion to proceed well, and dispersion in the liquid to the vicinity of the above-mentioned primary particle diameter is possible.
[0059] Next, the slurry prepared by the wet bead mill is spray-dried to obtain a powder molded into a spherical shape. The particles crushed to the vicinity of the primary particles by the wet bead mill have a small particle size, so the van der Waals force acts strongly on them. Therefore, when the crushed particles are re-aggregated by spray drying, they can maintain their shape. Spherical secondary particles can be formed based on the principle of spray drying, which quickly dries spherical droplets.
[0060] In the powder after spray drying, the surface becomes amorphous due to the collision of the media and the particles during the wet bead mill, and the crystallinity of the newly formed particle active surface when dispersed is reduced by hydration with the solvent water. For this reason, firing is performed again to restore the crystallinity. The firing temperature is preferably 500°C or higher and 650°C or lower. Since the non-periodic crystal structure (for example, FIG. 1) of the composite metal oxide contained in the active material according to the embodiment is a low-temperature phase, it is possible to improve the crystallinity even at a low re-firing temperature. Furthermore, since the low temperature does not cause thermal diffusion to proceed, re-agglomeration does not occur. For this reason, it is possible to recrystallize while maintaining the shape of the spherical particles obtained by spray drying.
[0061] <Various measurement methods> The measurement methods for the active material are described below, specifically, confirmation of the composite metal oxide, measurement of the average particle size of the active material particles, measurement of the roughness coefficient FU of the secondary particles, and measurement of the specific surface area of the active material.
[0062] When the active material contained in the electrode of a battery is used as a sample, the measurement sample is prepared by pre-treating it as follows. First, the battery is fully discharged. Next, the battery is disassembled in a glove box under an argon atmosphere, and the electrodes are removed. Next, the removed electrodes are washed with a solvent such as ethyl methyl carbonate. Further processing is performed for each measurement to prepare a sample in an appropriate form.
[0063] (Confirmation of complex metal oxides) It can be confirmed that the active material has the above-mentioned crystal structure by combining wide-angle X-ray diffraction (XRD) and high-angle annular dark-field (HAADF) methods. It can be confirmed that the active material contains a composite metal oxide containing Mo, Nb, and at least one of the above-mentioned elements M by combining inductively coupled plasma (ICP) emission spectrometry and inert gas dissolution-infrared absorption spectroscopy. The valence of the element can be measured, for example, by X-ray photoelectron spectroscopy (XPS) using characteristic X-rays.
[0064] The XRD measurement is carried out as follows. First, the active material is pulverized as necessary to obtain a powdered sample. The average particle size of the powdered sample is preferably 20 μm or less. This average particle size can be determined by a laser diffraction particle size distribution analyzer.
[0065] Next, the powdered sample is filled into the holder of a glass sample plate, and the surface is made flat. For example, the glass sample plate may have a holder depth of 0.2 mm.
[0066] Next, the glass sample plate is placed in a powder X-ray diffractometer, and the XRD spectrum is measured using Cu-Kα radiation. Specific measurement conditions are, for example, as follows: X-ray diffraction equipment: Rigaku SmartLab X-ray source: CuKα ray Output: 40kV, 200mA Package measurement name: General purpose measurement (concentration method) Incident parallel slit aperture angle: 5° Length of entrance longitudinal limiting slit: 10mm Light receiving PSA: None Receiving parallel slit aperture angle: 5° Monochromatization method: Kβ filter method Measurement mode: Continuous Entrance slit width: 0.5° Receiving slit width: 20mm Measurement range (2θ): 5~70° Sampling width (2θ): 0.01° Scan speed: 1° ~ 20° / min.
[0067] In this manner, an XRD spectrum of the active material is obtained. In this XRD spectrum, the horizontal axis indicates the angle of incidence (2θ) and the vertical axis indicates the diffraction intensity (cps). The scan speed can be adjusted within a range such that the count number of the main peak of the XRD spectrum is 50,000 or more and 150,000 or less.
[0068] When the active material contained in a battery electrode is used as a sample, the electrode after cleaning obtained by carrying out the above-mentioned pretreatment is cut into a piece having an area approximately equal to the area of the glass sample plate holder to prepare a measurement sample.
[0069] Next, the obtained measurement sample is directly attached to a glass holder and subjected to XRD measurement. Next, materials other than the active material that may be contained in the electrode, such as a current collector, a conductive agent, and a binder, are measured using XRD to grasp the XRD pattern derived from them. Next, if there is a peak that is thought to be derived from the active material in the measurement sample and a peak of the other material overlap, the peak of the material other than the active material is separated. In this way, an XRD spectrum related to the active material is obtained.
[0070] In order to more strictly confirm whether the measured sample contains a crystal structure that belongs to the tetragonal crystal structure shown in Figure 2, the Rietveld method is used. For example, RIETAN-FP is used as an analysis program, and the reliability factor R wpIt can be confirmed by confirming that the value is at least 20% or less, more preferably 15% or less. At this time, if there is a peak containing impurities and it overlaps with the phase to be analyzed, the analysis accuracy may be deteriorated. In this case, it is preferable to perform an analysis in which the portion that clearly overlaps with the peak derived from the impurity is excluded from the analysis range. However, this is not the case when the sample contains a material other than the active material according to the first embodiment, when the orientation of the sample is extremely high, or when coarse particles are mixed in, since the intensity ratio changes, and the structure is confirmed by confirming that there is no contradiction in the positions and relative intensities of all peaks attributed to the crystal structure. In addition, when the intensity of the spectrum is low and the background intensity is low, R wp The value may be small, and the reliability factor does not have any significance in its absolute value, but rather in judging the relative quality of the fitting under certain measurement conditions.
[0071] The analytical method using RIETAN-FP is explained in detail, for example, in Chapter 9 "Let's try using RIETAN-FP" of Non-Patent Document 4 ("Practical Application of Powder X-Ray Analysis" First Edition (2002), edited by the X-Ray Analysis Research Forum of the Japan Society for Analytical Chemistry, edited by Nakai Izumi and Izumi Fujio (Asakura Publishing)).
[0072] RIETAN-FP is a Rietveld analysis program that was distributed for free on its developer's internet webpage (closed as of January 2023). As of March 2023, the program is available from the following web archive: http: / / web.archive.org / web / 20220209014122fw_ / http: / / fujioizumi.verse.jp / download / download.html
[0073] The structure in Figure 1 does not have periodicity, so it is difficult to analyze it by XRD measurement. In order to confirm the structure in Figure 1, it is preferable to directly observe the microstructure. The observation can be performed by the High Angle Annular Dark-Field (HAADF) method using a Scanning Transmission Electron Microscope (STEM). From the viewpoint of improving the measurement resolution, it is preferable to use spherical aberration correction. The structure can be confirmed by acquiring an atomic image (10 nm × 10 nm) from a direction perpendicular to the ReO3 type block and confirming the positional relationship of the metal elements that make up the ReO3 block.
[0074] The content of each element in the active material particles contained in the sample can be confirmed by ICP atomic emission spectrometry for metal elements. The amount of O element can be quantified by inert gas dissolution-infrared absorption spectroscopy, but precise quantification is difficult.
[0075] The active material particles contained in the electrode are further subjected to the following treatment after the above-mentioned pretreatment. From the washed electrode, a member containing active material (e.g., the active material-containing layer described in the second embodiment) is peeled off, for example, from the current collector of the electrode. The part peeled off from the electrode is heated in air for a short time (about 1 hour at 500°C) to burn off unnecessary parts such as binder components and carbon. Thereafter, the content of each element can be quantified by performing ICP emission analysis or the like.
[0076] The measurement of the valence of the metal elements contained in the composite oxide by the XPS method can be carried out as follows. It is preferable to use hard X-rays for the measurement, since they have a deep detection depth and can measure a state closer to the bulk. Spectroscopic techniques using hard X-rays are also called HAXPES. The valence can be determined by checking the position of the binding energy of the narrow spectrum of each element. For example, for the Ti element, Ti2p 3 / 2The peak of the fourth valence due to Mo is observed at 459.0±0.4 eV. 5 / 2 The 6-valent peak due to Nb3d is observed at 232.2±0.4 eV. 5 / 2 A peak due to the 5-valence element is observed at 207.5±0.4 eV. If a low-valence element is included, it can be identified by detecting a peak at a lower energy position than the previous valence. In particular, Mo element may contain a valence of 5 or less.
[0077] Sample measurements are performed non-destructively so that element valence does not change. Therefore, for measurements of complex oxides contained in electrodes, the electrode is used as a sample without extracting materials. Measurements are performed with care so that charge-up during sample measurement does not affect the peak position. It is preferable to measure the electrode in a fully discharged state to prevent peak shifts due to charge-up. If the electrode contains a conductive agent, charge-up can be reduced. Note that long-term X-ray irradiation can also damage the sample, causing changes in element valence. In addition, when materials with different structures are mixed, the peak may shift due to changes in the bonding state, so be careful not to confuse this with changes in valence. When elements with different valences are mixed, that is, when the spectrum is mixed with multiple peaks, the spectrum can be separated by least squares fitting, and the mixing ratio can be estimated from the area ratio of the separated peaks.
[0078] As a result of combining the above measurements, it was found that the compound has a non-periodic crystal structure and is represented by the general formula Li a M b NbMo c O d (The element M and each subscript are as described above; hereinafter omitted) is contained in the active material. a M b NbMo c O dThe Li content represented by the subscript a in the above formula changes depending on the charging state of the electrode in which the composite metal oxide is used as the active material. For example, in the composite oxide contained in the negative electrode, Li is inserted as the battery is charged, and the subscript a increases, and Li is removed as the battery is discharged, and the subscript a decreases. The subscript d reflects the amount of cation vacancies and oxygen vacancies.
[0079] (Measurement of average particle size) The average primary particle size of the active material can be determined by observation using a scanning electron microscope (SEM). Specifically, the average primary particle size determined by SEM observation can be calculated by the following method.
[0080] First, the length of the longest axis and the length of the shortest axis are measured for the primary particles included in the SEM image of the secondary particles obtained by SEM observation, and the arithmetic mean value of these is taken as the primary particle diameter. This measurement of the primary particle diameter is performed for 100 randomly selected particles, and the average value of these is taken as the average primary particle diameter.
[0081] The average secondary particle diameter of the active material can be determined from the particle size distribution measured using a laser diffraction particle size distribution measuring device. A dispersion diluted with N-methyl-2-pyrrolidone so that the concentration of the active material is 0.1% by mass to 1% by mass is used as a sample for measuring the particle size distribution. The particle diameter at which the volumetric integrated value is 50% in the obtained particle size distribution is defined as the average secondary particle diameter.
[0082] (Measurement of the roughness coefficient) The average value of the roughness coefficient FU for the secondary particles of the composite metal oxide contained in the active material is FU ave This section describes how to measure the above.
[0083] Specifically, first, the average particle diameter (D 50 ) is calculated. The particle size distribution chart is measured using a laser diffraction particle size distribution measuring device. 50100 secondary particles are extracted from a number of secondary particles having particle diameters (diameters) between 0.2 and 4 times the value of FU. Next, for each of these particles, the above formula 1 (FU = 4πa / l 2 ) is used to calculate the value of the unevenness coefficient FU. In formula 1, l is the perimeter of each secondary particle in the projected cross section, a is the cross-sectional area of each secondary particle in the projected cross section, and π is the constant of the circumference of a circle, which is considered to be 3.14. As described above, the unevenness coefficient FU is 1.00 in the case of a perfect sphere, but for the secondary particles of the complex oxide contained in the active material according to the first embodiment, the average value FU ave is in the range of 0.80 to 1.00. In other words, secondary particles with a roughness coefficient FU of 0.8 or more are judged to be "spherical particles."
[0084] 100 secondary particles are extracted as follows. Measurements are performed by attaching the active material powder or an electrode piece containing it to an SEM stage with carbon tape and observing with an SEM. When observing the electrode piece, it is machined in the direction perpendicular to the electrode by Ar ion milling, and the machined surface (cross section) is observed. SEM observations are performed randomly, and a total of 100 secondary particles in which the boundary line of the outer periphery (outline) of the secondary particle is clearly visible are observed. The observation magnification is set to the magnification of the particle in which the boundary line of the outer periphery (outline) of the secondary particle is clearly visible, for example, 5000 to 20000 times.
[0085] Next, the average value of the unevenness coefficient FU ave The calculation is as follows. First, the center of gravity is calculated from the projected area of each secondary particle. Here, the previously determined D 50 Let X be the circle with radius of D. 50 A circle having a radius of 0.1 times the value of X is defined as circle Y. An explanation will be given using Example 1 described later as an example. Fig. 13 shows an SEM image of the active material powder produced in Example 1 at a magnification of 10,000 times. As shown in Fig. 13, when the centers of circles X and Y are superimposed on the center of gravity of the secondary particle to be measured, a secondary particle is determined at each observation point such that the outer periphery L of the secondary particle is larger than circle Y and smaller than circle X.
[0086] For the images of these 100 secondary particles, an image analysis tool is used to determine the circumferential length l of the periphery L of the target particle and the cross-sectional area a of the target particle. As an image analysis tool, for example, ImageJ shown in Non-Patent Document 5 (Dr. Michael et al., Image Processing with ImageJ, Biophotonics International, July 2004 issue) can be used. From the obtained circumferential length l and cross-sectional area a, the roughness coefficient FU is calculated for each of the selected 100 secondary particles according to the above formula 1. Furthermore, the average value FU of the calculated roughness coefficients FU of the 100 particles is calculated. ave Calculate.
[0087] In the case of electrode pieces, if the load applied during rolling to produce the electrode is strong, the shape of the secondary particles may change. This may cause the particles to deviate from the ideal sphere, and the average value of the unevenness coefficient FU may be lower than that of the powder. However, even in such cases, for electrodes with an average unevenness coefficient FU of 0.8 or more, this means that the conductive path can be secured uniformly, and the above-mentioned effects can be obtained.
[0088] (BET specific surface area measurement) The BET specific surface area of the active material particles can be determined by the following method.
[0089] First, 4 g of active material is collected as a sample. Then, the evaluation cell of the measuring device is dried under reduced pressure at a temperature of 100°C or higher for 15 hours to perform a degassing treatment. For example, a 1 / 2 inch cell can be used as the evaluation cell. Then, the sample is placed in the measuring device. For example, Shimadzu Micromeritics Tristar II 3020 can be used as the measuring device. Next, in nitrogen gas at 77K (boiling point of nitrogen), the nitrogen gas pressure P (mmHg) is gradually increased, and the nitrogen gas adsorption amount (mL / g) of the sample is measured for each pressure P. Next, the pressure P (mmHg) is divided by the saturated vapor pressure P0 (mmHg) of nitrogen gas to obtain a relative pressure P / P0, and the nitrogen gas adsorption amount for each relative pressure P / P0 is plotted to obtain an adsorption isotherm. Next, a BET plot is calculated from this nitrogen adsorption isotherm and the BET formula, and the specific surface area is obtained using this BET plot. The BET plot is calculated using the BET multipoint method.
[0090] The active material according to the first embodiment includes spherical particles of a composite metal oxide containing Mo, Nb, and at least one element M. The composite metal oxide has a non-periodic crystal structure. The spherical particles are secondary particles, and have an average primary particle diameter of 10 nm to 300 nm and an average secondary particle diameter of 1 μm to 10 μm. An electrode using the composite oxide as an electrode active material has high capacity per volume and high life performance. In addition, a secondary battery and a battery pack using the composite oxide as an electrode active material have high capacity per volume and high life performance. That is, the active material exhibits high capacity and long life.
[0091] Second Embodiment According to a second embodiment, an electrode is provided.
[0092] The electrode according to the second embodiment includes the active material according to the first embodiment. This electrode can be a battery electrode that includes the active material according to the first embodiment as a battery active material. The electrode as a battery electrode can be, for example, a negative electrode that includes the active material according to the first embodiment as a negative electrode active material. Alternatively, the electrode can be a positive electrode that includes the active material according to the first embodiment as a positive electrode active material.
[0093] Such an electrode may include a current collector and an active material-containing layer. The active material-containing layer may be formed on one or both sides of the current collector. The active material-containing layer may include an active material and, optionally, a conductive agent and a binder.
[0094] The active material-containing layer may contain the active material according to the first embodiment alone, or may contain two or more types of active materials according to the first embodiment. Furthermore, it may contain a mixture of one or more types of active materials according to the first embodiment and one or more types of other active materials. It is desirable that the content ratio of the active material according to the first embodiment to the total mass of the active material according to the first embodiment and the other active materials is 10 mass % or more and 100 mass % or less.
[0095] For example, when the active material according to the first embodiment is contained as a negative electrode active material, examples of other active materials include lithium titanate having a ramsdellite structure (e.g., Li 2+x Ti3O7, 0≦x≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12 , 0≦x≦3), titanium dioxide (TiO2), anatase type titanium dioxide, rutile type titanium dioxide, niobium pentoxide (Nb2O5), hollandite type titanium composite oxide, orthorhombic titanium composite oxide, and monoclinic type niobium titanium oxide, niobium oxide, niobium titanium oxide, niobium molybdenum composite oxide, and niobium tungsten composite oxide.
[0096] As an example of the above-mentioned orthorhombic titanium-containing composite oxide, Li 2+e M I 2-f Ti 6-g MII h O 14+σ In this case, the compound represented by M I is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb and K. II is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦e≦6, 0≦f<2, 0≦g<6, 0≦h<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+e Na2Ti6O 14 (0≦e≦6).
[0097] As an example of the monoclinic niobium titanium oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium oxide include Li x Examples include Nb2TiO7 (0≦x≦5).
[0098] Another example of monoclinic niobium titanium oxide is Li x Ti 1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from the group consisting of Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.
[0099] The conductive agent is blended to improve the current collecting performance and to suppress the contact resistance between the active material and the current collector. Examples of the conductive agent include carbonaceous materials such as vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanotubes and carbon nanofibers. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. Alternatively, instead of using the conductive agent, a carbon coat or an electronically conductive inorganic material coat may be applied to the surface of the active material particles. In addition, the current collecting performance of the active material-containing layer can be improved by using the conductive agent and coating the active material surface with carbon or a conductive material.
[0100] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0101] The mixing ratio of the active material, conductive agent and binder in the active material-containing layer can be appropriately changed depending on the application of the electrode. For example, when the electrode is used as a negative electrode of a secondary battery, it is preferable to mix the active material (negative electrode active material), conductive agent and binder at a ratio of 68% by mass or more and 96% by mass or less, 2% by mass or more and 30% by mass or less, and 2% by mass or more and 30% by mass or less, respectively. By making the amount of the conductive agent 2% by mass or more, the current collection performance of the active material-containing layer can be improved. In addition, by making the amount of the binder 2% by mass or more, the binding property between the active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the conductive agent and the binder 30% by mass or less, respectively, in order to increase the capacity.
[0102] When the surface of the active material is coated with carbon or a conductive material, the amount of the coating material can be considered to be included in the amount of conductive material. The amount of carbon or conductive material coated is preferably 0.5% by mass or more and 5% by mass or less. If the amount of coating is within this range, the current collection performance and electrode density can be improved.
[0103] The current collector is made of a material that is electrochemically stable at the potential at which lithium (Li) is inserted and removed from the active material. For example, when the active material is used as a negative electrode active material, the current collector is preferably made of copper, nickel, stainless steel, or aluminum, or an aluminum alloy containing one or more elements selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.
[0104] The current collector may also include a portion on the surface of which no active material-containing layer is formed, and this portion can function as a current collecting tab.
[0105] The electrode can be produced, for example, by the following method. First, an active material, a conductive agent, and a binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. After that, the laminate is pressed. In this manner, an electrode is produced.
[0106] Alternatively, the electrode may be prepared by the following method: first, the active material, the conductive agent, and the binder are mixed to obtain a mixture, then the mixture is formed into pellets, and then the pellets are placed on a current collector to obtain an electrode.
[0107] The electrode according to the second embodiment contains the active material according to the first embodiment, and therefore the electrode according to the second embodiment can realize a secondary battery having high capacity per volume and high life performance.
[0108] (Third embodiment) According to the third embodiment, a secondary battery including a negative electrode, a positive electrode, and an electrolyte is provided. This secondary battery includes the electrode according to the second embodiment as the negative electrode or the positive electrode. That is, the secondary battery according to the third embodiment includes an electrode including the active material according to the first embodiment as a battery active material as a battery electrode. A secondary battery according to a desirable aspect includes an electrode according to the second embodiment as a negative electrode. That is, a secondary battery according to a desirable aspect includes an electrode including the active material according to the first embodiment as a battery active material as a negative electrode. Desired aspects will be described below.
[0109] The secondary battery may further include a separator disposed between the positive electrode and the negative electrode. The negative electrode, the positive electrode, and the separator may constitute an electrode group. The electrolyte may be held in the electrode group.
[0110] Moreover, such a secondary battery can further include an exterior member that houses the electrode group and the electrolyte.
[0111] Furthermore, such a secondary battery may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.
[0112] The secondary battery according to the third embodiment may be, for example, a lithium secondary battery. The secondary battery includes a non-aqueous electrolyte secondary battery that contains a non-aqueous electrolyte.
[0113] The negative electrode, the positive electrode, the electrolyte, the separator, the exterior member, the negative electrode terminal, and the positive electrode terminal will be described in detail below.
[0114] 1) Negative electrode The negative electrode may include a negative electrode current collector and a negative electrode active material-containing layer. The negative electrode current collector and the negative electrode active material-containing layer may be the current collector and the active material-containing layer that can be included in the electrode according to the second embodiment, respectively. The negative electrode active material-containing layer includes the active material according to the first embodiment as a negative electrode active material.
[0115] Among the details of the negative electrode, the parts overlapping with the details described in the second embodiment are omitted.
[0116] The density of the negative electrode active material-containing layer (excluding the current collector) is 1.8 g / cm 3 or more and 2.8 g / cm 3 or less, which is preferable. A negative electrode with the density of the negative electrode active material-containing layer within this range is excellent in energy density and electrolyte retention. The density of the negative electrode active material-containing layer is 2.1 g / cm 3 or more and 2.6 g / cm 3 or less, which is more preferable.
[0117] The negative electrode can be manufactured, for example, by the same method as the electrode according to the second embodiment.
[0118] 2) Positive electrode The positive electrode can include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode active material-containing layer can be formed on one or both sides of the positive electrode current collector. The positive electrode active material-containing layer can include a positive electrode active material, and optionally a conductive agent and a binder.
[0119] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode may contain, as the positive electrode active material, one type of compound alone, or may contain a combination of two or more types of compounds. Examples of the oxide and the sulfide include compounds into which Li or Li ions can be inserted and desorbed.
[0120] Examples of such compounds include manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (e.g., Li x Mn2O4 or Li x MnO2; 0 < x ≦ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≦ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Coy O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), lithium phosphate having an olivine structure (e.g., Li x FePO4; 0 < x ≤ 1, Li x Fe 1-y Mn y PO4; 0 < x ≤ 1, 0 < y ≤ 1, Li x CoPO4; 0 < x ≤ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) is included.
[0121] Among the above, examples of more preferable compounds as the positive electrode active material include lithium manganese composite oxide having a spinel structure (e.g., Li x Mn2O4; 0 < x ≤ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≤ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≤ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium iron phosphate (e.g., Li xFePO4; 0 < x ≤ 1), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included. When these compounds are used as the positive electrode active material, the positive electrode potential can be increased.
[0122] When a room-temperature molten salt is used as the electrolyte of the battery, it is preferable to use a positive electrode active material containing lithium iron phosphate, Li x VPO4F (0 ≤ x ≤ 1), lithium manganese composite oxide, lithium nickel composite oxide, lithium nickel cobalt composite oxide, or a mixture thereof. Since these compounds have low reactivity with the room-temperature molten salt, the cycle life can be improved. Details of the room-temperature molten salt will be described later.
[0123] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. A positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. A positive electrode active material with a primary particle size of 1 μm or less can allow the solid-state diffusion of lithium ions to proceed smoothly.
[0124] The specific surface area of the positive electrode active material is preferably 0.1 m 2 / g or more and 10 m 2 / g or less. A positive electrode active material having a specific surface area of 0.1 m 2 / g or more can sufficiently secure the insertion / desorption sites of Li ions. A positive electrode active material having a specific surface area of 10 m 2 / g or less is easy to handle in industrial production and can ensure good charge / discharge cycle performance.
[0125] The binder is blended to fill the gaps between the dispersed positive electrode active material and to bind the positive electrode active material and the positive electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0126] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.
[0127] In the positive electrode active material-containing layer, the positive electrode active material and the binder are preferably mixed in an amount of 80% by mass to 98% by mass and 2% by mass to 20% by mass, respectively.
[0128] By making the amount of binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.
[0129] When a conductive agent is added, the positive electrode active material, the binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 95% by mass or less, 2% by mass or more and 20% by mass or less, and 3% by mass or more and 15% by mass or less, respectively.
[0130] By making the amount of the conductive agent 3% by mass or more, the above-mentioned effects can be achieved. Also, by making the amount of the conductive agent 15% by mass or less, the ratio of the conductive agent in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.
[0131] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from the group consisting of Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si.
[0132] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99 mass% or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1 mass% or less.
[0133] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.
[0134] The positive electrode can be produced, for example, by using a positive electrode active material in the same manner as in the electrode according to the second embodiment.
[0135] 3) Electrolyte The electrolyte may be, for example, a liquid nonaqueous electrolyte or a gel nonaqueous electrolyte. The liquid nonaqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.
[0136] Examples of the electrolyte salt include lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium salts such as lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2), lithium bis(fluorosulfonyl)imide (LiN(SO2F)2; LiFSI), and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potentials, and LiPF6 is most preferred.
[0137] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.
[0138] The gelled non-aqueous electrolyte is prepared by combining a liquid non-aqueous electrolyte with a polymeric material, such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), or a mixture thereof.
[0139] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.
[0140] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.
[0141] The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it.
[0142] The inorganic solid electrolyte is a solid substance that has Li-ion conductivity. Here, Li-ion conductivity is defined as a Li-ion conductivity of 1×10 -6 It means that the inorganic solid electrolyte has a lithium ion conductivity of 1.0 S / cm or more. Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes. Specific examples of the inorganic solid electrolyte are as follows.
[0143] The oxide-based solid electrolyte has a NASICON (Sodium (Na) Super Ionic Conductor) type structure and is represented by the general formula Li 1+xIt is preferable to use a lithium phosphate solid electrolyte represented by Mα2(PO4)3. In the above general formula, Mα is, for example, one or more selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is within the range of 0 ≦ x ≦ 2.
[0144] Specific examples of the lithium phosphate solid electrolyte having a NASICON-type structure include LATP compounds represented by Li 1+x Al x Ti 2-x (PO4)3 with 0.1 ≦ x ≦ 0.5; Li 1+x Al y Mβ 2-y (PO4)3 where Mβ is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca and 0 ≦ x ≦ 1 and 0 ≦ y ≦ 1; Li 1+x Al x Ge 2-x (PO4)3 with 0 ≦ x ≦ 2; and, Li 1+x Al x Zr 2-x (PO4)3 with 0 ≦ x ≦ 2; Li 1+x+y Al x Mγ 2-x Si y P 3-y O 12 represented by where Mγ is one or more selected from the group consisting of Ti and Ge and 0 < x ≦ 2, 0 ≦ y < 3; Li 1+2x Zr 1-x Ca x (PO4)3 with 0 ≦ x < 1 can be mentioned.
[0145] In addition, as the oxide-based solid electrolyte, in addition to the above lithium phosphate solid electrolyte, there is also an amorphous LIPON compound represented by Li x PO y N z where 2.6 ≦ x ≦ 3.5, 1.9 ≦ y ≦ 3.8, and 0.1 ≦ z ≦ 1.3 (for example, Li 2.9 PO 3.3 N 0.46); Garnet-type structure La 5+ xA x La 3-x MδO 12 A is 1 or more selected from the group consisting of Ca, Sr, and Ba, Mδ is 1 or more selected from the group consisting of Nb and Ta, and 0≦x≦0.5; Li3Mδ 2-x L2O 12 wherein Mδ is at least one selected from the group consisting of Nb and Ta, and L may contain Zr, and 0≦x≦0.5; Li 7-3x Al x La3Zr3O 12 and 0≦x≦0.5; Li 5+x La3Mδ 2-x Zr x O 12 where Mδ is at least one selected from the group consisting of Nb and Ta, and 0≦x≦2. LLZ compounds (e.g., Li7La3Zr2O 12 ); and La 2 / 3-x Li x Examples of such compounds include those represented by TiO3, where x is 0.3≦x≦0.7.
[0146] One or more of the above compounds can be used as the solid electrolyte. Two or more of the above solid electrolytes can also be used.
[0147] Alternatively, instead of the non-aqueous electrolyte, a liquid aqueous electrolyte or a gel aqueous electrolyte can be used as the electrolyte. The liquid aqueous electrolyte is prepared by dissolving, for example, the above-mentioned electrolyte salt as a solute in an aqueous solvent. The gel aqueous electrolyte is prepared by compounding the liquid aqueous electrolyte with the above-mentioned polymer material. As the aqueous solvent, a solution containing water can be used. The solution containing water may be pure water or a mixed solvent of water and an organic solvent.
[0148] 4) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.
[0149] 5) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.
[0150] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.
[0151] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.
[0152] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.
[0153] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains a transition metal such as iron, copper, nickel, and chromium, the content of the transition metal is preferably 1 mass % or less.
[0154] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin, or button. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.
[0155] 6) Negative terminal The negative electrode terminal can be formed from a material that is electrochemically stable at the Li insertion / extraction potential of the above-mentioned negative electrode active material and has electrical conductivity. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.
[0156] 7) Positive terminal The positive electrode terminal has a potential range of 3V to 4.5V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.
[0157] Above, the embodiment including the electrode according to the second embodiment as the negative electrode has been described. In the embodiment of the secondary battery according to the third embodiment including the electrode according to the second embodiment as the positive electrode, the negative electrode which is the counter electrode thereof can be, for example, the following counter electrode. At least one electrode selected from lithium metal, lithium metal alloy, graphite, silicon, silicon oxide, tin oxide, silicon, tin, and other alloys can be used as the negative electrode. A material that does not contain Li in the active material can be used as the negative electrode by pre-doping with Li element.
[0158] In an embodiment including the electrode according to the second embodiment as a positive electrode, details of the positive electrode overlap with those described in the second embodiment, and therefore will be omitted.
[0159] Next, the secondary battery according to the third embodiment will be described more specifically with reference to the drawings.
[0160] Fig. 3 is a cross-sectional view showing an example of a secondary battery, and Fig. 4 is an enlarged cross-sectional view of part A of the secondary battery shown in Fig. 3.
[0161] The secondary battery 100 shown in Figures 3 and 4 includes an electrode group 1 shown in Figure 3, a bag-shaped exterior member 2 shown in Figures 3 and 4, and an electrolyte (not shown). The electrode group 1 and the electrolyte are stored in the bag-shaped exterior member 2. The electrolyte (not shown) is held in the electrode group 1.
[0162] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0163] As shown in Fig. 3, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 4, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.
[0164] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 4. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.
[0165] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.
[0166] As shown in FIG. 3, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.
[0167] The secondary battery according to the embodiment is not limited to the secondary battery having the configuration shown in FIGS. 3 and 4, but may be a battery having the configuration shown in FIGS.
[0168] Fig. 5 is a partially cutaway perspective view showing a schematic diagram of another example of a secondary battery, and Fig. 6 is an enlarged cross-sectional view of part B of the secondary battery shown in Fig. 5.
[0169] The secondary battery 100 shown in Figures 5 and 6 includes an electrode group 1 shown in Figures 5 and 6, an exterior member 2 shown in Figure 5, and an electrolyte (not shown). The electrode group 1 and the electrolyte are housed in the exterior member 2. The electrolyte is held in the electrode group 1.
[0170] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0171] The electrode group 1 is a laminated type electrode group, as shown in Fig. 6. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.
[0172] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.
[0173] The negative electrode current collector 3a of each negative electrode 3 includes a portion on one side where the negative electrode active material-containing layer 3b is not supported on any surface. This portion serves as a negative electrode current collector tab 3c. As shown in FIG. 6, the negative electrode current collector tab 3c does not overlap with the positive electrode 5. The negative electrode current collector tabs 3c are electrically connected to a belt-shaped negative electrode terminal 6. The tip of the belt-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.
[0174] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab 3c. The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab 3c. The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side of the negative electrode terminal 6 and is drawn out to the outside of the exterior member 2.
[0175] The secondary battery according to the third embodiment includes the electrode according to the second embodiment. That is, the secondary battery according to the third embodiment includes the electrode including the active material according to the first embodiment. Therefore, the secondary battery according to the third embodiment has high capacity per volume and high life performance.
[0176] (Fourth embodiment) According to a fourth embodiment, there is provided a battery pack including a plurality of secondary batteries according to the third embodiment.
[0177] In such a battery pack, the individual cells may be electrically connected in series or parallel, or may be arranged in a combination of series and parallel connections.
[0178] Next, an example of a battery pack according to a fourth embodiment will be described with reference to the drawings.
[0179] Fig. 7 is a perspective view showing an example of a battery pack. The battery pack 200 shown in Fig. 7 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the third embodiment.
[0180] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 7 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, so that the plurality of cells are electrically connected to each other.
[0181] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 22 for external connection. Also, the negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 23 for external connection.
[0182] The battery pack according to the fourth embodiment includes the secondary battery according to the third embodiment, and therefore has high capacity per volume and long life performance.
[0183] Fifth embodiment According to a fifth embodiment, there is provided a battery pack. The battery pack includes the battery assembly according to the fourth embodiment. The battery pack may include a single secondary battery according to the third embodiment, instead of the battery assembly according to the fourth embodiment.
[0184] Such a battery pack may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.
[0185] The battery pack may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.
[0186] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0187] Fig. 8 is an exploded perspective view showing an example of a battery pack, and Fig. 9 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 8.
[0188] The battery pack 300 shown in Figs. 8 and 9 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).
[0189] 8 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be capable of housing a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to house the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.
[0190] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.
[0191] At least one of the plurality of unit cells 100 is a secondary battery according to the third embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 9. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.
[0192] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.
[0193] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.
[0194] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.
[0195] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.
[0196] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.
[0197] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.
[0198] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.
[0199] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.
[0200] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.
[0201] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.
[0202] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.
[0203] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.
[0204] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal 352 and a negative terminal 353, respectively, of the external terminal 350 for current supply.
[0205] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.
[0206] The battery pack according to the fifth embodiment includes the secondary battery according to the third embodiment or the battery pack according to the fourth embodiment, and therefore has high capacity per volume and long life performance.
[0207] Sixth embodiment According to a sixth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the fifth embodiment.
[0208] In such a vehicle, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy.
[0209] Examples of vehicles include, for example, two to four wheel hybrid electric vehicles, two to four wheel electric vehicles, power assisted bicycles, and rail vehicles.
[0210] The mounting position of the battery pack in the vehicle is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.
[0211] The vehicle may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections.
[0212] Next, an example of a vehicle according to an embodiment will be described with reference to the drawings.
[0213] FIG. 10 is a partially see-through view that diagrammatically illustrates an example of a vehicle.
[0214] A vehicle 400 shown in Fig. 10 includes a vehicle body 40 and a battery pack 300 according to the fifth embodiment. In the example shown in Fig. 10, the vehicle 400 is a four-wheeled automobile.
[0215] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.
[0216] 10 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.
[0217] Next, an embodiment of a vehicle according to the present embodiment will be described with reference to FIG.
[0218] Fig. 11 is a diagram illustrating an example of a control system for an electrical system in a vehicle. The vehicle 400 illustrated in Fig. 11 is an electric vehicle.
[0219] The vehicle 400 shown in FIG. 11 comprises a vehicle body 40, a vehicle power supply 41, a vehicle ECU (ECU: Electric Control Unit) 42 which is a higher-level control device of the vehicle power supply 41, an external terminal (terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45.
[0220] The vehicle 400 has a vehicle power supply 41 mounted, for example, in an engine compartment, the rear of the vehicle body, or under a seat. Note that, in the vehicle 400 shown in FIG. 11, the mounting location of the vehicle power supply 41 is shown diagrammatically.
[0221] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.
[0222] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (for example, VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a to 300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a to 200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a to 200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.
[0223] Each of the assembled batteries 200a to 200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the third embodiment. Each of the assembled batteries 200a to 200c is charged and discharged via a positive terminal 413 and a negative terminal 414.
[0224] The battery management device 411 communicates with the assembled battery monitoring devices 301a to 301c, and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a to 200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.
[0225] The battery management unit 411 and the assembled battery monitoring units 301a to 301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a to 301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.
[0226] The battery pack monitoring devices 301a to 301c measure the voltage and temperature of each of the cells constituting the battery packs 200a to 200c based on commands communicated from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.
[0227] The vehicle power supply 41 may also have an electromagnetic contactor (for example, a switch device 415 shown in FIG. 11) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a to 200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a to 200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed near the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.
[0228] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.
[0229] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.
[0230] Although not shown, the vehicle 400 is also equipped with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when the vehicle 400 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.
[0231] One terminal of a connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to a negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417 on the connection line L1.
[0232] One terminal of a connection line L2 is connected to the positive electrode terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to a positive electrode input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive electrode terminal 413 and the positive electrode input terminal 418.
[0233] The external terminal 43 is connected to the battery management unit 411. The external terminal 43 can be connected to, for example, an external power source.
[0234] In response to operational inputs from the driver or the like, the vehicle ECU 42 coordinates with other management devices and control devices including the battery management device 411 to control the vehicle power supply 41, the switch device 415, the inverter 44, etc. Through the coordinated control of the vehicle ECU 42, etc., the output of power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data relating to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transferred between the battery management device 411 and the vehicle ECU 42 via a communication line.
[0235] The vehicle according to the sixth embodiment is equipped with the battery pack according to the fifth embodiment. Since the capacity per volume of the battery pack is high, the degree of freedom in vehicle design is high. Therefore, it is possible to provide a variety of vehicles without compromising the performance of the vehicle. In addition, since the battery pack has a long life performance, a highly reliable vehicle can be provided. EXAMPLES
[0236] The above-mentioned embodiment will be described in more detail below based on examples, but the present invention is not limited to the examples listed below.
[0237] <Synthesis> Example 1 A titanium-niobium-molybdenum composite oxide was synthesized as follows.
[0238] As raw materials, ammonium niobium oxalate, ammonium molybdate, and titanium tetraisopropoxide were prepared. These raw materials were weighed according to a predetermined composition ratio. Ammonium niobium oxalate and ammonium molybdate were dissolved in pure water to prepare solution A. Next, titanium tetraisopropoxide was added to an aqueous oxalic acid solution with a concentration of 1M, and dissolved by heating and stirring to prepare solution B. After mixing solutions A and B, ammonia solution was added while heating and stirring to adjust the pH to 7, thereby obtaining a sol. The sol was spray-dried at a drying temperature of 160°C to evaporate the solvent, and a white precursor powder was obtained. The precursor powder was placed in an alumina crucible and fired (first firing) in the air at 600°C for 4 hours to form amorphous particles consisting of a titanium-niobium-molybdenum composite oxide phase. Then, after crushing the coarse particles with a dry ball mill, a slurry was prepared with a solvent of water and a solid content ratio of 6 by mass. A dispersant made of polyvinyl alcohol was added to the slurry at an active material mass ratio of 0.5. The slurry prepared as described above was subjected to a wet bead mill to disperse the slurry. For the wet bead mill, the media material was zirconia and the media diameter was 0.2 mm. After the wet bead mill, the slurry was spray-dried at a drying temperature of 140°C to evaporate the solvent, and a powder made of spherical particles was collected. Then, the powder was put into an alumina crucible and re-fired (second firing) in the air at 600°C for 4 hours. The active material powder was obtained as described above.
[0239] (Examples 2 to 4) Active material particles were synthesized in the same manner as in Example 1, except that the compounding ratio of the raw materials was changed.
[0240] Example 5 Active material particles were synthesized in the same manner as in Example 1, except that when the precursor was fired, the firing temperature was changed to 700°C in the first firing and to 650°C in the second firing.
[0241] Example 6 Active material particles were synthesized in the same manner as in Example 1, except that when the precursor was fired, the firing temperature was changed to 800°C in the first firing and to 650°C in the second firing.
[0242] (Examples 7 and 8) In the spray drying process after the wet bead mill, the secondary particle size was controlled by changing the solid content ratio and the total liquid amount, but otherwise the active material particles were synthesized in the same manner as in Example 1.
[0243] Comparative Example 1 A titanium-niobium-molybdenum composite oxide was synthesized as follows.
[0244] As raw materials, ammonium niobium oxalate, ammonium molybdate, and titanium tetraisopropoxide were prepared. These raw materials were weighed according to a predetermined composition ratio. Ammonium niobium oxalate and ammonium molybdate were dissolved in pure water to prepare solution A. Next, titanium tetraisopropoxide was added to an aqueous oxalic acid solution with a concentration of 1M, and dissolved by heating and stirring to prepare solution B. After mixing solution A and solution B, ammonia solution was added while heating and stirring to adjust the pH to 7, thereby obtaining a sol. The sol was spray-dried at a drying temperature of 160°C to evaporate the solvent, and a white precursor powder was obtained. The precursor powder was put into an alumina crucible and fired in the air at 600°C for 4 hours. As described above, an active material powder was obtained.
[0245] Comparative Example 2 A titanium-niobium composite oxide was synthesized as follows.
[0246] As raw materials, ammonium niobium oxalate and titanium tetraisopropoxide were prepared. These raw materials were weighed according to a predetermined composition ratio. Ammonium niobium oxalate was dissolved in pure water to prepare solution A. Next, titanium tetraisopropoxide was added to an aqueous oxalic acid solution with a concentration of 1M, and dissolved by heating and stirring to prepare solution B. After mixing solutions A and B, ammonia solution was added while heating and stirring to adjust the pH to 7, thereby obtaining a sol. The sol was spray-dried at a drying temperature of 160°C to evaporate the solvent, and a white precursor powder was obtained. The precursor powder was put into an alumina crucible and fired in the air at 1000°C for 4 hours to form amorphous particles consisting of a titanium-niobium composite oxide phase. After that, the coarse particles were pulverized using a dry ball mill, and a slurry with a solid content ratio of 6 by mass and water as the solvent was prepared. A dispersant made of polyvinyl alcohol was added to the slurry at an active material mass ratio of 0.5. The slurry prepared as above was subjected to a wet bead mill to disperse the slurry. For the wet bead mill, the media material was zirconia and the media diameter was 0.2 mm. After the wet bead mill, the slurry was spray-dried at a drying temperature of 140° C. to evaporate the solvent and collect a powder consisting of spherical particles. Then, the slurry was placed in an alumina crucible and re-fired in the air at 700° C. for 4 hours. As described above, an active material powder was obtained.
[0247] <Measurement> The powders obtained in each of the above examples and comparative examples were observed using a scanning transmission electron microscope. Specifically, as described above in detail, the microstructure was observed using a 10 nm x 10 nm image using a STEM-HAADF image with a spherical aberration correction function. In addition, wide-angle X-ray scattering measurement was performed. The measurement was performed according to the details described above. Crystal structure analysis was performed using the Rietveld method on the obtained spectrum. In addition, ICP emission analysis, BET specific surface area measurement using N2 gas adsorption method, particle size distribution measurement, and scanning electron microscope observation were performed.
[0248] For the composite metal oxides obtained in Example 1 and Comparative Example 1, the microstructure was observed by STEM-HAADF images, and it was confirmed that the size of the ReO3 blocks in the field of view was different, and that the crystal structure was connected by octahedral edge sharing without periodicity. Therefore, it was identified as the crystal structure shown in Figure 1. As a result of measurement by ICP optical emission spectrometry, the composition of the metal elements was determined to be Ti:Nb:Mo = 0.33:1.00:0.33.
[0249] It was confirmed that the composite oxides obtained in Examples 2 to 4, 7, and 8 have a non-periodic crystal structure in which octahedral edges are connected by sharing, as in Example 1. For this reason, the crystal structure was identified as that shown in Figure 1. It was confirmed that the composite oxides obtained in Examples 5 and 6 have a mixture of a non-periodic crystal structure as shown in Figure 1 and a tetragonal crystal structure as shown in Figure 2.
[0250] The composite oxide obtained in Comparative Example 2 was confirmed to have a crystal structure of monoclinic titanium niobium oxide TiNb2O7 from the XRD pattern and the results of its Rietveld analysis. Specifically, the crystal structure is assigned to the space group notation C2 / m (space group number: 12), does not include a tetrahedral corner-sharing structure, has 3×3=9 rhenium oxide type block structures, and has a ratio of the number of oxygen atoms to the number of metal elements in a unit cell of A O / A M =2.33. When this crystal structure was estimated, it was possible to analyze it as a single phase. As a result of measurement by ICP emission spectrometry, the composition of the metal elements was determined to be Ti:Nb=0.50:1.00.
[0251] The composite metal oxide powder obtained in Example 1 had an average particle diameter of 2.43 μm calculated by particle size distribution measurement. FIG. 12 shows an example of the observation result of a SEM image of primary particles at a magnification of 50,000 times. The average value of the primary particle diameter was 0.05 μm. Based on the above-mentioned method described with reference to FIG. 13 for the first embodiment, secondary particles were observed by observing an SEM image at a magnification of 10,000 times. As shown in FIG. 13, it can be confirmed that the secondary particles are formed in a spherical shape. Using the image software ImageJ, the particle shape was determined as shown in FIG. 13, the cross-sectional area and the perimeter were calculated, and the unevenness coefficient was calculated according to the details described above, resulting in 0.92. The same operation was performed on 100 particles to obtain the average unevenness coefficient FU of FU. ave The result was 0.86.
[0252] The composite metal oxide powder obtained in Comparative Example 1 had an average particle diameter of 2.67 μm calculated by particle size distribution measurement. FIG. 14 shows an example of the observation result of a SEM image of primary particles at a magnification of 50,000 times. The average value of the primary particle diameter was 0.05 μm. Secondary particles were observed by observing an SEM image at a magnification of 10,000 times based on the same method as that described with reference to FIG. 13 for the first embodiment. An example is shown in FIG. 15. It can be confirmed that the secondary particles are formed by agglomeration of primary particles in an indefinite shape. Using the image software ImageJ, the particle shape was determined as shown in FIG. 15, the cross-sectional area and the perimeter were calculated, and the unevenness coefficient was calculated according to the details described above, resulting in 0.63. The same operation was performed on 100 particles to obtain the average unevenness coefficient FU, FU. ave The result was 0.65.
[0253] The composite metal oxide powder obtained in Comparative Example 2 had an average particle diameter of 1.00 μm calculated by particle size distribution measurement. FIG. 16 shows an example of the observation result of a SEM image of primary particles at a magnification of 20,000 times. The average value of the primary particle diameter was 0.05 μm. Based on the method described in the first embodiment, the particles were observed by observing an SEM image at a magnification of 10,000 times. An example is shown in FIG. 17. Although the particles appear to be joined to adjacent particles by necking or aggregation, in Comparative Example 2, the formation of secondary particles by multiple particles was not observed, and it was difficult to determine the secondary particles. For this reason, the unevenness coefficient was not calculated.
[0254] The measurement results for the composite metal oxide powders obtained in Examples 2 to 8 are shown in Table 2 below.
[0255] <Evaluation of battery performance> Using the active material powders obtained in the above Examples and Comparative Examples, electrodes were fabricated as follows.
[0256] First, 100 parts by mass of active material, 6 parts by mass of conductive agent, and 4 parts by mass of binder were dispersed in a solvent to prepare a slurry. The composite material powder obtained by the above-mentioned method was used as the active material. The conductive agent was a mixture of acetylene black, carbon nanotubes, and graphite. The binder was a mixture of carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR). Pure water was used as the solvent.
[0257] The resulting slurry was then applied to one side of a current collector, and the coating was dried to form an active material-containing layer. An aluminum foil with a thickness of 12 μm was used as the current collector. The current collector and the active material-containing layer were then pressed together to obtain an electrode. The weight of the electrode was 60 g / m 2 It was.
[0258] A non-aqueous electrolyte was prepared as follows. An electrolyte salt was dissolved in an organic solvent to obtain a liquid non-aqueous electrolyte. LiPF6 was used as the electrolyte salt. The molar concentration of LiPF6 in the non-aqueous electrolyte was 1 mol / L. A mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) was used as the organic solvent. The volume ratio of EC to DEC was 1:2.
[0259] A three-electrode beaker cell was fabricated using the electrode obtained by the above-mentioned method as a working electrode, metallic lithium foil as a counter electrode and a reference electrode, and the nonaqueous electrolyte prepared by the above-mentioned method.
[0260] The initial charge / discharge performance and cycle life performance of each cell were evaluated. Specifically, the evaluation temperature was 25°C, and the potential range was the lower limit potential of 0.4V (vs. Li / Li + ), upper limit potential 3.2V (vs. Li / Li + ) and charging / discharging was performed. Charging was performed in constant current-constant voltage mode, and discharging was performed in constant current mode. The current value for the initial charging / discharging was 0.2C. The capacity during discharging was measured to determine the initial discharge capacity. After confirming the initial discharge capacity, the cycle life was evaluated. Charging / discharging at a current value of 1C was repeated, and the retention rate of the discharge capacity at the 30th cycle relative to the discharge capacity at the 1st cycle was calculated and evaluated (cycle capacity retention rate (%) = [discharge capacity at 30th cycle / discharge capacity at 1st cycle] × 100%). The calculated values are summarized in Table 2 below.
[0261] Table 1 below shows the temperature conditions for the first and second firings in the firing of the precursor when synthesizing the composite metal oxide, the composition of the resulting composite metal oxide, and the crystal structure contained in the resulting composite metal oxide. As the composition of the composite oxide, the stoichiometric ratio of element M, Nb element, and Mo element is shown. Table 2 shows the average secondary particle size and average primary particle size, BET specific surface area, and average roughness coefficient FU, which were obtained by particle size distribution measurement and SEM observation. ave , as well as the initial discharge capacity and cycle capacity retention rate determined by the above-mentioned battery performance evaluation.
[0262] [Table 1]
[0263] [Table 2]
[0264] As shown in Table 1, in Examples 1 to 8, the composite metal oxide crystal structure contained a non-periodic crystal structure as shown in FIG. 1, and the average roughness coefficient FU ave As indicated by the fact that the average particle diameter was 0.8 or more, spherical particles were obtained. As shown in Table 2, the batteries using the active materials obtained in Examples 1 to 8 had high initial discharge capacities and good cycle capacity retention rates.
[0265] In contrast, although a non-periodic crystal structure was obtained in Comparative Example 1, spherical particles could not be obtained. The average roughness coefficient FU for the secondary particles in Comparative Example 1 that were not formed into a spherical shape ave was less than 0.8 as described above. The battery using the active material obtained in Comparative Example 1 exhibited a high initial discharge capacity due to the non-periodic crystal structure as shown in Table 1, but the cycle capacity retention rate was lower than those of Examples 1 to 8.
[0266] In Comparative Example 2, as shown in Table 1, no non-periodic crystal structure was obtained, and distinct secondary particles could not be identified as shown in Fig. 17. The initial discharge capacity of the battery using the active material not containing a non-periodic crystal structure obtained in Comparative Example 2 was lower than those of Examples 1 to 8.
[0267] According to one or more of the embodiments and examples described above, an active material containing a composite metal oxide is provided. The composite metal oxide contains Mo, Nb, and at least one element M. The element M is selected from the group consisting of Ti, V, Ta, Fe, Co, Mn, Ni, Bi, Sb, As, P, Cr, W, B, Na, K, Mg, Al, Ca, Y, and Si. The crystal structure of the composite metal oxide has a non-periodic crystal structure. The composite metal oxide is contained as spherical particles. The spherical particles are secondary particles of the composite metal oxide, and the average particle diameter of the primary particles is 10 nm or more and 300 nm or less, and the average particle diameter of the secondary particles is 1 μm or more and 10 μm or less. The active material can provide an electrode that can realize a high-capacity and long-life secondary battery, a high-capacity and long-life secondary battery and battery pack, and a vehicle equipped with the battery pack.
[0268] Several embodiments according to the present invention will be described below. [1] An active material comprising a composite metal oxide containing Mo and Nb elements and at least one element M selected from the group consisting of Ti, V, Ta, Fe, Co, Mn, Ni, Bi, Sb, As, P, Cr, W, B, Na, K, Mg, Al, Ca, Y and Si, wherein the composite metal oxide has a non-periodic crystal structure and contains the composite metal oxide as spherical particles, the spherical particles comprising primary particles of the composite metal oxide having an average particle diameter of 10 nm or more and 300 nm or less, and secondary particles having an average particle diameter of 1 μm or more and 10 μm or less. [2] The average roughness coefficient FU for the spherical particles ave The active material according to [1], wherein the n-type charge-dissipating capacity is 0.8 or more. [3] The BET specific surface area of the spherical particles is 5 g / m 2 More than 40 g / m 2 The active material according to [1] or [2] below. [4] An electrode comprising the active material according to any one of [1] to [3]. [5] The electrode according to [4], further comprising an active material-containing layer containing the active material. [6] A positive electrode; A negative electrode; Electrolytes and A secondary battery comprising: The secondary battery, wherein the positive electrode or the negative electrode is the electrode according to [4] or [5]. [7] A battery pack comprising the secondary battery described in [6]. [8] An external terminal for supplying current; Protection circuit and The battery pack according to [7], further comprising: [9] A battery comprising a plurality of the secondary batteries, The battery pack according to [7] or [8], wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.
[10] A vehicle equipped with a battery pack described in any one of [7] to [9].
[11] A vehicle as described in
[10] , including a mechanism for converting kinetic energy of the vehicle into regenerative energy.
[0269] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0270] 1...electrode group, 2...exterior member, 3...negative electrode, 3a...negative electrode current collector, 3b...negative electrode active material containing layer, 3c...negative electrode current collecting tab, 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material containing layer Layered, 6... Negative electrode terminal, 7... Positive electrode terminal, 10... Crystal structure, 10a... Octahedron, 10b... Tetrahedron, 11... Crystal structure, 11a... Octahedron, 11b... Tetrahedron, 18... Metal element, 19... Oxygen element, 21...bus bar, 22...positive electrode lead, 23...negative electrode lead, 24...adhesive tape, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 40...vehicle body, 41...vehicle power source, 42...electrical control device, 43...external terminal, 44...inverter, 45...driving motor, 100...secondary battery, 200...battery pack, 200a...battery pack, 200b... Battery pack, 200c... battery pack, 300... battery pack, 300a... battery pack, 300b... battery pack, 300c... battery pack, 301a... battery pack monitoring device, 301b... battery pack monitoring device, 301c... battery pack monitoring device, 342... positive connector, 343... negative connector, 345... thermistor, 346... protection circuit, 342a... wiring, 343a... wiring, 350... for energizing External terminal, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 411...battery management device, 412...communication bus, 413...positive terminal, 414...negative terminal, 415...switch device, 416...current detection unit, 417...negative input terminal, 418...positive input terminal, L1...connection line, L2...connection line, W...drive wheel.
Claims
1. An active material comprising a composite metal oxide containing Mo element, Nb element, and at least one element M selected from the group consisting of Ti, V, Ta, Fe, Co, Mn, Ni, Bi, Sb, As, P, Cr, W, B, Na, K, Mg, Al, Ca, Y and Si, wherein the crystal structure of the composite metal oxide has a non-periodic crystal structure, and the composite metal oxide is contained as spherical particles, the spherical particles comprising primary particles of the composite metal oxide having an average particle diameter of 10 nm or more and 300 nm or less, and secondary particles having an average particle diameter of 1 μm or more and 10 μm or less.
2. The average value FU of the roughness coefficient FU for the spherical particles ave The active material according to claim 1 , wherein the n-th order is 0.8 or more.
3. The spherical particles have a BET specific surface area of 5 g / m 2 More than 40 g / m 2 3. The active material according to claim 1, wherein:
4. An electrode comprising the active material according to claim 1 or 2.
5. The electrode according to claim 4 , comprising an active material-containing layer containing the active material.
6. A positive electrode and A negative electrode; Electrolytes and A secondary battery comprising: The positive electrode or the negative electrode is the electrode according to claim 4 .
7. A battery pack comprising the secondary battery according to claim 6.
8. An external terminal for supplying electricity; Protection circuit and The battery pack of claim 7 further comprising:
9. A battery comprising a plurality of the secondary batteries, The battery pack according to claim 7 , wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.
10. A vehicle comprising the battery pack according to claim 7.
11. The vehicle of claim 10 including a mechanism for converting kinetic energy of the vehicle into regenerative energy.
Citation Information
Patent Citations
Active material for batteries, nonaqueous electrolyte battery and battery pack
JP2016177972A
Electrode, secondary battery, battery pack, and vehicle
JP2019169348A
Active material, electrode, secondary battery, battery pack, and vehicle
JP2022145421A
Active material, electrode, secondary battery, battery pack, and vehicle
JP2024043464A
Active material, electrode, secondary battery, battery pack, and vehicle
JP2024043465A