Long-fiber composite material for solar module

A long fiber composite material with specific plastic and glass fiber ratios addresses the weight and corrosion issues of metal brackets, providing lightweight and durable solar module supports.

JP2024137583AInactive Publication Date: 2024-10-07NANYA PLASTICS CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023087535
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-25
Filing Date
2023-05-29
Publication Date
2024-10-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Solar module brackets made of aluminum alloy or stainless steel are heavy and prone to corrosion, which affects their durability and increases construction difficulty.

Method used

A long fiber composite material comprising 35-55% plastic pellets, 30-65% glass long fibers, 0.1-1% ultraviolet absorber, and 0.1-1% light stabilizer, with a weight ratio of plastic pellets to glass fibers ranging from 90:10 to 35:65, is used to create lightweight and corrosion-resistant solar brackets.

Benefits of technology

The composite material reduces the weight of solar brackets while enhancing their corrosion resistance and mechanical properties, making them suitable for outdoor use in solar modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137583000001
    Figure 2024137583000001
  • Figure 2024137583000002
    Figure 2024137583000002
  • Figure 2024137583000003
    Figure 2024137583000003
Patent Text Reader

Abstract

To provide a long-fiber composite material for a solar module.SOLUTION: A long-fiber composite material for a solar module includes: (a) 35 wt.%-55 wt.% of plastic pellets that are composed of polypropylene or nylon, (b) 30 wt.%-65 wt.% of glass filaments, (c) 0.1 wt.%-1 wt.% of an ultraviolet absorber, and (d) 0.1 wt.%-1 wt.% of a photostabilizer. The weight ratio of the plastic pellets to the glass filaments (plastic pellet:glass filament) is 90:10-35:65.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to long fiber composite materials, in particular long fiber composite materials for solar modules. [Background technology]

[0002] Solar modules mainly use brackets to support the structure of the solar panels, but the brackets in the prior art are usually made of aluminum alloy or stainless steel, which makes the total weight of the brackets heavy and difficult to construct. In addition, metal materials such as aluminum alloy and stainless steel are easily corroded by rainwater, which can cause galvanic corrosion and shorten the life of the brackets.

[0003] Therefore, by improving the material composition and manufacturing a lightweight solar bracket out of plastic materials, the disadvantages of metal brackets being prone to corrosion and heavy weight can be overcome, which is an important problem to be solved in this project. Summary of the Invention [Problem to be solved by the invention]

[0004] The technical problem that the present invention aims to solve is to provide a long fiber composite material for solar modules in response to the shortcomings of the prior art. [Means for solving the problem]

[0005] The long fiber composite material for solar modules contains (a) 35wt% to 55wt% of plastic pellets which are polypropylene or nylon, (b) 30wt% to 65wt% of long glass fibers, (c) 0.1wt% to 1wt% of an ultraviolet absorber, and (d) 0.1wt% to 1wt% of a light stabilizer. The weight ratio of the plastic pellets to the long glass fibers (the plastic pellets:the long glass fibers) is 90:10 to 35:65.

[0006] In one embodiment, the content of the ultraviolet absorbing agent is 0.4 wt% to 0.8 wt%.

[0007] In one embodiment, the content of the light stabilizer is 0.4 wt% to 0.8 wt%.

[0008] In one embodiment, the density of the long fiber composite material is 1.12 g / cm 3 ~1.56g / cm 3 It is.

[0009] In one embodiment, the plastic pellets have a melt index of 0.5 to 30.

[0010] In one embodiment, the long glass fibers have a fiber length of 5 μm to 25 μm.

[0011] In one embodiment, the long fiber composite further comprises 0.5 wt% to 10 wt% of a toughening agent.

[0012] In one embodiment, the long fiber composite material further comprises 0.5 wt % to 10 wt % of a compatibilizer.

[0013] In one embodiment, the long fiber composite material further comprises 0.1 wt% to 0.6 wt% of an antioxidant.

[0014] In one embodiment, the long fiber composite material further comprises 0.1 wt % to 2 wt % of a lubricant. Effect of the Invention

[0015] As an advantageous effect of the present invention, the long fiber composite material for solar modules of the present invention has the technical features of "containing 30 wt% to 65 wt% of long glass fiber" and "the weight ratio of the plastic pellets to the long glass fiber (plastic pellets:long glass fiber) is 90:10 to 35:65", thereby reducing the weight of the solar bracket and improving the corrosion resistance of the solar bracket. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] In order to better understand the features and technical contents of the present invention, please refer to the following detailed description of the present invention. However, the detailed description provided is only for reference and explanation, and is not intended to limit the scope of the present invention.

[0017] The "long fiber composite material for solar modules" according to the present invention will be described below by certain specific embodiments, and those skilled in the art can understand the advantages and effects of the present invention based on the contents disclosed in this specification. The present invention can be implemented or applied by other different specific embodiments, and various modifications and changes can be made to each detail in this specification based on different perspectives and applications without departing from the concept of the present invention. The technical contents according to the present invention will be described in more detail based on the following embodiments, but the disclosure does not limit the protection scope of the present invention. In addition, the term "or" used in this specification may include any one or more combinations of the relevant items listed according to the actual situation.

[0018] A first embodiment of the present invention provides a long fiber composite material for a solar module, comprising: (a) 35 wt% to 55 wt% of plastic pellets which are polypropylene or nylon; (b) 30 wt% to 65 wt% of long glass fibers; (c) 0.1 wt% to 1 wt% of an ultraviolet absorber; and (d) 0.1 wt% to 1 wt% of a light stabilizer.

[0019] The density of polypropylene is approximately 0.89 g / cm 3 ~0.91g / cm 3 In the long fiber composite material according to the present invention, the density is 1.12 g / cm3 by using plastic pellets. 3 ~1.56g / cm 3By manufacturing the long fiber composite material of the present invention, the weight of the solar bracket can be reduced according to the needs of the solar bracket. In addition, polypropylene is a recycled plastic material, and its resin identification code according to the American Plastics Industry Association is 5. Thus, the long fiber composite material of the present invention has recycling properties.

[0020] For example, the polypropylene used in the present invention may be homopolypropylene (PP-H), random copolymer polypropylene (PP-R) or block copolymer polypropylene (PP-B). Considering the processing characteristics of the plastic pellets, plastic pellets having a melt index of 0.5 to 30 are used. If the melt index of the plastic pellets is less than 0.5, the fluidity is poor and processing is difficult. If the melt index of the plastic pellets is more than 30, the viscosity after melting the plastic material is low, making it difficult to perform molding processing.

[0021] It is worth noting that the rigidity of the plastic pellets is low, which is disadvantageous in the manufacture of solar brackets. In the present invention, in order to improve the rigidity of the plastic pellets, long glass fibers are further added. Based on the total weight of the long fiber composite material, the amount of the long glass fibers added is 30wt% to 65wt%, and preferably 30wt% to 60wt%. If the amount of the long glass fibers added is less than 30wt%, the rigidity of the long fiber composite material is insufficient. If the amount of the long glass fibers added is more than 65wt%, the impact resistance of the long fiber composite material is reduced. Thus, in order to achieve both the rigidity and impact resistance of the long fiber composite material, the weight ratio of the plastic pellets to the long glass fibers (plastic pellets:long glass fibers) is 90:10 to 35:65, and preferably 75:25 to 40:60.

[0022] In one embodiment of the present invention, the fiber length of the long fiber composite material (Long Glass Fiber, LGF) is 5 μm to 25 μm. If the fiber length is less than 5 μm, the effect of improving the rigidity of the long fiber composite material cannot be achieved. If the fiber length exceeds 25 μm, it affects the dispersibility of the long glass fiber in the long fiber composite material, which affects the molding processability and the use function of the product.

[0023] In addition, polypropylene does not have UV resistance, so when it is irradiated with UV for a long time, its mechanical properties deteriorate, leading to discoloration, cracking, or surface chalking due to aging. Therefore, the long fiber composite material according to the present invention may be added with 0.1wt% to 1wt% of UV absorber in order to be suitable for manufacturing solar brackets. If the amount of UV absorber added is less than 0.1wt%, the bracket surface will chalk and the strength will decrease. If the amount of UV absorber added is more than 1wt%, the material will be wasted.

[0024] For example, the UV absorber according to the present invention may be one or more of phenyl salicylate, 2-hydroxy-4-methoxybenzophenone, 2,4-dihydroxybenzophenone, resorcinol monobenzoate, 2-(3',5'-di-tert-butyl-2'-hydroxyphenyl)-5-chlorobenzotriazole, 2-hydroxy-4-n-octyloxybenzophenone, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, hydroxyphenyltriazine, and 2-[2'-hydroxy-3',5'-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole. Preferably, the UV absorber may be a UV absorber (Cyasorb UV 531) manufactured by Cytec Industries.

[0025] More specifically, by combining the ultraviolet absorber of the present invention with a light stabilizer, the light stabilization effect can be further improved, and damage to the long fiber composite material caused by sunlight can be reduced. More specifically, in order to achieve an excellent light stabilization effect, the long fiber composite material of the present invention contains 0.1wt% to 1wt% of a light stabilizer. If the amount of the light stabilizer added is less than 0.1wt%, chalking of the bracket surface occurs and the strength decreases. If the amount of the light stabilizer added is more than 1wt%, the material is wasted.

[0026] For example, the light stabilizer according to the present invention may be one or more of 2,2'-thiobis(4-tert-octylphenoxy)nickel, 2,4,6-tris(4-butoxy-2-hydroxyphenyl)-1,3,5-triazine, tris(1,2,2,6,6-pentamethyl-piperidyl)phosphite, polymer of succinic acid and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol, hexamethylphosphoric triamide, bis(2,2,6,6-tetramethylpiperidyl) sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, and hindered phenol. Preferably, the light stabilizer is Chimassorb® 2020 manufactured by BASF.

[0027] In one embodiment of the present invention, the long fiber composite material may further contain 0.5wt% to 10wt% of a toughening agent to improve the impact resistance of the long fiber composite material. If the content of the toughening agent contained in the long fiber composite material is less than 0.5wt%, the impact resistance of the long fiber composite material will be insufficient. If the content of the toughening agent contained in the long fiber composite material is more than 10wt%, the tensile strength and bending strength will be reduced.

[0028] For example, the toughening agent may be polyolefin elastomer (POE), which is a polyolefin-like material obtained by copolymerizing ethylene with propylene or other α-olefins (e.g., 1-butene, 1-hexene, 1-octene, etc.). Compared with polyolefin plastics, the amount of copolymerized monomer in the molecular chain of the polyolefin-like material is relatively high, and the density is low, making it suitable for manufacturing lightweight solar brackets.

[0029] Polyolefin elastomers mainly include two kinds: ethylene propylene copolymer and ethylene / α-olefin copolymer. Ethylene propylene copolymer elastomers mainly include two kinds: ethylene propylene rubber (EPM) and ethylene propylene diene rubber (EPDM). Ethylene / α-olefin copolymer elastomers mainly include two kinds: ethylene / α-olefin random copolymer (POE) and ethylene / α-olefin block copolymer (OBC).

[0030] In one embodiment of the present invention, the long fiber composite material may further include 0.5wt% to 10wt% of a compatibilizer. If the content of the compatibilizer in the long fiber composite material is less than 0.5wt%, the compatibility is insufficient, resulting in deterioration of physical and mechanical properties. If the content of the compatibilizer in the long fiber composite material is more than 10wt%, the heat resistance temperature of the plastic alloy is reduced and the extrusion processability is reduced.

[0031] For example, the compatibilizer may be ethylene-propylene-diene monomer (EPDM) grafted with glycidyl methacrylate (GMA; EPDM-g-GMA or EPDM-GMA), poly(ethylene octene) grafted with glycidyl methacrylate (POE-g-GMA or POE-GMA), ethylene-propylene-diene monomer (EPDM), styrene-butadiene-styrene copolymer (SBS), styrene-ethylene-butylene-styrene copolymer (SEBS), polyolefin elastomer (POE), polyolefin elastomer grafted with maleic anhydride ... anhydride; POE-g-MA or POE-MA).

[0032] In one embodiment of the present invention, the long fiber composite material may further include 0.1wt% to 0.6wt% of an antioxidant. If the content of the antioxidant in the long fiber composite material is less than 0.1wt%, problems related to thermal decomposition will occur. If the content of the antioxidant in the long fiber composite material is more than 0.6wt%, material will be wasted. For example, the antioxidant may be one of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris(2,4-di-tert-butylphenyl)phosphite, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate, or a mixture of more than one of them.

[0033] In one embodiment of the present invention, the long fiber composite material may further contain 0.1wt% to 2wt% of a lubricant. If the content of the lubricant in the long fiber composite material is less than 0.1wt%, shear heat may occur due to insufficient lubrication during extrusion processing, leading to decomposition. If the content of the lubricant in the long fiber composite material is more than 2wt%, the lubricant may precipitate and lead to slippage during extrusion. For example, the lubricant may be at least one selected from the group consisting of a hydrocarbon-based lubricant, a fatty acid amide-based lubricant, a higher fatty acid-based lubricant, an ester-based lubricant, an alcohol-based lubricant, a metal soap-based lubricant, and a composite-based lubricant, but the above-mentioned specific examples are merely examples that can be implemented, and the present invention is not limited thereto.

[0034] In one embodiment of the present invention, a solar bracket with dimensions of 6.0 cm (height) x 4.2 cm (width) or 2.0 cm (height) x 3.0 cm (width) is manufactured by profile extrusion using long fiber composite material, but the length of the solar bracket can be adjusted as needed.

[0035] [Example 1] The long fiber composite material according to the first embodiment of the present invention contained 45 wt% plastic pellets, 50 wt% long glass fiber, 1 wt% UV absorber, 0.5 wt% light stabilizer, 1 wt% toughener, 1 wt% compatibilizer, and 1 wt% lubricant. Then, a solar bracket with a size of 6.0 cm (height) x 4.2 cm (width) was manufactured by profile extrusion.

[0036] [Comparative Example 1-1] Using the same long fiber composite material as in the first example, a solar bracket of 2.0 cm (height) x 3.0 cm (width) was manufactured by profile extrusion.

[0037] [Comparative Example 1-2] A solar bracket measuring 2.0 cm (height) x 3.0 cm (width) was manufactured using aluminum alloy T-6061.

[0038] [Model analysis of mold flow analysis software] In the present invention, the strains of the examples and comparative examples of the present application are evaluated by model analysis using mold flow analysis software, and the reliability of product design is improved. Here, the yield strength indicates the toughness of the material, and indicates the state in which the stress-strain ratio of a ductile material changes repeatedly when a load exceeds the elastic limit, and is the stress value at which a small increase in load causes breakage. Here, the long fiber composite material is a steel material, and does not have a yield strength. The break strength is the ratio of the tensile load required to break the material to the cross-sectional area, that is, the stress. The elongation ratio is the ratio of the total deformation of the gauge part after the sample is pulled to break to the original length of the gauge part. The Young's modulus evaluates the stiffness of an isotropic elastomer, and is the ratio of uniaxial stress to uniaxial deformation within the range applicable to Hooke's law. The Poisson's ratio is the ratio of the strain in the width direction of the material to the strain in the longitudinal direction of the material when the material is deformed by a force pulling or compressing the material. The maximum torque is the maximum force applied to the bracket, i.e. the maximum force is the force the bracket can withstand when simulating 17 levels of wind. The maximum stress is the stress the bracket can withstand. The experimental results are shown in Table 1.

[0039] [Table 1]

[0040] In the failure analysis, if the maximum stress of the bracket is greater than the breaking strength of the material itself, it is deemed to be a fail. For example, the maximum stress of the bracket of Comparative Example 1-1, 289.69 MPa, is greater than the breaking strength of the material, 100 MPa, and therefore was evaluated as a fail in the failure analysis. In comparison, the stress of the bracket of Example 1 is 100.91 MPa, which is close to the breaking strength of the material, 100 MPa, and therefore was evaluated as a pass in the failure analysis. The maximum stress of the bracket of Comparative Example 1-2, 253.42 MPa, is less than the breaking strength of the material, 313 MPa, and therefore was evaluated as a pass in the failure analysis. As shown in the results of Table 1, the breaking strength, elongation rate, and Young's modulus of the long fiber composite material are lower than those of the aluminum alloy, but the improvement of the structure allows it to meet the requirements of the solar bracket in the bracket simulation test.

[0041] [Weather resistance measurement] The weather resistance of plastics is evaluated mainly by natural exposure method and artificial accelerated test method. However, the natural exposure method is a method of directly or indirectly exposing to the natural environment, so it takes time and is highly affected by environmental factors, so it has low reproducibility. Therefore, the main method for evaluating the weather resistance of plastics is artificial aging test, and the most common method is light aging test. Plastics such as polypropylene (PP) and low-density polyethylene (LDPE) and rubber products can age when exposed to UV light for a long time, for example, becoming brittle, discoloring, and losing elasticity, while metals do not suffer from this phenomenon.

[0042] In the present invention, a solar bracket of 30 mm (height) x 30 mm (width) x 2.0 mm (thickness) was manufactured using different materials, and weather resistance was measured. As a test method, a lamp light source UVB (wavelength 313 nm) was irradiated for 4000 hours, and the mechanical strength was measured at 0 hours, 1200 hours, 2400 hours, 3000 hours, and 4000 hours, and the maintenance rate was calculated. The experimental materials and results are as shown in Table 2.

[0043] [Table 2] *SMC: Sheet molding compound, a thermosetting plastic reinforced with glass fibers.

[0044] As shown in Table 2, polyethylene (PE) was used in Example 2-1, and PP was used in Example 2-2. After 1200 hours of UV light irradiation, the tensile strength of Examples 2-1 and 2-2 respectively decreased to 31% and 22% of the original (measured at 0 hours), indicating that the weather resistance of PP and PE without UV absorbers is poor. According to Examples 2-3 and 2-4, the weather resistance obtained by adding long glass fiber composite material to PP is better than that obtained by adding long glass fiber composite material to PE. Specifically, even after 2400 hours of UV light irradiation, the tensile strength of Example 2-4, which added long fiber composite material to PP, can still maintain 80% of the original. Furthermore, according to Examples 2-5 and 2-6, it was shown that the effect of improving weather resistance was excellent when 0.5% UV absorber was added to PE and PP reinforced with long glass fiber. Preferably, when 0.5% UV absorber is added to the PP reinforced with long glass fiber, it is estimated that even after being irradiated with UV light for 4000 hours, its tensile strength can still maintain 92% of the original, that is, it can withstand outdoor sunlight for 20 years, which meets the requirements of solar modules.

[0045] [Upward tension test] The upward tensile test was performed using an M8 screw, but since the material is already beyond its elastic range in the process of being destroyed, it is difficult to define the start of destruction in a simulation analysis, and stress analysis is prone to inaccuracies. Therefore, the test method used was strain analysis, and the occurrence of maximum strain was set as the end point of the experiment. The experimental results are shown in Table 3.

[0046] [Table 3]

[0047] The maximum upward tensile force reached about 7000N, which was shown to be sufficient for use as a solar bracket. As shown in Table 3, the maximum strain of the aluminum alloy used in the comparative example occurred when the maximum upward tensile force was 9000N. The maximum strain of Example 3-2 occurred when the maximum upward tensile force was 1500N, but by increasing the width through structural improvement, the maximum upward tensile force (N) can reach 7000N. It should be noted that since the density of the long fiber composite material is relatively low, the weight of the solar bracket does not increase excessively even when the width is increased.

[0048] [Comparison of the functions of each material] Specific strength is the tensile strength divided by density, and specific flexural modulus is the flexural modulus divided by density. Specific strength and specific flexural modulus are properties of the material per unit weight. In the salt spray test according to the present invention, a standard solution of 5% sodium chloride (NaCl) was used to simulate a highly corrosive environment. The performance comparison of each material is shown in Table 4.

[0049] [Table 4] *If the salt spray resistance met the C3 level of the corrosive environment classification of ISO 9223, it was rated as good, otherwise it was rated as poor. *After 4000 hours of UV irradiation, if the tensile strength maintained 80% or more of its original value, it was rated "good", if it maintained 50-80% of its original value, it was rated "fair", and if it maintained less than 50% of its original value, it was rated "poor".

[0050] According to Table 4, the zinc-aluminum-magnesium alloy, aluminum alloy T-6061, and SS302 stainless steel were inferior in salt fog resistance, while 50% LGF-PP and 50% LGF nylon 6 were resistant to potential corrosion caused by salty rainwater, and the composite material of long fiber material and polypropylene was both resistant to potential corrosion and resistant to UV irradiation.

[0051] [Material price comparison] The LFT base unit price was estimated based on estimating the cost unit price based on 2022 / 3 and assuming an extrusion yield of 95%.

[0052] [Table 5]

[0053] As shown in Table 5, 50% LGF PP has the smallest density, which is advantageous for manufacturing light-weight solar brackets. In addition, since the raw material cost is low and no freon disposal fee is required, it is possible to manufacture environmentally friendly and economical solar brackets.

[0054] [Comparison of advantages and disadvantages of replacing alloys with LFT]

[0055] [Table 6]

[0056] As shown in Table 6, the long fiber composite has a low density, so it has a relatively light weight when manufacturing solar brackets. From the cost perspective, the composite of long fiber material and polypropylene is more economical to compound.

[0057] [Advantageous Effects of the Embodiments] The advantageous effects of the present invention are that the long fiber composite material for solar modules of the present invention has the technical features of "containing 30 wt% to 65 wt% of long glass fiber" and "the weight ratio of plastic pellets to long glass fiber (plastic pellets:long glass fiber) is 90:10 to 35:65", thereby reducing the weight of solar brackets and improving the corrosion resistance of the solar brackets.

[0058] In further detail, in the long fiber composite material of the present invention, since the plastic material replaces the metal material, there is no need to pay for freon disposal, and an environmentally friendly solar bracket can be manufactured. In addition, by using a composite of the long fiber material and polypropylene, the manufacturing cost of the plastic pellets can be further reduced.

[0059] The above disclosure is merely a preferred embodiment of the present invention, and the scope of the claims of the present invention is not limited thereto. Therefore, all equivalent technical modifications made by utilizing the contents of the specification and drawings of the present invention are included in the scope of the claims of the present invention.

Claims

1. (a) 35 wt % to 55 wt % of plastic pellets which are polypropylene or nylon; (b) 30 wt % to 65 wt % long glass fiber; (c) 0.1 wt % to 1 wt % of an ultraviolet absorber; (d) 0.1 wt % to 1 wt % of a light stabilizer; A long fiber composite material for a solar module, characterized in that a weight ratio of the plastic pellets to the long glass fibers (the plastic pellets:the long glass fibers) is 90:10 to 35:

65.

2. 2. The long fiber composite material for solar modules according to claim 1, wherein the content of the ultraviolet absorber is 0.4 wt% to 0.8 wt%.

3. The long fiber composite material for solar modules according to claim 1 , wherein the content of the light stabilizer is 0.4 wt % to 0.8 wt %.

4. The density of the long fiber composite material is 1.12 g / cm 3 ~1.56g / cm 3 2. The long fiber composite material for a solar module according to claim 1,

5. 2. The long fiber composite material for solar modules according to claim 1, wherein the melt index of the plastic pellets is 0.5-30.

6. 2. The long fiber composite material for solar modules according to claim 1, wherein the long glass fibers have a fiber length of 5 μm to 25 μm.

7. 10. The long fiber composite material for solar modules according to claim 1, further comprising 0.5 wt% to 10 wt% of a toughening agent.

8. 10. The long fiber composite material for solar modules according to claim 1, further comprising 0.5 wt% to 10 wt% of a compatibilizer.

9. 10. The long fiber composite material for solar modules according to claim 1, further comprising 0.1 wt% to 0.6 wt% of an antioxidant.

10. 10. The long fiber composite material for solar modules according to claim 1, further comprising 0.1 wt% to 2 wt% of a lubricant.

Citation Information

Patent Citations

  • Sheet-like composite material and its production

    JP1995300777A

  • Colored glass fiber-reinforced polyolefin composition

    JP1997183869A

  • Vehicle exterior part using stabilized weathering long glass-fiber reinforced polypropylene resin composition

    JP1997207233A

  • External part of vehicle using long glass fiber-reinforced polypropylene resin composition stabilized for weathering resistance

    JP1997208756A

  • Door handle, bezel, and grip using weather resistance stabilized long fiber glass reinforced polypropylene resin composition

    JP1997209617A