Electrolytic capacitor

By using a cathode body with a carbon layer and specific carbon-containing electrolytes, the capacitance of electrolytic capacitors is stabilized, addressing the issue of capacitance fluctuations and extending their operational life.

JP2024140480APending Publication Date: 2024-10-10NIPPON CHEMI CON CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023051632
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Electrolytic capacitors experience significant changes in capacitance over time, leading to potential failure of electronic or electrical circuits, necessitating frequent replacements that require equipment downtime and backup.

Method used

Incorporating a cathode body with a carbon layer and using an electrolytic solution containing monocarboxylic or dicarboxylic acids with 8 or more carbon atoms to stabilize capacitance.

Benefits of technology

The capacitance of electrolytic capacitors is less likely to change over time, extending their lifespan and reducing the need for frequent replacements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140480000001_ABST
    Figure 2024140480000001_ABST
Patent Text Reader

Abstract

To provide an electrolytic capacitor which is less susceptible to fluctuations in capacitance over time.SOLUTION: An electrolytic capacitor includes an anode body, a cathode body having a carbon layer laminated on its surface, and an electrolyte. The electrolyte contains a monocarboxylic acid or a dicarboxylic acid having 8 or more carbon atoms.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolytic capacitor. [Background technology]

[0002] An electrolytic capacitor has valve metals such as tantalum or aluminum as anode and cathode foils. Electrolytic capacitors obtain their anode capacitance through the dielectric polarization of the dielectric film. The anode foil is enlarged by forming the valve metal into a sintered or etched foil, etc., and has a dielectric film layer on the enlarged surface. An electrolyte is interposed between the anode foil and the cathode foil. The electrolyte comes into contact with the uneven surface of the anode foil and functions as the true cathode.

[0003] This electrolytic capacitor can increase the surface area by expanding the surface area of ​​the anode foil. Also, since the electrolyte is a liquid, the contact area between the anode foil and the dielectric film increases. Therefore, the electrolytic capacitor can easily meet various rated capacitances required for electronic or electric circuits.

[0004] For example, in the field of power electronics, a power conversion circuit converts the power of an AC power source into DC power using a converter circuit, and then converts this DC power into a desired AC power using an inverter circuit. In this case, a smoothing capacitor is provided in order to suppress and smooth the pulsation of the DC output from the converter circuit before inputting it to the inverter circuit. In addition, a decoupling capacitor is provided near the semiconductor switching element to ensure stable operation of the semiconductor switching element and to remove noise.

[0005] In such electronic devices or electric circuits, if the capacitance of the electrolytic capacitor fluctuates over time, such as decreasing or increasing significantly beyond the design range, it can cause the entire electronic or electric circuit, such as a power conversion device, to stop operating. Therefore, a capacitance measuring device that monitors the state of the electrolytic capacitor has been proposed (for example, see Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent Publication No. 2021-151182 Summary of the Invention [Problem to be solved by the invention]

[0007] Although it is possible to monitor the capacitance of an electrolytic capacitor and replace the electrolytic capacitor before the entire electronic or electric circuit stops working, the device must be temporarily stopped or a backup device must be prepared when replacing the electrolytic capacitor. Therefore, there is a demand for an electrolytic capacitor whose capacitance is less likely to change over time.

[0008] The present invention has been proposed to solve the above problems, and an object of the present invention is to provide an electrolytic capacitor that is less susceptible to fluctuations in capacitance over time. [Means for solving the problem]

[0009] In order to solve the above problems, the electrolytic capacitor of the present embodiment includes an anode body, a cathode body having a carbon layer laminated on the surface thereof, and an electrolyte solution containing a monocarboxylic acid or a dicarboxylic acid having 8 or more carbon atoms.

[0010] The electrolytic solution may contain the monocarboxylic acid having 5 or more carbon atoms, or the dicarboxylic acid having 12 or more carbon atoms.

[0011] The cathode body may have a cathode foil having a surface-expanding layer formed on its surface, the carbon layer containing a carbon material, and a portion of the carbon material of the carbon layer may be laminated on the cathode foil and may fill some or all of the recesses, holes or voids in the surface-expanding layer.

[0012] The carbon layer may be a pressed layer on the cathode foil, or a vapor-deposited layer on the cathode foil. Effect of the Invention

[0013] According to the present invention, the capacitance of the electrolytic capacitor is less likely to vary over time. [Brief description of the drawings]

[0014] [Figure 1] 1 is a graph showing the rate of capacity change when various cathode bodies are combined with an electrolyte solution containing a dicarboxylic acid having seven or less carbon atoms. [Diagram 2] 1 is a graph showing the rate of capacity change when various cathode bodies are combined with an electrolyte solution containing a dicarboxylic acid having 8 or more and 10 or less carbon atoms. [Diagram 3] 1 is a graph showing the rate of capacity change when various cathode bodies are combined with an electrolyte solution containing a dicarboxylic acid having 12 or more carbon atoms. [Figure 4] 1 is a graph showing the rate of capacity change when various cathode bodies are combined with an electrolyte solution containing a monocarboxylic acid having one carbon atom. [Diagram 5] 1 is a graph showing the rate of capacity change when various cathode bodies are combined with an electrolyte solution containing a monocarboxylic acid having 5 or more carbon atoms. [Figure 6] 1 is a graph showing the rate of capacity change when various cathode bodies are combined with an aromatic-containing electrolyte solution. [Figure 7] 1 is a graph showing a capacitance reduction rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described below with reference to the preferred embodiments. However, the present invention is not limited to the preferred embodiments described below.

[0016] (Overall composition) An electrolytic capacitor is a passive device that obtains capacitance by the dielectric polarization of a dielectric film and stores and discharges electric charge. The electrolytic capacitor includes a capacitor element. The capacitor element is an assembly including an anode body, a cathode body, a separator, and an electrolyte.

[0017] A dielectric film is formed on the surface of the anode body. The anode body and cathode body face each other via a separator. An electrolyte is impregnated in the gaps in the capacitor element, particularly between the anode body and the cathode body. This electrolyte comes into contact with the dielectric film of the anode body and is arranged so as to connect between the dielectric film and the cathode body, creating a conductive path and functioning as a true cathode.

[0018] The anode and cathode are alternately stacked with a separator sandwiched between them in a stacked arrangement. In the stacked arrangement, the capacitor element may be a flat plate type that omits the exterior, or may be sealed by, for example, covering the capacitor element with a laminate film, or by molding, dip coating, or printing with a resin such as a heat-resistant resin or an insulating resin.

[0019] Alternatively, the anode body and the cathode body are wound in a wound arrangement in which they are alternately stacked with a separator sandwiched therebetween. In the wound arrangement, for example, the capacitor element is inserted into a cylindrical exterior case with a bottom, and the open end of the exterior case is sealed with a sealing body by crimping. The sealing body is made of, for example, rubber, or a laminate of rubber and a hard substrate. Examples of rubber include ethylene propylene rubber and butyl rubber.

[0020] An example of a method for manufacturing this electrolytic capacitor is outlined below. In the first step, an anode body and a cathode body, each having a dielectric film formed on its surface, are stacked with a separator between them to form a capacitor element. In the second step, the capacitor element is impregnated with an electrolyte. To promote the impregnation of the electrolyte into the capacitor element, a depressurization treatment or a pressurization treatment may be performed as necessary. The impregnation step may be repeated multiple times. In the third step, packaging is performed, such as by sealing the open end of the case into which the capacitor element is inserted with a sealing body, and aging is performed to repair defective parts by applying a voltage.

[0021] (Anode body) In such an electrolytic capacitor, the anode body has an anode foil made of a valve metal, such as aluminum, tantalum, niobium, niobium oxide, titanium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony. The purity of the anode body is preferably 99.9% or more, but impurities such as silicon, iron, copper, magnesium, and zinc may be included.

[0022] The anode foil is a long strip of valve metal in a wound electrolytic capacitor, and a flat plate in a laminated electrolytic capacitor. The anode foil is formed by stretching valve metal into a foil shape, or by molding and sintering powder into a foil shape. A surface expansion layer is formed on one or both sides of the anode body. The surface expansion layer is a surface layer that has been treated to increase the surface area beyond the projected area.

[0023] The surface-expanding layer may be, for example, an etching layer obtained by subjecting a foil to electrolytic or chemical etching, a sintered layer obtained by sintering valve metal powder, or a deposition layer obtained by depositing valve metal particles onto a foil. That is, the surface-expanding layer has a porous structure and is composed of holes or recesses such as tunnel-like or spongy pits, or voids between densely packed powder or particles.

[0024] The dielectric film is formed on one or both surfaces of the anode body along the unevenness of the surface expansion layer. The dielectric film is typically an oxide film formed by anodizing the surface layer of the anode body, and if the anode foil is made of aluminum, it is an aluminum oxide layer formed by oxidizing the surface of the surface expansion layer. In the chemical conversion treatment for forming the dielectric film, a voltage is applied to the anode body in a chemical conversion solution so as to achieve a desired withstand voltage. The chemical conversion solution is a solution that does not contain halogen ions, and examples of such solutions include phosphoric acid-based chemical conversion solutions such as ammonium dihydrogen phosphate, boric acid-based chemical conversion solutions such as ammonium borate, and adipic acid-based chemical conversion solutions such as ammonium adipate.

[0025] (cathode body) The cathode body has a two-layer structure of a cathode foil and a carbon layer. The cathode foil of the wound electrolytic capacitor is a long, drawn foil made of valve metal. The purity is preferably about 99% or more, but impurities such as silicon, iron, copper, magnesium, and zinc may be included. For the cathode foil, for example, an aluminum material having a temper code of H as specified in JIS standard H0001, so-called H material, or an aluminum material having a temper code of O as specified in JIS standard H0001, so-called O material, may be used. When a metal foil made of H material with high rigidity is used, deformation of the cathode foil due to press processing, which will be described later, can be suppressed. The cathode body of the laminated electrolytic capacitor may be a metal layer such as a silver layer.

[0026] Although a plain foil without a surface-expanding layer may be used as the cathode foil, it is preferable that the cathode foil has a surface-expanding layer on one or both sides, similar to the anode body. The carbon layer contains a carbon material as a main material. The carbon material of the carbon layer enters the recesses, holes, or gaps of the surface-expanding layer, so that the interface between the carbon layer and the cathode foil has a labyrinth structure, and the solute components of the electrolyte are less likely to come into contact with the surface of the cathode foil. Therefore, the electrolytic capacitor is prevented from varying in capacitance over time, and the electrostatic capacitance is stabilized. This cathode foil may have a natural oxide film or a thin oxide film (about 1 to 10 V) formed by chemical conversion treatment. The natural oxide film is formed by the reaction of the cathode body with oxygen in the air.

[0027] The carbon layer includes a carbon material and is laminated on the surface of the cathode foil. The carbon material is fibrous carbon, carbon powder, or a mixture thereof. The fibrous carbon is carbon nanotubes, carbon nanofibers, etc. The carbon nanotubes may be single-walled carbon nanotubes with one graphene sheet, or multi-walled carbon nanotubes (MWCNTs) with two or more graphene sheets rolled coaxially to form multiple tube walls. The carbon powder may be activated carbon derived from natural plant tissues such as coconut shells, synthetic resins such as phenol, fossil fuels such as coal, coke, and pitch, carbon blacks such as ketjen black, acetylene black, and channel black, carbon nanohorns, amorphous carbon, natural graphite, artificial graphite, graphitized ketjen black, mesoporous carbon, etc.

[0028] The fibrous carbon or carbon powder may be subjected to a porous treatment such as an activation treatment or an opening treatment to form holes. The activation method of the carbon powder varies depending on the raw material used, but generally, a conventionally known activation treatment such as a gas activation method or a chemical activation method can be used. Examples of the gas used in the gas activation method include water vapor, air, carbon monoxide, carbon dioxide, hydrogen chloride, oxygen, or a gas consisting of a mixture of these. Examples of the chemical used in the chemical activation method include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, alkaline earth metal hydroxides such as calcium hydroxide, inorganic acids such as boric acid, phosphoric acid, sulfuric acid, and hydrochloric acid, and inorganic salts such as zinc chloride. During this activation treatment, a heat treatment is performed as necessary.

[0029] This carbon layer can be formed by preparing a slurry containing a carbon material, applying the slurry to the cathode foil, and then drying and pressing the slurry. The slurry is applied to the cathode foil by a slurry casting method, a doctor blade method, a spray atomization method, or the like. After application, the solvent is evaporated by drying.

[0030] The slurry is prepared by dispersing the carbon material in a solvent and adding a binder. The carbon material may be pulverized by a pulverizing means such as a bead mill or a ball mill to adjust the particle size. The solvent for the slurry may be an alcohol such as methanol, ethanol, or 2-propanol, a hydrocarbon solvent, an aromatic solvent, an amide solvent such as N-methyl-2-pyrrolidone (NMP) or N,N-dimethylformamide (DMF), water, or a mixture thereof.

[0031] Dispersion methods include a mixer, jet mixing (jet collision), ultracentrifugation, ultrasonic treatment, etc. In the dispersion process, the graphite, spherical carbon, and binder in the mixed solution are finely divided and homogenized, and dispersed in the solution. Examples of binders include styrene butadiene rubber, polyvinylidene fluoride, and polytetrafluoroethylene.

[0032] In the pressing process of the carbon layer, for example, a cathode body consisting of the carbon layer and the cathode foil is sandwiched between press rollers and a linear press pressure is applied. The pressing pressure is 0.01 to 100 t / cm 2 According to this method for producing a carbon layer by coating and pressing, the carbon material of the carbon layer can be made to enter the recesses, holes or gaps of the surface-expanding layer, and the interface between the carbon layer and the cathode foil has a labyrinth structure.

[0033] The carbon layer may be formed by laminating a carbon material on the cathode foil by a vapor deposition method such as ion plating. Examples of the vapor deposition method include a resistance heating vapor deposition method and an electron beam heating vapor deposition method. In the vapor deposition method, the carbon material is evaporated by heating the carbon material by electrical current in a vacuum, or by irradiating the carbon material with an electron beam in a vacuum, to form a film of the carbon material on the cathode foil. This vapor deposition method for forming the carbon layer also allows the carbon material of the carbon layer to enter the recesses, holes, or gaps of the surface-expanding layer, and the interface between the carbon layer and the cathode foil has a labyrinth structure.

[0034] Alternatively, the carbon layer may be formed into a sheet and placed on the cathode foil. The formed sheet is prepared by dispersing the carbon material to be contained in the carbon layer in a dispersion solvent, adding a binder as necessary, filtering under reduced pressure, drying, and then peeling off the deposit from the filter paper. Methods for forming the carbon layer on the cathode foil include sputtering, CVD, electrolytic plating, and electroless plating.

[0035] (electrolyte) The electrolyte is a mixed solution in which a solute is dissolved in a solvent and an additive is added as necessary. The solute contained in the electrolyte contains an anion and a cation, typically an organic acid or a salt thereof, an inorganic acid or a salt thereof, or a complex compound of an organic acid and an inorganic acid or an ion-dissociable salt thereof, and is used alone or in combination of two or more. An acid that becomes an anion and a base that becomes a cation may be added separately to the electrolyte as solute components.

[0036] The electrolyte contains, as the anion component, a monocarboxylic acid, a dicarboxylic acid having 8 or more carbon atoms, or both of these. The carbon number indicates the total carbon number of each compound. When the electrolyte contains a dicarboxylic acid having 7 or less carbon atoms, there is no significant difference in the capacitance fluctuation between an electrolytic capacitor having a cathode body with a carbon layer, an electrolytic capacitor having a cathode foil with no oxide film formed, and an electrolytic capacitor having a cathode foil with an oxide film formed. In addition, even when an aromatic anion component is contained in the electrolyte, there is no significant difference in the capacitance fluctuation between an electrolytic capacitor having a cathode body with a carbon layer, an electrolytic capacitor having a cathode foil with no oxide film formed, and an electrolytic capacitor having a cathode foil with an oxide film formed.

[0037] However, when the cathode body has a carbon layer and the electrolyte contains a monocarboxylic acid or a dicarboxylic acid having 8 or more carbon atoms, the capacitance of the electrolytic capacitor changes little over time, and the capacitance of the electrolytic capacitor becomes stable. Also, when the cathode body has a carbon layer and the electrolyte contains a monocarboxylic acid having 5 or more carbon atoms or a dicarboxylic acid having 12 or more carbon atoms, the capacitance of the electrolytic capacitor changes little over time, and the capacitance of the electrolytic capacitor becomes stable.

[0038] Examples of monocarboxylic acids contained in the electrolyte include formic acid, pivalic acid, octylic acid, or a combination of these. Octylic acid, also called pivalic acid and caprylic acid, is a monocarboxylic acid having 5 or more carbon atoms. Examples of dicarboxylic acids having 8 or more carbon atoms contained in the electrolyte include suberic acid, azelaic acid, t-butyl adipic acid, sebacic acid, 2-butyl octanedioic acid, brassylic acid, 11-vinyl-8-octadecenedioic acid, or a combination of these. 2-butyl octanedioic acid, brassylic acid, and 11-vinyl-8-octadecenedioic acid are dicarboxylic acids having 12 or more carbon atoms.

[0039] Here, the embodiment in which the cathode body has a carbon layer and the electrolytic solution contains a monocarboxylic acid or a dicarboxylic acid having 8 or more carbon atoms is particularly useful in electrolytic capacitors for medium to high voltage applications of 100V or more. Electrolytic capacitors for medium to high voltage applications of 100V or more are also required to have a thinner dielectric film while maintaining a withstand voltage. However, as the dielectric film is made thinner, the valve metal becomes more likely to come into contact with the moisture in the electrolytic solution, and the opportunities for reaction between the valve metal and the moisture in the electrolytic solution increase, resulting in an increased amount of hydrogen gas generation. If the amount of gas generated in the electrolytic capacitor increases, it will cause the exterior case to swell, the valve to open, or the electrolyte to leak, and the electrolytic capacitor will reach the end of its life.

[0040] On the other hand, the carbon layer formed on the surface of the cathode body has the effect of suppressing hydrogen gas generation. Therefore, in an electrolytic capacitor using a cathode body having a carbon layer formed on its surface, the time until the occurrence of a valve opening due to hydrogen gas is extended. As a result, the time when the capacitance of the electrolytic capacitor changes so greatly that the operation of the entire electronic circuit or electric circuit of the power conversion device or the like stops may arrive earlier than the time when the life of the electrolytic capacitor ends due to the valve opening.

[0041] That is, in the conventional electrolytic capacitor, the period until the end of the life due to the generation of hydrogen gas is shorter than the period until the end of the life due to the solute, and the life due to the generation of hydrogen gas comes first. However, by using a cathode body having a carbon layer that suppresses hydrogen gas generation, the life of the electrolytic capacitor due to hydrogen gas is extended, so the period until the end of the life of the electrolytic capacitor due to the solute is relatively short, and the time when the life of the electrolytic capacitor due to the rate of change of the capacitance comes first. As a result, the problem of the life of the electrolytic capacitor due to the change of the capacitance has become apparent. However, by having a cathode body with a carbon layer and including a monocarboxylic acid or a dicarboxylic acid having 8 or more carbon atoms in the electrolytic solution, the rate of change of the capacitance of the electrolytic capacitor is suppressed from increasing, and the life of the electrolytic capacitor can be extended. From this point of view, it can be seen that including a monocarboxylic acid or a dicarboxylic acid having 8 or more carbon atoms in the electrolytic solution is particularly effective in solving the problems caused by using a cathode body having a carbon layer in the electrolytic capacitor.

[0042] As organic acids that become anion components in the electrolyte, oxalic acid, succinic acid, glutaric acid, pimelic acid, phthalic acid, isophthalic acid, terephthalic acid, maleic acid, adipic acid, benzoic acid, toluic acid, enanthic acid, malonic acid, 1,6-decanedicarboxylic acid, 1,7-octanedicarboxylic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, and other carboxylic acids, phenols, and sulfonic acids may be further included. In addition, as inorganic acids, boric acid, phosphoric acid, phosphorous acid, hypophosphorous acid, carbonic acid, silicic acid, and the like may be included. As composite compounds of organic acids and inorganic acids, borodisalicylic acid, borodioxalic acid, borodiglycolic acid, and the like may be included.

[0043] In addition, examples of at least one salt of an organic acid, an inorganic acid, and a complex compound of an organic acid and an inorganic acid include ammonium salt, quaternary ammonium salt, quaternary amidinium salt, amine salt, sodium salt, potassium salt, etc. Examples of quaternary ammonium include tetramethylammonium, triethylmethylammonium, tetraethylammonium, etc. Examples of quaternary amidinium include ethyldimethylimidazolinium, tetramethylimidazolinium, etc. Examples of amines in amine salts include primary amines, secondary amines, and tertiary amines. Examples of primary amines include methylamine, ethylamine, propylamine, etc., examples of secondary amines include dimethylamine, diethylamine, ethylmethylamine, dibutylamine, etc., and examples of tertiary amines include trimethylamine, triethylamine, tributylamine, ethyldimethylamine, ethyldiisopropylamine, etc.

[0044] Examples of the solvent include water, an organic solvent, or a mixture thereof. Examples of the protic organic solvent include monohydric alcohols, polyhydric alcohols, and oxyalcohol compounds. Examples of the monohydric alcohols include ethanol, propanol, butanol, pentanol, hexanol, cyclobutanol, cyclopentanol, cyclohexanol, and benzyl alcohol. Examples of the polyhydric alcohols and oxyalcohol compounds include alkylene oxide adducts of polyhydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, glycerin, methyl cellosolve, ethyl cellosolve, methoxypropylene glycol, dimethoxypropanol, polyglycerin, polyethylene glycol, polyoxyethylene glycerin, and polypropylene glycol.

[0045] Representative examples of aprotic organic polar solvents that serve as solvents include sulfones, amides, lactones, cyclic amides, nitriles, and sulfoxides. Examples of sulfones include dimethyl sulfone, ethyl methyl sulfone, diethyl sulfone, sulfolane, 3-methyl sulfolane, and 2,4-dimethyl sulfolane. Examples of amides include N-methylformamide, N,N-dimethylformamide, N-ethylformamide, N,N-diethylformamide, N-methylacetamide, N,N-dimethylacetamide, N-ethylacetamide, and N,N-diethylacetamide. Examples of lactones and cyclic amides include γ-butyrolactone, γ-valerolactone, δ-valerolactone, N-methyl-2-pyrrolidone, ethylene carbonate, propylene carbonate, butylene carbonate, and isobutylene carbonate. Examples of the nitriles include acetonitrile, 3-methoxypropionitrile, glutaronitrile, etc. Examples of the sulfoxides include dimethyl sulfoxide, etc.

[0046] Furthermore, other additives can be added to the electrolyte. Examples of additives include polyethylene glycol, complex compounds of boric acid and polysaccharides (mannitol, sorbitol, etc.), complex compounds of boric acid and polyhydric alcohols, boric acid esters, nitro compounds (o-nitrobenzoic acid, m-nitrobenzoic acid, p-nitrobenzoic acid, o-nitrophenol, m-nitrophenol, p-nitrophenol, etc.), and phosphoric acid esters. These may be used alone or in combination of two or more.

[0047] In addition, there are so-called hybrid types of electrolytic capacitors that use a solid electrolyte, but it is preferable that these electrolytic capacitors only have an electrolytic solution as the electrolyte. In electrolytic capacitors that only have an electrolytic solution as the electrolyte, when monocarboxylic acid and dicarboxylic acid are used as the solute of the electrolytic solution, the electrolytic capacitor tends to exhibit fluctuations in capacitance over time. In electrolytic capacitors that only have an electrolytic solution as the electrolyte, when the cathode body has a carbon layer and the electrolytic solution contains a monocarboxylic acid or a dicarboxylic acid having 8 or more carbon atoms, the suppression of fluctuations in capacitance over time of the electrolytic capacitor becomes significant.

[0048] (Separator) Examples of the separator include cellulose papers such as kraft, Manila hemp, esparto, hemp, and rayon, and mixed papers thereof; polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and derivatives thereof; polytetrafluoroethylene-based resins, polyvinylidene fluoride-based resins, vinylon-based resins, polyamide-based resins such as aliphatic polyamides, semi-aromatic polyamides, and fully aromatic polyamides; polyimide-based resins, polyethylene resins, polypropylene resins, trimethylpentene resins, polyphenylene sulfide resins, acrylic resins, and polyvinyl alcohol resins. These resins can be used alone or in combination. EXAMPLES

[0049] The electrolytic capacitor and the manufacturing method thereof will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0050] Three types of cathode bodies for electrolytic capacitors were produced. First, the three types of cathode bodies have the following in common. That is, both sides of the aluminum foil were enlarged by etching. The aluminum foil was enlarged by AC etching. In AC etching, an AC current was passed through the aluminum foil in an aqueous solution containing hydrochloric acid. As a result, spongy etching pits were formed on both sides of the aluminum foil.

[0051] For the first type of cathode, an oxide film was formed on the surface of the aluminum foil with an enlarged surface. In the chemical conversion treatment process to form the oxide film, a voltage was applied in an aqueous solution of ammonium dihydrogen phosphate. For the second type of cathode, the oxide film was not formed, and the aluminum foil with an enlarged surface was used as the second type of cathode.

[0052] For the third type of cathode, a carbon layer was laminated on the surface-expanded layer. The acid material of the carbon layer was carbon black, and the carbon layer was laminated on the surface-expanded aluminum foil by coating. After laminating the carbon layer, the cathode was pressed.

[0053] Next, these various cathode bodies were immersed in various electrolytic solutions. Each electrolytic solution had ethylene glycol as a solvent, ammonia as a cationic component of the solute, moisture, and an anionic component of the solute. The composition ratio of each electrolytic solution was also common, and the anionic component was added so that it was 64 mmol according to the valence. However, the solute species of the anionic component differed between each electrolytic solution.

[0054] The anion components of the various electrolytes are broadly classified into dicarboxylic acid, monocarboxylic acid, and aromatic. From the dicarboxylic acid group, succinic acid with 4 carbon atoms, adipic acid with 6 carbon atoms, pimelic acid with 7 carbon atoms, suberic acid with 8 carbon atoms, azelaic acid with 9 carbon atoms, t-butyl adipic acid with 10 carbon atoms, sebacic acid with 10 carbon atoms, 2-butyl octanedioic acid with 12 carbon atoms, brassylic acid with 13 carbon atoms, and 11-vinyl-8-octadecenedioic acid with 20 carbon atoms were selected. From the monocarboxylic acid group, formic acid with 1 carbon atom, pivalic acid with 5 carbon atoms, and octylic acid with 8 carbon atoms were selected. From the aromatic group, benzoic acid with 7 carbon atoms, phthalic acid with 8 carbon atoms, cumic acid also called 4-isopropylbenzoic acid with 10 carbon atoms, and t-butyl benzoic acid with 11 carbon atoms were selected.

[0055] For all combinations of each cathode body and each electrolyte, the initial foil capacitance before the cathode body was immersed in the electrolyte and the foil capacitance after the cathode body was immersed in the electrolyte and left at 105 °C for 426 hours were measured. The initial foil capacitance (μF / cm 2 ) vs. foil capacitance after 426 hours (μF / cm 2 ) was calculated as the capacity change rate (%).

[0056] The foil capacitance of the cathode body was measured as follows: 2 Two test pieces were cut out, and the two test pieces were placed facing each other and immersed in a capacitance measurement solution in a glass measurement tank, and the value measured using a capacitance meter was doubled. The capacitance measurement solution was an aqueous solution of ammonium adipate at 30°C, the capacitance meter was an LCR meter, and the measurement conditions were an AC amplitude of 0.5 Vms and a measurement frequency of 120 Hz.

[0057] The capacity change rates (%) for each of the examples and comparative examples are shown in Tables 1 to 3 below. (Table 1) TIFF2024140480000002.tif60168

[0058] (Table 2) TIFF2024140480000003.tif60168

[0059] (Table 3) TIFF2024140480000004.tif60168

[0060] Based on Tables 1 to 3, the capacity change rates of the examples and comparative examples are shown in the graphs of Figures 1 to 6. In each figure, the vertical axis represents the capacity change rate (%), and the horizontal axis represents the solute species of the electrolyte. In each figure, a group of three bars represents the same solute species, but the left bar represents a cathode body without an oxide film, the middle bar represents a cathode body with an oxide film, and the right bar represents a cathode body with a carbon layer.

[0061] Fig. 1 is a graph showing the rate of capacity change when various cathode bodies are combined with an electrolyte solution containing a dicarboxylic acid having a carbon number of 7 or less. As shown in Table 1 and Fig. 1, there is no significant difference in the rate of capacity change in the reference examples in which various cathode bodies are combined with an electrolyte solution containing a dicarboxylic acid having a carbon number of 7 or less.

[0062] On the other hand, Fig. 2 is a graph showing the rate of capacity change when various cathode bodies are combined with an electrolyte solution containing a dicarboxylic acid having 8 to 10 carbon atoms. As shown in Table 1 and Fig. 2, in the comparative example in which a cathode body without an oxide film was combined with an electrolyte solution containing a dicarboxylic acid having 8 or more carbon atoms, the rate of capacity change over time was large and the electrostatic capacitance was significantly reduced. In contrast, in the example in which a cathode body having a carbon layer was combined with an electrolyte solution containing a dicarboxylic acid having 8 or more carbon atoms, the rate of capacity change over time was smaller than that of the comparative example.

[0063] Moreover, in the comparative example in which a cathode body on which an oxide film had been formed was combined with an electrolyte solution containing suberic acid, azelaic acid, t-butyl adipic acid, and sebacic acid, the foil capacitance after being left at 105°C for 426 hours was 58.7 μF / cm, respectively. 2 , 57.8μF / cm 2 , 60.1μF / cm 2 , 59.5μF / cm 2In contrast, in the example in which a cathode body having a carbon layer was combined with an electrolyte solution containing suberic acid, azelaic acid, t-butyl adipic acid, and sebacic acid, the foil capacitance after being left at 105°C for 426 hours was 394.0 μF / cm, respectively. 2 , 437.7μF / cm 2 , 389.8μF / cm 2 , 400.5μF / cm 2 That is, the Example had a large capacitance and a small change in capacitance over time.

[0064] Furthermore, Fig. 3 is a graph showing the rate of change in capacity when various cathode bodies are combined with an electrolyte solution containing a dicarboxylic acid having 12 or more carbon atoms. As shown in Table 1 and Fig. 3, not only the comparative example in which a cathode body without an oxide film is combined with an electrolyte solution containing a dicarboxylic acid having 12 or more carbon atoms, but also the comparative example in which a cathode body with an oxide film is combined with an electrolyte solution containing a dicarboxylic acid having 12 or more carbon atoms, show a large rate of change in capacity over time, and the capacitance is significantly reduced. In contrast, in the examples in which a cathode body having a carbon layer is combined with an electrolyte solution containing a dicarboxylic acid having 12 or more carbon atoms, the change in capacitance over time is significantly suppressed compared to these comparative examples.

[0065] For the example in which a cathode body having a carbon layer was combined with an electrolyte solution containing 2-butyloctanedioic acid, brassylic acid, and 11-vinyl-8-octadecenedioic acid, the foil capacitance after being left at 105°C for 426 hours was 379.2 μF / cm, respectively. 2 , 391.8μF / cm 2 , 333.5μF / cm 2 That is, the Examples had a large capacitance and the change in capacitance over time was small. On the other hand, the foil capacitance of the Comparative Examples after being left at 105°C for 426 hours was only 0.5 to 3.8 μF / cm 2 was within the range.

[0066] 4 is a graph showing the rate of change in capacity when various cathode bodies are combined with an electrolyte solution containing a monocarboxylic acid having one carbon atom. As shown in Table 1 and FIG. 4, in the comparative example in which a cathode body without an oxide film was combined with an electrolyte solution containing a monocarboxylic acid having one carbon atom, the rate of change in capacity over time was large and the electrostatic capacitance was significantly reduced. In contrast, in the example in which a cathode body having a carbon layer was combined with an electrolyte solution containing a monocarboxylic acid having one carbon atom, the rate of change in capacity over time was smaller than in the comparative examples.

[0067] Moreover, when comparing the Comparative Example, which combines a cathode body on which an oxide film is formed and an electrolyte containing a monocarboxylic acid having a carbon number of 1, with the Example, which combines a cathode body having a carbon layer and an electrolyte containing a monocarboxylic acid having a carbon number of 1, the foil capacitance after being left at 105°C for 426 hours is 69.1 μF / cm 2 The example had a value of 456.8μF / cm 2 That is, the Example has a large capacitance and a small change in capacitance over time.

[0068] Furthermore, Fig. 5 is a graph showing the rate of change in capacity when various cathode bodies are combined with an electrolyte solution containing a monocarboxylic acid having 5 or more carbon atoms. As shown in Table 1 and Fig. 5, not only the comparative example in which a cathode body without an oxide film is combined with an electrolyte solution containing a monocarboxylic acid having 5 or more carbon atoms, but also the comparative example in which a cathode body with an oxide film is combined with an electrolyte solution containing a monocarboxylic acid having 5 or more carbon atoms, show a large rate of change in capacity over time, and the capacitance is significantly reduced. In contrast, in the examples in which a cathode body having a carbon layer is combined with an electrolyte solution containing a monocarboxylic acid having 5 or more carbon atoms, the change in capacitance over time is significantly suppressed compared to these comparative examples.

[0069] In the example in which a cathode body having a carbon layer was combined with an electrolyte solution containing pivalic acid or octylic acid, the foil capacitance after being left at 105°C for 426 hours was 293.8 μF / cm 2 , 216.8μF / cm 2That is, the Examples had a large capacitance and the change in capacitance over time was small. On the other hand, the foil capacitance of the Comparative Example after being left at 105° C. for 426 hours was only 0.1 to 0.3 μF / cm 2 was within the range.

[0070] In addition, Fig. 6 is a graph showing the capacity change rate when various cathode bodies are combined with an aromatic electrolyte. As shown in Table 1 and Fig. 6, there was no significant difference in the capacity change rate when various cathode bodies were combined with an aromatic electrolyte.

[0071] Here, the electrolytic capacitor can be regarded as a series capacitor having a foil capacitance Cp on the anode side and a foil capacitance Cn on the cathode side. Therefore, the capacitance C of the electrolytic capacitor is C = (Cp x Cn) / (Cp + Cn), and if the capacitance change rate of the cathode body is suppressed, the capacitance of the electrolytic capacitor is also suppressed.

[0072] Therefore, an electrolytic capacitor of the embodiment was prepared, which contains a cathode body having a carbon layer and 2-butyloctanedioic acid having 12 carbon atoms in the electrolyte, and the initial capacitance and the capacitance after being left at 105°C for 330 hours were measured. An anode foil with tunnel-shaped etching pits and a separator made of craft paper were used in this electrolytic capacitor. In addition to 2-butyloctanedioic acid, the electrolyte is composed of ethylene glycol, water, polyethylene glycol, p-nitrobenzyl alcohol, and ammonia. With respect to the weight of ethylene glycol, it contains 1 wt% water, 13 wt% polyethylene glycol, 1 wt% p-nitrobenzyl alcohol, 1.3 wt% ammonia, and 15 wt% 2-butyloctanedioic acid.

[0073] In addition, an electrolytic capacitor of a comparative example was produced, which had the same configuration except that the carbon layer was not formed on the cathode body.

[0074] The initial capacitance of the electrolytic capacitors of the examples and comparative examples and the capacitance after being left in a temperature environment of 105°C for 335 hours were measured. The capacitance reduction rate (%) after being left in a temperature environment of 105°C for 335 hours relative to the initial capacitance was calculated. The capacitance was measured at room temperature using an LCR meter (manufactured by NF Corporation, model number ZM2376). The measurement frequency was 120Hz, the DC bias was 1.5V, and the AC current level was a sine wave of 1.0Vms.

[0075] The measurement results are shown in Figure 7. Figure 7 is a graph showing the rate of decrease in capacitance. In Figure 7, the open circle plots show electrolytic capacitors using cathode bodies with a carbon layer, and the open triangle plots show electrolytic capacitors using cathode bodies without a carbon layer.

[0076] As shown in Figure 7, the electrolytic capacitor containing a cathode body with a carbon layer and an electrolyte containing 2-butyloctanedioic acid, which has 12 carbon atoms, exhibits suppressed fluctuations in capacitance over time. In other words, the result was the same as that of the foil capacitance when the cathode body with a carbon layer was immersed in an electrolyte containing 2-butyloctanedioic acid, which has 12 carbon atoms.

[0077] It was confirmed that the change in capacitance of an electrolytic capacitor over time is suppressed when a cathode body having a carbon layer laminated on its surface is combined with an electrolyte solution containing a monocarboxylic acid or a dicarboxylic acid having 8 or more carbon atoms. It was also confirmed that the change in capacitance of an electrolytic capacitor over time is further significantly suppressed when a cathode body having a carbon layer laminated on its surface is combined with an electrolyte solution containing a monocarboxylic acid having 5 or more carbon atoms or a dicarboxylic acid having 12 or more carbon atoms.

[0078] Next, cathode bodies having a carbon layer were prepared in various examples in which the carbon layer and the cathode foil had different shapes. First, in addition to an example in which a carbon layer was laminated on an aluminum foil with an enlarged surface by a coating method and pressed, a cathode body was prepared in an example in which the carbon layer was formed without pressing. A cathode body was also prepared in an example in which a carbon layer was laminated on an aluminum foil with an enlarged surface by a coating method and heat treatment. A cathode body was also prepared in an example in which a carbon layer was laminated on an aluminum foil with an enlarged surface by a vapor deposition method. A reference cathode body was also prepared in which a titanium layer was laminated on an aluminum foil with an enlarged surface by a vapor deposition method.

[0079] The carbon layer was deposited by sputtering, and the titanium layer was deposited by vacuum arc deposition to form a conductive layer containing titanium carbide.

[0080] The electrolyte in which each cathode body is immersed has the same composition and composition ratio. This electrolyte is composed of ethylene glycol as a solvent, 2-butyloctanedioic acid as an anion component of the solute, and ammonia and water as a cation component of the solute. For all combinations of each cathode body and each electrolyte, the initial foil capacity before the cathode body is immersed in the electrolyte and the foil capacity after the cathode body is immersed in the electrolyte and left at 105°C for 744 hours were measured. The initial foil capacity (μF / cm 2 ) vs. foil capacitance after 426 hours (μF / cm 2 ) was calculated as the capacity change rate (%).

[0081] The capacity change rate (%) for each of the examples and comparative examples is shown in Table 4 below. (Table 4) TIFF2024140480000005.tif67166

[0082] As shown in Table 4, when the carbon layer is formed by coating and pressing while forming a surface-expanding layer, the capacity change rate is 78%, meaning that the change over time is limited to 22% compared to the initial foil capacity. This is thought to be because the carbon material of the carbon layer is embedded in the surface-expanding layer. Also, when the carbon layer is formed by vapor deposition, the capacity change rate is 137%, meaning that the change over time is limited to 37% compared to the initial foil capacity.

[0083] This confirmed that when the carbon layer is a coating and pressing layer on the cathode foil, or when the carbon layer is a vapor deposition layer on the cathode foil, the fluctuation in capacitance of the electrolytic capacitor over time is suppressed.

Claims

1. An anode body; A cathode body having a carbon layer laminated on its surface; an electrolyte solution containing a monocarboxylic acid or a dicarboxylic acid having 8 or more carbon atoms; To have An electrolytic capacitor characterized by:

2. the electrolytic solution contains the monocarboxylic acid having 5 or more carbon atoms or the dicarboxylic acid having 12 or more carbon atoms; 2. The electrolytic capacitor according to claim 1 .

3. The cathode body has a cathode foil having a surface enlarging layer formed on a surface layer, The carbon layer includes a carbon material, A part of the carbon material of the carbon layer is laminated on the cathode foil and fills a part or all of the recesses, holes or voids of the surface-expanding layer; 3. The electrolytic capacitor according to claim 1 or 2,

4. the carbon layer is a pressed layer on the cathode foil or a vapor-deposited layer on the cathode foil; 4. The electrolytic capacitor according to claim 3 .

Citation Information

Patent Citations

  • Method and device for on-line monitoring DC-bus capacitor

    JP2021151182A