Resin composition, molded article, and pellet
The resin composition addresses the lack of flame retardancy and mechanical strength in polybutylene terephthalate-based materials by incorporating specific acrylonitrile-styrene copolymers and glass fiber, resulting in improved flame retardancy and mechanical strength at high temperatures with reduced warpage.
Patent Information
- Application Number
- JP2023051783
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing resin compositions based on polybutylene terephthalate resin and acrylonitrile-styrene copolymers lack sufficient flame retardancy and mechanical strength, especially at high temperatures, and exhibit warpage issues.
A resin composition comprising 15 to 50 parts by mass of polybutylene terephthalate resin with an intrinsic viscosity of 0.3 to 0.75 dL/g, 50 to 85 parts by mass of styrene resin with at least 10% by mass being an acrylonitrile-styrene copolymer with a weight average molecular weight of 400,000 or less, and 5 to 100 parts by mass of glass fiber, along with a halogen flame retardant, is used to enhance flame retardancy and mechanical strength.
The composition achieves excellent flame retardancy and high mechanical strength at high temperatures, with reduced warpage and improved dimensional stability, maintaining deflection temperature under load.
Smart Images

Figure 2024140588000001 
Figure 2024140588000002 
Figure 2024140588000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a molded article, and a pellet, and in particular to a resin composition containing a polybutylene terephthalate resin and a styrene-based resin as main components. [Background technology]
[0002] Thermoplastic polyester resins, typified by polybutylene terephthalate resin and polyethylene terephthalate resin, are excellent in mechanical strength, chemical resistance, electrical insulation, and the like, and are therefore widely used in electrical and electronic equipment parts, automotive interior and exterior parts, other electrical parts, machine parts, and the like. Here, in order to improve the low warpage property, heat resistance and mechanical strength of molded articles formed from polybutylene terephthalate resin, it has been considered to blend a styrene-based resin, particularly an acrylonitrile-styrene copolymer. Specifically, Patent Document 1 discloses a thermoplastic resin composition that contains (A) 15 to 50 parts by mass of a polybutylene terephthalate resin having an intrinsic viscosity (IV) of 0.3 to 0.75 dL / g, (B) 50 to 85 parts by mass of an acrylonitrile-styrene copolymer having a weight average molecular weight (Mw) of 200,000 or more, and (C) 5 to 100 parts by mass of glass fiber, relative to a total of 100 parts by mass of (A) and (B). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-186293 A Summary of the Invention [Problem to be solved by the invention]
[0004] The resin composition has a high deflection temperature under load, small warpage, and excellent mechanical strength, but flame retardancy has not been examined. In addition, depending on the application, mechanical strength at high temperatures may be required. The present invention aims to solve the above problems, and to provide a resin composition, a molded article, and pellets that can provide a molded article having excellent flame retardancy and high mechanical strength at high temperatures. [Means for solving the problem]
[0005] In view of the above-mentioned problems, the present inventors have conducted research and found that the above-mentioned problems can be solved by using an acrylonitrile-styrene copolymer as at least a part of the styrene-based resin, and further using an acrylonitrile-styrene copolymer having a predetermined molecular weight. Specifically, the above problems were solved by the following means. <1> A resin composition comprising 15 to 50 parts by mass of a polybutylene terephthalate resin having an intrinsic viscosity (IV) of 0.3 to 0.75 dL / g, 50 to 85 parts by mass of a styrene-based resin, a total of 100 parts by mass, and further comprising 5 to 100 parts by mass of glass fiber, a flame retardant, and at least 10% by mass of the styrene-based resin being an acrylonitrile-styrene copolymer having a weight average molecular weight (Mw) of 400,000 or less. <2> The flame retardant includes a halogen-based flame retardant. <1> The resin composition according to claim 1. <3> The flame retardant comprises a brominated flame retardant. <1> The resin composition according to claim 1. <4> Further, the present invention includes a polycarbonate resin. <1> ~ <3> 10. The resin composition according to claim 9 . <5> Further, the composition contains a flame retardant synergist. <1> ~ <4> 10. The resin composition according to claim 9 . <6> The flame retardant contains a brominated flame retardant and further contains a polycarbonate resin; Further, the composition contains a flame retardant synergist. <1> ~ <5> 10. The resin composition according to claim 9 . <7> The weight average molecular weight (Mw) of the acrylonitrile-styrene copolymer is less than 350,000; <1> ~ <6> 10. The resin composition according to claim 9 . <8> The weight average molecular weight (Mw) of the acrylonitrile-styrene copolymer is less than 200,000; <1> ~ <7> 10. The resin composition according to claim 9 . <9> The flame retardant contains a halogen-based flame retardant, the flame retardant contains a bromine-based flame retardant, and further contains a polycarbonate resin and further contains a flame retardant auxiliary, and the weight average molecular weight (Mw) of the acrylonitrile-styrene copolymer is less than 200,000. <1> ~ <8> 10. The resin composition according to claim 9 . <10> The resin composition is molded into a test piece having a thickness of 1.6 mm, and when subjected to a UL-94 test, it satisfies V-0. <1> ~ <9> 10. The resin composition according to claim 9 . <11> <1> ~ <9> 2. A molded article formed from the resin composition according to claim 1. <12> <1> ~ <9> 2. A pellet of the resin composition according to claim 1. <13> <12> A molded article formed from the pellets according to claim 1. Effect of the Invention
[0006] The present invention makes it possible to provide a resin composition, a molded article, and pellets that are capable of producing a molded article having excellent flame retardancy and high mechanical strength at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Hereinafter, an embodiment of the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the present embodiment is an example for explaining the present invention, and the present invention is not limited to the present embodiment. In this specification, the use of "to" means that the numerical values before and after it are included as the lower limit and upper limit. In this specification, various physical properties and characteristic values are those at 23° C. unless otherwise specified. If the measurement methods, etc. described in the standards shown in this specification vary from year to year, they will be based on the standards as of January 1, 2022, unless otherwise stated.
[0008] The resin composition of the present embodiment contains 15 to 50 parts by mass of a polybutylene terephthalate resin having an intrinsic viscosity (IV) of 0.3 to 0.75 dL / g, 50 to 85 parts by mass of a styrene-based resin, and 5 to 100 parts by mass of glass fiber, for a total of 100 parts by mass. The resin composition further contains a flame retardant, The styrene resin is characterized in that 10% by mass or more is an acrylonitrile-styrene copolymer having a weight average molecular weight (Mw) of 400,000 or less. By adopting such a constitution, a resin composition capable of providing a molded article having excellent flame retardancy and high mechanical strength at high temperatures is obtained. Furthermore, a resin composition capable of providing a molded article having small warpage is obtained. In addition, a resin composition capable of providing a molded article having excellent dimensional stability is obtained. In addition, the deflection temperature under load can be maintained at a high level. It is presumed that a resin composition capable of providing molded articles having excellent flame retardancy and high mechanical strength at high temperatures tends to have improved mechanical properties at high temperatures by using an acrylonitrile-styrene copolymer of a specified molecular weight.
[0009] <Polybutylene terephthalate resin> The resin composition of the present embodiment contains a polybutylene terephthalate resin having an intrinsic viscosity (IV) of 0.3 to 0.75 dL / g. By using one having an intrinsic viscosity (IV) in the range of 0.3 to 0.75 dL / g, the characteristics of the polybutylene terephthalate resin are strongly exhibited, and the resin composition has excellent heat resistance and low warpage, as well as excellent mechanical strength and chemical resistance. If one having an intrinsic viscosity (IV) of less than 0.3 dL / g is used, the heat resistance of polybutylene terephthalate is not exhibited, and the mechanical strength is likely to be low. If one having an intrinsic viscosity (IV) of more than 0.75 dL / g is used, the above-mentioned sea-island structure is difficult to form, and the acrylonitrile-styrene copolymer is likely to become a sea, which reduces the fluidity of the resin composition and tends to deteriorate the moldability. The intrinsic viscosity (IV) is preferably 0.4 dL / g or more, more preferably 0.5 dL / g or more, further preferably 0.55 dL / g or more, particularly preferably 0.6 dL / g or more, and is preferably 0.72 dL / g or less.
[0010] The intrinsic viscosity is measured by the following method. Polybutylene terephthalate resin pellets are dissolved in a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (mass ratio 1 / 1) by stirring at 110°C for 1 hour to a concentration of 1.00 g / dL. The solution is then cooled to 30°C. The time it takes for the sample solution and the solvent alone to fall at 30°C is measured using a fully automatic solution viscometer, and the intrinsic viscosity is calculated using the formula: Intrinsic viscosity=((1+4K H η sp ) 0.5 -1) / (2K H C) Here, η sp = η / η0-1, where η is the time it takes for the sample solution to fall, η0 is the time it takes for the solvent alone to fall, C is the concentration of the sample solution (g / dL), and K H is Huggins' constant. K H was set to 0.33. The fully automatic solution viscometer used is a product of Shibayama Scientific Co., Ltd. When the resin composition of the present embodiment contains two or more types of polybutylene terephthalate resins, the intrinsic viscosity is the intrinsic viscosity of the mixture.
[0011] The polybutylene terephthalate resin used in the resin composition of this embodiment is a polyester resin having a structure in which terephthalic acid units and 1,4-butanediol units are ester-bonded, and includes, in addition to polybutylene terephthalate resin (homopolymer), a polybutylene terephthalate copolymer containing other copolymerization components other than terephthalic acid units and 1,4-butanediol units, and a mixture of a homopolymer and a polybutylene terephthalate copolymer.
[0012] The polybutylene terephthalate resin may contain one or more types of dicarboxylic acid units other than terephthalic acid. Specific examples of other dicarboxylic acids include aromatic dicarboxylic acids such as isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, biphenyl-2,2'-dicarboxylic acid, biphenyl-3,3'-dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, bis(4,4'-carboxyphenyl)methane, anthracenedicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and 4,4'-dicyclohexyldicarboxylic acid; and aliphatic dicarboxylic acids such as adipic acid, sebacic acid, azelaic acid, and dimer acid. In the polybutylene terephthalate resin used in this embodiment, terephthalic acid units preferably account for 80 mol % or more of all dicarboxylic acid units, more preferably 90 mol % or more, even more preferably 95 mol % or more, and may even account for 99 mol % or more.
[0013] The diol unit may contain one or more other diol units in addition to 1,4-butanediol. Specific examples of other diol units include aliphatic or alicyclic diols having 2 to 20 carbon atoms, bisphenol derivatives, etc. Specific examples include ethylene glycol, propylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, decamethylene glycol, cyclohexanedimethanol, 4,4'-dicyclohexylhydroxymethane, 4,4'-dicyclohexylhydroxypropane, ethylene oxide adduct diol of bisphenol A, etc. In addition to the above-mentioned bifunctional monomers, a small amount of a trifunctional monomer such as trimellitic acid, trimesic acid, pyromellitic acid, pentaerythritol, trimethylolpropane, etc., can be used in combination to introduce a branched structure, or a monofunctional compound such as a fatty acid, etc., can be used in combination to adjust the molecular weight. In the polybutylene terephthalate resin used in this embodiment, 1,4-butanediol units preferably account for 80 mol % or more of all diol units, more preferably 90 mol % or more, even more preferably 95 mol % or more, and may even be 99 mol % or more.
[0014] As described above, the polybutylene terephthalate resin is preferably a polybutylene terephthalate homopolymer obtained by polycondensation of terephthalic acid and 1,4-butanediol. In addition, it may be a polybutylene terephthalate copolymer containing one or more dicarboxylic acids other than the terephthalic acid as the carboxylic acid unit and / or one or more diols other than the 1,4-butanediol as the diol unit. When the polybutylene terephthalate resin is a polybutylene terephthalate resin modified by copolymerization, specific preferred copolymers include polyester ether resins copolymerized with polyalkylene glycols, particularly polytetramethylene glycol, dimer acid copolymerized polybutylene terephthalate resins, and isophthalic acid copolymerized polybutylene terephthalate resins. Among them, it is preferable to use a polyester ether resin copolymerized with polytetramethylene glycol. In addition, when the polybutylene terephthalate resin is a copolymer, the copolymerization amount is 1 mol% or more and less than 50 mol% of all polybutylene terephthalate resin units. In particular, the copolymerization amount is preferably 2 mol% or more and less than 50 mol%, more preferably 3 to 40 mol%, and further preferably 5 to 20 mol%. By setting the copolymerization ratio in this manner, it is preferable because a molded product having a small mold shrinkage rate and high impact resistance can be obtained.
[0015] The amount of terminal carboxyl groups in the polybutylene terephthalate resin may be appropriately selected and determined, but is usually 60 eq / ton or less, preferably 50 eq / ton or less, and more preferably 30 eq / ton or less. By setting it to the above upper limit or less, the alkali resistance and hydrolysis resistance tend to be improved. The lower limit of the amount of terminal carboxyl groups is not particularly set, but considering the productivity of the production of the polybutylene terephthalate resin, it is preferably 5 eq / ton or more.
[0016] The amount of terminal carboxyl groups in the polybutylene terephthalate resin is a value measured by dissolving 0.5 g of the polybutylene terephthalate resin in 25 mL of benzyl alcohol and titrating it with a 0.01 mol / L benzyl alcohol solution of sodium hydroxide. The amount of terminal carboxyl groups can be adjusted by any conventionally known method, such as adjusting the polymerization conditions such as the raw material charge ratio during polymerization, the polymerization temperature, and the pressure reduction method, or by reacting a terminal blocking agent.
[0017] Polybutylene terephthalate resin can be produced by batch or continuous melt polymerization of a dicarboxylic acid component mainly composed of terephthalic acid or an ester derivative thereof and a diol component mainly composed of 1,4-butanediol. In addition, after producing a low molecular weight polybutylene terephthalate resin by melt polymerization, the degree of polymerization (or molecular weight) can be increased to a desired value by further solid-phase polymerization under a nitrogen gas flow or reduced pressure. The polybutylene terephthalate resin is preferably one obtained by a production method in which a dicarboxylic acid component mainly composed of terephthalic acid and a diol component mainly composed of 1,4-butanediol are melt-polycondensed in a continuous or batch manner.
[0018] The catalyst used in carrying out the esterification reaction may be a conventionally known catalyst, and examples thereof include titanium compounds, tin compounds, magnesium compounds, calcium compounds, etc. Among these, titanium compounds are particularly preferred. Specific examples of titanium compounds as esterification catalysts include titanium alcoholates such as tetramethyl titanate, tetraisopropyl titanate, and tetrabutyl titanate, and titanium phenolates such as tetraphenyl titanate.
[0019] The content of the polybutylene terephthalate resin in the resin composition of the present embodiment is preferably 10% by mass or more, more preferably 15% by mass or more, and is preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less, and may be 25% by mass or less, 20% by mass or less, depending on the application.
[0020] <Styrene-based resin> The resin composition of the present embodiment contains a styrene-based resin, and 10% by mass or more of the styrene-based resin is an acrylonitrile-styrene copolymer having a weight average molecular weight (Mw) of 400,000 or less. By containing such an acrylonitrile-styrene copolymer, flame retardancy is improved, and high mechanical strength can be achieved even at high temperatures.
[0021] The styrene-based resin means that 50% by mass or more of the monomers constituting the styrene-based resin are styrene-based monomers. Examples of the styrene-based monomer include styrene, α-methylstyrene, p-methylstyrene, vinylxylene, ethylstyrene, dimethylstyrene, p-tert-butylstyrene, vinylnaphthalene, methoxystyrene, monobromostyrene, dibromostyrene, fluorostyrene, and tribromostyrene, and styrene and α-methylstyrene are more preferable, and styrene is particularly preferable. Furthermore, among the monomers constituting the styrene-based resin, examples of monomers other than the styrene-based monomers include (meth)acrylic acid ester-based monomers, maleimide-based monomers such as maleimide, N-methylmaleimide, and N-phenylmaleimide, α,β-unsaturated carboxylic acids and their anhydrides such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, phthalic acid, and itaconic acid, and rubbers such as butadiene.
[0022] In the resin composition of the present embodiment, the proportion of the acrylonitrile-styrene copolymer having a weight average molecular weight (Mw) of 400,000 or less in the styrene-based resin is 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 70% by mass or more, and may be 80% by mass or more, 90% by mass or more, or 95% by mass or more. The upper limit of the proportion of the acrylonitrile-styrene copolymer having a weight average molecular weight (Mw) of 400,000 or less in the styrene-based resin is 100% by mass or less.
[0023] The weight average molecular weight (Mw) of the acrylonitrile-styrene copolymer is preferably less than 350,000, more preferably 300,000 or less, even more preferably 250,000 or less, and even more preferably less than 200,000, and may be 160,000 or less depending on the application, etc. The lower limit of the weight average molecular weight (Mw) of the acrylonitrile-styrene copolymer is preferably 10,000 or more, more preferably 50,000 or more, and even more preferably 80,000 or more, and may be 100,000 or more depending on the application, etc. When the resin composition of the present embodiment contains two or more types of acrylonitrile-styrene copolymers, the weight average molecular weight (Mw) is the weight average molecular weight of the mixture. In the present invention, the weight average molecular weight (Mw) of the acrylonitrile-styrene copolymer can be measured by GPC (gel permeation chromatography) and calculated in terms of polystyrene.
[0024] The acrylonitrile-styrene copolymer is a copolymer of acrylonitrile and a styrene-based monomer, and may be a copolymer further copolymerized with other copolymerizable monomers.
[0025] Examples of the styrene monomer constituting the acrylonitrile-styrene copolymer include styrene, α-methylstyrene, p-methylstyrene, vinylxylene, ethylstyrene, dimethylstyrene, p-tert-butylstyrene, vinylnaphthalene, methoxystyrene, monobromostyrene, dibromostyrene, fluorostyrene, and tribromostyrene. Styrene and α-methylstyrene are more preferred, and styrene is particularly preferred.
[0026] Examples of copolymerizable monomers other than styrene-based monomers and acrylonitrile include (meth)acrylic acid ester-based monomers, maleimide-based monomers such as maleimide, N-methylmaleimide, and N-phenylmaleimide, and α,β-unsaturated carboxylic acids and anhydrides thereof such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, phthalic acid, and itaconic acid. Of these, (meth)acrylic acid ester monomers are preferred, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, amyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, phenyl (meth)acrylate, and benzyl (meth)acrylate, and in particular, methyl methacrylate. The term "(meth)acrylate" includes both methacrylate and acrylate, and the term "(meth)acrylic acid ester" includes both methacrylic acid ester and acrylic acid ester.
[0027] The method for producing the acrylonitrile-styrene copolymer is not limited, and any known method can be used, such as bulk polymerization, emulsion polymerization, solution polymerization, and suspension polymerization.
[0028] The ratio of units derived from acrylonitrile monomers in the acrylonitrile-styrene copolymer is preferably in the range of 10 to 35% by mass, more preferably 15 to 35% by mass, and even more preferably 15 to 30% by mass, and the ratio of units derived from styrene monomers is preferably 65 to 90% by mass, more preferably 65 to 85% by mass, and even more preferably 70 to 85% by mass.
[0029] In the acrylonitrile-styrene copolymer, the total of styrene monomer units and acrylonitrile monomer units preferably accounts for 90 mass % or more of the total monomer units, and in particular, an acrylonitrile-styrene resin, also called AS resin, is preferred.
[0030] <Blend ratio of polybutylene terephthalate resin and styrene resin> In this embodiment, the styrene resin (acrylonitrile-styrene copolymer) is 50 parts by mass or more, preferably 55 parts by mass or more, and more preferably 60 parts by mass or more, per 100 parts by mass of the polybutylene terephthalate resin and the styrene resin in total. By making it equal to or more than the lower limit, the low warpage property tends to be further improved. In addition, the upper limit of the content of the styrene resin is 85 parts by mass or less, preferably 80 parts by mass or less, more preferably 75 parts by mass or less, and even more preferably 70 parts by mass or less, per 100 parts by mass of the polybutylene terephthalate resin and the styrene resin in total. By making it equal to or less than the upper limit, the heat resistance tends to be further improved.
[0031] The total content of the polybutylene terephthalate resin and the styrene-based resin in the resin composition of this embodiment is preferably 35% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more, in 100% by mass of the resin composition. By making it equal to or more than the lower limit, the fluidity of the resin tends to be further improved. In addition, the total content of the polybutylene terephthalate resin and the styrene-based resin in the resin composition of this embodiment is preferably 65% by mass or less, more preferably 60% by mass or less, even more preferably 55% by mass or less, and even more preferably 50% by mass or less, in 100% by mass of the resin composition. By making it equal to or less than the upper limit, the mechanical strength tends to be further improved. In addition, the weight of the obtained molded product can be reduced.
[0032] The resin composition of the present embodiment may contain only one type of polybutylene terephthalate resin and one type of styrene-based resin, or may contain two or more types of polybutylene terephthalate resin and one or more types of styrene-based resin.
[0033] <Glass fiber> The resin composition of the present embodiment contains 5 to 100 parts by mass of glass fiber per 100 parts by mass of the total of polybutylene terephthalate resin and styrene-based resin. By containing the glass fiber, the mechanical strength of the obtained molded article is improved. The glass fibers are selected from glass compositions such as A-glass, C-glass, E-glass, R-glass, D-glass, M-glass, and S-glass, with E-glass (alkali-free glass) being particularly preferred. Glass fiber refers to a fibrous material whose cross section cut perpendicularly to the length direction has a perfect circle or polygonal shape. The number average fiber diameter of the single fiber of the glass fiber is usually 1 to 25 μm, preferably 5 to 17 μm. By making the number average fiber diameter 1 μm or more, the moldability of the resin composition tends to be improved. By making the number average fiber diameter 25 μm or less, the appearance of the obtained structure tends to be improved, and the reinforcing effect also tends to be improved. The glass fiber may be a single fiber or a plurality of single fibers twisted together. The form of the glass fiber may be any of glass rovings obtained by continuously winding single fibers or multiple twisted fibers, chopped strands cut to a length of 1 to 10 mm (i.e., glass fibers having a number average fiber length of 1 to 10 mm), milled fibers pulverized to a length of about 10 to 500 μm (i.e., glass fibers having a number average fiber length of 10 to 500 μm), etc., but chopped strands cut to a length of 1 to 10 mm are preferred. Glass fibers of different forms can also be used in combination. Glass fibers having an irregular cross-sectional shape are also preferred. The irregular cross-sectional shape has an aspect ratio, which is the long axis / short axis ratio of a cross section perpendicular to the longitudinal direction of the fiber, of, for example, 1.5 to 10, preferably 2.5 to 10, more preferably 2.5 to 8, and even more preferably 2.5 to 5.
[0034] The glass fiber may be surface-treated with, for example, a silane-based compound, an epoxy-based compound, a urethane-based compound, or the like, or may be oxidized, in order to improve its affinity with the resin component, as long as this does not significantly impair the properties of the resin composition in this embodiment.
[0035] The content of the glass fiber in the resin composition of this embodiment is 5 parts by mass or more, preferably 15 parts by mass or more, and more preferably 35 parts by mass or more, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making it equal to or more than the lower limit, there is a tendency that the rigidity and heat resistance are improved, and the effect of reducing shrinkage during molding and reducing anisotropy is further improved. In addition, the upper limit of the content of the glass fiber is 100 parts by mass or less, preferably 80 parts by mass or less, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making it equal to or less than the upper limit, there is a tendency that the surface appearance of the molded product is improved.
[0036] The content of the glass fiber in the resin composition of the present embodiment is preferably 10% by mass or more, more preferably 20% by mass or more, and is preferably 50% by mass or less, and more preferably 40% by mass or less, based on 100% by mass of the resin composition. By keeping the content below the upper limit, the surface appearance of the molded product tends to be improved. The resin composition of the present embodiment may contain only one type of glass fiber, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.
[0037] <Flame retardants> The resin composition of the present embodiment contains a flame retardant. By containing the flame retardant, flame retardancy can be achieved. Examples of flame retardants include halogen-based flame retardants, phosphorus-based flame retardants (metal phosphinate, melamine polyphosphate, etc.), nitrogen-based flame retardants (melamine cyanurate, etc.), and metal hydroxides (magnesium hydroxide, etc.). Phosphorus-based flame retardants and halogen-based flame retardants are preferred, and halogen-based flame retardants are more preferred. As phosphorus-based flame retardants, metal phosphinate is more preferred. As halogen-based flame retardants, bromine-based flame retardants are more preferred.
[0038] When a brominated flame retardant is used as the flame retardant, the type thereof is not particularly limited, but brominated phthalimide, brominated poly(meth)acrylate, brominated polycarbonate, brominated epoxy, and brominated polystyrene are preferred, brominated phthalimide, brominated polycarbonate, and brominated epoxy are more preferred, brominated phthalimide and brominated epoxy are even more preferred, and brominated phthalimide is even more preferred.
[0039] The brominated phthalimide is preferably one represented by the formula (1). [ka] (In formula (1), D represents an alkylene group, an arylene group, -S(=O)2-, -C(=O)-, and a group formed by combining two or more of -O-. i is an integer of 1 to 4.)
[0040] In formula (1), D represents a group consisting of a combination of two or more of an alkylene group, an arylene group, -S(=O)2-, -C(=O)-, and -O-. A group consisting of a combination of an alkylene group or an arylene group and at least one of -S(=O)2-, -C(=O)-, and -O- is preferable, a group consisting of a combination of an alkylene group or an arylene group and one of -S(=O)2-, -C(=O)-, and -O- is more preferable, and an alkylene group is further preferable. The group consisting of a combination of an alkylene group and -O- is intended to include, for example, a combination of two alkylene groups and one -O- (the same applies to other combinations). The alkylene group represented by D is preferably an alkylene group having 1 to 6 carbon atoms, more preferably a methylene group, an ethylene group, a propylene group, or a butylene group. The arylene group is preferably a phenylene group. "i" is an integer of 1 to 4, and is preferably 4.
[0041] Examples of the brominated phthalimide represented by formula (1) include N,N'-(bistetrabromophthalimide)ethane, N,N'-(bistetrabromophthalimide)propane, N,N'-(bistetrabromophthalimide)butane, N,N'-(bistetrabromophthalimide)diethyl ether, N,N'-(bistetrabromophthalimide)dipropyl ether, N,N'-(bistetrabromophthalimide)dibutyl ether, N,N'-(bistetrabromophthalimide)diphenyl sulfone, N,N'-(bistetrabromophthalimide)diphenyl ketone, and N,N'-(bistetrabromophthalimide)diphenyl ether.
[0042] The brominated phthalimide represented by formula (1) is preferably a brominated phthalimide represented by formula (2). [ka] (In formula (2), i is an integer of 1 to 4.) "i" is an integer of 1 to 4, and is preferably 4.
[0043] The brominated poly(meth)acrylate is preferably a polymer obtained by polymerizing a bromine atom-containing benzyl (meth)acrylate alone, copolymerizing two or more kinds of the bromine atom-containing benzyl (meth)acrylate, or copolymerizing the bromine atom with another vinyl monomer, and the bromine atoms are added to a benzene ring with 1 to 5 bromine atoms, preferably 4 to 5 bromine atoms, added per benzene ring.
[0044] Examples of the benzyl acrylate containing a bromine atom include pentabromobenzyl acrylate, tetrabromobenzyl acrylate, tribromobenzyl acrylate, and mixtures thereof. Examples of the benzyl methacrylate containing a bromine atom include methacrylates corresponding to the above-mentioned acrylates.
[0045] Specific examples of other vinyl monomers that can be copolymerized with the bromine atom-containing benzyl (meth)acrylate include acrylic acid, methyl acrylate, ethyl acrylate, butyl acrylate, and benzyl acrylate; methacrylic acid, methyl methacrylate, ethyl methacrylate, butyl methacrylate, and benzyl methacrylate; unsaturated carboxylic acids or anhydrides thereof, such as styrene, acrylonitrile, fumaric acid, and maleic acid; vinyl acetate, and vinyl chloride.
[0046] These are usually used in an equimolar amount or less, particularly preferably 0.5 times the molar amount or less, relative to the bromine atom-containing benzyl (meth)acrylate.
[0047] Furthermore, examples of vinyl monomers that can be used include xylylene diacrylate, xylylene dimethacrylate, tetrabromo xylylene diacrylate, tetrabromo xylylene dimethacrylate, butadiene, isoprene, and divinylbenzene. These can usually be used in an amount of 0.5 or less by mole relative to the bromine atom-containing benzyl acrylate or benzyl methacrylate.
[0048] The brominated poly(meth)acrylate is preferably a polymer obtained by polymerizing a bromine atom-containing (meth)acrylate monomer, particularly benzyl (meth)acrylate, alone or by copolymerizing two or more kinds of the monomers, or by copolymerizing the monomers with other vinyl monomers. The bromine atoms are added to the benzene ring, and the number of added bromine atoms is preferably 1 to 5, more preferably 4 to 5, per benzene ring.
[0049] As the brominated poly(meth)acrylate, pentabromobenzyl poly(meth)acrylate is preferred due to its high bromine content.
[0050] The molecular weight of the brominated poly(meth)acrylate is arbitrary and may be appropriately selected and determined, but the weight average molecular weight (Mw) is preferably 3,000 or more, more preferably 10,000 or more, even more preferably 15,000 or more, even more preferably 20,000 or more, and even more preferably 25,000 or more. By making it equal to or greater than the lower limit, a molded product having higher mechanical strength tends to be obtained. In addition, the upper limit of the weight average molecular weight (Mw) is preferably equal to or less than 100,000, more preferably equal to or less than 80,000, even more preferably equal to or less than 60,000, even more preferably equal to or less than 50,000, and even more preferably equal to or less than 35,000. By making it equal to or less than the upper limit, the flowability of the resin composition tends to be further improved.
[0051] The brominated polycarbonate preferably has a free bromine content of 0.05% by mass or more, and preferably 0.20% by mass or less. By setting the content within such a range, the heat resistance stability of the resin composition tends to be further improved. The brominated polycarbonate also preferably has a chlorine atom content of 0.001% by mass or more, and preferably 0.20% by mass or less. By setting the content within such a range, the mold corrosion resistance during molding tends to be further improved. Specifically, the brominated polycarbonate is preferably a brominated polycarbonate obtained from, for example, brominated bisphenol A, particularly tetrabromobisphenol A. Examples of the terminal structure include a phenyl group, a 4-t-butylphenyl group, and a 2,4,6-tribromophenyl group, and in particular, one having a 2,4,6-tribromophenyl group in the terminal group structure is preferred.
[0052] The average number of carbonate constituent units in the brominated polycarbonate may be appropriately selected and determined, but is preferably 2-30, more preferably 3-15, and even more preferably 3-10.
[0053] The molecular weight of the brominated polycarbonate is optional and may be appropriately selected and determined, but it is preferably from 1,000 to 20,000, more preferably from 2,000 to 10,000, in terms of viscosity average molecular weight.
[0054] The brominated polycarbonate obtained from the above brominated bisphenol A can be obtained, for example, by a conventional method of reacting brominated bisphenol with phosgene. The end-capping agent includes an aromatic monohydroxy compound, which may be substituted with a halogen or an organic group.
[0055] Specific preferred examples of the brominated epoxy include bisphenol A type brominated epoxy compounds, such as tetrabromobisphenol A epoxy compounds and glycidyl brominated bisphenol A epoxy compounds.
[0056] The molecular weight of the brominated epoxy compound is arbitrary and may be appropriately selected and determined, but the weight average molecular weight (Mw) is preferably 3,000 or more, more preferably 10,000 or more, even more preferably 13,000 or more, even more preferably 15,000 or more, and even more preferably 18,000 or more. By making it equal to or more than the lower limit, a molded product having higher mechanical strength tends to be obtained. In addition, the upper limit of the weight average molecular weight (Mw) is preferably 100,000 or less, more preferably 80,000 or less, even more preferably 78,000 or less, even more preferably 75,000 or less, even more preferably 70,000 or less, and may be 50,000 or less, 30,000 or less, or 25,000 or less. By making it equal to or less than the upper limit, the flowability of the resin composition tends to be further improved. The brominated epoxy compound preferably has an epoxy equivalent of 3,000 to 40,000 g / eq, more preferably 4,000 to 35,000 g / eq, and particularly preferably 10,000 to 30,000 g / eq.
[0057] In addition, a brominated epoxy oligomer can be used in combination as the brominated epoxy. In this case, for example, by using an oligomer having Mw of 5,000 or less at a ratio of about 50 mass% or less, the flame retardancy, releasability, and flowability can be appropriately adjusted. The bromine atom content in the brominated epoxy compound is arbitrary, but in order to impart sufficient flame retardancy, it is usually 10 mass% or more, preferably 20 mass% or more, and particularly preferably 30 mass% or more, with the upper limit being 60 mass%, and preferably 55 mass% or less.
[0058] The brominated polystyrene preferably includes a brominated polystyrene containing a constitutional unit represented by the formula (3). [ka] (In formula (3), t is an integer of 1 to 5, and n is the number of constitutional units.)
[0059] Brominated polystyrene may be produced by brominating polystyrene or by polymerizing brominated styrene monomer, but the polymerized brominated styrene has a smaller amount of free bromine (atoms), and is therefore preferred. In formula (3), the CH group to which the brominated benzene is bonded may be substituted with a methyl group. Brominated polystyrene may also be a copolymer in which other vinyl monomers are copolymerized. Examples of the vinyl monomer in this case include styrene, α-methylstyrene, (meth)acrylonitrile, (meth)methyl acrylate, butadiene, and vinyl acetate. Brominated polystyrene may be used alone or as a mixture of two or more types with different structures, and may contain units derived from styrene monomers with different bromine numbers in a single molecular chain.
[0060] Specific examples of brominated polystyrene include poly(4-bromostyrene), poly(2-bromostyrene), poly(3-bromostyrene), poly(2,4-dibromostyrene), poly(2,6-dibromostyrene), poly(2,5-dibromostyrene), poly(3,5-dibromostyrene), poly(2,4,6-tribromostyrene), poly(2,4,5-tribromostyrene), poly(2,3,5-tribromostyrene), and poly(4-bromo-α-methylstyrene). Examples of suitable styrene copolymers include poly(2,4-dibromostyrene), poly(2,5-dibromo-α-methylstyrene), poly(2,4,6-tribromo-α-methylstyrene) and poly(2,4,5-tribromo-α-methylstyrene), of which poly(2,4,6-tribromostyrene), poly(2,4,5-tribromostyrene) and polydibromostyrene and polytribromostyrene containing an average of 2 to 3 bromine groups in the benzene ring are particularly preferred.
[0061] The number n (average degree of polymerization) of the constituent units in the formula (3) of the brominated polystyrene is preferably 30 to 1,500, more preferably 150 to 1,000, and particularly preferably 300 to 800. If the average degree of polymerization is less than 30, blooming is likely to occur, while if it exceeds 1,500, poor dispersion is likely to occur and mechanical properties are likely to deteriorate. The weight-average molecular weight (Mw) of the brominated polystyrene is preferably 5,000 to 500,000, more preferably 10,000 to 500,000, even more preferably 10,000 to 300,000, even more preferably 10,000 to 100,000, and even more preferably 10,000 to 70,000. In particular, in the case of the above-mentioned brominated polystyrene, the weight average molecular weight (Mw) is preferably 50,000 to 70,000, and in the case of brominated polystyrene by polymerization method, the weight average molecular weight (Mw) is preferably about 10,000 to 30,000. The weight average molecular weight (Mw) can be determined as a value converted into standard polystyrene by GPC measurement.
[0062] The bromine concentration in the bromine-based flame retardant is preferably 45% by mass or more, more preferably 48% by mass or more, and even more preferably 50% by mass or more. By making it equal to or more than the lower limit, the flame retardancy of the molded article tends to be effectively improved. The upper limit of the bromine concentration is preferably 75% by mass or less, more preferably 73% by mass or less, even more preferably 71% by mass or less, and may be 65% by mass or less.
[0063] When a metal phosphinate is used as a flame retardant, the type is not particularly limited, but it is preferable that the metal phosphinate has an anion portion represented by formula (4) or formula (5) and a metal ion of the cation portion is any one of calcium, magnesium, aluminum, and zinc.
[0064] [ka] (In the formula, R 1and R 2 each independently represents an alkyl group having 1 to 6 carbon atoms or an aryl group which may have a substituent; R 1 may be the same or different, R 3 represents an alkylene group having 2 to 10 carbon atoms, an arylene group which may have a substituent, or a group consisting of a combination thereof; R 3 may be the same or different, and n represents an integer of 0 to 2.) The aryl group which may have a substituent is preferably a phenyl group which may have a substituent. When it has a substituent, it is preferably an alkyl group having 1 to 3 carbon atoms. It is also preferably unsubstituted. The arylene group which may have a substituent is preferably a phenylene group which may have a substituent. The arylene group which may have a substituent is preferably unsubstituted or has an alkyl group having 1 to 3 carbon atoms (preferably a methyl group) as a substituent. In this embodiment, a metal phosphinate represented by formula (5) is preferred. Also, in this embodiment, aluminum phosphinate is preferred.
[0065] Specific examples of the metal phosphinate include calcium dimethylphosphinate, magnesium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethylmethylphosphinate, magnesium ethylmethylphosphinate, aluminum ethylmethylphosphinate, zinc ethylmethylphosphinate, calcium diethylphosphinate, magnesium diethylphosphinate, aluminum diethylphosphinate, zinc diethylphosphinate, calcium methyl-n-propylphosphinate, magnesium methyl-n-propylphosphinate, aluminum methyl-n-propylphosphinate, zinc methyl-n-propylphosphinate, and calcium methanedi(methylphosphinate). Examples of such compounds include magnesium methane di(methylphosphinate), aluminum methane bis(methylphosphinate), zinc methane bis(methylphosphinate), calcium benzene-1,4-bis(methylphosphinate), magnesium benzene-1,4-bis(methylphosphinate), aluminum benzene-1,4-bis(methylphosphinate), zinc benzene-1,4-bis(methylphosphinate), calcium methylphenylphosphinate, magnesium methylphenylphosphinate, aluminum methylphenylphosphinate, zinc methylphenylphosphinate, calcium diphenylphosphinate, magnesium diphenylphosphinate, aluminum diphenylphosphinate, and zinc diphenylphosphinate. For details about the metal phosphinate, reference can be made to paragraphs 0052 to 0058 of WO 2010 / 010669, the contents of which are incorporated herein by reference.
[0066] The content of the flame retardant (preferably a bromine-based flame retardant) in the resin composition of this embodiment is preferably 1 part by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, even more preferably 7 parts by mass or more, even more preferably 10 parts by mass or more, and even more preferably 14 parts by mass or more, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making it equal to or more than the lower limit, the flame retardancy of the molded article obtained tends to be further improved. The upper limit of the content of the flame retardant is preferably 40 parts by mass or less, more preferably 35 parts by mass or less, even more preferably 30 parts by mass or less, even more preferably 25 parts by mass or less, even more preferably 22 parts by mass or less, even more preferably 20 parts by mass or less, and may be 19 parts by mass or less, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making it equal to or less than the upper limit, the decrease in mechanical strength of the molded article obtained can be more effectively suppressed. The resin composition of the present embodiment may contain only one type of flame retardant, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0067] <Flame retardant synergist> The resin composition of the present embodiment may contain a flame retardant assistant. By containing the flame retardant assistant, the flame retardancy of the molded article can be further improved. The flame retardant assistant is particularly preferably used when a halogen-based flame retardant is contained. The flame retardant assistant used in the present embodiment is exemplified by antimony compounds, such as antimony trioxide (Sb2O3), antimony pentoxide (Sb2O5), and sodium antimonate. In particular, antimony oxide, and particularly antimony trioxide, is preferred from the viewpoint of impact resistance. When a flame retardant auxiliary is blended, it may be blended as a master batch. The content of the antimony compound in the master batch is preferably 30 to 90 mass %, more preferably 40 to 85 mass %, and further preferably 50 to 85 mass %. The resin used in the master batch is preferably a polyester resin, more preferably a polybutylene terephthalate resin.
[0068] When the resin composition of the present embodiment contains a flame retardant auxiliary (for example, an antimony compound), the content is preferably 0.1 parts by mass or more, more preferably 1.0 parts by mass or more, even more preferably 2.0 parts by mass or more, and even more preferably 3.0 parts by mass or more, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making the content equal to or more than the lower limit, the flame retardancy tends to be more effectively exhibited. In addition, the upper limit of the content of the antimony compound is preferably 20.0 parts by mass or less, more preferably 15.0 parts by mass or less, and even more preferably 10.0 parts by mass or less, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making the content equal to or less than the upper limit, the mold release property and impact resistance of the obtained molded product tend to be improved. The resin composition of the present embodiment may contain only one type of flame retardant auxiliary, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0069] <Anti-drip agent> The resin composition of the present embodiment may contain an anti-dripping agent. As the anti-dripping agent, polytetrafluoroethylene (PTFE) is preferable, which has a fibril-forming ability, is easily dispersed in the resin composition, and tends to bond resins together to form a fibrous material. The content of the anti-dripping agent is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making the content of the anti-dripping agent 0.1 parts by mass or more, the flame retardancy effect is more sufficient, and by making it 20 parts by mass or less, the appearance of the obtained molded article tends to be improved. The content of the anti-dripping agent is more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. The resin composition of the present embodiment may contain only one type of anti-dripping agent, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0070] <Polycarbonate resin> The resin composition of the present embodiment may contain a polycarbonate resin. In the present embodiment, the polycarbonate resin functions as a compatibilizer between the polybutylene terephthalate resin and the styrene-based resin. Therefore, when the resin composition of the present embodiment contains another compatibilizer, the polycarbonate resin is not necessarily an essential component. In this specification, brominated polycarbonate is referred to as a flame retardant. Polycarbonate resins are homopolymers or copolymers, which may be branched, obtained by reacting a dihydroxy compound or a small amount of a polyhydroxy compound with phosgene or a carbonic acid diester. The method for producing the polycarbonate resin is not particularly limited, and polycarbonate resins produced by the conventionally known phosgene method (interfacial polymerization method) or melting method (ester exchange method) can be used.
[0071] The dihydroxy compound as the raw material is preferably an aromatic dihydroxy compound, more preferably bisphenol, further preferably 2,2-bis(4-hydroxyphenyl)propane (=bisphenol A), tetramethylbisphenol A, bis(4-hydroxyphenyl)-p-diisopropylbenzene, hydroquinone, resorcinol, 4,4-dihydroxydiphenyl, etc., and even more preferably bisphenol A. Also usable are compounds in which one or more tetraalkylphosphonium sulfonates are bonded to the above aromatic dihydroxy compounds.
[0072] As the polycarbonate resin, among the above, aromatic polycarbonate resin (bisphenol A type polycarbonate resin) derived from 2,2-bis(4-hydroxyphenyl)propane, or aromatic polycarbonate copolymer derived from 2,2-bis(4-hydroxyphenyl)propane and other aromatic dihydroxy compounds is preferable. In addition, it may be a copolymer mainly composed of aromatic polycarbonate resin, such as a copolymer with a polymer or oligomer having a siloxane structure. Furthermore, two or more of the above polycarbonate resins may be mixed and used.
[0073] In order to adjust the molecular weight of the polycarbonate resin, a monovalent aromatic hydroxy compound may be used, such as m- and p-methylphenol, m- and p-propylphenol, p-tert-butylphenol, p-long-chain alkyl-substituted phenol, and the like.
[0074] The viscosity average molecular weight (Mv) of the polycarbonate resin is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 13,000 or more. By using a polycarbonate resin having a viscosity average molecular weight of 5,000 or more, the mechanical strength of the resulting resin composition tends to be improved. In addition, the viscosity average molecular weight (Mv) of the polycarbonate resin is preferably 60,000 or less, more preferably 40,000 or less, and even more preferably 30,000 or less. By using a polycarbonate resin having a viscosity average molecular weight of 60,000 or less, the flowability of the resin composition tends to be improved, and the moldability tends to be improved. When two or more types of polycarbonate resins are contained, it is preferable that the mixture satisfies the above range.
[0075] In this embodiment, the viscosity average molecular weight (Mv) of the polycarbonate resin is a value calculated from the intrinsic viscosity ([η]) of a methylene chloride solution of the polycarbonate resin measured at 20° C. using an Ubbelohde viscometer, and the intrinsic viscosity calculated from the following Schnell viscosity formula. [η]=1.23×10 -4 Mv0.83
[0076] The melt volume rate (MVR) of polycarbonate resin, measured in accordance with JIS K7210 (temperature 300°C, load 1.2 kgf), is usually 1 cm 3 / 10 minutes or more, 3cm 3 / 10 minutes or more is preferable, 10cm 3 / 10 minutes or more is preferable, and 20 cm 3 / 10 minutes or more is more preferable, and 30 cm 3 / 10 minutes or more is more preferable, and 40 cm 3 / 10 minutes or more is more preferable, 50 cm 3 / 10 minutes or more is even more preferable, and 55 cm 3 It is even more preferable that the MFR is 100 cm3 or more. By setting the MFR to the lower limit or more, the flowability of the obtained resin composition or molded article tends to be improved. In addition, the upper limit of the MFR is, for example, 100 cm3 or more. 3 / 10 minutes or less, and even 80 cm 3 / 10 minutes or less is acceptable.
[0077] The method for producing the polycarbonate resin is not particularly limited, and polycarbonate resins produced by either the phosgene method (interfacial polymerization method) or the melting method (ester exchange method) can be used. In addition, polycarbonate resins produced by the melting method and then subjected to post-treatment to adjust the amount of OH groups at the terminals are also preferred.
[0078] The polycarbonate resin may be a recycled product. Even if a recycled product is used as the polycarbonate resin, the same performance as that of a virgin polycarbonate resin can be achieved.
[0079] In addition, the content of the polycarbonate resin is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making it equal to or more than the lower limit, the compatibility with the polybutylene terephthalate resin and the styrene-based resin is improved, and the mechanical strength of the obtained molded body tends to be improved. In addition, the content of the polycarbonate resin is preferably 25 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making it equal to or less than the upper limit, the heat resistance of the obtained molded body tends to be maintained at a high level. The resin composition of the present embodiment may contain only one type of polycarbonate resin, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0080] <Other ingredients> The resin composition of the present embodiment may contain other components in addition to the above-mentioned components as necessary, as long as the desired physical properties are not significantly impaired. The other components may be contained alone or in any combination and ratio of two or more. Specific examples of resin additives include stabilizers (heat stabilizers, light stabilizers), release agents, colorants (pigments, dyes), nucleating agents, reactive compounds, antistatic agents, antifogging agents, antiblocking agents, flow improvers, plasticizers, dispersants, and antibacterial agents. The total amount of these other components is preferably 10% by mass or less, and more preferably 5% by mass or less, based on 100% by mass of the resin composition. In the resin composition of the present embodiment, the total amount of the polybutylene terephthalate resin, the styrene-based resin, the flame retardant, the glass fiber, and any other components blended as required is 100 mass %.
[0081] <<Stabilizer>> The resin composition of the present embodiment may contain a stabilizer (a light stabilizer and / or a heat stabilizer). Examples of the stabilizer include hindered phenol compounds, hindered amine compounds, phosphorus compounds, and sulfur stabilizers, and hindered phenol compounds and phosphorus compounds are preferred. In this embodiment, it is also preferred to use a hindered phenol compound, a phosphorus compound, and a sulfur stabilizer in combination. By using three types of stabilizers in combination in this way, the thermal stability is further improved and tends to continue for a long period of time. As the stabilizer, specifically, the description in paragraphs 0067 to 0075 of JP 2021-063196 A, the description in paragraphs 0046 to 0057 of JP 2018-070722 A, the description in paragraphs 0030 to 0037 of JP 2019-056035 A, and the description in paragraphs 0066 to 0078 of WO 2017 / 038949 can be referred to, the contents of which are incorporated herein by reference.
[0082] The melting point of the stabilizer used in this embodiment is preferably 50 to 140°C.
[0083] When the resin composition of the present embodiment contains a stabilizer, the content is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making the content equal to or more than the lower limit, the effect of suppressing thermal degradation and oxidative degradation of the resin during melt kneading, molding, and use as a molded product tends to be improved. In addition, the upper limit of the content of the stabilizer is preferably 2.0 parts by mass or less, more preferably 1.5 parts by mass or less, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making the content equal to or less than the upper limit, adverse effects on appearance and physical properties due to aggregation of additives such as stabilizers can be effectively suppressed. The resin composition of the present embodiment may contain only one type of stabilizer, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0084] <<Release agent>> The resin composition of the present embodiment may contain a release agent. Examples of the release agent include Montan acid ester wax, polyolefin wax, higher fatty acid, ester compound, ethylene bisstearamide, etc., and at least one selected from Montan acid ester wax, polyolefin wax, synthetic wax, and ethylene bisstearamide is preferable, and Montan acid ester wax is more preferable. For details of the release agent, see paragraphs 0063 to 0077 of JP 2018-070722 A and paragraphs 0090 to 0098 of JP 2019-123809 A, the contents of which are incorporated herein by reference.
[0085] The melting point of the release agent used in this embodiment is preferably 50 to 140°C.
[0086] When the resin composition of the present embodiment contains a mold release agent, the content is preferably 0.01 parts by mass or more, more preferably 0.08 parts by mass or more, relative to 100 parts by mass of the polybutylene terephthalate resin and the styrene-based resin in total. By making the content equal to or more than the lower limit, the mold releasability during molding tends to be improved. In addition, the upper limit of the content of the mold release agent is preferably 5.0 parts by mass or less, more preferably 12.0 parts by mass or less, relative to 100 parts by mass of the polybutylene terephthalate resin and the styrene-based resin in total. By making the content equal to or less than the upper limit, the decrease in hydrolysis resistance is suppressed, and mold contamination and outgassing during injection molding tend to be reduced. The resin composition of the present embodiment may contain only one type of release agent, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0087] <<Coloring agent>> The resin composition of the present embodiment may contain a colorant (dye and / or pigment). The colorant may be either a dye or a pigment, with the pigment being preferred. The colorant may be either an organic colorant or an inorganic colorant, and may be either a chromatic colorant or an achromatic colorant. Examples of colorants include those described in paragraphs 0121 to 0123 of JP 2021-101020 A and paragraphs 0088 to 0090 of JP 2019-188393 A, the contents of which are incorporated herein by reference. The resin composition of the present embodiment preferably contains carbon black. The carbon black is not limited in type, raw material type, or production method, and any of furnace black, channel black, acetylene black, ketjen black, etc. can be used. Among them, furnace black is preferable. There is no particular limit to the number average particle size, but it is preferably about 5 to 60 nm.
[0088] DBP oil absorption of carbon black (unit: cm 3 / 100g) is 40~300cm 3 / 100g. The upper limit is preferably 300 cm 3 / 100g or less is preferable, and 200cm 3 / 100g or less is more preferable, and 150cm 3 More preferably, the weight is 100g or less. 3 The lower limit may be 40 cm / 100 g or less. 3 / 100g or more is preferable, 50cm 3 / 100g or more is preferable, 60cm 3 By keeping the value within the upper and lower limits, the appearance of the molded product tends to be improved. 3 / 100g) can be measured in accordance with JIS K6217. The number average particle size of carbon black is preferably 5 to 60 nm. The upper limit is preferably 60 nm or less, more preferably 40 nm or less, even more preferably 30 nm or less, and even more preferably 25 nm or less. The lower limit is preferably 10 nm or more, more preferably 13 nm or more, even more preferably 16 nm or more, and even more preferably 19 nm or more. By keeping the upper and lower limits, the appearance of the molded product tends to be improved. The number average particle size can be obtained by obtaining an aggregate enlarged image according to the procedure described in the ASTM D3849 standard (Standard Test Method for Carbon Black-Morphological Characterization by Electron Microscopy), measuring the particle sizes of 3,000 unit constituent particles from this aggregate image, and taking the arithmetic average.
[0089] Carbon black is mixed in advance with a thermoplastic resin, preferably a polyester resin such as polybutylene terephthalate resin, or a styrene-based resin, to prepare a master batch, which tends to increase the dispersibility of the carbon black and improve the appearance of the molded product. The concentration of carbon black in the master batch is preferably 10 to 40% by mass.
[0090] When the resin composition of the present embodiment contains a colorant (preferably carbon black), the content is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, and even more preferably 0.5 parts by mass or more, per 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making the content equal to or more than the lower limit, the coloring effect is more effectively exhibited. In addition, the upper limit of the content of the colorant is preferably 4 parts by mass or less, per 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By making the content equal to or less than the upper limit, the mechanical strength of the obtained molded product tends to be further improved. The resin composition of the present embodiment may contain only one type of colorant, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0091] <<Nucleating agent>> The resin composition of the present embodiment may contain a nucleating agent in order to adjust the crystallization rate. The type of nucleating agent is not particularly limited, but may be an inorganic nucleating agent or an organic nucleating agent, and an inorganic nucleating agent is more preferable. Examples of inorganic nucleating agents include talc, boron nitride, mica, kaolin, barium sulfate, sodium phosphate, silicon nitride, and molybdenum disulfide. Among these, talc, barium sulfate, sodium phosphate, and boron nitride are preferred, and talc is more preferred because it tends to increase the rigidity of the resin composition.
[0092] As the organic nucleating agent, an organic alkali metal salt is preferable, an alkali metal salt of an aromatic carboxylic acid or a fatty acid is more preferable, and an alkali metal salt of a fatty acid (preferably a fatty acid having 5 to 50 carbon atoms) (preferably a sodium salt or a potassium salt, more preferably a sodium salt) is further preferable. Specific examples of the organic nucleating agent include ionomer, sodium benzoate, sodium palmitate, sodium stearate, sodium behenate, and sodium montanate, among which sodium stearate, sodium behenate, and sodium montanate are more preferable, and sodium montanate is even more preferable because the resin composition tends to have a good balance between rigidity and toughness. The acid value of the nucleating agent used in this embodiment is preferably 10 mg / 1 g-KOH or less, and is preferably 0 mg / 1 g-KOH or more. The acid value is measured in accordance with JIS K 0070-1992.
[0093] When the resin composition of the present embodiment contains a nucleating agent, the content thereof is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin, and depending on the application, for example, in applications where releasability is particularly required, it is even more preferably 0.15 parts by mass or more, and may be 0.2 parts by mass or more. By making the content equal to or more than the lower limit, the releasability and mechanical strength of the molded article tend to be improved. The upper limit of the content is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 6 parts by mass or less, and even more preferably 4 parts by mass or less, relative to 100 parts by mass of the total of the polybutylene terephthalate resin and the styrene-based resin. By setting the content below the upper limit, the decomposition of the composition is suppressed, and the mechanical strength tends to be improved. In addition, the strength retention rate after a wet heat test tends to be high.
[0094] <Physical properties of resin composition> The resin composition of the present embodiment preferably has excellent flame retardancy. For example, when the resin composition is molded into a test piece having a thickness of 1.6 mm and subjected to a UL-94 test, it preferably satisfies V-0. Flame retardancy is measured as described in the Examples section below.
[0095] <Method of producing resin composition> The resin composition of this embodiment can be produced by a conventional method for preparing a resin composition. Usually, each component and various additives added as desired are mixed together thoroughly, and then melt-kneaded in a single-screw or twin-screw extruder. Alternatively, the resin composition of this embodiment can be prepared without premixing each component, or by premixing only a portion of each component, feeding the mixture to an extruder using a feeder, and melt-kneading the mixture. A portion of the components, such as a colorant, may be melt-kneaded with a thermoplastic resin to prepare a master batch, and then the remaining components may be blended therewith and melt-kneaded. The glass fibers are preferably fed from a side feeder midway through the cylinder of the extruder. The heating temperature during melt kneading can be appropriately selected from the range of 220 to 300°C. If the temperature is too high, decomposition gas is likely to be generated, which may cause opacity. Therefore, it is desirable to select a screw configuration that takes into consideration shear heat generation, etc. In order to suppress decomposition during kneading and molding in the subsequent process, it is desirable to use an antioxidant or heat stabilizer.
[0096] <Method of manufacturing molded products> The resin composition of the present embodiment is molded according to a known method. The manufacturing method of the molded product is not particularly limited, and any molding method generally used for resin compositions can be used. Examples of such molding methods include injection molding, ultra-high speed injection molding, injection compression molding, two-color molding, gas-assisted hollow molding, molding using a heat-insulating mold, molding using a rapid heating mold, foam molding (including supercritical fluid), insert molding, IMC (in-mold coating molding), extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, blow molding, etc., and among these, injection molding is preferred. For details of the injection molding method, refer to paragraphs 0113 to 0116 of Japanese Patent No. 6183822, the contents of which are incorporated herein by reference. The mold temperature during molding such as injection molding is preferably 40 to 150°C.
[0097] <Application> The resin composition of the present embodiment is used as pellets or molded articles formed from the resin composition. The use of the resin composition (pellets or molded articles) is not particularly limited, but is preferably for vehicle parts or electric / electronic parts. Vehicle parts include lamp housings, reflectors, bezels, extensions, connectors, ECU cases, housings for in-vehicle cameras and millimeter-wave radars, battery cases, and sensor housings. Examples of electric and electronic components include various housings, display devices such as computers, game consoles and televisions, printers, copy machines, scanners, fax machines, electronic organizers and PDAs, electronic desk calculators, electronic dictionaries, cameras, video cameras, mobile phones, battery packs, drives and readers for recording media, mice, numeric keypads, CD players, MD players, portable radio and audio players, housings, covers, keyboards, buttons, switch components, casings for power meters, battery cases, battery transport trays, relays, sensors, actuators, terminal switches, and grill cooking equipment parts. EXAMPLES
[0098] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or the like, measurements can be made using other instruments with equivalent performance.
[0099] 1.Raw materials The following raw materials were used: [Table 1]
[0100] 2. Examples 1 to 6 and Comparative Examples 1 to 2 <Compound> The components shown in Table 1 were uniformly mixed with a tumbler mixer at the ratios shown in Table 2 or Table 3 (each component in Tables 2 and 3 is shown in parts by mass), excluding the glass fiber. The resulting mixture was fed into a twin-screw extruder (TEX30α manufactured by Japan Steel Works, Ltd.) from the main feed port. The cylinder set temperature of the first kneading section was set at 260 °C, and the glass fiber was fed from the side feeder. The resin composition melt-kneaded under the conditions of a cylinder set temperature of 260 °C and a screw rotation speed of 200 rpm after the addition of the glass fiber was rapidly cooled in a water tank and pelletized using a pelletizer to obtain pellets of the resin composition.
[0101] <Tensile properties> After drying the pellets obtained above at 110 °C for 5 hours, using an injection molding machine (J85AD manufactured by Japan Steel Works, Ltd.), an ISO test piece with a thickness of 4 mm was injection molded under the conditions of a cylinder temperature of 250 °C and a mold temperature of 80 °C. Regarding the ISO test piece (4 mm thickness) obtained above, in accordance with ISO527-1 and ISO527-2, the tensile modulus (unit: MPa), fracture elongation at break (unit: %), tensile strength (unit: MPa), and fracture strain (unit: %) were measured. Also, regarding the test piece after standing for 1 hour under the condition of 90 °C, the tensile strength (unit: MPa) was similarly measured (high-temperature tensile strength). It can be said that when the high-temperature tensile strength is 47 MPa or more, preferably 48 MPa or more, and more preferably 49 MPa or more, it is excellent.
[0102] <DTUL (after annealing)> Regarding the test piece after annealing, in accordance with ISO75-1 and ISO75-2, the heat deflection temperature under load (unit: °C) was measured under the condition of a load of 1.80 MPa. The pre-annealing condition of the test piece was 160 °C × 3 hours.
[0103] <Warpage characteristics> The resin composition pellets obtained above were molded into a disk having a diameter of 100 mm and a thickness of 1.6 mm using an injection molding machine ("NEX80" manufactured by Nissei Plastic Industrial Co., Ltd.) under the conditions of a cylinder temperature of 260°C, a mold temperature (MT) of 80°C, and a holding pressure value of 80% of the peak injection pressure using a side gate mold, and the amount of warping of the disk (unit: mm) was measured. The amount of warping here was determined as the distance between the flat plate and the disc (flat plate side) at the point where the flat plate and the disc were furthest apart when the disc was placed on a flat plate.
[0104] <Flame retardancy> The resin composition pellets obtained above were dried at 110°C for 5 hours, and then injection molded into combustion test specimens (12.7 mm width x 127 mm length x 1.6 mm thickness) using an injection molding machine (Japan Steel Works, Ltd., "J-50AD") under conditions of a cylinder temperature of 250°C and a mold temperature of 80°C. The flame retardancy of the obtained combustion test specimens was evaluated according to the Underwriters Laboratories Subject 94 (UL94) method.
[0105] [Table 2]
[0106] [Table 3]
[0107] As is clear from the above results, the molded article formed from the resin composition of the present invention had high flame retardancy and also had high mechanical strength at high temperatures.
Claims
1. For a total of 100 parts by mass of 15 to 50 parts by mass of a polybutylene terephthalate resin having an intrinsic viscosity (IV) of 0.3 to 0.75 dL / g and 50 to 85 parts by mass of a styrene-based resin, Contains 5 to 100 parts by mass of glass fiber; Further, it contains a flame retardant, 10% by mass or more of the styrene-based resin is an acrylonitrile-styrene copolymer having a weight average molecular weight (Mw) of 400,000 or less; Resin composition.
2. The resin composition according to claim 1 , wherein the flame retardant comprises a halogen-based flame retardant.
3. The resin composition according to claim 1 , wherein the flame retardant comprises a brominated flame retardant.
4. The resin composition according to claim 1 , further comprising a polycarbonate resin.
5. The resin composition according to claim 1 , further comprising a flame retardant auxiliary.
6. The flame retardant comprises a brominated flame retardant, Further, the present invention includes a polycarbonate resin. The resin composition according to claim 1 , further comprising a flame retardant auxiliary.
7. The resin composition according to claim 1, wherein the weight average molecular weight (Mw) of the acrylonitrile-styrene copolymer is less than 350,000.
8. The resin composition according to claim 1, wherein the weight average molecular weight (Mw) of the acrylonitrile-styrene copolymer is less than 200,000.
9. The flame retardant includes a halogen-based flame retardant, The flame retardant comprises a brominated flame retardant, Further, the present invention includes a polycarbonate resin. Further, it contains a flame retardant assistant, The resin composition according to claim 1, wherein the weight average molecular weight (Mw) of the acrylonitrile-styrene copolymer is less than 200,000.
10. The resin composition according to any one of claims 1 to 9, wherein when the resin composition is molded into a test piece having a thickness of 1.6 mm and subjected to a UL-94 test, the resin composition satisfies V-0.
11. A molded article formed from the resin composition according to any one of claims 1 to 9.
12. A pellet of the resin composition according to any one of claims 1 to 9.
13. A molded article formed from the pellets of claim 12.
Citation Information
Patent Citations
Thermoplastic resin composition and molded article
JP2020186293A
Cited By
Flame-retardant polybutylene terephthalate resin composition and molded article made therefrom
JP2026166967A