Catalyst for hydrogen generating electrode of water electrolysis, manufacturing method thereof, and water electrolysis method

A high-entropy composite oxide catalyst with Al, Cr, Fe, Co, Ni, and Mn addresses the overvoltage and stability issues in water electrolysis, enhancing the efficiency and durability of oxygen generating electrodes.

JP2024139228APending Publication Date: 2024-10-09JIKU CHEM CO LTD +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023050075
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing water electrolysis catalysts face challenges in reducing overvoltage and ensuring long-term stability, particularly those using platinum alternatives like transition metal chalcogenides, which often suffer from structural collapse during repeated use.

Method used

A high-entropy composite oxide catalyst containing Al, Cr, Fe, Co, Ni, and Mn is used, which is applied to an electrode base material to form a stable oxygen generating electrode, suppressing overvoltage increase and enhancing durability.

Benefits of technology

The catalyst effectively suppresses overvoltage and maintains stability over a long period, improving the efficiency and durability of water electrolysis, especially in seawater conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139228000002
    Figure 2024139228000002
  • Figure 2024139228000003
    Figure 2024139228000003
  • Figure 2024139228000004
    Figure 2024139228000004
Patent Text Reader

Abstract

To provide a catalyst for a hydrogen generating electrode of water electrolysis capable of suppressing an overvoltage increase during electrolysis and being stably used for a long period of time.SOLUTION: A catalyst for a hydrogen generating electrode of water electrolysis comprises a catalyst on an electrode base material. The catalyst contains a composite oxide. The composite oxide is an oxide containing Al or Cr, Fe, Co, Ni, and Mn. The catalyst for a hydrogen generating electrode of water electrolysis can suppress an overvoltage increase during electrolysis and be stably used for a long period of time.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst for a hydrogen generating electrode in water electrolysis, a catalyst for an oxygen generating electrode in water electrolysis, a method for producing a catalyst for water electrolysis, and a method for electrolyzing water. [Background technology]

[0002] Hydrogen emits zero CO2 when burned, and is expected to be a clean energy source that can replace fossil fuels. In particular, hydrogen production through water electrolysis, which uses renewable energy sources such as solar, wind, and hydroelectric power, does not emit any CO2 whatsoever, and is therefore highly anticipated as a clean method of producing hydrogen.

[0003] As an electrode for electrolysis of water, a platinum particle catalyst is fixed on an electrode substrate such as a carbon substrate. However, platinum is expensive and the amount of resources is limited, so there is a demand for technology to reduce the amount of platinum used and development of platinum alternative catalysts and / or electrodes.

[0004] From this perspective, novel materials such as sulfides or oxides of transition metals (e.g., Co, Ni, Mn, etc.) having nano-sized fine structures have attracted attention as electrodes for water electrolysis, and research into these materials is actively progressing (e.g., Patent Document 1). Although these materials exhibit good activity, the nanostructure often collapses with repeated use, leaving room for improvement in terms of the long-term stability of the electrodes.

[0005] Recently, non-noble metal electrocatalysts, such as transition metal chalcogenides, transition metal carbides, phosphides, phosphorus sulfides, nitrides, borides, and selenides, have been researched as electrocatalysts for water electrolysis, taking advantage of their unique physical and chemical properties. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2000-000470 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in recent years, there has been a strong demand for further improvement in the performance of electrode catalysts in order to increase the efficiency of electrolysis in water electrolysis. From this perspective, there is an urgent need to develop a water electrolysis catalyst that can reduce overpotential and can be used stably for a long period of time.

[0008] The present invention has been made in view of the above, and has an object to provide a catalyst for an oxygen evolving electrode in water electrolysis that can suppress an increase in overvoltage during electrolysis and can be used stably for a long period of time. [Means for solving the problem]

[0009] As a result of extensive research into achieving the above-mentioned objective, the inventors discovered that the above-mentioned objective can be achieved by using a high-entropy complex oxide containing five specific metals as a catalyst, and thus completed the present invention.

[0010] That is, the present invention includes, for example, the subject matter described in the following sections. Item 1 A catalyst is provided on an electrode substrate, The catalyst contains a composite oxide, The composite oxide is Al, Cr or Zn, Fe and Co and Ni, Mn and The catalyst for oxygen evolution electrode in water electrolysis is an oxide containing Section 2 Item 2. The catalyst for an oxygen generating electrode in water electrolysis according to Item 1, wherein the composite oxide is in the form of microsphere particles. Section 3 Item 3. A method for producing a catalyst for an oxygen generating electrode in water electrolysis according to item 1 or 2, The method includes a step of calcining the precursor to obtain a catalyst for an oxygen generating electrode, The precursor is Al, Cr or Zn, Fe and Co and Ni, Mn and The present invention relates to a method for producing a catalyst for an oxygen generating electrode in water electrolysis, comprising the steps of: Section 4 Item 3. A method for electrolyzing water, comprising a step of performing an electrolysis treatment using the oxygen generating catalyst according to item 1 or 2. Effect of the Invention

[0011] The catalyst for oxygen evolution electrode in water electrolysis of the present invention can suppress an increase in overvoltage during water electrolysis and can be used stably for a long period of time. [Brief description of the drawings]

[0012] [Figure 1] 4(a), (b), and (c) are SEM images of the catalyst portion of the oxygen evolution electrode catalyst obtained in the example, and (d) is a TEM image. [Diagram 2] FIG. 1(a) shows the measurement results of linear sweep voltammetry using the oxygen evolution electrode catalysts obtained in Example 1 and Comparative Examples 1 to 3 as electrodes, and FIG. 1(b) shows the Tafel slope calculated from the linear sweep voltammetry curve shown in FIG. [Diagram 3] 1A is a measurement result of linear sweep voltammetry using the oxygen evolution electrode catalyst obtained in Example 1 as an electrode, and FIG. 1B is a bar graph of the overvoltage measured in the measurement of FIG. [Figure 4] 1 shows the results of chronopotentiometry measurement using the oxygen evolution electrode catalyst obtained in Example 1 as an electrode. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "comprise" include the concepts of "containing", "comprises", "consists essentially of" and "consists only of".

[0014] 1. Catalyst for oxygen evolution electrode The present invention relates to a catalyst for an oxygen generating electrode for water electrolysis, which contains a high-entropy complex oxide. The catalyst for an oxygen generating electrode for water electrolysis of the present invention comprises a catalyst on an electrode substrate, and the catalyst contains a complex oxide. In particular, the complex oxide is Al, Cr or Zn, Fe and Co and Ni, Mn and It is an oxide containing

[0015] That is, the composite oxide is any one of the following high entropy oxides. A high-entropy oxide containing Al, Fe, Co, Ni, and Mn. A high-entropy oxide containing Cr, Fe, Co, Ni, and Mn. A high-entropy oxide containing Zn, Fe, Co, Ni, and Mn.

[0016] The composite oxide is a high-entropy catalyst containing five kinds of metals. Hereinafter, in this specification, an oxide containing Al, Cr or Zn, Fe, Co, Ni, and Mn may be referred to as a "high-entropy composite oxide."

[0017] The catalyst for an oxygen generating electrode for water electrolysis of the present invention (hereinafter simply referred to as "catalyst for an oxygen generating electrode") can be used for the electrolysis of water, can suppress an increase in overvoltage in the electrolysis of water, and can be used stably for a long period of time.

[0018] All of the oxygen generating electrode catalysts include an electrode substrate. The type of the electrode substrate is not particularly limited, and may be, for example, any substrate that can be used as an electrode for electrolysis of water. Specific examples of the electrode substrate include various substrates such as metal substrates, carbon substrates, and glass substrates.

[0019] Examples of the metal substrate include substrates of simple metals such as nickel, titanium, iron, and copper, substrates of nickel-phosphorus alloys, nickel-tungsten alloys, and stainless steel alloys, and various metal foams (e.g., nickel foam, copper foam), etc. Among them, nickel foam is preferable as the metal substrate.

[0020] Examples of the carbon substrate include carbon paper, carbon fiber paper, carbon rods, etc. Examples of the glass substrate include conductive glass, etc. The electrode substrate may be, for example, a porous body such as foam.

[0021] More preferably, the electrode substrate is a metal substrate, more preferably a nickel substrate, and most preferably nickel foam.

[0022] The electrode substrate can be obtained, for example, by a known manufacturing method, or can be obtained from a commercial product. The shape and size of the electrode substrate are not particularly limited and can be appropriately selected depending on the purpose of use and the required performance. For example, the shape of the electrode substrate can be foam, sheet, plate, rod, mesh, etc., and is preferably foam.

[0023] The oxygen generating electrode catalyst is a catalyst formed on the electrode substrate. Such a catalyst contains the high entropy complex oxide. As described above, the high entropy complex oxide is an oxide containing Al, Cr or Zn, Fe, Co, Ni, and Mn. That is, the complex oxide is an oxide containing Al, Fe, Co, Ni, and Mn, an oxide containing Cr, Fe, Co, Ni, and Mn, or an oxide containing Zn, Fe, Co, Ni, and Mn.

[0024] The metal elements contained in the high entropy complex oxide may consist only of Al, Fe, Co, Ni, and Mn. The metal elements contained in the high entropy complex oxide may consist only of Cr, Fe, Co, Ni, and Mn. The metal elements contained in the high entropy complex oxide may consist only of Zn, Fe, Co, Ni, and Mn. However, in these cases, the inclusion of other metal elements that may be inevitably contained in the high entropy complex oxide is not excluded, and for example, the inclusion of other metal elements that are inevitably contained in the production process of the catalyst is permitted.

[0025] The high entropy complex oxide is particularly preferably an oxide of Al, Fe, Co, Ni, or Mn. In this case, the oxygen generating electrode catalyst can particularly suppress an increase in overvoltage in the electrolysis of water, and can be used stably for a long period of time.

[0026] The content ratio of each metal element contained in the high entropy complex oxide is not particularly limited. For example, based on Al in the high entropy complex oxide, that is, assuming the number of moles of Al to be 1, each metal element can be contained as follows. That is, Al:Fe=1:1 to 1:4, Al:Co=1:1 to 1:5, Al:Ni=1:1 to 1:5, The Al:Mn ratio can be set to 1:3 to 1:14. Even when Al is replaced with Cr or Zn, the above ratio is the same.

[0027] In the high entropy complex oxide, the content of oxygen (O) is not particularly limited. For example, the content of O is preferably 20 to 40 mol % relative to the total amount of the high entropy complex oxide.

[0028] In the composite oxide, the valences of Al, Cr, Zn, Fe, Co, Ni and Mn are not particularly limited, and each can be divalent or trivalent.

[0029] In the catalyst for oxygen generating electrodes, the catalyst formed on the electrode substrate may consist only of the high-entropy complex oxide, or may contain components other than the high-entropy complex oxide as long as the effects of the present invention are not impaired. In the catalyst for oxygen generating electrodes, the catalyst preferably contains 80 mass% or more of the high-entropy complex oxide, more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 99 mass% or more.

[0030] The shape of the high entropy complex oxide is not particularly limited, and may be, for example, a film, a particle, a wire, a fiber, a needle, a rod, a scale, etc., and among them, the high entropy complex oxide is preferably a microsphere particle. In this case, the oxygen generating electrode catalyst can further suppress the increase in overvoltage in the electrolysis of water and can be used stably for a longer period of time.

[0031] The microsphere particles of the high entropy complex oxide are particles of the micron order, and the average particle size is not particularly limited. The average particle size of the microsphere particles of the high entropy complex oxide is preferably 1 to 10 μm, more preferably 2 to 8 μm, in terms of being able to suppress the increase in overvoltage and being able to be used stably for a longer period of time. The average particle size here refers to the arithmetic average value of the circle equivalent diameters of 50 particles randomly selected by direct observation with a scanning electron microscope and measured.

[0032] The microsphere particles of the high entropy complex oxide may be spherical or irregular in shape. The microsphere particles of the complex oxide may be porous particles. In this case, mass transfer and gas release are easily caused, and catalytic activity is easily increased.

[0033] The porous particles may be, for example, particles with a pleated (or petal-like) surface. In this case, the high-entropy complex oxide has a large surface area, which enhances the catalytic activity and improves the efficiency of water electrolysis. When the microsphere particle surface of the high-entropy complex oxide is pleated, for example, the thickness of the pleated portion is preferably 100 nm or less. Therefore, the microsphere particle may be in the form of a so-called nanoflower, which allows the inner surface to be used as a reaction field, thereby further enhancing the catalytic activity and further improving the efficiency of water electrolysis.

[0034] In the oxygen generating electrode catalyst, the catalyst formed on the electrode substrate can cover a part or the whole of the electrode substrate. The catalyst can be formed directly on the electrode substrate (without other layers, etc.). The catalyst is preferably disposed on the outermost layer of the electrode substrate.

[0035] The oxygen generating electrode catalyst of the present invention can provide excellent oxygen generating efficiency when used as an electrode for electrolysis of water, and specifically can be used as an anode.

[0036] By using the oxygen generating electrode catalyst of the present invention as an anode to electrolyze water, the increase in overvoltage can be further suppressed, the Tafel slope can be lowered, and electrolysis can be performed stably for a longer period of time.

[0037] The oxygen generating electrode catalyst of the present invention can also be used as an electrode for electrolysis of seawater. The seawater may be natural seawater or may be imitation seawater (e.g., an aqueous solution containing 1M KOH and 0.5M NaCl).

[0038] 2. Manufacturing method of catalyst for oxygen evolution electrode The method for producing the catalyst for oxygen generating electrodes of the present invention is not particularly limited, and for example, known production methods can be widely adopted. For example, the catalyst for oxygen generating electrodes of the present invention can be produced using an electrode base material on which a precursor is formed. Specifically, the catalyst for oxygen generating electrodes of the present invention can be produced by a method of calcining the precursor on the electrode base material. The precursor is Al, Cr or Zn, Fe and Co and Ni, Contains Mn.

[0039] In one embodiment, the production method of the present invention can include a step of obtaining an oxygen evolving electrode catalyst by calcining a precursor containing Al, Cr or Zn, Fe, Co, Ni, and Mn.

[0040] The method of forming the precursor on the electrode substrate is not particularly limited, and for example, the precursor can be formed on the electrode substrate by hydrothermal synthesis. In such hydrothermal synthesis, for example, the electrode substrate is heat-treated in an aqueous solution containing an Fe source, a Co source, a Ni source, a Mn source, and an Al source (or a Cr source or a Zn source), thereby forming a precursor on the electrode substrate. The electrode substrate used here is the same as the electrode substrate used in the above-mentioned electrode catalyst, and therefore can include a metal substrate, a carbon substrate, a glass substrate, etc., preferably a metal substrate, more preferably a nickel substrate, and particularly preferably a nickel foam.

[0041] Examples of the Fe source, Co source, Ni source, Mn source, and Al source (or Cr source or Zn source) include compounds of the respective metals, and specifically include inorganic acid salts, organic acid salts, hydroxides, and halides containing the respective metals. More specifically, examples include nitrates of the respective metals. That is, examples of the Fe source, Co source, Ni source, Mn source, and Al source include Fe(NO3)3, Co(NO3)2, Ni(NO3)2, Mn(NO3)2, and Al(NO3)3, respectively. An example of the Cr source is Cr(NO3)3, and an example of the Zn source is Zn(NO3)2Cr, etc.

[0042] The concentration of the aqueous solution containing the Fe source, Co source, Ni source, Mn source and Al source (or Cr source or Zn source) is not particularly limited, and the concentration of each metal can be 1 to 100 mM, more preferably 2 to 80 mM, even more preferably 3 to 70 mM, and particularly preferably 5 to 65 mM per 1 L of solvent. In the aqueous solution, the concentrations of the Fe source, Co source, Ni source, Mn source and Al source (or Cr source or Zn source) may be equal or different. The molar ratio of each metal in the aqueous solution can be considered to be the same as the molar ratio of each metal in the precursor (hydroxide) to be generated.

[0043] The aqueous solution may contain other additives. Examples of the other additives include a pH adjuster. Examples of the pH adjuster include urea (CO(NH2)2), NH4F, ammonium hydroxide, etc. The pH adjuster may be used alone or in combination of two or more. When the aqueous solution contains a pH adjuster, the concentration of the pH adjuster may be, for example, 100 to 500 mM.

[0044] In the hydrothermal synthesis, the method of immersing the electrode substrate in the aqueous solution is not particularly limited, and the electrode substrate can usually be entirely immersed in the aqueous solution. The electrode substrate can be immersed in, for example, a pressure-resistant autoclave. The inner surface of the autoclave can be coated with, for example, a fluororesin such as Teflon (registered trademark).

[0045] In the hydrothermal synthesis, the electrode substrate is immersed in the solution and subjected to a heat treatment. The temperature of the heat treatment is not particularly limited as long as the condition is such that the precursor is formed, and may be, for example, 80 to 200°C, and preferably 100 to 150°C. The time of the heat treatment is also not particularly limited, and may be, for example, 2 to 24 hours. The pressure inside the vessel during the hydrothermal synthesis may also be appropriately set.

[0046] The above-mentioned hydrothermal synthesis forms a precursor on the electrode substrate. Such a precursor is, for example, a composite hydroxide having Fe, Co, Ni, Mn, and Al (Al can be replaced with Cr or Zn). The precursor is calcined on the electrode substrate to produce the above-mentioned composite oxide.

[0047] The firing method is not particularly limited, and for example, a wide variety of known firing methods can be used. For firing, for example, a known heating device such as a commercially available heating furnace can be used.

[0048] The firing temperature can be, for example, 150 to 500° C., preferably 200 to 450° C., and more preferably 250 to 400° C. The firing time is not particularly limited and can be appropriately set depending on the firing temperature. For example, the firing time can be 1.5 to 5 hours.

[0049] The calcination may be performed in air or in an inert gas atmosphere. It is preferable to perform the calcination in an inert gas atmosphere, in which case the overvoltage of the resulting electrode catalyst is easily suppressed. The type of inert gas is not particularly limited, and may be, for example, argon, nitrogen, or the like.

[0050] The above-mentioned calcination treatment converts the precursor on the electrode substrate into a composite oxide, and a high-entropy composite oxide containing Fe, Co, Ni, Mn, and Al can be formed on the electrode substrate. This can be obtained as the oxygen generating electrode catalyst of the present invention.

[0051] 3. Water electrolysis method The method for electrolyzing water of the present invention includes a step of carrying out electrolysis using an oxygen generating electrode catalyst as an electrode.

[0052] In the water electrolysis method of the present invention, the oxygen generating electrode catalyst can be used as an anode, that is, it can generate oxygen.

[0053] In the water electrolysis method of the present invention, the cathode may be any electrode generally used in water electrolysis. For example, any electrode generally used in water electrolysis may be used, such as a carbon rod or a platinum wire.

[0054] The aqueous solution used in the electrolysis of water of the present invention can be alkaline water or seawater. The seawater can be natural seawater, or imitation seawater (e.g., an aqueous solution containing 1M KOH and 0.5M NaCl) can be used as seawater.

[0055] As a specific example of the electrolysis of water according to the present invention, a voltage is applied to an oxygen generating electrode catalyst as the anode, a platinum plate as the cathode, and simulated seawater as the electrolyte. This allows oxygen to be generated at the anode and hydrogen at the cathode. In addition, the hydrogen generation rate can be increased by increasing the applied voltage. The hydrogen produced can be preferably used as fuel for fuel cells, hydrogen engines, and the like.

[0056] In the water electrolysis of the present invention, an oxygen generating electrode catalyst is used as an electrode (anode), so that an increase in overvoltage is unlikely to occur and the Tafel slope can be made low. In addition, since the electrode catalyst has excellent durability, performance degradation is unlikely to occur even with long-term use. EXAMPLES

[0057] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.

[0058] (Preparation Example 1) First, a 2 x 2 cm foamed nickel (nickel foam) was treated with 3M hydrochloric acid for 30 minutes, washed several times with ethanol and deionized water, and then dried in a vacuum oven at 60 °C for 12 hours to pretreat the nickel foam. Meanwhile, an aqueous solution containing Fe(NO3)3, Co(NO3)2, Ni(NO3)2, Mn(NO3)2, and Al(NO3)3 was prepared, and urea and NH4F were added to this aqueous solution and mixed under magnetic stirring to obtain a uniform solution. The solution had a concentration of 10 mM Fe(NO3)3, 20 mM Co(NO3)2, 20 mM Ni(NO3)2, 60 mM Mn(NO3)2, and 10 mM Al(NO3)3, as well as 200 mM urea and 400 mM NH4F. The entire amount of this solution was transferred to a 50 mL capacity autoclave lined with Teflon (registered trademark), the above-mentioned pretreated nickel foam was immersed therein, and the container was sealed. The inside of the container was then heated at 140°C for 16 hours (hydrothermal synthesis). After that, it was allowed to cool naturally, and the nickel foam was removed, washed with ethanol and deionized water, and dried in a vacuum oven at 60°C for 12 hours. As a result, a precursor made of a composite hydroxide (hereinafter referred to as a precursor-coated electrode substrate) was formed on the electrode substrate.

[0059] (Preparation Example 2) First, nickel foam (nickel foam) with a size of 2 x 2 cm was treated with 3M hydrochloric acid for 30 minutes, washed several times with ethanol and deionized water, and then dried in a vacuum oven at 60 ° C for 12 hours to pretreat the nickel foam. Meanwhile, an aqueous solution in which Fe (NO3)3, Co (NO3)2, and Ni (NO3)2 were dissolved was prepared, and urea and NH4F were added to this aqueous solution and mixed under magnetic stirring to obtain a uniform solution. The solution had a concentration of 10 mM Fe (NO3)3, 20 mM Co (NO3)2, 20 mM Ni (NO3)2, 200 mM urea, and 400 mM NH4F. The entire amount of this solution was transferred to a 50 mL autoclave lined with Teflon (registered trademark), and the pretreated nickel foam was immersed therein, and the container was sealed. Then, the inside of the container was heated at 140 ° C for 16 hours (hydrothermal synthesis). After that, it was allowed to cool naturally, and the nickel foam was taken out, washed with ethanol and deionized water, and dried for 12 hours in a vacuum oven at 60° C. As a result, a precursor made of a composite hydroxide (precursor-coated electrode substrate) was formed on the electrode substrate.

[0060] (Preparation Example 3) First, nickel foam (nickel foam) with a size of 2 x 2 cm was treated with 3M hydrochloric acid for 30 minutes, then washed several times with ethanol and deionized water, and then dried in a vacuum oven at 60 ° C for 12 hours to pretreat the nickel foam. Meanwhile, an aqueous solution in which Fe(NO3)3, Co(NO3)2, Ni(NO3)2, and Mn(NO3)2 were dissolved was prepared, and urea and NH4F were added to this aqueous solution and mixed under magnetic stirring to obtain a uniform solution. The solution had a concentration of 10 mM Fe(NO3)3, 20 mM Co(NO3)2, 20 mM Ni(NO3)2, 60 mM Mn(NO3)2, 200 mM urea, and 400 mM NH4F. The entire amount of this solution was transferred to a 50 mL capacity autoclave lined with Teflon (registered trademark), and the pretreated nickel foam was immersed therein, and the container was sealed. The inside of the container was then heated at 140°C for 16 hours (hydrothermal synthesis). After that, it was allowed to cool naturally, and the nickel foam was removed, washed with ethanol and deionized water, and dried in a vacuum oven at 60°C for 12 hours. As a result, a precursor made of a composite hydroxide (precursor-coated electrode substrate) was formed on the electrode substrate.

[0061] (Preparation Example 4) First, nickel foam (nickel foam) with a size of 2 x 2 cm was treated with 3M hydrochloric acid for 30 minutes, then washed several times with ethanol and deionized water, and then dried in a vacuum oven at 60 ° C for 12 hours to pretreat the nickel foam. Meanwhile, an aqueous solution in which Fe(NO3)3, Co(NO3)2, Ni(NO3)2, and Al(NO3)3 were dissolved was prepared, and urea and NH4F were added to this aqueous solution and mixed under magnetic stirring to obtain a uniform solution. The solution had a concentration of 10 mM Fe(NO3)3, 20 mM Co(NO3)2, 20 mM Ni(NO3)2, 10 mM Al(NO3)3, 200 mM urea, and 400 mM NH4F. The entire amount of this solution was transferred to a 50 mL capacity autoclave lined with Teflon (registered trademark), and the pretreated nickel foam was immersed therein, and the container was sealed. The inside of the container was then heated at 140°C for 16 hours (hydrothermal synthesis). After that, it was allowed to cool naturally, and the nickel foam was removed, washed with ethanol and deionized water, and dried in a vacuum oven at 60°C for 12 hours. As a result, a precursor made of a composite hydroxide (precursor-coated electrode substrate) was formed on the electrode substrate.

[0062] (Example 1: Synthesis of Complex Oxide) The precursor-coated electrode substrate obtained in Preparation Example 1 was calcined in air at 350°C for 2 hours in a muffle furnace. This calcination process oxidized the precursor, and a high-entropy composite oxide containing Fe, Co, Ni, Mn, and Al was formed as a catalyst on the electrode substrate (nickel foam), which was obtained as a catalyst for oxygen generating electrodes for water electrolysis. This water electrolysis catalyst was designated as "FeCoNiMnAlO / NF".

[0063] Comparative Example 1 A water electrolysis catalyst in which a composite oxide containing Fe, Co, and Ni was formed as a catalyst was obtained in the same manner as in Example 1, except that the precursor-coated electrode base material obtained in Preparation Example 1 was changed to the precursor-coated electrode base material obtained in Preparation Example 2. This water electrolysis catalyst was designated "FeCoNiO / NF".

[0064] Comparative Example 2 A water electrolysis catalyst in which a composite oxide containing Fe, Co, Ni, and Mn was formed as a catalyst was obtained in the same manner as in Example 1, except that the precursor-coated electrode base material obtained in Preparation Example 1 was changed to the precursor-coated electrode base material obtained in Preparation Example 3. This water electrolysis catalyst was designated "FeCoNiMnO / NF".

[0065] Comparative Example 3 A water electrolysis catalyst in which a composite oxide containing Fe, Co, Ni, and Al was formed as a catalyst was obtained in the same manner as in Example 1, except that the precursor-coated electrode base material obtained in Preparation Example 1 was changed to the precursor-coated electrode base material obtained in Preparation Example 4. This water electrolysis catalyst was designated "FeCoNiAlO / NF".

[0066] (Evaluation Results) 1(a), (b) and (c) are SEM images of the catalyst portion of the oxygen evolution electrode catalyst obtained in Example 1, and (d) is a TEM image.

[0067] From the SEM image in FIG. 1, it was confirmed that the catalyst in the oxygen evolution electrode catalyst obtained in Example 1 was formed as microsphere particles on the electrode substrate, specifically, had a porous particle, more specifically, a nanoflower-like form, and formed stacking (FIGS. 1(a) and (b)). The microsphere particles had an average particle size of about 4.8 μm (FIG. 1(c)). In addition, from the TEM image in FIG. 2(d), it was also found that the microsphere particles had nanoholes, and it was expected that the nanoflowers would provide more electroactive sites for the catalytic reaction and accelerate the mass transfer.

[0068] From the above, it was found that the oxygen evolution electrode catalyst obtained in Example 1 was formed of microsphere particles made of a composite oxide of Fe, Co, Ni, Mn, and Al.

[0069] 2(a) shows the results of linear sweep voltammetry measurements using the oxygen evolving electrode catalysts obtained in Example 1 and Comparative Examples 1 to 3 as electrodes. In this measurement, the oxygen evolving electrode catalyst obtained in Example 1 was used as the anode, and an Ag / AgCl electrode was used as the reference electrode. The electrolyte used in the measurement was a 1 M KOH aqueous solution. The scan rate was 2 mV / s, and the current density was 50 or 100 mAcm. -2 The evaluation of electrical properties such as linear sweep voltammetry curves was performed using a VersaSTAT4 potentiostat galvanostat electrochemical workstation (USA) together with a standard three-electrode cell.

[0070] FIG. 2(b) shows the Tafel slope calculated from the linear sweep voltammetry curve shown in (a).

[0071] Table 1 summarizes the results of Figure 2. -2 and 100mAcm -2 The values ​​of the overpotential at 1000 .mu.m and the Tafel slope are shown.

[0072] [Table 1]

[0073] From FIG. 2 and Table 1, it was found that the oxygen evolution electrode catalyst obtained in Example 1 can suppress an increase in overvoltage and reduce the Tafel slope in the electrolysis of water.

[0074] Fig. 3(a) shows the measurement results of linear sweep voltammetry using the oxygen evolution electrode catalyst obtained in Example 1 as an electrode. Three types of electrolytes were used in the measurement: 1M KOH aqueous solution, alkaline simulated seawater (a mixture of 1MKOH and 0.5M NaCl aqueous solutions), and alkaline natural seawater (a mixture of 1MKOH and seawater). The other measurement conditions were the same as in Fig. 2(a).

[0075] Figure 3(b) shows a bar graph of the overpotential in each electrolyte measured in the measurement of Figure 3(a). For each electrolyte, the left and right bars show the overpotential at 50 mAcm -2 and 100mAcm -2 This shows the overvoltage at

[0076] 3(a) and (b) show that the increase in overvoltage is suppressed when any of the electrolytes, 1M KOH aqueous solution, alkaline simulated seawater, and alkaline natural seawater, is used. Therefore, it can be said that the oxygen evolution electrode catalyst obtained in Example 1 has excellent catalytic performance for various electrolytes.

[0077] FIG. 4 shows the results of chronopotentiometry using the oxygen evolution electrode catalyst obtained in Example 1 as an electrode. In this measurement, the current density was set at 500 mA / cm 2 The electrolytes used were the aforementioned 1M KOH aqueous solution, alkaline simulated seawater, and alkaline natural seawater (top, middle, and bottom rows in Fig. 4, respectively). The measurements were performed using a two-electrode cell and a VersaSTAT4 potentiostat galvanostat electrochemical workstation (USA).

[0078] 4, the oxygen generating electrode catalyst obtained in Example 1 exhibited excellent stability for more than 50 hours. Therefore, it was demonstrated that the oxygen generating electrode catalyst obtained in Example 1 can be operated stably for a long period of time even at a high current density.

[0079] From the above results, the oxygen evolution electrode catalyst obtained in Example 1 was able to suppress an increase in overvoltage during electrolysis, reduce the Tafel slope, and be used stably for a long period of time. Furthermore, it was able to efficiently split water not only in alkaline solutions, but also in alkaline simulated seawater and alkaline natural seawater, and is promising for application to industrial seawater electrolysis.

Claims

1. A catalyst is provided on an electrode substrate, The catalyst contains a composite oxide, The composite oxide is Al, Cr or Zn, Fe, Co., Ni, Mn and The catalyst for oxygen evolution electrode in water electrolysis is an oxide containing

2. The catalyst for an oxygen generating electrode in water electrolysis according to claim 1 , wherein the composite oxide is in the form of microsphere particles.

3. A method for producing the catalyst for an oxygen evolution electrode in water electrolysis according to claim 1 or 2, comprising the steps of: The method includes a step of calcining the precursor to obtain a catalyst for an oxygen generating electrode, The precursor is Al, Cr or Zn; Fe, Co., Ni, Mn and The present invention relates to a method for producing a catalyst for an oxygen generating electrode in water electrolysis, comprising the steps of:

4. A method for electrolyzing water, comprising a step of carrying out an electrolysis treatment using the oxygen generating catalyst according to claim 1 or 2.

Citation Information

Patent Citations

  • Perovskite oxide catalyst for oxygen evolution reaction

    JP2016221471A

  • Electrode catalyst and production method thereof

    JP2020070450A

  • Electrode catalyst, method for producing the same, and method for producing hydrogen

    JP2021070864A

  • Hydrogenation catalyst and method for hydrogenating heavy oil

    JP2000000470A