Positive electrode active material for lithium ion secondary battery, method for producing the same, and lithium ion secondary battery

Coating lithium transition metal composite oxide particles with a lithium niobium compound addresses the issues of cycle characteristics and gas generation in lithium-nickel composite oxides, enhancing battery performance by maintaining capacity and reducing resistance.

JP2024135142APending Publication Date: 2024-10-04SUMITOMO METAL MINING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023045681
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Lithium-nickel composite oxides used in lithium ion secondary batteries suffer from inferior cycle characteristics and gas generation due to high nickel compositions, leading to battery expansion and capacity degradation.

Method used

A positive electrode active material for lithium ion secondary batteries is developed, comprising lithium transition metal composite oxide particles coated with a lithium niobium compound, where the coating layer contains a specific amount of niobium to suppress gas generation and improve cycle characteristics.

Benefits of technology

The coated lithium transition metal composite oxide particles enhance cycle characteristics, reduce gas generation, and maintain high initial discharge capacity with low internal resistance, thereby improving battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135142000003
    Figure 2024135142000003
  • Figure 2024135142000004
    Figure 2024135142000004
  • Figure 2024135142000005
    Figure 2024135142000005
Patent Text Reader

Abstract

To provide a positive electrode active material for a lithium ion secondary battery which has excellent cycle characteristics and can constitute a lithium ion secondary battery that generates less gas during charging and discharging.SOLUTION: A positive electrode active material for a lithium ion secondary battery has particles of a lithium transition metal composite oxide and a coating layer covering at least a part of the surfaces of the particles. The lithium transition metal composite oxide has a substance ratio of components other than oxygen of Li:Ni:Co:M which is represented by t:1-x-y:x:y (in the formula, M is at least one element selected from the group consisting of Mg, Al, Ca, Si, Mn, Ti, V, Fe, Cu, Cr, Zn, Zr, Nb, Mo and W, and 0.95≤t≤1.20, 0<x≤0.22, 0≤y≤0.15). The coating layer contains a lithium niobium compound, and the amount of Nb in the coating layer per surface area of 1 m2 of the lithium transition metal composite oxide excluding the coating layer is 0.14 mmol or more and 0.29 mmol or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery, a method for producing the same, and a lithium ion secondary battery. [Background technology]

[0002] In recent years, with the widespread use of small information terminals such as smartphones and tablet PCs, there is an increasing demand for small, lightweight secondary batteries with high energy density and durability. There is also a strong demand for the development of high-output secondary batteries as power sources for electric vehicles, including hybrid vehicles, or large secondary batteries for power storage.

[0003] Lithium ion secondary batteries are a type of secondary battery that meets these requirements. Lithium ion secondary batteries are composed of a negative electrode, a positive electrode, an electrolyte, and the like, and the active materials used as the materials for the negative and positive electrodes are materials that can release and store lithium ions. Currently, research and development of such lithium ion secondary batteries is being actively conducted. Among them, lithium ion secondary batteries that use lithium transition metal composite oxides as the positive electrode active material can obtain a voltage of 4V class, and are being put into practical use as batteries with high energy density.

[0004] Specifically, lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel, which is cheaper than cobalt, and lithium nickel cobalt manganese composite oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 Lithium transition metal composite oxides using lithium nickel (LiMn2O2) and manganese (LiMn2O4) have been proposed. Among these lithium transition metal composite oxides, lithium nickel composite oxide has been attracting attention in recent years as a material with high energy density, which can realize secondary batteries with high battery capacity without using cobalt, which is scarce in reserve.

[0005] However, compared with other lithium transition metal composite oxides, lithium nickel composite oxides have the problem that the battery capacity decreases with repeated charge and discharge, i.e., they have poor cycle characteristics, and the problem that the battery expands due to gas generation inside the battery when it is held at high temperatures in a charged state or when it is repeatedly charged and discharged at high temperatures.

[0006] One of the causes of the decrease in battery capacity and gas generation is the reversal of the Li-ion charge in the charged state, when Li is extracted from the lithium nickel composite oxide crystals. 1-x The presence of NiO2 is one of the reasons. 1-x NiO2 is prone to oxygen desorption from its crystal structure due to charge balance, and Li 1-x When oxygen is released from NiO2 and an electrochemically inactive NiO phase is formed, the charge / discharge capacity decreases. In addition, it is believed that the released oxygen oxidizes the electrolyte and generates CO2 gas, which causes the battery to expand. For this reason, in order to improve the cycle characteristics of lithium-ion secondary batteries that use lithium-nickel composite oxide as the positive electrode active material and suppress gas generation, it is considered important to control the surface state of the lithium-nickel composite oxide particles, which act as a reaction site with the electrolyte.

[0007] Incidentally, as an example of a method for controlling the surface state of lithium-nickel composite oxide particles, Patent Documents 1 and 2 disclose that improvements in initial discharge capacity and cycle characteristics can be achieved by coating layered rock-salt type lithium-nickel composite oxide particles having a high nickel composition, in which nickel accounts for 60 mass % or more of the transition metals, with lithium niobate. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2019-46716 A [Patent Document 2] JP 2019-139862 A Summary of the Invention

Problems to be Solved by the Invention

[0009] However, in the above proposal, prevention of battery swelling due to gas generation in a lithium-ion secondary battery has not been considered. In particular, particles having a high nickel composition in which nickel occupies 60 mol% or more among metal elements other than lithium have not been verified, and the gas generation problem peculiar to the high nickel composition has been unknown.

[0010] Therefore, in view of the problems of the above prior art, an object of the present invention is to provide a positive electrode active material for a lithium-ion secondary battery that can constitute a lithium-ion secondary battery having excellent cycle characteristics and little gas generation during charge and discharge.

Means for Solving the Problems

[0011] A positive electrode active material for a lithium-ion secondary battery according to one aspect of the present invention is a positive electrode active material for a lithium-ion secondary battery having particles of a lithium transition metal composite oxide and a coating layer covering at least a part of the surface of the particles, wherein a molar ratio Li:Ni:Co:M of components other than oxygen in the lithium transition metal composite oxide is t:1-x-y:x:y (wherein M is at least one element selected from the group consisting of Mg, Al, Ca, Si, Mn, Ti, V, Fe, Cu, Cr, Zn, Zr, Nb, Mo and W, 0.95≦t≦1.20, 0<x≦0.22, 0≦y≦0.15), the coating layer contains a lithium niobium compound, and an Nb amount of the coating layer per 1 m 2 of the surface area of the lithium transition metal composite oxide excluding the coating layer is 0.14 mmol or more and 0.29 mmol or less.

[0012] In this way, it is possible to provide a positive electrode active material for a lithium-ion secondary battery having excellent cycle characteristics and little gas generation during charge and discharge. Further, it is possible to prevent a decrease in the initial discharge capacity and an increase in the internal resistance by using a niobium compound for the coating layer.

[0013] In this case, in one aspect of the present invention, the ratio Nbs / (Nis+Cos+Nbs) of the amount of substance Nbs of Nb present on the surface of the positive electrode active material for a lithium ion secondary battery to the sum of the amounts of substances Nis+Cos+Nbs of Ni, Co, and Nb may be 0.70 or more and 0.97 or less.

[0014] In this way, side reactions between the positive electrode active material and the electrolyte can be suppressed, thereby suppressing excessive decomposition of the electrolyte.

[0015] In this case, in one aspect of the present invention, the lithium transition metal composite oxide may have a crystal structure belonging to the space group R-3m.

[0016] In this way, the internal resistance of a lithium ion secondary battery (hereinafter also referred to as a "secondary battery") using the positive electrode active material for lithium ion secondary batteries (hereinafter also referred to as a "positive electrode active material") according to one embodiment of the present invention can be suppressed.

[0017] In this case, in one aspect of the present invention, the carbon content of the positive electrode active material for a lithium ion secondary battery may be 0.05% by mass or more and 0.40% by mass or less.

[0018] In this way, the generation of carbon dioxide due to, for example, the decomposition of organic components contained in the coating layer during charging and discharging of the secondary battery can be sufficiently suppressed, thereby preventing the battery from expanding, etc.

[0019] In this case, in one aspect of the present invention, the amount of moisture relative to the entire positive electrode active material for a lithium ion secondary battery, as measured by the Karl Fischer method when the positive electrode active material is heated to 300° C., may be 0.12 mass % or less.

[0020] In this way, the hydrolysis reaction of the electrolyte in the electrolytic solution can be suppressed, and deterioration of the positive electrode active material caused by acidic components such as hydrogen fluoride can be suppressed.

[0021] In one embodiment of the present invention, the specific surface area of ​​the lithium transition metal composite oxide particles is 0.1 m2 / g or more 1.0m 2 / g or less.

[0022] In this way, it is possible to sufficiently promote the desorption / insertion of lithium ions during charging and discharging of the secondary battery, to sufficiently suppress the internal resistance, and to suppress excessive decomposition of the electrolyte.

[0023] In this case, in one embodiment of the present invention, the lithium transition metal composite oxide particles may have a volume average particle size of 2 μm or more and 20 μm or less.

[0024] In this way, the battery capacity per unit volume of the lithium ion secondary battery can be made sufficiently large, and excellent battery characteristics such as high safety and high output can be obtained.

[0025] Another aspect of the present invention is a lithium ion secondary battery including a positive electrode using the above-described positive electrode active material for lithium ion secondary batteries, a negative electrode, a separator, and a nonaqueous electrolyte.

[0026] In this way, it is possible to provide a lithium ion secondary battery that has excellent cycle characteristics and generates little gas during charging and discharging, and also has a high initial discharge capacity and a small internal resistance.

[0027] Further, one aspect of the present invention is a method for producing a positive electrode active material for a lithium ion secondary battery having lithium transition metal composite oxide particles and a coating layer that coats at least a portion of the surface of the particles, the method comprising: a precursor crystallization step of preparing a transition metal composite hydroxide, which is a precursor of the lithium transition metal composite oxide, by a crystallization reaction; an oxidizing roasting step of oxidizing and roasting the transition metal composite hydroxide obtained in the precursor crystallization step to obtain a transition metal composite oxide; a lithium transition metal composite oxide synthesis step of mixing the transition metal composite oxide obtained in the oxidizing roasting step with a lithium compound and firing the mixture to obtain a lithium transition metal composite oxide; and a coating step of forming the coating layer containing a lithium niobium compound on at least a portion of the surface of the lithium transition metal composite oxide particles obtained in the lithium transition metal composite oxide synthesis step, the coating step being characterized in that the lithium transition metal composite oxide particles obtained in the lithium transition metal composite oxide synthesis step are mixed with a coating agent containing a lithium compound and a niobium compound, dried, and heat-treated.

[0028] In this way, it is possible to provide a positive electrode active material for a lithium ion secondary battery that has excellent cycle characteristics and generates little gas during charging and discharging, and also has a high initial discharge capacity and a low internal resistance.

[0029] In this case, in one aspect of the present invention, the lithium transition metal composite oxide synthesis step may involve firing in an oxygen atmosphere at a temperature of 700° C. or higher and 800° C. or lower.

[0030] In this way, the crystal structure of the lithium transition metal composite oxide can be grown sufficiently, and cation mixing can be suppressed, thereby preventing deterioration of the battery characteristics of the secondary battery.

[0031] In one embodiment of the present invention, the coating step is carried out such that the amount of Nb in the lithium niobium compound is equal to or larger than 1 m of the surface area of ​​the lithium transition metal composite oxide. 2The niobium compound is added so that the amount is 0.14 mmol or more and 0.29 mmol or less per unit area. Components other than oxygen in the lithium transition metal composite oxide obtained in the coating step are represented by Li:Ni:Co:M = t:1-x-y:x:y (where M is at least one element selected from the group consisting of Mg, Al, Ca, Si, Mn, Ti, V, Fe, Cu, Cr, Zn, Zr, Nb, Mo, and W, 0.95 ≦ t ≦ 1.20, 0 < x ≦ 0.22, 0 ≦ y ≦ 0.15). The ratio Nbs / (Nis+Cos+Nbs) of the amount of substance Nbs of Nb present on the surface of the positive electrode active material for the lithium ion secondary battery to the sum Nis+Cos+Nbs of the amounts of substance of Ni, Co, and Nb may be 0.70 or more.

[0032] In this way, the coating layer can be uniformly disposed on the entire surface of the particles of the lithium transition metal composite oxide. And in the secondary battery, deterioration of the positive electrode active material and decomposition of the electrolytic solution can be suppressed, and the internal resistance can be reduced.

[0033] At this time, in one aspect of the present invention, in the coating step, the lithium compound and the niobium compound may be added so that the molar ratio of Li to Nb (Li / Nb) in the lithium niobium compound of the coating layer is 0.3 or more and 3.0 or less.

[0034] In this way, a positive electrode active material for a lithium ion secondary battery with more excellent cycle characteristics, less gas generation during charge and discharge, a high initial discharge capacity, and a small internal resistance can be provided.

[0035] At this time, in one aspect of the present invention, the heat treatment may be performed in an oxygen atmosphere at a temperature of 200°C or higher and 500°C or lower for 1 hour or more and 5 hours or less.

[0036] In this way, a lithium niobium compound can be included in the coating layer, and the form of the coating layer can be maintained. And a positive electrode active material for a lithium ion secondary battery with more excellent cycle characteristics, less gas generation during charge and discharge, a high initial discharge capacity, and a small internal resistance can be provided.

[0037] In this case, in one aspect of the present invention, the coating agent may contain the lithium compound and the niobium compound used in the coating step dissolved in a solvent, or a mixture of the lithium compound and the niobium compound that is liquid at room temperature or has a low melting point that melts during heat treatment in the coating step.

[0038] In this way, the coating layer can be disposed more uniformly over the entire surface of the lithium transition metal composite oxide particle.

[0039] In this case, in one embodiment of the present invention, the niobium compound used in the coating step may be one or more of niobium ethoxide, niobium pentaisopropoxide, niobium pentabutoxide, and niobium oxide.

[0040] This can prevent impurities from being mixed into the coating layer. Effect of the Invention

[0041] According to the present invention, it is possible to provide a positive electrode active material for a lithium ion secondary battery having excellent cycle characteristics and little gas generation during charging and discharging, and also to provide a positive electrode active material for a lithium ion secondary battery having a high initial discharge capacity and a low internal resistance. [Brief description of the drawings]

[0042] [Figure 1] FIG. 1 is a process diagram illustrating an outline of a method for producing a positive electrode active material for a lithium ion secondary battery according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a coin-type secondary battery used for evaluating the battery characteristics. [Diagram 3] FIG. 3 shows a laminated battery used in evaluating battery characteristics, where (A) is a schematic explanatory diagram of the laminated battery, and (B) is a front view of the laminated battery. [Figure 4] 1 shows an example of impedance evaluation measurement, and an equivalent circuit diagram and a Nyquist plot used in the analysis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] As a result of intensive research to solve the above problems, the inventors of the present invention have found that by coating at least a part of a lithium transition metal composite oxide with a coating layer containing a lithium niobium compound and controlling the ratio of niobium to the transition metal element and the amount of niobium per surface area, it is possible to improve cycle characteristics and suppress gas generation during charging and discharging at the same time, and have completed the present invention. Preferred embodiments of the present invention will be described below.

[0044] The following describes the embodiments of the present invention, but the present invention is not limited to the following embodiments, and various modifications and substitutions can be made to the following embodiments without departing from the scope of the present invention. Furthermore, not all of the configurations described in the present embodiments are necessarily essential as the solution of the present invention.

[0045] A positive electrode active material for a lithium ion secondary battery according to one embodiment of the present invention, a method for producing the same, and a lithium ion secondary battery will be described in the following order. 1. Positive electrode active material for lithium-ion secondary batteries 1-1. Lithium transition metal composite oxide particles 1-2.Coating layer 1-3. Characteristics of positive electrode active material 2. Manufacturing method of positive electrode active material for lithium-ion secondary batteries 2-1. Precursor crystallization process 2-2. Oxidation roasting process 2-3. Lithium transition metal composite oxide synthesis process 2-4.Coating process 3. Lithium-ion secondary battery 3-1. Positive electrode 3-2. Negative electrode 3-3.Separator 3-4.Nonaqueous electrolyte 3-5. Shape and structure of secondary batteries 3-6.Characteristics of secondary batteries

[0046] <1. Cathode active material for lithium-ion secondary battery> First, a configuration example of the cathode active material for the lithium-ion secondary battery of the present embodiment will be described.

[0047] The cathode active material of the present embodiment has particles of a lithium transition metal composite oxide and a coating layer that covers at least a part of the surface of the particles. The lithium transition metal composite oxide particles of the cathode active material for the lithium-ion secondary battery of the present embodiment can contain lithium (Li), nickel (Ni), cobalt (Co), and element M (M) in a molar ratio of Li:Ni:Co:M = t:1-x-y:x:y. However, it is preferable to satisfy 0.95 ≦ t ≦ 1.20, 0 < x ≦ 0.22, and 0 ≦ y ≦ 0.15. Element M can be at least one element selected from magnesium (Mg), aluminum (Al), calcium (Ca), silicon (Si), manganese (Mn), titanium (Ti), vanadium (V), iron (Fe), copper (Cu), chromium (Cr), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), and tungsten (W).

[0048] The coating layer contains a lithium niobium compound, and niobium can be contained at a ratio of 0.14 mmol or more and 0.29 mmol or less per 1 m 2 of the surface area of the lithium transition metal composite oxide before coating, that is, excluding the coating layer. Lithium niobate may be used as the lithium niobium compound.

[0049] For the cathode active material for the lithium-ion secondary battery of the present embodiment, the ratio of the amount of substance of Nb present on the surface to the sum of the amounts of substance of Nb, Ni, and Co (Nbs / (Nis+Cos+Nbs)) can be 0.70 or more and 0.97 or less.

[0050] Hereinafter, the cathode active material for the lithium-ion secondary battery of the present embodiment (hereinafter, also simply referred to as "cathode active material") will be specifically described.

[0051] The positive electrode active material of the present embodiment may have a lithium transition metal composite oxide particle and a coating layer that coats at least a part of the lithium transition metal composite oxide particle. The lithium transition metal composite oxide particle and the coating layer will be described below.

[0052] <1-1. Lithium transition metal composite oxide particles> The lithium transition metal composite oxide particles can contain lithium (Li), nickel (Ni), cobalt (Co), and element M (M) in a substance ratio of Li:Ni:Co:M=t:1-xy:x:y.

[0053] In the formula representing the mass ratio of each element in the above-mentioned lithium transition metal composite oxide, the value of t representing the lithium (Li) content can be 0.95 or more and 1.20 or less, preferably 0.98 or more and 1.10 or less, and more preferably 1.00 or more and 1.10 or less.

[0054] By setting the value of t to 0.95 or more, the internal resistance of the secondary battery using the positive electrode active material containing the lithium transition metal composite oxide can be suppressed and the output characteristics can be improved. Also, by setting the value of t to 1.20 or less, the initial discharge capacity of the secondary battery using the positive electrode active material containing the lithium transition metal composite oxide can be kept high. That is, by setting the value of t in the above-mentioned range, the output characteristics and capacity characteristics of the secondary battery using the positive electrode active material containing the lithium transition metal composite oxide can be improved.

[0055] Nickel (Ni) in the above-mentioned lithium transition metal composite oxide is an element that contributes to increasing the capacity of a secondary battery that uses a positive electrode active material containing a lithium transition metal composite oxide.

[0056] Cobalt (Co) in the lithium transition metal composite oxide is an element that contributes to reducing the irreversible capacity of a secondary battery using a positive electrode active material containing the lithium transition metal composite oxide. The value of x, which indicates the content of cobalt, can be more than 0 and 0.22 or less, preferably 0.10 to 0.22, and more preferably 0.10 to 0.20.

[0057] By setting the value of x to be greater than 0, it is possible to reduce the irreversible capacity, which is the difference between the charge capacity and the discharge capacity, in a secondary battery using a positive electrode active material containing the lithium transition metal composite oxide. Also, by setting the value of x to be 0.22 or less, it is possible to obtain a high battery capacity.

[0058] The lithium transition metal composite oxide may contain an element M as an additive element in addition to the above metal elements. As the above-mentioned element M, at least one element selected from magnesium (Mg), aluminum (Al), calcium (Ca), silicon (Si), manganese (Mn), titanium (Ti), vanadium (V), iron (Fe), copper (Cu), chromium (Cr), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), and tungsten (W) can be used. The element M is appropriately selected depending on the application and required performance of the secondary battery formed using the positive electrode active material.

[0059] Since the element M itself does not contribute to the redox reaction, the value of y indicating the content of the element M can be 0.15 or less, preferably 0.10 or less, and more preferably 0.05 or less. Since the lithium transition metal composite oxide does not need to contain the element M, the lower limit of y indicating the content of the element M can be 0.

[0060] It is preferable that the lithium transition metal composite oxide particles have a diffraction pattern obtained by X-ray diffraction (XRD) measurement, from which a peak attributed to the layered rock salt crystal structure of the "R-3m" structure is detected. In particular, it is more preferable that only peaks attributed to the layered rock salt crystal structure of the "R-3m" structure are detected from the diffraction pattern. This is because the layered rock salt oxide of the "R-3m" structure is preferable because it can suppress the internal resistance in particular when a positive electrode active material containing the lithium transition metal composite oxide particles is used as a secondary battery.

[0061] However, a lithium transition metal composite oxide having a layered rock-salt type crystal structure cannot be obtained in a single phase, and impurities may be mixed in. Even if impurities are mixed in, it is preferable that the intensity of the peak of a different phase other than the layered rock-salt type structure of the "R-3m" structure does not exceed the peak intensity attributable to the layered rock-salt type structure of the "R-3m" structure.

[0062] When observed with an electron microscope such as SEM or TEM, the particles of the lithium transition metal composite oxide are preferably in the form of secondary particles having a particle size of 3.0 μm to 15.0 μm formed by agglomeration of many primary particles having a particle size of 0.1 μm to 2.0 μm, single primary particles having a particle size of 1.0 μm to 7.0 μm, or a mixture thereof. Each particle may have a space or void surrounded by one or more primary particles.

[0063] The lithium transition metal composite oxide particles have a specific surface area of ​​0.1 m 2 / g or more 1.0m 2 / g or less, and 0.1m 2 / g or more 0.8m 2 / g or less is more preferable. The desorption / insertion of lithium ions that occurs in the lithium transition metal composite oxide particles during charging / discharging of the secondary battery occurs at the interface between the lithium transition metal composite oxide particles and the electrolyte, i.e., through the surface of the lithium transition metal composite oxide particles. The specific surface area of ​​the lithium transition metal composite oxide particles contained in the positive electrode active material is preferably 0.1 m 2 By setting the specific surface area of ​​the lithium transition metal composite oxide particles to 1.0 m / g or more, the desorption / insertion of lithium ions can be sufficiently promoted and the internal resistance can be sufficiently suppressed, which is preferable. In addition, as described above, the electrolyte may be decomposed due to a side reaction occurring at the interface between the particles of the positive electrode active material and the electrolyte. 2 / g or less, excessive decomposition of the electrolyte can be suppressed. Regarding the initial discharge capacity of the secondary battery, a larger BET specific surface area is preferable because it increases the number of reaction sites.

[0064] The specific surface area of ​​the lithium transition metal composite oxide particles of this embodiment can be measured, for example, by the BET method utilizing nitrogen adsorption.

[0065] The volume average particle diameter of the lithium transition metal composite oxide particles of this embodiment, as measured by a laser diffraction scattering type particle size distribution analyzer, is preferably 2 μm to 20 μm, more preferably 2 μm to 15 μm, and even more preferably 3 μm to 15 μm. This is because, when the volume average particle diameter of the lithium transition metal composite oxide particles is 2 μm to 20 μm, a secondary battery using a positive electrode active material containing the lithium transition metal composite oxide particles in the positive electrode can have a sufficiently large battery capacity per volume and can obtain excellent battery characteristics such as high safety and high output.

[0066] <1-2. Covering layer> The coating layer contains a compound containing niobium, i.e., a niobium compound, and coats at least a part of the lithium transition metal composite oxide particles. The coating layer may be composed of a lithium niobium compound. By disposing the coating layer, deterioration of the positive electrode active material and decomposition of the electrolyte can be suppressed in a secondary battery having a positive electrode containing the positive electrode active material of this embodiment.

[0067] There is no need for a clear boundary between the coating layer and the lithium transition metal composite oxide particles. Therefore, the coating layer refers to a portion or region on the surface side of the positive electrode active material of this embodiment that has a higher niobium concentration than the lithium transition metal composite oxide particles, i.e., the central region, which is the coated material. The coating layer may be partially dissolved in the lithium transition metal composite oxide.

[0068] The niobium content of the coating layer is not particularly limited, but it is preferable to adjust the content according to the specific surface area of ​​the lithium transition metal composite oxide particles to be coated. Specifically, the coating layer is, for example, a niobium content of 1 m2 of the surface area (hereinafter, simply referred to as "surface area") of the lithium transition metal composite oxide particles before coating, i.e., excluding the coating layer. 2In this case, the niobium content is preferably 0.14 mmol or more and 0.29 mmol or less, and more preferably 0.18 mmol or more and 0.27 mmol or less.

[0069] This is the surface area (specific surface area) of a lithium transition metal composite oxide particle of 1 m 2 By setting the niobium content per unit area to 0.14 mmol or more, the coating layer can be uniformly disposed over the entire surface of the lithium transition metal composite oxide particle, and the effect of the coating layer in suppressing deterioration of the surface of the lithium transition metal composite oxide particle appears during cycle performance evaluation.

[0070] In addition, the provision of a coating layer can improve cycle characteristics and suppress swelling of the battery, but at the same time, it may increase internal resistance and reduce discharge capacity. 2 By setting the niobium content per unit area to 0.29 mmol or less, the coating layer is prevented from interfering with the intercalation / deintercalation reaction of lithium into the lithium transition metal composite oxide, the internal resistance can be reduced, and a decrease in discharge capacity can be suppressed, which is preferable.

[0071] The method for evaluating and calculating the niobium content of the coating layer is not particularly limited, but an example of the method is shown below. First, the niobium content (mmol / g) in 1 g of the positive electrode active material after coating with a lithium niobium compound is measured by a method such as chemical analysis. For example, the measurement can be performed by ICP (Inductively Coupled Plasma) emission spectrometry. In addition, the specific surface area (m2) of the particles of the lithium transition metal composite oxide before coating with the lithium niobium compound is measured. 2 The niobium content (mmol / g) in 1 g of the positive electrode active material after the coating treatment with the lithium niobium compound is measured by the specific surface area (m 2 / g), the surface area of ​​the lithium transition metal composite oxide particles is calculated as 1 m 2Niobium content per unit (mmol / m 2 ) can be calculated.

[0072] The niobium content in 1 g of the positive electrode active material after coating with a lithium niobium compound is different from the specific surface area of ​​the lithium transition metal composite oxide particles before coating, because the denominators are different. However, since the amount of niobium used for coating is small, it can be approximately calculated as the specific surface area of ​​1 m of the lithium transition metal composite oxide. 2 The amount of niobium supported can be used as the amount of niobium supported.

[0073] When the lithium transition metal composite oxide particles before the coating treatment contain niobium, it is preferable to use the difference in the niobium content before and after the coating treatment as the amount of niobium used in the coating.

[0074] The extent of the coverage area of ​​the lithium transition metal composite oxide particles in the coating layer can be determined from the ratio of the amount of Nb present on the surface to the sum of the amounts of Nb, Ni, and Co (Nbs / (Nis+Cos+Nbs)) (hereinafter also referred to as the "ratio of the amount of coated metal surface"), which is known from semi-quantitative analysis using X-ray photoelectron spectroscopy (XPS).

[0075] Due to its characteristics, XPS can selectively obtain information on the surface of the measurement target from 1 nm to 5 nm, so that the composition ratio of the surface layer of the material can be known. The ratio of the coated metal surface amount is preferably 0.70 or more. By setting the ratio of the coated metal surface amount to 0.70 or more, it means that the niobium present as a coating layer, that is, the niobium present as a coating layer without diffusing to the side of the lithium transition metal composite oxide particles, is sufficiently secured, and a coating layer that is sufficiently uniform to suppress side reactions between the active material and the electrolyte is formed. And, by suppressing side reactions between the positive electrode active material and the electrolyte, excessive decomposition of the electrolyte can be suppressed. When the ratio of the coated metal surface amount is 0.80 or more, it is more preferable because particularly high cycle characteristics can be obtained. In addition, the ratio of the coated metal surface amount is preferably 0.97 or less.

[0076] By introducing lithium into the coating layer to form a lithium niobium compound such as lithium niobate, the lithium ion conductivity is improved compared to when a niobium compound is used as the coating layer, the internal resistance can be reduced, and a decrease in discharge capacity can be suppressed.

[0077] The ratio of the amount of substance of Li and Nb (Li / Nb) of the lithium niobium compound in the coating layer is preferably 0.3 or more and 3.0 or less. By setting the ratio of the amount of substance of Li and Nb of the lithium niobium compound in the coating layer to 0.3 or more, a lithium niobium compound with high lithium ion conductivity is generated, which is preferable. In addition, by setting the ratio of the amount of substance of Li and Nb of the lithium niobium compound in the coating layer to 3.0 or less, the amount of unreacted lithium compound can be reduced, and the deterioration of battery characteristics such as a decrease in initial discharge capacity and an increase in positive electrode resistance can be suppressed. In addition, by setting the ratio of the amount of substance of Li and Nb of the lithium niobium compound (Li / Nb) to 0.3 or more and 3.0 or less, the cycle characteristics can be further improved, the swelling of the battery can be further reduced, the initial discharge capacity can be further increased, and the internal resistance can be further reduced. In addition, the lithium niobium compound preferably contains any one of LiNbO3, Li3NbO4, and LiNb3O8, and more preferably is any one of LiNbO3, Li3NbO4, and LiNb3O8.

[0078] <1-3. Characteristics of positive electrode active material> Up to this point, the lithium transition metal composite oxide particles and the coating layer have been described. It is preferable that the positive electrode active material of this embodiment has the following properties.

[0079] The positive electrode active material of this embodiment is preferably composed only of the above-mentioned lithium transition metal composite oxide particles and the coating layer, but impurities may be mixed in during production. In particular, moisture and carbon are impurities that may increase due to the coating process. Since moisture and carbon may affect cycle characteristics, it is preferable that the moisture and carbon are controlled within a predetermined range.

[0080] The positive electrode active material of this embodiment preferably has a carbon content of 0.05% by mass or more and 0.40% by mass or less, and more preferably 0.05% by mass or more and 0.20% by mass or less. By setting the carbon content to 0.40% by mass or less, the generation of carbon dioxide due to, for example, decomposition of an organic component contained in a coating layer during charging and discharging of a secondary battery using the positive electrode active material can be sufficiently suppressed, and the occurrence of battery expansion or the like can be prevented. However, since carbon is mixed into the positive electrode active material of this embodiment due to carbon dioxide in the air, etc., it is difficult to set the carbon content to less than 0.01 mass. For this reason, the lower limit of the carbon content is preferably 0.05% by mass. Here, the carbon content of the positive electrode active material is the carbon content relative to the entire positive electrode active material expressed in mass%. The carbon content of the positive electrode active material of this embodiment can be evaluated, for example, by infrared absorption method or the like.

[0081] In addition, the positive electrode active material of the present embodiment preferably has a water content (moisture content) of 0.12 mass % or less. By setting the water content to 0.12 mass % or less, the hydrolysis reaction of the electrolyte in the electrolytic solution can be more reliably suppressed in a secondary battery using the positive electrode active material.

[0082] When the electrolyte of the electrolytic solution is hydrolyzed, acidic components such as hydrogen fluoride are generated, and the acidic components react with the positive electrode active material to cause deterioration. However, as described above, by setting the water content of the positive electrode active material of this embodiment to 0.12 mass% or less, the hydrolysis reaction of the electrolyte of the electrolytic solution can be more reliably suppressed, and the deterioration can be suppressed, which is preferable. The water content of the positive electrode active material of this embodiment can be evaluated by, for example, the Karl Fischer method at a heating temperature of 300°C.

[0083] According to the positive electrode active material for lithium ion secondary batteries according to one embodiment of the present invention, it is possible to provide a positive electrode active material for lithium ion secondary batteries which has excellent cycle characteristics and generates little gas during charging and discharging.

[0084] <2. Method for producing positive electrode active material for lithium ion secondary batteries> Next, a method for producing a positive electrode active material for a lithium ion secondary battery according to one embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a process diagram showing an outline of a method for producing a positive electrode active material for a lithium ion secondary battery according to one embodiment of the present invention. The method for producing a positive electrode active material for a lithium ion secondary battery according to one embodiment of the present invention is a method for producing a positive electrode active material for a lithium ion secondary battery having particles of a lithium transition metal composite oxide and a coating layer that coats at least a part of the surface of the particles.

[0085] As shown in FIG. 1, a method for producing a positive electrode active material according to one embodiment of the present invention can include the following four steps.

[0086] 1st step: [Precursor crystallization step S1] In the precursor crystallization step S1, a transition metal composite hydroxide, which is a precursor of the lithium transition metal composite oxide, is prepared by a crystallization reaction. Specifically, for example, a mixed aqueous solution is prepared using water-soluble raw materials so that the substance amount ratio of each element is Ni:Co:M=1-xy:x:y, and the mixed aqueous solution is reacted in a reaction tank together with an alkali metal aqueous solution to obtain a transition metal composite hydroxide. Note that x and y in the above formula can be in the same suitable range as x and y described in the lithium transition metal composite oxide particles.

[0087] 2nd process: [Oxidation roasting process S2] In the oxidation roasting step S2, a transition metal composite oxide is prepared. Specifically, for example, the transition metal composite hydroxide obtained in the precursor crystallization step S1 is fired in an oxidizing atmosphere at a temperature of 500° C. or more and 700° C. or less to obtain the transition metal composite oxide.

[0088] Third step: [Lithium transition metal composite oxide synthesis step S3] In the lithium transition metal composite oxide synthesis step S3, the transition metal composite oxide obtained in the oxidation roasting step S2 is mixed with a lithium compound and fired at a temperature of 700°C or higher and 800°C or lower in an oxygen atmosphere to obtain a lithium transition metal composite oxide.

[0089] 4th step: [Coating step S4] In the coating step S4, a coating layer is formed on the surface of the lithium transition metal composite oxide particles. Specifically, for example, the lithium transition metal composite oxide particles obtained in the lithium transition metal composite oxide synthesis step S3 are mixed with a liquid coating agent containing a lithium compound and a niobium compound, dried, and then heat-treated in an oxygen atmosphere at a temperature of 200° C. to 500° C. to provide a coating layer on the surface of the lithium transition metal composite oxide particles.

[0090] An example of a method for producing a positive electrode active material according to the present embodiment will be described in more detail below. Note that the following description is merely an example of the production method, and is not intended to limit the production method.

[0091] <2-1. Precursor crystallization step S1> In the precursor crystallization step S1, first, a metal compound containing nickel, a metal compound containing cobalt, and, in some cases, a metal compound containing an element M (M is at least one element selected from the group consisting of Mg, Al, Ca, Si, Mn, Ti, V, Fe, Cu, Cr, Zn, Zr, Nb, Mo, and W) are dissolved in water in a predetermined ratio to prepare a mixed aqueous solution (mixed aqueous solution preparation step). The composition ratio of each metal in the mixed aqueous solution is the same as the composition ratio of the transition metal composite hydroxide finally obtained. Therefore, it is preferable to prepare the mixed aqueous solution by adjusting the ratio of the metal compound dissolved in water so that the composition ratio of each metal in the mixed aqueous solution is the same as the composition ratio of each metal in the intended transition metal composite hydroxide particles. As long as the metal compound is water-soluble, sulfates, chlorides, nitrates, etc. can be used, but sulfates are preferable from the viewpoint of cost. Note that, if a suitable water-soluble raw material cannot be found for the element M, it may be added in the oxidizing roasting step S2 described later or in the lithium transition metal composite oxide synthesis step S3 without being added to the mixed aqueous solution.

[0092] Next, water is poured into the reaction tank, and an alkaline substance and an ammonium ion donor are added in appropriate amounts to prepare an initial aqueous solution (initial aqueous solution preparation step). At this time, it is preferable to prepare the initial aqueous solution so that the pH value is 11.2 to 12.2 at a liquid temperature of 25° C. and the ammonia concentration is 2 g / L to 15 g / L.

[0093] When the precursor crystallization step S1 is performed to prepare a transition metal composite hydroxide, impurities resulting from anions constituting the metal compounds contained in the mixed aqueous solution used may be mixed into the transition metal composite hydroxide. However, by setting the pH value of the initial aqueous solution to 11.2 or more, it is possible to suppress the mixing of impurities resulting from anions constituting the metal compounds of the raw materials, which is preferable. In addition, by setting the pH value of the initial aqueous solution to 12.2 or less, it is possible to suppress the resulting transition metal composite hydroxide particles from being microparticulated, and to obtain an optimal size, which is preferable.

[0094] In addition, by setting the ammonia concentration of the initial aqueous solution to 2 g / L or more, the particles of the resulting transition metal composite hydroxide can be made particularly likely to have a spherical shape, which is preferable, and by setting the ammonia concentration of the initial aqueous solution to 15 g / L or less, the solubility of the transition metal forming the ammonia complex can be prevented from increasing excessively, and the composition of the resulting transition metal composite hydroxide can be made to be the target composition more reliably, which is preferable.

[0095] The alkaline substance used in preparing the initial aqueous solution is not particularly limited, but is preferably one or more selected from sodium carbonate, sodium bicarbonate, potassium carbonate, sodium hydroxide, and potassium hydroxide. It is preferable to add it in the form of an aqueous solution, since the amount added can be easily adjusted. The ammonium ion donor is not particularly limited, but is preferably one or more selected from an aqueous ammonium carbonate solution, an aqueous ammonia solution, an aqueous ammonium chloride solution, and an aqueous ammonium sulfate solution.

[0096] In the precursor crystallization step S1, the above-mentioned mixed aqueous solution can be dropped into the initial aqueous solution to prepare a reaction aqueous solution. It is preferable to maintain the pH value and ammonia concentration of the reaction aqueous solution within the above-mentioned suitable ranges.

[0097] The atmosphere in the reaction vessel is preferably a non-oxidizing atmosphere, for example, an atmosphere with an oxygen concentration of 1% by volume or less. This is because a non-oxidizing atmosphere, for example, an atmosphere with an oxygen concentration of 1% by volume or less, is preferable because it can suppress the oxidation of the raw materials, etc. Therefore, for example, it is possible to prevent oxidized cobalt from precipitating as fine particles.

[0098] The temperature of the reaction tank in the precursor crystallization step S1 is preferably maintained at 40° C. or higher and 60° C. or lower, and more preferably at 45° C. or higher and 55° C. or lower. In order to maintain the reaction tank in this temperature range, it is preferable that the initial aqueous solution and the reaction aqueous solution placed in the reaction tank are also maintained within the same temperature range.

[0099] Since the temperature of the reaction tank naturally rises due to the heat of reaction and the energy of stirring, it is preferable to set the temperature at 40° C. or higher since it does not consume extra energy for cooling. In addition, it is preferable to set the temperature of the reaction tank at 60° C. or lower since it is possible to suppress the amount of ammonia evaporation from the initial aqueous solution and the reaction aqueous solution, and it is possible to easily maintain the target ammonia concentration.

[0100] Then, in the precursor crystallization process S1, the initial aqueous solution is placed in a reaction tank, and after adjusting the temperature, etc., the mixed aqueous solution is dropped into the reaction tank at a constant rate to prepare a reaction aqueous solution, thereby crystallizing the precursor transition metal composite hydroxide particles (crystallization step).

[0101] As described above, it is preferable that the pH value and ammonia concentration of the reaction aqueous solution are in the same suitable range as those described for the initial aqueous solution. Therefore, when the mixed aqueous solution is dropped into the initial aqueous solution or the reaction aqueous solution, it is preferable to drop the ammonium ion donor and the alkaline substance into the initial aqueous solution or the reaction aqueous solution at a constant rate. It is preferable to control the pH value of the reaction aqueous solution to be 11.2 or more and 12.2 or less at a liquid temperature of 25°C, and the ammonia concentration to be maintained at 2 g / L or more and 15 g / L or less.

[0102] Thereafter, the slurry containing the transition metal composite hydroxide particles is collected from an overflow port provided in the reaction tank, and then filtered and dried to obtain powdered transition metal composite hydroxide particles as a precursor.

[0103] <2-2. Oxidation roasting process S2> Next, the oxidizing roasting step S2 will be described. In the oxidizing roasting step S2, the transition metal composite hydroxide obtained in the precursor crystallization step S1 is oxidizing roasted to obtain a transition metal composite oxide. In the oxidizing roasting step S2, the transition metal composite hydroxide produced in the precursor crystallization step S1 is fired in an oxidizing atmosphere and then cooled to room temperature to obtain a transition metal composite oxide.

[0104] The roasting conditions in the oxidation roasting step S2 are not particularly limited, but it is preferable to roast in an oxidizing atmosphere, for example, in an air atmosphere, at a temperature of 500°C to 700°C for 1 hour to 12 hours. This is because a roasting temperature of 500°C or higher is preferable because the transition metal composite hydroxide particles can be completely converted into transition metal composite oxides. In addition, a roasting temperature of 700°C or lower is preferable because it is possible to prevent the specific surface area of ​​the transition metal composite oxide from becoming excessively small.

[0105] By setting the calcination time to 1 hour or more, the temperature in the calcination vessel can be particularly uniform, and the reaction can proceed uniformly, which is preferable. Furthermore, even if the calcination is performed for a time longer than 12 hours, no significant change is observed in the physical properties of the resulting transition metal composite oxide, so from the viewpoint of energy efficiency, the calcination time is preferably set to 12 hours or less.

[0106] The oxygen concentration in the oxidizing atmosphere during firing is preferably equal to or higher than the oxygen concentration in the air atmosphere, i.e., 20% by volume or higher. Since an oxygen atmosphere can also be used, the upper limit of the oxygen concentration in the oxidizing atmosphere can be 100% by volume.

[0107] For example, when the compound containing element M cannot be coprecipitated in the precursor crystallization step S1, the compound containing element M may be added to the transition metal composite hydroxide to be subjected to the oxidizing roasting step S2 so as to have a desired composition ratio, and then calcined. The compound containing element M to be added is not particularly limited, and for example, an oxide, hydroxide, carbonate, or a mixture thereof may be used.

[0108] After completion of the oxidizing roasting step S2, if slight sintering is observed in the transition metal composite oxide particles, a crushing treatment may be added.

[0109] <2-3. Lithium transition metal composite oxide synthesis process S3> In the lithium transition metal composite oxide synthesis step S3, the transition metal composite oxide obtained in the oxidation roasting step S2 is mixed with a lithium compound and then calcined to obtain a lithium transition metal composite oxide.

[0110] In the lithium transition metal composite oxide synthesis step S3, first, a lithium compound is added to and mixed with the transition metal composite oxide particles obtained in the oxidation roasting step S2 so that the amount of lithium is 95% or more and 120% or less of the total amount of substance of the component metal elements contained in the particles, thereby obtaining a lithium mixture (lithium mixture preparation step).

[0111] The lithium compound to be added is not particularly limited, and may be, for example, lithium hydroxide, lithium nitrate, lithium carbonate, or a mixture thereof. As the lithium compound, it is particularly preferable to use lithium hydroxide, which has a low melting point and high reactivity.

[0112] Next, the obtained lithium mixture is calcined in an oxygen atmosphere and then cooled to room temperature to obtain a lithium-containing lithium transition metal composite oxide (calcination step). Although the calcination conditions are not particularly limited, it is preferable to calcinate at a temperature of 700° C. to 800° C. for 1 hour to 24 hours.

[0113] The oxygen atmosphere is preferably an atmosphere containing 80% by volume or more of oxygen. This is because by setting the oxygen concentration in the atmosphere to 80% by volume or more, it is possible to particularly suppress cation mixing, in which Ni atoms are mixed into the Li sites in the obtained lithium transition metal composite oxide, and it is preferable to prevent deterioration of the battery characteristics of the secondary battery. Since an oxygen atmosphere can be used, the upper limit of the oxygen concentration of the oxygen atmosphere can be set to 100% by volume.

[0114] A calcination temperature of 700° C. or higher is preferable because it stabilizes the crystal structure of the lithium transition metal composite oxide and allows the lithium transition metal composite oxide particles to grow sufficiently, whereas a calcination temperature of 800° C. or lower is preferable because it suppresses cation mixing, in which Ni atoms are mixed into the Li sites in the resulting lithium transition metal composite oxide, and prevents deterioration of the battery characteristics of the secondary battery.

[0115] The calcination time is preferably 1 hour or more because the temperature in the calcination vessel can be made uniform and the reaction can proceed uniformly. Moreover, even if the calcination is performed for a time longer than 24 hours, no significant change is observed in the obtained lithium transition metal composite oxide, so from the viewpoint of energy efficiency, the calcination time is preferably 24 hours or less.

[0116] In addition, if slight sintering is observed in the lithium transition metal composite oxide obtained after the lithium transition metal composite oxide synthesis step S3, a crushing treatment may be added. By crushing, the average particle size and particle size distribution of the obtained positive electrode active material can be adjusted to a suitable range. In addition, crushing refers to an operation of inputting mechanical energy into an aggregate of multiple secondary particles generated by sintering necking between secondary particles during firing, separating the secondary particles themselves almost without destroying them, and loosening the aggregates.

[0117] <2-4. Covering process S4> In the coating step S4, a coating layer containing a lithium niobium compound is formed on at least a part of the surface of the particles of the lithium transition metal composite oxide obtained in the lithium transition metal composite oxide synthesis step S3.

[0118] In the coating process S4, first, the specific surface area of ​​the lithium transition metal composite oxide obtained in the lithium transition metal composite oxide synthesis process S3 is measured, and a liquid coating agent can be prepared according to the target niobium loading in the coating layer (coating agent preparation step).

[0119] In the coating agent preparation step, a coating agent containing a niobium compound and a lithium compound is prepared. By using a coating agent containing a niobium compound and a lithium compound, a coating layer containing a lithium niobium compound can be generated in a heat treatment step described later. The surface of the lithium transition metal composite oxide particles can be uniformly coated with the coating layer. Note that it is also possible to use a niobium compound as a coating agent, add a lithium compound after a drying step described later, and perform a heat treatment step described later, but there is a possibility that the lithium compound may peel off during the heat treatment step.

[0120] The coating agent is not particularly limited as long as it contains niobium, a niobium compound, and a lithium compound. For uniform coating, a coating agent in which a niobium compound and a lithium compound are dissolved in a solvent, or a niobium compound and a lithium compound having a low melting point that are liquid at room temperature or melted by low-temperature heat treatment can be preferably used.

[0121] Examples of the niobium compound include at least one selected from alkoxides such as niobium ethoxide, niobium pentaisopropoxide, and niobium pentabutoxide, and niobium oxide sol aqueous solutions in which fine particles of niobium oxide are uniformly dispersed in an aqueous solution. The lithium compound is not particularly limited, and examples thereof include lithium hydroxide, lithium oxide, lithium nitrate, lithium ethoxide, lithium acetate, lithium formate, lithium chloride, lithium sulfate, lithium carbonate, and mixtures thereof. As the coating agent, a mixture of a lithium hydroxide aqueous solution in a niobium oxide sol can be preferably used, which can be more easily prepared and can further suppress the inclusion of impurities.

[0122] In the coating agent preparation step, it is preferable to adjust the amount of the niobium compound and the lithium compound added so that the Li / Nb substance ratio of the lithium niobium compound in the coating layer is 0.3 or more and 3.0 or less. By setting the Li / Nb substance ratio of the lithium niobium compound in the coating layer to 0.3 or more, a lithium niobium compound with high lithium ion conductivity is generated, which is preferable. In addition, by setting the Li / Nb substance ratio of the lithium niobium compound in the coating layer to 3.0 or less, the amount of unreacted lithium compound can be reduced, and deterioration of battery characteristics such as a decrease in initial discharge capacity and an increase in positive electrode resistance can be suppressed. In addition, by setting the Li / Nb substance ratio of the lithium niobium compound in the coating layer to 0.3 or more and 3.0 or less, the cycle characteristics can be further improved, the swelling of the battery can be further reduced, the initial discharge capacity can be further increased, and the internal resistance can be further reduced.

[0123] In the coating step S4, the lithium transition metal composite oxide particles and the coating agent can be mixed. A general mixer can be used for mixing (mixture preparation step). After mixing, the mixture is dried (drying step), and further heat-treated to fix the lithium niobium compound as a coating layer (heat treatment step).

[0124] In the drying step, drying can be performed at a temperature at which the solvent of the coating agent can be removed, for example, at 80°C or higher and lower than 300°C.

[0125] The heat treatment conditions in the heat treatment step are not particularly limited, but it is preferable to perform the heat treatment in an oxygen atmosphere for 1 hour to 5 hours at a temperature of 200° C. to 500° C., more preferably 300° C. to 450° C. After the heat treatment, the mixture is cooled to room temperature to obtain the final product, which is a positive electrode active material that is a lithium transition metal composite oxide particle having a coating layer.

[0126] The oxygen concentration in the oxygen atmosphere during the heat treatment is preferably 80% by volume or more. By setting the oxygen concentration in the oxygen atmosphere during the heat treatment to 80% by volume or more, it is possible to particularly suppress the occurrence of oxygen defects in the obtained positive electrode active material, which is preferable. Since the oxygen atmosphere can also be used, the upper limit of the oxygen concentration in the oxygen atmosphere can be 100% by volume.

[0127] The calcination temperature during the heat treatment is preferably 200°C or higher, since it can particularly suppress the impurities contained in the coating agent from remaining in the positive electrode active material, and the niobium compound in the coating layer reacts with the lithium compound to exist as a lithium niobium compound. In addition, it is preferable to set the calcination temperature to 500°C or lower, since it can suppress the components of the coating layer from being excessively diffused and maintain the shape of the coating layer. It is preferable to select the calcination temperature during the heat treatment so that the coating layer can sufficiently maintain its thickness according to the target amount of niobium carried in the coating layer, etc.

[0128] By setting the calcination time of the heat treatment to 1 hour or more, it is possible to particularly suppress the impurities contained in the coating agent from remaining in the positive electrode active material, which is preferable. Moreover, since no significant change is observed in the obtained positive electrode active material even if the calcination is performed for a time longer than 5 hours, it is preferable to set the calcination time to 5 hours or less from the viewpoint of energy efficiency.

[0129] When slight sintering is observed in the positive electrode active material obtained after the coating step S4, a crushing treatment may be added.

[0130] As described above, according to the method for producing a positive electrode active material for a lithium ion secondary battery according to one embodiment of the present invention, it is possible to provide a positive electrode active material for a lithium ion secondary battery that has excellent cycle characteristics and generates little gas during charging and discharging.

[0131] <3. Lithium-ion secondary battery> Next, a configuration example of the lithium ion secondary battery of this embodiment will be described. The lithium ion secondary battery of this embodiment (hereinafter, also simply referred to as "secondary battery") can have a configuration including a positive electrode using the above-mentioned positive electrode active material, a negative electrode, a separator, and a non-aqueous electrolyte. Each member of the secondary battery of this embodiment will be described below. Note that the embodiment described below is merely an example, and the lithium ion secondary battery of the present invention can be embodied in a form in which various changes and improvements are made based on the embodiment described in this specification and on the knowledge of a person skilled in the art. In addition, the lithium ion secondary battery of the present invention is not particularly limited in its use.

[0132] <3-1. Positive electrode> The positive electrode is a sheet-like member, and can be formed, for example, by applying a positive electrode mixture paste containing the above-mentioned positive electrode active material to the surface of a current collector made of, for example, aluminum foil, and drying it. The positive electrode can also be formed by molding the positive electrode mixture. The positive electrode is appropriately processed according to the battery to be used. For example, a cutting process to form the positive electrode into an appropriate size according to the target battery, or a pressurized compression process using a roll press or the like to increase the electrode density can be performed.

[0133] The above-mentioned positive electrode mixture paste can be formed by adding a solvent to the positive electrode mixture as necessary and kneading the mixture. The positive electrode mixture can be formed by mixing the above-mentioned powdered positive electrode active material, a conductive agent, and a binder.

[0134] The conductive agent is added to the electrode to give it suitable electrical conductivity. The material of the conductive agent is not particularly limited, but examples of the conductive agent include graphite such as natural graphite, artificial graphite, and expanded graphite, and carbon black materials such as acetylene black and Ketjen Black (registered trademark).

[0135] The binder plays a role of binding the positive electrode active material. The binder used in the positive electrode mixture is not particularly limited, but may be one or more selected from the group consisting of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene butadiene, cellulose-based resin, polyacrylic acid, and the like.

[0136] In addition, activated carbon or the like can be added to the positive electrode mixture. By adding activated carbon or the like to the positive electrode mixture, the electric double layer capacity of the positive electrode can be increased.

[0137] The solvent has a function of dissolving the binder and dispersing the positive electrode active material, the conductive agent, the activated carbon, etc. in the binder. The solvent is not particularly limited, but an organic solvent such as N-methyl-2-pyrrolidone can be used.

[0138] The mixing ratio of each material in the positive electrode mixture paste is not particularly limited, and may be the same as that of the positive electrode of a general lithium ion secondary battery. For example, when the solid content of the positive electrode mixture excluding the solvent is 100 parts by mass, the content of the positive electrode active material may be 60 parts by mass or more and 95 parts by mass or less, the content of the conductive agent may be 1 part by mass or more and 20 parts by mass or less, and the content of the binder may be 1 part by mass or more and 20 parts by mass or less.

[0139] However, the method for producing the positive electrode is not limited to the above-mentioned example, and other methods may be used.

[0140] <3-2. Negative electrode> The negative electrode is a sheet-like member formed by applying a negative electrode mixture paste to the surface of a metal foil current collector such as copper and drying it. The negative electrode can also be a sheet-like member made of a material containing lithium, such as metallic lithium.

[0141] Although the components constituting the negative electrode mixture paste and their composition, the material of the current collector, etc. are different, the negative electrode is formed in substantially the same manner as the above-mentioned positive electrode, and various treatments are performed as necessary in the same manner as the positive electrode.

[0142] The negative electrode mixture paste can be prepared by adding a suitable solvent to a negative electrode mixture obtained by mixing a negative electrode active material and a binder to form a paste. For example, a substance containing lithium such as metallic lithium or a lithium alloy, or an occlusion substance capable of releasing and occluding lithium ions can be used as the negative electrode active material.

[0143] The storage material is not particularly limited, and may be one or more selected from, for example, natural graphite, artificial graphite, organic compound sintered bodies such as phenolic resin, and powders of carbon materials such as coke. When such a storage material is used as the negative electrode active material, a fluorine-containing resin such as PVDF may be used as the binder, as in the case of the positive electrode, and an organic solvent such as N-methyl-2-pyrrolidone may be used as the solvent for dispersing the negative electrode active material in the binder.

[0144] <3-3. Separator> The separator is sandwiched between the positive electrode and the negative electrode, and has the function of separating the positive electrode and the negative electrode and retaining the electrolyte. The material of the separator may be, for example, a thin membrane such as polyethylene or polypropylene having a large number of fine pores, but is not particularly limited as long as it has the above function.

[0145] <3-4. Non-aqueous electrolyte> A non-aqueous electrolyte can be used as the non-aqueous electrolyte. For example, the non-aqueous electrolyte may be a solution in which a lithium salt as a supporting salt is dissolved in an organic solvent. Alternatively, the non-aqueous electrolyte may be a solution in which a lithium salt is dissolved in an ionic liquid. The ionic liquid refers to a salt that is composed of cations and anions other than lithium ions and is liquid even at room temperature.

[0146] The organic solvent may be one selected from cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and trifluoropropylene carbonate; chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane; sulfur compounds such as ethyl methyl sulfone and butane sultone; and phosphorus compounds such as triethyl phosphate and trioctyl phosphate. These may be used alone or in combination of two or more.

[0147] Examples of the supporting salt that can be used include LiPF6, LiBF4, LiClO4, LiAsF6, LiN(CF3SO2)2, and composite salts thereof. The non-aqueous electrolyte may contain a radical scavenger, a surfactant, a flame retardant, etc., in order to improve the battery characteristics.

[0148] The non-aqueous electrolyte may be a solid electrolyte. The solid electrolyte has a property of being able to withstand high voltage. Examples of the solid electrolyte include inorganic solid electrolytes and organic solid electrolytes.

[0149] As the inorganic solid electrolyte, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or the like is used.

[0150] The oxide-based solid electrolyte is not particularly limited, and any oxide-based solid electrolyte that contains oxygen (O) and has lithium ion conductivity and electronic insulation properties can be used. Examples of oxide-based solid electrolytes include lithium phosphate (Li3PO4), Li3PO4NX , LiBON X , LiNbO3, LiTaO3, Li2SiO3, Li4SiO4-Li3PO4, Li4SiO4-Li3VO4, Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3-ZnO, Li 1+X Al X Ti 2-X (PO4)3(0≦X≦1), Li 1+X Al X Ge 2-X (PO4)3(0≦X≦1), LiTi2(PO4)3, Li 3X La 2 / 3-X TiO3(0≦X≦2 / 3), Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6BaLa2Ta2O 12 , Li 3.6 S 0.6 P 0.4 Examples include O4.

[0151] The sulfide-based solid electrolyte is not particularly limited, and any electrolyte that contains sulfur (S) and has lithium ion conductivity and electronic insulation can be used. Examples of sulfide-based solid electrolytes include Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, LiI-Li2S-P2O5, and LiI-Li3PO4-P2S5.

[0152] As the inorganic solid electrolyte, materials other than those mentioned above may be used, for example, Li3N, LiI, Li3N-LiI-LiOH, etc. may be used.

[0153] The organic solid electrolyte is not particularly limited as long as it is a polymer compound exhibiting ion conductivity, and examples of the organic solid electrolyte that can be used include polyethylene oxide, polypropylene oxide, copolymers thereof, etc. The organic solid electrolyte may also contain a supporting salt (lithium salt).

[0154] <3-5. Shape and composition of secondary batteries> Next, an example of the arrangement and configuration of the components of the secondary battery of this embodiment will be described. The secondary battery of this embodiment, which is composed of the positive electrode, negative electrode, separator, and non-aqueous electrolyte described above, can be made into various shapes, such as a cylindrical shape or a laminated shape. In any shape, the positive electrode and the negative electrode can be laminated via a separator to form an electrode body, and the obtained electrode body can be impregnated with a non-aqueous electrolyte. Then, the positive electrode current collector and the positive electrode terminal leading to the outside, and the negative electrode current collector and the negative electrode terminal leading to the outside can be connected using a current collecting lead or the like, and the battery case can be sealed to form a secondary battery.

[0155] The secondary battery of this embodiment using the above-described positive electrode active material can be a secondary battery with excellent cycle characteristics and little swelling of the battery.

[0156] Specifically, a 2032-type coin battery is constructed using the positive electrode active material of this embodiment as a positive electrode, and the current density is 0.13 mA / cm 2 The initial discharge capacity, which is the discharge capacity when the battery is charged to a cut-off voltage of 4.3 V, rested for one hour, and then discharged to a cut-off voltage of 3.0 V, is preferably 190 mAh / g or more, and more preferably 198 mAh / g or more.

[0157] The cycle characteristics are evaluated by the capacity retention rate. The capacity retention rate can be evaluated, for example, by the following procedure. For example, a laminated battery is constructed using a sheet formed by applying a negative electrode mixture paste, which is a mixture of graphite powder and polyvinylidene fluoride, to copper foil as the negative electrode. Then, the laminated battery is charged in a thermostatic chamber maintained at 25° C. with a current density of 0.33 mA / cm. 2 The battery was conditioned by charging it to a cut-off voltage of 4.3 V, resting for 1 hour, and discharging it to a cut-off voltage of 3.0 V for 5 cycles. Next, the ... 2The battery was charged to a cut-off voltage of 4.3 V, rested for one hour, and then discharged to a cut-off voltage of 3.0 V. This cycle was repeated 200 times.

[0158] The capacity retention rate can be calculated by dividing the discharge capacity obtained in the 200th cycle by the discharge capacity obtained in the first cycle after conditioning.

[0159] Furthermore, the secondary battery of this embodiment using the above-mentioned positive electrode active material preferably has a capacity retention rate of 80% or more, and more preferably 90% or more.

[0160] The swelling of the battery can be evaluated by the thickness of the laminated battery after the high voltage retention test. A laminated battery with the same structure as the cycle test was conditioned and the current was 0.27 mA / cm up to 4.3 V. 2 The battery is charged at 4.3V and charging is continued until the current value drops to 1 / 10 while maintaining the voltage at 4.3V. After the battery is charged, it is kept at 60°C for 3 days, and then returned to room temperature. The battery is then sandwiched between SUS plates so that 10mm of the short side of the battery protrudes, and the SUS plates are pressed with 3.9kN. The thickness of the center of the part of the battery protruding from the SUS plates can be regarded as the degree of battery expansion.

[0161] In addition, in the secondary battery of this embodiment using the above-mentioned positive electrode active material, the battery swelling is preferably 0.18 mm or less, and more preferably 0.15 mm or less.

[0162] The positive electrode resistance of a battery can be evaluated by measuring the positive electrode resistance using a coin-type battery. An example of a method for measuring the positive electrode resistance is as follows. When the frequency dependence of the battery reaction is measured using the AC impedance method, which is a common electrochemical evaluation method, a Nyquist diagram based on the solution resistance, the negative electrode resistance and negative electrode capacity, and the positive electrode resistance and positive electrode capacity is obtained. The battery reaction at the electrode consists of a resistance component associated with charge transfer and a capacity component due to the electric double layer, and when these are represented by an electric circuit, they become a parallel circuit of resistance and capacity, and the entire battery is represented by an equivalent circuit in which the solution resistance and the parallel circuits of the negative electrode and positive electrode are connected in series. A fitting calculation is performed on the Nyquist diagram measured using this equivalent circuit, and each resistance component and capacity component can be estimated. The positive electrode resistance is equal to the diameter of the semicircle on the low frequency side of the obtained Nyquist diagram. Therefore, the positive electrode resistance can be estimated by performing an AC impedance measurement on the positive electrode and performing a fitting calculation on the obtained Nyquist diagram using an equivalent circuit.

[0163] In addition, the secondary battery of this embodiment using the above-mentioned positive electrode active material preferably has a positive electrode resistance of less than 4.0Ω, and more preferably less than 3.0Ω.

[0164] The use of the secondary battery of this embodiment is not particularly limited, and it can be suitably used in applications requiring various power sources. Since the secondary battery of this embodiment has the above characteristics, it can be suitably used as a power source for small portable electronic devices (such as notebook personal computers and mobile phone terminals) that always require high cycle characteristics and high capacity. In addition, since the secondary battery of this embodiment has excellent cycle characteristics and can be miniaturized, it is also suitable as a power source for electric vehicles that are repeatedly charged and discharged and are subject to mounting space restrictions. EXAMPLES

[0165] Next, the positive electrode active material for a lithium ion secondary battery according to one embodiment of the present invention, the manufacturing method thereof, and the lithium ion secondary battery will be described in detail with reference to examples. Note that the present invention is not limited to these examples. Note that the analysis method of the metal contained in the positive electrode active material and the various evaluation methods of the positive electrode active material in the examples and comparative examples are as follows.

[0166] [Example 1] 1. Preparation of Lithium Transition Metal Composite Oxide Particles The positive electrode active material was produced by carrying out the following steps.

[0167] (a) Precursor crystallization step First, 2.5 L of pure water was placed in a reaction tank (5 L) and the temperature inside the tank was set to 40° C. while stirring. At this time, the inside of the reaction tank was kept in a nitrogen atmosphere with an oxygen concentration of 1% by volume or less. An initial aqueous solution was prepared by adding an appropriate amount of 25% by mass sodium hydroxide aqueous solution and 25% by mass ammonia water to the water in the reaction tank so that the pH value was 11.5 at a liquid temperature of 25° C. and the ammonia concentration was 5 g / L (initial aqueous solution preparation step).

[0168] At the same time, nickel sulfate, cobalt sulfate, and aluminum sulfate were dissolved in pure water so that the mass ratio of nickel, cobalt, and aluminum was Ni:Co:Al=0.82:0.15:0.03, to prepare a 2.0 mol / L mixed aqueous solution (mixed aqueous solution preparation step).

[0169] This mixed aqueous solution was added dropwise at a constant rate to the initial aqueous solution in the reaction tank to obtain a reaction aqueous solution. At this time, 25% by mass ammonia water and 25% by mass sodium hydroxide aqueous solution were also added dropwise at a constant rate to the initial aqueous solution to control the pH value of the reaction aqueous solution to 11.5 at a liquid temperature of 25°C and the ammonia concentration to 5 g / L. Through this operation, transition metal composite hydroxide particles (hereinafter referred to as "composite hydroxide particles"), which are precursors of lithium transition metal composite oxides, were crystallized (crystallization step).

[0170] Thereafter, the slurry containing the composite hydroxide particles was collected from an overflow port provided in the reaction tank, filtered, and water-soluble impurities were removed by washing with ion-exchanged water. The slurry was then dried to obtain powdered composite hydroxide particles.

[0171] (b) Oxidation roasting process The composite hydroxide particles thus prepared were calcined in an atmospheric calcination furnace (BM-50100M, manufactured by Siliconit Corporation) in an air atmosphere with an oxygen concentration of 20% by volume at 600°C for 2 hours, and then cooled to room temperature to obtain transition metal composite oxide particles.

[0172] (c) Lithium transition metal composite oxide synthesis process Lithium hydroxide monohydrate was weighed out so that the ratio of the amount of lithium to the total amount of nickel, cobalt, and aluminum contained in the transition metal composite oxide particles was 1.02, and mixed using a Turbula shaker mixer (T2F, manufactured by Dalton Co., Ltd.) to obtain a lithium mixture (lithium mixture preparation step).

[0173] The lithium mixture was placed in an alumina sagger and calcined in an atmosphere calcination furnace (BM-50100M, manufactured by Siliconit Co., Ltd.) at 750°C for 10 hours in an oxygen atmosphere with an oxygen concentration of 90% by volume or more, and then cooled to room temperature (calcination step). This produced lithium transition metal composite oxide particles.

[0174] 2. Characterization of Lithium Transition Metal Composite Oxide Particles The resulting lithium transition metal composite oxide particles were subjected to the following evaluations.

[0175] (a) Composition Quantitative analysis using an ICP optical emission spectrometer (VARIAN, 725ES) confirmed that the lithium transition metal composite oxide had a mass ratio of Li, Ni, Co, and Al expressed as Li:Ni:Co:Al=1.02:0.82:0.15:0.03.

[0176] (b) Crystal structure The crystal structure of the lithium transition metal composite oxide particles was measured using XRD (X'Pert, PROMRD, manufactured by PANALYTICAL Corporation), and it was confirmed that the crystal structure was a layered rock salt type, with peaks belonging to the R-3m structure detected in the diffraction pattern.

[0177] (c) Specific surface area The BET specific surface area of ​​the lithium transition metal composite oxide particles was measured using a fully automatic BET specific surface area measuring device (Maxsorb, manufactured by Mountec Co., Ltd.). 2 / g.

[0178] (d) Volume average particle size The volume average particle size of the lithium transition metal composite oxide particles was measured using a laser diffraction scattering type particle size distribution measuring device (Microtrack HRA, manufactured by Nikkiso Co., Ltd.) and was found to be 6.6 μm.

[0179] 3. Manufacturing of positive electrode active material The lithium transition metal composite oxide particles were subjected to the following coating process to manufacture a positive electrode active material. The total surface area of ​​the total weight of the lithium transition metal composite oxide particles, which are the particles to be coated, was calculated from the specific surface area of ​​the lithium transition metal composite oxide particles. 1.35 g of lithium hydroxide, weighed out so that the mass ratio (Li / Nb) of Li to Nb in the lithium niobium compound of the coating layer was 1, was added to 105 mL of pure water and stirred to dissolve the lithium hydroxide. Next, a 1 m2 coating was applied to the total surface area. 2 114 g of niobium oxide sol (manufactured by Taki Chemical Industry Co., Ltd., product name: Baylar Nb-G6000) weighed out so that the amount of niobium per unit weight was 0.16 mmol was added to and mixed with the lithium hydroxide aqueous solution (coating agent preparation step).

[0180] 500 g of lithium transition metal composite oxide particles were placed in a rolling fluidized coating device (Powrex Corporation, model: FP-MP-01D), the supply air temperature was set to 120°C, and the coating agent was added at a rate of 2.6 μL / min per 1 g of lithium transition metal composite oxide particles for 170 minutes, followed by drying while mixing (mixture preparation step and drying step).

[0181] Using a small electric furnace (manufactured by Nitto Kagaku Co., Ltd., model: NHK-170AF), heat treatment was performed for 2 hours at 230°C in an oxygen atmosphere with an oxygen concentration of 95% by volume (heat treatment step). After that, it was cooled to room temperature to obtain particles of lithium transition metal composite oxide having a coating layer as a positive electrode active material.

[0182] 4. Evaluation of positive electrode active material The positive electrode active material thus obtained was evaluated as follows.

[0183] (a) Composition Analysis using an ICP emission spectrometer (VARIAN, 725ES) revealed that this positive electrode active material contained 0.99 mass% Nb, and a comparison with the specific surface area before and after the coating treatment revealed that the amount of niobium supported in the coating layer was 0.16 mmol / m 2 It was found to be.

[0184] (b) Surface analysis The obtained positive electrode active material was measured using XPS (Versa Probe II, manufactured by ULVAC-PHI). 2 P 3 / 2 Spectrum, Co 2 P 3 / 2 The amount of substance on the surface of the positive electrode active material was obtained from the semi-quantitative value calculated from the peak areas of the Nb3d spectrum and the Nb3d spectrum, and together with the results of the composition analysis described above, it was found that the ratio of the amount of Nb present on the surface to the sum of the amounts of Ni, Co, and Nb (Nbs / Nis+Cos+Nbs) was 0.85.

[0185] (c) Carbon content The carbon content of the obtained positive electrode active material was measured by a high-frequency combustion infrared absorption method using a carbon analyzer (manufactured by LECO, model: CS-600) and found to be 0.20 mass %.

[0186] (d) Moisture content The moisture content of the obtained positive electrode active material was measured using a Karl Fischer moisture meter (manufactured by Kyoto Electronics Manufacturing Co., Ltd., Model: MKC210) at a heating temperature of 300° C., and was found to be 0.08% by mass.

[0187] 5. Fabrication of Secondary Batteries To evaluate the capacity of the obtained positive electrode active material, a 2032 type coin battery 10 (hereinafter referred to as a "coin battery") shown in Fig. 2 was used. The coin battery 10 is composed of a case 11 and an electrode 12 housed in the case 11.

[0188] Case 11 has a hollow positive electrode can 111 with one end open, and a negative electrode can 112 placed in the opening of positive electrode can 111, and is configured so that when negative electrode can 112 is placed in the opening of positive electrode can 111, a space for accommodating electrode 12 is formed between negative electrode can 112 and positive electrode can 111.

[0189] Electrode 12 is composed of positive electrode 121, separator 122, and negative electrode 123, which are laminated in this order, and housed in case 11 so that positive electrode 121 contacts the inner surface of positive electrode can 111, and negative electrode 123 contacts the inner surface of negative electrode can 112. Case 11 is provided with gasket 113, which prevents relative movement between positive electrode can 111 and negative electrode can 112 and maintains a non-contact state between them.

[0190] Gasket 113 also has the function of sealing the gap between positive electrode can 111 and negative electrode can 112 to provide airtight and liquid-tight insulation between the inside of case 11 and the outside. Such a coin battery 10 was produced as follows.

[0191] First, 20.0 g of the obtained positive electrode active material, 2.35 g of acetylene black, and 1.18 g of polyvinylidene fluoride were dispersed in N-methyl-2-pyrrolidone (NMP) to form a slurry. The slurry was then spread over an Al foil to a thickness of 1 cm. 2 After applying the positive electrode active material so that 5.0 mg was present per foil, the foil was dried in the air at 120° C. for 30 minutes to remove the NMP. The Al foil to which the positive electrode active material was applied was cut into a strip of 66 mm in width and roll-pressed with a load of 1.2 t to prepare a positive electrode 121. The positive electrode 121 was punched into a circle of 13 mm in diameter and dried in a vacuum dryer at 120° C. for 12 hours.

[0192] Next, a coin-type battery 10 was produced using the positive electrode 121 in a glove box in an Ar atmosphere with a dew point controlled at −80° C. In this case, for the negative electrode 123, a lithium foil punched into a disk shape with a diameter of 14 mm was used.

[0193] For the evaluation of cycle characteristics and battery expansion, a laminate type battery 100 shown in Fig. 3 was used. Such a laminate type battery 100 was fabricated as follows.

[0194] A positive electrode was prepared in the same manner as the coin-type battery 10, cut into a rectangle of 50 mm × 30 mm, and dried in a vacuum dryer at 120 ° C. for 12 hours. Next, a laminated battery 100 was prepared using the positive electrode 110 in a dry room controlled at a dew point of -80 ° C. In this case, a negative electrode sheet was used for the negative electrode 120, in which a negative electrode mixture paste, which is a mixture of graphite powder with an average particle size of about 20 μm and polyvinylidene fluoride, was applied to copper foil.

[0195] A 25 μm-thick polyethylene porous film was used for the separator 130, and a 3:7 mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) with 1 M LiPF6 as the supporting electrolyte (manufactured by Toyama Pharmaceutical Co., Ltd.) was used for the electrolyte. The laminated battery 100 was then sealed with a laminate film 140 to complete the battery.

[0196] 6. Evaluation of secondary batteries The performance of the produced secondary batteries, which indicate the initial discharge capacity, the positive electrode resistance, the cycle characteristics, and the swelling of the battery, were evaluated as follows.

[0197] (a) Initial discharge capacity The initial discharge capacity was measured by leaving the coin-type battery with lithium foil as the negative electrode for about 24 hours and applying a current density of 0.13 mA / cm to the positive electrode after the open circuit voltage (OCV) had stabilized. 2 The battery was evaluated by charging it to a cut-off voltage of 4.3 V, resting for 1 hour, and then measuring the discharge capacity (initial discharge capacity) when it was discharged to a cut-off voltage of 3.0 V. The measurement result was 199 mAh / g.

[0198] (b) Cycle characteristics The cycle characteristics were evaluated by measuring the capacity retention rate after 200 charge / discharge cycles. Specifically, a laminated battery using a negative electrode made of a sheet in which a mixture of graphite powder and polyvinylidene fluoride was applied to copper foil was first placed in a thermostatic chamber maintained at 25°C and charged at a current density of 0.33 mA / cm. 2 The battery was conditioned by repeating five cycles of charging to a cut-off voltage of 4.3 V, resting for one hour, and discharging to a cut-off voltage of 3.0 V. Next, the battery was placed in a thermostatic chamber maintained at 60°C, and discharged at a current density of 2.7 mA / cm 2 The battery was charged to a cut-off voltage of 4.3 V, and after a one-hour rest, discharged to a cut-off voltage of 3.0 V. This cycle was repeated 200 times, and the discharge capacity after each cycle was measured and evaluated.

[0199] The capacity retention rate, which is the ratio of the discharge capacity obtained in the first cycle after conditioning of the laminated battery of Example 1 divided by the discharge capacity obtained in the 200th cycle after conditioning, was 80%.

[0200] (c) Battery swelling The battery swelling was evaluated by measuring the thickness of the laminated battery after a high-voltage retention test. Specifically, after conditioning a laminated battery with the same structure as in the cycle test, the battery was charged to 0.27 mA / cm up to 4.3 V. 2 The battery was charged at 1000V and continued to be charged until the current value was 1 / 10 while being held at 4.3V. The charged battery was held at 60°C for 3 days. The battery was then returned to room temperature, sandwiched between SUS plates so that 10 mm of the short side of the battery protruded, and the SUS plates were pressed with 3.9 kN. The thickness of the center of the part of the battery protruding from the SUS plates was measured with a dial gauge and was taken as the degree of expansion of the battery. The expansion of the battery after the retention test of the laminated battery of Example 1 was 0.12 mm.

[0201] (d) Positive electrode resistance In addition, when the positive electrode resistance is measured by an AC impedance method using a frequency response analyzer and a potentiogalvanostat (Solartron, 1255B) while charging the coin battery 10 at a charging potential of 4.1 V, the Nyquist plot shown in FIG. 4 is obtained. This Nyquist plot is expressed as the sum of characteristic curves showing the solution resistance, the negative electrode resistance and its capacity, and the positive electrode resistance and its capacity, so fitting calculations were performed using an equivalent circuit based on this Nyquist plot to calculate the value of the positive electrode resistance. The measured result of the positive electrode resistance was 3.1 Ω.

[0202] [Example 2] When carrying out the coating process of "3. Production of positive electrode active material", the heat treatment temperature was set to 300°C in the heat treatment step, and the same conditions were used as in Example 1 to obtain lithium transition metal composite oxide particles, a positive electrode active material, and a secondary battery using the positive electrode active material.

[0203] [Example 3] When carrying out the coating process of “3. Production of positive electrode active material”, the heat treatment temperature was set to 380° C. in the heat treatment step, and other conditions were the same as those in Example 1 to obtain lithium transition metal composite oxide particles, a positive electrode active material, and a secondary battery using the positive electrode active material.

[0204] [Example 4] When carrying out the coating process of “3. Production of positive electrode active material”, the heat treatment temperature was set to 450° C. in the heat treatment step, and other conditions were the same as those in Example 1 to obtain lithium transition metal composite oxide particles, a positive electrode active material, and a secondary battery using the positive electrode active material.

[0205] [Comparative Example 1] A lithium transition metal composite oxide particle, a positive electrode active material, and a secondary battery using the positive electrode active material were obtained under the same conditions as in Example 1, except that the coating step in Example 1 was not performed. Since the coating step was not performed, the lithium transition metal composite oxide particle obtained in "1. Production of lithium transition metal composite oxide particles" serves as the positive electrode active material.

[0206] [Comparative Example 2] When carrying out the coating process of "3. Production of positive electrode active material", lithium transition metal composite oxide particles, a positive electrode active material, and a secondary battery using the positive electrode active material were obtained under the same conditions as in Example 1, except that the lithium hydroxide aqueous solution was not mixed in the coating agent preparation step.

[0207] Table 1 shows the BET specific surface area and volume average particle diameter of the lithium transition metal composite oxide particles before the coating step, the niobium loading in the coating layer, the ratio of the amount of Nb present on the surface of the positive electrode active material to the sum of the amounts of Ni, Co, and Nb (Nbs / Nis+Cos+Nbs), the carbon content of the positive electrode active material, the water content of the positive electrode active material, and the heat treatment temperature conditions in the heat treatment step in the examples and comparative examples.

[0208] [Table 1]

[0209] Here, the amount of niobium supported in the coating layer is determined based on the niobium content (mass%) in the positive electrode active material, the atomic weight of niobium, and the BET specific surface area (0.66 m) of the particles of the lithium transition metal composite oxide described above. 2 / g).

[0210] It is clear from Table 1 that Comparative Example 1 is a condition in which no coating layer exists on the lithium transition metal composite oxide particles, and Comparative Example 2 is a condition in which the coating layer contains insufficient lithium.

[0211] Table 2 shows the measurement results of the substance ratio of lithium to niobium (Li / Nb) in the coating layer, the initial discharge capacity of the secondary battery, the capacity retention rate, the battery swelling, and the positive electrode resistance in the examples and comparative examples.

[0212] [Table 2]

[0213] Here, the substance ratio of lithium to niobium (Li / Nb) in the coating layer was calculated from the amount of niobium and the amount of lithium added in the coating agent preparation step of the coating process.

[0214] The initial discharge capacity of the secondary batteries of Examples 1, 2, 3, and 4 was higher than that of Comparative Example 2. This is believed to be because the surface of the positive electrode active material was sufficiently coated with a lithium niobium compound, thereby improving the lithium ion conductivity. In Comparative Example 1, the initial discharge capacity was equivalent to that of the Examples, but the capacity retention rate was smaller than that of the Examples, and the swelling of the battery was larger than that of the Examples. From this, it was found that the cycle characteristics could be improved and the swelling of the battery could be suppressed by providing a coating layer.

[0215] Although the embodiments and examples of the present invention have been described in detail above, those skilled in the art will easily understand that many modifications are possible without substantially departing from the novel features and effects of the present invention. Therefore, all such modifications are intended to be included within the scope of the present invention.

[0216] For example, a term described at least once in the specification or drawings together with a different term having a broader or similar meaning can be replaced with that different term anywhere in the specification or drawings. The positive electrode active material for a lithium ion secondary battery, the manufacturing method thereof, and the configuration and operation of the lithium ion secondary battery are not limited to those described in the embodiments and examples of the present invention, and various modifications are possible. [Explanation of symbols]

[0217] S1 precursor crystallization process, S2 oxidation roasting process, S3 lithium transition metal composite oxide synthesis process, S4 coating process, 10 coin battery, 11 case, 12 electrode, 111 positive electrode can, 112 negative electrode can, 113 gasket, 121 positive electrode, 122 separator, 123 negative electrode, 100 laminated battery, 110 positive electrode, 120 negative electrode, 130 separator, 140 laminate film

Claims

1. A positive electrode active material for a lithium ion secondary battery comprising particles of a lithium transition metal composite oxide and a coating layer that coats at least a portion of the surface of the particles, a substance amount ratio Li:Ni:Co:M of components other than oxygen in the lithium transition metal composite oxide is expressed by t:1-x-y:x:y (wherein M is at least one element selected from the group consisting of Mg, Al, Ca, Si, Mn, Ti, V, Fe, Cu, Cr, Zn, Zr, Nb, Mo, and W, and 0.95≦t≦1.20, 0<x≦0.22, and 0≦y≦0.15); The coating layer contains a lithium niobium compound, The surface area of ​​the lithium transition metal composite oxide excluding the coating layer is 1 m 2 a Nb content in the coating layer is 0.14 mmol or more and 0.29 mmol or less per unit area.

2. 2. The positive electrode active material for lithium ion secondary batteries according to claim 1, wherein the ratio Nbs / (Nis+Cos+Nbs) of the amount of Nb present on the surface of the positive electrode active material for lithium ion secondary batteries to the sum of the amounts of Ni, Co, and Nb, Nis+Cos+Nbs, is 0.70 or more and 0.97 or less.

3. The positive electrode active material for lithium ion secondary batteries according to claim 1 or 2, wherein the lithium transition metal composite oxide has a crystal structure belonging to the space group R-3m.

4. 3. The positive electrode active material for a lithium ion secondary battery according to claim 1, wherein the carbon content of the positive electrode active material for a lithium ion secondary battery is 0.05% by mass or more and 0.40% by mass or less.

5. 3. The positive electrode active material for lithium ion secondary batteries according to claim 1, wherein the amount of moisture, measured by a Karl Fischer method when the positive electrode active material is heated to 300° C., is 0.12% by mass or less relative to the entire positive electrode active material for lithium ion secondary batteries.

6. The specific surface area of ​​the lithium transition metal composite oxide particles is 0.1 m 2 / g or more 1.0m 2 The positive electrode active material for a lithium ion secondary battery according to claim 1 or 2, wherein the molecular weight of the positive electrode active material is 1000 or less.

7. 3. The positive electrode active material for a lithium ion secondary battery according to claim 1, wherein the volume average particle diameter of the particles of the lithium transition metal composite oxide is 2 μm or more and 20 μm or less.

8. A lithium ion secondary battery comprising at least a positive electrode using the positive electrode active material for lithium ion secondary batteries according to claim 1 or 2, a negative electrode, a separator, and a non-aqueous electrolyte.

9. A method for producing a positive electrode active material for a lithium ion secondary battery, the positive electrode active material having a lithium transition metal composite oxide particle and a coating layer that coats at least a part of the surface of the particle, comprising: a precursor crystallization step of preparing a transition metal composite hydroxide, which is a precursor of the lithium transition metal composite oxide, by a crystallization reaction; an oxidizing roasting step of oxidizing and roasting the transition metal composite hydroxide obtained in the precursor crystallization step to obtain a transition metal composite oxide; a lithium transition metal composite oxide synthesis step of mixing the transition metal composite oxide obtained in the oxidation roasting step with a lithium compound and calcining the mixture to obtain a lithium transition metal composite oxide; a coating step of forming the coating layer containing a lithium niobium compound on at least a part of the surface of the lithium transition metal composite oxide particles obtained in the lithium transition metal composite oxide synthesis step, The method for producing a positive electrode active material for a lithium ion secondary battery is characterized in that, in the coating step, the particles of the lithium transition metal composite oxide obtained in the lithium transition metal composite oxide synthesis step are mixed with a coating agent containing a lithium compound and a niobium compound, followed by drying and heat treatment.

10. 10. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 9, wherein the lithium transition metal composite oxide synthesis step comprises firing in an oxygen atmosphere at a temperature of 700° C. or more and 800° C. or less.

11. The coating step is performed in such a manner that the Nb content of the lithium niobium compound is equal to or larger than 1 m of the surface area of ​​the lithium transition metal composite oxide. 2 The niobium compound is added so that the amount per unit area is 0.14 mmol or more and 0.29 mmol or less, The lithium-ion secondary battery positive electrode active material according to claim 9 or 10, wherein the components other than oxygen of the lithium transition metal composite oxide obtained in the coating step are represented by Li:Ni:Co:M = t:1-x-y:x:y (wherein M is at least one element selected from the group consisting of Mg, Al, Ca, Si, Mn, Ti, V, Fe, Cu, Cr, Zn, Zr, Nb, Mo and W, and 0.95≦t≦1.20, 0<x≦0.22, 0≦y≦0.15), and the ratio Nbs / (Nis+Cos+Nbs) of the amount of substance Nb present on the surface of the lithium-ion secondary battery positive electrode active material to the sum of the amounts of substance Nis+Cos+Nbs of Ni, Co and Nb is 0.70 or more.

12. 11. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 9 or 10, wherein in the coating step, the lithium compound and the niobium compound are added so that a substance amount ratio (Li / Nb) of Li to Nb in the lithium niobium compound of the coating layer is 0.3 or more and 3.0 or less.

13. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 9 or 10, wherein the heat treatment is performed in an oxygen atmosphere at a temperature of 200° C. or more and 500° C. or less for 1 hour or more and 5 hours or less.

14. 11. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 9 or 10, characterized in that the coating agent contains a solution of the lithium compound and the niobium compound used in the coating step in a solvent, or a mixture of the lithium compound and the niobium compound that is liquid at room temperature or has a low melting point that melts during heat treatment in the coating step.

15. 11. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 9 or 10, wherein the niobium compound used in the coating step is at least one of niobium ethoxide, niobium pentaisopropoxide, niobium pentabutoxide, and niobium oxide.

Citation Information

Patent Citations

  • Positive electrode active material for all-solid lithium ion secondary battery, manufacturing method thereof, and all-solid lithium ion secondary battery

    JP2021103671A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, method for manufacturing the same, and nonaqueous electrolyte secondary battery

    JP2019046716A

  • Positive electrode active material for lithium ion battery, method for manufacturing the same, positive electrode for lithium ion battery and lithium ion battery

    JP2019139862A