Electrolyte
By integrating a lithium imide salt, ionic liquid, and inorganic oxide particles, the electrolyte prevents ionic liquid outflow, maintaining conductivity and reducing resistance in batteries.
Patent Information
- Application Number
- JP2023051774
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The outflow of ionic liquid from the polymer electrolyte leads to increased resistance in batteries, which affects ionic conductivity.
Incorporating a lithium imide salt, ionic liquid, filler, and binder resin electrolyte, with bis(trifluoromethanesulfonyl)amine anion (TFSA) and inorganic oxide particles, enhances the electrolyte's ability to retain the ionic liquid, thereby reducing resistance.
The electrolyte maintains ionic conductivity by suppressing the outflow of ionic liquid, ensuring stable battery performance.
Smart Images

Figure 2024140583000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to electrolytes containing ionic liquids. [Background technology]
[0002] In recent years, development of batteries employing electrolytes containing flame-retardant ionic liquid and polymer binder resin has been progressing. For example, Patent Document 1 discloses a lithium ion conductive polymer electrolyte containing an ionic liquid, a polymer, a lithium salt, and an inorganic electrolyte, which has high ionic conductivity even at low temperatures, a high lithium ion migration rate at the interface between an electrode and an SPE (Solid Polymer Electrolyte), high thermal and electrochemical stability, and a wide voltage window (Claim 1, paragraph 0006). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-035587 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, when a polymer electrolyte containing an ionic liquid is added, the ionic liquid may flow out of the polymer, which corresponds to the outflow of the ionic liquid from the electrode. When the ionic liquid flows out of the electrode, the ionic conductivity is changed and the resistance value tends to increase.
[0005] The problem to be solved by the present disclosure is to provide an electrolyte that suppresses an increase in resistance value caused by outflow of ionic liquid from an electrode. [Means for solving the problem]
[0006] Means for solving the above problems include the following means. <1> A lithium imide salt; An ionic liquid; Filler, A binder resin, Electrolytes. <2> At least one of the lithium imide salt and the ionic liquid contains bis(trifluoromethanesulfonyl)amine anion (TFSA) as an anion species. <1> The electrolyte according to claim 1. <3> The electrolyte solution containing the lithium imide salt and the ionic liquid has a peak shift width due to SN stretching vibration of 2 cm before and after mixing with a filler, as measured by Raman spectroscopy. -1 More than 10cm -1 Below is the <2> The electrolyte according to claim 1. <4> The filler is an inorganic oxide particle, The inorganic oxide particles include at least one selected from the group consisting of SiO2, TiO2, and Al2O3. <1> ~ <3> 2. The electrolyte according to claim 1 , <5> The binder resin contains a structural unit derived from a vinylidene fluoride monomer. <1> ~ <4> 13. The electrolyte according to claim 12 . Effect of the Invention
[0007] According to the present disclosure, there is provided an electrolyte that suppresses an increase in resistance value caused by outflow of ionic liquid from an electrode. [Brief description of the drawings]
[0008] [Figure 1] 1 is a table showing the relative values of the resistance increase rate after 200 cycles with respect to the band shift of the SN stretching vibration when composited with a filler in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment that is an example of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the present invention. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples.
[0010] Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.
[0011] [Electrolytes] The electrolyte according to the present disclosure contains a lithium imide salt, an ionic liquid, a filler, and a binder resin. The electrolyte according to the present disclosure is configured so that the ionic liquid interacts with the substance in the electrolyte. Specifically, it is believed that by including a filler in the electrolyte, the filler interacts with the ionic liquid, thereby increasing the retention of the ionic liquid as a whole electrolyte. Thus, according to the present disclosure, the addition of the filler can suppress an increase in resistance value caused by the outflow of the ionic liquid from the electrode. Thus, the ionic conductivity can be maintained.
[0012] The electrolyte according to the present disclosure can be used for both positive and negative electrodes. In particular, since the electrolyte contains an ionic liquid, it is softer than an electrolyte that does not contain an ionic liquid, and is useful for a solid-state battery having an electrode (e.g., a negative electrode, more specifically, a silicon-containing negative electrode) that contains an active material that is prone to expansion and contraction.
[0013] [Lithium imide salt] The electrolyte according to the present disclosure includes a lithium imide salt. Examples of the lithium imide salt include lithium bis(trifluoromethanesulfonyl)imide (LiTFSA), lithium bis(fluorosulfonyl)imide (LiFSA), lithium difluoro(oxalato)borate (LiDFOB), and lithium bis(oxalato)borate (LiBOB). The lithium imide salt may be used alone or in combination of two or more.
[0014] Among the above, lithium bis(trifluoromethanesulfonyl)imide (or lithium bistrifluoromethanesulfonylamide, LiTFSA) is preferred. LiTFSA is preferred because it has low reactivity with solid electrolytes such as sulfides.
[0015] [Ionic liquid] The electrolyte according to the present disclosure includes an ionic liquid. Examples of the ionic liquid include N-methyl-N-propylpyrrolidinium bis(trifluoromethanesulfonyl)amide [PP13TFSA], N-methyl-N-propylpiperidinium bis(trifluoromethanesulfonyl)amide [P13TFSA], cesium bis(trifluoromethylsulfonyl)amide [CsTFSA], and N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium bis(trifluoromethanesulfonyl)amide [DEMETFSA]. One type of ionic liquid may be used alone, or two or more types may be used in combination.
[0016] Among the above, N-methyl-N-propylpiperidinium bis(trifluoromethanesulfonyl)amide [P13TFSA] is preferred. P13TFSA is preferred from the viewpoint of battery performance.
[0017] [Filler] The electrolyte according to the present disclosure includes a filler. The filler preferably interacts with the ionic liquid. Examples of the filler include inorganic oxides such as silica (SiO2), titania (TiO2), alumina (Al2O3), and magnesia (MgO); nitrides such as aluminum nitride and silicon nitride; metal hydroxides such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide; clay minerals such as mica, talc, boehmite, zeolite, apatite, and kaolin; glass materials; and cellulose nanofibers. One type of filler may be used alone, or two or more types may be used in combination.
[0018] Among the above, boehmite (Al2O3·H2O), alumina (Al2O3), and silica (SiO2) are preferred. These fillers are preferred because they are stable in quality, inexpensive, and easily available.
[0019] The average particle size of the filler is 0.01 μm or more and 3 μm or less, preferably 0.05 μm or more and 0.5 μm or less, and particularly preferably 0.1 μm or more and 0.3 μm or less. The filler may be either untreated or surface-treated (e.g., hydrophobized). Here, the average particle size means the cumulative 50% particle size from the fine particle side in the volume-based particle size distribution measured by the laser diffraction scattering method.
[0020] [Binder resin] The electrolyte according to the present disclosure includes a binder resin. Examples of the binder resin include fluororesins such as resins containing structural units derived from vinylidene fluoride monomers. For example, the binder resin may be polytetrafluoroethylene (PTFE), polyvinylene difluoride (PVdF), or a copolymer of polyvinylene difluoride and hexafluoropropylene (PVdF-HFP). The binder resin may be used alone or in combination of two or more kinds.
[0021] Among the above, a copolymer of polyvinylene difluoride and hexafluoropropylene (PVdF-HFP) is preferred, since PVdF-HFP is resistant to reduction.
[0022] [Other ingredients] The electrolyte according to the present disclosure may further contain other components as necessary within the range in which the effects of the present disclosure are achieved. Examples of the other components include sulfide solid electrolytes, oxide solid electrolytes, halide solid electrolytes, polymers or rubbers other than the binder resins, and conductive assistants (e.g., fibrous carbon materials).
[0023] The conductive assistant is not particularly limited as long as it is a normal conductive assistant that can be used in lithium ion batteries. Examples of the conductive assistant include carbon black such as acetylene black and ketjen black, and carbon materials such as vapor grown carbon fiber.
[0024] The conductive assistant is not particularly limited as long as it is a material having conductivity. For example, it may be a metal such as aluminum, stainless steel (SUS), silver, gold, copper, titanium, etc. Or it may be carbon such as graphite and carbon black (acetylene black, ketjen black, furnace black, channel black, thermal lamp black, etc.) Or it may be an alloy or metal acid thereof. The conductive assistant may be used alone or in combination of two or more kinds. Furthermore, the conductive assistant is not limited to particles, and may be a so-called filler-based conductive assistant such as carbon nanofibers and carbon nanotubes.
[0025] [Content] The concentration of the lithium imide salt is from 3 mass % to 15 mass %, preferably from 6 mass % to 12 mass %, and particularly preferably from 8 mass % to 10 mass %, based on the total mass of the electrolyte. The concentration of the ionic liquid is from 20% by mass to 60% by mass, preferably from 25% by mass to 55% by mass, and particularly preferably from 30% by mass to 50% by mass, based on the total mass of the electrolyte. The concentration of the filler is from 1 to 10% by mass, preferably from 2 to 9% by mass, and particularly preferably from 3 to 8% by mass, based on the total mass of the electrolyte. The concentration of the binder resin is from 10% by mass to 80% by mass, preferably from 20% by mass to 70% by mass, and particularly preferably from 30% by mass to 60% by mass, based on the total mass of the electrolyte.
[0026] [Raman measurements] In the electrolyte according to the present disclosure, the electrolyte solution of lithium imide salt and ionic liquid has a peak shift width due to the SN stretching vibration of TFSA before and after mixing with the filler, measured by Raman spectroscopy, of 2 cm -1 More than 10cm -1 It may be less than 4 cm. -1 Over 9cm -1 Less than 6 cm, particularly preferably -1 Over 8cm -1 The shift width of the peak due to the SN stretching vibration is 2 cm or less. -1 More than 10cm -1 It is preferable that the amount is not more than this because the interaction between the ionic liquid and the filler is more effective.
[0027] [Electrolyte manufacturing method] The method for producing the electrolyte of the present disclosure is not particularly limited, and a known method for producing an electrolyte can be applied. For example, the electrolyte of the present disclosure is produced by preparing an electrolyte solution from a lithium imide salt and an ionic liquid, and further kneading a filler to produce a composite. The composite may be mixed with a binder resin dissolved in a solvent, and the solvent may be dried to produce the electrolyte.
[0028] [battery] The battery of the present disclosure includes the electrolyte of the present disclosure. The method for manufacturing the battery is not particularly limited, and a known method for manufacturing a battery can be applied. For example, the method described in the examples can be mentioned. The battery of the present disclosure includes, for example, a positive electrode layer, a negative electrode layer, and an electrolyte layer disposed between the positive electrode layer and the negative electrode layer.
[0029] The battery of the present disclosure may be a solid-state lithium-ion secondary battery. Examples of solid-state batteries include power sources for vehicles, electronic devices, and electricity storage. Examples of vehicles include electric four-wheeled vehicles, electric two-wheeled vehicles, gasoline automobiles, and diesel automobiles. Examples of electric four-wheeled vehicles include electric vehicles (BEVs), plug-in hybrid vehicles (PHEVs), and hybrid automobiles (BEVs). Examples of electric two-wheeled vehicles include electric motorcycles and power-assisted bicycles. Examples of electronic devices include handheld devices (e.g., smartphones, tablet computers, audio players, etc.), portable devices (e.g., notebook computers, CD (Compact Disc) players, and movable devices (e.g., power tools, commercial video cameras, etc.). Among these, the battery of the present disclosure is preferably used as a driving power source for hybrid automobiles, plug-in hybrid automobiles, or electric automobiles. EXAMPLES
[0030] Examples will be described below, but the present invention is not limited to these examples. In the following examples, the batteries produced using the composites produced in Examples 1-3 and Comparative Example 1 are referred to as the batteries of Examples 1-3 and Comparative Example 1.
[0031] [Raman measurements] Example 1 P13TFSA and LiTFSA were mixed in a molar ratio of 7:3 to obtain an electrolyte. This electrolyte was weighed out so that the weight ratio was electrolyte:SiO2 = 100:15, and the mixture was uniformly kneaded in a mortar to obtain a composite of ionic liquid, lithium salt, and SiO2 filler. The SiO2 used here was AEROSIL R972 manufactured by Nippon Aerosil. The surface was hydrophobized with dimethyldichlorosilane, and the average particle size was 16 nm. Example 2 A complex was prepared in the same manner as in Example 1, except that the molar ratio of P13TFSA and LiTFSA was 7.5:2.5. Example 3 A complex was prepared in the same manner as in Example 1, except that the molar ratio of P13TFSA and LiTFSA was 8:2. Comparative Example 1 A complex was prepared in the same manner as in Example 1, except that the molar ratio of P13TFSA and LiTFSA was 6:4.
[0032] The composite and the electrolyte solution before being composited with the filler were sealed in a closed measuring cell in a glove box, and the Raman spectrum was measured. The Raman spectrum was measured using a LabRAM HR800 manufactured by Horiba, Ltd. The sample surface in the cell was measured using a laser with a wavelength of 457 nm. The peak due to SN stretching vibration (745 cm -1 The shift width before and after mixing the electrolyte and the filler was calculated using the wave number of the peak top of the electrolytic solution (around 1000 nm).
[0033] [Method of preparing polymer electrolyte] P13TFSA and LiTFSA were mixed in a specified molar ratio to obtain an electrolyte solution. This electrolyte solution was weighed out so that the weight ratio of electrolyte solution:SiO2 was 100:15, and the mixture was uniformly kneaded in a mortar to obtain a composite of ionic liquid, lithium salt, and SiO2 filler. To prepare the polymer solution, PVdF-HFP (KF8300 manufactured by Kureha) was dissolved in dimethyl carbonate at a predetermined ratio. The above complex was added to the polymer solution so that the weight ratio of PVdF-HFP:complex was 1:1, and the mixture was stirred uniformly to obtain a polymer electrolyte solution. The polymer electrolyte solution was cast onto a PP film, heated, and the dimethyl carbonate was dried to obtain the desired polymer electrolyte. All of the above operations were carried out in an Ar glove box.
[0034] [Preparation of batteries containing polymer electrolytes] Example 1 An electrolyte was obtained by mixing P13TFSA and LiTFSA in a molar ratio of 7:3. This electrolyte was weighed out so that the weight ratio of electrolyte:SiO2 was 100:15, and the mixture was uniformly kneaded in a mortar to obtain a composite of ionic liquid, lithium salt, and SiO2 filler. To prepare the polymer solution, PVdF-HFP (KF8300 manufactured by Kureha) was dissolved in dimethyl carbonate at a predetermined ratio. The above complex was added to the polymer solution so that the weight ratio of PVdF-HFP:complex was 1:1, and the mixture was stirred uniformly to obtain a polymer electrolyte solution. 1 g of porous Si and the above polymer electrolyte solution were weighed out into a mortar so that the amount of polymer electrolyte excluding the solvent was 0.1 g, and the mixture was kneaded while heating to dry the dimethyl carbonate, thereby obtaining a composite of porous Si and polymer electrolyte (Si active material granules). Example 2 A composite of porous Si and polymer electrolyte (Si active material granules) was produced in the same manner as in Example 1, except that the molar ratio of P13TFSA and LiTFSA was changed to 7.5:2.5. Example 3 A composite of porous Si and polymer electrolyte (Si active material granules) was produced in the same manner as in Example 1, except that the molar ratio of P13TFSA and LiTFSA was 8:2. Comparative Example 1 A composite of porous Si and polymer electrolyte (Si active material granules) was produced in the same manner as in Example 1, except that the molar ratio of P13TFSA and LiTFSA was 6:4.
[0035] [Preparation of positive electrode layer] A PP container is filled with butyl butyrate, a 5 wt% butyl butyrate solution of a PVDF-based binder, and LiNi with an average particle size of 6 μm as the positive electrode active material. 1 / 3 Co 1 / 3 Mn 1 / 3O2, Li2S-P2S5-based glass ceramic as a sulfide solid electrolyte, and VGCF (vapor-grown carbon fiber) as a conductive additive were added to the container and stirred for 30 seconds with an ultrasonic dispersion device (UH-50 manufactured by SMT). Next, the container was shaken for 3 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.), and further stirred for 30 seconds with the ultrasonic dispersion device. After shaking for 3 minutes with the shaker, the mixture was applied to an Al foil (manufactured by Showa Denko) using an applicator by the blade method. The coated electrodes were dried on a hot plate at 100° C. for 30 minutes. The weight ratio of the positive electrode active material to the solid electrolyte is preferably 85 / 15 to 30 / 70, and more preferably 80 / 20 to 50 / 50. The thickness of the positive electrode is preferably 1 to 100 μm, and more preferably 30 to 100 μm.
[0036] [Creation of negative electrode layer] A PP container was charged with mesitylene as a solvent, a 5 wt% mesitylene solution of SBR binder, VGCF as a conductive assistant, Li2S-P2S5 glass ceramic as a solid electrolyte, and the above-mentioned Si active material granules in a predetermined ratio, and the charged particles were stirred for 30 seconds with an ultrasonic dispersion device (UH-50, manufactured by SMT). The container was then shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.). The mixture was applied to a Cu foil (manufactured by UACJ) using an applicator by the blade method. The coated electrodes were dried on a hot plate at 100° C. for 30 minutes. The weight ratio of the negative electrode active material to the solid electrolyte is preferably 85 / 15 to 30 / 70, and more preferably 80 / 20 to 50 / 50. The thickness of the negative electrode is preferably 1 to 100 μm, and more preferably 30 to 100 μm.
[0037] [Preparation of solid electrolyte layer] Heptane, a 5 wt% heptane solution of SBR binder, and Li2S-P2S5 glass ceramic as a solid electrolyte were added to a PP container and stirred for 30 seconds with an ultrasonic disperser (UH-50 manufactured by SMT Co., Ltd.).The container was then shaken for 30 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.). The coating was applied onto an Al foil by the blade method using an applicator. The coated electrodes were dried on a hot plate at 100° C. for 30 minutes.
[0038] [Battery construction] The positive electrode layer and the first solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. in the first pressing step to obtain a positive electrode laminate. The negative electrode layer and a Cu foil as a negative electrode current collector layer were laminated in this order. This laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. in the second pressing step to obtain a negative electrode laminate. Further, the above-mentioned negative electrode laminate having an Al foil as a release sheet, an intermediate solid electrolyte layer formed on the Al foil, a second solid electrolyte layer, and a Cu foil as a negative electrode current collector layer was laminated in this order. The laminate was set in a flat uniaxial press and temporarily pressed at 100 MPa and 25°C for 10 seconds. The Al foil was peeled off from the intermediate solid electrolyte layer of the laminate to obtain a negative electrode laminate further laminated with an intermediate solid electrolyte layer. The negative electrode laminate and the positive electrode laminate were produced so that the area of the negative electrode laminate was larger than the area of the positive electrode laminate. The positive electrode laminate and the negative electrode laminate further having an intermediate solid electrolyte layer laminated thereon were laminated in this order. The laminate was set in a flat uniaxial press and pressed for 1 minute at a pressure of 200 MPa and a temperature of 120° C. in the third pressing step. A battery was thus obtained.
[0039] [Battery evaluation] The prepared cell was restrained at a predetermined restraining pressure using a restraining jig, charged at a constant current to 4.55V at 1 / 10C, discharged to 3.0V at 1C, constant current-constant voltage charged to 4.35V at 1 / 3C, constant current-constant voltage discharged to 3.35V at 1 / 3C, and then discharged at 5C for 10 seconds to measure the initial cell resistance. After that, it was discharged to 3.0V at 1C, and then a constant current charge-discharge test was repeated 200 times at 2C as a cycle test. After the cycle test, it was discharged at a constant current-constant voltage to 4.35V at 1 / 3C, constant current-constant voltage discharged to 3.35V at 1 / 3C, and then discharged at 5C for 10 seconds to measure the cell resistance.
[0040] The horizontal axis of FIG. 1 is the shift width of the band originating from the SN stretching vibration of the composites of Examples 1 to 3 and Comparative Example 1 measured by Raman spectroscopy before and after mixing with the filler. The larger the shift width of the Raman band, the stronger the interaction (trap) with the filler. The vertical axis of FIG. 1 is the resistance increase rate after 200 cycles of the batteries of Examples 1 to 3 and Comparative Example 1. The relative value of the increase rate is shown when Comparative Example 1 is taken as the standard (1). In Examples 1, 2, and 3, the content ratio of LiTFSA is decreased in this order. That is, the content ratio of P13TFSA as an ionic liquid increases. However, the width of the band shift increases in the order of Examples 1, 2, and 3. That is, it indicates that the interaction with the filler is improved. Furthermore, the result is obtained that the resistance increase rate of the battery decreases as the interaction with the filler improves.
Claims
1. A lithium imide salt; An ionic liquid; Filler and A binder resin, Electrolytes.
2. At least one of the lithium imide salt and the ionic liquid contains bis(trifluoromethanesulfonyl)amine anion (TFSA) as an anion species. The electrolyte of claim 1.
3. The electrolyte solution containing the lithium imide salt and the ionic liquid has a peak shift width due to S-N stretching vibration of 2 cm before and after mixing with a filler, as measured by Raman spectroscopy. -1 10cm or more -1 Below is the The electrolyte of claim 2.
4. The filler is an inorganic oxide particle, The inorganic oxide particles are SiO 2 , TiO 2 , and Al 2 O 3 At least one selected from the group consisting of The electrolyte according to any one of claims 1 to 3.
5. The binder resin contains a structural unit derived from a vinylidene fluoride monomer. The electrolyte according to any one of claims 1 to 3.
Citation Information
Patent Citations
Lithium ion conductive polymer electrolyte
JP2020035587A