Composite and catalyst layer

The composite structure with ionomer-coated substrate and catalyst particles addresses the trade-off in proton resistance and gas diffusion resistance, improving fuel cell performance by shortening proton conduction paths and maintaining porosity, thus enhancing power generation across different environmental conditions.

JP2024165981APending Publication Date: 2024-11-28KK TOYOTA CHUO KENKYUSHO

Patent Information

Application Number
JP2023082631
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing catalyst layers in polymer electrolyte fuel cells face a trade-off between high proton resistance under high temperature, low humidity conditions and low gas diffusion resistance under low temperature, high humidity conditions, leading to reduced power generation performance due to long-distance proton conduction through high-resistance paths.

Method used

A composite structure is developed where the surface of substrate particles is coated with ionomer A, and the electrode catalyst is coated with ionomer B, forming a thin and uniform ionomer/catalyst composite, reducing the distance of proton conduction paths by heat-treating the ionomer/substrate composite to make it insoluble, and evaporating the dispersion medium.

Benefits of technology

This structure suppresses performance degradation by shortening proton conduction paths, enhancing power generation performance across varying temperature and humidity conditions by reducing proton resistance and maintaining porosity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165981000001_ABST
    Figure 2024165981000001_ABST
Patent Text Reader

Abstract

To provide a composite capable of suppressing a decrease in performance caused by protons moving long distances through a proton conduction path having high proton resistance, and a catalyst layer including the composite.SOLUTION: A composite includes an ionomer / substrate composite in which the surface of a substrate particle is coated with ionomer A, and an ionomer / catalyst composite in which the surface of an electrode catalyst is coated with ionomer B. The electrode catalyst includes a carrier and catalyst particles supported on the surface of the carrier. The surface of the ionomer / substrate composite is coated with the ionomer / catalyst composite. The catalyst layer includes such a composite.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite and a catalyst layer, and more particularly to a composite including an ionomer / substrate composite and an ionomer / catalyst composite, and a catalyst layer provided with the same. [Background technology]

[0002] A polymer electrolyte fuel cell is equipped with a membrane electrode assembly (MEA) in which catalyst layers are bonded to both sides of an electrolyte membrane. The catalyst layer is the reaction field for the electrode reaction, and is generally made of a composite of carbon carrying catalyst particles such as platinum and a solid polymer electrolyte (catalyst layer ionomer). Usually, a gas diffusion layer is further disposed on the outside of the catalyst layer. The gas diffusion layer is used to supply reactant gases and electrons to the catalyst layer, and is made of carbon paper, carbon cloth, or the like. Furthermore, a separator having a gas flow path is disposed on the outer side of the gas diffusion layer. A polymer electrolyte fuel cell generally has a structure (stack structure) in which a plurality of unit cells each having such an MEA, a gas diffusion layer, and a separator are stacked.

[0003] Polymer electrolyte fuel cells are required to show high power generation performance in a wide range of temperature and humidity environments, from low temperature and high humidity conditions to high temperature and low humidity conditions. To achieve both of these performances, it is necessary to improve the catalyst layer where the reaction occurs. To improve power generation performance under high temperature and low humidity conditions, it is necessary to lower the proton resistance and reduce IR loss. In addition, to improve power generation performance under low temperature and high humidity conditions, it is possible to reduce gas diffusion resistance by increasing the porosity of the catalyst layer and improving the water discharge performance. However, these properties have a trade-off relationship: for example, if the volume fraction of the ionomer is increased, the proton resistance can be reduced, but the porosity decreases accordingly.

[0004] In order to solve this problem, various proposals have been made in the past. For example, Patent Document 1 states: An ionomer-coated catalyst is produced in which the surface of an electrode catalyst is coated with a first ionomer; Producing an ionomer / substrate composite in which the surface of a substrate particle is coated with a second ionomer; Using a dry coating method, a mixture of the ionomer coat catalyst and the ionomer / substrate composite is applied to the surface of the substrate. The catalyst layer obtained by the above process is disclosed.

[0005] The document describes that when a catalyst layer is produced using such a method, if the ionomer ratio (I1 / C1) of the ionomer-coated catalyst is made smaller than the ionomer ratio (I2 / C2) of the ionomer / substrate composite, a catalyst layer that exhibits high performance under both high-temperature, low-humidity conditions and low-temperature, high-humidity conditions can be obtained.

[0006] In Patent Document 2, Sheet-like core particles; an electrolyte polymer that coats the surface of the core particle; Equipped with The diameter D1 is 1 μm or more and 50 μm or less, Thickness t1 is less than D1 x 0.5 Sheet-like particle composites are disclosed.

[0007] The same document states: (A) when a dispersion containing sheet-like core particles and an electrolyte polymer is whipped, the whipped dispersion is freeze-dried, and the freeze-dried product is pulverized, a sheet-like particle complex is obtained in which the core particles are coated with the electrolyte polymer while maintaining their sheet shape; and (B) When such a sheet-like particle composite is added to a catalyst layer, the proton conductivity of the catalyst layer is improved. is stated.

[0008] In Patent Document 3, a nonwoven fabric comprising an assembly of fibers containing a proton conductor; The electrode catalyst attached to the surface of the fiber A catalyst layer comprising:

[0009] The same document states: (A) When the deposition of fibers containing a proton conductor on the surface of the substrate and the spraying of a catalytic ink containing an electrode catalyst on the surface of the fibers are performed simultaneously, the voids in the nonwoven fabric are maintained and the probability of occurrence of isolated catalyst particles in the nonwoven fabric is reduced; and (B) This increases the electrochemically effective surface area (ECSA) of the catalyst particles. is stated.

[0010] As described in Patent Document 1, when a mixture of an ionomer-coated catalyst with a low ionomer ratio (I1 / C1) and an ionomer / substrate composite with a high ionomer ratio (I2 / C2) is dry-coated, a catalyst layer that exhibits high performance under both high-temperature, low-humidity conditions and low-temperature, high-humidity conditions is obtained.

[0011] However, when a mixture of the ionomer-coated catalyst and the ionomer / substrate composite is dry-coated on the surface of a substrate, a part of the electrode catalyst is located at a position distant from the ionomer / substrate composite. Protons are supplied to the electrode catalyst located at a position distant from the ionomer / substrate composite via the ionomer contained in the ionomer-coated catalyst, but the ionomer-coated catalyst has a higher proton resistance than the ionomer / substrate composite. As a result, protons supplied to an electrode catalyst located away from the ionomer / substrate composite must travel a long distance through the ionomer-coated catalyst, which has high proton resistance, causing a decrease in the power generation performance of the fuel cell. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] JP 2022-181252 A [Patent Document 2] JP 2022-143571 A [Patent Document 3] Patent Publication No. 2021-068638 Summary of the Invention [Problem to be solved by the invention]

[0013] An object of the present invention is to provide a composite capable of suppressing the deterioration of performance caused by the long-distance migration of protons through a proton conduction path having high proton resistance. Another object of the present invention is to provide a catalyst layer including such a composite. [Means for solving the problem]

[0014] In order to solve the above problems, the composite of the present invention comprises: an ionomer / substrate composite in which the surface of a substrate particle is coated with ionomer A; The surface of the electrode catalyst is coated with ionomer B to produce an ionomer / catalyst composite. Equipped with The electrode catalyst comprises a support and catalyst particles supported on a surface of the support, The surface of the ionomer / substrate composite is coated with the ionomer / catalyst composite.

[0015] The catalyst layer according to the present invention comprises the composite according to the present invention. Effect of the Invention

[0016] The complex according to the present invention comprises (a) preparing an ionomer / substrate composite in which the surface of a substrate particle is coated with ionomer A; (b) heat-treating the ionomer / substrate composite to make the ionomer A insoluble in the solvent; (c) A dispersion liquid containing the insolubilized ionomer / substrate composite, an electrode catalyst, and ionomer B is prepared, and the dispersion medium is volatilized. This is obtained by:

[0017] The composite obtained in this manner has a structure in which all or part of the surface of the ionomer / substrate composite is thinly and uniformly covered with fine (less aggregated) ionomer / catalyst composite. Therefore, the distance of the proton conduction path from the ionomer / substrate composite to the electrode catalyst is shorter than when a pre-produced ionomer / substrate composite and an ionomer / catalyst composite are mixed. As a result, it is possible to suppress the performance degradation caused by protons moving long distances through a proton conduction path with high proton resistance. [Brief description of the drawings]

[0018] [Figure 1] 1 is a schematic diagram of a dry deposition catalyst layer obtained by the method according to the present invention and a conventional method. [Diagram 2] 1 is an SEM photograph of the composite (Naf / Pt / C / Naf / GNS) obtained in Example 1. [Diagram 3] 1 is an SEM photograph of the composite (HOPI / Pt / C / Naf / GNS) obtained in Example 2.

[0019] [Figure 4] 1 is a SEM photograph of the mixed powder (Naf / Pt / C+Naf / GNS_Mix) obtained in Comparative Example 1. [Diagram 5] 1 is a SEM photograph of the mixed powder (HOPI / Pt / C+Naf / GNS_Mix) obtained in Comparative Example 2.

[0020] [Figure 6] 1 shows the current density at 0.6 V (IR corrected voltage) at 82° C. and 30% RH for the cells obtained in Example 1, Comparative Example 1, and Comparative Example 3. [Figure 7] 1 shows the proton resistance of the catalyst layer at 82° C. and 30% RH for the cells obtained in Example 1, Comparative Example 1, and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] [Configuration 1] an ionomer / substrate composite in which the surface of a substrate particle is coated with ionomer A; The surface of the electrode catalyst is coated with ionomer B to produce an ionomer / catalyst composite. Equipped with The electrode catalyst comprises a support and catalyst particles supported on a surface of the support, The surface of the ionomer / substrate composite is coated with the ionomer / catalyst composite. Complex.

[0022] [Configuration 2] 2. The composite of claim 1, wherein the substrate particle comprises a graphite nanosheet.

[0023] [Configuration 3] The ionomer A includes a perfluorocarbon sulfonic acid polymer, The ionomer B includes a perfluorocarbon sulfonic acid polymer and / or a highly oxygen permeable ionomer. 3. The complex according to claim 1 or 2.

[0024] [Configuration 4] The ionomer / substrate composite according to any one of configurations 1 to 3, wherein the ionomer / substrate composite satisfies the following formula (1): 0.5≦I1 / S1≦10.0 …(1) however, I1 is the mass of the ionomer A, S1 is the mass of the substrate.

[0025] [Configuration 5] The ionomer / catalyst composite according to any one of configurations 1 to 4, wherein the ionomer / catalyst composite satisfies the following formula (2): 0.1≦I2 / S2≦1.2 …(2) however, I2 is the mass of the ionomer B, S2 is the mass of the support.

[0026] [Configuration 6] A complex according to any one of configurations 1 to 5, which satisfies the following formula (3): 0.01≦t2 / t1≦3.0 …(3) however, t1 is the thickness of the ionomer / substrate composite; t2 is the thickness of the ionomer / catalyst composite covering the surface of the ionomer / substrate composite.

[0027] [Configuration 7] A composite according to any one of configurations 1 to 6, which satisfies the following formula (4): 0.1≦W2 / W1≦10.0 …(4) however, W1 is the mass of the ionomer / substrate composite; W2 is the mass of the ionomer / catalyst composite coating the surface of the ionomer / substrate composite.

[0028] [Configuration 8] A composite according to any one of configurations 1 to 7, which satisfies the following formulas (5) and (6): 1μm≦D1≦50μm …(5) 0.001≦t2 / D1≦3.0 …(6) however, D1 is the maximum length of the ionomer / substrate composite; t2 is the thickness of the ionomer / catalyst composite covering the surface of the ionomer / substrate composite.

[0029] [Configuration 9] A composite according to any one of configurations 1 to 8, which satisfies the following formula (7): 0.3≦A2 / A1≦1.0 …(7) however, A1 is the total surface area of ​​the ionomer / substrate composite; A2 is the area of ​​the ionomer / catalyst composite covering the surface of the ionomer / substrate composite.

[0030] [Configuration 10] A catalyst layer comprising a composite according to any one of configurations 1 to 9.

[0031] An embodiment of the present invention will be described in detail below. [1. Complex] The complex according to the present invention comprises an ionomer / substrate composite in which the surface of a substrate particle is coated with ionomer A; The surface of the electrode catalyst is coated with ionomer B to produce an ionomer / catalyst composite. It is equipped with:

[0032] [1.1. Ionomer / substrate composite] The ionomer / substrate composite is A substrate particle; Ionomer A that coats the surface of the base particle; It is equipped with:

[0033] [1.1.1. Base material particles] [A. Materials] When a catalyst layer is produced using the composite according to the present invention, the ionomer / substrate composite functions as a proton conductive material in the catalyst layer. Therefore, the material of the substrate particles is not particularly limited as long as it does not inhibit proton conduction. The material of the substrate particles may be a conductive material or an insulating material.

[0034] The base particle is preferably a sheet-like particle. The term "sheet-like particle" refers to a plate-like or thin plate-like particle whose dimensions in the x-axis direction and y-axis direction (in-plane directions of the plate) are greater than its dimension in the z-axis direction (thickness direction of the plate). When an ionomer / substrate composite is used as a proton conductive material, it becomes possible to control the amount of voids introduced into the catalyst layer over a relatively wide range depending on the shape of the substrate particles. In particular, when sheet-shaped particles are used as the substrate particles, it becomes possible to improve the proton conductivity in a specific direction (for example, the thickness direction of the catalyst layer).

[0035] Examples of the sheet-like base particles include: (a) Sheet-like particles made of conductive materials such as graphene sheets, graphite nanosheets, and conductive metal oxide nanosheets; (b) Sheet-like particles made of insulating materials such as mica, boron nitride, and silicates; etc. The base particle may consist of any one of these, or may consist of two or more of these.

[0036] Among these, the base particle is preferably a graphene sheet and / or a graphite nanosheet. The base particle is particularly preferably a graphite nanosheet. Here, the term "graphite nanosheet" refers to a sheet-like particle obtained by cleaving graphite and having a thickness on the order of nanometers. When a graphene sheet and / or a graphite nanosheet is used as a substrate particle, high performance is exhibited under both low temperature and high humidity conditions and high temperature and low humidity conditions. This is believed to be because the use of a graphene sheet and / or a graphite nanosheet as a substrate introduces a relatively large amount of voids into the catalyst layer.

[0037] [B. Average particle size] The "average particle size of the base material particles" refers to the median diameter (D 50 ) The average particle size of the base particles is not particularly limited, and an optimal particle size can be selected according to the purpose. In general, if the average particle size of the base particles is too small, the connection between the particles becomes poor, and the proton resistance may become large. Therefore, the average particle size is preferably 0.1 μm or more. The average particle size is more preferably 0.5 μm or more, or 1.0 μm or more. On the other hand, if the average particle size of the base material particles is too large, the uniformity of the catalyst layer is lost, and in some cases, the electrolyte membrane may be damaged when pressed. Therefore, the average particle size is preferably 50 μm or less. The average particle size is more preferably 30 μm or less, 20 μm or less, 10 μm or less, or 5 μm or less.

[0038] [1.1.2. Ionomer A] [A. Materials] The surface of the substrate particle is coated with ionomer A. The ionomer / substrate composite is (a) A case in which the surface of one base particle is coated with ionomer A, and (b) A single ionomer / substrate composite is formed by coating multiple substrate particles with ionomer A. There is.

[0039] In the present invention, the material of the ionomer A is not particularly limited. Examples of the material for ionomer A include: (a) perfluorocarbon sulfonic acid polymers such as Nafion®, Flemion®, Aciplex®, and Aquivion®; (b) High Oxygen Permeable Ionomer (HOPI) The details of highly oxygen-permeable ionomers will be described later. Ionomer A may consist of any one of these, or may be a mixture of two or more of them.

[0040] A perfluorocarbon sulfonic acid polymer is particularly preferred as the ionomer A. Since a perfluorocarbon sulfonic acid polymer has high proton conductivity, the use of this as the ionomer A makes it possible to obtain an ionomer / substrate composite exhibiting high proton conductivity.

[0041] [B. Ionomer ratio (I1 / S1)] The ionomer / substrate composite preferably satisfies the following formula (1). 0.5≦I1 / S1≦10.0 …(1) however, I1 is the mass of the ionomer A, S1 is the mass of the substrate.

[0042] In formula (1), "I1 / S1" represents the ionomer ratio, that is, the ratio of the mass of ionomer A (I1) to the mass of the base particle (S1). When a catalyst layer is produced using the composite according to the present invention, ionomer A mainly plays a role of transporting protons in the thickness direction of the catalyst layer. In order to obtain high power generation performance in a wide range of temperature and humidity conditions, from low temperature and high humidity conditions to high temperature and low humidity conditions, it is preferable that I1 / S1 satisfies a predetermined condition.

[0043] Proton conduction in the thickness direction of the catalyst layer is mainly carried out by ionomer A. In order to reduce the proton resistance in the thickness direction of the catalyst layer, I1 / S1 is preferably 0.5 or more. I1 / S1 is more preferably 1.0 or more, or 2.0 or more. On the other hand, even if I1 / S1 is made larger than necessary, there is no difference in the effect and no practical benefit. Therefore, I1 / S1 is preferably 10.0 or less. I1 / S1 is more preferably 7.5 or less, or 5.0 or less.

[0044] [C. Ion exchange capacity] In the present invention, the ion exchange capacity of the ionomer A is not particularly limited. In the case of producing a catalyst layer using the composite according to the present invention, in order to suppress flooding, it is preferable that the ion exchange capacity of ionomer A is larger than the ion exchange capacity of ionomer B that covers the periphery of the electrode catalyst. This point will be described later.

[0045] [1.2. Ionomer / catalyst complex] The ionomer / catalyst complex is An electrode catalyst; Ionomer B that coats the surface of the electrode catalyst It is equipped with:

[0046] In addition, the electrode catalyst is A carrier; Catalyst particles supported on the surface of the support; It is equipped with:

[0047] 1.2.1. Carrier [A. Materials] The material of the support is not particularly limited as long as it is conductive and can be used in a fuel cell environment.

[0048] Examples of the carrier include: (a) carbon black, (b) Porous carbon such as mesoporous carbon; (c) SnO2, nonstoichiometric titanium dioxide (TiO x Conductive oxide particles made of conductive metal oxides or composite metal oxides such as etc. The carrier may be any one of these, or a combination of two or more of them.

[0049] [B. Average particle size] The "average particle size of the carrier" is the median diameter (D 50 ) The average particle size of the carrier is not particularly limited, and an optimal particle size can be selected according to the purpose. In general, if the average particle size of the carrier is too small, the connection between the particles becomes poor, and the electronic resistance may become large. Therefore, the average particle size is preferably 0.1 μm or more. The average particle size is more preferably 0.3 μm or more, or 0.5 μm or more. On the other hand, if the average particle size of the carrier becomes too large, the uniformity of the catalyst layer is lost, and in some cases, the electrolyte membrane may be damaged when pressed. Therefore, the average particle size is preferably 20 μm or less. The average particle size is more preferably 10 μm or less, or 5 μm or less.

[0050] [1.2.2. Catalyst particles] [A. Materials] In the present invention, the material of the catalyst particles is not particularly limited as long as it has activity in the hydrogen oxidation reaction or the oxygen reduction reaction. Examples of materials for the catalyst particles include: (a) Precious metals (Pt, Au, Ag, Pd, Rh, Ir, Ru, Os), (b) An alloy containing two or more precious metal elements; (c) Alloys containing one or more precious metal elements and one or more base metal elements (e.g., Fe, Co, Ni, Cr, V, Ti, etc.); etc.

[0051] Among these, the catalyst particles are preferably made of Pt or a Pt alloy, since they have high activity in the electrode reaction of the fuel cell. Examples of Pt alloys include Pt-Fe alloys, Pt-Co alloys, Pt-Ni alloys, Pt-Pd alloys, Pt-Cr alloys, Pt-V alloys, Pt-Ti alloys, Pt-Ru alloys, and Pt-Ir alloys.

[0052] [B. Average particle size] "Average particle size of catalyst particles" refers to the average maximum dimension of catalyst particles measured under a microscope for 20 or more randomly selected catalyst particles. The average particle size of the catalyst particles is not particularly limited, and the most suitable average particle size can be selected according to the purpose. In general, if the average particle size of the catalyst particles is too small, the catalyst particles tend to dissolve. Therefore, the average particle size is preferably 1 nm or more. On the other hand, if the average particle size of the catalyst particles is too large, the mass activity decreases. Therefore, the average particle size of the catalyst particles is preferably 20 nm or less. The average particle size is preferably 10 nm or less, and more preferably 5 nm or less.

[0053] [C. Loading amount] The term "catalyst particle loading amount" refers to the ratio of the mass of the catalyst particles to the total mass of the electrode catalyst. The amount of catalyst particles supported is not particularly limited, and an optimal amount can be selected depending on the purpose. In general, if the amount of catalyst particles supported is too small, the thickness of the catalyst layer required to obtain a specified basis weight becomes large, and the electronic resistance, proton resistance, and / or gas diffusion resistance of the catalyst layer increases. Therefore, the amount of catalyst particles supported is preferably 5 mass% or more. The amount is more preferably 10 mass% or more, or 15 mass% or more. On the other hand, if the amount of catalyst particles supported is excessive, the catalyst particles will aggregate on the support surface, and the activity of the electrode catalyst will decrease. Therefore, the amount of catalyst particles supported is preferably 60 mass% or less. The amount is more preferably 50 mass% or less, or 40 mass% or less.

[0054] [1.2.3. Ionomer B] [A. Materials] The surface of the electrocatalyst is coated with ionomer B. The ionomer / catalyst composite is (a) The surface of one electrode catalyst is covered with ionomer B. (b) Multiple electrode catalysts are coated with ionomer B to form a single ionomer / catalyst composite. There is. Ionomer B may coat only the surface of the support, or may coat the surface of the support and the surface of the catalyst particles. In order to reduce poisoning of the catalyst particles by ionomer B, it is preferable that ionomer B coats only the surface of the support.

[0055] In the present invention, the material of ionomer B is not particularly limited. Examples of the material for ionomer B include: (a) perfluorocarbon sulfonic acid polymers such as Nafion®, Flemion®, Aciplex®, and Aquivion®; (b) High Oxygen Permeable Ionomer (HOPI) etc.

[0056] Ionomer B may consist of any one of these, or may consist of two or more of them. When ionomer B contains two or more types of ionomers, ionomer B may be a mixture of two or more types of ionomers, or may be a laminate film of two or more types of ionomers. For example, ionomer B may be a laminated membrane having a first layer made of a highly oxygen-permeable ionomer formed on the surface of the electrode catalyst and a second layer made of a perfluorocarbon sulfonic acid polymer formed on the surface of the first layer.

[0057] Here, the term "highly oxygen-permeable ionomer" refers to a polymeric compound that contains an acid group and a cyclic structure in its molecular structure. The highly oxygen-permeable ionomer has a high oxygen permeability coefficient because it contains a cyclic structure in its molecular structure. Therefore, when this ionomer is used as ionomer B, the oxygen transfer resistance at the interface with the catalyst particles becomes relatively small. In other words, the "highly oxygen-permeable ionomer" refers to an ionomer having an oxygen permeability coefficient higher than that of perfluorocarbon sulfonic acid polymers such as Nafion (registered trademark).

[0058] In general, the power generation performance of a fuel cell in the high current density region is determined by the diffusion of oxygen to the catalyst particle surface. By contrast, coating the surface of the catalyst particle with a highly oxygen-permeable ionomer improves the oxygen permeability of the catalyst layer, thereby improving the performance of the fuel cell. The molecular structure of the highly oxygen-permeable ionomer is not particularly limited as long as it exhibits a relatively small oxygen transfer resistance. In particular, ionomers containing a cyclic structure (aliphatic cyclic structure) in their molecular structure have a smaller oxygen transfer resistance than ionomers that do not contain a cyclic structure, and are therefore suitable as polymers for coating electrode catalysts.

[0059] Examples of highly oxygen-permeable ionomers include: (a) an electrolyte polymer including a perfluorocarbon unit having an aliphatic ring structure and an acid group unit having a perfluorosulfonic acid in a side chain; (b) an electrolyte polymer including a perfluorocarbon unit having an aliphatic ring structure and an acid group unit having a perfluoroimide in a side chain; (c) an electrolyte polymer containing a unit in which perfluorosulfonic acid is directly bonded to a perfluorocarbon having an aliphatic ring structure; etc. (See References 1 to 4). [Reference 1] JP 2003-036856 A [Reference 2] International Publication No. 2012 / 088166 [Reference 3] JP 2013-216811 A [Reference 4] JP 2006-152249 A

[0060] [B. Ionomer ratio (I2 / S2)] The ionomer / catalyst composite preferably satisfies the following formula (2). 0.1≦I2 / S2≦1.2 …(2) however, I2 is the mass of the ionomer B, S2 is the mass of the support.

[0061] In formula (2), "I2 / S2" represents the ionomer ratio, that is, the ratio of the mass of ionomer B (I2) to the mass of the support (S2). When a catalyst layer is prepared using the composite according to the present invention, the ionomer B mainly plays a role of transferring protons between the catalyst particles. In order to obtain high power generation performance in a wide range of temperature and humidity conditions, from low temperature and high humidity conditions to high temperature and low humidity conditions, it is preferable that I2 / S2 satisfies a predetermined condition.

[0062] Ionomer B is mainly responsible for localized proton conduction around the catalyst particles. Therefore, the smaller I2 / S2 is, the better, as long as a minimum level of proton conductivity can be ensured. However, if I2 / S2 is too small, it may be difficult to transport protons to the catalyst particle surface. Therefore, I2 / S2 is preferably 0.1 or more. I2 / S2 is more preferably 0.2 or more, or 0.4 or more.

[0063] On the other hand, if I2 / S2 is too large, the porosity around the electrode catalyst becomes too small, and the gas diffusion resistance may increase. Therefore, I2 / S2 is preferably 1.2 or less. I2 / S2 is more preferably 1.0 or less, and even more preferably 0.8 or less. Furthermore, in order to obtain a catalyst layer that exhibits high performance under both high temperature and low humidity conditions and low temperature and high humidity conditions, it is preferable that the ionomer ratio (I2 / S2) of the ionomer / catalyst composite is smaller than the ionomer ratio (I1 / S1) of the ionomer / substrate composite.

[0064] [C. Ion exchange capacity] In the present invention, the ion exchange capacity of the ionomer B is not particularly limited. In the case of producing a catalyst layer using the composite according to the present invention, in order to suppress flooding, it is preferable that the ion exchange capacity of ionomer B is smaller than that of ionomer A. When the ion exchange capacity of ionomer B that covers the periphery of the electrode catalyst is relatively small, the periphery of the electrode catalyst becomes relatively hydrophobic. As a result, water generated by the electrode reaction is easily discharged to the outside of the ionomer / catalyst composite, and flooding (blockage of voids by liquid water) is suppressed.

[0065] Here, the difference (IEC1-IEC2) between the ion exchange capacity of ionomer A (IEC1) and the ion exchange capacity of ionomer B (IEC2) is defined as "ΔIEC". If ΔIEC is too small, the flooding suppression effect becomes insufficient. Therefore, ΔIEC is preferably 0.02 meq / g or more. ΔIEC is more preferably 0.05 meq / g or more, and even more preferably 0.1 meq / g or more.

[0066] On the other hand, if IEC2 is too small relative to IEC1, the proton resistance of the ionomer / catalyst composite may increase. Also, if IEC1 is too large relative to IEC2, too much water may accumulate around the ionomer / substrate composite, making it difficult to supply the reaction gas around the ionomer / catalyst composite. Therefore, ΔIEC is preferably 0.9 meq / g or less. ΔIEC is more preferably 0.5 meq / g or less, and even more preferably 0.4 meq / g or less.

[0067] [1.3. Structure of the complex] In the composite of the present invention, the surface of the ionomer / substrate composite is coated with an ionomer / catalyst composite, which is different from the conventional one. Here, "the surface of the ionomer / substrate composite is coated with the ionomer / catalyst composite" means that the ionomer / catalyst composite is deposited in the form of a layer on the surface of the ionomer / substrate composite.

[0068] When the dispersion of ionomer B and the electrode catalyst is evaporated to dryness as is, an ionomer / catalyst composite is usually produced in which the surface of the electrode catalyst is coated with ionomer B, and at the same time, many of the ionomer / catalyst composites aggregate to form coarse aggregates. When the coarse ionomer / catalyst composite thus obtained is mixed with an ionomer / substrate composite, the distance between the ionomer / substrate composite and the electrode catalyst becomes relatively long. In contrast, when the method described below is used, a composite is obtained in which isolated ionomer / catalyst composites or fine aggregates thereof are thinly and uniformly deposited on the surface of the ionomer / substrate composite, resulting in a relatively short distance between the ionomer / substrate composite and the electrode catalyst, and a decrease in the proton resistance of the proton conduction path that supplies protons to the electrode catalyst.

[0069] In producing the composite according to the present invention, controlling the production conditions changes the thickness and coverage area of ​​the ionomer / catalyst composite deposited in layers. In addition, in producing a catalyst layer using such a composite, optimizing the production conditions can suppress performance degradation caused by increased proton resistance. Specifically, the composite according to the present invention preferably satisfies the following conditions:

[0070] [1.3.1. Thickness ratio (t2 / t1)] The complex according to the present invention preferably satisfies the following formula (3). 0.01≦t2 / t1≦3.0 …(3) however, t1 is the thickness of the ionomer / substrate composite; t2 is the thickness of the ionomer / catalyst composite covering the surface of the ionomer / substrate composite.

[0071] In formula (3), "t2 / t1" represents the thickness ratio, ie, the ratio of the thickness of the ionomer / catalyst composite (t2) to the thickness of the ionomer / substrate composite (t1). In the present invention, "t2 / t1" refers to the average value of values ​​measured at multiple randomly selected locations (for example, 10 or more locations).

[0072] When a catalyst layer is produced using the composite according to the present invention, the larger t1 is, the wider the proton conduction path in the catalyst layer, and therefore the proton resistance can be reduced. Also, the smaller t2 is, the shorter the proton conduction path from the ionomer / substrate composite to the electrode catalyst, and therefore the proton resistance can be reduced. In order to reduce the proton resistance of the catalyst layer, t2 / t1 is preferably 3.0 or less. t2 / t1 is more preferably 1.0 or less, or 0.5 or less.

[0073] On the other hand, when a catalyst layer is produced using the composite according to the present invention, if t2 / t1 is too small, the weight of the catalyst particles will be small. In this case, the catalyst layer needs to be thickened to obtain a predetermined weight, but if the catalyst layer is too thick, the proton resistance of the catalyst layer will increase. Therefore, t2 / t1 is preferably 0.01 or more. t2 / t1 is more preferably 0.05 or more, or 0.10 or more.

[0074] [1.3.2. Mass ratio (W2 / W1)] The complex according to the present invention preferably satisfies the following formula (4). 0.1≦W2 / W1≦10.0 …(4) however, W1 is the mass of the ionomer / substrate composite; W2 is the mass of the ionomer / catalyst composite coating the surface of the ionomer / substrate composite.

[0075] In formula (4), "W2 / W1" represents the mass ratio, i.e., the ratio of the mass (W2) of the ionomer / catalyst composite contained in the composite to the mass (W1) of the ionomer / substrate composite contained in the composite.

[0076] When a catalyst layer is produced using the composite according to the present invention, the larger W1 is, the wider the proton conduction path in the catalyst layer, and therefore the proton resistance can be reduced. Also, the smaller W2 is, the shorter the proton conduction path from the ionomer / substrate composite to the electrode catalyst, and therefore the proton resistance can be reduced. In order to reduce the proton resistance, W2 / W1 is preferably 10.0 or less. W2 / W1 is more preferably 4.0 or less, or 2.0 or less.

[0077] On the other hand, when a catalyst layer is produced using the composite of the present invention, if W2 / W1 is too small, the weight of the catalyst particles will be small. In this case, the catalyst layer needs to be thickened to obtain a predetermined weight, but if the catalyst layer is too thick, the proton resistance of the catalyst layer will increase. Therefore, W2 / W1 is preferably 0.1 or more. W2 / W1 is more preferably 0.5 or more, or 1.0 or more.

[0078] [1.3.3. Relative thickness (t2 / D1)] The complex according to the present invention preferably satisfies the following formulas (5) and (6). 1μm≦D1≦50μm …(5) 0.001≦t2 / D1≦3.0 …(6) however, D1 is the maximum length of the ionomer / substrate composite; t2 is the thickness of the ionomer / catalyst composite covering the surface of the ionomer / substrate composite.

[0079] In equation (6), "t2 / D1" represents the relative thickness, ie, the ratio of the thickness (t2) of the ionomer / catalyst composite to the maximum thickness (D1) of the ionomer / substrate composite. "Maximum length (D1)" refers to the length of the longest side of a rectangular parallelepiped with the minimum volume that circumscribes the ionomer / substrate composite. In the present invention, the term "t2 / D1" refers to the average value of values ​​measured at multiple randomly selected locations (for example, 10 or more locations).

[0080] In the case of producing a catalyst layer using the composite according to the present invention, if D1 is too small, the connection between particles may become poor, and the proton resistance may become large. Therefore, D1 is preferably 1.0 μm or more. D1 is more preferably 2.0 μm or more, or 3.0 μm or more. On the other hand, if D1 is too large, the uniformity of the catalyst layer is lost, and in some cases, the electrolyte membrane may be damaged when pressed. Therefore, D1 is preferably 50 μm or less. D1 is more preferably 30 μm or less, 20 μm or less, 10 μm or less, or 5 μm or less.

[0081] If t2 / D1 is too large, proton resistance may be lower if protons pass through the ionomer / catalyst composite rather than the ionomer / substrate composite. Therefore, t2 / D1 is preferably 3.0 or less. t2 / D1 is more preferably 1.0 or less, or 0.5 or less.

[0082] On the other hand, when a catalyst layer is produced using the composite according to the present invention, if t2 / D1 is too small, the weight of the catalyst particles will be small. In this case, the catalyst layer needs to be thickened to obtain a predetermined weight, but if the catalyst layer is too thick, the proton resistance of the catalyst layer will increase. Therefore, t2 / D1 is preferably 0.001 or more. t2 / D1 is more preferably 0.003 or more, or 0.005 or more.

[0083] [1.3.4. Area ratio (A2 / A1)] The complex according to the present invention preferably satisfies the following formula (7). 0.3≦A2 / A1≦1.0 …(7) however, A1 is the total surface area of ​​the ionomer / substrate composite; A2 is the area of ​​the ionomer / catalyst composite covering the surface of the ionomer / substrate composite.

[0084] In formula (7), "A2 / A1" represents the area ratio, ie, the ratio of the area of ​​the ionomer / catalyst composite (A2) to the total surface area of ​​the ionomer-based composite (A1). In the present invention, unless otherwise specified, "A2 / A1" refers to the average value measured for a number of randomly selected complexes (for example, 10 or more complexes).

[0085] In the case of manufacturing a catalyst layer using the composite of the present invention, if A2 / A1 is too small, the weight of the catalyst particles will be small. In this case, the catalyst layer needs to be thickened to obtain a predetermined weight, but if the catalyst layer is too thick, the proton resistance of the catalyst layer will increase. Therefore, A2 / A1 is preferably 0.3 or more. A2 / A1 is preferably 0.4 or more, 0.5 or more, or 0.6 or more. A2 / A1 may be 1.0.

[0086] [2. Manufacturing method of the composite] The complex according to the present invention comprises (a) preparing an ionomer / substrate composite in which the surface of a substrate particle is coated with ionomer A; (b) heat-treating the ionomer / substrate composite to make the ionomer A insoluble in the solvent; (c) A dispersion liquid containing the insolubilized ionomer / substrate composite, an electrode catalyst, and ionomer B is prepared, and the dispersion medium is volatilized. It can be produced by the above method.

[0087] [2.1. 1st step] First, an ionomer / substrate composite is produced in which the surface of a substrate particle is coated with ionomer A. In the present invention, the method for producing the ionomer / substrate composite is not particularly limited. When the substrate particles are sheet-like particles, the ionomer / substrate composite is (a) preparing a dispersion containing base particles and ionomer A; (b) whipping the dispersion, freeze-drying the whipped dispersion, and pulverizing the freeze-dried product. It is preferable to produce the product by the above method. When the base particles are sheet-like particles, using such a method makes it possible to obtain an ionomer / base material composite in which the base particles are coated with ionomer A while maintaining the sheet shape.

[0088] [2.2. 2nd process] Next, the ionomer / substrate composite is heat-treated, which makes it possible to make the ionomer A that coats the surfaces of the substrate particles insoluble in the solvent. The heat treatment conditions are not particularly limited as long as they can make the ionomer A insoluble in the solvent. For example, when the ionomer A is a perfluorocarbon sulfonic acid polymer, the ionomer / substrate composite is preferably heat-treated at 130° C. to 200° C. for 1 to 3 hours.

[0089] [2.3. Third step] Next, a dispersion containing the insolubilized ionomer / substrate composite, an electrode catalyst, and ionomer B is prepared, and the dispersion medium is volatilized. As a result, an ionomer / catalyst composite in which the surface of the electrode catalyst is coated with ionomer B is formed, and at the same time, the surface of the ionomer / substrate composite is coated with the ionomer / catalyst composite.

[0090] In the present invention, the method for producing the composite (i.e., the method for volatilizing the dispersion medium) is not particularly limited. When the base material particles are sheet-like particles, the composite is (a) preparing a dispersion containing an insolubilized ionomer / substrate composite, an electrode catalyst, and ionomer B; (b) whipping the dispersion, freeze-drying the whipped dispersion, and pulverizing the freeze-dried product. It is preferable to produce the product by the above method. When the ionomer / substrate composite is a sheet-like composite, the use of such a method makes it possible to coat the surface of the ionomer / substrate composite with the ionomer / catalyst composite while the ionomer / substrate composite maintains its sheet shape.

[0091] In the above method, instead of the electrode catalyst, a composite obtained by coating the surface of the electrode catalyst with ionomer B' and insolubilizing the ionomer B' may be used. By using such a composite, a composite including an ionomer / substrate composite and an ionomer / catalyst composite in which the surface of the electrode catalyst is coated with a laminated film of two or more types of ionomers can be obtained.

[0092] [3. Catalyst layer] The catalyst layer according to the present invention can be obtained by applying the composite according to the present invention to the surface of a substrate (for example, an electrolyte membrane) by dry coating. Here, the term "dry coating method" refers to a method of forming a coating film using a dry paint that does not contain a solvent. In the present invention, the type of dry coating method is not particularly limited, and various methods can be used depending on the purpose. Examples of dry coating methods include electrostatic screen printing, electrostatic spraying, and fluidized bed dipping.

[0093] [4. Effect] FIG. 1 shows a schematic diagram of a dry-formed catalyst layer obtained by the method according to the present invention and the conventional method. An ionomer / catalyst composite (ionomer / Pt / C) and a proton conductive material (ionomer / graphite nanosheet=ionomer / substrate composite) are separately prepared, and a mixture of these is dry-coated on the substrate surface, to produce a catalyst layer containing an ionomer / catalyst composite and a proton conductive material. However, the ionomer / catalyst composite is usually in a state where many electrode catalysts are aggregated. Therefore, as shown in FIG. 1(a), a part of the electrode catalyst is located away from the proton conductive material.

[0094] Protons are supplied to the electrode catalyst located away from the ionomer / substrate composite via the ionomer contained in the ionomer / catalyst composite, but the ionomer / catalyst composite has a higher proton resistance than the ionomer / substrate composite. As a result, protons supplied to an electrode catalyst located away from the ionomer / substrate composite must travel a long distance through the ionomer / catalyst composite, which has high proton resistance, causing a decrease in the power generation performance of the fuel cell.

[0095] In contrast, when the method of the present invention is used, a composite can be obtained in which all or part of the surface of the proton conductive material (ionomer / substrate composite) is thinly and uniformly covered with fine (less aggregated) ionomer / catalyst composite, as shown in FIG. 1(b). Therefore, the distance of the proton conduction path from the proton conductive material to the electrode catalyst is shorter than when a pre-produced proton conductive material is mixed with an ionomer / catalyst composite, and as a result, it is possible to suppress the performance degradation caused by protons moving long distances through a proton conduction path with high proton resistance. EXAMPLES

[0096] (Examples 1 to 2, Comparative Examples 1 to 3) [1. Sample preparation] 1.1. Powder preparation [1.1.1. Comparative Example 1] A. Preparation of Nafion® / Platinum-loaded Carbon Composite Powder A first dispersion was obtained by adding 2 g of platinum-loaded carbon (Tanaka Kikinzoku Kogyo K.K., TEC10V30E, platinum loading rate 29 mass%) and 4.89 g of Nafion (registered trademark) solution (Chemours, DE2020CS, concentration: 20.9 mass%) (corresponding to I2 / S2=0.75) to 15.9 g of ultrapure water. This first dispersion was stirred with a planetary degassing mixer (KK-250S, manufactured by Kuraray Industries, Ltd.) and dispersed with a high-pressure homogenizer (Starburst Mini, manufactured by Sugino Machine Ltd., nozzle diameter: 200 μm, pressure: 50 MPa, one treatment) to obtain a catalyst ink.

[0097] The prepared catalyst ink was whipped using an electric creamer while gradually adding 9 g of ultrapure water. The whipped catalyst ink was poured onto a stainless steel pad coated with fluororesin and frozen in a pre-cooled freeze dryer (DF-05H, manufactured by ULVAC, Inc.). After confirming that the whipped catalyst ink had reached -40°C, a vacuum was pulled. The cooling location was switched from the tank to the cold trap side, and the sample was dried for more than 24 hours. After confirming that the sample temperature was equivalent to room temperature, the sample was removed from the freeze dryer. Hereafter, this sample is referred to as "Naf / Pt / C".

[0098] [B. Preparation of ionomer / graphite nanosheet composite powder] Graphite (SG-BH8, manufactured by Ito Graphite Industries Co., Ltd.): 4 g and Nafion (registered trademark) solution: 57.4 g (corresponding to I1 / S1 = 3.0) were added to ultrapure water: 98.57 g to obtain a second dispersion. This second dispersion was stirred with a planetary degassing stirrer and dispersed with a high-pressure homogenizer (nozzle diameter: 100 μm, pressure: 245 MPa, treatment three times) to cleave the graphite, obtaining a third dispersion containing ionomer and graphite nanosheets. The third dispersion was then foamed and freeze-dried in the same manner as in the case of Naf / Pt / C. Hereinafter, this sample is referred to as "Naf / GNS."

[0099] [C. Preparation of mixed powder] Naf / Pt / C and Naf / GNS were mixed in a mass ratio of 3:2 to obtain a mixed powder.

[0100] [1.1.2. Example 1: Preparation of Nafion (registered trademark) / Platinum-loaded carbon / Ionomer / Graphite nanosheet composite] The Naf / GNS prepared in Comparative Example 1 was dried under reduced pressure at 165° C. for 2 hours using a vacuum dryer to make Nafion (registered trademark) insoluble in the solvent. 1.9 g of platinum-supported carbon and 4.63 g of Nafion (registered trademark) solution (corresponding to I2 / S2=0.75) were added to 16.93 g of ultrapure water to obtain a fourth dispersion.

[0101] After stirring this fourth dispersion with a planetary defoaming stirrer, 1.88 g of heat-treated Naf / GNS (equivalent to 40 mass% of the total solid content, W2 / W1 = 60 / 40) was added and stirred again with the planetary defoaming stirrer. This was dispersed with a high-pressure homogenizer (nozzle diameter: 200 μm, pressure: 50 MPa, treated three times) to obtain a catalyst ink. The catalyst ink thus prepared was further whipped with an electric creamer while gradually adding 9 g of ultrapure water. The following procedure was repeated to freeze-dry the mixture in the same manner as in Comparative Example 1. Hereinafter, this sample will be referred to as "Naf / Pt / C / Naf / GNS".

[0102] [1.1.3. Comparative Example 2] [A. Preparation of HOPI / Platinum-loaded carbon composite powder] A fifth dispersion was obtained by adding 2 g of platinum-loaded carbon (Tanaka Kikinzoku Kogyo Co., Ltd., TEC10V30E, platinum loading rate: 29 mass%) and 9.72 g of HOPI solution (EW: 884 g / mol, concentration: 10.5 mass%) (corresponding to I2 / S2 = 0.75) to 15.18 g of ultrapure water. This fifth dispersion was stirred with a planetary degassing mixer (KK-250S, manufactured by Kuraray Industries, Ltd.) and dispersed with a high-pressure homogenizer (Starburst Mini, manufactured by Sugino Machine Ltd., nozzle diameter: 200 μm, pressure: 50 MPa, treatment three times) to obtain a catalyst ink.

[0103] The prepared catalyst ink was whipped using an electric creamer while gradually adding 6 g of ultrapure water. The whipped catalyst ink was poured onto a stainless steel pad coated with fluororesin and frozen in a pre-cooled freeze dryer (DF-05H, manufactured by ULVAC, Inc.). After confirming that the whipped catalyst ink had reached -40°C, a vacuum was pulled. The cooling location was switched from the tank to the cold trap side, and the sample was dried for more than 24 hours. After confirming that the sample temperature was equivalent to room temperature, the sample was removed from the freeze dryer. Hereafter, this sample is referred to as "HOPI / Pt / C".

[0104] [B. Preparation of mixed powder] HOPI / Pt / C and Naf / GNS were mixed in a mass ratio of 3:2 to obtain a mixed powder.

[0105] [1.1.4. Example 2: Preparation of HOPI / Platinum-loaded carbon / Ionomer / Graphite nanosheet composite (Example 2)] The Naf / GNS prepared in Comparative Example 1 was dried under reduced pressure at 165° C. for 2 hours using a vacuum dryer to make Nafion (registered trademark) insoluble in the solvent. 2.0 g of platinum-supported carbon and 9.72 g of the HOPI solution (corresponding to I2 / S2=0.75) were added to 15.17 g of ultrapure water to obtain a sixth dispersion.

[0106] After stirring this sixth dispersion with a planetary defoaming stirrer, 1.97 g of heat-treated Naf / GNS (equivalent to 40 mass% of the total solid content, W2 / W1 = 60 / 40) was added and stirred again with the planetary defoaming stirrer. This was dispersed with a high-pressure homogenizer (nozzle diameter: 200 μm, pressure: 50 MPa, treated three times) to obtain a catalyst ink. The catalyst ink thus prepared was further whipped with an electric creamer while gradually adding 18 g of ultrapure water. The following procedure was repeated to freeze-dry the mixture in the same manner as in Comparative Example 1. Hereinafter, this sample will be referred to as "HOPI / Pt / C / Naf / GNS".

[0107] [1.2. Preparation of cathode catalyst layer and membrane electrode assembly by dry deposition] Using an electrostatic screen printer (Belk Kogyo Co., Ltd., T1 type, #250 mesh), the powder was applied onto the fluorine-based electrolyte membrane to form a 10 mm square cathode catalyst layer. (a) Naf / Pt / C only (Comparative Example 3), (b) A mixed powder of Naf / Pt / C and Naf / GNS (Comparative Example 1), or (c) Naf / Pt / C / Naf / GNS only (Example 1) was used.

[0108] The applied voltage was 2 kV. The gap between the screen and the electrolyte membrane surface was 8 mm. The platinum weight was approximately 0.15 mg. -Pt / cm 2 It was decided. Furthermore, an anode catalyst layer was formed by thermal transfer on the surface opposite to the surface on which the cathode catalyst was formed, to obtain a membrane electrode assembly.

[0109] 2. Test Method [2.1. SEM Observation] The obtained powder was observed by SEM.

[0110] [2.2. Cell testing] The surface area of ​​the electrode is 1 cm 2 A small cell was assembled using the membrane electrode assembly and connected to an evaluation bench for evaluation. Carbon paper (with microporous layer) and SIGRACET (registered trademark) 22BB manufactured by SGL were used for the gas diffusion layer. A gold-plated copper plate with a 0.4 mm wide linear flow channel molded into it was used for the current collector.

[0111] A large amount of gas was passed through the small cell and a cell test was carried out. The evaluation items were: (a) Power generation evaluation test by voltage sweep (IV measurement: pure hydrogen-air), and (b) Proton resistance measurement of the catalyst layer using AC impedance spectroscopy (10% hydrogen-nitrogen) The cell temperature was 82°C, and the bubbler temperature was 55°C (equivalent to 30% RH).

[0112] [3. Results] [3.1. SEM Observation] 3.1.1. Example 1 The obtained Naf / Pt / C / Naf / GNS was crushed with a blade mill, and the crushed powder was observed by SEM. Figure 2 shows an SEM photograph of the composite (Naf / Pt / C / Naf / GNS) obtained in Example 1. Although it is difficult to see because the Naf / Pt / C with fine irregularities covers almost the entire Naf / GNS, the base of Naf / GNS without irregularities was confirmed in part of the composite. From Figure 2, it can be seen that a composite was obtained in which the surface of Naf / GNS was coated with Naf / Pt / C. In the case of Example 1, t2 / t1 = 0.4, t2 / D1 = 0.01, and A2 / A1 = 0.95.

[0113] 3.1.2. Example 2 The obtained HOPI / Pt / C / Naf / GNS was crushed with a blade mill, and the crushed powder was observed by SEM. Figure 3 shows an SEM photograph of the composite (HOPI / Pt / C / Naf / GNS) obtained in Example 2. A smooth Naf / GNS base was confirmed in part of the composite. From Figure 3, it can be seen that a composite was obtained in which the surface of Naf / GNS was coated with HOPI / Pt / C with fine irregularities. In the case of Example 2, t2 / t1 = 0.5, t2 / D1 = 0.02, and A2 / A1 = 0.9.

[0114] [3.1.3. Comparative Example 1] A mixed powder of Naf / Pt / C and Naf / GNS (mass ratio 3:2) was mixed and crushed using a blade mill, and the crushed powder was observed using an SEM. Figure 4 shows an SEM photograph of the mixed powder (Naf / Pt / C+Naf / GNS_Mix) obtained in Comparative Example 1. Naf / Pt / C and Naf / GNS were observed separately. Small pieces of Naf / Pt / C were attached to the surface of Naf / GNS, but the proportion of Naf / Pt / C attached was very small.

[0115] [3.1.4. Comparative Example 2] A mixed powder of HOPI / Pt / C and Naf / GNS (mass ratio 3:2) was mixed and crushed using a blade mill, and the crushed powder was observed using an SEM. Figure 5 shows an SEM photograph of the mixed powder (HOPI / Pt / C+Naf / GNS_Mix) obtained in Comparative Example 2. HOPI / Pt / C and Naf / GNS were observed separately. Small pieces of HOPI / Pt / C were attached to the surface of Naf / GNS, but the proportion of attached HOPI / Pt / C was very small.

[0116] [3.2. Cell testing] 6 shows the current density at 0.6 V (IR corrected voltage) at 82° C. and 30% RH for the cells obtained in Example 1, Comparative Example 1, and Comparative Example 3. The current density of Example 1 was higher than those of Comparative Example 1 and Comparative Example 3.

[0117] 7 shows the catalyst layer proton resistance at 82°C and 30% RH for the cells obtained in Example 1, Comparative Example 1, and Comparative Example 3. The "catalyst layer proton resistance" refers to the proton resistance (R / 3) in the membrane thickness direction obtained by the AC impedance method in a non-power generation state at 82°C and 30% RH. Comparative Example 3 had the highest proton resistance because it did not contain Naf / GNS, which is a proton conductive material. In contrast, Comparative Example 1 and Example 1, which contain a proton conductive material, had lower proton resistance than Comparative Example 3.

[0118] The proton resistances of Example 1 and Comparative Example 1 were almost the same. However, it should be noted that this proton resistance represents the proton resistance in the film thickness direction of the catalyst layer, and does not reflect the proton resistance of the proton conduction path from the proton conductive material to the catalyst. Considering the results of the power generation evaluation, the proton resistance in the film thickness direction is the same between Example 1 and Comparative Example 1, but the current density at 82°C and 30% RH of Example 1 is thought to be improved compared to that of Comparative Example 1 because the proton resistance up to the catalyst can be reduced.

[0119] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]

[0120] The composite according to the present invention can be used as a raw material for producing a catalyst layer of a polymer electrolyte fuel cell.

Claims

1. an ionomer / substrate composite in which the surface of a substrate particle is coated with ionomer A; An ionomer / catalyst composite in which the surface of the electrode catalyst is coated with ionomer B. Equipped with The electrode catalyst comprises a support and catalyst particles supported on a surface of the support, The surface of the ionomer / substrate composite is coated with the ionomer / catalyst composite. Complex.

2. The composite of claim 1 , wherein the substrate particle comprises a graphite nanosheet.

3. The ionomer A includes a perfluorocarbon sulfonic acid polymer, The ionomer B includes a perfluorocarbon sulfonic acid polymer and / or a highly oxygen permeable ionomer. The composite of claim 1.

4. The composite of claim 1 , wherein the ionomer / substrate composite satisfies the following formula (1): 0.5≦I 1 / S 1 ≦10.0 ... (1) however, I 1 is the mass of the ionomer A, S 1 is the mass of the substrate.

5. The composite of claim 1 , wherein the ionomer / catalyst composite satisfies the following formula (2): 0.1≦I 2 / S 2 ≦1.2 … (2) however, I 2 is the mass of the ionomer B, S 2 is the mass of the support.

6. The composite according to claim 1, which satisfies the following formula (3): 0.01≦t 2 / t 1 ≦3.0 ... (3) however, t 1 is the thickness of the ionomer / substrate composite, t 2 is the thickness of the ionomer / catalyst composite covering the surface of the ionomer / substrate composite.

7. The composite according to claim 1, which satisfies the following formula (4): 0.1≦W 2 / W 1 ≦10.0 ... (4) however, W 1 is the mass of the ionomer / substrate composite, W 2 is the mass of the ionomer / catalyst composite coating the surface of the ionomer / substrate composite.

8. The composite according to claim 1, which satisfies the following formulas (5) and (6). 1 μm≦D 1 ≦50 μm ... (5) 0.001≦t 2 / D 1 ≦3.0 ... (6) however, D 1 is the maximum length of the ionomer / substrate composite, t 2 is the thickness of the ionomer / catalyst composite covering the surface of the ionomer / substrate composite.

9. The composite according to claim 1, which satisfies the following formula (7): 0.3≦A 2 / A 1 ≦1.0 ... (7) however, A 1 is the total surface area of ​​the ionomer / substrate composite, A 2 is the area of ​​the ionomer / catalyst composite covering the surface of the ionomer / substrate composite.

10. A catalyst layer comprising the composite according to claim 1.

Citation Information

Patent Citations

  • Catalyst layer

    JP2021068638A

  • Sheet-like particle composite and manufacturing method thereof

    JP2022143571A

  • Catalyst layer

    JP2022181252A

Cited By

  • Printer device

    CN121733957A