Toner, toner storage unit, image formation apparatus and image formation method
A bimodal toner with specific particle size distribution and surface area addresses contamination and scattering issues, enhancing transferability and image quality in toner technologies.
Patent Information
- Application Number
- JP2023046826
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing toner technologies face issues with high image defects such as fog and development streaks due to increased contacts and collisions between toners and toner carriers, leading to toner deterioration and contamination, especially when particle sizes are reduced for higher resolution and quality.
A toner composition with a bimodal particle size distribution, featuring a peak in the range of 4 μm to less than 8 μm and a secondary peak in 1 μm to less than 3 μm, with a specific intensity ratio and BET specific surface area between 2.0 m²/g to 4.0 m²/g, which minimizes scattering and enhances transferability and image quality.
The bimodal toner composition reduces in-machine contamination and improves transferability, enabling high-quality image formation with reduced defects.
Smart Images

Figure 2024135921000004 
Figure 2024135921000005 
Figure 2024135921000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner, a toner storage unit, an image forming apparatus, and an image forming method. [Background technology]
[0002] In recent years, image forming devices such as printers using toner have come to be widely used not only as office copy machines for copying text documents, but also as high-quality full-color output and high-definition computer output. Furthermore, as computers have become more commonplace, image forming devices have come to be used in the personal field, and as a result, low-temperature fixing properties have been required to reduce power consumption. For example, LED or LBP printers have become the mainstream of image forming devices in recent years, and the trend in technology is toward higher resolution. Accordingly, there is a demand for higher definition in the development method as well. In addition, copiers are also becoming more sophisticated, and as a result, they are moving toward digitalization. This is mainly a method of forming electrostatic images with a laser, so they are also moving toward higher resolution, and here too, like printers, there is a demand for high-resolution and high-definition development methods.
[0003] In recent years, there has been a demand for high image quality using toner, and reducing the average particle size of the toner is one effective means for improving graininess and character reproducibility. However, reducing the particle size of the toner increases the frequency of contact and collision between toner particles or between the toner and the toner carrier or toner regulating member, making the toner more susceptible to deterioration, and can lead to problems such as contamination of the toner carrier or toner regulating member by the toner, resulting in image defects such as fog and development streaks. In response to the above problems, for example, a toner has been proposed which is composed of a binder resin, a colorant, a wax component, and inorganic fine powder, and in the particle size distribution, has a number average particle size D1(T) of 3.0 μm to 8.0 μm, a coefficient of variation of the number-based particle size distribution of 35.0 or less, and a ratio of particles with a number average particle size of less than 2.0 μm of 1.0 to 15.0% by number (see, for example, Patent Document 1). Also, a toner has been proposed in which the particle size of the toner particles is 0.5 to 5.0 μm in number average particle size, and the content of toner particles having a size of 6.0 μm or more is 5% by number or less (see, for example, Patent Document 2). Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a toner which has excellent transferability, is capable of forming high-quality images, and is capable of suppressing contamination inside a machine. [Means for solving the problem]
[0005] The toner of the present invention as a means for solving the above problems is The number particle size distribution has a maximum peak in the range of 4 μm or more and less than 8 μm, and a second peak in the range of 1 μm or more and less than 3 μm, When the particle size of the second peak in the number particle size distribution is X μm, the ratio A / B of the intensity A of the particle size of X μm in the volume particle size distribution to the intensity B of the maximum peak in the range of 4 μm or more and less than 8 μm in the volume particle size distribution is 0.2 or less, The BET specific surface area of the toner base particles and the BET specific surface area of the toner particles less than 5 μm in the volume particle size distribution are 2.0 m 2 / g or more 4.0m 2 / g or less. Effect of the Invention
[0006] According to the present invention, it is possible to provide a toner that has excellent transferability, is capable of forming high-quality images, and is capable of suppressing contamination inside a machine. [Brief description of the drawings]
[0007] [Figure 1A] FIG. 1A is a schematic diagram showing an example of the number particle size distribution and the volume particle size distribution of the toner base particles having a small particle size (1 μm or more and less than 3 μm: added toner) of the toner of the present invention. [Figure 1B]FIG. 1B is a schematic diagram showing an example of the number particle size distribution and the volume particle size distribution of the toner base particles having a normal particle size (4 μm or more and less than 8 μm: main toner) of the toner of the present invention. [Figure 1C] FIG. 1C is a schematic diagram showing an example of the number particle size distribution and the volume particle size distribution of the toner of the present invention, which is a mixture of the additive toner and the main toner. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the image forming apparatus of the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing another example of the image forming apparatus of the present invention. [Figure 4] FIG. 4 is a schematic diagram showing another example of the image forming apparatus of the present invention. [Diagram 5] FIG. 5 is a schematic diagram showing another example of the image forming apparatus of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] (toner) The toner of the present invention contains a binder resin and a release agent, and further contains other components as required. The toner of the present invention has a maximum peak in the range of 4 μm or more and less than 8 μm in the number particle size distribution, and a second peak in the range of 1 μm or more and less than 3 μm, When the particle size of the second peak in the number particle size distribution is X μm, the ratio A / B of the intensity A of the particle size of X μm in the volume particle size distribution to the intensity B of the maximum peak in the range of 4 μm or more and less than 8 μm in the volume particle size distribution is 0.2 or less, The BET specific surface area of the toner base particles and the BET specific surface area of the toner particles less than 5 μm in the volume particle size distribution are 2.0 m 2 / g or more 4.0m 2 / g or less.
[0009] The method for measuring the volumetric particle size distribution of the toner is not particularly limited and can be appropriately selected depending on the purpose. For example, the measurement can be performed using a particle size measuring device. Specifically, it can be measured using a Multisizer3 (manufactured by Beckman Coulter, Inc.).
[0010] The method for measuring the number particle size distribution of the toner is not particularly limited and may be appropriately selected depending on the purpose. For example, the method may be measured using a particle size measuring device. Specifically, it can be measured using a Multisizer3 (manufactured by Beckman Coulter, Inc.).
[0011] It is already known in Patent Documents 1 and 2 that small particle size can be used to achieve high image quality, but small particle size can cause problems such as toner deterioration and scattering inside the machine, so no manufacturer has been able to address this issue. By adding a small particle size toner that is less likely to scatter, it is possible to provide a toner that can be used to achieve high image quality while suppressing scattering inside the machine. It is known that the BET specific surface area is inversely proportional to the particle size, and it has not been possible to reduce the BET specific surface area of only the small particle size toner in the toner distribution. On the other hand, if one tries to reduce the BET specific surface area of the entire toner distribution, the BET specific surface area of the normal particle size toner also becomes small, resulting in a problem that the charging performance decreases and the toner no longer functions as a toner.
[0012] Therefore, the inventors conducted extensive research and found that by mixing small particle size (number average particle size of 1 μm or more and less than 3 μm: additive toner) toner base particles with normal particle size (4 μm or more and less than 8 μm: main toner) toner base particles, it is possible to obtain a BET specific surface area suitable for the particle size, suppress toner scattering, and form high-quality images. In the toner of the present invention, in the filtration step of the toner production method, the fine powder passing through the filter cloth is collected together with the filtrate, and the filtrate is heated to eliminate cavities in the fine powder, thereby producing a toner that is difficult to charge. The filtrate is dried to extract only the fine powder, which is then added to a normal toner, thereby producing a toner that contains fine powder that is difficult to scatter and has excellent image quality.
[0013] FIG. 1A is a schematic diagram showing an example of the number particle size distribution and the volume particle size distribution of the toner base particles having a small particle size (1 μm or more and less than 3 μm: added toner) of the toner of the present invention. FIG. 1B is a schematic diagram showing an example of the number particle size distribution and the volume particle size distribution of the toner base particles having a normal particle size (4 μm or more and less than 8 μm: main toner) of the toner of the present invention. FIG. 1C is a schematic diagram showing an example of the number particle size distribution and the volume particle size distribution of the toner of the present invention, which is a mixture of the additive toner and the main toner. The toner of the present invention has a maximum peak in the range of 4 μm or more and less than 8 μm, and a second peak in the range of 1 μm or more and less than 3 μm, as shown in the number particle size distribution in Fig. 1C. When the particle size of the second peak is X μm, the ratio A / B of the intensity A of the particle size X μm in the volume particle size distribution to the intensity B of the maximum peak in the range of 4 μm or more and less than 8 μm in the volume particle size distribution is 0.2 or less.
[0014] The toner has a ratio A / B of 0.2 or less between the intensity A of the particle size X μm in the volume particle size distribution and the intensity B of the maximum peak in the range of 4 μm or more and less than 8 μm in the volume particle size distribution, where A is the particle size of the second peak in the number particle size distribution, when the particle size is X μm. This makes it possible to obtain a toner with excellent blade cleaning properties.
[0015] The toner has a BET specific surface area of the toner base particles and a BET specific surface area of the toner particles of less than 5 μm in the volume particle size distribution of 2.0 m 2 / g or more 4.0m 2 This makes it possible to provide a toner with excellent blade cleaning properties.
[0016] The BET specific surface area (m 2 The method for measuring the specific surface area (g) is not particularly limited and can be appropriately selected depending on the purpose. For example, it can be measured using a BET specific surface area measuring device. Specifically, the measurement can be performed using a TriStar 3000 (manufactured by Shimadzu Corporation).
[0017] The BET specific surface area (m 2 / g) is not particularly limited and can be appropriately selected depending on the purpose, but the BET specific surface area (m 2 / g) or less is preferred. In addition, the BET specific surface area (m 2 / g) is 2.0m 2 / g or more 4.0m 2 / g is preferred.
[0018] <Binding resin> The binder resin is not particularly limited and can be appropriately selected according to the purpose. For example, polyester resin, silicone resin, styrene-acrylic resin, styrene resin, acrylic resin, epoxy resin, diene resin, phenol resin, terpene resin, coumarin resin, amide-imide resin, butyral resin, urethane resin, ethylene vinyl acetate resin, etc. can be mentioned. These may be used alone or in combination of two or more. Among these, polyester resin and resins combining polyester resin with other binder resins are preferred in terms of excellent low-temperature fixing property and sufficient flexibility even when the molecular weight is reduced.
[0019] -Polyester resin- The polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but unmodified polyester resins and modified polyester resins are preferred. These may be used alone or in combination of two or more.
[0020] --Unmodified polyester resin-- The unmodified polyester resin is not particularly limited and can be appropriately selected depending on the purpose. For example, it may be a polyester resin obtained by polyesterifying a polyol represented by the following general formula (1) and a polycarboxylic acid represented by the following general formula (2), or a crystalline polyester resin. [ka] In the general formula (1), A represents an alkyl group, an alkylene group, an aromatic group or a heterocyclic aromatic group having 1 to 20 carbon atoms, which may have a substituent; and m represents an integer of 2 to 4. In addition, in the general formula (2), B represents an alkyl group, an alkylene group, an aromatic group or a heterocyclic aromatic group having 1 to 20 carbon atoms, which may have a substituent; The polyol represented by the general formula (1) is not particularly limited and can be appropriately selected according to the purpose. For example, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,4-butenediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, 1,3,5-trihydroxymethylbenzene, etc. can be mentioned. These may be used alone or in combination of two or more.
[0021] The polycarboxylic acid represented by the general formula (2) is not particularly limited and can be appropriately selected depending on the purpose. For example, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, n-dodecenylsuccinic acid, isooctylsuccinic acid, isododecenylsuccinic acid, n-dodecylsuccinic acid, isododecylsuccinic acid, n-octenylsuccinic acid, n-octylsuccinic acid, isooctylsuccinic acid, isooctylsuccinic acid, 1,2,4-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarb Examples of such compounds include carboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, empol trimer acid, cyclohexanedicarboxylic acid, cyclohexenedicarboxylic acid, butanetetracarboxylic acid, diphenylsulfonetetracarboxylic acid, and ethylene glycol bis(trimellitic acid). These compounds may be used alone or in combination of two or more.
[0022] --Modified polyester resin-- The modified polyester resin is not particularly limited and can be appropriately selected according to the purpose. For example, a resin obtained by elongation reaction and / or crosslinking reaction of an active hydrogen group-containing compound and a polyester (hereinafter, sometimes referred to as "polyester prepolymer") that can react with the active hydrogen group-containing compound can be mentioned. The elongation reaction and / or crosslinking reaction may be terminated by a reaction terminator (diethylamine, dibutylamine, butylamine, laurylamine, ketimine compound, or the like, which is a blocked monoamine).
[0023] ---Compounds containing active hydrogen groups--- The active hydrogen group-containing compound acts as an elongation agent, a crosslinking agent, etc. when the polyester prepolymer undergoes an elongation reaction, a crosslinking reaction, etc. in the aqueous phase. The active hydrogen group-containing compound is not particularly limited as long as it has an active hydrogen group, and can be appropriately selected according to the purpose. Among them, when the polyester prepolymer is an isocyanate group-containing polyester prepolymer described later, amines are preferred because they can be made into a high molecular weight. The active hydrogen group is not particularly limited and can be appropriately selected according to the purpose. For example, hydroxyl group (alcoholic hydroxyl group or phenolic hydroxyl group), amino group, carboxyl group, mercapto group, etc. can be included. These may be included alone or in combination of two or more. The amines, which are the active hydrogen group-containing compounds, are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include diamines, trivalent or higher polyamines, amino alcohols, amino mercaptans, amino acids, and amines obtained by blocking the amino groups of these amines. Examples of the diamine include aromatic diamines (phenylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenylmethane, etc.); alicyclic diamines (4,4'-diamino-3,3'-dimethyldicyclohexylmethane, diaminecyclohexane, isophoronediamine, etc.); and aliphatic diamines (ethylenediamine, tetramethylenediamine, hexamethylenediamine, etc.). Examples of the trivalent or higher polyamines include diethylenetriamine and triethylenetetramine. Examples of the amino alcohol include ethanolamine and hydroxyethylaniline. Examples of the amino mercaptan include aminoethyl mercaptan and aminopropyl mercaptan. Examples of the amino acid include aminopropionic acid and aminocaproic acid. Examples of compounds in which the amino group of these amines is blocked include ketimine compounds and oxazoline compounds obtained from any of these amines (diamines, trivalent or higher polyamines, amino alcohols, amino mercaptans, amino acids, etc.) and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.). These may be used alone or in combination of two or more. Among these, the amines are particularly preferably diamines or mixtures of diamines with a small amount of trivalent or higher polyamines.
[0024] ---Polymers that can react with compounds containing active hydrogen groups--- The polymer capable of reacting with the active hydrogen group-containing compound is not particularly limited as long as it is a polymer having at least a group capable of reacting with the active hydrogen group-containing compound, and can be appropriately selected according to the purpose. Among them, urea bond-forming group-containing polyester resin (RMPE) is preferred, and isocyanate group-containing polyester prepolymer is more preferred, in terms of high fluidity and excellent transparency when melted, ease of adjusting the molecular weight of the polymer component, and excellent oil-less low-temperature fixing property and release property in dry toner.
[0025] The isocyanate group-containing polyester prepolymer is not particularly limited and may be appropriately selected depending on the purpose. For example, a polycondensation product of a polyol and a polycarboxylic acid, or a product obtained by reacting an active hydrogen group-containing polyester resin with a polyisocyanate may be mentioned.
[0026] The polyol is not particularly limited and can be appropriately selected according to the purpose. For example, alkylene glycol (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, etc.), alkylene ether glycol (diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, etc.), alicyclic diol (1,4-cyclohexanedimethanol, hydrogenated bisphenol A, etc.), bisphenols (bisphenol A, bisphenol F, bisphenol S, etc.), polyhydric aliphatic alcohols (glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, etc.), trihydric or higher phenols (phenol novolac, cresol novolac, etc.), alkylene oxide adducts of trihydric or higher polyphenols, trihydric or higher polyols, mixtures of diols and trihydric or higher polyols, etc. These may be used alone or in combination of two or more. Among these, the polyol is preferably the diol alone or a mixture of the diol with a small amount of the trihydric or higher polyol.
[0027] The diol preferably contains as a main component an alkylene glycol having 2 to 12 carbon atoms or an alkylene oxide adduct of a bisphenol (a 2-mol ethylene oxide adduct of bisphenol A, or a 3-mol ethylene oxide adduct of bisphenol A).Alkylene glycols (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, etc.) may also be used for the purpose of adjusting the molecular weight or molecular weight mobility.
[0028] The content of the polyol in the isocyanate group-containing polyester prepolymer is not particularly limited and can be appropriately selected according to the purpose. For example, it is preferably 0.5% by mass or more to 40% by mass, more preferably 1% by mass or more to 30% by mass or less, and particularly preferably 2% by mass or more to 20% by mass or less. If the content is less than 0.5% by mass, the hot offset resistance may deteriorate, and it may be difficult to achieve both the storage stability and low-temperature fixability of the toner, and if it exceeds 40% by mass, the low-temperature fixability may deteriorate.
[0029] The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. For example, alkylene dicarboxylic acid (succinic acid, adipic acid, sebacic acid, etc.); alkenylene dicarboxylic acid (maleic acid, fumaric acid, etc.); aromatic dicarboxylic acid (terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid, etc.); trivalent or higher polycarboxylic acid (aromatic polycarboxylic acid having 9 to 20 carbon atoms such as trimellitic acid and pyromellitic acid, etc.) can be mentioned. These can be used alone or in combination of two or more kinds. Among these, the polycarboxylic acid is preferably an alkenylene dicarboxylic acid having 4 to 20 carbon atoms, or an aromatic dicarboxylic acid having 8 to 20 carbon atoms. Instead of the polycarboxylic acid, anhydrides and lower alkyl esters (methyl ester, ethyl ester, isopropyl ester, etc.) of polycarboxylic acid may be used.
[0030] The mixing ratio of the polyol and the polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. The equivalent ratio [OH] / [COOH] of the hydroxyl group [OH] of the polyol to the carboxyl group [COOH] of the polycarboxylic acid is preferably 2 / 1 to 1 / 1, more preferably 1.5 / 1 to 1 / 1, and particularly preferably 1.3 / 1 to 1.02 / 1.
[0031] The polyisocyanate is not particularly limited and can be appropriately selected depending on the purpose. For example, aliphatic polyisocyanates (tetramethylene diisocyanate, hexamethylene diisocyanate, 2,6-diisocyanatomethyl caproate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, tetramethylhexane diisocyanate, etc.); alicyclic polyisocyanates (isophorone diisocyanate, cyclohexylmethane diisocyanate, etc.); aromatic diisocyanates (tolylene diisocyanate, diphenylmethane diisocyanate, 1,5- naphthylene diisocyanate, diphenylene-4,4'-diisocyanate, 4,4'-diisocyanato-3,3'-dimethyldiphenyl, 3-methyldiphenylmethane-4,4'-diisocyanate, diphenylether-4,4'-diisocyanate, etc.); aromatic aliphatic diisocyanates (α,α,α',α'-tetramethylxylylene diisocyanate, etc.); isocyanurates (tris-isocyanatoalkyl-isocyanurate, triisocyanatocycloalkyl-isocyanurate, etc.); phenol derivatives thereof; those blocked with oxime, caprolactam, etc. These may be used alone or in combination of two or more.
[0032] The mixing ratio of the polyisocyanate and the active hydrogen group-containing polyester resin (hydroxyl group-containing polyester resin) is not particularly limited and can be appropriately selected according to the purpose. The equivalent ratio [NCO] / [OH] of the isocyanate group [NCO] of the polyisocyanate and the hydroxyl group [OH] of the hydroxyl group-containing polyester resin is preferably 5 / 1 to 1 / 1, more preferably 4 / 1 to 1.2 / 1, and particularly preferably 3 / 1 to 1.5 / 1. If the equivalent ratio [NCO] / [OH] is less than 1 / 1, the offset resistance may deteriorate, and if it exceeds 5 / 1, the low temperature fixability may deteriorate.
[0033] The content of the polyisocyanate in the isocyanate group-containing polyester prepolymer is not particularly limited and can be appropriately selected according to the purpose. It is preferably 0.5% by mass or more and 40% by mass or less, more preferably 1% by mass or more and 30% by mass or less, and particularly preferably 2% by mass or more and 20% by mass or less. If the content is less than 0.5% by mass, the hot offset resistance may deteriorate, and it may be difficult to achieve both storage stability and low-temperature fixability, and if it exceeds 40% by mass, the low-temperature fixability may deteriorate.
[0034] The average number of isocyanate groups contained per molecule of the isocyanate group-containing polyester prepolymer is preferably 1 or more, more preferably 1.2 to 5, and even more preferably 1.5 to 4. If the average number is less than 1, the molecular weight of the polyester resin modified with a urea bond-forming group (RMPE) becomes low, and the hot offset resistance may deteriorate.
[0035] The mixing ratio of the isocyanate group-containing polyester prepolymer and the amines is not particularly limited and can be appropriately selected according to the purpose. The mixing equivalent ratio [NCO] / [NHx] of the isocyanate group [NCO] in the isocyanate group-containing polyester prepolymer and the amino group [NHx] in the amines is preferably 1 / 3 to 3 / 1, more preferably 1 / 2 to 2 / 1, and particularly preferably 1 / 1.5 to 1.5 / 1. If the mixing equivalent ratio ([NCO] / [NHx]) is less than 1 / 3, low-temperature fixability may decrease, and if it exceeds 3 / 1, the molecular weight of the urea-modified polyester resin may decrease, resulting in poor hot offset resistance.
[0036] ---Method for synthesizing polymers capable of reacting with compounds containing active hydrogen groups--- The synthesis method of the polymer that can react with the active hydrogen group-containing compound is not particularly limited and can be appropriately selected according to the purpose.For example, in the case of the isocyanate group-containing polyester prepolymer, the polyol and the polycarboxylic acid are heated to 150°C to 280°C in the presence of a known esterification catalyst (titanium tetrabutoxide, dibutyltin oxide, etc.), and if necessary, the polyol and the polycarboxylic acid are generated while being appropriately reduced pressure, and water is distilled off to obtain a hydroxyl group-containing polyester, and then the hydroxyl group-containing polyester is reacted with the polyisocyanate at 40°C to 140°C to synthesize the polyester.
[0037] The weight average molecular weight (Mw) of the polymer capable of reacting with the active hydrogen group-containing compound is not particularly limited and can be appropriately selected according to the purpose. The molecular weight distribution of the tetrahydrofuran (THF) soluble matter by GPC (gel permeation chromatography) is preferably 3,000 to 40,000, more preferably 4,000 to 30,000. If the weight average molecular weight (Mw) is less than 3,000, the storage stability may deteriorate, and if it exceeds 40,000, the low temperature fixability may deteriorate.
[0038] The weight average molecular weight (Mw) can be measured, for example, as follows. First, a column is stabilized in a heat chamber at 40° C., tetrahydrofuran (THF) is passed as a column solvent at this temperature at a flow rate of 1 mL per minute, and 50 μL to 200 μL of a tetrahydrofuran sample solution of the resin, the sample concentration of which is adjusted to 0.05% by mass to 0.6% by mass, is injected and measured. When measuring the molecular weight of the sample, the molecular weight distribution of the sample is calculated from the relationship between the logarithm of a calibration curve prepared from several types of monodisperse polystyrene standard samples and the count number.
[0039] Standard polystyrene samples for creating the calibration curve were manufactured by Pressure Chemical Co. or Toyo Soda Kogyo Co., Ltd., with molecular weights of 6×10 and 2.1×10. 2 , 4×10 2 , 1.75×10 4 , 1.1×10 5 , 3.9×105 , 8.6×10 5 , 2×10 6 , and 4.48×10 6 It is preferable to use at least about 10 standard polystyrene samples. As a detector, an RI (refractive index) detector can be used.
[0040] The content of the binder resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 70% by mass or more and 90% by mass or less with respect to the toner.
[0041] <Release agent> The release agent is not particularly limited and can be appropriately selected according to the purpose. For example, waxes and waxes such as vegetable wax (carnauba wax, cotton wax, wood wax, rice wax, etc.), animal wax (beeswax, lanolin, etc.), mineral wax (ozokerite, cerusine, etc.), petroleum wax (paraffin, microcrystalline, petrolatum, etc.); synthetic hydrocarbon wax (Fischer-Tropsch wax, polyethylene wax, etc.), synthetic wax (ester, ketone, ether, etc.) and other waxes other than natural wax; fatty acid amides such as 1,2-hydroxystearic acid amide, stearic acid amide, phthalic anhydride imide, chlorinated hydrocarbon; crystalline polymers having long chain alkyl groups on the side chain, such as polyacrylate homopolymers or copolymers (acrylic acid n-stearyl-methacrylate ethyl copolymers, etc.) such as polymethacrylate n-lauryl, which is a low molecular weight crystalline polymer; and the like. Among these, Fischer-Tropsch wax, paraffin wax, microcrystalline wax, monoester wax, and rice wax are preferred in that they generate less unnecessary volatile organic compounds during fixing.
[0042] The release agent may be a commercially available product. Examples of the microcrystalline wax include "HI-MIC-1045", "HI-MIC-1070", "HI-MIC-1080", and "HI-MIC-1090" manufactured by Nippon Seiro Co., Ltd., "B-Square 180 White" and "B-Square 195" manufactured by Toyo Adle Co., Ltd., "BARECO C-1035" manufactured by WAXPetrolife Co., Ltd., and "CRAYVALLAC WN-1442" manufactured by Cray Valley Co., Ltd.
[0043] The melting point of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 60° C. to 100° C., and more preferably 65° C. to 90° C. A melting point of 60° C. or higher can suppress the exudation of the release agent from the toner matrix even during high-temperature storage at about 30 to 50° C., and can maintain good heat-resistant storage stability, while a melting point of 100° C. or lower is preferable because cold offset is less likely to occur during fixing at low temperatures.
[0044] The method for measuring the melting point is not particularly limited and can be appropriately selected depending on the purpose. For example, the melting point can be measured using TA-60WS and DSC-60 manufactured by Shimadzu Corporation under the following measurement conditions. (Measurement conditions) Sample container: Aluminum sample pan (with lid) Sample size: 5mg Reference: Aluminum sample pan (alumina 10 mg) Atmosphere: Nitrogen (flow rate 50mL / min) Temperature conditions 1st heating Start temperature: 20℃, heating rate: 10℃ / min, end temperature: 150℃, holding time: none 1st. Temperature drop Temperature drop temperature: 10℃ / min, End temperature: 20℃, Holding time: None 2nd. Temperature increase: Temperature increase rate: 10℃ / min, End temperature: 150℃ The measured results are analyzed using data analysis software (TA-60, version 1.52) manufactured by Shimadzu Corporation. The melting point is the temperature at the top of the endothermic peak measured in the second heating step. The release agent is preferably present in a dispersed state in the toner base particles, and therefore, it is preferable that the release agent and the binder resin are not compatible with each other. The method for finely dispersing the release agent in the toner base particles is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include a method of dispersing the release agent by applying a shear force during kneading during toner production. The dispersion state of the release agent can be confirmed by observing a thin film slice of the toner particles with a transmission electron microscope (TEM). The smaller the dispersion diameter of the release agent, the better, but if it is too small, there is a possibility that the exudation during fixing is insufficient. Therefore, if the release agent can be confirmed at a magnification of 10,000 times, it means that the release agent is present in a dispersed state. If the release agent cannot be confirmed at a magnification of 10,000 times, even if it is finely dispersed, the exudation during fixing is insufficient.
[0045] The content of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 3% by mass or more and 15% by mass or less, and more preferably 5% by mass or more and 10% by mass or less, based on the toner. When the content is 3% by mass or more, hot offset resistance is excellent. When the content is 15% by mass or less, the amount of exudation of the release agent during fixing becomes appropriate, and heat resistance storage stability is excellent.
[0046] <Other ingredients> The other components are not particularly limited and may be appropriately selected depending on the purpose. Examples of the other components include colorants, organically modified layered inorganic minerals, charge control agents, and external additives.
[0047] -Coloring agent- The colorant used in the toner is not particularly limited, and can be appropriately selected from known colorants depending on the purpose. The color of the colorant of the toner can be at least one selected from yellow toners, and can be obtained by appropriately selecting the type of colorant.
[0048] Examples of yellow coloring pigments include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 55, 65, 73, 74, 83, 97, 110, 139, 151, 154, 155, 180, and 185; CI Bat Yellow 1, 3, 20, and Orange 36.
[0049] The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1% by mass or more and 15% by mass or less, and more preferably 3% by mass or more and 10% by mass or less. When the content is 1% by mass or more, the toner has excellent coloring power. When the content is 15% by mass or less, poor dispersion of the pigment in the toner is suppressed, and the toner has excellent coloring power and electrical properties.
[0050] The colorant may be used as a master batch combined with a resin. There are no particular limitations on the resin, but it is preferable to use a binder resin or a resin having a structure similar to that of the binder resin in terms of compatibility with the binder resin.
[0051] The master batch can be produced by mixing or kneading the resin and the colorant under high shear force. In this case, it is preferable to add an organic solvent to enhance the interaction between the colorant and the resin. The so-called flushing method is also suitable in that the wet cake of the colorant can be used as is and does not need to be dried. The flushing method is a method in which an aqueous paste containing water of the colorant is mixed or kneaded with the resin and the organic solvent, and the colorant is transferred to the resin side to remove the water and the organic solvent. For example, a high shear dispersion device such as a three-roll mill can be used for mixing or kneading.
[0052] -Organic modified layered inorganic mineral- The organic modified layered inorganic mineral is an organic modified layered inorganic mineral in which at least a part of the ions present between layers of the layered inorganic mineral is modified with an organic ion. The layered inorganic mineral is a layered inorganic mineral formed by stacking layers having a thickness of several nm. The term "modified" is synonymous with the introduction of an organic ion into the ions present between the layers of the layered inorganic mineral, and in a broad sense, is intercalation.
[0053] It is known that the organic layered inorganic mineral exerts the greatest effect when it is disposed near the surface, and is likely to be disposed near the surface. In addition, it is desirable that the organically modified layered inorganic mineral in the present invention is contained in the toner particles at a uniform ratio regardless of the size of the toner particle diameter. Therefore, the organically modified layered inorganic mineral is uniformly disposed near the surface of each toner particle. As a result, for example, the content of the organically modified layered inorganic mineral is small in toner particles with a small particle diameter, and therefore the ratio of the organically modified layered inorganic mineral disposed on the surface is reduced, the toner particle surface becomes relatively soft, and the external additive added to the toner base material is easily embedded, which has the effect of avoiding the phenomenon that the detachment of the external additive, which is advantageous for imparting fluidity to the toner, is hindered.
[0054] Here, the state of the organically modified layered inorganic mineral in the toner can be confirmed by cutting a sample in which toner particles are embedded in epoxy resin or the like with a micromicrotome or ultramicrotome, and observing the cross section of the toner with a scanning electron microscope (SEM) or the like. In the case of observation with an SEM, it is preferable to confirm with a backscattered electron image, since the presence of the organically modified layered inorganic mineral can be observed with strong contrast. Alternatively, a FIB-STEM (HD-2000, manufactured by Hitachi, Ltd.) may be used to cut a sample in which toner particles are embedded in epoxy resin or the like with an ion beam, and the cross section of the toner may be observed. In this case, too, it is preferable to confirm with a backscattered electron image, since it is easy to visually confirm.
[0055] In addition, the vicinity of the toner surface referred to in the present invention is defined as a region from the outermost surface of the toner to 0 nm to 300 nm inside the toner in an observation image of a cross section of the toner obtained by cutting a sample in which toner particles are embedded in an epoxy resin or the like with a micromicrotome, ultramicrotome, or FIB-STEM.
[0056] The organic layered inorganic mineral is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include smectite group clay minerals (montmorillonite, saponite, hectorite, etc.), kaolin group clay minerals (kaolinite, etc.), bentonite, attapulgite, magadiite, kanemite, etc. These may be used alone or in combination of two or more.
[0057] The organically modified layered inorganic mineral is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include organically modified layered inorganic minerals in which at least a part of the ions present between the layers of the layered inorganic minerals are modified with organic ions. Among these, smectite group clay minerals having a basic smectite crystal structure in which at least a part of the ions between the layers are modified with organic cations are preferred from the viewpoint of dispersion stability in the vicinity of the toner surface, and montmorillonite in which at least a part of the ions between the layers are modified with organic cations and bentonite in which at least a part of the ions between the layers are modified with organic cations are particularly preferred.
[0058] The organically modified layered inorganic mineral can be confirmed by gas chromatography mass spectrometry (GCMS) that at least a part of the ions present between the layers of the layered inorganic mineral are modified with organic ions. For example, a suitable method is to filter a solution in which the binder resin in the toner sample is dissolved in a solvent, to pyrolyze the obtained solid matter in a pyrolysis device, and to identify the structure of the organic matter by GCMS. Specifically, a pyrolysis device is used, Py-2020D (manufactured by Frontier Labs), and the pyrolysis is performed at 550°C, and then the structure is identified by a GCMS device QP5000 (manufactured by Shimadzu Corporation).
[0059] Further, the organically modified layered inorganic mineral may be a layered inorganic compound in which a part of the divalent metal of the layered inorganic mineral is replaced with a trivalent metal to introduce a metal anion, and at least a part of the metal anion is further modified with an organic anion.
[0060] The organically modified layered inorganic mineral may be a commercially available product. Examples of the commercially available product include quaternium 18 bentonite such as Bentone 3, Bentone 38, Bentone 38V (manufactured by Rheox), Thixogel VP (manufactured by United Catalyst), Kraton 34, Kraton 40, and Kraton XL (manufactured by Southern Clay); stearalkonium bentonite such as Bentone 27 (manufactured by Rheox), Thixogel LG (manufactured by United Catalyst), Kraton AF, and Kraton APA (manufactured by Southern Clay); quaternium 18 / benzalkonium bentonite such as Kraton HT and Kraton PS (manufactured by Southern Clay); organically modified montmorillonite such as Kraton HY (manufactured by Southern Clay); and organically modified sucmetite such as Lucentite SPN (manufactured by Co-op Chemical). Among these, Kraton AF and Kraton APA are particularly preferred.
[0061] The organically modified layered inorganic mineral is DHT-4A (manufactured by Kyowa Chemical Industry Co., Ltd.) 1 (OR 2 )nOSO 3 M (where R 1 is an alkyl group with 13 carbon atoms, R 2 is an alkylene group having 2 to 6 carbon atoms, n is an integer of 2 to 10, and M is a monovalent metal element). 1 (OR 2 )nOSO 3 An example of the compound having the organic ion represented by M is Hitenol 330T (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).
[0062] The organically modified layered inorganic mineral may be mixed with a resin to be used as a composite master batch. The resin is not particularly limited and may be appropriately selected from known resins depending on the purpose.
[0063] The organic ion modifier, which is a compound having the organic ion and capable of modifying at least a part of the ions present between the layers of the layered inorganic mineral to organic ions, is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include quaternary alkyl ammonium salts, phosphonium salts, imidazolium salts; branched, unbranched or cyclic alkyl having 1 to 44 carbon atoms, branched, unbranched or cyclic alkenyl having 1 to 22 carbon atoms, branched, unbranched or cyclic alkoxy having 8 to 32 carbon atoms, branched, unbranched or cyclic hydroxyalkyl having 2 to 22 carbon atoms, sulfates having a skeleton such as ethylene oxide or propylene oxide, sulfonates having the skeleton, carboxylates having the skeleton, and phosphates having the skeleton. Among these, quaternary alkyl ammonium salts and carboxylic acids having an ethylene oxide skeleton are preferred, and quaternary alkyl ammonium salts are particularly preferred. These may be used alone or in combination of two or more.
[0064] Examples of the quaternary alkyl ammonium include trimethylstearyl ammonium, dimethylstearylbenzyl ammonium, dimethyloctadecyl ammonium, and oleylbis(2-hydroxyethyl)methyl ammonium.
[0065] The content of the organically modified layered inorganic mineral is not particularly limited and can be appropriately selected according to the purpose, but is preferably 0.1% by mass to 3.0% by mass, more preferably 0.3% by mass to 1.5% by mass, based on the toner. When the content is 0.1% by mass or more, the effect of the layered inorganic mineral is exerted. When the content is 3.0% by mass or less, low-temperature fixing property is excellent.
[0066] -Charge control agent- Any known charge control agent can be used as the charge control agent. Since the use of a colored material may cause a change in color tone, a colorless or nearly white material is preferred, and examples thereof include triphenylmethane dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus alone or its compounds, tungsten alone or its compounds, fluorine-based activators, metal salts of salicylic acid, and metal salts of salicylic acid derivatives. These may be used alone or in combination of two or more.
[0067] The content of the charge control agent is determined by the type of binder resin and the toner manufacturing method including the dispersion method, and is not uniquely limited, but is preferably 0.01% by mass to 5% by mass relative to the binder resin, and more preferably 0.02% by mass to 2% by mass. If the amount added exceeds 5% by mass, the chargeability of the toner becomes too high, reducing the effect of the charge control agent, increasing the electrostatic attraction force with the developing roller, which may lead to a decrease in the fluidity of the developer and a decrease in image density, and if it is less than 0.01% by mass, the charge rise property and charge amount are insufficient, which may easily affect the toner image.
[0068] <External additives> The external additive is not particularly limited, and can be appropriately selected from known additives according to purpose.For example, silica fine particles, hydrophobized silica fine particles, fatty acid metal salts (e.g. zinc stearate, aluminum stearate, etc.), metal oxides (e.g. titania, alumina, tin oxide, antimony oxide, etc.) or their hydrophobic counterparts, fluoropolymers, etc. are included.Among these, hydrophobized silica fine particles, titania particles, and hydrophobized titania fine particles are preferably included. Examples of the hydrophobic silica fine particles include HDK H2000T, HDK H2000 / 4, HDK H2050EP, HVK21, HDK H1303VP (all manufactured by Clariant Japan); R972, R974, RX200, RY200, R202, R805, R812, NX90G (all manufactured by Nippon Aerosil Co., Ltd.).
[0069] Examples of the titania microparticles include P-25 (manufactured by Nippon Aerosil Co., Ltd.); STT-30, STT-65C-S (both manufactured by Titanium Kogyo Co., Ltd.); TAF-140 (manufactured by Fuji Titanium Kogyo Co., Ltd.); MT-150W, MT-500B, MT-600B, MT-150A (all manufactured by Teika Co., Ltd.); and the like. Examples of the hydrophobic titanium oxide fine particles include T-805 (manufactured by Nippon Aerosil Co., Ltd.); STT-30A, STT-65S-S (both manufactured by Titanium Kogyo Co., Ltd.); TAF-500T, TAF-1500T (both manufactured by Fuji Titanium Kogyo Co., Ltd.); MT-100S, MT-100T (both manufactured by Teika Co., Ltd.); and IT-S (manufactured by Ishihara Sangyo Co., Ltd.).
[0070] The content of the external additive is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.3 parts to 3.0 parts, and more preferably 0.5 parts to 2.0 parts, based on 100 parts of the toner base particles. The total coverage of the external additives with respect to the toner base particles is not particularly limited, but is preferably from 50% to 90%, and more preferably from 60% to 80%.
[0071] <Toner manufacturing method> The toner manufacturing method and materials in the present invention may be any known method and material that satisfies the conditions, and are not particularly limited. Examples of the method and materials include a kneading and grinding method and a so-called chemical method in which toner particles are granulated in an aqueous medium.
[0072] Examples of the chemical method include suspension polymerization, emulsion polymerization, seed polymerization, and dispersion polymerization, which are produced using a monomer as a starting material; a dissolution suspension method in which a resin or a resin precursor is dissolved in an organic solvent and dispersed or emulsified in an aqueous medium; a method in which an oil phase composition containing a resin precursor (reactive group-containing prepolymer) having a functional group capable of reacting with an active hydrogen group is emulsified or dispersed in an aqueous medium containing resin fine particles in the dissolution suspension method, and an active hydrogen group-containing compound is reacted with the reactive group-containing prepolymer in the aqueous medium (ester extension method); a phase inversion emulsification method in which water is added to a solution consisting of a resin or a resin precursor and a suitable emulsifier to invert the phase; and an aggregation method in which the resin particles obtained by these methods are dispersed in an aqueous medium and aggregated, and then granulated into particles of a desired size by heating and melting, etc. Among these, the toner obtained by the dissolution suspension method, the ester extension method, and the aggregation method are preferred from the viewpoint of granulation properties (particle size distribution control, particle shape control, etc.), and the toner obtained by the ester extension method is more preferred. These manufacturing methods are described in detail below.
[0073] The kneading and pulverizing method is a method for producing base particles of the toner by melting and kneading toner materials including at least a colorant, a binder resin, and a release agent, pulverizing the mixture, and classifying the mixture. In the melt-kneading, the toner materials are mixed, and the mixture is placed in a melt-kneader and melt-kneaded. As the melt-kneader, for example, a single-screw or twin-screw continuous kneader or a batch-type kneader using a roll mill can be used. For example, a KTK twin-screw extruder manufactured by Kobe Steel, Ltd., a TEM-type extruder manufactured by Toshiba Machine Co., Ltd., a twin-screw extruder manufactured by KCK Corporation, a PCM-type twin-screw extruder manufactured by Ikegai Iron Works, a co-kneader manufactured by Buss Co., Ltd., etc. are preferably used. This melt-kneading is preferably performed under appropriate conditions that do not cause scission of the molecular chain of the binder resin. Specifically, the melt-kneading temperature is performed with reference to the softening point of the binder resin. If the temperature is higher than the softening point, scission occurs violently, and if the temperature is too low, dispersion may not proceed.
[0074] In the pulverization, the kneaded product obtained by the kneading is pulverized. In this pulverization, it is preferable to first coarsely pulverize the kneaded product and then finely pulverize it. In this case, a method of pulverizing by colliding with a collision plate in a jet stream, pulverizing by colliding particles with each other in a jet stream, or pulverizing in a narrow gap between a mechanically rotating rotor and a stator is preferably used.
[0075] The classification is performed by classifying the pulverized product obtained by the pulverization to adjust the particles to a predetermined particle size. The classification can be performed, for example, by removing fine particles using a cyclone, a decanter, a centrifugal separator, or the like. After the above-mentioned pulverization and classification are completed, the pulverized material is classified in an air current by centrifugal force or the like, whereby toner base particles having a predetermined particle size can be produced.
[0076] The dissolution suspension method is a method for producing toner base particles by dispersing or emulsifying an oil phase composition in an aqueous medium, the oil phase composition being prepared by dissolving or dispersing a toner composition containing at least a binder resin or a resin precursor, a colorant, and a release agent in an organic solvent.
[0077] The organic solvent used for dissolving or dispersing the toner composition is preferably volatile with a boiling point of less than 100° C., from the viewpoint of facilitating subsequent removal of the solvent.
[0078] Examples of the organic solvent include ester or ester ether solvents such as ethyl acetate, butyl acetate, methoxybutyl acetate, methyl cellosolve acetate, and ethyl cellosolve acetate; ether solvents such as diethyl ether, tetrahydrofuran, dioxane, ethyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, di-n-butyl ketone, and cyclohexanone; alcohol solvents such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, t-butanol, 2-ethylhexyl alcohol, and benzyl alcohol; and mixed solvents of two or more of these.
[0079] In the dissolution suspension method, an emulsifier or a dispersant may be used, if necessary, when dispersing or emulsifying the oil phase composition in the aqueous medium.
[0080] As the emulsifier or dispersant, known surfactants, water-soluble polymers, etc. can be used. The surfactant is not particularly limited, and examples thereof include anionic surfactants (alkylbenzenesulfonic acid, phosphate ester, etc.), cationic surfactants (quaternary ammonium salt type, amine salt type, etc.), amphoteric surfactants (carboxylate type, sulfate ester salt type, sulfonate type, phosphate ester salt type, etc.), nonionic surfactants (AO addition type, polyhydric alcohol type, etc.). The surfactant may be used alone or in combination of two or more surfactants.
[0081] Examples of the water-soluble polymer include cellulose compounds (e.g., methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, ethylhydroxyethyl cellulose, carboxymethyl cellulose, hydroxypropyl cellulose, and saponified products thereof), gelatin, starch, dextrin, gum arabic, chitin, chitosan, polyvinyl alcohol, polyvinylpyrrolidone, polyethylene glycol, polyethyleneimine, polyacrylamide, acrylic acid (salt)-containing polymers (sodium polyacrylate, potassium polyacrylate, ammonium polyacrylate, partially neutralized polyacrylic acid with sodium hydroxide, sodium acrylate-acrylic acid ester copolymer), partially neutralized styrene-maleic anhydride copolymer with sodium hydroxide, and water-soluble polyurethanes (reaction products of polyethylene glycol, polycaprolactone diol, etc. with polyisocyanate, etc.). The above-mentioned organic solvents and plasticizers can also be used in combination as emulsifying or dispersing aids.
[0082] The toner according to the present invention is preferably obtained by dispersing or emulsifying an oil phase composition containing at least a binder resin, a binder resin precursor (reactive group-containing prepolymer) having a functional group capable of reacting with an active hydrogen group, a colorant, and a release agent in an aqueous medium containing resin fine particles, and granulating base particles of the toner by a method (ester elongation method) in which an active hydrogen group-containing compound contained in the oil phase composition and / or the aqueous medium is reacted with the reactive group-containing prepolymer in a solution suspension method.
[0083] The resin fine particles can be formed by a known polymerization method, but are preferably obtained as an aqueous dispersion of resin fine particles. Examples of a method for preparing an aqueous dispersion of resin fine particles include the following methods (a) to (h). (a) A method in which a vinyl monomer is used as a starting material and an aqueous dispersion of resin fine particles is directly prepared by a polymerization reaction of any one of a suspension polymerization method, an emulsion polymerization method, a seed polymerization method and a dispersion polymerization method. (b) A method in which a precursor (monomer, oligomer, etc.) of a polyaddition or condensation resin such as a polyester resin, polyurethane resin, or epoxy resin, or a solvent solution thereof is dispersed in an aqueous medium in the presence of a suitable dispersant, and then the precursor is cured by heating or by adding a curing agent to prepare an aqueous dispersion of resin microparticles. (c) A method in which a suitable emulsifier is dissolved in a precursor (monomer, oligomer, etc.) of a polyaddition or condensation resin such as a polyester resin, polyurethane resin, or epoxy resin, or a solvent solution thereof (preferably liquid, which may be liquefied by heating), and then water is added to cause phase inversion emulsification, thereby preparing an aqueous dispersion of resin microparticles. (d) A method in which a resin synthesized in advance by a polymerization reaction (e.g., addition polymerization, ring-opening polymerization, polyaddition, addition condensation, condensation polymerization, etc.) is pulverized using a mechanical rotary or jet type fine grinder, and classified to obtain resin fine particles, which are then dispersed in water in the presence of a suitable dispersant to prepare an aqueous dispersion of resin fine particles. (e) A method in which a resin synthesized in advance by a polymerization reaction (e.g., addition polymerization, ring-opening polymerization, polyaddition, addition condensation, condensation polymerization, etc.) is dissolved in a solvent and a resin solution is sprayed in a mist form to form resin microparticles, and then the resin microparticles are dispersed in water in the presence of a suitable dispersant to prepare an aqueous dispersion of resin microparticles. (f) A method in which a poor solvent is added to a resin solution in which a resin synthesized in advance by a polymerization reaction (e.g., addition polymerization, ring-opening polymerization, polyaddition, addition condensation, condensation polymerization, etc.) is dissolved in a solvent, or a resin solution in which a resin has been heated and dissolved in a solvent in advance is cooled to precipitate resin microparticles, the solvent is removed to form resin microparticles, and the resin microparticles are then dispersed in water in the presence of a suitable dispersant to prepare an aqueous dispersion of resin microparticles. (g) A method in which a resin solution prepared by dissolving a resin previously synthesized by a polymerization reaction (e.g., addition polymerization, ring-opening polymerization, polyaddition, addition condensation, condensation polymerization, etc.) in a solvent is dispersed in an aqueous medium in the presence of a suitable dispersant, and the solvent is then removed by heating, reducing pressure, etc. to prepare an aqueous dispersion of resin microparticles. (h) A method in which a resin synthesized in advance by a polymerization reaction (e.g., addition polymerization, ring-opening polymerization, polyaddition, addition condensation, condensation polymerization, etc.) is dissolved in a solvent to prepare a resin solution, and then water is added to cause phase inversion emulsification to prepare an aqueous dispersion of resin microparticles.
[0084] The volume average particle diameter of the resin particles is preferably 10 nm to 300 nm, more preferably 30 nm to 120 nm. If the volume average particle diameter of the resin particles is less than 10 nm or exceeds 300 nm, the particle size distribution of the toner may deteriorate, which is not preferable. The solids concentration of the oil phase is preferably about 40% to 80%. If the concentration is too high, dissolution or dispersion becomes difficult, and the viscosity becomes high and handling becomes difficult, whereas if the concentration is too low, the productivity of the toner decreases.
[0085] The colorant, release agent, and other toner components other than the binder resin, such as the organically modified layered inorganic mineral, and masterbatches thereof may be dissolved or dispersed individually in an organic solvent, and then mixed with the binder resin solution or dispersion.
[0086] The aqueous medium may be water alone, or may be used in combination with a solvent miscible with water, such as alcohol (methanol, isopropanol, ethylene glycol, etc.), dimethylformamide, tetrahydrofuran, cellosolves (methyl cellosolve, etc.), and lower ketones (acetone, methyl ethyl ketone, etc.).
[0087] The method of dispersion or emulsification in the aqueous medium is not particularly limited, but known equipment such as low-speed shear type, high-speed shear type, friction type, high-pressure jet type, and ultrasonic wave type can be applied. Among them, from the viewpoint of reducing the particle size, high-speed shear type is preferable. When using a high-speed shear type dispersing machine, the rotation speed is not particularly limited, but is usually 1000 to 30000 rpm, preferably 5000 to 20000 rpm. The temperature during dispersion is usually 0 to 150°C (under pressure), preferably 20 to 80°C.
[0088] When a high-speed shearing method is used for dispersion or emulsification in an aqueous solvent, small oil droplets are also generated, and the re-agglomeration process of these small oil droplets is likely to cause variations in particle size and raw material arrangement. For this reason, for example, by applying a weak shearing force again after granulation, the re-agglomeration process can be controlled, making it possible to generate uniform particle size and raw material arrangement.
[0089] The method of applying shear force is not particularly limited, but for example, when using a low-speed shear type, the rotation speed is not particularly limited, but is usually 1000 to 8000 rpm, preferably 1000 to 3000 rpm. It is particularly important to apply appropriate energy, and if the shear energy is large, it may inhibit re-aggregation. In addition, the idle time between high-speed shear and low-speed shear also affects granulation, and since there is an optimal time for each toner production line, it is not particularly limited, but it is desirable to perform low-speed shear after an idle time of, for example, 5 to 120 seconds, preferably 5 to 30 seconds.
[0090] There is no particular limitation on the method for removing the organic solvent from the obtained emulsion dispersion, and a known method can be used. For example, a method can be adopted in which the temperature of the entire system is gradually increased while being stirred under normal pressure or reduced pressure, and the organic solvent in the droplets is completely evaporated and removed.
[0091] Known techniques are used as a method for washing and drying the toner base particles dispersed in an aqueous medium. That is, after performing solid-liquid separation using a centrifuge, filter press, etc., the obtained toner cake is redispersed in ion-exchanged water at room temperature to about 40°C, and the pH is adjusted with an acid or alkali as necessary, and then solid-liquid separation is repeated several times to remove impurities and surfactants, and then the toner powder is obtained by drying using an airflow dryer, a circulation dryer, a reduced pressure dryer, a vibration flow dryer, etc. In this case, fine particle components of the toner may be removed by centrifugation, etc., and after drying, a known classifier may be used to obtain a desired particle size distribution.
[0092] In the aggregation method, for example, a resin particle dispersion liquid consisting of at least a binder resin, a colorant particle dispersion liquid, and optionally a release agent particle dispersion liquid are mixed and aggregated to produce toner base particles. The resin particle dispersion liquid is obtained by a known method such as emulsion polymerization, seed polymerization, phase inversion emulsification method, etc., and the colorant particle dispersion liquid and the release agent particle dispersion liquid are obtained by dispersing a colorant and a release agent in an aqueous medium by a known wet dispersion method, etc.
[0093] For controlling the state of aggregation, methods such as application of heat, addition of a metal salt, and adjustment of pH are preferably used.
[0094] The metal salt is not particularly limited, and examples thereof include monovalent metals that form salts, such as sodium and potassium; divalent metals that form salts, such as calcium and magnesium; and trivalent metals that form salts, such as aluminum.
[0095] Examples of anions constituting the salt include chloride ions, bromide ions, iodide ions, carbonate ions, and sulfate ions, and among these, magnesium chloride, aluminum chloride, and their complexes and polymers are preferred. In addition, heating during or after the aggregation is completed can promote fusion between the resin particles, which is preferred from the viewpoint of toner uniformity. Furthermore, the shape of the toner can be controlled by heating, and the more heat is applied, the more the toner becomes spherical.
[0096] The method for washing and drying the toner base particles dispersed in the aqueous medium can be the above-mentioned method, etc. In order to improve the fluidity, storage stability, developability, and transferability of the toner, the coalesced particles are added and mixed to the toner base particles produced as described above, and inorganic fine particles such as hydrophobic silica fine powder may also be added and mixed.
[0097] A general powder mixer is used to mix the additives, but it is preferable to equip it with a jacket or the like so that the internal temperature can be adjusted. The history of the load applied to the additives can be changed by adding the additives during or gradually. In this case, the number of revolutions, rolling speed, time, temperature, etc. of the mixer may be changed. A strong load may be applied first, and then a relatively weak load, or vice versa. Examples of mixing equipment that can be used include a V-type mixer, a rocking mixer, a Loedige mixer, a Nauter mixer, and a Henschel mixer. Next, the mixture is passed through a sieve of 250 mesh or more to remove coarse particles and agglomerated particles, and the toner is obtained.
[0098] (Developer) The developer of the present invention contains at least the toner and appropriately selected other components such as a carrier, etc. The developer may be a one-component developer or a two-component developer, but when used in a high-speed printer or the like that corresponds to the recent improvement in information processing speed, the two-component developer is preferred in terms of life extension, etc.
[0099] In the case of the one-component developer using the toner, the toner is unlikely to aggregate over time even in response to stress from the developing means, and there is no toner filming on the developing roller as a developer carrier, nor toner fusion to a layer thickness regulating member such as a blade for thinning the toner layer, and good image density stability and transferability are maintained, thereby obtaining good and stable image quality. In the case of the two-component developer using the toner, the toner is unlikely to aggregate over time even in response to stirring stress from the developing means, and the occurrence of abnormal images is suppressed, and good image density stability and transferability are maintained, thereby obtaining good and stable image quality.
[0100] <Career> The carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably one having core particles and a resin layer (coating layer) that coats the core particles.
[0101] <<Core particle>> The core particles are not particularly limited as long as they are magnetic core particles and can be appropriately selected depending on the purpose, and examples thereof include ferromagnetic metals such as iron and cobalt, iron oxides such as magnetite, hematite and ferrite, and resin particles in which magnetic materials such as various alloys and compounds are dispersed in a resin, etc. Among these, Mn-based ferrite, Mn-Mg-based ferrite, Mn-Mg-Sr-based ferrite, etc. are preferred from the viewpoint of environmental consideration.
[0102] -Weight average particle diameter of core particles Dw- The weight average particle diameter Dw of the core particles refers to the particle diameter at 50% of the integrated value in the particle size distribution of the core particles obtained by a laser diffraction or scattering method. The weight average particle diameter Dw of the core particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10 μm or more and 80 μm or less, and more preferably 20 μm or more and 65 μm or less. The weight average particle diameter Dw of the core particles is measured by measuring the particle size distribution (relationship between number frequency and particle size) of the particles measured on a number basis using a Microtrack particle size distribution meter (HRA9320-X100, manufactured by Honeywell) under the conditions described below, and calculating using the following formula (I). Each channel represents a length for dividing the particle size range in the particle size distribution diagram into measurement width units, and the representative particle size is the lower limit value of the particle size stored in each channel. Dw={1 / Σ(nD3)}×{Σ(nD4)} ···(I) In the above formula (I), D represents the representative particle size (μm) of the core particles present in each channel, and n represents the total number of core particles present in each channel. [Measurement conditions] [1] Particle size range: 100μm to 8μm [2] Channel length (channel width): 2 μm [3] Number of channels: 46 [4] Refractive index: 2.42
[0103] <<Coating layer>> The coating layer contains at least a resin, and may contain other components such as a filler, if necessary.
[0104] -resin- The resin for forming the coating layer of the carrier is not particularly limited and can be appropriately selected according to the purpose. For example, polyolefin (e.g., polyethylene, polypropylene, etc.) and its modified products, crosslinkable copolymers including polystyrene, acrylic resin, acrylonitrile, vinyl acetate, vinyl alcohol, vinyl chloride, vinylcarbazole, vinyl ether, etc.; silicone resins consisting of organosiloxane bonds or modified products thereof (e.g., modified products with alkyd resin, polyester resin, epoxy resin, polyurethane, polyimide, etc.); polyamide; polyester; polyurethane; polycarbonate; urea resin; melamine resin; benzoguanamine resin; epoxy resin; ionomer resin; polyimide resin, and derivatives thereof. These may be used alone or in combination of two or more. Among these, silicone resins are preferred.
[0105] The silicone resin is not particularly limited and can be appropriately selected from commonly known silicone resins according to the purpose. Examples of the silicone resin include straight silicone resins consisting only of organosiloxane bonds, and silicone resins modified with alkyd, polyester, epoxy, acrylic, urethane, etc.
[0106] Examples of the straight silicone resin include KR271, KR272, KR282, KR252, KR255, and KR152 (manufactured by Shin-Etsu Chemical Co., Ltd.), SR2400, SR2405, and SR2406 (manufactured by Dow Corning Toray Silicones Co., Ltd.).
[0107] Specific examples of the modified silicone resin include epoxy modified product: ES-1001N, acrylic modified silicone: KR-5208, polyester modified product: KR-5203, alkyd modified product: KR-206, urethane modified product: KR-305 (all manufactured by Shin-Etsu Chemical Co., Ltd.), epoxy modified product: SR2115, alkyd modified product: SR2110 (manufactured by Toray Dow Corning Silicones Co., Ltd.), and the like. The silicone resin may be used alone, or may be used together with a crosslinking reactive component, a charge amount adjusting component, etc. Examples of the crosslinking reactive component include silane coupling agents, etc. Examples of the silane coupling agents include methyltrimethoxysilane, methyltriethoxysilane, octyltrimethoxysilane, and aminosilane coupling agents.
[0108] -Filler- The filler is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include conductive fillers and non-conductive fillers. These may be used alone or in combination of two or more. Among these, it is preferable that the coating layer contains a conductive filler and a non-conductive filler.
[0109] The powder resistivity of the filler can be measured using a powder resistivity measurement system (MCP-PD51, manufactured by Dia Instruments) and a resistivity meter (four-terminal four-probe type, Loresta-GP, manufactured by Mitsubishi Chemical Analytech Co., Ltd.) under the conditions of a 1.0 g sample, an electrode spacing of 3 mm, a sample radius of 10.0 mm, and a load of 20 kN.
[0110] --Conductive filler-- The conductive filler is not particularly limited and can be appropriately selected depending on the purpose. For example, conductive fillers formed by forming a layer of tin dioxide or indium oxide on a substrate such as aluminum oxide, titanium oxide, zinc oxide, barium sulfate, silicon oxide, zirconium oxide, etc., and conductive fillers formed by using carbon black are included. Among these, conductive fillers containing aluminum oxide, titanium oxide, and barium sulfate are preferred.
[0111] The conductive filler refers to a filler having a powder resistivity of 100 Ω·cm or less.
[0112] --Non-conductive filler-- The non-conductive filler is not particularly limited and can be appropriately selected depending on the purpose. For example, non-conductive fillers formed using aluminum oxide, titanium oxide, barium sulfate, zinc oxide, silicon dioxide, zirconium oxide, etc. are exemplified. Among these, non-conductive fillers containing aluminum oxide, titanium oxide, and barium sulfate are preferred.
[0113] The non-conductive filler refers to a filler having a powder resistivity of more than 100 Ω·cm.
[0114] <Toner manufacturing method> The method for producing the toner of the present invention is not particularly limited and may be appropriately selected depending on the purpose. For example, a kneading and pulverizing method, a dissolution and suspension method, etc. may be used. In the kneading and pulverizing method, it is preferable to pulverize the raw materials in a state where they are more uniformly dispersed in the binder resin, for example, by finely dispersing the raw materials in advance, increasing the intensity of the kneading process, or preventing re-aggregation by controlling the temperature.
[0115] The dissolution suspension method is not particularly limited and may be appropriately selected depending on the purpose. For example, a detailed description will be given below as an example. After dissolving a toner composition containing at least a binder resin, a colorant, and a release agent in an organic solvent, the materials are pulverized by shearing force or collision force. At this time, by using shearing force and collision force in combination, it is possible to efficiently reduce toner with a raw material arrangement different from the target design, in which the LC varies by 25.0% or more in absolute value from the median value of the LC distribution.
[0116] The dispersion method is not particularly limited, but the preferred method for fine dispersion by shear is to crush the material with high shear force generated in the narrow gap between the rotor and stator, while the preferred method for fine dispersion by collision is to fill a vessel with beads such as zirconia and rotate the vessel to crush the material by collision between the beads or between the beads and the vessel.
[0117] Collision pulverization is particularly effective for large materials exceeding 1 μm in size, while shear pulverization is effective for further pulverizing submicron-order materials. The two methods have different target areas for pulverization, so using them together can improve the uniformity of the material, making it particularly preferable to use the two methods together. There is no restriction on the order of shear dispersion and collision dispersion.
[0118] In order to efficiently pulverize materials, it is preferable that the rotor circumferential speed exceeds 12 m / s in shearing microdispersion. In addition, it is preferable that the disk circumferential speed is 6 m / s or more in collision pulverization, and more preferably 10 m / s to 12 m / s. In collision pulverization, if the disk circumferential speed is less than 6 m / s, sufficient collision pulverization energy cannot be obtained and beads are biased, making it impossible to disperse sufficiently. Conversely, if the disk circumferential speed is increased too much, there is a concern that the cleaning performance will deteriorate due to the reduction in background toner due to excessive dispersion. There is also a risk of re-aggregation due to an increase in liquid temperature and overdispersion.
[0119] The media diameter is preferably 0.5 mm or less, and more preferably 0.3 mm or less. The smaller the beads, the greater the total surface area of the beads, which increases the opportunities for dispersion through collision and improves dispersion efficiency. If the beads are too small, the openings of the screen separating the beads and the process liquid must be narrowed, which means that the flow rate cannot be achieved and the liquid temperature rises, which creates the risk of re-agglomeration.
[0120] Furthermore, in order to reduce toner particles with raw material arrangements that differ from the target design, where the LC has varied by 25.0% or more in absolute value from the median of the LC distribution, it is also effective to add inorganic substances that are harder than organic substances such as pigments and release agents to the dispersion liquid and disperse them.
[0121] The inorganic substance is not particularly limited, but as an example, the case where montmorillonite, which is an organically modified layered inorganic mineral, is added will be described below.
[0122] After dissolving a toner composition containing at least a binder resin, a colorant, a release agent, and an organically modified layered inorganic mineral in an organic solvent, the material is finely divided by collision force using a media-type disperser. Compared to when the organically modified layered inorganic mineral is not included, the material can be finely dispersed more efficiently, and it is possible to reduce toner particles with non-uniform composition. This is because collision opportunities arise not only between beads and between beads and vessels, but also between beads and inorganic matter, and between vessels and inorganic matter, making it possible to effectively disperse organic matter with low hardness.
[0123] In rotor-stator type shear dispersion, the addition of inorganic substances does not increase the grinding efficiency, so it is important to utilize inorganic substances as grinding media.
[0124] The amount of inorganic matter added is preferably 0.2% by mass to 2.0% by mass, more preferably 0.7% by mass to 1.5% by mass, based on the total solid content. By adding an amount of 0.2% by mass to 2.0% by mass, the function as a grinding medium is sufficiently exhibited, and the LC distribution is narrowed.
[0125] In addition, the shape, size, etc. of the toner are not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the toner has an average circularity, a volume average particle size, a ratio of the volume average particle size to the number average particle size (volume average particle size / number average particle size), etc. as described below.
[0126] The average circularity is a value obtained by dividing the perimeter of a circle having the same projected area as the shape of the toner by the perimeter of an actual particle, and is preferably 0.950 to 0.980, more preferably 0.960 to 0.975. It is preferable that the number of particles having an average circularity of less than 0.950 is 15.0% or less.
[0127] If the average circularity is less than 0.950, it may not be possible to obtain a high-quality image without satisfactory transferability or dust. If it exceeds 0.980, in an image forming system using blade cleaning or the like, cleaning failure occurs on the photoreceptor and transfer belt, etc., and dirt on the image may occur. For example, in the case of forming an image with a high image area ratio such as a photographic image, the toner that formed an image that was not transferred due to a paper feed failure or the like becomes a transfer residual toner on the photoreceptor and accumulates on the photoreceptor, resulting in background dirt on the image. Alternatively, it may contaminate the charging roller that contact-charges the photoreceptor, and the original charging ability may not be exhibited.
[0128] The average circularity can be measured using a flow type particle image analyzer ("FPIA-2100", manufactured by Sysmex Corporation) and analyzed using analysis software (FPIA-2100 Data Processing Program for FPIA version 00-10).
[0129] As a specific example, 0.1 to 0.5 mL of 10% by mass surfactant (alkylbenzene sulfonate, Neogen SC-A, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) is added to a 100 mL glass beaker, 0.1 to 0.5 g of each toner is added and stirred with a micro spatula, and then 80 mL of ion-exchanged water is added. The resulting dispersion is dispersed for 3 minutes using an ultrasonic disperser (manufactured by Honda Electronics Co., Ltd.). The shape and distribution of the toner are measured using the FPIA-2100 until a concentration of 5,000 to 15,000 particles / μL is obtained.
[0130] In this measurement method, it is important that the dispersion concentration is 5,000 to 15,000 particles / μL from the viewpoint of measurement reproducibility of the average circularity. In order to obtain the dispersion concentration, it is necessary to change the conditions of the dispersion, that is, the amount of surfactant added and the amount of toner. The amount of surfactant required varies depending on the hydrophobicity of the toner, as in the measurement of the toner particle size described above. If too much surfactant is added, noise due to bubbles will occur, and if too little, the toner cannot be sufficiently wetted, resulting in insufficient dispersion. The amount of toner added also varies depending on the particle size, and it is necessary to add less for small particles and more for large particles. When the toner particle size is 3 μm to 10 μm, the dispersion concentration can be adjusted to 5,000 particles / μL to 15,000 particles / μL by adding 0.1 g to 0.5 g of toner.
[0131] The volume average particle diameter of the toner is not particularly limited and can be appropriately selected according to the purpose, but for example, 3 μm to 10 μm is preferable, and 4 μm to 7 μm is more preferable. If the volume average particle diameter is less than 3 μm, the toner may be fused to the surface of the carrier during long-term stirring in a developing device in a two-component developer, which may reduce the charging ability of the carrier, and if it exceeds 10 μm, it may be difficult to obtain a high-resolution, high-quality image, and the variation in the particle diameter of the toner may be large when the toner balance in the developer is performed.
[0132] The ratio of the volume average particle diameter to the number average particle diameter in the toner (volume average particle diameter / number average particle diameter) is preferably from 1.00 to 1.25, and more preferably from 1.00 to 1.15. The volume average particle diameter and the ratio of the volume average particle diameter to the number average particle diameter (volume average particle diameter / number average particle diameter) can be measured using a particle size measuring device ("Multisizer III", manufactured by Beckman Coulter) with an aperture diameter of 100 μm, and analyzed using analysis software (Beckman CoulterMutlisizer 3 Version 3.51).
[0133] As a specific example, 0.5 mL of 10% by weight surfactant (alkylbenzene sulfonate, Neogen SC-A, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) is added to a 100 mL glass beaker, 0.5 g of each toner is added, and the mixture is stirred with a microspatula, and then 80 mL of ion-exchanged water is added. The resulting dispersion is subjected to dispersion treatment for 10 minutes using an ultrasonic disperser (W-113MK-II, manufactured by Honda Electronics Co., Ltd.). The dispersion can be measured using the Multisizer III and Isoton III (manufactured by Beckman Coulter, Inc.) as the measurement solution.
[0134] The toner sample dispersion is dropped so that the concentration indicated by the device is 8±2%. It is important for this measurement method to keep the concentration at 8±2% from the viewpoint of reproducibility of particle size measurement. Within this concentration range, no error occurs in the particle size.
[0135] <Carrier manufacturing method> The carrier manufacturing method is not particularly limited and can be appropriately selected according to the purpose, but a manufacturing method is preferably a method of applying a coating layer forming solution containing the resin and the filler to the surface of the core particle using a fluidized bed type coating device. In addition, when applying the coating layer forming solution, the condensation of the resin contained in the coating layer may be promoted, or the condensation of the resin contained in the coating layer may be promoted after applying the coating layer forming solution. The method for condensing the resin is not particularly limited and may be appropriately selected depending on the purpose. For example, there may be mentioned a method in which heat, light, or the like is applied to the coating layer forming solution to condense the resin.
[0136] - Weight average particle size of carrier Dw - The weight average particle diameter Dw of the carrier refers to the particle diameter at 50% of the integrated value in the particle size distribution of the core particles obtained by a laser diffraction / scattering method. The weight average particle diameter Dw of the carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10 μm or more and 80 μm or less, and more preferably 20 μm or more and 65 μm or less. The weight average particle diameter Dw of the carrier is measured by measuring the particle size distribution (relationship between number frequency and particle size) of the particles measured on a number basis using a Microtrack particle size distribution meter (HRA9320-X100, manufactured by Honewell) under the conditions described below, and calculating using the following formula (II). Each channel represents a length for dividing the particle size range in the particle size distribution diagram into measurement width units, and the representative particle size is the lower limit value of the particle size stored in each channel. Dw={1 / Σ(nD3)}×{Σ(nD4)} ···(II) In the above formula (II), D represents the typical particle size (μm) of the carriers present in each channel, and n represents the total number of carriers present in each channel. [Measurement conditions] [1] Particle size range: 100μm to 8μm [2] Channel length (channel width): 2 μm [3] Number of channels: 46 [4] Refractive index: 2.42 When the developer is a two-component developer, the mixture ratio of the toner and the carrier in the two-component developer is preferably such that the mass ratio of the toner to the carrier is 2.0% by mass or more and 12.0% by mass or less, and more preferably 2.5% by mass or more and 10.0% by mass or less.
[0137] The toner storage unit in the present invention refers to a unit having a function of storing toner and storing the toner. Examples of the toner storage unit include a toner storage container, a developing unit, and a process cartridge. The toner storage container refers to a container that stores toner. The developing device has a means for containing toner and developing the toner. The process cartridge is a cartridge that integrates at least an image carrier and a developing means, contains toner, and is detachably mountable to an image forming apparatus. The process cartridge may further include at least one selected from a charging means, an exposure means, and a cleaning means.
[0138] By mounting the toner storage unit of the present invention in an image forming apparatus and forming an image, the image is formed using the toner of the present invention, and therefore a toner having excellent transferability, capable of forming high-quality images, and capable of suppressing contamination inside the machine can be provided.
[0139] (Image forming method and image forming apparatus) The image forming method of the present invention comprises an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier, a developing step of developing the electrostatic latent image to form a visible image using the toner or developer of the present invention, a transfer step of transferring the visible image onto a recording medium, and a fixing step of fixing the transferred image onto the recording medium, and further comprises other steps appropriately selected as necessary, such as a static elimination step, a cleaning step, a recycling step, and a control step. The image forming apparatus of the present invention comprises an electrostatic latent image carrier, an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image carrier, a developing means for developing the electrostatic latent image to form a visible image using the toner or developer of the present invention, a transfer means for transferring the visible image onto a recording medium, and a fixing means for fixing the transferred image onto the recording medium. It further comprises other means appropriately selected as necessary, such as a charge removing means, a cleaning means, a recycling means, a control means, etc. Details will be described below.
[0140] -Electrostatic latent image forming process and electrostatic latent image forming means- The electrostatic latent image forming step is a step of forming an electrostatic latent image on an electrostatic latent image bearing member. The electrostatic latent image carrier (sometimes referred to as "electrophotographic photoreceptor" or "photoreceptor") is not particularly limited in terms of material, shape, structure, size, etc., and can be appropriately selected from known ones, but the shape is preferably a drum shape, and the material can be, for example, inorganic photoreceptors such as amorphous silicon and selenium, organic photoreceptors (OPC) such as polysilane and phthalopolymethine, etc. Among these, organic photoreceptors (OPC) are preferred in that higher resolution images can be obtained. The electrostatic latent image can be formed, for example, by uniformly charging the surface of the electrostatic latent image carrier and then exposing it to light in an imagewise manner, and can be performed by an electrostatic latent image forming means.
[0141] The electrostatic latent image forming unit includes, for example, at least a charging unit (charger) that uniformly charges the surface of the electrostatic latent image carrier, and an exposure unit (exposure unit) that imagewise exposes the surface of the electrostatic latent image carrier. The charging can be performed, for example, by applying a voltage to the surface of the electrostatic latent image carrier using the charger.
[0142] The charger is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charger include a contact charger known per se having a conductive or semiconductive roll, brush, film, rubber blade, or the like, and a non-contact charger utilizing corona discharge such as a corotron or scorotron.
[0143] The charger is preferably one that is arranged in contact or non-contact with the electrostatic latent image carrier and charges the surface of the electrostatic latent image carrier by applying superimposed DC and AC voltages to the electrostatic latent image carrier. Also, the charger is preferably a charging roller that is arranged in close proximity to the electrostatic latent image carrier in a non-contact manner via a gap tape and charges the surface of the electrostatic latent image carrier by applying superimposed DC and AC voltages to the charging roller.
[0144] The exposure can be carried out, for example, by exposing the surface of the electrostatic latent image bearing member imagewise using the exposure unit.
[0145] The exposure device is not particularly limited as long as it can expose the surface of the electrostatic latent image carrier charged by the charger in the shape of an image to be formed, and can be appropriately selected depending on the purpose. Examples of the exposure device include various exposure devices such as a copying optical system, a rod lens array system, a laser optical system, and a liquid crystal shutter optical system. In the present invention, a light back system may be adopted in which exposure is performed imagewise from the back side of the electrostatic latent image bearing member.
[0146] -Developing process and developing means- The developing step is a step of developing the electrostatic latent image with the toner to form a visible image.
[0147] The visible image can be formed, for example, by developing the electrostatic latent image with the toner, and can be formed by the developing unit.
[0148] The developing means preferably has at least a developing unit that contains the toner and can apply the toner to the electrostatic latent image in a contact or non-contact manner, and more preferably has a developing unit equipped with a toner container.
[0149] The developing device may be a single-color developing device or a multi-color developing device, and a suitable example is one having an agitator that charges the toner by friction and agitation, and a rotatable magnetic roller.
[0150] In the developing device, for example, the toner and the carrier are mixed and stirred, and the toner is charged by friction during this process and held in a standing state on the surface of a rotating magnet roller to form a magnetic brush. Since the magnet roller is disposed near the electrostatic latent image carrier (photoconductor), a part of the toner constituting the magnetic brush formed on the surface of the magnet roller moves to the surface of the electrostatic latent image carrier (photoconductor) by electrical attraction. As a result, the electrostatic latent image is developed by the toner, and a visible image by the toner is formed on the surface of the electrostatic latent image carrier (photoconductor).
[0151] -Transfer process and transfer means- The transfer step is a step of transferring the visible image onto a recording medium. A preferred embodiment is one in which an intermediate transfer body is used, the visible image is primarily transferred onto the intermediate transfer body, and then the visible image is secondarily transferred onto the recording medium. A more preferred embodiment is one in which a toner of two or more colors, preferably a full-color toner, is used as the toner, and the toner includes a primary transfer step of transferring the visible image onto the intermediate transfer body to form a composite transfer image, and a secondary transfer step of transferring the composite transfer image onto a recording medium.
[0152] The transfer can be performed, for example, by charging the electrostatic latent image carrier (photoconductor) with the visible image using a transfer charger, and can be performed by the transfer means. The transfer means preferably has a first transfer means for transferring the visible image onto an intermediate transfer body to form a composite transfer image, and a second transfer means for transferring the composite transfer image onto a recording medium.
[0153] The intermediate transfer body is not particularly limited and can be appropriately selected from known transfer bodies depending on the purpose. For example, a transfer belt is preferably used.
[0154] The transfer means (the primary transfer means, the secondary transfer means) preferably has at least a transfer device that peels and charges the visible image formed on the electrostatic latent image carrier (photoconductor) onto the recording medium. The number of the transfer means may be one or more.
[0155] Examples of the transfer device include a corona transfer device using corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, and an adhesive transfer device.
[0156] The recording medium is not particularly limited and can be appropriately selected from known recording media (recording paper).
[0157] - Fixing process and fixing means - The fixing step is a step of fixing the visible image transferred to the recording medium using a fixing device, and may be performed for each color developer each time it is transferred to the recording medium, or may be performed simultaneously for each color developer in a stacked state.
[0158] The fixing device is not particularly limited and can be appropriately selected depending on the purpose, but a known heating and pressurizing means is suitable. Examples of the heating and pressurizing means include a combination of a heating roller and a pressure roller, a combination of a heating roller, a pressure roller and an endless belt, etc.
[0159] The fixing device preferably has a heating body having a heat generating element, a film in contact with the heating body, and a pressure member in pressure contact with the heating body via the film, and is a means for heat fixing by passing a recording medium on which an unfixed image has been formed between the film and the pressure member. Heating in the heating and pressure means is preferably at 80°C to 200°C.
[0160] In the present invention, depending on the purpose, for example, a known optical fixing device may be used together with or instead of the fixing step and fixing means. The charge removing step is a step of removing electricity by applying a charge removing bias to the electrostatic latent image bearing member, and can be suitably performed by a charge removing means.
[0161] The discharging means is not particularly limited as long as it can apply a discharging bias to the electrostatic latent image bearing member, and can be appropriately selected from known discharging devices. For example, a discharging lamp is preferably used.
[0162] The cleaning step is a step of removing the toner remaining on the electrostatic latent image bearing member, and can be suitably performed by a cleaning unit.
[0163] The cleaning means is not particularly limited as long as it can remove the toner remaining on the electrostatic latent image carrier, and can be appropriately selected from among known cleaners. Suitable examples of the cleaning means include magnetic brush cleaners, electrostatic brush cleaners, magnetic roller cleaners, blade cleaners, brush cleaners, and web cleaners.
[0164] The recycling step is a step of recycling the toner removed by the cleaning step to the developing means, and can be suitably performed by a recycling means. The recycling means is not particularly limited, and examples thereof include known transport means.
[0165] The control step is a step of controlling each of the steps, and each step can be suitably performed by a control means.
[0166] The control means is not particularly limited as long as it can control the movement of each of the means, and can be appropriately selected depending on the purpose. For example, the control means includes devices such as a sequencer and a computer.
[0167] A first example of an image forming apparatus of the present invention is shown in Fig. 2. The image forming apparatus 100A includes a photoconductor drum 10, a charging roller 20, an exposure device, a developing device 40, an intermediate transfer belt 50, a cleaning device 60 having a cleaning blade, and a static elimination lamp 70.
[0168] The intermediate transfer belt 50 is an endless belt stretched around three rollers 51 arranged on the inside, and can move in the direction of the arrow in the figure. Some of the three rollers 51 also function as transfer bias rollers capable of applying a transfer bias (primary transfer bias) to the intermediate transfer belt 50. A cleaning device 90 having a cleaning blade is arranged near the intermediate transfer belt 50. Furthermore, a transfer roller 80 capable of applying a transfer bias (secondary transfer bias) for transferring a toner image to a transfer paper 95 is arranged facing the intermediate transfer belt 50.
[0169] In addition, a corona charging device 58 for applying an electric charge to the toner image transferred to the intermediate transfer belt 50 is disposed around the intermediate transfer belt 50, between the contact point between the photosensitive drum 10 and the intermediate transfer belt 50 and the contact point between the intermediate transfer belt 50 and the transfer paper 95, in the direction of rotation of the intermediate transfer belt 50.
[0170] The developing device 40 is composed of a developing belt 41, and a black developing unit 45K, a yellow developing unit 45Y, a magenta developing unit 45M, and a cyan developing unit 45C arranged around the developing belt 41. Each developing unit 45 of each color includes a developer container 42, a developer supply roller 43, and a developing roller (developer carrier) 44. The developing belt 41 is an endless belt stretched by a plurality of belt rollers, and can move in the direction of the arrow in the figure. A part of the developing belt 41 contacts the photosensitive drum 10. Next, a method of forming an image using the image forming apparatus 100A will be described. First, the surface of the photosensitive drum 10 is uniformly charged using the charging roller 20, and then the photosensitive drum 10 is exposed to exposure light L using an exposure device (not shown) to form an electrostatic latent image. Next, the electrostatic latent image formed on the photosensitive drum 10 is developed with toner supplied from the developing device 40 to form a toner image. Furthermore, the toner image formed on the photosensitive drum 10 is transferred (primary transfer) onto the intermediate transfer belt 50 by the transfer bias applied from the roller 51, and then transferred (secondary transfer) onto the transfer paper 95 by the transfer bias applied from the transfer roller 80. Meanwhile, the photosensitive drum 10 from which the toner image has been transferred onto the intermediate transfer belt 50 is discharged by the discharge lamp 70 after the toner remaining on the surface is removed by the cleaning device 60.
[0171] A second example of an image forming apparatus used in the present invention is shown in Fig. 3. Image forming apparatus 100B has the same configuration as image forming apparatus 100A, except that it does not have developing belt 41 and has black developing unit 45K, yellow developing unit 45Y, magenta developing unit 45M, and cyan developing unit 45C arranged directly opposite each other around photoconductor drum 10.
[0172] 4 shows a third example of an image forming apparatus used in the present invention. Image forming apparatus 100C is a tandem type color image forming apparatus, and includes copying machine main body 150, paper feed table 200, scanner 300, and automatic document feeder (ADF) 400.
[0173] Intermediate transfer belt 50, provided in the center of copying machine main body 150, is an endless belt stretched around three rollers 14, 15, and 16, and can move in the direction of the arrow in the figure. Near roller 15, a cleaning device 17 having a cleaning blade for removing toner remaining on intermediate transfer belt 50 after a toner image has been transferred to recording paper is disposed. Facing intermediate transfer belt 50 stretched around rollers 14 and 15, yellow, cyan, magenta, and black image forming units 120Y, 120C, 120M, and 120K are arranged in parallel along the conveying direction.
[0174] An exposure device 21 is disposed near the image forming unit 120. A secondary transfer belt 24 is disposed on the side of the intermediate transfer belt 50 opposite to the side on which the image forming unit 120 is disposed. The secondary transfer belt 24 is an endless belt stretched over a pair of rollers 23, and the recording paper transported on the secondary transfer belt 24 and the intermediate transfer belt 50 can come into contact with each other between the rollers 16 and 23.
[0175] Further, disposed near the secondary transfer belt 24 is a fixing device 25 including a fixing belt 26, which is an endless belt stretched over a pair of rollers, and a pressure roller 27 disposed so as to be pressed against the fixing belt 26. Further, disposed near the secondary transfer belt 24 and the fixing device 25 is a sheet inverting device 28 for inverting the recording paper when images are formed on both sides of the recording paper.
[0176] Next, a method of forming a full-color image using the image forming apparatus 100C will be described. First, a color document is set on the document table 130 of the automatic document feeder (ADF) 400, or the automatic document feeder 400 is opened and a color document is set on the contact glass 32 of the scanner 300, and the automatic document feeder 400 is closed. When the start switch is pressed, if the document is set on the automatic document feeder 400, the document is transported and moved onto the contact glass 32, while if the document is set on the contact glass 32, the scanner 300 is immediately driven and the first traveling body 33 having a light source and the second traveling body 34 having a mirror travel. At this time, the reflected light from the document surface of the light irradiated from the first traveling body 33 is reflected by the second traveling body 34 and then received by the reading sensor 36 via the imaging lens 35, so that the document is read and image information of black, yellow, magenta, and cyan is obtained.
[0177] The image information of each color is transmitted to the image forming unit 120 of each color, and a toner image of each color is formed. As shown in Fig. 5, each image forming unit 120 of each color includes a photoconductor drum 10, a charging roller 160 that uniformly charges the photoconductor drum 10, an exposure device that exposes the photoconductor drum 10 to exposure light L based on the image information of each color to form an electrostatic latent image of each color, a developing device 61 that develops the electrostatic latent image with a developer of each color to form a toner image of each color, a transfer roller 62 that transfers the toner image onto the intermediate transfer belt 50, a cleaning device 63 having a cleaning blade, and a static elimination lamp 64.
[0178] The toner images of each color formed by the image forming units 120 of each color are transferred in sequence (primary transfer) onto the intermediate transfer body 50 moving while being stretched around rollers 14, 15, and 16, and are superimposed to form a composite toner image.
[0179] Meanwhile, in the paper feed table 200, one of the paper feed rollers 142 is selectively rotated to feed recording paper from one of the paper feed cassettes 144 provided in multiple stages in the paper bank 143, which is separated one by one by the separation roller 145 and sent to the paper feed path 146, transported by the transport roller 147 and guided to the paper feed path 148 in the copying machine main body 150, where it is stopped by hitting the registration rollers 49. Alternatively, the paper feed roller is rotated to feed recording paper on the manual feed tray 54, which is separated one by one by the separation roller 52 and guided to the manual feed path 53, where it is stopped by hitting the registration rollers 49.
[0180] The registration roller 49 is generally grounded when used, but may be used with a bias applied to it in order to remove paper dust from the recording paper. Next, the registration roller 49 is rotated in time with the composite toner image formed on the intermediate transfer belt 50, thereby sending the recording paper between the intermediate transfer belt 50 and the secondary transfer belt 24, and the composite toner image is transferred (secondary transfer) onto the recording paper. Any toner remaining on the intermediate transfer belt 50 after the composite toner image has been transferred is removed by a cleaning device 17. The recording paper onto which the composite toner image has been transferred is transported by secondary transfer belt 24, and then the composite toner image is fixed by fixing device 25. Next, the transport path of the recording paper is switched by switching claw 55, and the recording paper is discharged onto paper discharge tray 57 by discharge rollers 56. Alternatively, the transport path of the recording paper is switched by switching claw 55, the sheet is inverted by sheet inverting device 28, an image is formed on the back side in the same manner, and then the recording paper is discharged onto paper discharge tray 57 by discharge rollers 56.
[0181] According to the image forming method and the image forming apparatus of the present invention, high quality images can be provided for a long period of time. EXAMPLES
[0182] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples. In the examples, [%] indicates % by mass and "parts" indicates "parts by mass".
[0183] Example 1 <Production of Toner 1> -Synthesis of polyester resin- The polyester resin was obtained by carrying out the following reactions 1 to 3. Reaction 1: In a reaction vessel equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, bisphenol A ethylene oxide 3 mole adduct (EO) and 1,2-propylene glycol (PG) in a molar ratio of 90 / 10, terephthalic acid (TPA) and adipic acid (APA) in a molar ratio of 70 / 30 with an OH / COOH ratio of 1.33 were charged, and reacted with 500 ppm of titanium tetraisopropoxide at normal pressure, 230°C, and 10 hours. Reaction 2: Next, the reaction was carried out for 5 hours under reduced pressure of 10 mmHg to 15 mmHg. Reaction 3: Next, 10 parts of trimellitic anhydride (TMA) was placed in a reaction vessel and reacted at 180° C. and normal pressure for 3 hours to obtain a [polyester resin].
[0184] -Synthesis of prepolymer- Into a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 682 parts of ethylene oxide 2-mol adduct of bisphenol A, 81 parts of propylene oxide 2-mol adduct of bisphenol A, 283 parts of terephthalic acid, 22 parts of trimellitic anhydride, and 2 parts of dibutyltin oxide were placed and reacted at normal pressure at 230°C for 8 hours, and then further reacted at a reduced pressure of 10 mmHg to 15 mmHg for 5 hours to obtain an [intermediate polyester resin]. The obtained [intermediate polyester resin] had a number average molecular weight of 2,100, a weight average molecular weight of 9,500, a glass transition temperature (Tg) of 55° C., an acid value of 0.5 mg KOH / g, and a hydroxyl value of 51 mg KOH / g. Next, 410 parts of the [intermediate polyester resin], 89 parts of isophorone diisocyanate, and 500 parts of ethyl acetate were placed in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, and reacted at 100°C for 5 hours to obtain a [prepolymer]. The free isocyanate % of the obtained [prepolymer] was 1.53%.
[0185] -Preparation of release agent dispersion- A container equipped with a stirring rod and a thermometer was charged with 70 parts of carnauba wax (WA-05, manufactured by Cerarica Noda Co., Ltd.), 140 parts of [polyester resin], and 290 parts of ethyl acetate. The mixture was heated to 75°C with stirring, and was maintained at 75°C for 1.5 hours. The mixture was then cooled to 30°C in 1 hour. A bead mill (Ultraviscomill, manufactured by Imex Co., Ltd.) was used to disperse the mixture under the conditions of a liquid delivery rate of 5 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume of 0.5 mm zirconia beads, and 3 passes to obtain a [release agent dispersion].
[0186] - Preparation of master batch - 1,000 parts of water, 1,000 parts of carbon black, and 1,000 parts of [polyester resin] were added and mixed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.). The mixture was kneaded using two rolls at 150°C for 30 minutes, then rolled and cooled, and pulverized in a pulverizer to obtain [Masterbatch 1].
[0187] -Preparation of layered inorganic mineral masterbatch- 100 parts of [polyester resin], 100 parts of a montmorillonite compound modified with a quaternary ammonium salt having at least a benzyl group (Clayton APA, manufactured by Southern Clay Products, particle size 500 nm), and 50 parts of ion-exchanged water were thoroughly mixed and kneaded in an open roll kneader (Kneadex / manufactured by Mitsui Mining Co., Ltd.). The kneading temperature was started at 90°C, and then gradually cooled to 50°C to produce [layered inorganic mineral master batch 1] with a resin to pigment ratio (mass ratio) of 1:1.
[0188] - Preparation of oil phase 1 - In a vessel equipped with a thermometer and a stirrer, 70.4 parts of [polyester resin], 113 parts of [release agent dispersion], 68 parts of [master batch 1], 1.6 parts of [layered inorganic mineral master batch 1], and 122 parts of ethyl acetate were placed and dispersed using a shear disperser (TK Homomixer) at a peripheral speed of 13.5 m / sec. Then, using a bead mill (Ultra Visco Mill, manufactured by Imex Co., Ltd.), dispersion was performed under conditions of a liquid delivery speed of 5 kg / hr, a disk peripheral speed of 10 m / sec, 80 volume % filling of 0.3 mm zirconia beads, and 3 passes to obtain [oil phase 1].
[0189] -Production of aqueous dispersion of resin particles- In a reaction vessel equipped with a stirring rod and a thermometer, 600 parts of water, 120 parts of styrene, 100 parts of methacrylic acid, 45 parts of butyl acrylate, 10 parts of sodium alkylarylsulfosuccinate (Eleminol JS-2, Sanyo Chemical Industries Co., Ltd.), and 1 part of ammonium persulfate were charged and stirred at 400 rpm for 20 minutes, resulting in a white emulsion. The emulsion was heated to an internal temperature of 75°C and reacted for 6 hours. 30 parts of a 1% aqueous solution of ammonium persulfate was further added, and the mixture was aged at 75°C for 6 hours to obtain an aqueous dispersion of resin fine particles. The volume average particle size of the particles contained in this aqueous dispersion of resin fine particles was 60 nm, the weight average molecular weight of the resin content was 140,000, and Tg was 73°C.
[0190] - Preparation of aqueous phase - 990 parts of water, 83 parts of [aqueous dispersion of resin fine particles], 37 parts of a 48.5% aqueous solution of sodium dodecyldiphenyletherdisulfonate (Eleminol MON-7, manufactured by Sanyo Chemical Industries, Ltd.), and 90 parts of ethyl acetate were mixed and stirred to obtain an [aqueous phase].
[0191] -Emulsification or dispersion- 77 parts of ethyl acetate solution of [prepolymer] and 2.5 parts of 50% ethyl acetate solution of isophoronediamine were added to 374 parts of the [oil phase 1], and the mixture was stirred at 5,000 rpm with a TK homomixer (manufactured by Tokushu Kika Co., Ltd.) to uniformly dissolve and disperse the mixture to obtain [oil phase 1']. Next, 550 parts of [water phase] were placed in another container equipped with a stirrer and a thermometer, and [oil phase 1'] was added while stirring at 11,000 rpm with a TK homomixer (manufactured by Tokushu Kika Co., Ltd.), and emulsified for 1 minute to obtain [emulsion slurry 1].
[0192] -Desolvation-Washing-Drying- [Emulsified slurry 1] was placed in a container equipped with a stirrer and a thermometer, and the solvent was removed under reduced pressure at 30°C for 8 hours to obtain [Slurry 1]. The obtained [Slurry 1] was kept at 45°C for 2 hours, filtered under reduced pressure, and subjected to the following washing treatment. (1) 100 parts of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at 6,000 rpm for 5 minutes), and then filtered. (2) 100 parts of ion-exchanged water was added to the filter cake of (1) and mixed with a TK homomixer (at a rotation speed of 6,000 rpm for 5 minutes), and then 1% hydrochloric acid was added under stirring until the pH reached about 3.3. Stirring was continued in that state for 1 hour, and then the mixture was filtered. (3) 300 parts of ion-exchanged water was added to the filter cake of (2), and the mixture was mixed with a TK homomixer (at a rotation speed of 6,000 rpm for 5 minutes), followed by filtering twice to obtain [Filter Cake 1].
[0193] The obtained [filter cake 1] was dried in a circulating air dryer at 40° C. for 48 hours, and then sieved through a 75 μm mesh to prepare [toner base particles 1].
[0194] -Smoothing process- The filtrate obtained in the above-mentioned step (2) was heated at 43°C for 20 minutes and filtered. 300 parts of ion-exchanged water was added to the filter cake obtained by this, and the mixture was mixed with a TK homomixer (at a rotation speed of 6,000 rpm for 5 minutes) and then filtered twice to obtain [filter cake 2].
[0195] The obtained [filter cake 2] was dried in a circulating air dryer at 40° C. for 48 hours, and then classified in an elbow jet classifier to prepare [toner base particles 2] having a peak of 2 μm in the number particle size distribution.
[0196] -mixture- [Toner base particle 2] was added to the above [toner base particle 1] to form base particles, and 1.5 parts of hydrophobic silica (HDK-2000, manufactured by Wacker Chemie) was added to 100 parts of base particles, and mixed for 5 minutes at a peripheral speed of 33 m / s in a 20 L Henschel mixer (manufactured by Mitsui Mining Co., Ltd.). The above was air-sieved through a 500 mesh sieve to obtain [toner 1]. The volume particle size distribution and number particle size distribution of the obtained [toner 1] were measured using a Multisizer3 (manufactured by Beckman Coulter, Inc.), and the ratio A / B of the intensity A of the particle size X μm in the volume particle size distribution to the intensity B of the maximum peak in the range of 4 μm to 8 μm in the volume particle size distribution was calculated, where X μm is the particle size of the second peak in the range of 1 μm to 3 μm in the number particle size distribution.
[0197] Example 2 [Filter cake 2] was prepared in the same manner as in Example 1, except that the treatment conditions of the filtrate in the smoothing treatment in Example 1 were changed from 43° C. and 20 minutes to 50° C. and 15 minutes. Thereafter, the mixture was dried under the same conditions as in Example 1, and classified using the same classifier to prepare [toner base particles 2] having a peak in the number particle size distribution of 1.2 μm. [Toner base particles 2] were added to the above [Toner base particles 1] to form base particles, and hydrophobic silica was mixed and air-sieved under the same conditions as in Example 1 to obtain [Toner 2].
[0198] Example 3 [Filter cake 2] was prepared in the same manner as in Example 1, except that the treatment conditions of the filtrate in the smoothing treatment in Example 1 were changed from 20 minutes at 43° C. to 15 minutes at 43° C. Thereafter, the mixture was dried under the same conditions as in Example 1, and classified using the same classifier to prepare [toner base particles 2] having a peak in the number particle size distribution of 2.8 μm. [Toner base particles 2] were added to the above [Toner base particles 1] to prepare base particles, and hydrophobic silica was mixed and air-sieved under the same conditions as in Example 1 to obtain [Toner 3].
[0199] Example 4 [Filter cake 2] was prepared in the same manner as in Example 1, except that the treatment conditions of the filtrate in the smoothing treatment in Example 1 were changed from 43° C. for 20 minutes to 50° C. for 20 minutes. Thereafter, the mixture was dried under the same conditions as in Example 1, and classified using the same classifier to prepare [toner base particles 2] having a peak in the number particle size distribution of 1.1 μm. [Toner base particles 2] were added to the above [Toner base particles 1] to prepare base particles, and hydrophobic silica was mixed and air-sieved under the same conditions as in Example 1 to obtain [Toner 4].
[0200] Example 5 [Filter cake 2] was prepared in the same manner as in Example 1, except that the treatment conditions of the filtrate in the smoothing treatment in Example 1 were changed from 43° C. and 20 minutes to 40° C. and 30 minutes. Thereafter, the mixture was dried under the same conditions as in Example 1, and a [toner base 2] having a peak in the number particle size distribution of 3.0 μm was prepared using the same classifier. [Toner base particles 2] were added to the above [Toner base particles 1] to prepare base particles, and hydrophobic silica was mixed and air-sieved under the same conditions as in Example 1 to obtain [Toner 5].
[0201] Example 6 The toner was dried under the same conditions as in Example 1, and classified using the same classifier to prepare a toner base 2 having a peak in the number particle size distribution of 3.0 μm. [Toner base particles 2] were added to the above [Toner base particles 1] to prepare base particles, and hydrophobic silica was mixed and air-sieved under the same conditions as in Example 1 to obtain [Toner 6].
[0202] Comparative Example 1 [Filter cake 2] was prepared in the same manner as in Example 1, except that the treatment conditions of the filtrate in the smoothing treatment in Example 1 were changed from 43° C. and 20 minutes to 50° C. and 30 minutes. Thereafter, the mixture was dried under the same conditions as in Example 1, and a [toner base 2] having a peak in the number particle size distribution of 0.8 μm was prepared using the same classifier. [Toner base particles 2] were added to the above [Toner base particles 1] to prepare base particles, and hydrophobic silica was mixed and air-sieved under the same conditions as in Example 1 to obtain [Toner 7].
[0203] Comparative Example 2 [Filter cake 2] was prepared in the same manner as in Example 1, except that the treatment conditions of the filtrate in the smoothing treatment in Example 1 were changed from 43° C. and 20 minutes to 40° C. and 15 minutes. Thereafter, the mixture was dried under the same conditions as in Example 1, and a [toner base 2] having a peak in the number particle size distribution of 3.2 μm was prepared using the same classifier. [Toner base particle 2] was added to the above [Toner base particle 1] to prepare base particles, and hydrophobic silica was mixed and air-sieved under the same conditions as in Example 1 to obtain [Toner 8].
[0204] Comparative Example 3 Toner base particles 1 of Example 1 having a peak in the volumetric particle size distribution of 3.8 μm, toner base particles 2 having a peak in the number particle size distribution of 2.5 μm were added, and hydrophobic silica was mixed and air-sieved under the same conditions as in Example 1 to obtain toner 9.
[0205] Comparative Example 4 Toner base particles 1 in Example 1 having a volume particle size distribution peak of 8.3 μm, toner base particles 2 having a number particle size distribution peak of 2.8 μm were added, and hydrophobic silica was mixed and air-sieved under the same conditions as in Example 1 to obtain toner 10.
[0206] Table 1 shows the preparation conditions of the toner obtained as above and the measurement results of the BET specific surface area. The BET specific surface area was measured by the following procedure. Specifically, the BET specific surface area can be measured using an automatic specific surface area / pore distribution measuring device (TriStar3000: manufactured by Shimadzu Corporation). In detail, 5.0 g of the sample is weighed into a sample cell, and this is vacuum-dried for 24 hours using a pretreatment Smart Presso (manufactured by Shimadzu Corporation) to remove impurities and moisture from the sample surface. The sample cell after pretreatment is set in the TriStar3000, and the relationship between the amount of nitrogen gas adsorption and the relative pressure is obtained. From this relationship, the BET specific surface area of the sample is measured using the BET multipoint method. [Table 1]
[0207] <Preparation of developer> 5 parts of the above [Toner 1] and 95 parts of the carrier described below were mixed in a Turbula Shaker Mixer (manufactured by Shinmaru Enterprises) to obtain a developer. -Creating the carrier- Silicone resin (organo straight silicone) 100 parts Toluene 100 parts γ-(2-aminoethyl)aminopropyltrimethoxysilane 5 parts Carbon black 10 parts The above mixture was dispersed in a homomixer for 20 minutes to prepare a coating layer forming liquid. The coating layer forming liquid was coated on the surface of 1000 parts of spherical magnetite having a particle size of 50 μm using a fluidized bed type coating device to obtain a magnetic carrier.
[0208] Using an image forming apparatus using [Developer 1] containing [Toner 1], the image transferability, in-machine staining, and cleanability were evaluated by the evaluation methods described below.
[0209] [Evaluation of transferability] Using a Ricoh Co., Ltd. copy machine (Imagio MP 7501) evaluation machine tuned to a linear speed of 162 mm / sec and a transfer time of 40 msec, the above [Developer 1] was tested on an A4 size sheet with a toner adhesion of 0.6 mg / cm 2A running test was conducted in which a solid pattern of the above was output as a test image. At the beginning of the test image and after 100K output, the transfer efficiency in the primary transfer was calculated using the following formula (2), and the transfer efficiency in the secondary transfer was calculated using the following formula (3). The evaluation criteria are as follows: Primary transfer efficiency (%)=(amount of toner transferred onto intermediate transfer body / amount of toner developed onto electrophotographic photoreceptor)×100 (Equation 2) Secondary transfer efficiency (%) = (amount of toner transferred onto intermediate transfer body - amount of toner remaining on intermediate transfer body) / amount of toner transferred onto intermediate transfer body) × 100 (Equation 3) -Evaluation criteria- The evaluation criteria were as follows: the primary transfer rate was multiplied by the secondary transfer rate, and the result was evaluated according to the following criteria. Rank: Transcription rate 10: 99.0% or more 9: 98.0% or more but less than 99.0% 8: 96.0% or more but less than 98.0% 7: 94.0% or more but less than 96.0% 6: 92.0% or more but less than 94.0% 5: 90.0% or more but less than 92.0% 4: 88.0% or more but less than 90.0% 3: 86.0% or more but less than 88.0% 2: 84.0% or more but less than 86.0% 1: Less than 84.0%
[0210] [Evaluation of in-flight contamination] The developer 1 of the above example was placed in a modified Ricoh digital color imagio Neo C600 machine and evaluated. After running output of 100,000 sheets of an image chart with a 50% image area in monochrome mode, the prints and dirt around the fixing and paper discharge sections were visually observed and evaluated by comparing them with samples on a 10-level scale (R1 to R10). The rank of the stains on the printed matter and around the fixing and ejecting section indicates the degree of staining in ascending order. The evaluation of R1 shows unacceptable levels of dirt both around the fixing section and on the printed matter, and is at a level that cannot be used as a product.
[0211] [Evaluation of shatterability] The scattering evaluation was carried out to measure the amount of toner scattered inside the machine that cannot be confirmed by the inside-machine contamination evaluation. Although the amount of toner scattered does not cause any adverse effects inside the machine in the medium term, in the long term, the scattered toner causes contamination inside the machine and affects images as stains. The developer 1 of the above example was placed in a developing roller removed from a Ricoh imagio-MPC5002 and evaluated. The developing roller was rotated at 700 rpm for 1 minute, and the toner scattered from the developing roller was collected and its mass was measured. --Evaluation criteria-- Rank: Scattered mass 10: Less than 10 mg 9: 10 mg or more but less than 15 mg 8: 15 mg or more but less than 20 mg 7: 20 mg or more but less than 25 mg 6: 25 mg or more but less than 30 mg 5: 30 mg or more but less than 35 mg 4: 35 mg or more but less than 40 mg 3: 40 mg or more but less than 45 mg 2: 45 mg or more but less than 50 mg 1: 50mg or more
[0212] [Evaluation of blade cleaning ability] The blade cleaning performance was evaluated by using a color copier (Ipsio Color8100; manufactured by Ricoh Co., Ltd.) loaded with the developer and the electrostatic latent image carrier (electrophotographic photoconductor, photoconductor), running 100,000 sheets using 6000 paper (manufactured by Ricoh Co., Ltd.) at a print rate of 7% image occupancy, and then outputting 10 images with an image occupancy of 50% continuously in an environment at 10°C and 15% RH, and stopping during development of the 10th sheet. During this process, the toner on the drum before and after the cleaning blade on the photoconductor was transferred to the tape. The transfer tape was attached to 6000 paper and the ID was measured using an X-Rite eXact (X-Rite Corporation), and the cleaning rate was calculated from the ID using the following formula (4). Note that 2 is equivalent to the conventional product, and 1 is a level that cannot be used as a product. Cleaning rate [%] = ΔID (transfer residual ID - post-cleaning ID) / transfer residual ID (Formula 4) -Evaluation criteria- Rank: Cleaning rate 5: 80% or more 4: 60% to less than 80% 3: 40% to less than 60% 2: 20% to less than 40% 1: Less than 20%
[0213] [Image quality evaluation] The developer 1 of the above example was placed in a modified Ricoh digital color imagio Neo C600 machine and evaluated. Ten lines, each 300 μm wide and 100 mm long, were printed in monochrome mode, and the printed matter was observed using an optical microscope to measure the length L1 covered by the toner and the distance L2 to which the toner was fixed. The length of L2 relative to L1 (L2 / L1) was treated as one piece of data, and several points were evaluated at random locations on each of the 10 output lines, and the lines were ranked by comparing them with our company's ranking table. Specifically, the output printout is observed with an optical microscope or the like, and the point on the top surface of the line segment where the focus is located is taken as H0, and the paper surface is taken as H100. The distance from H0 to H100 is divided into 100 equal parts, and the width of the line segment at point H20, which is moved 20 equal parts in height from H0 toward the paper surface, is taken as L1. The length of both ends of the line segment where toner is fixed on the paper surface is taken as L2. -Evaluation criteria- Rank: L2 / L1 10: less than 1.01 7: 1.01 or more and less than 1.05 4: 1.05 or greater but less than 1.10 1:1.10 or higher
[0214] <Overall Judgment> The evaluation criteria for the overall judgment are as follows: The total score of the ranks of "transferability," "in-machine staining," "scattering," "blade cleanability," and "image quality" was calculated, and an overall judgment was made based on the following evaluation criteria. "A" is extremely good, "B" is very good, "C" is good, "D" is equivalent to the conventional product, and "E" is not practically usable. "A", "B" and "C" are considered pass, and "D" and "E" are fail. Moreover, those with a blade cleaning performance rank of "1" were given an overall rating of "E" regardless of the total score. The results are shown in Table 2. Overall rating: Total score of the rank A: 42 or more B: 40 or more and 41 or less C: 36 or more and 39 or less D: 35 or less E: Blade cleaning rank 1
[0215] [Table 2]
[0216] As is clear from the evaluation results in Table 2, the transferability, in-machine staining, scattering, blade cleanability, and image quality are all at high levels for Examples 1 to 6. On the other hand, the results for Comparative Examples 1 to 4 are at low levels for any of the four items.
[0217] For example, aspects of the present invention are as follows. <1> The number particle size distribution has a maximum peak in the range of 4 μm or more and less than 8 μm, and a second peak in the range of 1 μm or more and less than 3 μm, When the particle size of the second peak in the number particle size distribution is X μm, the ratio A / B of the intensity A of the particle size of X μm in the volume particle size distribution to the intensity B of the maximum peak in the range of 4 μm or more and less than 8 μm in the volume particle size distribution is 0.2 or less, The BET specific surface area of the toner base particles and the BET specific surface area of the toner particles less than 5 μm in the volume particle size distribution are 2.0 m 2 / g or more 4.0m 2 / g or less. <2> The BET specific surface area (m 2 / g) is the BET specific surface area (m 2 / g) or less. <1> The toner is as described above. <3> The BET specific surface area (m 2 / g) is 2.0m 2 / g or more 3.0m 2 / g or less. <1> from <2> The toner according to any one of claims 1 to 5, <4> The above <1> from <2> 2. A toner storage unit comprising the toner according to claim 1, wherein the toner is a toner containing material. <5> The above <4> a toner storage unit according to claim 1, an electrostatic latent image forming means for forming an electrostatic latent image on an electrostatic latent image carrier; a developing means for developing the electrostatic latent image with the toner to form a toner image; a transfer means for transferring the toner image onto a recording medium; and a fixing unit for fixing the transferred image transferred onto the recording medium. <6> an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; The above <1> from <2> a developing step of developing the electrostatic latent image with the toner according to any one of claims 1 to 4 to form a toner image; a transfer step of transferring the toner image onto a recording medium; and a fixing step of fixing the transferred image transferred onto the recording medium.
[0218] The above <1> from <3> The toner according to any one of the preceding claims. <4> The toner storage unit according to <5> and the image forming apparatus according to the above. <6> According to the image forming method described in the above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]
[0219] 10 Electrostatic latent image carrier (photoconductor drum) 10K Black Electrostatic Latent Image Carrier 10Y Yellow electrostatic latent image carrier 10M Magenta electrostatic latent image carrier 10C Cyan electrostatic latent image carrier 14 Support roller 15 Support roller 16 Support roller 17 Intermediate transfer cleaning device 18 Image forming means 20 Charging roller 21 Exposure equipment 22 Secondary transfer device 23 Laura 24 Secondary transfer belt 25 Fixing device 26 Fixing belt 27 Pressure roller 28 Sheet reversing device 32 Contact Glass 33 First Running Body 34 Second Running Body 35 Imaging Lens 36 Reading sensor 40 Developing device 41 Developing belt 42K Developer compartment 42Y Developer storage unit 42M Developer compartment 42C Developer container 43K Developer supply roller 43Y Developer supply roller 43M Developer supply roller 43C Developer supply roller 44K developing roller 44Y Developing roller 44M Developing roller 44C Developing roller 45K Black Development Unit 45Y Yellow Development Unit 45M Magenta Development Unit 45C Cyan Development Unit 49 Registration roller 50 Intermediate transfer belt 51 Lola 52 Separation roller 53 Manual feed path 54 Manual feed tray 55 Switching claw 56 Discharge roller 57 Output Tray 58 Corona charging device 60 Cleaning Equipment 61 Developing device 62 Transfer roller 63 Photoconductor cleaning device 64 Static electricity removal lamp 70 Static electricity removal lamp 80 Transfer roller 90 Cleaning Equipment 95 Transfer paper 100A, 100B, 100C image forming device 120 Image forming unit 130 Manuscript stand 142 Paper feed roller 143 Paper Bank 144 Paper feed cassette 145 Separation roller 146 Paper feed path 147 Transport roller 148 Paper feed path 150 Copying device body 160 Charging device 200 Paper feed table 300 Scanner 400 Automatic Document Feeder (ADF) 401 Fixing roller 402 Pressure roller 403 Load Cell 404 Fulcrum 405 Measuring claw 406 Load S Recording medium N Nip [Prior art documents] [Patent documents]
[0220] [Patent Document 1] JP 2008-287150 A [Patent Document 2] Japanese Patent Application Publication No. 7-92738
Claims
1. The number particle size distribution has a maximum peak in the range of 4 μm or more and less than 8 μm, and a second peak in the range of 1 μm or more and less than 3 μm, When the particle size of the second peak in the number particle size distribution is X μm, the ratio A / B of the intensity A of the particle size X μm in the volume particle size distribution to the intensity B of the maximum peak in the range of 4 μm or more and less than 8 μm in the volume particle size distribution is 0.2 or less, The BET specific surface area of the toner base particles and the BET specific surface area of the toner particles less than 5 μm in the volume particle size distribution are 2.0 m 2 / g or more 4.0m 2 / g or less.
2. The BET specific surface area (m 2 / g) is the BET specific surface area (m 2 2. The toner according to claim 1, wherein the toner has a molecular weight of 1 / g or less.
3. The BET specific surface area (m 2 / g) is 2.0 m 2 / g or more 3.0m 2 The toner according to claim 1 , wherein the toner has a molecular weight of 1 / g or less.
4. A toner storage unit containing the toner according to claim 1 or 2.
5. The toner storage unit according to claim 4 , an electrostatic latent image forming means for forming an electrostatic latent image on an electrostatic latent image carrier; a developing means for developing the electrostatic latent image with the toner to form a toner image; a transfer means for transferring the toner image onto a recording medium; and a fixing unit for fixing the transferred image transferred onto the recording medium.
6. an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image with the toner according to claim 1 to form a toner image; a transfer step of transferring the toner image onto a recording medium; a fixing step of fixing the transferred image transferred onto the recording medium.
Citation Information
Patent Citations
Electrostatic charge image developing toner, one-component developer, two-component developer, and manufacture of toner particle
JP1995092738A
Toner and image forming method
JP2008287150A