Battery, separation method of battery, and manufacturing method of battery

The battery design with controlled peel strengths and argyrodite-type sulfide solid electrolytes addresses separation and interfacial resistance issues, enhancing rapid charging and recyclability.

JP2024134906APending Publication Date: 2024-10-04PANASONIC HOLDINGS CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023045346
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing lithium ion secondary batteries face challenges in separating positive and negative electrodes for replacement or recycling, and they struggle with high interfacial resistance and dendrite growth leading to internal short circuits, especially during rapid charging.

Method used

The battery design features a structure with controlled peel strengths between electrode layers and solid electrolyte layers, utilizing argyrodite-type sulfide solid electrolytes, and adjusting porosity to minimize interfacial resistance and facilitate easy separation.

Benefits of technology

This design enables easy separation of electrodes, reduces dendrite growth, and enhances battery characteristics such as rapid charging capacity and efficiency, improving safety and recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134906000001_ABST
    Figure 2024134906000001_ABST
Patent Text Reader

Abstract

To provide a battery and the like having high battery characteristics in addition to the possibility of easy separation of positive and negative electrodes.SOLUTION: A battery 10 has a structure in which a positive electrode current collector layer 14, a positive electrode layer 11, a solid electrolyte layer 13, a negative electrode layer 12, and a negative electrode current collector layer 15 are stacked in this order. The peel strength between the positive electrode layer 11 and the solid electrolyte layer 13 is 1.8 N / cm or less. A 1 Hz AC resistance of the battery 10 at 25°C with an SOC (State Of Charge) of 50% is less than 100 Ωcm2.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to batteries, methods of separating batteries, and methods of manufacturing batteries. [Background technology]

[0002] A lithium ion secondary battery is a storage battery that has a negative electrode layer, a positive electrode layer, and an electrolyte sandwiched between the negative electrode layer and the positive electrode layer, and is capable of charging and discharging by moving lithium ions back and forth between the two electrode layers. Conventionally, an organic electrolyte has been used as the electrolyte in a lithium ion secondary battery. However, the organic electrolyte is prone to leakage, and there is also a risk of short circuiting inside the battery due to overcharging, so there is a demand for further improvement in reliability and safety.

[0003] Under these circumstances, development of all-solid-state lithium-ion secondary batteries using inorganic solid electrolytes instead of organic electrolytes is underway. Hereinafter, batteries using solid electrolytes as electrolytes, such as all-solid-state lithium-ion secondary batteries, will be referred to as "all-solid-state batteries". All-solid-state batteries are made of solids in the negative electrode layer, electrolyte layer, and positive electrode layer, and are said to be able to greatly improve the safety and reliability that are issues with batteries using organic electrolytes, and to enable longer life. In addition, due to the characteristics of the solid electrolyte, such as high flame retardancy, high pack energy density due to no need for a cooling unit, and high-rate charging, it is expected that it will be put to practical use, for example, in automobile applications.

[0004] In an all-solid-state battery, the interface resistance can be reduced by increasing the bonding strength of each layer, thereby improving the battery characteristics. For example, Patent Document 1 describes how increasing the peel strength between the solid electrolyte layer and other layers can suppress warping of each layer and ensure adhesion.

[0005] Furthermore, Patent Document 2 describes that, in anticipation of recycling of an all-solid-state battery after it has been used up, a thermoplastic resin is disposed on the surface of the solid electrolyte layer, and the positive and negative electrodes are separated by heating to a temperature equal to or higher than the melting point of the thermoplastic resin during recycling. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2015 / 147122 [Patent Document 2] JP 2016-134254 A Summary of the Invention [Problem to be solved by the invention]

[0007] For batteries, excellent battery characteristics such as excellent charging load characteristics are required for rapid charging in automotive applications, etc. In addition, it is also important that the positive and negative electrodes can be separated for electrode replacement in case of initial defective electrode layers and for recycling after the battery has been used up.

[0008] Therefore, an object of the present disclosure is to provide a battery or the like that not only allows easy separation of the positive and negative electrodes but also has excellent battery characteristics. [Means for solving the problem]

[0009] A battery according to one embodiment of the present disclosure has a structure in which a positive electrode current collector layer, a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, and the peel strength between the positive electrode layer and the solid electrolyte layer is 1.8 N / cm or less, and the AC resistance of the battery at 1 Hz at 25°C when the SOC (State Of Charge) is 50% is 100 Ω cm 2 The following is the result.

[0010] A method for separating a battery according to an aspect of the present disclosure includes separating the battery between the positive electrode layer and the solid electrolyte layer.

[0011] A battery according to an embodiment of the present disclosure has a structure in which a positive electrode current collector layer, a positive electrode layer, two or more solid electrolyte layers, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, and at least one of a peel strength between adjacent solid electrolyte layers of the two or more solid electrolyte layers and a peel strength between the positive electrode layer and a solid electrolyte layer adjacent to the positive electrode layer of the two or more solid electrolyte layers is 1.8 N / cm or less, and an AC resistance of the battery at 25°C at 1 Hz when the SOC is 50% is 100 Ω cm 2 The following is the result.

[0012] Furthermore, a battery separation method according to one embodiment of the present disclosure is a battery separation method, in which the battery is separated between adjacent solid electrolyte layers of the two or more solid electrolyte layers, or between the positive electrode layer and a solid electrolyte layer adjacent to the positive electrode layer of the two or more solid electrolyte layers.

[0013] A method for producing a battery according to an embodiment of the present disclosure is a method for producing a battery having a structure in which a positive electrode current collector layer, a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, the method comprising the steps of: adjusting a peel strength between the positive electrode layer and the solid electrolyte layer to 1.8 N / cm or less; and determining whether the AC resistance of the battery at 1 Hz at 25° C. and SOC of 50% is 100 Ω cm 2 and adjusting so that:

[0014] A method for manufacturing a battery according to an embodiment of the present disclosure is a method for manufacturing a battery having a structure in which a positive electrode current collector layer, a positive electrode layer, two or more solid electrolyte layers, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, the method comprising adjusting at least one of a peel strength between adjacent solid electrolyte layers of the two or more solid electrolyte layers and a peel strength between the positive electrode layer and a solid electrolyte layer adjacent to the positive electrode layer of the two or more solid electrolyte layers to 1.8 N / cm or less, and adjusting the AC resistance at 1 Hz of the battery at 25° C. when SOC is 50% to 100 Ω cm 2 and adjusting so that: Effect of the Invention

[0015] According to the present disclosure, in addition to being able to easily separate positive and negative electrodes, it is possible to provide a battery or the like having excellent battery characteristics. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a battery according to the first embodiment. [Diagram 2] FIG. 2 is a flowchart showing an example of a method for manufacturing the battery according to the first embodiment. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing an example of the positive electrode side laminate according to the first embodiment. As shown in FIG. [Figure 4] FIG. 4 is a schematic cross-sectional view showing an example of the negative electrode side laminate according to the first embodiment. As shown in FIG. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing an example of a battery provided with an exterior body and a restraining member according to embodiment 1. As shown in FIG. [Figure 6] FIG. 6 is a diagram for explaining a method of separating the battery according to the first embodiment. [Figure 7] FIG. 7 is a schematic cross-sectional view showing an example of the battery according to the second embodiment. [Figure 8] FIG. 8 is a flowchart showing an example of a method for manufacturing a battery according to the second embodiment. [Figure 9] FIG. 9 is a schematic cross-sectional view showing an example of the positive electrode side laminate according to the second embodiment. As shown in FIG. [Figure 10] FIG. 10 is a schematic cross-sectional view showing an example of the negative electrode side laminate according to the second embodiment. As shown in FIG. [Figure 11] FIG. 11 is a diagram for explaining a method of separating the battery according to the second embodiment. [Figure 12] FIG. 12 is another diagram for explaining the battery separation method according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] (How one aspect of the present disclosure was achieved) In an all-solid-state battery, for example, lithium ions are released from the lithium transition metal composite oxide or the like that constitutes the positive electrode layer during charging, and these lithium ions reach the negative electrode layer through the solid electrolyte and are absorbed in the negative electrode active material. At this time, a phenomenon may occur in which some of the lithium ions absorbed in the negative electrode active material capture electrons and precipitate as metallic lithium. If this metallic lithium precipitate grows into dendrites (branched crystals) due to repeated charging and discharging, it will eventually come into contact with the positive electrode layer, causing an internal short circuit and making it unable to function as a secondary battery. In particular, for automotive applications, etc., rapid charging is required, but when a battery is rapidly charged, dendrites tend to grow inside the battery, which tends to cause an internal short circuit in the battery. Furthermore, if the interfacial resistance between the positive electrode layer, solid electrolyte layer, and negative electrode layer is high, the internal resistance of the battery will increase, making rapid charging difficult. Therefore, it is important to suppress the growth of dendrites made of metallic lithium and the like to suppress the occurrence of internal short circuits, and to reduce the interfacial resistance between the positive electrode layer, solid electrolyte layer, and negative electrode layer in order to enable rapid charging and extend the life of the battery.

[0018] As described above, Patent Document 1 describes that warping of each layer is suppressed and the layers are adhered to each other by increasing the peel strength between the solid electrolyte layer and other layers. However, all solid-state batteries are made of solids, and when joining each layer and when fabricating a stacked battery, the relatively hard positive electrode layer causes cracks in the solid electrolyte layer. In particular, when the areas of the positive electrode layer, the solid electrolyte layer, and the negative electrode layer are different from each other, cracks expand from the end of the layer with the smaller area when the positive electrode layer, the solid electrolyte layer, and the negative electrode layer are joined, resulting in a problem of low yield during production.

[0019] In addition, if all the layers of a battery are firmly bonded together, the positive and negative electrodes cannot be easily separated, making it difficult to replace the electrodes if any electrode layers are defective at the beginning, and lowering the production yield.In addition, the positive and negative electrodes cannot be easily separated when recycling the battery after it has been used up, making efficient resource recovery difficult.

[0020] To address this issue, the battery described in Patent Document 2 has a thermoplastic resin disposed on the surface of the solid electrolyte layer, so that the positive and negative electrodes can be separated by heating to a temperature equal to or higher than the melting point of the thermoplastic resin during recycling. However, there is a concern that disposing the thermoplastic resin, which is an insulator, on the surface of the solid electrolyte layer may directly lead to a decrease in battery characteristics.

[0021] In view of the above problems, the present disclosure provides a battery or the like that allows easy separation of positive and negative electrodes and also has excellent battery characteristics.

[0022] (Summary of the Disclosure) As an outline of the present disclosure, examples of a battery, a battery separation method, and a battery manufacturing method according to the present disclosure are described below.

[0023] A battery according to a first aspect of the present disclosure has a structure in which a positive electrode current collector layer, a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, and the peel strength between the positive electrode layer and the solid electrolyte layer is 1.8 N / cm or less, and the AC resistance of the battery at 1 Hz at 25°C when the SOC (State Of Charge) is 50% is 100 Ω cm 2 The following is the result.

[0024] This allows the battery characteristics to be improved while the battery can be easily separated between the positive electrode layer and the solid electrolyte layer, thereby realizing a battery with excellent battery characteristics in addition to allowing the positive and negative electrodes to be easily separated.

[0025] Furthermore, for example, the battery according to the second aspect of the present disclosure may be the battery according to the first aspect, in which the porosity of the solid electrolyte layer is 7% or less.

[0026] This makes it possible to suppress the growth of dendrites by the dense solid electrolyte layer.

[0027] Furthermore, for example, a battery according to a third aspect of the present disclosure may be the battery according to the first or second aspect, in which the porosity of the positive electrode layer is 12% or less.

[0028] This allows the charging capacity of the battery to be increased.

[0029] Furthermore, for example, a battery according to a fourth aspect of the present disclosure may be the battery according to the first or second aspect, in which the porosity of the positive electrode layer is 9% or less.

[0030] This allows the charging capacity of the battery to be further increased.

[0031] Furthermore, for example, a battery according to a fifth aspect of the present disclosure is the battery according to any one of the first to fourth aspects, wherein the solid electrolyte layer includes an argyrodite-type sulfide-based solid electrolyte as the solid electrolyte.

[0032] As a result, the argyrodite-type sulfide-based solid electrolyte has high ionic conductivity and is stable over a wide temperature range, which makes it possible to improve the battery characteristics and expand the temperature range over which the battery can be used.

[0033] A battery separation method according to a sixth aspect of the present disclosure is the battery separation method according to any one of the first to fifth aspects, in which the battery is separated between the positive electrode layer and the solid electrolyte layer.

[0034] This allows the positive and negative electrodes of the battery having the above-mentioned excellent battery characteristics to be easily separated.

[0035] A battery according to a seventh aspect of the present disclosure is a battery having a structure in which a positive electrode current collector layer, a positive electrode layer, two or more solid electrolyte layers, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, wherein at least one of a peel strength between adjacent solid electrolyte layers of the two or more solid electrolyte layers and a peel strength between the positive electrode layer and a solid electrolyte layer adjacent to the positive electrode layer of the two or more solid electrolyte layers is 1.8 N / cm or less, and an AC resistance of the battery at 25°C at 1 Hz when SOC is 50% is 100 Ω cm 2 The following is the result.

[0036] This makes it possible to easily separate the battery between the positive electrode layer and the solid electrolyte layer adjacent to the positive electrode layer, or between adjacent solid electrolyte layers, while improving the battery characteristics. Therefore, in addition to being able to easily separate the positive and negative electrodes, a battery with excellent battery characteristics can be realized.

[0037] Furthermore, for example, in a battery according to an eighth aspect of the present disclosure, in the battery according to the seventh aspect, the porosity of the solid electrolyte layer adjacent to the negative electrode layer among the two or more solid electrolyte layers may be 7% or less.

[0038] This makes it possible to suppress the growth of dendrites by the dense solid electrolyte layer.

[0039] Furthermore, for example, the battery according to a ninth aspect of the present disclosure may be the battery according to the seventh or eighth aspect, in which the porosity of the positive electrode layer is 12% or less.

[0040] This allows the charging capacity of the battery to be increased.

[0041] Furthermore, for example, the battery according to a tenth aspect of the present disclosure may be the battery according to the seventh or eighth aspect, in which the porosity of the positive electrode layer is 9% or less.

[0042] This allows the charging capacity of the battery to be further increased.

[0043] Furthermore, for example, a battery according to an eleventh aspect of the present disclosure is the battery according to any one of the seventh to tenth aspects, wherein the solid electrolyte layer includes an argyrodite-type sulfide-based solid electrolyte as the solid electrolyte.

[0044] As a result, the argyrodite-type sulfide-based solid electrolyte has high ionic conductivity, which can improve the characteristics of the battery.

[0045] A battery separation method according to a twelfth aspect of the present disclosure is a battery separation method according to any one of the seventh to eleventh aspects, in which the battery is separated between the positive electrode layer and a solid electrolyte layer adjacent to the positive electrode layer among the two or more solid electrolyte layers.

[0046] This allows the positive and negative electrodes of the battery having the above-mentioned excellent battery characteristics to be easily separated.

[0047] A method for producing a battery according to a thirteenth aspect of the present disclosure is a method for producing a battery having a structure in which a positive electrode current collector layer, a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, the method comprising adjusting a peel strength between the positive electrode layer and the solid electrolyte layer to 1.8 N / cm or less, and adjusting the AC resistance of the battery at 1 Hz at 25° C. when the SOC is 50% to 100 Ω cm 2 and adjusting so that:

[0048] This allows the positive and negative electrodes to be easily separated, and also allows the production of the above-mentioned battery having excellent battery characteristics.

[0049] A method for producing a battery according to a fourteenth aspect of the present disclosure is a method for producing a battery having a structure in which a positive electrode current collector layer, a positive electrode layer, two or more solid electrolyte layers, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, the method comprising adjusting at least one of a peel strength between adjacent solid electrolyte layers of the two or more solid electrolyte layers and a peel strength between the positive electrode layer and a solid electrolyte layer adjacent to the positive electrode layer of the two or more solid electrolyte layers to 1.8 N / cm or less, and adjusting the AC resistance at 1 Hz of the battery at 25° C. when SOC is 50% to 100 Ω cm 2 and adjusting so that:

[0050] This allows the positive and negative electrodes to be easily separated, and also allows the production of the above-mentioned battery having excellent battery characteristics.

[0051] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the drawings. Note that the embodiments described below are all comprehensive or specific examples. The numerical values, shapes, materials, components, arrangement and connection forms of the components, steps, and processes shown in the following embodiments are merely examples and are not intended to limit the present disclosure. In addition, among the components in the following embodiments, components that are not described in the independent claims will be described as optional components.

[0052] Furthermore, in this specification, terms indicating the relationship between elements, such as parallel and perpendicular, terms indicating the shape of an element, such as rectangle, and numerical ranges are not expressions that only express a strict meaning, but are expressions that also include substantially equivalent ranges.

[0053] In addition, each figure is a schematic diagram and is not necessarily illustrated precisely. Therefore, for example, the scales in each figure do not necessarily match. In addition, in each figure, substantially the same configurations are given the same reference numerals, and duplicated explanations are omitted or simplified.

[0054] In this specification, a cross-sectional view is a view showing a cross section of a laminate such as a battery cut along a stacking direction at the center thereof, and the stacking direction corresponds to the thickness direction of each layer of the battery and the direction perpendicular to the main surface of each layer of the battery.

[0055] (Embodiment 1) [1. Configuration] First, the configuration of the battery according to the present embodiment will be described.

[0056] [1-1.Battery] First, an overview of the battery according to the present embodiment will be described.

[0057] FIG. 1 is a schematic cross-sectional view showing an example of a battery according to an embodiment of the present invention.

[0058] As shown in FIG. 1, the battery 10 includes a positive electrode layer 11 including a positive electrode active material, a negative electrode layer 12 including a negative electrode active material and disposed opposite the positive electrode layer 11, a solid electrolyte layer 13 disposed between the positive electrode layer 11 and the negative electrode layer 12, a positive electrode current collector layer 14 that collects current from the positive electrode layer 11, and a negative electrode current collector layer 15 that collects current from the negative electrode layer 12. The battery 10 has a structure in which the positive electrode current collector layer 14, the positive electrode layer 11, the solid electrolyte layer 13, the negative electrode layer 12, and the negative electrode current collector layer 15 are laminated in this order. The positive electrode layer 11 and the positive electrode current collector layer 14 may be collectively referred to as a positive electrode, and the negative electrode layer 12 and the negative electrode current collector layer 15 may be collectively referred to as a negative electrode.

[0059] The battery 10 is, for example, an all-solid-state battery in which the positive electrode layer 11, the negative electrode layer 12, and the solid electrolyte layer 13 are all solid. The battery 10 is not particularly limited as long as it includes the positive electrode layer 11, the negative electrode layer 12, and the solid electrolyte layer 13. The shape of the battery 10 is, for example, a coin type, a pouch type, a cylindrical type, a square type, or the like. The positive electrode layer 11, the negative electrode layer 12, the solid electrolyte layer 13, the positive electrode collector layer 14, and the negative electrode collector layer 15 may have the same planar shape and area as each other, and at least one of these layers may have a different planar shape and area from the other layers.

[0060] The battery 10 according to the present embodiment can be applied to various applications. There is no particular limitation on the application of the battery 10. For example, when the battery 10 is mounted in an electronic device, the electronic device may be a notebook computer, a pen-input computer, a mobile computer, an electronic book player, a mobile phone, a cordless phone handset, a pager, a handheld terminal, a mobile fax machine, a mobile copy machine, a mobile printer, a headphone stereo, a video movie machine, a liquid crystal television, a handheld cleaner, a portable CD, a mini disc, an electric shaver, a transceiver, an electronic organizer, a calculator, a memory card, a mobile tape recorder, a radio, a backup power source, and the like. Other consumer applications of the battery 10 include automobiles, electric vehicles, motors, lighting equipment, toys, game equipment, road conditioners, clocks, strobes, cameras, medical equipment (pacemakers, hearing aids, shoulder massagers, and the like), and the like. Furthermore, the battery 10 can be used for space applications. The battery 10 can also be combined with a solar cell.

[0061] Each component of the battery 10 will be described below.

[0062] [1-2.Solid electrolyte layer] First, a description will be given of the solid electrolyte layer 13. In this embodiment, one solid electrolyte layer 13 is disposed between the positive electrode layer 11 and the negative electrode layer 12. The solid electrolyte layer 13 is in contact with both the positive electrode layer 11 and the negative electrode layer 12.

[0063] The solid electrolyte layer 13 contains a solid electrolyte as a main component. The solid electrolyte may be, for example, Li2S-P2S5 (Li7P3S 11 ), Li 10 GeP2S 12 Sulfide-based solid electrolytes such as Li6PS5Cl and Li6PS5I, and Li 1.4 Al 0.4 Ti 1.6 (PO4)3, Li7La3Zr2O 12 and Li 1.5 Al 0.5 Ge 1.5Examples of the inorganic solid electrolyte include oxide-based solid electrolytes such as (PO4)3. Two or more of these may be used in the solid electrolyte layer 13. Among these, from the viewpoint of ion conductivity, the solid electrolyte layer 13 may contain a sulfide-based solid electrolyte.

[0064] The solid electrolyte layer 13 may contain an argyrodite-type sulfide-based solid electrolyte as the solid electrolyte. The argyrodite-type sulfide-based solid electrolyte is a type of sulfide-based solid electrolyte, and is a sulfide-based solid electrolyte having an argyrodite-type crystal structure. The argyrodite-type sulfide-based solid electrolyte has high lithium ion conductivity and is stable over a wide temperature range, so that the use of the argyrodite-type sulfide-based solid electrolyte can improve the characteristics of the battery 10 and expand the operating temperature range of the battery 10. The argyrodite-type sulfide-based solid electrolyte is relatively hard, so that it is easy to adjust the peel strength, which will be described later.

[0065] The solid electrolyte layer 13 may also contain a binder as a constituent material. The solid electrolyte layer 13 contains a binder, which improves the strength of the solid electrolyte layer. The binder is not particularly limited as long as it is chemically and electrically stable, and examples of the binder include organic binders such as fluorine-based binders such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE), rubber-based binders such as styrene butadiene rubber (SBR), olefin-based binders such as polypropylene (PP) and polyethylene (PE), and cellulose-based binders such as carboxymethyl cellulose (CMC). The solid electrolyte layer 13 may further contain other components in addition to the solid electrolyte and the binder. The content and type of each constituent material in the solid electrolyte layer 13 are set appropriately and are not limited.

[0066] The thickness of the solid electrolyte layer 13 is appropriately set and is not limited. The thickness of the solid electrolyte layer 13 is, for example, 0.01 μm or more and 1 mm or less, or may be 0.1 μm or more and 100 μm or less, or may be 1 μm or more and 25 μm or less.

[0067] Here, by reducing the porosity of the solid electrolyte layer 13 disposed adjacent to the negative electrode layer 12, even if some of the lithium ions absorbed in the negative electrode active material contained in the negative electrode layer 12 capture electrons and precipitate as metallic lithium, the dense solid electrolyte layer 13 makes it easier to suppress the growth of dendrites.

[0068] The porosity of the solid electrolyte layer 13 is, for example, 7% or less. When the porosity of the solid electrolyte layer 13 is 7% or less, when some of the lithium ions absorbed in the negative electrode active material contained in the negative electrode layer 12 take up electrons and precipitate as metallic lithium, dendrites are less likely to grow in the voids of the solid electrolyte layer 13, and the occurrence of an internal short circuit can be suppressed. Therefore, for example, rapid charging is possible. The porosity of each layer is the ratio of the volume occupied by the voids in the layer to the apparent volume of the layer. The apparent volume is calculated from the area and thickness of the layer, the volume occupied by the constituent material of the layer is calculated from the mass of the layer and the true density of the constituent material of the layer, the difference between the apparent volume and the volume occupied by the constituent material is taken as the volume occupied by the voids, and the volume occupied by the voids is divided by the apparent volume to calculate the porosity.

[0069] [1-3. Positive electrode layer] Next, a description will be given of the positive electrode layer 11. The positive electrode layer 11 is disposed between the positive electrode current collector layer 14 and the solid electrolyte layer 13. The positive electrode layer 11 contains, as main components, a positive electrode active material and a solid electrolyte.

[0070] Examples of the positive electrode active material include LiCoO2, LiMnO2, LiNiO2, ternary lithium metal composite oxides of Ni, Co, and Mn, ternary lithium metal composite oxides of Ni, Co, and Al, and LiFePO4. The positive electrode layer 11 may contain two or more of these materials.

[0071] As the solid electrolyte, for example, the solid electrolytes exemplified in the above [1-2. Solid electrolyte layer] can be used. For example, the positive electrode layer 11 may contain an argyrodite-type sulfide-based solid electrolyte as the solid electrolyte.

[0072] When a sulfide-based solid electrolyte is used as the solid electrolyte, the surface of the positive electrode active material may be coated with LiNbO3 in order to suppress the reaction of the positive electrode active material.

[0073] The positive electrode layer 11 may contain a binder as a constituent material. The positive electrode layer 11 containing a binder improves the strength of the positive electrode layer 11. As the binder, for example, the binders exemplified in [1-2. Solid electrolyte layer] above can be used.

[0074] The positive electrode layer 11 may also contain a conductive material as a constituent material. When the positive electrode layer 11 contains a conductive material, the electronic conductivity of the positive electrode layer 11 is improved. Examples of the conductive material include carbon materials such as carbon nanofiber, acetylene black, and Ketjen Black (registered trademark), and metal materials such as nickel, aluminum, and stainless steel.

[0075] Moreover, the positive electrode layer 11 may further contain other components as constituent materials other than the positive electrode active material, the solid electrolyte, the binder, and the conductive material.

[0076] There are no particular limitations on the content of each constituent material in the positive electrode layer 11 and the shape of the positive electrode layer 11. The thickness of the positive electrode layer 11 is, for example, 0.1 μm to 30 mm, or may be 1 μm to 1 mm, or may be 2 μm to 250 μm.

[0077] The content of the positive electrode active material in the positive electrode layer 11 is, for example, 50% by mass or more and 99% by mass or less, and % or more and 98% or less by mass, or may be 90% or more and 97% or less by mass.

[0078] From the viewpoint of improving the energy density and battery characteristics, the porosity of the positive electrode layer 11 is, for example, 12% or less, and may be 9% or less.

[0079] [1-4. Negative electrode layer] Next, a description will be given of the negative electrode layer 12. The negative electrode layer 12 is disposed between the negative electrode current collector layer 15 and the solid electrolyte layer 13. The negative electrode layer 12 contains, as main components, a negative electrode active material and a solid electrolyte.

[0080] Examples of the negative electrode active material include graphite, hard carbon, lithium titanate, titanium oxide, silicon, silicon oxide, etc. The negative electrode layer 12 may contain two or more of these materials.

[0081] As the solid electrolyte, for example, the solid electrolytes exemplified in [1-2. Solid electrolyte layer] above can be used.

[0082] The negative electrode layer 12 may contain a binder as a constituent material. The strength of the negative electrode layer 12 is improved by the negative electrode layer 12 containing a binder. As the binder, for example, the binders exemplified in [1-2. Solid electrolyte layer] above can be used.

[0083] Furthermore, the negative electrode layer 12 may further contain other components as constituent materials in addition to the negative electrode active material, the solid electrolyte, and the binder.

[0084] There are no particular limitations on the content of each constituent material in the negative electrode layer 12 and the shape of the negative electrode layer 12. The thickness of the negative electrode layer 12 is, for example, 0.1 μm to 30 mm, or may be 1 μm to 1 mm, or may be 2 μm to 250 μm.

[0085] The content of the negative electrode active material in the negative electrode layer 12 is, for example, 50% by mass or more and 99% by mass or less, alternatively 70% by mass or more and 98% by mass or less, or 90% by mass or more and 97% by mass or less.

[0086] [1-5. Current collector layer] Next, the positive electrode current collector layer 14 and the negative electrode current collector layer 15 will be described. The positive electrode layer 11 is laminated on one main surface of the positive electrode current collector layer 14. The positive electrode current collector layer 14 and the positive electrode layer 11 are in contact with each other. The negative electrode layer 12 is laminated on one main surface of the negative electrode current collector layer 15. The negative electrode current collector layer 15 and the negative electrode layer 12 are in contact with each other.

[0087] The materials constituting the positive electrode current collector layer 14 and the negative electrode current collector layer 15 are preferably those that do not react with the solid electrolyte or with charging and discharging at the operating potential, and have low electrical resistivity. The positive electrode current collector layer 14 and the negative electrode current collector layer 15 are, for example, made of metal foil. Examples of materials used for the positive electrode current collector layer 14 and the negative electrode current collector layer 15 include aluminum, stainless steel (SUS, austenitic, martensite, ferritic, austenitic-ferritic (two-phase)), nickel, and copper. The positive electrode current collector layer 14 and the negative electrode current collector layer 15 may contain two or more of these materials.

[0088] Furthermore, when the positive electrode layer 11 and the negative electrode layer 12 contain a sulfide-based solid electrolyte as the solid electrolyte, depending on the material of the current collector layer used, the current collector layer may react with the sulfide-based solid electrolyte, which may increase the internal resistance of the battery 10. In such a case, it is preferable to use a material that has low reactivity with the sulfide-based solid electrolyte as the material for the positive electrode current collector layer 14 and the negative electrode current collector layer 15. For example, stainless steel or nickel may be used as the material for the negative electrode current collector layer 15. Also, for example, aluminum may be used as the material for the positive electrode current collector layer 14.

[0089] [1-6. Other configurations] The battery 10 may further include other components in addition to the layers described above. As the other components, any typical components used in batteries can be applied without any particular limitations.

[0090] The battery 10 may include, for example, a positive electrode terminal connected to the positive electrode collector layer 14 and a negative electrode terminal connected to the negative electrode collector layer 15. Examples of materials constituting the positive electrode terminal and the negative electrode terminal include aluminum, copper, stainless steel, and nickel. The positive electrode terminal and the negative electrode terminal may contain two or more of these materials. In addition, a sealant film using a thermoplastic resin such as polypropylene may be disposed on the positive electrode terminal and the negative electrode terminal at a location where the terminal comes into contact with an exterior body described later. This makes it possible to strengthen the sealing by thermocompression bonding.

[0091] The battery 10 may also include, for example, an exterior body that collectively covers each layer of the battery 10. For example, a metal resin composite film or the like is used for the exterior body. In order to suppress deterioration of the solid electrolyte in the battery 10 due to reaction with moisture contained in the atmospheric atmosphere, the exterior body has, for example, gas barrier properties. The exterior body is formed, for example, by vacuum sealing. The vacuum sealing can reduce the interface resistance of each layer. The battery 10 may also include, for example, a restraining member that sandwiches the battery 10 in the thickness direction. The type of the restraining member is not particularly limited, and a general restraining member such as a member that sandwiches the battery 10 between metal plates can be used.

[0092] [2. Battery peel strength and AC resistance] Next, the peel strength and AC resistance of the battery 10 according to the present embodiment will be described.

[0093] In the battery 10, the peel strength between the positive electrode layer 11 and the solid electrolyte layer 13 is 1.8 N / cm or less. In addition, for example, in the battery 10, the peel strength between the positive electrode layer 11 and the solid electrolyte layer 13 is the lowest among the peel strengths between the layers. With such a peel strength, the positive electrode layer 11 containing the positive electrode active material and the negative electrode layer 12 containing the negative electrode active material can be easily separated, and the battery 10 can be easily separated without the positive electrode active material and the negative electrode active material being mixed. In addition, when the positive electrode collector layer 14 and the negative electrode collector layer 15 are made of different materials, the positive electrode collector layer 14 and the negative electrode collector layer 15 can be taken out separately without being mixed. This makes it possible to replace the electrode when there is an initial defective electrode layer, and improves the yield during production. In addition, the positive and negative electrodes can be easily separated during recycling after the battery 10 has been used up in the future, enabling efficient resource recovery. In addition, from the viewpoint of making it easier to separate the positive and negative electrodes, the peel strength between the positive electrode layer 11 and the solid electrolyte layer 13 may be 1.0 N / cm or less, 0.5 N / cm or less, or 0.1 N / cm or less. The peel strength between each layer is measured by the following method. First, when the battery 10 includes a restraining member and an exterior body, the restraining member and the exterior body are removed from the battery 10 to prepare a test sample. When the battery 10 does not include a restraining member and an exterior body, the battery 10 as is is prepared as a test sample. Next, the outermost surface of the positive electrode collector layer 14 of the sample is attached to the sample stage of the tester via double-sided tape. Next, a polyimide tape of a predetermined width (specifically, 2.0 cm) is attached to the outermost surface of the negative electrode collector layer 15 so as to cover at least the area facing the positive electrode layer 11. Then, a cellophane film is attached to one end of the polyimide tape, and the cellophane film is attached to the clip of the force gauge. Finally, the force gauge is swept at an angle of 180° to the sample at a speed of 10 cm / min. In other words, a so-called 180° peel test is performed. The peel load at this time is divided by the peel surface width to calculate the peel strength. In addition, it is visually confirmed which layers have peeled off during the 180° peel test, and the peel strength between which layers is determined.

[0094] In addition, the 1 Hz AC resistance of battery 10 at 25°C with an SOC of 50% is 100 Ω cm 2 This improves the battery characteristics such as the coulombic efficiency during rapid charging. In order to further improve the battery characteristics, the AC resistance of the battery 10 at 1 Hz at 25°C when the SOC is 50% is set to 50 Ω cm 2 or less. The AC resistance of the battery 10 is measured by using an AC resistance meter to measure the AC resistance between the positive electrode collector layer 14 or the positive electrode terminal connected to the positive electrode collector layer 14 and the negative electrode terminal connected to the negative electrode collector layer 15 or the negative electrode collector layer 15. Specifically, the battery 10 in a fully discharged state is first charged by CCCV (Constant Current Constant Voltage) at 25°C and a current of 0.1C, and the SOC is adjusted to 50%. Then, the AC resistance at 1Hz between the positive electrode terminal connected to the positive electrode collector layer 14 or the positive electrode collector layer 14 and the negative electrode terminal connected to the negative electrode collector layer 15 or the negative electrode collector layer 15 of the battery 10 at 25°C is measured by using an AC resistance meter. Note that 1C is a current that charges the entire capacity of the battery 10 in 1 hour. In other words, 0.1C is a current that charges the entire capacity in 10 hours. In addition, the SOC is the ratio of the amount of electricity charged in the battery 10 to the amount of electricity charged when the battery 10 is charged from a completely discharged state to a fully charged state using CCCV (Constant Current Constant Voltage) charging at 25°C and a current of 0.1C, assuming that this is 100%.

[0095] In addition, when the battery 10 includes a restraining member, the AC resistance is measured by the above method without changing the restraining pressure caused by the restraining member. In other words, the AC resistance is measured by the above method in a state in which the restraining pressure when the battery 10 is used is applied to the battery 10.

[0096] In this way, when the battery 10 has the above-mentioned peel strength and AC resistance, the positive and negative electrodes can be easily separated and the battery characteristics can be improved.

[0097] [3. Battery manufacturing method] Next, a method for manufacturing the battery 10 according to the embodiment will be described.

[0098] 2 is a flowchart showing an example of a method for manufacturing the battery 10 according to the embodiment. Note that the manufacturing method described below is just an example, and the manufacturing method for the battery 10 according to the embodiment is not limited to the following example.

[0099] In the manufacturing method of the battery 10, as shown in FIG. 2, first, the positive electrode layer 11 is formed (step S11). For example, a metal foil constituting the positive electrode collector layer 14 is prepared, and a composition such as a slurry containing the constituent material of the positive electrode layer 11 is applied onto the surface of the positive electrode collector layer 14, and then dried to form the positive electrode layer 11. This also forms a positive electrode side laminate in which the positive electrode layer 11 is laminated on the positive electrode collector layer 14. FIG. 3 is a schematic cross-sectional view showing an example of the positive electrode side laminate according to the present embodiment. As shown in FIG. 3, the positive electrode side laminate 30 has a structure in which the positive electrode layer 11 is laminated on one main surface of the positive electrode collector layer 14.

[0100] Examples of the coating method for forming the positive electrode layer 11 include a doctor blade method, a die coater, a comma coater, and the like, and a continuous manufacturing method such as screen printing to form a printed layer. In addition, a roll-to-roll method may be used for coating the constituent material of the positive electrode layer 11.

[0101] In addition, in order to increase the packing density, the formed positive electrode layer 11 may be pressurized. The method of pressurization is not particularly limited, but the positive electrode layer 11 may be pressurized by a method that is performed continuously after the above-mentioned coating, such as a method of pressing using a roll-to-roll method, or by a normal method such as a flat plate press, a roll press, or an isostatic press (ISP). In addition, heating may be performed during pressurization. Various pressurization conditions such as the pressurization pressure, pressurization temperature, and pressurization time are not particularly limited, but the porosity of the positive electrode layer 11 can be adjusted by these pressurization conditions. For example, the porosity can be reduced by increasing the pressurization pressure, increasing the pressurization temperature, or increasing the pressurization time. In this way, in the manufacturing method of the battery 10, the positive electrode layer 11 may be formed with a porosity of 12% or less or 9% or less by adjusting the porosity of the positive electrode layer 11. Pressurization may be performed on the positive electrode layer 11 alone, or may be performed on multiple layers at once after other layers are stacked on the positive electrode layer 11.

[0102] Next, the negative electrode layer 12 is formed (step S12). For example, a metal foil constituting the negative electrode current collector layer 15 is prepared, and a composition such as a slurry containing the constituent material of the negative electrode layer 12 is applied onto the surface of the negative electrode current collector layer 15, and then dried to form the negative electrode layer 12. The application method can be the same as the application method used in forming the positive electrode layer 11 described above.

[0103] In addition, in order to increase the packing density, the formed negative electrode layer 12 may be pressurized. The pressurizing method may be the same as the pressurizing method used in forming the positive electrode layer 11. As in the case of the positive electrode layer 11, the porosity of the negative electrode layer 12 can be adjusted by the pressurizing conditions. Pressurization may be applied to the negative electrode layer 12 alone, or may be applied to multiple layers at once after other layers are laminated on the negative electrode layer 12.

[0104] Next, the solid electrolyte layer 13 is formed (step S13). For example, a substrate such as a metal foil or a resin film is prepared, and a composition such as a slurry containing the constituent materials of the solid electrolyte layer 13 is applied onto the surface of the substrate, followed by drying, to form the solid electrolyte layer 13. The application method can be the same as that used in forming the positive electrode layer 11 described above.

[0105] Next, the solid electrolyte layer 13 formed in step S13 is laminated on the negative electrode layer 12 formed in step S12 to form a negative electrode side laminate (step S14). FIG. 4 is a schematic cross-sectional view showing an example of a negative electrode side laminate according to the present embodiment. As shown in FIG. 4, the negative electrode side laminate 40 has a structure in which the negative electrode current collector layer 15, the negative electrode layer 12, and the solid electrolyte layer 13 are laminated in this order along the thickness direction. For example, the solid electrolyte layer 13 is transferred onto the negative electrode layer 12 by pressure to form the negative electrode side laminate 40. The method of pressing when transferring can be the same as the method of pressing when forming the positive electrode layer 11. The porosity of the solid electrolyte layer 13 can be adjusted by the pressing conditions in this pressing. For example, the porosity can be reduced by increasing the pressing force, increasing the pressing temperature, or increasing the pressing time. The porosity of the solid electrolyte layer 13 can also be adjusted by changing the conditions in the application. In addition, the porosity may be adjusted by pressing the solid electrolyte layer 13 before transferring the solid electrolyte layer 13. In this manner, in the method for manufacturing the battery 10, the porosity of the solid electrolyte layer 13 may be adjusted to form a solid electrolyte layer 13 having a porosity of 7% or less.

[0106] The solid electrolyte layer 13 may be formed directly on the negative electrode layer 12. In this case, steps S13 and S14 are performed simultaneously. For example, the solid electrolyte layer 13 is formed by applying a composition such as a slurry containing the constituent materials of the solid electrolyte layer 13 onto the negative electrode layer 12, and the porosity of the solid electrolyte layer 13 is adjusted by pressurizing the solid electrolyte layer 13 as necessary. In this way, the negative electrode side laminate 40 can also be formed by forming the solid electrolyte layer 13 on the negative electrode layer 12.

[0107] Next, the positive electrode side laminate 30 and the negative electrode side laminate 40 are laminated so that the positive electrode layer 11 and the solid electrolyte layer 13 face each other (step S15). As a result, the positive electrode current collector layer 14 and the negative electrode current collector layer 15 face each other with the positive electrode layer 11, the solid electrolyte layer 13, and the negative electrode layer 12 interposed therebetween, and the positive electrode layer 11 and the solid electrolyte layer 13 come into contact with each other, thereby obtaining a battery 10. When laminating the positive electrode side laminate 30 and the negative electrode side laminate 40, pressure may be applied as necessary. The method of applying pressure may be the same as the method of applying pressure in forming the positive electrode layer 11 described above.

[0108] Furthermore, terminals may be formed on each of the positive electrode current collector layer 14 and the negative electrode current collector layer 15 of the obtained battery 10. The terminals may be formed during the manufacturing process of the battery 10.

[0109] If necessary, an exterior body may be formed on the battery 10. If necessary, a restraining pressure may be applied to the battery 10 in the thickness direction by a restraining member or the like. Fig. 5 is a schematic cross-sectional view showing an example of a battery 10 to which an exterior body 50 and a restraining member 60 are attached.

[0110] For example, an exterior body 50 is formed on the battery 10 obtained in step S15 (step S16). For example, a metal resin composite film is prepared as the exterior body 50, and the obtained battery 10 is vacuum-sealed with the metal resin composite film. As a result, the positive electrode current collector layer 14, the positive electrode layer 11, the solid electrolyte layer 13, the negative electrode layer 12, and the negative electrode current collector layer 15 are collectively covered by the exterior body 50, and atmospheric pressure is applied to the battery 10.

[0111] Next, the battery 10 is restrained by the restraining members 60, thereby applying a restraining pressure in the thickness direction of the battery 10 (step S17). The application of the restraining pressure by the restraining members 60 may be a step instead of the pressurization of each layer described above. For example, a pair of metal plates such as SUS steel plates are prepared as the restraining members 60, and the battery 10 is sandwiched between the pair of metal plates in the thickness direction. The pair of metal plates are fixed to each other by, for example, screws or the like (not shown in FIG. 5), and the restraining pressure on the battery 10 is adjusted depending on the strength of the fixation.

[0112] In addition, in the manufacturing method of the battery 10 according to the embodiment, the peel strength between the positive electrode layer 11 and the solid electrolyte layer 13 is adjusted to be 1.8 N / cm or less. In the above manufacturing method, the peel strength between the positive electrode layer 11 and the solid electrolyte layer 13 can also be said to be the peel strength between the positive electrode side laminate 30 and the negative electrode side laminate 40. For example, in step S15, the peel strength between the positive electrode side laminate 30 and the negative electrode side laminate 40 can be adjusted by not applying pressure when laminating the positive electrode side laminate 30 and the negative electrode side laminate 40, or by adjusting the pressure conditions when applying pressure when laminating the positive electrode side laminate 30 and the negative electrode side laminate 40. When adjusting the peel strength by adjusting the pressure conditions, for example, among the pressures in each of the above steps, the pressure in step S15 is applied under conditions that result in the lowest peel strength (for example, conditions with the lowest pressure). For example, the peel strength can be reduced by reducing the pressure, lowering the pressure temperature, shortening the pressure time, etc.

[0113] In addition, in the manufacturing method of the battery 10 according to the present embodiment, the AC resistance of the battery 10 at 1 Hz at 25° C. and SOC of 50% is 100 Ω·cm 2 The AC resistance is adjusted as follows. For example, the AC resistance can be adjusted by adjusting the pressurizing conditions in each of the above steps. For example, the AC resistance can be lowered by increasing the pressurizing force, increasing the pressurizing temperature, or lengthening the pressurizing time. In addition, the AC resistance can be adjusted by adjusting the restraining pressure applied by the restraining member 60 in step S17. For example, the AC resistance can be lowered by increasing the restraining pressure. Other methods for lowering the AC resistance include increasing the ion conductivity of the solid electrolyte used to form the solid electrolyte layer 13, softening the solid electrolyte used to form the solid electrolyte layer 13, and the like.

[0114] 2 is an example, and the steps may be interchanged or two or more steps may be performed in parallel as long as the battery 10 can be manufactured. For example, step S11 and steps S12 to S14 may be performed in parallel, or at least some of steps S12 to S14 may be performed before step S11.

[0115] Although the above manufacturing method includes a step of forming the negative electrode layer 12 on the negative electrode current collector layer 15 by coating, the negative electrode layer 12 may be formed by forming a laminate of the battery 10 without the negative electrode layer 12 and then precipitating lithium metal as the negative electrode active material on the negative electrode current collector layer 15 by charging. The negative electrode layer 12 may be a layer formed by depositing or forming lithium metal powder, or a lithium metal layer such as a lithium foil or a lithium vapor deposition film.

[0116] The formed battery 10 can also be stacked as a unit cell to form a stacked battery in which a plurality of unit cells are connected in parallel or in series. The battery according to the present embodiment may be a stacked battery in which a plurality of such unit cells are stacked. In the case of a stacked battery, the exterior body 50 and the binding member 60 may, for example, seal and bind a plurality of unit cells collectively. Even in the case of a stacked battery, if there is an electrode layer with an initial defect, only the electrode layer with an initial defect can be replaced without replacing the entire battery, thereby improving the yield during production. In addition, by stacking the positive electrode side laminate 30 and the negative electrode side laminate 40, it is possible to simplify the manufacturing process and increase the manufacturing efficiency.

[0117] [4. How to separate the battery] Next, a method for separating the battery 10 according to the embodiment described above will be described.

[0118] FIG. 6 is a diagram for explaining a method of separating the battery 10. As shown in FIG. 6, when the battery 10 is separated, it is separated between the positive electrode layer 11 and the solid electrolyte layer 13. As a result, the battery 10 is separated into the positive electrode side laminate 30 and the negative electrode side laminate 40. This allows the positive and negative electrodes to be easily separated when replacing the positive and negative electrodes when there is an initial defective electrode layer, and when recycling after use, and allows efficient resource recovery. The method of separating the battery 10 is not particularly limited, but examples include a method of separating the positive electrode side laminate 30 and the negative electrode side laminate 40 by applying a load of 1.8 N / cm or more vertically or horizontally from both sides of the positive electrode side laminate 30 and the negative electrode side laminate 40, and a method of separating the weakest interface between the positive electrode layer 11 and the solid electrolyte layer 13 by inserting a plate-shaped wedge. In this way, the positive electrode side laminate 30 and the negative electrode side laminate 40 can be easily separated, so that they can be separated without adopting an environmentally heavy method such as applying a high voltage, firing, thermal melting, and dissolving in a liquid.

[0119] (Embodiment 2) Next, a description will be given of embodiment 2. The battery 10 according to embodiment 1 has a configuration in which one solid electrolyte layer 13 is provided between the positive electrode layer 11 and the negative electrode layer 12, but in embodiment 2, a configuration in which two solid electrolyte layers are provided between the positive electrode layer 11 and the negative electrode layer 12 will be described. The following description will focus on the differences from embodiment 1, and the description of commonalities will be omitted or simplified.

[0120] [composition] First, the configuration of the battery according to the embodiment will be described. Fig. 7 is a schematic cross-sectional view showing an example of the battery according to the embodiment.

[0121] As shown in FIG. 7 , the battery 20 according to this embodiment differs from the battery 10 according to the first embodiment in that it further includes a solid electrolyte layer 16, that is, it includes two solid electrolyte layers 13, 16 between the positive electrode layer 11 and the negative electrode layer 12.

[0122] Battery 20 has a structure in which a positive electrode collector layer 14, a positive electrode layer 11, two solid electrolyte layers 13 and 16, a negative electrode layer 12, and a negative electrode collector layer 15 are laminated in this order. Battery 20 is, for example, an all-solid-state battery in which the positive electrode layer 11, the negative electrode layer 12, and the solid electrolyte layers 13 and 16 are all made of solids.

[0123] Of the two solid electrolyte layers 13 and 16, the solid electrolyte layer 13 is a solid electrolyte layer adjacent to the anode layer 12, and the solid electrolyte layer 16 is a solid electrolyte layer adjacent to the cathode layer 11. The solid electrolyte layer 13 is disposed between the solid electrolyte layer 16 and the anode layer 12, and is in contact with both the solid electrolyte layer 16 and the anode layer 12. The solid electrolyte layer 16 is disposed between the solid electrolyte layer 13 and the cathode layer 11, and is in contact with both the solid electrolyte layer 13 and the cathode layer 11.

[0124] The solid electrolyte layers 13 and 16 contain a solid electrolyte as a main component. For example, the solid electrolytes exemplified in [1-2. Solid electrolyte layer] above can be used as the solid electrolyte. For example, each of the two solid electrolyte layers 13 and 16 may contain an argyrodite-type sulfide-based solid electrolyte as the solid electrolyte.

[0125] The solid electrolyte layers 13 and 16 may also contain a binder as a constituent material. For example, the binders exemplified in [1-2. Solid electrolyte layer] above may be used as the binder. At least one of the solid electrolyte layers 13 and 16 may further contain other components in addition to the solid electrolyte and the binder.

[0126] The content and type of each constituent material in solid electrolyte layers 13 and 16 are set appropriately and are not limited. In addition, the content and type of each constituent material in solid electrolyte layer 13 and solid electrolyte layer 16 may be the same, at least one of the content and type of each constituent material may be different, or both the content and type of each constituent material may be different.

[0127] The thickness of the solid electrolyte layers 13 and 16 is set appropriately and is not limited. The thickness of the solid electrolyte layers 13 and 16 is, for example, 0.01 μm to 1 mm, may be 0.1 μm to 100 μm, or may be 1 μm to 25 μm. The thickness of the solid electrolyte layers 13 and 16 may be the same or different.

[0128] The ratio of the thickness of solid electrolyte layer 13 to the thickness of solid electrolyte layer 16 is, for example, 1 / 100 or more and 100 / 1 or less, optionally 1 / 50 or more and 50 / 1 or less, optionally 1 / 30 or more and 30 / 1 or less, or optionally 1 / 10 or more and 10 / 1 or less.

[0129] Even when the porosity of the positive electrode layer 11 and the solid electrolyte layer 13 is reduced as described in the first embodiment, the solid electrolyte layer 16 is disposed between the solid electrolyte layer 13 and the positive electrode layer 11 in this manner, thereby making it possible to reduce the interface resistance between the positive electrode layer 11 and the solid electrolyte layer 16. For example, when the porosity of the solid electrolyte layer 16 is higher than the porosity of the solid electrolyte layer 13, even when the positive electrode layer 11 and the solid electrolyte layer 13 have a low porosity, when the solid electrolyte layer 16 is brought into contact with or joined to the positive electrode layer 11 and the solid electrolyte layer 13, the surface of the solid electrolyte layer 16 is plastically deformed due to the high porosity of the solid electrolyte layer 16, and the contact between the solid electrolyte layer 16 and the positive electrode layer 11 and the solid electrolyte layer 13 is improved. Therefore, the interface resistance between the solid electrolyte layer 16 and the positive electrode layer 11 and the solid electrolyte layer 13 is reduced, and a good lithium ion conduction path is formed, which is considered to suppress the local deposition and growth of metallic lithium.

[0130] Furthermore, when the layers of the battery 20 are joined, if the positive electrode layer 11 and the solid electrolyte layer 16 are brought into contact or joined in a state in which the positive electrode layer 11 has a high porosity, the relatively hard positive electrode layer 11 will cause cracks in the solid electrolyte layer 16 when the positive electrode layer 11 is subsequently processed to have a low porosity. In particular, when the positive electrode layer 11, the solid electrolyte layer 13, and the negative electrode layer 12 have different areas and shapes, the cracks will expand from the ends of the layers with smaller areas, complicating the manufacturing process and reducing the yield during production. To address this issue, the high porosity of the solid electrolyte layer 16 makes the solid electrolyte layer 16 relatively soft and suppresses the occurrence of cracks, thereby suppressing the decrease in yield during production.

[0131] The porosity of the solid electrolyte layer 16 is, for example, 16% or more and 40% or less. When the porosity of the solid electrolyte layer 16 is 16% or more, the surface of the solid electrolyte layer 16 is easily plastically deformed, and the interface resistance with the positive electrode layer 11 and the solid electrolyte layer 13 can be reduced. Therefore, it is considered that a good lithium ion conduction path is formed, and local deposition and growth of metallic lithium can be suppressed. In addition, when the porosity of the solid electrolyte layer 16 is 40% or less, the occurrence of problems in manufacturing, such as the solid electrolyte falling off due to too many voids, can be suppressed, and the ion conductivity inside the solid electrolyte layer 16 can be increased, thereby improving the characteristics of the battery 20.

[0132] On the other hand, as described above, by reducing the porosity of the solid electrolyte layer 13 adjacent to the negative electrode layer 12, the dense solid electrolyte layer 13 can suppress the growth of dendrites.

[0133] Thus, the battery 20 has two solid electrolyte layers, the solid electrolyte layer 13 and the solid electrolyte layer 16, which have different roles. This increases the contact area between the high-porosity solid electrolyte layer 16 and the positive electrode layer 11 and the solid electrolyte layer 13 adjacent to the solid electrolyte layer 16, thereby reducing reaction irregularities and interface resistance, and suppressing local deposition and growth of metallic lithium. In addition, the dense solid electrolyte layer 13 can suppress the growth of dendrites. This makes it possible to suppress internal short circuits in the battery 20 and improve the battery characteristics.

[0134] Although the battery 20 includes two solid electrolyte layers, the solid electrolyte layer 13 and the solid electrolyte layer 16, the present invention is not limited to this. The battery 20 may include three or more solid electrolyte layers between the positive electrode layer 11 and the negative electrode layer 12. For example, the battery 20 may include another solid electrolyte layer between the solid electrolyte layer 13 and the solid electrolyte layer 16.

[0135] Furthermore, like the battery 10, the battery 20 may further include other components such as a terminal, an exterior body, and a restraining member.

[0136] [Battery peel strength and AC resistance] Next, the peel strength and AC resistance of the battery 20 according to this embodiment will be described.

[0137] In the battery 20, at least one of the peel strength between the solid electrolyte layer 13 and the solid electrolyte layer 16 adjacent to each other and the peel strength between the positive electrode layer 11 and the solid electrolyte layer 16 is 1.8 N / cm or less. In addition, for example, in the battery 20, among the peel strengths between the layers, the peel strength between the solid electrolyte layer 13 and the solid electrolyte layer 16 adjacent to each other or the peel strength between the positive electrode layer 11 and the solid electrolyte layer 16 is the lowest. With such a peel strength, it is possible to easily separate the positive electrode layer 11 containing the positive electrode active material and the negative electrode layer 12 containing the negative electrode active material, and the battery 20 can be easily separated without the positive electrode active material and the negative electrode active material being mixed. In addition, from the viewpoint of making it easier to separate the battery 20, at least one of the peel strength between the solid electrolyte layer 13 and the solid electrolyte layer 16 adjacent to each other and the peel strength between the positive electrode layer 11 and the solid electrolyte layer 16 may be 1.0 N / cm or less, 0.5 N / cm or less, or 0.1 N / cm or less.

[0138] In addition, the 1 Hz AC resistance of battery 20 at 25°C with an SOC of 50% is 100 Ω cm 2This improves the battery characteristics such as the coulombic efficiency during rapid charging. In order to further improve the battery characteristics, the AC resistance of the battery 20 at 1 Hz at 25°C when the SOC is 50% is set to 50 Ω cm 2 It may be the following.

[0139] In this way, when the battery 20 has the above-mentioned peel strength and AC resistance, the positive and negative electrodes can be easily separated and the battery characteristics can be improved.

[0140] [Battery manufacturing method] Next, a method for manufacturing the battery 20 according to the embodiment will be described.

[0141] Fig. 8 is a flow chart showing an example of a method for manufacturing the battery 20 according to the embodiment. Note that the manufacturing method described below is just an example, and the manufacturing method for the battery 20 according to the embodiment is not limited to the following example. For example, like the manufacturing method for the battery 10, the order of the manufacturing steps shown in Fig. 8 is just an example, and as long as the battery 20 can be manufactured, the steps may be interchanged, or two or more steps may be performed in parallel.

[0142] In the method for producing the battery 20, first, the positive electrode layer 11 is formed (step S21) as shown in Fig. 8. Step S21 is performed in the same manner as step S11 described above.

[0143] Next, the negative electrode layer 12 is formed (step S22). Step S22 is performed in the same manner as step S12 described above.

[0144] Next, the two solid electrolyte layers 13 and 16 are formed (step S23). For example, the solid electrolyte layer 13 and the solid electrolyte layer 16 are separately formed by a method similar to that for the solid electrolyte layer 13 in step S13.

[0145] Next, the solid electrolyte layer 16 formed in step S23 is laminated on the positive electrode layer 11 formed in step S21 to form a positive electrode side laminate (step S24). FIG. 9 is a schematic cross-sectional view showing an example of a positive electrode side laminate according to the present embodiment. As shown in FIG. 9, the positive electrode side laminate 31 has a structure in which the positive electrode current collector layer 14, the positive electrode layer 11, and the solid electrolyte layer 16 are laminated in this order along the thickness direction. For example, the positive electrode side laminate 31 is formed by transferring the solid electrolyte layer 16 onto the positive electrode layer 11 by applying pressure. The same method as the pressurization in forming the positive electrode layer 11 can be used as the method of applying pressure when transferring. The porosity of the solid electrolyte layer 16 can be adjusted by applying pressure under the conditions of this pressure. For example, the porosity can be reduced by increasing the pressure, increasing the pressure temperature, or increasing the pressure time. The porosity of the solid electrolyte layer 16 can also be adjusted by changing the conditions of application. The porosity may also be adjusted by applying pressure to the solid electrolyte layer 16 before the transfer of the solid electrolyte layer 16. In this manner, in the method for manufacturing the battery 20, the porosity of the solid electrolyte layer 16 may be adjusted to form a solid electrolyte layer 16 having a porosity of 16% or more and 40% or less.

[0146] The solid electrolyte layer 16 may be formed directly on the positive electrode layer 11. In this case, part of step S23 and step S24 are performed simultaneously. For example, the solid electrolyte layer 16 is formed by applying a composition such as a slurry containing the constituent materials of the solid electrolyte layer 16 onto the positive electrode layer 11, and the porosity of the solid electrolyte layer 16 is adjusted by pressurizing the solid electrolyte layer 16 as necessary. In this way, the positive electrode side laminate 31 can also be formed by forming the solid electrolyte layer 16 directly on the positive electrode layer 11.

[0147] Next, the solid electrolyte layer 13 formed in step S23 is laminated on the negative electrode layer 12 formed in step S22 to form the negative electrode side laminate 40 (step S25). Step S25 is performed in the same manner as in step S14 described above. As a result, the negative electrode side laminate 40 shown in FIG. 4 is obtained. The pressure applied when the solid electrolyte layer 13 is transferred onto the negative electrode layer 12 by pressure in step S25 is greater than the pressure applied when the solid electrolyte layer 16 is transferred onto the positive electrode layer 11 by pressure in step S24, for example.

[0148] Next, the positive electrode side laminate 31 and the negative electrode side laminate 40 are laminated so that the solid electrolyte layer 16 and the solid electrolyte layer 13 face each other (step S26). As a result, the positive electrode current collector layer 14 and the negative electrode current collector layer 15 face each other with the positive electrode layer 11, the two solid electrolyte layers 13, 16, and the negative electrode layer 12 interposed therebetween, and the solid electrolyte layer 16 and the solid electrolyte layer 13 come into contact with each other, thereby obtaining a battery 20. When laminating the positive electrode side laminate 31 and the negative electrode side laminate 40, pressure may be applied as necessary. The same method of pressure application as that used in forming the above-mentioned positive electrode layer 11 can be used.

[0149] In addition, in manufacturing the battery 20, terminals may be formed in the same manner as in the battery 10.

[0150] In manufacturing the battery 20, similarly to the battery 10, the formation of the exterior body 50 (step S27) and the restraint by the restraining member 60 (step S28) may be performed.

[0151] In manufacturing the battery 20, the negative electrode layer 12 may be formed by depositing lithium metal on the negative electrode current collector layer 15, as in the case of the battery 10. The formed battery 20 may be further stacked as a unit cell to form a stacked battery in which a plurality of unit cells are connected in parallel or in series.

[0152] In addition, in the manufacturing method of the battery 20 according to the present embodiment, at least one of the peel strength between the solid electrolyte layer 16 and the solid electrolyte layer 13 and the peel strength between the positive electrode layer 11 and the solid electrolyte layer 16 is adjusted to be 1.8 N / cm or less. In the above manufacturing method, the lower of the peel strength between the solid electrolyte layer 16 and the solid electrolyte layer 13 and the peel strength between the positive electrode layer 11 and the solid electrolyte layer 16 can be said to be the peel strength between the positive electrode side laminate 31 and the negative electrode side laminate 40. For example, in step S26, the peel strength between the solid electrolyte layer 16 and the solid electrolyte layer 13 can be adjusted by not applying pressure when laminating the positive electrode side laminate 31 and the negative electrode side laminate 40, or by adjusting the pressure conditions for applying pressure when laminating the positive electrode side laminate 31 and the negative electrode side laminate 40. When adjusting the peel strength by adjusting the pressure conditions, for example, among the pressures in the above steps, the pressure in step S26 is applied under conditions that result in the lowest peel strength.

[0153] In addition, in the manufacturing method of the battery 20 according to the present embodiment, the AC resistance of the battery 20 at 1 Hz at 25° C. and SOC of 50% is 100 Ω·cm 2 The AC resistance is adjusted to be as follows. The adjustment of the AC resistance can be performed, for example, by the same method as the adjustment of the AC resistance in the battery 10. In the battery 20, the AC resistance can also be adjusted by adjusting the porosity of the solid electrolyte layer 16. For example, by adjusting the porosity of the solid electrolyte layer 16 to be 16% or more and 40% or less, the AC resistance can be made lower than when the porosity is adjusted to be outside this range.

[0154] The lamination configuration of each layer in the positive electrode side laminate 31 and the negative electrode side laminate 40 is not limited to the above example. FIG. 10 is a schematic cross-sectional view showing an example of the negative electrode side laminate according to the present embodiment. As shown in FIG. 10, the negative electrode side laminate 41 has a structure in which the negative electrode current collector layer 15, the negative electrode layer 12, the solid electrolyte layer 13, and the solid electrolyte layer 16 are laminated in this order along the thickness direction. The negative electrode side laminate 41 is formed by forming the negative electrode side laminate 40 in step S25, and then laminating the solid electrolyte layer 16 formed in step S23 on the solid electrolyte layer 13 of the negative electrode side laminate 40. For example, the negative electrode side laminate 41 is formed by transferring the solid electrolyte layer 16 onto the solid electrolyte layer 13 by pressure. The method of pressure application during transfer can be the same as the method of pressure application in the formation of the positive electrode layer 11 described above. In addition, the porosity of the solid electrolyte layer 16 can be adjusted by the pressure application conditions, etc., as in the above step S24.

[0155] The two solid electrolyte layers 13, 16 may be successively formed directly on the negative electrode layer 12. In this case, step S23 and step S25 are performed simultaneously. If necessary, the solid electrolyte layers 13, 16 may be pressurized after each layer is formed. In this manner, the negative electrode side laminate 41 can also be formed by forming the two solid electrolyte layers 13, 16 directly on the negative electrode layer 12.

[0156] When the negative electrode side laminate 41 is formed in step S25, step S24 is omitted, and the positive electrode side laminate 30 shown in FIG. 3 to be formed in step S21 is used in step S26. That is, in step S26, the positive electrode side laminate 30 and the negative electrode side laminate 41 are laminated so that the positive electrode layer 11 and the solid electrolyte layer 16 face each other. As a result, the positive electrode current collector layer 14 and the negative electrode current collector layer 15 face each other with the positive electrode layer 11, the two solid electrolyte layers 13 and 16, and the negative electrode layer 12 sandwiched therebetween, and the positive electrode layer 11 and the solid electrolyte layer 16 come into contact with each other, thereby obtaining the battery 20. In addition, after laminating the positive electrode side laminate 30 and the negative electrode side laminate 41, pressure may be applied as necessary.

[0157] When the battery 20 is formed by stacking the positive electrode side laminate 30 and the negative electrode side laminate 41, at least one of the peel strength between the solid electrolyte layer 16 and the solid electrolyte layer 13 and the peel strength between the positive electrode layer 11 and the solid electrolyte layer 16 is adjusted to be 1.8 N / cm or less. In this case, the lower of the peel strength between the solid electrolyte layer 16 and the solid electrolyte layer 13 and the peel strength between the positive electrode layer 11 and the solid electrolyte layer 16 can also be said to be the peel strength between the positive electrode side laminate 30 and the negative electrode side laminate 41. The method of adjusting the peel strength is the same as when stacking the positive electrode side laminate 31 and the negative electrode side laminate 40.

[0158] [How to separate the battery] Next, a method for separating the battery 20 according to the above-mentioned embodiment will be described. Fig. 11 is a diagram for explaining the method for separating the battery 20. Fig. 12 is another diagram for explaining the method for separating the battery 20.

[0159] 11, when the battery 20 is separated, the separation is performed between the solid electrolyte layer 13 and the solid electrolyte layer 16 adjacent to each other. As a result, the battery 20 is separated into a positive electrode side laminate 31 and a negative electrode side laminate 40. In this case, for example, the battery 20 manufactured by laminating the positive electrode side laminate 31 and the negative electrode side laminate 40 in the above step S26 is used.

[0160] 12, for example, when the battery 20 is separated, the separation is performed between the positive electrode layer 11 and the solid electrolyte layer 13. As a result, the battery 20 is separated into a positive electrode side laminate 30 and a negative electrode side laminate 41. In this case, for example, the battery 20 manufactured by laminating the positive electrode side laminate 30 and the negative electrode side laminate 41 in the above step S26 is used.

[0161] By separating the battery 20 in this manner, the positive and negative electrodes can be easily separated for replacement when there is an initial defective electrode layer, and for recycling after use, etc., enabling efficient resource recovery. The method for separating the battery 20 is not particularly limited, but the same method as that for separating the battery 10 described above can be used.

[0162] (Example) Next, the results of evaluating the battery according to the present disclosure will be described in examples. The present disclosure is not limited to the examples. Specifically, batteries in the examples and comparative examples were fabricated and the fabricated batteries were evaluated.

[0163] [Evaluation method] First, the methods for evaluating the batteries in each of the Examples and Comparative Examples will be described. The batteries were evaluated by performing a battery characteristic evaluation, a porosity evaluation, and a peeling test.

[0164] <Battery characteristic evaluation> The battery characteristics were evaluated by AC resistance, 6C charge capacity, and 6C coulombic efficiency.

[0165] First, for the batteries in each of the examples and comparative examples, CCCV charge and discharge was carried out at 25° C., in the voltage range of 3.00 V to 4.35 V, and at a current of 0.1 C while both sides of the battery were sandwiched and pressed between binding members.

[0166] Thereafter, the battery was subjected to CCCV charging at a current of 0.1 C, and the SOC was adjusted to 50%, and the 1 Hz AC resistance of the battery was measured at 25° C. by the method described above.

[0167] Finally, the battery was CC-charged at a current of 6C at 60°C in the voltage range of 3.00V to 4.35V, and CCCV-discharged at a current of 0.1C to measure the charge and discharge capacity. The charge capacity during this charge was taken as the 6C charge capacity, and the coulombic efficiency when charging at a current of 6C (6C coulombic efficiency) was calculated by dividing the discharge capacity by the 6C charge capacity x 100 (%). Charging at a current of 6C is a rapid charge that can charge the entire capacity of the battery in 10 minutes. When the 6C coulombic efficiency was 99% or more, no signs of internal short circuit were observed and rapid charging was possible, and the battery was evaluated as "good", and when the 6C coulombic efficiency was less than 99%, signs of internal short circuit were observed and the battery was evaluated as "bad".

[0168] <Porosity evaluation> For the evaluation of the porosity of each layer of the battery, first, a cross-sectional SEM (Scanning Electron Microscope) image was obtained for each battery in each Example and Comparative Example after the above-mentioned characteristic evaluation, and the thickness of each layer was measured from the obtained cross-sectional SEM. Then, the porosity was calculated by the above-mentioned method from the measured layer thickness, layer area, true density of the constituent material of the layer used, mass of the constituent material of the layer used, and content of the constituent material of the layer used.

[0169] <Peel test> In the battery peel test, first, the restraining member and the exterior body were removed from the batteries in each of the examples and comparative examples after the above-mentioned characteristic evaluation to obtain test samples, and the 180° peel test was performed by the above-mentioned method. The peel load at this time was divided by the peel surface width to calculate the peel strength, and it was determined which layer the peel strength was between. In addition, as an evaluation of whether the positive and negative electrodes could be separated, a case in which the positive electrode layer and the negative electrode layer were separated in the peel test was evaluated as "OK", and a case in which the positive electrode layer and the negative electrode layer were not separated was evaluated as "NO".

[0170] The peel strength of the sample that peeled off when the peel load was equal to or less than the lower limit load for detection by the force gauge was recorded as 0 N / cm.

[0171] [Battery construction] The batteries in the examples and comparative examples were fabricated in the following manner.

[0172] <Example 1> First, aluminum foil was used as the positive electrode current collector layer, and a ternary lithium metal composite oxide of Ni, Co, and Mn coated with LiNbO3 (true density: 4.75 g / cm3) was used as the positive electrode active material. 3 ), an argyrodite-type sulfide-based solid electrolyte (true density: 1.89 g / cm3) as a solid electrolyte, and carbon nanofiber (true density: 2.1 g / cm3) as a conductive material. 3 ) and an organic binder (true density: 0.93 g / cm 3) was prepared. Next, a positive electrode active material slurry, which was a mixture of the prepared positive electrode active material, solid electrolyte, conductive material, and binder, was applied onto the positive electrode current collector layer to form a positive electrode layer, and the positive electrode layer was pressurized under pressure conditions adjusted so that the porosity of the positive electrode layer was 9%. In this way, a positive electrode side laminate composed of the positive electrode layer and the positive electrode current collector layer was formed.

[0173] Next, stainless steel foil was used as the negative electrode current collector layer, and graphite (true density: 2.3 g / cm) was used as the negative electrode active material. 3 ), the same argyrodite-type sulfide-based solid electrolyte as above was prepared as the solid electrolyte, and the same organic binder as above was prepared as the binder. Next, the prepared negative electrode active material, solid electrolyte, and binder were mixed to form a negative electrode active material slurry, which was then applied onto the negative electrode current collector layer to form a negative electrode layer.

[0174] Next, a solid electrolyte slurry containing the same argyrodite-type sulfide-based solid electrolyte as above as a solid electrolyte and the same organic binder as above as a binding material was applied onto a stainless steel foil to form a solid electrolyte layer.

[0175] Next, the solid electrolyte layer was transferred onto the formed negative electrode layer under pressure conditions adjusted so that the porosity of the solid electrolyte layer was 4%, and the solid electrolyte layer was laminated onto the negative electrode layer. This resulted in the formation of a negative electrode-side laminate. The stainless steel foil used for coating the solid electrolyte layer was peeled off and removed during the transfer process.

[0176] Next, terminals were connected to the positive electrode current collector layer and the negative electrode current collector layer. Furthermore, the positive electrode side laminate and the negative electrode side laminate were laminated so that the positive electrode layer and the solid electrolyte layer faced each other, and vacuum sealed using a metal resin composite film as an exterior body. Note that no pressure was applied when laminating the positive electrode side laminate and the negative electrode side laminate. Finally, the battery sealed with the exterior body was restrained by sandwiching it from both sides using restraining members made of SUS steel plates, and the battery in Example 1 was obtained. The restraining pressure by the restraining member was determined in advance by changing the restraining pressure and measuring the AC resistance to confirm the relationship between the restraining pressure and the AC resistance, and it was found that the AC resistance was 38 Ω·cm. 2The lamination of the positive electrode side laminate and the negative electrode side laminate, the vacuum sealing, and the restraint by the restraining member were carried out so that the porosity of each layer would not change. The porosity of each layer did not change even after the battery characteristics evaluation.

[0177] <Example 2> When restrained using the restraining member, the AC resistance is 26 Ω cm 2 The battery in Example 2 was produced in the same manner as in Example 1, except that the confining pressure by the confining member was adjusted so that the confining pressure was 100%. Note that the porosity of each layer did not change after laminating the positive electrode side laminate and the negative electrode side laminate, after vacuum sealing, after confinement, and after evaluation of the battery characteristics.

[0178] <Example 3> (i) In forming the positive electrode layer, the positive electrode layer was pressurized under pressure conditions adjusted so that the porosity of the positive electrode layer was 12%; (ii) in laminating the solid electrolyte layer onto the negative electrode layer, the solid electrolyte layer was pressed and transferred under pressure conditions adjusted so that the porosity of the solid electrolyte layer was 7%; (iii) pressure was applied when laminating the positive electrode side laminate and the negative electrode side laminate; and (iv) when restraining using the restraining member, the AC resistance was 20 Ω cm 2 The battery in Example 3 was produced in the same manner as in Example 1, except that the confining pressure by the confining member was adjusted so that the confining pressure was 0.05 to 0.05. Note that the porosity of each layer did not change after laminating the positive electrode side laminate and the negative electrode side laminate, after vacuum sealing, after confinement, and after evaluation of the battery characteristics.

[0179] <Example 4> (i) a separate solid electrolyte layer was formed in the same manner as the aforementioned solid electrolyte layer, and the separate solid electrolyte layer was transferred onto the positive electrode layer under pressure under pressure conditions adjusted so that the porosity of the separate solid electrolyte layer was 18%; and (ii) when restrained using the restraining member, the AC resistance was 34 Ω cm 2 The battery in Example 4 was produced by the method of Example 1, except that the confining pressure by the confining member was adjusted so that the confining pressure was 100%. Note that the porosity of each layer did not change after laminating the positive electrode side laminate and the negative electrode side laminate, after vacuum sealing, after confinement, and after evaluation of the battery characteristics.

[0180] <Example 5> When restrained using the restraining member, the AC resistance is 28 Ω cm 2 The battery in Example 5 was produced in the same manner as in Example 4, except that the confining pressure by the confining member was adjusted so that the porosity of each layer did not change after laminating the positive electrode side laminate and the negative electrode side laminate, after vacuum sealing, after confinement, and after evaluation of the battery characteristics.

[0181] <Example 6> (i) a positive electrode-side laminate was used, which was formed by forming another solid electrolyte layer in the same manner as the above-mentioned solid electrolyte layer, and pressing and transferring this other solid electrolyte layer onto the positive electrode layer under pressure conditions adjusted so that the porosity of this other solid electrolyte layer was 18%; (ii) a pressure lower than that in Example 3 was applied when laminating the positive electrode-side laminate and the negative electrode-side laminate; and (iii) when restraining using the restraining member, the AC resistance was 27 Ω cm. 2 The battery in Example 6 was produced in the same manner as in Example 3, except that the confining pressure by the confining member was adjusted so that the porosity of each layer did not change after laminating the positive electrode side laminate and the negative electrode side laminate, after vacuum sealing, after confinement, and after evaluation of the battery characteristics.

[0182] <Comparative Example 1> A battery in Comparative Example 1 was produced in the same manner as in Example 1, except that the restraining pressure was adjusted so as not to be applied when the restraining member was used. The AC resistance was 3720 Ω cm 2 The porosity of each layer did not change after lamination of the positive electrode side laminate and the negative electrode side laminate, after vacuum sealing, after restraint, and after evaluation of the battery characteristics.

[0183] <Comparative Example 2> (i) A pressure greater than that in Example 3 was applied when laminating the positive electrode side laminate and the negative electrode side laminate, and (ii) when restraining with the restraining member, the AC resistance was 23 Ω cm 2A battery in Comparative Example 2 was produced in the same manner as in Example 3, except that the confining pressure by the confining member was adjusted so that the porosity of each layer did not change after laminating the positive electrode side laminate and the negative electrode side laminate, after vacuum sealing, after confinement, and after evaluation of the battery characteristics.

[0184] <Comparative Example 3> A battery in Comparative Example 3 was produced in the same manner as in Example 4, except that the restraining pressure was adjusted so as not to be applied when the battery was restrained using the restraining member. The AC resistance was 392 Ω cm 2 The porosity of each layer did not change after lamination of the positive electrode side laminate and the negative electrode side laminate, after vacuum sealing, after restraint, and after evaluation of the battery characteristics.

[0185] <Comparative Example 4> (i) A pressure greater than that in Example 6 was applied when laminating the positive electrode side laminate and the negative electrode side laminate, and (ii) when restraining with the restraining member, the AC resistance was 20 Ω cm 2 A battery in Comparative Example 4 was produced in the same manner as in Example 6, except that the confining pressure by the confining member was adjusted so that the porosity of each layer did not change after laminating the positive electrode side laminate and the negative electrode side laminate, after vacuum sealing, after confinement, and after evaluation of the battery characteristics.

[0186] <Comparative Example 5> (i) In forming the positive electrode layer, the positive electrode layer was pressurized under pressure conditions adjusted so that the porosity of the positive electrode layer was 18%; (ii) in laminating the solid electrolyte layer onto the negative electrode layer, the solid electrolyte layer was pressed and transferred under pressure conditions adjusted so that the porosity of the solid electrolyte layer was 20%; and (iii) when restraining using the restraining member, the AC resistance was 120 Ω cm 2 A battery in Comparative Example 5 was produced in the same manner as in Example 1, except that the confining pressure by the confining member was adjusted so that the porosity of each layer did not change after laminating the positive electrode side laminate and the negative electrode side laminate, after vacuum sealing, after confinement, and after evaluation of the battery characteristics.

[0187] [Battery evaluation results] The evaluation results of the batteries in Examples 1 to 6 and Comparative Examples 1 to 5 are shown in Table 1. In Table 1, the solid electrolyte layer is referred to as an "SE layer." The "6C charge capacity" shown in Table 1 is the charge capacity per unit mass obtained by dividing the 6C charge capacity measured by the above method by the mass of the positive electrode active material contained in the battery. In addition, "-" in the evaluation of the 6C charge capacity in Table 1 indicates that the battery was not evaluated because a sign of an internal short circuit was observed in the 6C coulombic efficiency evaluation.

[0188] [Table 1]

[0189] As shown in Table 1, in the batteries of Examples 1 to 6 and Comparative Examples 1, 3, and 5, peeling occurred between the positive electrode side laminate and the negative electrode side laminate in the peel test, and the positive and negative electrodes could be separated. Furthermore, in the batteries of Examples 1 to 6 and Comparative Examples 2 and 4, rapid charging such as charging at a current of 6 C was possible, and no signs of internal short circuit were observed. Therefore, whether the solid electrolyte layer is one layer or two layers as in the batteries of Examples 1 to 6, the peel strength between the positive electrode side laminate and the negative electrode side laminate should be 1.8 N / cm or less, and the AC resistance should be 100 Ω cm 2 By doing so, a battery with excellent battery characteristics can be realized, and the positive electrode active material and the negative electrode active material do not mix, and the positive electrode current collector layer and the negative electrode current collector layer do not mix, making it possible to easily separate the positive and negative electrodes.

[0190] For example, comparing Example 1 with Comparative Example 1, and Example 4 with Comparative Example 3, the porosity of the solid electrolyte layer adjacent to the negative electrode layer and the porosity of the positive electrode layer are the same, and peeling occurs between the positive electrode side laminate and the negative electrode side laminate in the peeling test. However, by fabricating the battery to reduce the AC resistance, a battery with excellent battery characteristics that allows rapid charging, such as charging at a current of 6 C, is realized.

[0191] In addition, for example, when Example 3 is compared with Comparative Example 2, and Example 6 is compared with Comparative Example 4, the porosity of the solid electrolyte layer adjacent to the negative electrode layer and the porosity of the positive electrode layer are the same, and the AC resistance is 100 Ω cm 2 The same applies to the points below, but by manufacturing a battery so that the peel strength between the positive electrode side laminate and the negative electrode side laminate is 1.8 N / cm or less, a battery in which the positive and negative electrodes can be easily separated can be realized.

[0192] For example, comparing Example 1 with Example 2, and Example 4 with Example 5, respectively, it is found that the AC resistance affects the battery characteristics, and the lower the AC resistance, the higher the 6C charge capacity. For example, comparing Example 1 with Example 3, and Example 4 with Example 6, respectively, it is found that the porosity of the positive electrode layer affects the battery characteristics, and the lower the porosity of the positive electrode layer, the higher the 6C charge capacity.

[0193] Furthermore, for example, when Example 3 is compared with Comparative Example 5, the battery in Comparative Example 5 has high AC resistance and the porosity of the positive electrode layer exceeds 12%, resulting in deteriorated characteristics.

[0194] In this way, in a battery in which a positive electrode layer, a solid electrolyte layer, and a negative electrode layer are laminated, whether the solid electrolyte layer is one layer or two layers, the peel strength between the positive electrode side laminate and the negative electrode side laminate is 1.8 N / cm or less, and the AC resistance of the battery at 1 Hz at 25°C when the SOC is 50% is 100 Ω cm 2 By satisfying the above condition, a battery having excellent battery characteristics and in which the positive and negative electrodes can be easily separated can be realized.

[0195] In this embodiment, the final AC resistance of the battery is adjusted by the confining pressure, but as described in each of the above embodiments, the AC resistance of the battery can be adjusted by other methods such as pressurizing conditions, etc. In other words, the application of confining pressure by a confining member is not essential in the battery according to the present disclosure.

[0196] (Other embodiments) Although the battery according to the present disclosure has been described above based on the embodiments and examples, the present disclosure is not limited to these embodiments and examples. As long as it does not deviate from the gist of the present disclosure, various modifications conceived by a person skilled in the art to the embodiments or examples, as well as other forms constructed by combining some of the components in the embodiments and examples, are also included in the scope of the present disclosure.

[0197] For example, in the above embodiment, the ions conducted in the batteries 10 and 20 are lithium ions, but this is not limiting. The ions conducted in the batteries 10 and 20 may be ions other than lithium ions, such as sodium ions, magnesium ions, potassium ions, calcium ions, or copper ions. [Industrial Applicability]

[0198] Batteries according to the present disclosure may be utilized as batteries in a variety of applications, such as in electronic devices, appliances, and electric vehicles. [Explanation of symbols]

[0199] 10, 20 batteries 11 Positive electrode layer 12 Negative electrode layer 13, 16 Solid electrolyte layer 14 Positive electrode current collector layer 15 Negative electrode current collector layer 30, 31 Positive electrode laminate 40, 41 Negative electrode laminate 50 Exterior body 60 Restraint member

Claims

1. A battery having a structure in which a positive electrode current collector layer, a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, The peel strength between the positive electrode layer and the solid electrolyte layer is 1.8 N / cm or less; The AC resistance of the battery at 1 Hz at 25°C when the SOC (State of Charge) is 50% is 100 Ω cm 2 Below is the battery.

2. The porosity of the solid electrolyte layer is 7% or less.

10. The battery of claim 1.

3. The porosity of the positive electrode layer is 12% or less.

10. The battery of claim 1.

4. The porosity of the positive electrode layer is 9% or less.

10. The battery of claim 1.

5. The solid electrolyte layer contains an argyrodite-type sulfide-based solid electrolyte as a solid electrolyte.

10. The battery of claim 1.

6. A method for separating a battery according to any one of claims 1 to 5, comprising the steps of: isolating the battery between the positive electrode layer and the solid electrolyte layer; How to separate the batteries.

7. A battery having a structure in which a positive electrode current collector layer, a positive electrode layer, two or more solid electrolyte layers, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, at least one of a peel strength between adjacent solid electrolyte layers of the two or more solid electrolyte layers and a peel strength between the positive electrode layer and a solid electrolyte layer adjacent to the positive electrode layer of the two or more solid electrolyte layers is 1.8 N / cm or less; The 1 Hz AC resistance of the battery at 25°C with an SOC of 50% is 100 Ω cm 2 Below is the battery.

8. the porosity of the solid electrolyte layer adjacent to the negative electrode layer among the two or more solid electrolyte layers is 7% or less; 8. The battery of claim 7.

9. The porosity of the positive electrode layer is 12% or less.

8. The battery of claim 7.

10. The porosity of the positive electrode layer is 9% or less.

8. The battery of claim 7.

11. Each of the two or more solid electrolyte layers contains an argyrodite-type sulfide-based solid electrolyte as a solid electrolyte.

8. The battery of claim 7.

12. A method for separating a battery according to any one of claims 7 to 11, comprising the steps of: isolating the battery between adjacent solid electrolyte layers of the two or more solid electrolyte layers, or between the positive electrode layer and a solid electrolyte layer adjacent to the positive electrode layer of the two or more solid electrolyte layers; How to separate the batteries.

13. A method for manufacturing a battery having a structure in which a positive electrode current collector layer, a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, comprising the steps of: adjusting the peel strength between the positive electrode layer and the solid electrolyte layer to 1.8 N / cm or less; The AC resistance of the battery at 1 Hz at 25°C when the SOC is 50% is 100 Ω cm 2 and adjusting the How batteries are manufactured.

14. A method for manufacturing a battery having a structure in which a positive electrode current collector layer, a positive electrode layer, two or more solid electrolyte layers, a negative electrode layer, and a negative electrode current collector layer are laminated in this order, comprising the steps of: adjusting at least one of a peel strength between adjacent solid electrolyte layers of the two or more solid electrolyte layers and a peel strength between the positive electrode layer and a solid electrolyte layer adjacent to the positive electrode layer of the two or more solid electrolyte layers to be 1.8 N / cm or less; The AC resistance of the battery at 1 Hz at 25°C when the SOC is 50% is 100 Ω cm 2 and adjusting the How batteries are manufactured.

Citation Information

Patent Citations

  • Method of manufacturing all-solid battery

    JP2016134254A

  • All-solid-state secondary battery

    WO2015147122A1