Solar cell, multi-junction solar cell, solar cell module, and photovoltaic power generation system
The solar cell design with varying crystal grain sizes in the p-type light absorption layer enhances light absorption and electron transport, addressing efficiency and cost challenges in cuprous oxide-based cells by optimizing grain sizes through a two-stage sputtering process.
Patent Information
- Application Number
- JP2023046061
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
Existing solar cells, particularly those using cuprous oxide (Cu2O), face challenges in achieving high conversion efficiency and cost-effectiveness due to limitations in light absorption and electron transport properties.
A solar cell design with a p-type light absorption layer comprising distinct regions of varying crystal grain sizes, where the first region has larger grains and the second region has smaller grains, optimized through a two-stage sputtering process at different temperatures, enhances light absorption and electron transport.
This design improves the quantum efficiency and conversion efficiency of solar cells by extending the optical path length and reducing electron recombination, leading to higher current density and overall energy output.
Smart Images

Figure 2024135402000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a solar cell, a multi-junction solar cell, a solar cell module, and a photovoltaic power generation system. [Background technology]
[0002] One of the new solar cells is one that uses cuprous oxide (Cu2O) in the light absorption layer. Cu2O is a wide-gap semiconductor. Cu2O is a safe and inexpensive material made from copper and oxygen, which are abundant on Earth, and is therefore expected to realize highly efficient, low-cost solar cells. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-154171 A Summary of the Invention [Problem to be solved by the invention]
[0004] The problem to be solved by the present invention is to provide a solar cell, a multi-junction solar cell, a solar cell module, and a solar power generation system that are excellent in conversion efficiency. [Means for solving the problem]
[0005] The solar cell of the embodiment includes a p-electrode, an n-electrode, a p-type light absorbing layer provided on the p-electrode and including a first region and a second region, and an n-type layer provided between the p-type light absorbing layer and the n-electrode. The first region is present on the n-type layer side of the p-type light absorbing layer. The second region is present on the p-electrode side of the p-type light absorbing layer. The first average crystal grain size, which is the average crystal grain size of the first region, is larger than the second average crystal grain size, which is the average crystal grain size of the second region. [Brief description of the drawings]
[0006] [Figure 1] FIG. 1 is a schematic cross-sectional view of a solar cell according to an embodiment. [Diagram 2] FIG. 2 is a diagram for explaining analysis spots of a solar cell according to an embodiment. [Diagram 3] FIG. 3 is a schematic cross-sectional view of a second region 3b according to the embodiment. [Figure 4] FIG. 4 is a flowchart of a method for manufacturing a p-type absorber layer according to an embodiment. [Diagram 5] FIG. 5 is a cross-sectional view of a multi-junction solar cell according to an embodiment. [Figure 6] FIG. 6 is a perspective view of a solar cell module according to an embodiment. [Figure 7] FIG. 7 is a cross-sectional view of a solar cell module according to an embodiment. [Figure 8] FIG. 8 is a configuration diagram of a solar power generation system according to an embodiment. [Figure 9] FIG. 9 is a schematic diagram of a vehicle according to an embodiment. [Figure 10] FIG. 10 is a schematic diagram of a flying object according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] A preferred embodiment of the present invention will be described in detail below with reference to the drawings. Unless otherwise specified, the physical property values shown are those at 25°C and 1 atmospheric pressure (atmosphere). The average indicates an arithmetic mean value. Each concentration is the average concentration of the target region or layer. In each layer, the inclusion of a specific element means, for example, an element whose presence is confirmed by SIMS (Secondary Ion Mass Spectrometry), and the absence of a specific element means, for example, an element whose presence cannot be confirmed by SIMS. When the cross-sectional area of a particle captured in a cross-sectional image is S, the particle size (diameter) of each particle is expressed as (4S / π) 1 / 2 It is.
[0008] In the specification, " / " represents a division symbol. However, " / " in "or / and" means "or." In the specification, "·" represents a multiplication symbol. In the numerical values in the specification, "." represents a decimal point.
[0009] (First embodiment) The first embodiment relates to a solar cell. FIG. 1 shows a schematic cross-sectional view of a solar cell 100 of the first embodiment. As shown in FIG. 1, the solar cell 100 according to this embodiment has a substrate 1, a p-electrode 2 as a first electrode, a p-type light absorbing layer 3, an n-type layer 4, and an n-electrode 5 as a second electrode. An intermediate layer (not shown) may be included between the n-type layer 4 and the n-electrode 5. Sunlight may be incident from either the n-electrode 5 side or the p-electrode 2 side, but it is more preferable that it is incident from the n-electrode 5 side. The solar cell 100 of the embodiment is a transparent solar cell, so it is preferable to use it on the top cell side (light incident side) of a multi-junction solar cell. In FIG. 1, the substrate 1 is provided on the opposite side of the p-electrode 2 from the p-type light absorbing layer 3 side, but the substrate 1 may be provided on the opposite side of the n-electrode 5 from the n-type layer 4 side. The embodiment shown in FIG. 1 will be described below, but the embodiment in which the substrate 1 is provided on the n-electrode 5 side is similar except that the position of the substrate 1 is different. In the solar cell 100 of the embodiment, light is incident from the n-electrode 5 side toward the p-electrode 2 side.
[0010] The substrate 1 is a transparent substrate. For the substrate 1, organic substrates such as light-transmitting acrylic, polyimide, polycarbonate, polyethylene terephthalate (PET), polypropylene (PP), fluorine-based resin (polytetrafluoroethylene (PTFE), perfluoroethylene propene copolymer (FEP), ethylene tetrafluoroethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), perfluoroalkoxyalkane (PFA), etc.), polyarylate, polysulfone, polyethersulfone, polyetherimide, etc., or inorganic substrates such as soda-lime glass, white plate glass, chemically strengthened glass, and quartz can be used. The substrate 1 may be a laminate of the substrates listed above.
[0011] The p-electrode 2 is provided on the substrate 1 and is disposed between the substrate 1 and the p-type light absorbing layer 3. The p-electrode 2 preferably forms an ohmic junction with the p-type light absorbing layer 3. The p-electrode 2 is a conductive layer having optical transparency provided on the p-type light absorbing layer 3 side. The thickness of the p-electrode 2 is typically 100 nm or more and 2000 nm or less. In FIG. 1, the p-electrode 2 is in direct contact with the p-type light absorbing layer 3. The p-electrode 2 preferably includes one or more layers of an oxide transparent conductive film. As the oxide transparent conductive film, a semiconductor conductive film such as indium tin oxide (ITO), aluminum doped zinc oxide (AZO), boron doped zinc oxide (BZO), gallium doped zinc oxide (GZO), doped tin oxide, titanium doped indium oxide (ITiO), indium zinc oxide (IZO), indium gallium zinc oxide (IGZO), hydrogen doped indium oxide (IOH) can be used, and is not particularly limited. The oxide transparent conductive film may be a laminated film having a plurality of films. The dopant for the tin oxide film is not particularly limited as long as it is one or more selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, Cl, etc. The p electrode 2 preferably includes a tin oxide film doped with one or more elements selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, Cl, etc. In the doped tin oxide film, it is preferable that the one or more elements selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, Cl, etc. are contained in an amount of 10 atomic % or less with respect to the tin contained in the tin oxide film. As the p electrode 2, a laminated film in which a transparent conductive oxide film and a metal film are laminated can be used.The metal film preferably has a thickness of 1 nm or more and 2 μm or less, and the metal (including alloy) contained in the metal film is not particularly limited to Mo, Au, Cu, Ag, Al, Ta, W, etc. In addition, the p electrode 2 preferably includes a dot-shaped, line-shaped, or mesh-shaped electrode (one or more selected from the group consisting of metal, alloy, graphene, conductive nitride, and conductive oxide) between the oxide transparent conductive film and the substrate 1, or between the oxide transparent conductive film and the p-type light absorbing layer 3. The dot-shaped, line-shaped, or mesh-shaped metal preferably has an aperture ratio of 50% or more with respect to the oxide transparent conductive film. The dot-shaped, line-shaped, or mesh-shaped metal is not particularly limited to Mo, Au, Cu, Ag, Al, Ta, W, etc. When a metal film is used for the p electrode 2, the thickness is preferably about 5 nm or less from the viewpoint of transparency. When a line-shaped or mesh-shaped metal film is used, transparency is ensured at the openings, so the thickness of the metal film is not limited to this.
[0012] A doped tin oxide film that forms an ohmic junction with the p-type light absorbing layer 3 is preferably provided on the outermost surface of the oxide transparent conductive film on the p-type light absorbing layer 3 side. It is preferable that at least a part of the doped tin oxide film provided on the outermost surface of the oxide transparent conductive film on the p-type light absorbing layer 3 side is in direct contact with the p-type light absorbing layer 3.
[0013] The p-type light absorbing layer 3 is a p-type semiconductor layer. The p-type light absorbing layer 3 is provided on the p-electrode 2. The p-type light absorbing layer 3 may be in direct contact with the p-electrode 2, or other layers may be present as long as electrical contact with the p-electrode 2 can be ensured. The p-type light absorbing layer 3 is disposed between the p-electrode 2 and the n-type layer 4. The p-type light absorbing layer 3 is in direct contact with the n-type layer 4. The p-type light absorbing layer 3 includes a first region 3a. The p-type light absorbing layer 3 is preferably a compound semiconductor. The p-type light absorbing layer 3 is preferably a p-type compound semiconductor when it is non-doped. As the p-type compound semiconductor layer when it is non-doped, a semiconductor layer containing any one of cuprous oxide (cuprous oxide compound), a compound having a chalcopyrite structure, a compound having a kesterite structure, and a compound having a stannite structure is preferably a semiconductor layer containing only any one of them. When a semiconductor layer containing any one of a compound having a chalcopyrite structure, a compound having a kesterite structure, and a compound having a stannite structure is used for the p-type light absorbing layer 3, and when cuprous oxide is used for the p-type light absorbing layer 3, the optical path length is increased and the quantum efficiency of light with a wavelength of 500 nm or more is improved.
[0014] When the p-type light absorbing layer 3 contains cuprous oxide, it is preferably a cuprous oxide compound mainly composed of cuprous oxide or a composite oxide of cuprous oxide. In other words, the p-type light absorbing layer 3 is preferably a semiconductor layer containing a cuprous oxide compound. The p-type light absorbing layer 3 is preferably a polycrystal of a cuprous oxide compound. The cuprous oxide compound may contain a trace amount of one or more cuprous oxide impurities selected from the group consisting of copper (Cu), copper oxide (CuO) and copper hydroxide (Cu(OH)2) as a partial impurity.
[0015] The number of oxygen atoms contained in the cuprous oxide compound is preferably 0.48 or more and 0.56 or less, assuming that the number of copper atoms is 1. If the amount of oxygen is large relative to the amount of copper, the ratio of copper oxide contained in the cuprous oxide compound increases, narrowing the band gap and reducing the translucency of the p-type light absorbing layer 3, which is not preferable. If the amount of oxygen is small relative to the amount of copper, the amount of copper contained in the cuprous oxide compound increases, which is not preferable, as it reduces the translucency.
[0016] The cuprous oxide compound is an oxide mainly composed of cuprous oxide. When all metal elements contained in the p-type light absorbing layer 3 are taken as 100%, the copper element contained in the p-type light absorbing layer 3 is preferably 95% or more and 100% or less, more preferably 98% or less and 100% or less, and even more preferably 99% or more and 100% or less.
[0017] Preferably, 95 wt% to 100 wt% of the p-type light absorbing layer 3 is a cuprous oxide compound, more preferably, 98 wt% to 100 wt% of the p-type light absorbing layer 3 is a cuprous oxide compound, and even more preferably, 99 wt% to 100 wt% of the p-type light absorbing layer 3 is a cuprous oxide compound. 100 wt% of the p-type light absorbing layer 3 can be composed of a cuprous oxide compound.
[0018] The p-type light absorbing layer 3 is preferably a polycrystal of cuprous oxide or / and a complex oxide of cuprous oxide. a M1 b O c It is an oxide represented by the formula: M1 is preferably one or more elements selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Fe, Ni, Pd, Ag, Zn, Cd, Al, Ga, In, C, Si, Ge, Sn, N, P, Sb, Ge, Bi, Cl, F, Br, I, Mn, Tc and Re. It is preferable that a, b and c satisfy 1.80≦a≦2.01, 0.00≦b≦0.20 and 0.98≦c≦1.02. It is preferable that the p-type light absorbing layer 3 contains almost no Cu or / and CuO, which is a heterophase. It is preferable that the p-type light absorbing layer 3 contains few heterophases and has good crystallinity, because this increases the light transmittance of the p-type light absorbing layer 3. It is preferable that the band gap of the p-type light absorbing layer 3 is 2.0 eV or more and 2.2 eV or less. With a band gap in this range, in a multi-junction solar cell using a solar cell with Si as the light absorption layer as the bottom cell and a solar cell of the embodiment as the top cell, sunlight can be efficiently utilized in both the top cell and the bottom cell.
[0019] The above composition ratio of the p-type light absorbing layer 3 is the composition ratio of the entire p-type light absorbing layer 3.
[0020] The thickness of the p-type light absorbing layer 3 is determined by cross-sectional observation using an electron microscope or a step gauge, and is preferably 2000 [nm] to 15000 [nm] (2 [μm] to 15 [μm]), more preferably 2500 [nm] to 10000 [nm], even more preferably 4000 [nm] to 10000 [nm], and preferably 4000 [nm] to 8000 [nm]. The p-type light absorbing layer 3 has a small unevenness on the surface, and the difference between the minimum thickness and the maximum thickness of the p-type light absorbing layer 3 is preferably 0 [nm] to 100 [nm], more preferably 0 [nm] to 50 [nm]. The p-type light absorbing layer 3 has a rectangular parallelepiped shape.
[0021] The p-type light absorbing layer 3 includes a first region 3a having a large grain size and a second region 3b having a small grain size. The first region 3a is present on the n-type layer 4 side. The second region 3b is present on the p-electrode 2 side. It is preferable that the first region 3a and the second region 3b are directly connected to each other.
[0022] The first average crystal grain size d1, which is the average crystal grain size of the first region 3a, is preferably larger than the second average crystal grain size d2, which is the average crystal grain size of the second region 3b.
[0023] In the case where the p-type light absorbing layer 3 and the n-type layer 4 are different compounds and have a pn heterojunction, when the elements of the n-type layer 4 diffuse into the p-type light absorbing layer 3 and / or the elements of the p-type light absorbing layer 3 diffuse into the n-type layer 4, a mixed region having a thickness of 20 [nm] or less where the elements of each other diffuse between the p-type light absorbing layer 3 and the n-type layer 4 may exist. 90 [atom%] or less of the metal elements in the mixed region are metals contained in the p-type light absorbing layer 3, and further, 10 [atom%] or more of the metal elements in the mixed region are metal elements contained in the n-type layer 4. In the case where a mixed region exists, the surface of the p-type light absorbing layer 3 on the n-type layer 4 side is the surface of the p-type light absorbing layer 3 on the n-type layer 4 side excluding the mixed region, and the surface of the n-type layer 4 on the p-type light absorbing layer 3 side is the surface of the n-type layer 4 on the p-type light absorbing layer 3 side excluding the mixed region.
[0024] The thickness of the p-type light absorbing layer 3 is determined by cross-sectional observation using an electron microscope or a step gauge, and is preferably 2000 [nm] to 15000 [nm] (1 [μm] to 15 [μm]), more preferably 2500 [nm] to 10000 [nm], even more preferably 4000 [nm] to 10000 [nm], and preferably 4000 [nm] to 8000 [nm]. The p-type light absorbing layer 3 has a small unevenness on the surface, and the difference between the minimum thickness and the maximum thickness of the p-type light absorbing layer 3 is preferably 0 [nm] to 100 [nm], and more preferably 0 [nm] to 50 [nm]. The p-type light absorbing layer 3 has a rectangular parallelepiped shape.
[0025] The thickness of the second region 3b is preferably 70 nm or more and 1000 nm or less. The presence of the second region 3b improves the quantum efficiency of light with a wavelength of 500 nm or more, contributing to an improvement in conversion efficiency. If the thickness of the second region 3b is thin, the effect of improving the quantum efficiency of light with a wavelength of 500 nm or more is small. If the thickness of the second region 3b is thick, there are many defects in the light absorption layer, which is not preferable because electron recombination is likely to occur. From the above viewpoint, the thickness of the second region 3b is preferably thicker than 70 nm and 1000 nm or less, and more preferably 100 nm or more and 1000 nm or less.
[0026] The thickness of the second region 3b is preferably 150 nm or more and 600 nm or less. The presence of the second region 3b improves the quantum efficiency of light with a wavelength of 500 nm or more, contributing to an improvement in conversion efficiency. If the thickness of the second region 3b is thin, the effect of improving the quantum efficiency of light with a wavelength of 500 nm or more is small. If the thickness of the second region 3b is thick, it is not preferable because it increases the number of defects in the light absorption layer and makes it easier for electrons to recombine. From the above viewpoint, the thickness of the second region 3b is more preferably 150 nm or more and 500 nm or less.
[0027] The method for measuring the thickness of the first region 3a and the thickness of the second region 3b will be described. By observing the cross sections of the analysis spots A1 to A9 in Fig. 2, the region with a large grain size on the n-type layer 4 side is designated as the first region 3a. By observing the cross sections of the analysis spots A1 to A9 in Fig. 2, the region with a small grain size on the p-electrode 2 side is designated as the second region 3b.
[0028] The thickness of the second region 3b is preferably 70 nm or more and 1000 nm or less, and 1% or more and less than 20% of the thickness of the p-type light absorbing layer 3. If the thickness of the second region 3b is relatively thin with respect to the thickness of the p-type light absorbing layer 3, the effect of increasing the optical path length is not obtained, which is not preferable. If the thickness of the second region 3b is relatively thick with respect to the thickness of the p-type light absorbing layer 3, the number of defects in the light absorbing layer increases, and electron recombination is likely to occur, which is not preferable. Therefore, the thickness of the second region 3b is preferably 70 nm or more and 1000 nm or less, and 3% or more and less than 15% of the thickness of the p-type light absorbing layer 3. From the above viewpoints, the thickness of the second region 3b is preferably greater than 70 [nm] and less than 1000 [nm] and is 3% or more and less than 15% of the thickness of the p-type light absorbing layer 3, and more preferably greater than 100 [nm] and less than 1000 [nm] and is 3% or more and less than 15% of the thickness of the p-type light absorbing layer 3.
[0029] The thickness of the second region 3b is preferably 150 [nm] or more and 600 [nm] or less, and 1 [%] or more and less than 20 [%] of the thickness of the p-type light absorbing layer 3. If the thickness of the second region 3b is relatively thin with respect to the thickness of the p-type light absorbing layer 3, the effect of increasing the optical path length is not obtained, which is not preferable. If the thickness of the second region 3b is relatively thick with respect to the thickness of the p-type light absorbing layer 3, the number of defects in the light absorbing layer increases, and electron recombination is likely to occur, which is not preferable. Therefore, the thickness of the second region 3b is preferably 150 [nm] or more and 600 [nm] or less, and 3 [%] or more and less than 15 [%] of the thickness of the p-type light absorbing layer 3. From the above viewpoint, the thickness of the second region 3b is preferably 150 [nm] or more and 500 [nm] or less, and 3 [%] or more and less than 15 [%] of the thickness of the p-type light absorbing layer 3.
[0030] When the thickness of the second region 3b is equal to or greater than 1% and less than 20% of the thickness of the p-type light absorbing layer 3, the thickness of the first region 3a is preferably equal to or greater than 80% and less than 99% of the thickness of the p-type light absorbing layer 3. When the first region 3a occupies most of the p-type light absorbing layer 3, a solar cell 100 with high conversion efficiency is obtained.
[0031] When the thickness of the second region 3b is equal to or greater than 3[%] and less than 15[%] of the thickness of the p-type light absorbing layer 3, the thickness of the first region 3a is preferably equal to or greater than 85[%] and less than 97[%] of the thickness of the p-type light absorbing layer 3. When the first region 3a occupies most of the p-type light absorbing layer 3, a solar cell 100 with high conversion efficiency is obtained.
[0032] The first average crystal grain size d1, which is the average crystal grain size of the first region 3a, is preferably 1.5 [μm] or more. The first average crystal grain size d1 is preferably 80 [%] or more and less than 100 [%] of the thickness of the p-type light absorbing layer 3. The first region 3a is the main region in the p-type light absorbing layer 3 that absorbs light and generates electricity. If the first average crystal grain size d1 of the first region 3a is a large grain size, the first region can absorb light of 350 [nm] or more and less than 650 [nm] to generate electricity with high efficiency. The first average crystal grain size d1 is preferably 90 [%] or more and 100 [%] or less of the thickness of the p-type light absorbing layer 3 minus the thickness of the second region 3b, that is, the thickness of the first region 3a, and more preferably 95 [%] or more and 100 [%] or less. Moreover, it is preferable that particles contained in the p-type light absorbing layer 3, the particles having a particle size of 50% or more and less than 100% of the thickness of the p-type light absorbing layer 3, are not in direct contact with the p-electrode 2.
[0033] The first average crystal grain size d1 is obtained by observing the p-type light absorbing layer 3 in each cross-sectional image of the analysis spots A1 to A9 in FIG. 2. For example, a scanning electron microscope (SEM) is used to obtain the cross-sectional image. The magnification is about 10,000 times or more and 200,000 times, and the photographing range is equal to or more than the thickness of the p-type light absorbing layer 3. The cross-sectional image includes the p-type light absorbing layer 3, the n-type layer 4, and the p-electrode 2. In the p-type light absorbing layer 3 on the n-type layer 4 side of the cross-sectional image, five crystals with the longest diameter in the stacking direction are selected. The average value of the diameters in the stacking direction of the selected five crystals is obtained. The average values obtained from the nine analysis spots A1 to A9 are further averaged, and the average value obtained is set as the average crystal grain size d1.
[0034] The second average crystal grain size d2 of the second region 3b is preferably 0.005 μm or more and 0.60 μm or less, and more preferably 0.15 μm or more and 0.45 μm or less. The presence of the second region 3b with a small grain size on the p-electrode 2 side allows the second region 3b to absorb light with long wavelengths that is not absorbed in the first region 3a. This improves the quantum efficiency of the solar cell 100 for light with wavelengths of 500 nm or more.
[0035] The maximum value of the crystal grain size in the second region 3b is preferably 0.05 μm or more and 2.00 μm or less, and more preferably 0.30 μm or more and 1.0 μm or less.
[0036] The second average crystal grain size d2 is obtained by measuring the analysis spots A1 to A9 in FIG. 2 using SEM-EBSD (scanning electron microscope-backscattered electron diffraction). Specifically, the boundary between the p-electrode 2 and the p-type light absorbing layer 3 is observed. In the observation, a region where the thickness of the second region 2b can be confirmed is selected. The acceleration voltage is 1 kV, the sample tilt is 70°, the measurement region is 0.8 μm × 11 μm, and the STEP is 0.01 μm. By irradiating the sample tilted by 70° with an electron beam, diffracted electron beams are created at each crystal plane, and the backscattered electron diffraction is analyzed to determine the crystal plane orientation in the image. Boundaries with an orientation difference of 5° or more in the crystal plane orientation are treated as crystal grain boundaries, and each particle is color-coded based on the crystal plane orientation. The color coding makes it easy to visually recognize the grain boundaries. The diameters of all particles included in the measurement area are calculated by multiplying the number of pixels by the square of the step size (0.01 μm), and the particle area is calculated by multiplying the particle area by 4 / π)^(1 / 2). When calculating the particle diameter, the area including the grain boundary is considered to be a particle, and the particle diameter is calculated. The average value of the diameters of all particles included in the measurement areas of analysis spots A1 to A9 is defined as the second average crystal grain size d2.
[0037] The ratio of the second average crystal grain size d2 of the second region 3b to the first average crystal grain size d1 of the first region 3a (d2 / d1) is preferably 0.005 to 0.300, more preferably 0.010 to 0.300, and even more preferably 0.020 to 0.100. When d2 / d1 is within the preferred range, electron recombination is reduced, and the optical path length on the back side is increased.
[0038] The second region 3b preferably includes voids G. The average cross-sectional diameter of the voids G is preferably 0.10 μm or more and 0.60 μm or less, and more preferably 0.15 μm or more and 0.45 μm or less. By keeping the voids within the above range, it is possible to prevent an increase in electron recombination.
[0039] It is preferable that the first region 3a contains almost no voids G. The area ratio R1 of the voids G to the cross section of the first region 3a ([total cross-sectional area of the voids G in the first region 3a] / [cross-sectional area of the first region 3a]) is preferably 0 or more and 0.1 or less, more preferably 0 or more and 0.01 or less.
[0040] The area ratio R2 of the voids G in the cross section of the second region 3b ([total cross-sectional area of the voids G in the second region 3b] / [cross-sectional area of the second region 3b]) is preferably 0.01 to 0.3, more preferably 0.05 to 0.1.
[0041] When the first region 3a contains voids G, the area ratio R1 (R1 / R2) of the voids G in the cross section of the first region 3a to the area ratio R2 of the voids G in the cross section of the second region 3b is preferably 0.001 or more and 0.1 or less.
[0042] When examining grain boundaries at analysis spots A1 to A9 in FIG. 2 by SEM-EBSD, regions determined to be other than crystals are regarded as voids G. The diameter of the voids G is calculated in the same manner as the second average crystal grain size d2. The average value of the diameters of all voids included in the measurement regions of analysis spots A1 to A9 is regarded as the average cross-sectional diameter of the voids G. In addition, the total cross-sectional area of the voids G in the first region 3a or the second region 3b is calculated by adding up the diameters of the voids G in the first region 3a or the second region 3b.
[0043] The particle size distribution of the second region 3b preferably includes two or more and three or less peaks in the range of 0.005 [μm] to 0.70 [μm], and more preferably includes two peaks (only two peaks) in the range of 0.005 [μm] to 0.70 [μm]. The particle size distribution of the second region 3b preferably includes a first peak P1 in the range (first range) of 0.005 [μm] to less than 0.30 [μm], and a second peak P2 in the range (second range) of 0.30 [μm] to 0.70 [μm]. The p-type light absorbing layer 3 produced by the manufacturing method of the embodiment has a second region 3b whose particle size distribution includes peaks in both the first and second ranges.
[0044] As shown in the schematic cross-sectional view of FIG. 3, the second region 3b of the embodiment includes large particles A, small particles B, small voids G, and the like. S and large gap G L It is preferred that the formula (I) is included.
[0045] The particle size distribution in the second region 3b in the range of 0.10 μm to 0.70 μm will be described. The class width is 0.05 μm. For example, the 0.10 μm class includes particles with particle sizes of 0.075 μm to 0.125 μm.
[0046] If the ratio of particles having a crystal grain size of 0.075 μm or more and 2.00 μm or less among the particles contained in the second region 3b is taken as 100%, it is preferable that the abundance ratio of the first peak (the ratio of particles contained in the first peak P1 ([number of particles contained in the first peak] / [number of particles having a crystal grain size of 0.075 μm or more and 2.00 μm or less])) and the abundance ratio of the second peak (the ratio of particles contained in the second peak P2 ([number of particles contained in the second peak] / [number of particles having a crystal grain size of 0.075 μm or more and 2.00 μm or less]))) are each 10% or more and 80% or less.
[0047] If the ratio of particles in the second region 3b having a crystal grain size of 0.075 μm or more and 2.00 μm is taken as 100%, it is preferable that the ratio of particles in the first peak P1 or the ratio of particles in the second peak P2 is highest in the range of crystal grain size of 0.075 μm or more and 2.00 μm.
[0048] It is preferable that the ratio of particles contained in the first peak P1 or the ratio of particles contained in the second peak P2 is 20% or more and 70% or less. It is preferable that the first peak P1 and the second peak P2 are neither very sharp peaks nor nearly flat peaks.
[0049] In the particle size distribution of the second region 3b, it is preferable that a valley exists between the first peak P1 and the second peak P2. More specifically, it is preferable that the particle size distribution of the second region 3b includes a class with a ratio of 0% or more and less than 4% between the peak top of the first peak P1 and the peak top of the second peak P2.
[0050] The grain size of each of the analysis spots A1 to A9 is determined in the same manner as in the method of determining the second average grain size d2 by SEM-EBSD. A grain size distribution is created from the determined grain sizes in a class width of 50 [nm]. The vertical axis of the grain size distribution indicates the abundance ratio (the ratio of the number of particles belonging to a class to the number of particles contained in the second region 3b). The first peak P1 and the second peak P2 can be identified from the created grain size distribution.
[0051] The crystal orientation of the particles in the second region 3b is preferably random. The p-type light absorbing layer 3 produced by the manufacturing method of the embodiment has the second region 3b with random crystal orientation. Whether the crystal orientation of the second region 3b in the embodiment is random or not is determined as follows. Observe each analysis spot to obtain an IPF (Inverse Pole Figure) map. Select the highest particle (selected central particle) at the center of the IPF map. Select 20 particles (selected peripheral particles) that are close to the particle closest to the selected central particle. Calculate the orientation difference between each of the selected 20 peripheral particles and the central particle. If there are 10 or more particles with an orientation difference of 15° or more, the crystal orientation of the particles in the second region 3b is considered to be random.
[0052] The cross section of the second region 3b preferably includes the (001) plane ((200) plane), the (101) plane, and the (111) plane. Even if the crystal orientation is random according to the above criteria, it is preferable that the cross section of the second region 3b includes a plurality of grains with different plane orientations, rather than being biased toward a specific plane orientation.
[0053] The crystal plane orientation in the cross section of the second region 3b is obtained as follows: Similar to the method of obtaining the second average crystal grain size d2 by SEM-EBSD, the orientation difference between the crystal plane orientation of each crystal and the central grain is obtained from the IPF maps of the analysis spots A1 to A9.
[0054] The second region 3b preferably contains small voids having a cross-sectional diameter of 0.01 μm or more and less than 0.1 μm, and large voids having a cross-sectional diameter of 0.1 μm or more and 0.6 μm or less.
[0055] The carrier concentration of the second region 3b is preferably higher than that of the first region 3a. When the carrier concentration of the second region 3b is higher than that of the first region 3a, recombination is suppressed by a back surface field (BSF), and the short circuit current density is improved, which preferably contributes to improving the conversion efficiency. The average carrier concentration of the second region 3b is preferably 10 times higher than the average carrier concentration of the first region 3a. 0 more than 10 times 6 The following is preferred:
[0056] When the carrier concentration of the second region 3b is higher than that of the first region 3a, the second region 3b is preferably one or more selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Fe, Ni, Pd, Ag, Zn, Cd, Al, Ga, In, C, Si, Ge, Sn, N, P, Sb, and Bi. When the second region 3b contains one or more elements selected from the group consisting of Cl, F, Br, I, Mn, Tc, and Re, the total concentration of the one or more elements selected from the group consisting of Cl, F, Br, I, Mn, Tc, and Re in the second region 3b is preferably less than 100% of the total concentration of the one or more elements selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Fe, Ni, Pd, Ag, Zn, Cd, Al, Ga, In, C, Si, Ge, Sn, N, P, Sb, and Bi in the second region 3b, and is more preferably 10% or less.
[0057] From the viewpoint of preventing recombination, it is preferable that the carrier concentration in the second region 3b is low on the first region 3a side and high on the p electrode 2 side. From the viewpoint of preventing recombination, it is preferable that the carrier concentration in the second region 3b is low on the first region 3a side and high on the p electrode 2 side, so that the carrier concentration changes gradually from the first region 3a side toward the p electrode 2 side.
[0058] The average carrier concentration in the second region 3b is 10 times that in the first region 3a. 0 more than 10 times 5 When the average carrier concentration of the second region 3b is 10 times or less than the average carrier concentration of the first region 3a, the thickness of the second region 3b is preferably 0.07 μm or more and 0.1 μm or less. 0 more than 10 times 5 When the thickness of the second region 3b is 0.01 to 0.05 times the thickness of the first region 3a, the average carrier concentration of the second region 3b is preferably 10 times or more than the average carrier concentration of the first region 3a. 1 more than 10 times 6 If not more than 0.6 μm, the thickness of the second region 3b is preferably not less than 0.1 μm and not more than 0.6 μm, and not less than 0.05 and not more than 0.3 times the thickness of the first region 3a.
[0059] The hole concentration of the p-type light absorbing layer 3 is obtained. For example, in the case where the thickness of the p-type light absorbing layer 3 is 8 [μm], the first region 3a is present at a depth of 7 [μm] from the surface of the p-type light absorbing layer 3 on the n-type layer 4 side toward the p-electrode 2 side, and the region of the p-type light absorbing layer 3 on the p-electrode 2 side excluding the first region 3a is 1 [μm] thick as the second region 3b, for example, first, the members are removed by polishing or etching from the n-type layer 4 side toward the p-type light absorbing layer 3 side, and the substrate 1 and the p-electrode 2 are removed from the p-electrode 2 side to measure the hole concentration of the entire p-type light absorbing layer 3 alone. Next, the hole concentration is measured while removing the p-type light absorbing layer 3 from the side of the p-type light absorbing layer 3 where the p-electrode 2 was present. For example, the hole concentration is measured every 200 [nm] of thickness to be removed. The measurement accuracy can be improved by setting the interval of 200 [nm], which is the interval of the removal thickness when obtaining the hole concentration, to a constant interval of 10 [nm] or more and 100 [nm] or less.
[0060] The first region 3a is preferably in direct contact with the second region 3b. The surface of the first region 3a facing the second region 3b is preferably in direct contact with the surface of the second region 3b facing the first region 3a. The surface of the first region 3a facing the n-type layer 4 is preferably in direct contact with the surface of the n-type layer 4 facing the p-type light absorbing layer 3. The surface of the second region 3b facing the p-electrode 2 is preferably in direct contact with the surface of the p-electrode 2 facing the p-type light absorbing layer 3.
[0061] The p-type light absorbing layer 3 is preferably formed by, for example, sputtering. Fig. 4 shows a flowchart of a method for manufacturing the p-type light absorbing layer 3. The method for manufacturing the p-type light absorbing layer 3 shown in the flowchart of Fig. 4 includes a low-temperature film formation step (S01) and a high-temperature film formation step (S02). By performing two-stage sputtering at different temperatures, the p-type light absorbing layer 3 including both the first region 3a and the second region 3b can be formed. An oxidation step (S03) may also be performed.
[0062] When the substrate 1 is provided on the p-electrode 2 side, it is preferable to carry out the low-temperature film formation step (S01), the high-temperature film formation step (S02), and the oxidation step (S03) in this order.
[0063] When the substrate 1 is provided on the n-electrode 5 side, it is preferable to partially reverse the order of the flow chart of FIG. 4 and perform the high-temperature film formation step (S02), the low-temperature film formation step (S01), and the oxidation step (S03) in that order.
[0064] In sputtering, atoms other than Cu can be introduced into the chamber to form a doped Cu2O film or a composite oxide film of cuprous oxide.
[0065] In sputtering, a component on which the p-type light absorbing layer 3 is to be formed (for example, a component having a p-electrode 2 formed on a substrate 1, or a component having an n-electrode 5 and an n-type layer 4 formed on a substrate 1) is placed on a stage in a chamber, the component is heated by heating the stage, and copper is oxidized in an oxidizing atmosphere using a target mainly composed of copper, causing it to adhere to the component and form a film.
[0066] The sputtering temperature is the temperature of the underlying member on which the p-type light absorbing layer 3 is formed. When the substrate 1 is provided on the p-electrode 2 side, the sputtering temperature is the temperature of the substrate 1 and / or the temperature of the p-electrode 2. When the substrate 1 is provided on the n-electrode 5 side, the sputtering temperature is the temperature of the substrate 1 and / or the temperature of the n-electrode 5. The stage temperature can be regarded as the temperature of the underlying member.
[0067] The sputtering temperature in the low-temperature film formation step (S01) is preferably 200° C. or more and less than 350° C., and more preferably 250° C. or more and 350° C. or less. The low temperature of the underlying layer makes it difficult for crystals of the p-type light absorbing layer 3 to grow, and the second region 3b having a small grain size is formed.
[0068] The oxygen partial pressure in the chamber in the low-temperature film formation step (S01) is preferably 0.01 [Pa] or more and 4.8 [Pa] or less.
[0069] When the deposition rate of the p-type absorber layer 3 in the low-temperature film formation step (S01) is d [μm / min], the oxygen partial pressure is preferably 0.5 to 1.5 times d (the dimension of the deposition rate is ignored in this calculation).
[0070] In the low-temperature film formation process (S01), the carrier concentration can be increased by introducing one or more atoms selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Fe, Ni, Pd, Ag, Zn, Cd, Al, Ga, In, C, Si, Ge, Sn, N, P, Sb, Ge, and Bi into the chamber together with Cu atoms.
[0071] The sputtering temperature in the high-temperature film formation step (S02) is preferably 350° C. or more and 600° C. or less, and more preferably 400° C. or more and 550° C. or less. The high temperature of the underlying layer causes crystals of the p-type light absorbing layer 3 to grow, and the first region 3a with a large grain size is formed.
[0072] The oxygen partial pressure in the chamber in the high-temperature film-forming step (S02) is preferably 0.01 [Pa] or more and 4.8 [Pa] or less.
[0073] When the deposition rate of the p-type absorber layer 3 in the high temperature film formation step (S02) is d [μm / min], the oxygen partial pressure is preferably 0.5 to 1.5 times d (the dimension of the deposition rate is ignored in this calculation).
[0074] The sputtering temperature in the high-temperature film-forming step (S02) is preferably 100° C. or more and 400° C. or less higher than the sputtering temperature in the low-temperature film-forming step (S01).
[0075] When shifting from the low-temperature film-forming process (S01) to the high-temperature film-forming process (S02), the temperature of the member may be changed after stopping sputtering, or the temperature may be changed while sputtering is being performed. When the temperature of the member is changed while sputtering is being performed, it is preferable to change the temperature of the member at a rate of 10°C / min to 100°C / min.
[0076] When shifting to the high-temperature film formation process (S02) or the low-high-temperature film formation process (S01), the temperature of the member may be changed after stopping sputtering, or the temperature may be changed while sputtering is being performed. When changing the temperature of the member while sputtering is being performed, it is preferable to change the temperature of the member at a rate of -100[℃ / min] or more and -10[℃ / min] or less.
[0077] In the high temperature film formation process (S01), one or more atoms selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Fe, Ni, Pd, Ag, Zn, Cd, Al, Ga, In, C, Si, Ge, Sn, N, P, Sb, Ge, Bi, Cl, F, Br, I, Mn, Tc, and Re can be introduced into the chamber together with Cu atoms.
[0078] In the oxidation step (S03), the member on which the p-type light absorbing layer 3 is formed is placed in an atmosphere having a low oxygen concentration (oxygen partial pressure of 100 [Pa]) to a high oxygen concentration (oxygen partial pressure of 200,000 [Pa]) or less, or in an atmosphere containing ozone, to cause oxidation. The oxidation treatment (S03) may be omitted. The oxidation treatment (S03) is preferably performed after the low-temperature film formation step (S01) and the high-temperature film formation step (S02) and before the formation of the n-type layer 4 (when the substrate 1 is provided on the p-electrode 2 side).
[0079] When the p-type light absorbing layer 3 contains a compound having a chalcopyrite structure, examples of the compound having a chalcopyrite structure include compounds containing elements of Group 11 (Cu, Ag), elements of Group 13 (Al, Ga, In), and elements of Group 16 (S, Se, Te). As an n-type dopant of the compound having a chalcopyrite structure, Zn and / or Cd are preferable.
[0080] When the p-type light absorbing layer 3 contains a compound having a kesterite structure, an example of the compound having a kesterite structure is Cu2ZnSn(S,Se)4. As an n-type dopant of the compound having a kesterite structure, Cd is preferable.
[0081] When the p-type light absorbing layer 3 contains a compound having a stannite structure, for example, Cu2(Fe,Zn)Sn(S,Se)4 can be given as the compound having the stannite structure. As an n-type dopant of the compound having the stannite structure, Cd is preferable.
[0082] The n-type layer 4 is an n-type semiconductor layer. The n-type layer 4 is disposed between the p-type light absorbing layer 3 and the n-electrode 5. The n-type layer 4 is preferably provided on the p-type light absorbing layer 3. The n-type layer 4 is in direct contact with the surface of the p-type light absorbing layer 3 opposite to the surface in contact with the p-electrode 2. The n-type layer 4 preferably includes a semiconductor layer including an oxide containing Ga, or a semiconductor layer including an n-type cuprous oxide compound. The semiconductor layer including an oxide containing Ga, or the semiconductor layer including an n-type cuprous oxide compound forms a pn junction (pin junction if the mixed region is i-type) with the p-type light absorbing layer 3. When a semiconductor layer including an oxide containing Ga is used for the n-type layer 4, the solar cell 100 is a heterojunction type solar cell. When a semiconductor layer including a cuprous oxide compound is used for the n-type layer 4, the solar cell 100 is a homojunction type solar cell. The n-type layer 4 may be a single layer of a semiconductor layer including an oxide containing Ga, or a semiconductor layer including an n-type cuprous oxide compound, or may be a multilayer. The multi-layer n-type layer 4 may be in a form including multiple semiconductor layers including oxides containing Ga with different compositions, or multiple semiconductor layers including an n-type cuprous oxide compound and multiple semiconductor layers including oxides containing Ga with different compositions. In both heterojunction solar cells and homojunction solar cells, the short-circuit current density is theoretically improved by expanding the depletion layer width, so that the short-circuit current density and conversion efficiency are improved by providing the first region 3a in heterojunction solar cells and homojunction solar cells.
[0083] It is preferable that the n-type layer 4 contains a compound (oxide) mainly composed of Ga. The n-type layer 4 may be an oxide mainly composed of Ga mixed with other oxides, an oxide mainly composed of Ga doped with other elements, or an oxide mainly composed of Ga doped with other elements and other oxides mixed. The n-type layer 4 is a single layer or a multilayer. Of the metal elements contained in the n-type layer 4, Ga is preferably 40 atomic % or more, and more preferably 50 atomic % or more. The metal elements contained in the n-type layer 4 may be inclined from the p-type light absorbing layer 3 side to the n-electrode 5 side.
[0084] The n-type layer 4 preferably contains an oxide containing an element represented by M3 and Ga. The oxide mainly containing Ga is, for example, an oxide containing an element represented by M3 and Ga. The n-type layer 4 preferably contains an oxide containing M3, which is one or more elements selected from the group consisting of H, Sn, Sb, Cu, Ag, Li, Na, K, Cs, Rb, Al, In, Zn, Mg, Si, Ge, N, B, Ti, Hf, Zr, and Ca, and Ga. The n-type layer 4 preferably contains 90 wt% or more and 100 wt% or less of an oxide containing M3, which is one or more elements selected from the group consisting of H, Sn, Sb, Cu, Ag, Li, Na, K, Cs, Rb, Al, In, Zn, Mg, Si, Ge, N, B, Ti, Hf, Zr, and Ca, and Ga. The compound mainly containing Ga in the n-type layer 4 has an average composition of Ga. h M3 i O j It is preferable that the oxide contains M3 and Ga, and is represented by the following formula: It is preferable that h, i, and j satisfy 1.8≦h≦2.1, 0≦i≦0.2, and 2.9≦j≦3.1.
[0085] It is preferable that 90 [wt%] or more and 100 [wt%] or less of the n-type layer 4 is an oxide containing M3 and Ga. It is more preferable that 95 [wt%] or more and 100 [wt%] or less of the n-type layer 4 is an oxide containing M3 and Ga. It is even more preferable that 98 [wt%] or more and 100 [wt%] or less of the n-type layer 4 is a compound represented by an oxide containing M3 and Ga. The Cu contained in the n-type layer 4 is not contained in the raw material for forming the n-type layer 4, but is Cu contained in the p-type light absorbing layer 3 that has diffused into the n-type layer 4. If other elements are also used when forming the p-type light absorbing layer 3, these elements may also diffuse into the n-type layer 4.
[0086] The thickness of the n-type layer 4 is typically 3 nm or more and 100 nm or less. If the thickness of the n-type layer 4 is less than 3 nm, leakage current may occur when the coverage of the n-type layer 4 is poor, resulting in a deterioration of characteristics. If the coverage is good, the thickness is not limited to the above. If the thickness of the n-type layer 4 exceeds 50 nm, the resistance of the n-type layer 4 may become excessively high, resulting in a deterioration of characteristics, and a decrease in short-circuit current may occur due to a decrease in transmittance. Therefore, the thickness of the n-type layer 4 is more preferably 3 nm or more and 20 nm or less, and even more preferably 5 nm or more and 20 nm or less.
[0087] The composition of the compound of the n-type layer 4 is the average composition of the entire n-type layer 4 unless otherwise specified. The composition of the n-type layer 4 is the average value of the composition at depths of 0.2d4, 0.5d4, and 0.8d4 from the surface of the n-type layer 4 on the p-type light absorbing layer 3 side, when the thickness of the n-type layer 4 is d4. Except for the condition that the element composition ratio of the compound of the n-type layer 4 is inclined, it is preferable that the n-type layer 4 satisfies the above and following suitable compositions at each depth. When the n-type layer 4 is very thin (for example, 5 [nm] or less), the composition at a depth of 0.5d from the surface of the n-type layer 4 on the p-type light absorbing layer 3 side can be regarded as the composition of the entire n-type layer 4. The composition analysis of the n-type layer 4 is the same as that of the p-type light absorbing layer 3.
[0088] In a configuration in which the p-type light absorbing layer 3 does not contain cuprous oxide, a suitable n-type semiconductor layer can be used as the n-type layer 4. In a configuration in which the p-type light absorbing layer 3 does not contain cuprous oxide, an n-type oxide can be used as the n-type layer 4.
[0089] The n-electrode 5 is an electrode on the n-type layer 4 side, which has optical transparency to visible light. The n-electrode 5 is preferably provided on the n-type layer 4. The n-electrode 5 and the p-type light absorbing layer 3 sandwich the n-type layer 4. An intermediate layer (not shown) can be provided between the n-type layer 4 and the n-electrode 5. The n-electrode 5 is preferably an oxide transparent conductive film. The oxide transparent conductive film used in the n-electrode 5 is preferably one or more semiconductor conductive films selected from the group consisting of indium tin oxide, aluminum doped zinc oxide, boron doped zinc oxide, gallium doped zinc oxide, indium doped zinc oxide, titanium doped indium oxide, indium gallium zinc oxide, and hydrogen doped indium oxide. The dopant for the tin oxide film is not particularly limited as long as it is one or more selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, Ta, W, Mo, F, Cl, etc. The n-electrode 5 may include a mesh or line-shaped electrode in order to reduce the resistance of the oxide transparent conductive film. The mesh or line-shaped electrode may be made of any material, including, but not limited to, Mo, Au, Cu, Ag, Al, Ta, or W. Graphene may also be used for the n-electrode 5. Graphene is preferably laminated with silver nanowires.
[0090] The thickness of n-electrode 5 is determined by cross-sectional observation using an electron microscope or a step gauge, and is not particularly limited, but is typically 50 nm or more and 2 μm or less.
[0091] The n-electrode 5 is preferably formed by, for example, sputtering.
[0092] Second embodiment The second embodiment relates to a multi-junction solar cell. Fig. 5 shows a cross-sectional conceptual diagram of a multi-junction solar cell of the second embodiment. The multi-junction solar cell 200 of Fig. 5 has the solar cell (first solar cell) 100 of the first embodiment and a second solar cell 201 on the light incident side. The band gap of the light absorption layer of the second solar cell 201 is smaller than the band gap of the p-type light absorption layer 3 of the solar cell 100 of the first embodiment. The multi-junction solar cell 200 of the embodiment also includes a solar cell in which three or more solar cells are joined together.
[0093] Since the band gap of the p-type light absorbing layer (cuprous oxide) 3 of the first solar cell 100 of the first embodiment is about 2.0 eV or more and 2.2 eV or less, the band gap of the light absorbing layer of the second solar cell 201 is preferably 1.0 eV or more and 1.6 eV or less. The light absorbing layer of the second solar cell 201 is preferably one or more compound semiconductor layers selected from the group consisting of CIGS and CdTe with a high In content, crystalline silicon, and a perovskite compound.
[0094] Third embodiment The third embodiment relates to a solar cell module. Fig. 6 shows a perspective view of a solar cell module 300 of the third embodiment. The solar cell module 300 in Fig. 6 is a solar cell module in which a first solar cell module 301 and a second solar cell module 302 are stacked. The first solar cell module 301 is on the light incident side, and uses the solar cell 100 of the first embodiment. It is preferable to use the second solar cell 201 for the second solar cell module 302.
[0095] FIG. 7 shows a cross-sectional view of a solar cell module 300. FIG. 7 shows the structure of the first solar cell module 301 in detail, but does not show the structure of the second solar cell module 302. For the second solar cell module 302, the structure of the solar cell module is appropriately selected depending on the light absorption layer of the solar cell to be used. The solar cell module 300 in FIG. 6 includes a plurality of submodules 303 surrounded by dashed lines in which a plurality of solar cells 100 (solar cells) are arranged in the horizontal direction and electrically connected in series by wiring 304, and the plurality of submodules 303 are electrically connected in parallel or in series. Adjacent submodules 303 are electrically connected by bus bars 305.
[0096] Adjacent solar cells 100 have their n-electrodes 5 on the upper side and p-electrodes 2 on the lower side connected by wiring 304. The solar cell 100 of the third embodiment has a substrate 1, a p-electrode 2, a p-type light absorbing layer 3, an n-type layer 4, and an n-electrode 5, similar to the solar cell 100 of the first embodiment. Both ends of the solar cell 100 in the submodule 303 are connected to a bus bar 305, and the bus bar 305 is preferably configured to electrically connect the multiple submodules 303 in parallel or series and adjust the output voltage with the second solar cell module 302. Note that the connection form of the solar cells 100 shown in the third embodiment is an example, and a solar cell module can be configured by other connection forms.
[0097] (Fourth embodiment) The fourth embodiment relates to a solar power generation system. The solar cell module of the fourth embodiment can be used as a generator that generates power in the solar power generation system of the fourth embodiment. The solar power generation system of the embodiment generates power using a solar cell module, and specifically includes a solar cell module that generates power, a means for converting the generated electricity into electric power, and a storage means for storing the generated electricity or a load for consuming the generated electricity. FIG. 8 shows a configuration diagram of a solar power generation system 400 of the embodiment. The solar power generation system of FIG. 8 includes a solar cell module 401 (300), a converter 402, a storage battery 403, and a load 404. Either the storage battery 403 or the load 404 may be omitted. The load 404 may be configured to be able to utilize the electric energy stored in the storage battery 403. The converter 402 is a device including a circuit or element that performs power conversion such as voltage transformation and DC-AC conversion, such as a DC-DC converter, a DC-AC converter, or an AC-AC converter. The converter 402 may have a suitable configuration depending on the generated voltage and the configurations of the storage battery 403 and the load 404 .
[0098] The solar cell included in the submodule 303 that receives light in the solar cell module 300 generates electricity, and the electric energy is converted by the converter 402 and stored in the storage battery 403 or consumed by the load 404. It is preferable to provide the solar cell module 401 with a solar tracking drive device for always directing the solar cell module 401 toward the sun, a collector for collecting sunlight, or other devices for improving power generation efficiency.
[0099] The solar power generation system 400 is preferably used in real estate such as residences, commercial facilities, and factories, and in movable property such as vehicles, aircraft, and electronic devices. By using the solar cell with excellent conversion efficiency of the embodiment in a solar cell module, an increase in the amount of power generation is expected.
[0100] A vehicle is shown as an example of use of the solar power generation system 400. FIG. 9 shows a schematic diagram of the vehicle 500. The vehicle 500 in FIG. 9 has a vehicle body 501, a solar cell module 502, a power converter 503, a storage battery 504, a motor 505, and tires (wheels) 506. Electric power generated by the solar cell module 502 provided on the upper part of the vehicle body 501 is converted by the power converter 503 and charged in the storage battery 504, or the electric power is consumed by a load such as the motor 505. The vehicle 500 can be moved by rotating the tires (wheels) 506 by the motor 505 using the electric power supplied from the solar cell module 502 or the storage battery 504. The solar cell module 502 may not be of a multi-junction type, but may be composed of only a first solar cell module equipped with the solar cell 100 of the first embodiment. When a transparent solar cell module 502 is adopted, it is also preferable to use the solar cell module 502 as a window for generating electricity on the side of the vehicle body 501 in addition to the upper part of the vehicle body 501.
[0101] An air vehicle (drone) is shown as an example of use of the solar power generation system 400. The air vehicle uses a solar cell module 401. The configuration of the air vehicle according to this embodiment will be briefly described using the schematic diagram of the air vehicle 600 in FIG. 10. The air vehicle 600 has a solar cell module 401, a body frame 601, a motor 602, a rotor 603, and a control unit 604. The solar cell module 401, the motor 602, the rotor 603, and the control unit 604 are arranged on the body frame 601. The control unit 604 converts the power output from the solar cell module 401 and adjusts the output. The motor 602 rotates the rotor 603 using the power output from the solar cell module 401. By making the air vehicle 600 of this configuration having the solar cell module 401 of the embodiment, a air vehicle that can fly using more power is provided.
[0102] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0103] (Example A: Examples A-1 to A-12, Comparative Examples A-1 to A-6) On the glass substrate 1, ITO (In:Sn=80:20, film thickness 20 [nm]) and ATO (Sn:Sb=98:2 150 [nm]) are deposited on the top surface of the glass substrate 1 as the p-electrode 2 on the back side. A Cu2O layer is formed on the ATO as the p-type light absorbing layer 3 by sputtering in an oxygen and argon gas atmosphere. The Cu2O layer is formed in two stages. First, a Cu2O film (second region 3b) with a thickness of 0.5 [μm] is formed on the substrate 1 at a temperature of 250 [℃], and then a Cu2O film (first region 3a) with a thickness of 5.0 [μm] is formed on the substrate 1 at a temperature of 450 [℃]. After the formation of the p-type light absorbing layer 3, a GaO film with a thickness of 10 [nm] is formed in sequence as the n-type layer 4. Then, a 0.1 μm thick AZO (ZnO:Al) film is formed as the n-electrode 5, and the solar cell 100 is obtained.
[0104] Examples A-2 to A-12 and Comparative Examples A-1 to A-6 are similar to Example A-1, except that the thicknesses of the first region 3a and the second region 3b are different. Table 1 shows the thickness, grain size, and d1>d2 of the first region 3a and the second region 3b of Examples A-1 to A-12 and Comparative Examples A-1 to A-6. In Example A, the region on the n-type layer 4 side is the first region 3a and the second region 3b. Table 1 shows comparative examples of each Example and Comparative Example. Here, the grain size in Table 1 is the average crystal grain size of the first region 3a and the average crystal grain size of the second region 3b. If d1>d2 is satisfied, it is evaluated as A. If d1>d2 is not satisfied, it is evaluated as B. The evaluation of d1>d2 is common to Examples A to C.
[0105] [Table 1]
[0106] A solar simulator that mimics an AM1.5G light source is used, and a reference Si cell is used under that light source, with the amount of light adjusted to 1 sun. Measurements are taken at atmospheric pressure with the temperature in the measurement room at 25°C. The voltage is swept and the current density (current divided by cell area) is measured. With the horizontal axis representing voltage and the vertical axis representing current density, the point where they intersect is the open circuit voltage Voc. On the measurement curve, the voltage and current density are multiplied together, and the maximum points are designated as Vmpp and Jmpp (maximum power point), respectively, and the fill factor can be calculated from FF = (Vmpp * Jmpp) / (Voc * Jsc). Conversion efficiency can be calculated from Eff. = Voc * Jsc * FF.
[0107] The results of Example A are shown in Table 2. Table 2 shows the open circuit voltage (Voc), current density (Jsc), fill factor (FF), conversion efficiency (Eff.), and light transmittance of light having a wavelength of 700 nm or more and 1000 nm or less for the example.
[0108] When the light transmittance is 60% or more and 100% or less, it is evaluated as A, when the light transmittance is 50% or more and less than 60%, it is evaluated as B, and when the light transmittance is less than 50%, it is evaluated as C. The evaluation criteria are common to Examples A to C.
[0109] When the Voc is less than that of the comparative example, it is evaluated as B, and when it is equal to or greater than that of the comparative example, it is evaluated as A. The evaluation criteria are the same for Examples A to C.
[0110] When Jsc is equal to or less than the Jsc of the comparative example, it is evaluated as B, and when it is greater than the Jsc of the comparative example, it is evaluated as A. The evaluation criteria are common to Examples A to C.
[0111] When the FF is less than the FF of the comparative example, it is evaluated as B, and when it is equal to or greater than the FF of the comparative example, it is evaluated as A. The evaluation criteria are common to Examples A to C.
[0112] When Eff is equal to or less than the Eff of the comparative example, it is evaluated as B, and when it is greater than the Eff of the comparative example, it is evaluated as A. The evaluation criteria are common to Examples A to C.
[0113] [Table 2]
[0114] In Examples A-1 to A-12, the first average crystal grain size d1 is larger than the second average crystal grain size d2. In Example A, when a film having a small crystal grain size is prepared in the Cu2O layer of the second region 3b, the optical path length is increased, the amount of light absorption in the entire Cu2O layer including the second region 3b is increased, the current density (Jsc) is increased, and the conversion efficiency (Eff.) is increased.
[0115] (Example B: Examples B-1 to B-12, Comparative Examples B-1 to B-10) On the glass substrate 1, ITO (In:Sn=80:20, thickness 20[nm]) and ATO (Sn:Sb=98:2 150[nm]) are deposited on the top surface of the glass substrate 1 as the p-electrode 2 on the back side, which is in contact with the glass. A Cu2O layer is formed on the ATO as the p-type light absorbing layer 3 by sputtering in an oxygen and argon gas atmosphere. The Cu2O layer is formed in two stages. First, a Cu2O film (second region 3b) with a thickness of 0.5[μm] is formed on the substrate 1 at a temperature of 250[℃], and then a Cu2O film (first region 3a) with a thickness of 5.0[μm] is formed on the substrate 1 at a temperature of 500[℃]. After the formation of the p-type light absorbing layer 3, GaO of 10[nm] and ZTO of 15[nm] are formed in this order as the n-type layer 4. Then, a 0.1 μm thick AZO film is formed as the n-electrode 5 to obtain the solar cell 100.
[0116] Solar cells 100 of Examples B-2 to B-12 and Comparative Examples B-1 to B-10 are fabricated by changing the thickness of the second region 3b and the thickness of the p-type light absorbing layer 3. Table 3 shows examples for comparison with each of the Examples and Comparative Examples.
[0117] Table 3 shows the thickness of the second region 3b, the thickness of the p-type light absorbing layer 3, [thickness of the second region 3b] / [thickness of the p-type light absorbing layer 3], and d1>d2 of the examples and comparative examples. The thickness values in Table 3 are shown to one significant digit (rounded off) except for Comparative Example B-4. Table 3 shows comparative examples of each example and comparative example. Since Comparative Example B-1 and Comparative Examples B-5 to B-10 do not have the second region 3b, d1>d2 is shown with a hyphen.
[0118] [Table 3]
[0119] The results of Example B are shown in Table 4. Table 4 shows the open circuit voltage (Voc), current density (Jsc), fill factor (FF), conversion efficiency (Eff.), and light transmittance for light having a wavelength of 700 nm or more and 1000 nm or less for the example.
[0120] Also, it is confirmed whether the crystal orientation of the particles in the second region 3b is random. When the crystal orientation of the particles in the second region 3b is random, it is evaluated as A, and when it is not random, it is evaluated as B. The evaluation criteria are common to Examples B to C.
[0121] The presence or absence of voids in the second region 3b is also evaluated. A case in which voids are present in the second region 3b is evaluated as A, and a case in which voids are not present is evaluated as B. The evaluation criteria are common to Examples B to C. In Comparative Example B-1 and Comparative Examples B-5 to B-10 in which the second region 3b is not present, the crystal orientation and voids in the region from the interface between the p-type light absorbing layer 3 and the p-electrode 2 to a position 200 nm in the direction of the n-type layer 4 are evaluated.
[0122] [Table 4]
[0123] When fabricated at a low substrate temperature and voids are intentionally created in the Cu2O layer of the second region 3b, light reflection and refraction become more likely to occur, the optical path length of the light becomes longer, and the amount of light absorbed in the Cu2O layer of the entire second region 3b increases, increasing the current density (Jsc) and the conversion efficiency (Eff.).
[0124] Table 5 shows the first average crystal grain size d1, the second average crystal grain size d2, and the maximum value of the crystal grain size in the second region 3b for Examples B-2 to B-6 and Comparative Examples B-1 to B-4.
[0125] [Table 5]
[0126] The average crystal grain size can be changed by adjusting not only the sputtering temperature but also the film thickness of the Cu2O layer in the second region 3b. By adjusting the average grain size in the second region 3b, a long optical path length can be ensured, the amount of light absorption in the entire Cu2O layer including the second region 3b can be increased, the current density (Jsc) can be improved, and the conversion efficiency (Eff.) can be improved. Since the second region 3b is not confirmed in Comparative Example B-1, the second average crystal grain size d2 of Comparative Example B-1 in Table 5 and the maximum value of the crystal grain size in the second region 3b and d1 / d2 are all indicated with hyphens.
[0127] In addition, the area ratio R1 of the voids G in the cross section of the first region 3a in the embodiment satisfies the above-mentioned preferred range. In addition, the area ratio R2 of the voids G in the cross section of the second region 3b in the embodiment satisfies the above-mentioned preferred range. In addition, R1 / R2 in the embodiment satisfies the above-mentioned preferred range.
[0128] Next, the results of examining the particle size distribution of the second region 3b of Examples B-2 to B-6 and Comparative Examples B-1 to B-4 are shown. Table 6 shows the number of peaks included in the particle size distribution of 0.005 μm or more and 0.70 μm or less (number of peaks 0.10-0.70), the number of peaks included in the particle size distribution of 0.005 μm or more and less than 0.30 μm (number of peaks 0.10-0.30), the number of peaks included in the particle size distribution of 0.30 μm or more and 0.70 μm or less (number of peaks 0.30-0.70), the abundance ratio of the first peak P1, and the abundance ratio of the second peak P2.
[0129] [Table 6]
[0130] By changing the film thickness of the Cu2O layer in the second region 3b, the distribution of the average crystal grain size can also be adjusted. By adjusting the average grain size, a long optical path length can be ensured, the amount of light absorption in the Cu2O layer in the entire second region 3b can be increased, the current density (Jsc) can be improved, and the conversion efficiency (Eff.) can be improved. In the Cu2O layer of the comparative example, no peak is observed in the second region 3b. Therefore, no peak or valley is observed in the comparative example, but a peak is observed in the example. In addition, both small and large voids are observed in the second region 3b of the example. In addition, the example C satisfies d1>d2.
[0131] (Example C: Examples C-1 to C-25) On the glass substrate 1, ITO (In:Sn=80:20, film thickness 20 [nm]) and ATO (Sn:Sb=98:2 150 [nm]) are deposited on the top surface of the glass substrate as the p-electrode 2 on the back side. A Cu2O layer is formed as the p-type light absorbing layer 3 on the ATO by sputtering in an oxygen and argon gas atmosphere. The Cu2O layer is formed in two stages. First, a N-doped Cu2O film (second region 3b) is formed with a thickness of 0.5 [μm] at a substrate temperature of 250 [℃], and then a non-doped Cu2O film (first region 3a) is formed with a thickness of 5.0 [μm] at a substrate temperature of 480 [℃]. After the formation of the p-type light absorbing layer 3, a GaO film with a thickness of 10 [nm] and a ZTO film with a thickness of 15 [nm] are formed in this order as the n-type layer 4. Then, a 0.1 μm thick AZO film is formed as the n-electrode 5 to obtain the solar cell 100.
[0132] Solar cells 100 of Examples C-2 to C-25 are fabricated by changing the thickness of the second region 3b and the dopant element. Table 7 shows the thickness [nm] of the first region 3a, the thickness [nm] of the second region 3b, the dopant, d1>d2, and a comparison example for each Example and Comparative Example.
[0133] [Table 7]
[0134] Table 8 shows the open circuit voltage (Voc), current density (Jsc), fill factor (FF), conversion efficiency (Eff.), light transmittance for light with a wavelength of 700 nm or more and 1000 nm or less, whether the crystallinity of the second region 3b is random, and whether or not there are voids in the second region 3b for Examples C-1 to C-25.
[0135] [Table 8]
[0136] When sputtering is performed at a low substrate temperature while adding impurities, the crystal grain size becomes smaller in the Cu2O layer of the second region 3b and voids become more likely to form, which increases the optical path length, increases the amount of light absorbed by the Cu2O layer of the entire second region 3b, increases the current density (Jsc), and increases the conversion efficiency (Eff.).
[0137] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and the components can be modified and embodied in the implementation stage without departing from the gist of the invention. In addition, various inventions can be formed by appropriately combining the multiple components disclosed in the above embodiment. For example, components from different embodiments may be appropriately combined as in the modified examples. In the present specification, some elements are shown only by their element symbols.
[0138] The technical solutions of the embodiments are described below. Technical proposal 1 A p-electrode; An n-electrode; a p-type light absorbing layer provided on the p-electrode and including a first region and a second region; an n-type layer provided between the p-type light absorbing layer and the n-electrode; the first region is present on the n-type layer side of the p-type light absorbing layer, the second region is present on the p-electrode side of the p-type light absorbing layer, A solar cell, wherein a first average crystal grain size which is an average crystal grain size of the first region is larger than a second average crystal grain size which is an average crystal grain size of the second region. Technical proposal 2 The solar cell according to Technical Scheme 1, wherein the p-type light absorbing layer is mainly composed of cuprous oxide or a composite oxide of cuprous oxide. Technical proposal 3 The thickness of the p-type light absorbing layer is 2000 [nm] or more and 15000 [nm] or less, The solar cell described in Technical Proposal 1 or 2, wherein the thickness of the second region is 70 nm or more and 1000 nm or less. Technical proposal 4 The thickness of the second region is 70 nm or more and 1000 nm or less, The solar cell according to any one of Technical Schemes 1 to 3, wherein the thickness of the second region is 3% or more and less than 15% of the thickness of the p-type light absorbing layer 3. Technical proposal 5 The thickness of the second region is 150 nm or more and 600 nm or less, The solar cell according to any one of Technical Schemes 1 to 4, wherein the thickness of the second region is 3% or more and less than 15% of the thickness of the p-type light absorbing layer 3. Technical plan 6 The solar cell according to any one of Technical Schemes 1 to 5, wherein the first average crystal grain size is 80% or more and less than 100% of the thickness of the p-type light absorbing layer. Technical proposal 7 A solar cell according to any one of Technical Schemes 1 to 6, wherein the second average crystal grain size is 0.005 μm or more and 0.60 μm or less. Technical proposal 8 A solar cell according to any one of Technical Schemes 1 to 7, wherein the maximum value of the crystal grain size in the second region is 0.05 μm or more and 2.00 μm or less. Technical proposal 9 A solar cell described in any one of technical proposals 1 to 8, wherein the second average crystal grain size relative to the first average crystal grain size ([average crystal grain size of the second region] / [average crystal grain size of the first region]) is 0.005 or more and 0.300 or less. Technical proposal 10 The second region includes a void; A solar cell according to any one of Technical Schemes 1 to 9, wherein the average cross-sectional diameter of the voids is 0.1 μm or more and 0.60 μm or less. Technical proposal 11 A solar cell described in any one of technical proposals 1 to 10, wherein the area ratio of the voids to the cross section of the second region ([total cross-sectional area of the voids in the second region] / [cross-sectional area of the second region]) is 0.01 or more and 0.3 or less. Technical proposal 12 A solar cell described in any one of technical proposals 1 to 11, wherein the area ratio of the voids to the cross section of the first region ([total cross-sectional area of the voids in the first region] / [cross-sectional area of the first region]) is greater than or equal to 0 and less than 0.1. Technical proposal 13 the first region includes a void; the second region includes a void; A solar cell described in any one of technical proposals 1 to 12, wherein the area ratio of the void in the cross section of the first region to the area ratio of the void in the cross section of the second region is 0.001 or more and 0.1 or less. Technical proposal 14 A solar cell according to any one of Technical Schemes 1 to 13, wherein the particle size distribution in the second region in the range of 0.005 μm or more and 0.70 μm or less includes two peaks. Technical proposal 15 The particle size distribution in the second region in the range of 0.005 [μm] or more and 0.70 [μm] or less includes two peaks, The particle size distribution includes a first peak in the range of 0.005 [μm] or more and less than 0.30 [μm], A solar cell according to any one of Technical Schemes 1 to 14, wherein the particle size distribution includes a second peak in the range of 0.30 μm or more and 0.70 μm or less. Technical proposal 16 A solar cell according to Technical Proposal 15, wherein the ratio of particles contained in the first peak or the ratio of particles contained in the second peak is 10% or more and 80% or less. Technical proposal 17 A solar cell according to any one of technical proposals 1 to 16, wherein the crystal orientation of the particles in the second region is random. Technical proposal 18 A solar cell described in any one of technical proposals 1 to 17, wherein the two regions include small voids having a cross-sectional diameter of 0.01 μm or more and less than 0.1 μm and large voids having a cross-sectional diameter of 0.1 μm or more and 0.6 μm or less. Technical proposal 19 A solar cell according to any one of Technical Schemes 1 to 18, wherein the second region contains one or more elements selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Fe, Ni, Pd, Ag, Zn, Cd, Al, Ga, In, C, Si, Sn, N, P, Sb, and Bi. Technical proposal 20 A multi-junction solar cell using the solar cell according to any one of Technical Schemes 1 to 19. Technical Scheme 21 A solar cell module using a solar cell according to any one of technical proposals 1 to 19. Technical proposal 22 A solar power generation system that generates electricity using the solar cell module described in Technical Proposal 21. Technical proposal 23 A p-electrode; An n-electrode; a p-type light absorbing layer provided on the p-electrode and including a first region having a large grain size and a second region having a small grain size; an n-type layer provided between the p-type light absorbing layer and the n-electrode; the first region is present on the n-type layer side of the p-type light absorbing layer, The second region is a solar cell that exists on the p-electrode side of the p-type light absorbing layer. [Explanation of symbols]
[0139] 1: Circuit board 2 :p electrode 3: p-type light absorbing layer 3a: 1st area 3b:Second area 4:N-type layer 5 :n electrode 100: Solar cell 200: Multijunction solar cell 201:Second solar cell 300: Solar cell module 301: First solar cell module 302: Second solar cell module 303: Submodule 304: Wiring 305: Busbar 400: Solar power generation system 401: Solar cell module 402: Converter 403: Battery 404: Load 500: Vehicle 501: Body 502: Solar cell module 503: Power conversion device 504: Battery 505: Motor 506: Tires (wheels) 600: Flying object 601: Aircraft frame 602: Motor 603: Rotor 604: Control unit
Claims
1. A p-electrode; An n-electrode; a p-type light absorbing layer provided on the p-electrode and including a first region and a second region; an n-type layer provided between the p-type light absorbing layer and the n-electrode; the first region is present on the n-type layer side of the p-type light absorbing layer, the second region is present on the p-electrode side of the p-type light absorbing layer, A solar cell, wherein a first average crystal grain size which is an average crystal grain size of the first region is larger than a second average crystal grain size which is an average crystal grain size of the second region.
2. 2. The solar cell according to claim 1, wherein the p-type light absorbing layer is mainly composed of cuprous oxide or a composite oxide of cuprous oxide.
3. The thickness of the p-type light absorbing layer is 2000 nm or more and 15000 nm or less, The solar cell according to claim 1 , wherein the second region has a thickness of 70 nm or more and 1000 nm or less.
4. The thickness of the second region is 70 nm or more and 1000 nm or less, The solar cell according to claim 1 , wherein the thickness of the second region is equal to or greater than 3% and less than 15% of the thickness of the p-type light absorbing layer.
5. The thickness of the second region is 150 nm or more and 600 nm or less, The solar cell according to claim 1 , wherein the thickness of the second region is equal to or greater than 3% and less than 15% of the thickness of the p-type light absorbing layer.
6. The solar cell according to claim 1 , wherein the first average crystal grain size is equal to or greater than 80% and less than 100% of a thickness of the p-type light absorbing layer.
7. The solar cell according to claim 1 , wherein the second average crystal grain size is not less than 0.005 μm and not more than 0.60 μm.
8. 2. The solar cell according to claim 1, wherein the maximum value of the crystal grain size in the second region is not less than 0.05 [μm] and not more than 2.00 [μm].
9. 2. The solar cell according to claim 1, wherein the ratio of the second average crystal grain size to the first average crystal grain size ([the second average crystal grain size] / [the first average crystal grain size]) is 0.005 or more and 0.300 or less.
10. The second region includes a void; 2. The solar cell according to claim 1, wherein the voids have an average cross-sectional diameter of 0.1 [mu]m or more and 0.6 [mu]m or less.
11. The solar cell according to claim 1 , wherein the area ratio of the voids to the cross section of the second region ([total cross-sectional area of the voids in the second region] / [cross-sectional area of the second region]) is 0.01 or more and 0.3 or less.
12. The solar cell according to claim 1 , wherein the area ratio of the voids to the cross section of the first region ([total cross-sectional area of the voids in the first region] / [cross-sectional area of the first region]) is greater than or equal to 0 and less than or equal to 0.
1.
13. the first region includes a void; the second region includes a void; The solar cell according to claim 1 , wherein an area ratio of the voids in the cross section of the first region to an area ratio of the voids in the cross section of the second region is 0.001 or more and 0.1 or less.
14. The solar cell according to claim 1 , wherein a particle size distribution in the second region in the range of 0.005 μm to 0.70 μm includes two peaks.
15. The particle size distribution in the second region in the range of 0.005 μm or more and 0.70 μm or less includes two peaks, The particle size distribution includes a first peak in the range of 0.005 [μm] or more and less than 0.30 [μm], The solar cell according to claim 1 , wherein the particle size distribution includes a second peak in the range of 0.30 μm to 0.70 μm.
16. The solar cell according to claim 15 , wherein a ratio of particles contained in the first peak or a ratio of particles contained in the second peak is 10% or more and 80% or less.
17. The solar cell according to claim 1 , wherein the crystal orientation of the grains in the second region is random.
18. 2. The solar cell according to claim 1, wherein the second region includes small voids having a cross-sectional diameter of 0.01 μm or more and less than 0.1 μm, and large voids having a cross-sectional diameter of 0.1 μm or more and 0.6 μm or less.
19. 2. The solar cell according to claim 1, wherein the second region contains one or more elements selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Fe, Ni, Pd, Ag, Zn, Cd, Al, Ga, In, C, Si, Ge, Sn, N, P, Sb, and Bi.
20. A multi-junction solar cell using the solar cell according to any one of claims 1 to 19.
21. A solar cell module using the solar cell according to any one of claims 1 to 19.
22. A solar power generation system that generates power using the solar cell module according to claim 21.
23. A p-electrode; An n-electrode; a p-type light absorbing layer provided on the p-electrode and including a first region having a large grain size and a second region having a small grain size; an n-type layer provided between the p-type light absorbing layer and the n-electrode; the first region is present on the n-type layer side of the p-type light absorbing layer, The second region is present on the p-electrode side of the p-type light absorbing layer.
Citation Information
Patent Citations
Photovoltaic cell with thin film cds layer
JP1996500209A
Solar power generation module
JP2018037615A
Solar cell, junction type solar cell, solar cell module and solar power generation system
JP2018056541A
CIGS solar cell and manufacturing method for the same
JP2016154171A
Cited By
Laminate, solar cell, multi-junction solar cell, solar cell module, solar power generation system, and method for manufacturing laminate