Positive electrode, and, lithium ion secondary battery

The positive electrode design with controlled pore and additive distribution in the interparticle region enhances lithium ion secondary batteries' capacity and discharge speed, addressing the need for high-performance batteries.

JP2024134235APending Publication Date: 2024-10-03TDK CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023044434
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

There is a demand for lithium ion secondary batteries that can achieve both high capacity and rapid discharge characteristics.

Method used

A positive electrode with a specific structure comprising a current collector and a positive electrode active material layer, where the interparticle region has a solid portion and dispersed pores, and the pore distribution and additive particle distribution are controlled to enhance electrolyte penetration and ion migration.

Benefits of technology

The electrode design enables both high capacity and rapid discharge characteristics, optimizing ion movement and improving electrostatic properties for enhanced battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134235000001_ABST
    Figure 2024134235000001_ABST
Patent Text Reader

Abstract

To provide a positive electrode and a lithium ion secondary battery, each having capacity and quick discharge characteristic which can be made compatible with each other.SOLUTION: A positive electrode active material layer 14 comprises: a plurality of positive electrode active material particles 14P; and an inter-particle region 14Z which is formed between the plurality of positive electrode active material particles 14P. The inter-particle region 14Z includes: a solid portion 14S; and a plurality of fine holes 14V scattered in the solid portion 14S. In a cross-sectional image of the positive electrode active material layer 14, a D50 which denotes area-based distribution of an area circle equivalent diameter of each fine holes 14V is 0.82 μm or less, and a D90 which denotes area-based distribution of an area circle equivalent diameter of each of fine holes 14V is 1.37 μm or less. In the cross-sectional image of the positive electrode active material layer, the inter-particle region 14Z is divided into a two dimensional tetragonal lattice GR. When an area ratio of each fine hole in each secondary tetragonal lattice GR is acquired, a variation coefficient cv1 of each of the fine hole 14V is 0.610 or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode and a lithium ion secondary battery. [Background technology]

[0002] Lithium ion secondary batteries are widely used in mobile devices such as mobile phones and notebook computers, as well as power sources for tools, hybrid cars, etc. In recent years, there has been a demand for lithium ion secondary batteries with high energy density and excellent output characteristics. For example, Patent Document 1 describes a lithium ion secondary battery that can suppress an increase in the internal resistance of the battery during charging and discharging under high output conditions. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2007-109636 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, there is a demand for lithium ion secondary batteries that are superior in capacity and rapid discharge characteristics.

[0005] The present invention has been made in view of the above problems, and has an object to provide a positive electrode and a lithium ion secondary battery that can achieve both high capacity and rapid discharge characteristics. [Means for solving the problem]

[0006] [1] A positive electrode having a current collector and a positive electrode active material layer in contact with at least one main surface of the current collector, the positive electrode active material layer includes a plurality of positive electrode active material particles and an interparticle region formed between the plurality of positive electrode active material particles, the interparticle region has a solid portion and a plurality of pores dispersed within the solid portion; In a cross-sectional image of the positive electrode active material layer, a D50 of an area-based distribution of the equivalent circle diameters of the pores is 0.82 μm or less, and a D90 of an area-based distribution of the equivalent circle diameters of the pores is 1.37 μm or less, a positive electrode, in which, when the interparticle region is divided into a two-dimensional square lattice in a cross-sectional image of the positive electrode active material layer and the area ratio of the pores in each two-dimensional square lattice is obtained, the coefficient of variation CV1 of the area ratio of the pores is 0.610 or less.

[0007] [2] The positive electrode according to [1], wherein the solid portion contains a binder and a conductive assistant.

[0008] [3] The positive electrode according to [1] or [2], wherein the solid portion contains additive particles made of Co3O4 powder, LiCoO2 powder, or a combination thereof.

[0009] [4] The positive electrode according to [3], wherein when the area ratio of the additive particles in each two-dimensional square lattice is obtained, the coefficient of variation CV2 of the area ratio of the additive particles is 0.601 or less.

[0010] [5] A lithium ion secondary battery comprising the positive electrode according to any one of [1] to [4] and a negative electrode. Effect of the Invention

[0011] A positive electrode and a lithium ion secondary battery are provided that are capable of achieving both high capacity and rapid discharge characteristics. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a lithium-ion secondary battery according to an example of the present embodiment. [Diagram 2] 2 is an enlarged schematic view of a cross section of the positive electrode active material layer in FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] (Lithium-ion secondary battery) 1 is a schematic cross-sectional view showing a lithium-ion secondary battery according to an example of the present embodiment. As shown in Fig. 1, the lithium-ion secondary battery 100 mainly includes a laminate 30, a case 50 that houses the laminate 30 in a sealed state, and a pair of leads 60, 62 connected to the laminate 30.

[0014] The laminate 30 includes one or more positive electrodes 10 and one or more negative electrodes 20, which are disposed facing each other with a separator 18 sandwiched therebetween. The positive electrode 10 includes a positive electrode active material layer 14 provided on one or both main surfaces of a plate-like (film-like) positive electrode current collector 12.

[0015] The negative electrode 20 has a negative electrode active material layer 24 provided on one or both main surfaces of a plate-like (film-like) negative electrode collector 22. The main surface of the positive electrode active material layer 14 and the main surface of the negative electrode active material layer 24 are in contact with the main surface of the separator 18. Leads 60, 62 are connected to ends of the positive electrode collector 12 and the negative electrode collector 22, respectively, and the ends of the leads 60, 62 extend to the outside of the case 50. First, the positive electrode 10 will be specifically described.

[0016] (positive electrode 10) (Positive electrode current collector 12) The positive electrode current collector 12 may be any conductive plate material, and may be, for example, a thin metal plate (metal foil) of aluminum, copper, nickel, or an alloy thereof.

[0017] (Cathode active material layer 14) 2 shows an enlarged cross-sectional view of the positive electrode active material layer 14. The positive electrode active material layer 14 includes a plurality of positive electrode active material particles 14P and interparticle regions 14Z formed between the plurality of positive electrode active material particles 14P. The interparticle regions 14Z include a solid portion 14S and a plurality of pores 14V dispersed within the solid portion 14S.

[0018] The solid portion 14S has binder portions 14B that bind the cathode active material particles 14P to each other and the cathode active material particles 14P to the cathode current collector 12, and the solid portion 14S may further have additive particles 14A. The binder portion 14B contains a binder and may further contain a conductive aid.

[0019] (Cathode active material particles 14P) The cathode active material is not particularly limited as long as it can reversibly proceed with the occlusion and release of lithium ions, the desorption and intercalation of lithium ions, or the doping and dedoping of lithium ions and the counter anion of the lithium ions (for example, ClO4 - ), and known active materials can be used. For example, lithium cobaltate (LiCoO2), lithium nickelate (LiNiO2), lithium manganese spinel (LiMn2O4), and the general formula: LiNi x Co y Mn z M a O2 (x + y + z + a = 1, 0 ≤ x ≤ 1, 0 ≤ y ≤ 1, 0 ≤ z ≤ 1, 0 ≤ a ≤ 1, M is one or more elements selected from Al, Mg, Nb, Ti, Cu, Zn, Cr), lithium vanadium compound (LiV2O5), olivine type LiMPO4 (where M represents one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, Zr or VO), lithium titanate (Li4Ti5O 12 ), LiNi x Co y Al z O2 (0.9 < x + y + z < 1.1), etc.

[0020] There is no particular limitation on the particle size of the cathode active material particles, but in terms of D50 of the area-based distribution of the equivalent circle diameter of the area of the cathode active material particles in the cross-sectional photograph of the cathode active material layer, it can be 0.1 to 30 μm.

[0021] (Binder portion 14B) The binder portion 14B bonds the positive electrode active material particles 14P to each other and also bonds the positive electrode active material particles 14P to the positive electrode current collector 12. The binder contained in the binder portion may be any binder capable of the above-mentioned bonding, and examples thereof include fluororesins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE). In addition to the above, examples of binders that may be used include cellulose, styrene-butadiene rubber, ethylene-propylene rubber, acrylic resin, polyimide resin, and polyamide-imide resin. In addition, examples of binders that may be used include electronically conductive conductive polymers and ionically conductive conductive polymers. Examples of electronically conductive conductive polymers include polyacetylene. In this case, the binder also functions as conductive additive particles, so that it is not necessary to add a conductive additive. As the ion-conductive conductive polymer, for example, one having ion conductivity such as lithium ion can be used, and examples thereof include a composite of a monomer of a polymer compound (polyether polymer compounds such as polyethylene oxide and polypropylene oxide, polyphosphazene, etc.) and a lithium salt such as LiClO4, LiBF4, LiPF6, or an alkali metal salt mainly composed of lithium. Examples of the polymerization initiator used for the composite include a photopolymerization initiator or a thermal polymerization initiator that is compatible with the above-mentioned monomer.

[0022] The content of the binder in the positive electrode active material layer 14 is not particularly limited, but is preferably 1 to 10 mass % based on the sum of the masses of the active material, the conductive assistant, and the binder. By setting the contents of the active material and the binder within the above ranges, it is possible to suppress the tendency that the amount of the binder is too small in the obtained positive electrode active material layer 14, making it impossible to form a strong active material layer. It is also possible to suppress the tendency that the amount of the binder that does not contribute to the electric capacity increases, making it difficult to obtain a sufficient volumetric energy density.

[0023] (Conductive assistant) The conductive assistant contained in the binder portion 14B is not particularly limited as long as it improves the conductivity of the positive electrode active material layer 14, and a known conductive assistant can be used. Examples of the conductive assistant include carbon-based materials such as graphite and carbon black, metal fine powders such as copper, nickel, stainless steel, and iron, mixtures of carbon materials and metal fine powders, and conductive oxides such as ITO.

[0024] The content of the conductive assistant in the positive electrode active material layer 14 is not particularly limited, but when added, the content is preferably 0.5 to 5 mass % relative to the mass of the active material.

[0025] (Additive Particle 14A) The solid portion 14S may contain additive particles 14A made of Co3O4 powder, LiCoO2 powder, or a combination thereof. The average particle size of the additive particles 14A is not particularly limited, but may be 5 to 150 nm in the area-based distribution D50 of the area-equivalent circle diameter of the additive particles 14A in a cross-sectional photograph of the positive electrode active material layer. When manufacturing a battery, these additive particles function as a decomposition catalyst for lithium carbonate nanoparticles contained in the positive electrode active material layer before the first charge / discharge. In addition, after the first charge / discharge, the electrostatic characteristics of the positive electrode active material layer are improved, the migration potential of lithium ions is increased, and the capacity and / or rapid discharge characteristics are further improved.

[0026] (14V pores) As described above, the inter-particle regions 14Z formed between the plurality of positive electrode active material particles 14P have the solid portion 14S and the plurality of pores 14V dispersed within the solid portion 14S, and are spongy.

[0027] In the cross-sectional image of the positive electrode active material layer, the area-based distribution D50 of the equivalent circle diameter of the area of ​​the pores 14V is 0.82 μm or less. The D50 may be 0.70 μm or less, or 0.60 μm or less. D50 is the particle size at which the number ratio of particles smaller than this value is 50%.

[0028] In the cross-sectional image of the positive electrode active material layer, the area-based distribution D90 of the area-equivalent circle diameter of the pores 14V is 1.37 μm or less. The D90 may be 1.30 μm or less, or 1.20 μm or less. D90 is the particle size at which 90% of the particles are smaller than this size.

[0029] In obtaining these particle size distributions, it is preferable that the number of pores 14V is, for example, about 200 to 700.

[0030] Furthermore, in this embodiment, as shown in Fig. 2, when the interparticle regions 14Z are divided into two-dimensional square lattices GR in a cross-sectional image of the positive electrode active material layer, and the area ratio of the pores 14V in each two-dimensional square lattice GR is obtained, the coefficient of variation CV1 of the area ratio of the pores 14V is 0.610 or less. The coefficient of variation is the standard deviation / average value.

[0031] When the interparticle region 14Z contains additive particles 14A, when the interparticle region 14Z is divided into two-dimensional square lattice GR and the area ratio of the additive particles 14A in each two-dimensional square lattice GR is obtained, it is preferable that the coefficient of variation CV2 of the area ratio of the additive particles is 0.601 or less.

[0032] The direction of the cross-sectional image of the positive electrode active material layer is not particularly limited, and the cross-section may be perpendicular to the main surface of the current collector or parallel to the main surface of the current collector, but a cross-section perpendicular to the main surface of the current collector is preferable. Each region in the cross-sectional image can be identified by the brightness of the image, the surface condition, element mapping, etc.

[0033] The size of the two-dimensional square lattice GR is preferably 0.5 to 4.0 μm on a side. The lattices to be measured for the area ratio of the pores and additive particles are limited to those in which the area ratio of the positive electrode active material particles 14P is 50% or less. Furthermore, the closed pores in the positive electrode active material particles 14P are not included in the interparticle regions 14Z. The number of two-dimensional square lattices to obtain the area ratio is preferably 90 to 360.

[0034] (action) In such a positive electrode, the diameter of the pores 14V is smaller than that of the conventional one, and the small diameter pores 14V are spatially uniformly dispersed. Therefore, it is considered that the electrolyte is easily permeated into the positive electrode active material layer 14, the electrolyte and salt can be quickly contacted with the positive electrode active material, and the insertion and desorption of Li ions is efficiently performed. Specifically, the capacity can be increased by increasing the amount of Li ions moving between the positive electrode and the negative electrode. In addition, the rapid discharge characteristic can be improved by increasing the movement speed of Li ions between the positive electrode and the negative electrode. Therefore, a lithium ion secondary battery that is particularly effective for tools, electric vehicles, etc. can be realized.

[0035] Furthermore, when the solid portion of the positive electrode active material layer contains additive particles, the electrostatic properties are improved, the ion migration potential is increased, and the capacity and / or rapid discharge characteristics are further improved.

[0036] Furthermore, the uniform spatial distribution of the additive particles leads to improved electrostatic properties, optimizing the dielectric material balance and providing a particularly high potential for ion migration, further enhancing the above properties.

[0037] (Manufacturing method of positive electrode) An example of a method for producing such a positive electrode is shown below.

[0038] (Preparation of lithium carbonate nanoparticles or composite particles containing the same) First, lithium carbonate powder with a large particle size (for example, several μm) is dissolved in water. The lower the lithium carbonate concentration of the lithium carbonate aqueous solution, the smaller the particle size of the lithium carbonate nanoparticles that are precipitated later. Next, when poor solvent 1 is added to the lithium carbonate aqueous solution, lithium carbonate nanoparticles, for example, particles with a particle size D50 of 1 to 1000 nm in the volume-based particle size distribution by laser diffraction, are precipitated to obtain a slurry (precipitation step). The amount of poor solvent 1 added is preferably 70 wt% or more relative to water. The larger the amount of poor solvent 1 added, the smaller the particle size of the precipitated lithium carbonate nanoparticles. The poor solvent 1 can be appropriately selected from those that are soluble in water and insoluble in lithium carbonate. In addition, it is preferable that the poor solvent 1 has a boiling point higher than that of water. This is because in the next step of extracting lithium carbonate nanoparticles from the slurry, if the poor solvent 1 evaporates before water when performing thermal drying, the precipitated lithium carbonate will re-dissolve in water. An example of poor solvent 1 is N-methyl-2-pyrrolidone (NMP).

[0039] The slurry can be heated and dried to separate the precipitated lithium carbonate nanoparticles from the slurry and obtain them as a dry powder, but there is a possibility that the lithium carbonate nanoparticles may crosslink with each other and aggregate during drying. Therefore, by further adding poor solvent 2 to the slurry containing lithium carbonate and poor solvent 1 from which the nanoparticles have been precipitated, the nanoparticles are lightly aggregated in the liquid, the aggregated nanoparticles are allowed to settle, the supernatant liquid is removed, and poor solvent 2 is further added. By repeating the same procedure, lithium carbonate nanoparticles dispersed in poor solvent 2, for example, with a particle size D50 of 1 to 1000 nm, can be easily obtained. There is no limitation on poor solvent 2 as long as it dissolves in water and NMP and does not dissolve lithium carbonate, but acetone, ethanol, etc. are preferable.

[0040] The resulting lithium carbonate nanoparticles preferably have a D50 of 500 nm or less, and more preferably 200 nm or less, in the area-based distribution of the area-equivalent circle diameter as determined by SEM observation.

[0041] Furthermore, when additive particles are added to the positive electrode active material layer, additive nanoparticles, for example, particles having a particle size D50 of 1 to 1000 nm are added and dispersed in the lithium carbonate aqueous solution before adding the poor solvent 1, and then the poor solvent 1 is added, thereby obtaining composite particles of lithium carbonate nanoparticles and additive nanoparticles.

[0042] Next, a coating material containing a positive electrode active material, a binder, a solvent, a conductive assistant, and lithium carbonate nanoparticles and / or the above composite particles is applied onto the positive electrode current collector, and the solvent in the coating material applied onto the positive electrode current collector is removed.

[0043] As the solvent, for example, water, N-methyl-2-pyrrolidone, N,N-dimethylformamide, etc. can be used.

[0044] The coating method is not particularly limited, and any method that is usually used for producing a positive electrode can be used, such as a slit die coating method or a doctor blade method.

[0045] The method for removing the solvent in the paint applied onto positive electrode current collector 12 is not particularly limited, and positive electrode current collector 12 to which the paint has been applied may be dried in an atmosphere at 80°C to 150°C, for example.

[0046] Then, the positive electrode having the positive electrode active material layer 14 thus formed may then be subjected to a pressing process, for example, by a roll press device, etc. The linear pressure of the roll press may be, for example, 10 to 50 kgf / cm.

[0047] Thereafter, when the positive electrode active material layer 14 containing lithium carbonate nanoparticles is exposed to the first charging process, lithium carbonate decomposes to generate lithium ions, which move to the negative electrode. That is, lithium carbonate functions as a pre-doping material for lithium. From the viewpoint of sufficiently decomposing lithium carbonate, the initial charging voltage is preferably 4.3 V or more. After the initial charging, due to the decomposition of lithium carbonate and the movement of lithium ions, the location where the lithium carbonate nanoparticles existed becomes pores 14V. In the above method, since lithium carbonate nanoparticles are used as a pre-doping agent, fine pores 14V can be spatially uniformly arranged with respect to the positive electrode that has undergone the first charge and discharge. When additive particles are used in combination, if lithium carbonate nanoparticles are precipitated in the presence of the additive particles, the diameter of the pores 14V can be reduced and they can be more easily distributed spatially uniformly. Furthermore, the additive particles 14A can also be more easily distributed spatially uniformly.

[0048] (Negative electrode) (Negative electrode current collector) The negative electrode current collector 22 may be a conductive plate material. For example, a thin metal plate (metal foil) of copper, nickel, stainless steel, or an alloy thereof can be used. From the viewpoint of conductivity, a copper foil is preferably used. The copper foil may be a rolled copper foil or other copper foil. There is no limitation on the thickness of the negative electrode current collector, but for example, it can be 5 to 20 μm.

[0049] (Negative electrode active material layer) The negative electrode active material layer 24 is mainly composed of a negative electrode active material, a binder, and, if necessary, a conductive auxiliary agent in an appropriate amount.

[0050] (Negative electrode active material) Examples of the negative electrode active material include carbon materials such as graphite, graphitizable carbon, easily graphitizable carbon, and low-temperature calcined carbon that can occlude and release (intercalate and deintercalate, or dope and de-dope) lithium ions, metals and alloys such as Al, Si, and Sn that can combine with lithium, and crystalline or amorphous compounds mainly composed of oxides such as SiO x (0 < x < 2), TiO2, SnO2, etc., and lithium titanate (Li4Ti5O 12) and the like.

[0051] (Negative electrode binder and negative electrode conductive additive) The binder and conductive assistant may be the same as the materials used in the positive electrode 10 described above. The contents of the binder and conductive assistant may be appropriately adjusted when the magnitude of the volume change of the negative electrode active material or the adhesion to the foil must be taken into consideration, and the same contents as those in the positive electrode 10 described above may be adopted. When added, the amount of the binder added is preferably 2 to 20 mass% with respect to the mass of the active material. The amount of the conductive assistant added is preferably 0.5 to 5 mass% with respect to the mass of the active material. In addition, some types of binders, such as thermosetting binders, require heat treatment at any temperature of 200°C or higher.

[0052] (Method of manufacturing negative electrode) Methods for producing a negative electrode are known, and include, for example, applying a coating material containing a negative electrode active material, a binder, a solvent, and a conductive assistant onto a negative electrode current collector, and then removing the solvent from the coating material applied to the current collector.

[0053] (Separator) There are no particular limitations on the separator as long as it is stable to the electrolyte and has excellent electrolyte retention properties, but typical examples include porous sheets of polyolefins such as polyethylene and polypropylene, or nonwoven fabrics.

[0054] (electrolyte) The electrolyte is contained in the positive electrode active material layer 14, the negative electrode active material layer 24, and the separator 18. The electrolyte is not particularly limited, and for example, in this embodiment, an electrolyte solution containing a lithium salt (aqueous electrolyte solution, an electrolyte solution using an organic solvent) can be used. However, since the electrolyte aqueous solution has a low electrochemical decomposition voltage and therefore the withstand voltage during charging is limited to a low level, an electrolyte solution using an organic solvent (non-aqueous electrolyte solution) is preferable. As the electrolyte solution, one in which a lithium salt is dissolved in a non-aqueous solvent (organic solvent) is preferably used. As the lithium salt, there is no particular limit, and lithium salts used as electrolytes for lithium ion secondary batteries can be used. As the lithium salt, for example, inorganic acid anion salts such as LiPF6, LiBF4, etc., organic acid anion salts such as LiCF3SO3, (CF3SO2)2NLi, etc. can be used.

[0055] Examples of the organic solvent include aprotic high-dielectric constant solvents such as ethylene carbonate, propylene carbonate, etc., and aprotic low-viscosity solvents such as acetates or propionates such as dimethyl carbonate, ethyl methyl carbonate, etc. It is desirable to use these aprotic high-dielectric constant solvents and aprotic low-viscosity solvents in combination at an appropriate mixing ratio. Furthermore, ionic liquids using imidazolium, ammonium, and pyridinium type cations can be used. The counter anion is not particularly limited, but examples thereof include BF4 - , PF6 - , (CF3SO2)2N - The ionic liquid can be used by mixing with the above-mentioned organic solvent.

[0056] From the viewpoint of electrical conductivity, the concentration of the lithium salt in the electrolyte is preferably 0.5 to 2.0 M. The conductivity of this electrolyte at a temperature of 25° C. is preferably 0.01 S / m or more, and is adjusted by the type or concentration of the electrolyte salt.

[0057] When the electrolyte is a solid electrolyte or a gel electrolyte, it is possible to include silicone gel, poly(vinylidene fluoride), or the like as a polymer material.

[0058] Furthermore, various additives may be added to the electrolyte solution of the present embodiment as necessary, such as vinylene carbonate, methylvinylene carbonate, etc. for improving cycle life, biphenyl, alkylbiphenyl, etc. for preventing overcharging, and various carbonate compounds, various carboxylic acid anhydrides, and various nitrogen- and sulfur-containing compounds for deoxidization and dehydration.

[0059] (case) The case 50 seals the laminate 30 and the electrolyte therein. The case 50 is not particularly limited as long as it can prevent leakage of the electrolyte to the outside and intrusion of moisture from the outside into the lithium ion secondary battery 100. For example, as shown in FIG. 1, a metal laminate film in which a metal foil 52 is coated on both sides with a polymer film 54 can be used as the case 50. For example, an aluminum foil can be used as the metal foil 52, and a film such as polypropylene can be used as the polymer film 54. For example, a polymer with a high melting point, such as polyethylene terephthalate (PET) or polyamide, is preferable as the material of the outer polymer film 54, and a polyethylene (PE) or polypropylene (PP) is preferable as the material of the inner polymer film 54.

[0060] (Lead) The leads 60, 62 are made of a conductive material such as aluminum.

[0061] Then, by a known method, the leads 60, 62 are welded to the positive electrode current collector 12 and the negative electrode current collector 22, respectively, and the separator 18 is sandwiched between the positive electrode active material layer 14 of the positive electrode 10 and the negative electrode active material layer 24 of the negative electrode 20. This state is then inserted into the case 50 together with the electrolyte, and the entrance of the case 50 is sealed.

[0062] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-mentioned embodiments. For example, the lithium ion secondary battery is not limited to the shape shown in Fig. 1, and may be a coin type in which an electrode and a separator punched into a coin shape are laminated, or a cylinder type in which an electrode sheet and a separator are spirally wound. EXAMPLES

[0063] [Example 1] (Preparation of lithium carbonate particles) 600mL of NMP was added to 200mL of a 0.4wt% lithium carbonate aqueous solution to precipitate lithium carbonate nanoparticles. The D50 of the area-based distribution of the area-equivalent circle diameter of the lithium carbonate nanoparticles observed by SEM was 200nm.

[0064] (Preparation of positive electrode) A slurry was prepared by dispersing heated and dried lithium carbonate nanoparticles, lithium-containing nickel-cobalt-manganese composite oxide particles as a positive electrode active material, acetylene black as a conductive assistant, and polyvinylidene fluoride as a binder in a solvent, N-methyl-2-pyrrolidone (NMP). The slurry was prepared so that the weight ratio of the nickel-cobalt-manganese composite oxide particles, acetylene black, and polyvinylidene fluoride in the slurry was 97:1.5:1.5. This slurry was applied onto an aluminum foil as a current collector, dried, and then rolled to prepare a positive electrode on which the positive electrode active material layer of Example 1 was formed.

[0065] (Preparation of negative electrode) [Preparation of negative electrode cell for evaluation] A slurry was prepared by dispersing a mixture of silicon-containing particles, a binder polyimide (PI), and acetylene black in a solvent N-methyl-2-pyrrolidone (NMP). The weight ratio of silicon particles, acetylene black, and polyimide in the slurry was 80:10:10. This slurry was applied to a copper foil negative electrode current collector, dried, and then rolled to produce a negative electrode.

[0066] (Battery Construction) Next, the negative electrode and the negative electrode were punched out so that the capacity of the battery was 1000mAh, and then a separator made of a polyethylene microporous film was sandwiched between the negative electrode and the positive electrode to obtain a laminate (power generation element). This laminate was placed in an aluminum laminator pack, and an electrolyte solution was mixed in a volume ratio of fluoroethylene carbonate (FEC):vinylene carbonate (VC):ethyl methyl carbonate (EMC) = 1:1:8, and LiPF6 was dissolved in the electrolyte solution to a concentration of 1.3mol / L, and then the pack was vacuum sealed to produce the lithium ion secondary battery of Example 1.

[0067] (Initial charge / discharge) The lithium-ion secondary battery was initially charged in a thermostatic chamber at 25°C with an upper limit voltage of 4.48V and a charge rate of 0.1C (the current value at which charging is completed in 10 hours when constant current charging is performed).Then, the lithium-ion secondary battery was initially discharged in a thermostatic chamber at 25°C with a lower limit voltage of 2.5V and a discharge rate of 0.1C.

[0068] (Evaluation of battery characteristics) Next, the discharge capacity and discharge rate characteristics (rapid discharge characteristics) of the lithium-ion secondary battery were determined. The charge capacity was measured in a thermostatic chamber at 25°C when the charge rate was 0.1C (the current value at which charging is completed in 10 hours when constant current charging is performed), and then the initial discharge capacity was measured in a thermostatic chamber at 25°C when the discharge rate was 0.2C to determine the discharge capacity.

[0069] The 4C discharge rate characteristics were determined by charging at a 0.1C charge rate (the current value at which discharge ends in 10 hours when constant current discharge is performed at 25°C), then measuring the discharge capacity at a 0.2C discharge rate in a thermostatic chamber at 25°C, and again charging at a 0.1C charge rate (the current value at which discharge ends in 10 hours when constant current discharge is performed at 25°C), then measuring the discharge capacity at a 4C discharge rate in a thermostatic chamber at 25°C, and calculating the ratio of the 4C discharge capacity to the 0.2C discharge capacity.

[0070] A SEM image of a cross section perpendicular to the main surface of the current collector of the positive electrode active material layer after initial charge and discharge was obtained. The image size was 1357 x 967 pixels, and the image size was 12.7 x 9.0 μm. A solid portion 14S and a plurality of pores 14V dispersed in the solid portion 14S were observed in the interparticle region 14Z formed between a plurality of positive electrode active material particles 14P. The area circle equivalent diameter of each pore was calculated to obtain the area-based distribution of the pore diameter, and D50 and D90 were obtained. The number of pores used in the calculation was 261.

[0071] The obtained SEM image was divided into a two-dimensional square lattice with a side length of 1 μm. The pore area ratio was obtained for each lattice in which the area ratio of the positive electrode active material particles 14P was 50% or less, and the coefficient of variation CV1 was obtained. The number of lattices was 95.

[0072] [Example 2] (Preparation of composite particles) 0.4 g of cobalt oxide (Co3O4) particles with a particle size D50 of 30 nm were added as an additive and dispersed in 200 ml of a lithium carbonate aqueous solution with a concentration of 0.4 wt%. 200 ml of NMP was added to this dispersion to precipitate composite particles that are lithium carbonate nanoparticles with cobalt oxide particles supported on the surface. The size of the lithium carbonate particles that make up the composite particles was 1000 nm as D50. The other procedures were the same as in Example 1, and a lithium ion secondary battery was obtained and evaluated.

[0073] The area ratio of additive particles within each two-dimensional square lattice was also obtained. The number of lattices was the same as that for voids.

[0074] [Example 3] A lithium ion secondary battery was obtained and evaluated in the same manner as in Example 2, except that the amount of NMP added was 600 ml and the size of the lithium carbonate particles constituting the composite particles was 200 nm as D50.

[0075] [Example 4] A lithium ion secondary battery was obtained and evaluated in the same manner as in Example 2, except that the amount of NMP added was 800 ml and the size of the lithium carbonate particles constituting the composite particles was 100 nm as D50.

[0076] [Example 5] A lithium ion secondary battery was obtained in the same manner as in Example 2, except that the amount of NMP added was 1000 ml and the size of the lithium carbonate particles constituting the composite particles was 80 nm as D50.

[0077] [Example 6] A lithium ion secondary battery was obtained in the same manner as in Example 2, except that the amount of NMP added was 600 ml, the size of the lithium carbonate particles constituting the composite particles was 200 nm as D50, and lithium cobalt oxide particles having a particle size of 30 nm were used instead of the cobalt oxide particles.

[0078] [Example 7] A lithium ion secondary battery was obtained in the same manner as in Example 6, except that the amount of NMP added was 800 ml and the size of the lithium carbonate particles constituting the composite particles was 100 nm as D50.

[0079] [Example 8] A lithium ion secondary battery was obtained in the same manner as in Example 6, except that the amount of NMP added was 1000 ml and the size of the lithium carbonate particles constituting the composite particles was 80 nm as D50.

[0080] [Comparative Example 1] A lithium ion secondary battery was obtained in the same manner as in Example 2, except that in the preparation of the composite particles, a precipitation step of lithium carbonate in the presence of additive particles as in the Examples was not used, and composite particles were used in which cobalt oxide particles having a particle size of 30 nm were supported by a migration method on the surface of lithium carbonate particles having a particle size D50 of 2000 nm.

[0081] [Comparative Example 2] A lithium ion secondary battery was obtained in the same manner as in Example 2, except that in the preparation of the composite particles, instead of using a precipitation process as in the Example, lithium carbonate raw material powder was mixed with cobalt oxide particles having a particle size of 30 nm, and composite particles having a particle size of 1000 nm as D50 of the lithium carbonate particles and having cobalt oxide particles supported on the surface were obtained by a mechanochemical method. The conditions and results are shown in Table 1.

[0082] [Table 1] [Explanation of symbols]

[0083] 10...positive electrode, 12...positive electrode current collector, 14...positive electrode active material layer, 14P...positive electrode active material particle, 14S...solid portion, 14V...pore, 14Z...interparticle region, 20...negative electrode, 22...negative electrode current collector, 24...negative electrode active material layer, 100...lithium ion secondary battery, GR...two-dimensional square lattice.

Claims

1. A positive electrode having a current collector and a positive electrode active material layer in contact with at least one main surface of the current collector, the positive electrode active material layer includes a plurality of positive electrode active material particles and an interparticle region formed between the plurality of positive electrode active material particles, the interparticle region has a solid portion and a plurality of pores dispersed within the solid portion; In a cross-sectional image of the positive electrode active material layer, a D50 of an area-based distribution of the equivalent circle diameters of the pores is 0.82 μm or less, and a D90 of an area-based distribution of the equivalent circle diameters of the pores is 1.37 μm or less, a positive electrode, in which, when the interparticle region is divided into a two-dimensional square lattice in a cross-sectional image of the positive electrode active material layer and the area ratio of the pores in each two-dimensional square lattice is obtained, a coefficient of variation CV1 of the area ratio of the pores is 0.610 or less.

2. The positive electrode according to claim 1 , wherein the solid portion comprises a binder and a conductive additive.

3. The solid portion is Co 3 O 4 Powder, LiCoO 2 10. The positive electrode of claim 1 , further comprising additive particles of a zeolite, a zeolite powder, or a combination thereof.

4. 4. The positive electrode according to claim 3, wherein when the area ratio of the additive particles in each two-dimensional square lattice is obtained, a coefficient of variation CV2 of the area ratio of the additive particles is 0.601 or less.

5. A lithium ion secondary battery comprising the positive electrode according to any one of claims 1 to 4 and a negative electrode.

Citation Information

Patent Citations

  • High-nickel ternary precursor, positive electrode material and preparation method thereof

    CN112250091A

  • Lithium compound for nonaqueous lithium-type storage element

    JP2019029110A

  • Composite particle, positive electrode, and lithium-ion secondary battery

    JP2022150407A

  • Electrode for battery

    JP2007109636A