Transparent film and method for producing the same, near-infrared absorbing filter, and thermal insulation filter

A transparent film using copper-containing oxidized cellulose nanofibers with controlled properties addresses the need for enhanced near-infrared absorption and transparency, achieving high absorption selectivity and mechanical strength.

JP2024141945APending Publication Date: 2024-10-10ZEON CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023053833
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing transparent films lack excellent near-infrared absorption and transparency, necessitating improved light absorption selectivity and mechanical strength.

Method used

A transparent film made of copper-containing oxidized cellulose nanofibers with specific number average fiber diameter, length, and polymerization, along with controlled dispersibility and smoothness, is developed.

Benefits of technology

The film achieves high near-infrared absorption while maintaining transparency and mechanical strength, with improved light absorption selectivity and smoothness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141945000001_ABST
    Figure 2024141945000001_ABST
Patent Text Reader

Abstract

To provide a transparent film with superior near-infrared absorbing properties.SOLUTION: A transparent film is composed of copper-containing oxidized cellulose nanofibers that contain copper in salt form, with a number average fiber diameter of 100 nm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a transparent film and a method for producing the same, a near-infrared absorbing filter, and a heat shielding filter. [Background technology]

[0002] Transparent films that transmit visible light but reflect and / or absorb infrared light are used to suppress heat rays from sunlight in buildings, vehicles, etc., and to correct the visibility of digital cameras. For example, Patent Document 1 discloses such an infrared-shielding film that contains an infrared-shielding resin obtained by adding a metal compound to a copolymer of a reaction product of (meth)acrylamide and phosphoric acid or a hydrolyzate thereof, and a compound having an ethylenically unsaturated bond. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-134457 A Summary of the Invention [Problem to be solved by the invention]

[0004] Here, there is a demand for further development of a film that is excellent in near-infrared absorptivity and transparency.

[0005] Therefore, an object of the present invention is to provide a transparent film having excellent near-infrared absorptivity and transparency. Another object of the present invention is to provide a method for producing the above transparent film. Another object of the present invention is to provide a near-infrared absorbing filter comprising the above transparent film. Another object of the present invention is to provide a heat shielding filter including the above transparent film. [Means for solving the problem]

[0006] The present inventors have conducted extensive research with the aim of solving the above problems, and have newly discovered that the above problems can be solved by a transparent film made of copper-containing oxidized cellulose nanofibers that have a predetermined number average fiber diameter and contain copper in the form of a salt, thereby completing the present invention.

[0007] That is, the present invention aims to advantageously solve the above-mentioned problems, and [1] the present invention is a transparent film made of copper-containing oxidized cellulose nanofibers having a number average fiber diameter of 100 nm or less and containing copper in the form of a salt. The transparent film as described above has excellent near-infrared absorbing properties and transparency. In addition, the transparent film as described above can efficiently absorb near-infrared rays while transmitting visible light well. In other words, the transparent film as described above has excellent light absorption selectivity. In this specification, the "number average fiber diameter" of the copper-containing oxidized cellulose nanofibers can be determined by measuring the fiber diameters of five or more copper-containing oxidized cellulose nanofibers using an atomic force microscope and calculating the number average of the measured fiber diameters. As the atomic force microscope, for example, a Dimension FastScan AFM (manufactured by BRUKER, Tapping mode) can be used.

[0008] [2] In the transparent film of [1] above, the number average fiber length of the copper-containing oxidized cellulose nanofibers is preferably 50 nm or more and 2000 nm or less. When the number average fiber length of the copper-containing oxidized cellulose nanofibers is equal to or greater than the above lower limit, the transparent film can be imparted with sufficiently high mechanical strength. On the other hand, if the number average fiber length of the copper-containing oxidized cellulose nanofibers is equal to or less than the upper limit, the dispersibility of the copper-containing oxidized cellulose nanofibers is ensured, and a transparent film can be efficiently produced. In addition, the transparency of the transparent film can be improved. In this specification, the "number average fiber length" of the copper-containing oxidized cellulose nanofibers can be determined by measuring the fiber lengths of five or more copper-containing oxidized cellulose nanofibers using an atomic force microscope and calculating the number average of the measured fiber lengths. As the atomic force microscope, for example, a Dimension FastScan AFM (manufactured by BRUKER, Tapping mode) can be used.

[0009] [3] In the transparent film of [1] or [2] above, the average degree of polymerization of the copper-containing oxidized cellulose nanofibers is preferably 100 or more and 2,000 or less. When the average degree of polymerization of the copper-containing oxidized cellulose nanofibers is equal to or higher than the above lower limit, the transparent film can be imparted with sufficiently high mechanical strength. On the other hand, when the average degree of polymerization of the copper-containing oxidized cellulose nanofibers is equal to or less than the above upper limit, the dispersibility of the copper-containing oxidized cellulose nanofibers is ensured, and a transparent film can be efficiently produced. In this specification, the "average degree of polymerization" of the copper-containing oxidized cellulose nanofibers is, for example, as described in "Isogai, A., Mutoh, N., Onabe, F., Usuda, M., "Viscosity measurements of cellulose / SO 2- The measurement can be performed in accordance with the method described in "Sen'i Gakkaishi, 45, 299-306 (1989)."

[0010] [4] In any of the transparent films [1] to [3] above, the copper-containing oxidized cellulose nanofibers are preferably copper-containing carboxylated cellulose nanofibers. When the copper-containing oxidized cellulose nanofibers are copper-containing carboxylated cellulose nanofibers, the dispersibility of the copper-containing oxidized cellulose nanofibers is ensured, and a transparent film can be efficiently produced.

[0011] [5] In any of the transparent films [1] to [4] above, the light transmittance of light with a wavelength of 550 nm is preferably 80% or more. If the light transmittance for light with a wavelength of 550 nm is equal to or higher than the above lower limit, the transparency of the transparent film can be improved. In this specification, the light transmittance of a transparent film can be measured according to the method described in the Examples.

[0012] [6] In any of the transparent films [1] to [5] above, the light transmittance of light with a wavelength of 800 nm is preferably 80% or less. When the light transmittance for light with a wavelength of 800 nm is equal to or less than the upper limit, the near-infrared absorptivity of the transparent film can be improved.

[0013] [7] In any of the transparent films [1] to [6] above, the value obtained by subtracting the light transmittance of light with a wavelength of 800 nm from the light transmittance of light with a wavelength of 550 nm is preferably 10% or more. When the value is equal to or greater than the lower limit, the light absorption selectivity of the transparent film can be improved.

[0014] [8] In any of the transparent films [1] to [7] above, the arithmetic mean height Sa is preferably 60 μm or less. When the arithmetic mean height Sa is equal to or less than the upper limit, the smoothness of the transparent film can be improved. In this specification, the arithmetic mean height Sa of the transparent film can be measured according to the method described in the Examples.

[0015] The present invention also aims to advantageously solve the above-mentioned problems, and [9] the present invention is a method for producing a transparent film according to any one of the above [1] to [8], comprising a dispersing step of dispersing copper-containing oxidized cellulose nanofibers, which have a number average fiber diameter of 100 nm or less and contain copper in the form of a salt, in a dispersion medium to obtain a dispersion, and a drying step of drying the dispersion to obtain a film. The transparent film of the present invention can be obtained by the above-mentioned transparent film manufacturing method.

[0016]

[10] In the method for producing a transparent film according to [9] above, the dispersion medium is preferably water. When the dispersion medium is water, the copper-containing oxidized cellulose nanofibers are well dispersed in the dispersion liquid, and the productivity of the transparent film can be improved.

[0017]

[11] In the method for producing a transparent film according to [9] or

[10] above, the relative humidity during drying is preferably 50% or more and 95% or less in the drying step. When the relative humidity during drying is equal to or higher than the above lower limit, the smoothness of the obtained transparent film can be improved. On the other hand, if the relative humidity during drying is equal to or lower than the above upper limit, the drying speed can be increased, and the productivity of the transparent film can be improved.

[0018] Another object of the present invention is to advantageously solve the above problems, and

[12] the present invention is a near-infrared absorbing filter comprising the transparent film according to any one of [1] to [8] above. The near-infrared absorbing filter as described above is excellent in desired performance.

[0019] The present invention also aims to advantageously solve the above problems, and

[13] the present invention is a heat shielding filter comprising the transparent film according to any one of [1] to [8] above. The above-mentioned heat insulating filter is excellent in desired performance. Effect of the Invention

[0020] According to the present invention, a transparent film having excellent near-infrared absorptivity and transparency can be provided. Furthermore, according to the present invention, a method for producing the transparent film can be provided. Moreover, according to the present invention, a near-infrared absorbing filter including the above transparent film can be provided. Moreover, according to the present invention, a heat shielding filter including the above transparent film can be provided. [Brief description of the drawings]

[0021] [Figure 1] 1 is a graph showing the measurement results of the light transmittance of the film obtained in Example 1. [Diagram 2] 1 is a graph showing the measurement results of the light transmittance of the film obtained in Example 2. [Diagram 3] 2 is a graph showing the measurement results of the light transmittance of the film obtained in Comparative Example 1. [Figure 4] 1 is a graph showing the measurement results of the light transmittance of the film obtained in Comparative Example 2. [Diagram 5] 1 is a graph showing the measurement results of the light transmittance of the film obtained in Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, an embodiment of the present invention will be described in detail. Here, the transparent film of the present invention can be suitably used for, for example, image sensor parts such as CCD (Charge Coupled Device) and CMOS (Complementary Metal Oxide Semiconductor) built into digital photographic equipment, media requiring high security such as those in which letters or pictures appear or disappear when exposed to desired light, dye-sensitized solar cells, near-infrared absorbing filters (near-infrared cut filters) attached to glasses, sunglasses, etc. for the purpose of absorbing and / or cutting near-infrared rays; heat shielding filters attached to window materials, aquariums, etc. for the purpose of blocking heat; and the like. The transparent film of the present invention can be produced, for example, by using the method for producing a transparent film of the present invention described below.

[0023] (Transparent film) The transparent film of the present invention is made of copper-containing oxidized cellulose nanofibers that have a number average fiber diameter of 100 nm or less and contain copper in the form of a salt. The transparent film as described above is excellent in near-infrared absorbing property and transparency. Since the transparent film of the present invention is made of a specific copper-containing oxidized cellulose nanofiber, it does not usually contain any components other than impurities that are inevitably mixed in during production. The content of the copper-containing oxidized cellulose nanofiber in the transparent film of the present invention is usually 99% by mass or more, preferably 99.5% by mass or more, and more preferably 99.9% by mass or more.

[0024] <Copper-containing oxidized cellulose nanofiber containing copper in the form of salt> The copper-containing oxidized cellulose nanofibers constituting the transparent film of the present invention contain copper in the form of a salt. By using such copper-containing oxidized cellulose nanofibers, the transparent film can exhibit excellent near-infrared absorption properties. In the following, copper-containing oxidized cellulose nanofibers that contain copper in the form of a salt may be simply referred to as "copper-containing oxidized cellulose nanofibers."

[0025] The copper-containing oxidized cellulose nanofibers are preferably copper-containing carboxylated cellulose nanofibers. If the copper-containing oxidized cellulose nanofibers are copper-containing carboxylated cellulose nanofibers, the dispersibility of the copper-containing oxidized cellulose nanofibers is ensured, and a transparent film can be efficiently produced.

[0026] Here, the carboxylated cellulose nanofibers constituting the copper-containing carboxylated cellulose nanofibers are those in which the primary hydroxyl groups at the 6-positions of the β-glucose units of the raw cellulose have been oxidized to carboxy groups via aldehyde groups. From the viewpoint of imparting sufficient desired properties to the copper-containing carboxylated cellulose nanofibers, it is preferred that the primary hydroxyl groups in the carboxylated cellulose nanofibers are oxidized to carboxy groups by preferably 50 mol % or more, more preferably 70 mol % or more, and even more preferably 90 mol % or more. The amount of carboxy groups in the copper-containing carboxylated cellulose nanofibers can be measured according to the method described in JP-A-2016-141777 or JP-A-2019-199622.

[0027] The amount of copper in the copper-containing oxidized cellulose nanofibers is not limited as long as it can impart the desired properties to the resulting transparent film.For example, in the copper-containing carboxylated cellulose nanofibers, copper is preferably present in a ratio of 1 / 3 or more of the molar amount of the carboxyl group of the carboxylated cellulose nanofibers, more preferably 1 / 2 or more.The higher the copper content in the copper-containing oxidized cellulose nanofibers, the more the near-infrared absorptivity of the resulting transparent film can be improved. In addition, the copper in the copper-containing oxidized cellulose nanofibers can be qualitatively and quantitatively analyzed by ICP-AES according to the method described in, for example, JP 2016-141777 A or JP 2019-199622 A.

[0028] The copper-containing oxidized cellulose nanofibers must have a number-average fiber diameter of 100 nm or less. By using such copper-containing oxidized cellulose nanofibers, transparent films can be made to exhibit excellent transparency. The number average fiber diameter of the copper-containing oxidized cellulose nanofibers is preferably 50 nm or less, more preferably 10 nm or less, and even more preferably 5 nm or less. When the number average fiber diameter of the copper-containing oxidized cellulose nanofibers is equal to or less than the above upper limit, the transparency of the transparent film can be improved. On the other hand, the number average fiber diameter of the copper-containing oxidized cellulose nanofibers is, for example, 0.5 nm or more, and may be 1 nm or more.

[0029] The number average fiber length of the copper-containing oxidized cellulose nanofibers is preferably 50 nm or more, more preferably 70 nm or more, even more preferably 100 nm or more, even more preferably 400 nm or more, and is preferably 2000 nm or less, more preferably 1500 nm or less, even more preferably 1000 nm or less, and even more preferably 600 nm or less. When the number average fiber length of the copper-containing oxidized cellulose nanofibers is equal to or greater than the above lower limit, the transparent film can be imparted with sufficiently high mechanical strength. On the other hand, if the number average fiber length of the copper-containing oxidized cellulose nanofibers is equal to or less than the upper limit, the dispersibility of the copper-containing oxidized cellulose nanofibers is ensured, and a transparent film can be efficiently produced. In addition, the transparency of the transparent film can be improved. The number average fiber length of the copper-containing oxidized cellulose nanofibers can be adjusted, for example, by changing the number average fiber length of the natural cellulose used as the raw material, the oxidation treatment conditions, and the conditions for dispersing (defibrating) the carboxylated cellulose nanofibers after the oxidation treatment. Specifically, the number average fiber length can be shortened by extending the time of the dispersion treatment (defibrating treatment).

[0030] The average degree of polymerization of the copper-containing oxidized cellulose nanofibers (the average number of glucose units contained in a cellulose molecule) is preferably 100 or more, more preferably 300 or more, and even more preferably 500 or more, and is preferably 2000 or less, more preferably 1500 or less, even more preferably 1000 or less, and even more preferably 700 or less. When the average degree of polymerization of the copper-containing oxidized cellulose nanofibers is equal to or higher than the above lower limit, the transparent film can be imparted with sufficiently high mechanical strength. On the other hand, when the average degree of polymerization of the copper-containing oxidized cellulose nanofibers is equal to or less than the above upper limit, the dispersibility of the copper-containing oxidized cellulose nanofibers is ensured, and a transparent film can be efficiently produced. The average degree of polymerization of the copper-containing oxidized cellulose nanofibers can be adjusted by changing the average degree of polymerization of the natural cellulose used as the raw material, the oxidation treatment conditions, the conditions for dispersing (defibrating) the carboxylated cellulose nanofibers after the oxidation treatment, and the conditions for dispersing (defibrating) after the copper substitution process.

[0031] The above-mentioned copper-containing oxidized cellulose nanofibers can be produced, for example, according to the methods described in JP-A-2016-141777 and JP-A-2019-199622. The copper-containing oxidized cellulose nanofibers produced as described above are usually obtained as a dispersion in a dispersion medium such as water.

[0032] <Properties of transparent film> The transparent film of the present invention preferably has a light transmittance of 70% or more, more preferably 80% or more, and even more preferably 85% or more, for light with a wavelength of 550 nm. If the light transmittance for light with a wavelength of 550 nm is equal to or higher than the above lower limit, the transparency of the transparent film can be improved. On the other hand, the light transmittance of the transparent film for light with a wavelength of 550 nm is, for example, 99% or less, may be 95% or less, or may be 90% or less.

[0033] The transparent film of the present invention preferably has a light transmittance of 85% or less, more preferably 80% or less, and even more preferably 60% or less, for light with a wavelength of 800 nm. When the value is equal to or less than the upper limit, the light absorption selectivity of the transparent film can be improved. On the other hand, the light transmittance of the transparent film for light with a wavelength of 800 nm is, for example, 10% or more, may be 20% or more, or may be 30% or more.

[0034] The transparent film of the present invention preferably has a light transmittance of 550 nm light minus the light transmittance of 800 nm light of a wavelength of 5% or more, more preferably 10% or more, and even more preferably 20% or more. When the value is equal to or greater than the lower limit, the light absorption selectivity of the transparent film can be improved. On the other hand, the above value in the transparent film is, for example, 80% or less, may be 60% or less, or may be 50% or less.

[0035] The transparent film of the present invention has an arithmetic mean height Sa of preferably 70 μm or less, more preferably 60 μm or less, and even more preferably 55 μm or less. When the arithmetic mean height Sa is equal to or less than the upper limit, the smoothness of the transparent film can be improved. On the other hand, the arithmetic mean height Sa of the transparent film is, for example, 10 μm or more, may be 20 μm or more, or may be 30 μm or more. The arithmetic mean height Sa of the transparent film can be adjusted by the drying temperature in the drying process of the transparent film, the relative humidity during drying, etc., which will be described later.

[0036] The transparent film of the present invention has a thickness of preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more, and preferably 100 μm or less, more preferably 70 μm or less, and even more preferably 50 μm or less. When the thickness of the transparent film is equal to or more than the above lower limit, the near-infrared absorptivity of the transparent film can be improved. On the other hand, when the thickness of the transparent film is equal to or less than the above upper limit, the transparency of the transparent film can be improved. In this specification, the "thickness" of the transparent film can be measured according to the method described in the Examples.

[0037] (Transparent film manufacturing method) The method for producing a transparent film of the present invention includes a dispersing step in which copper-containing oxidized cellulose nanofibers, which have a number average fiber diameter of 100 nm or less and contain copper in the form of a salt, are dispersed in a dispersion medium to obtain a dispersion, and a drying step in which the dispersion is dried to obtain a film. The above-mentioned method for producing a transparent film can provide the transparent film of the present invention, that is, a transparent film having excellent near-infrared absorptivity and transparency can be obtained. The method for producing a transparent film of the present invention may further include any step other than the dispersion step and the drying step (hereinafter, these steps may be referred to as "other steps"). Examples of the other steps include a degassing step for removing dissolved gas in the dispersion obtained in the dispersion step, and a coating step for applying the dispersion to obtain a coating film before the drying step.

[0038] <Dispersion process> In the dispersion step, copper-containing oxidized cellulose nanofibers having a number average fiber diameter of 100 nm or less and containing copper in the form of a salt are dispersed in a dispersion medium to obtain a dispersion liquid.

[0039] As the copper-containing oxidized cellulose nanofibers that contain copper in the form of a salt, those described above can be used. In the preparation of the copper-containing oxidized cellulose nanofibers, when the copper-containing oxidized cellulose nanofibers are obtained in the form of a dispersion, the dispersion can be used as is in the method for producing a transparent film of the present invention.

[0040] Here, the solids concentration of the copper-containing oxidized cellulose nanofibers in the dispersion is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and is preferably 2.0% by mass or less, more preferably 1.0% by mass or less, and even more preferably 0.5% by mass or less. When the solids concentration of the copper-containing oxidized cellulose nanofibers in the dispersion is equal to or higher than the above lower limit, a transparent film can be efficiently obtained. On the other hand, when the solids concentration of the copper-containing oxidized cellulose nanofibers in the dispersion is equal to or lower than the above upper limit, the dispersion state of the dispersion becomes good, and unevenness in the thickness of the obtained transparent film can be effectively suppressed. The solids concentration of the copper-containing oxidized cellulose nanofibers in the dispersion can be adjusted by the amount of dispersion medium used (described later) or by concentrating a dispersion with a low solids concentration using an evaporator or the like.

[0041] The dispersion medium used in the dispersion is not particularly limited as long as it can disperse the copper-containing oxidized cellulose nanofibers, but water is preferred because the copper-containing oxidized cellulose nanofibers disperse well in the dispersion and the productivity of the transparent film can be improved. When water is used as the dispersion medium, the water contained in the dispersion may be, for example, water derived from the aqueous dispersion in the case where the copper-containing oxidized cellulose nanofibers are obtained in the form of an aqueous dispersion in the preparation of the copper-containing oxidized cellulose nanofibers.

[0042] <Drying process> In the drying step, the dispersion obtained in the dispersion step is dried to obtain a film. The film obtained in this step may be used as the transparent film of the present invention. The dispersion may be dried, for example, after being placed in a container having a predetermined shape in accordance with the shape of the film to be obtained.

[0043] The drying temperature for the dispersion is not particularly limited as long as it is a temperature at which the dispersion medium evaporates, but is preferably 20° C. or higher, more preferably 30° C. or higher, and even more preferably 35° C. or higher. On the other hand, the drying temperature of the dispersion is preferably 60°C or less, more preferably 50°C or less, and even more preferably 45°C or less, in order to prevent rapid drying, effectively prevent discoloration of the resulting transparent film, and improve smoothness.

[0044] Here, the relative humidity during drying is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more, and is preferably 95% or less, more preferably 90% or less, and even more preferably 85% or less. When the relative humidity during drying is equal to or higher than the above lower limit, the smoothness of the obtained transparent film can be improved. On the other hand, if the relative humidity during drying is equal to or lower than the above upper limit, the drying speed can be increased, and the productivity of the transparent film can be improved.

[0045] The drying time is not particularly limited, but is usually from 1 day to 5 days.

[0046] The drying may be performed using a dryer capable of simultaneously controlling the temperature and humidity, such as a thermo-hygrostat, although there is no particular limitation.

[0047] (Near infrared absorbing filter) The near-infrared absorbing filter of the present invention comprises the transparent film of the present invention. Since the near-infrared absorbing filter of the present invention comprises the transparent film of the present invention, it is excellent in near-infrared absorbency, transparency, and light absorption selectivity.

[0048] The near infrared absorbing filter of the present invention may be made of the transparent film of the present invention, or may be provided with the transparent film of the present invention on a support, provided that the object of the present invention is not impaired. The transparent film may be provided on the support via an adhesive layer or the like, although it is not particularly limited thereto. Examples of supports that the near-infrared absorption filter of the present invention may optionally include transparent substrates such as substrates made of materials such as silicon, alkali-free glass, soda glass, Pyrex (registered trademark) glass, and quartz glass, as well as copper-containing glass substrates and resin substrates.

[0049] The near-infrared absorbing filter of the present invention may further include a dielectric multilayer film, an ultraviolet absorbing layer, etc., in addition to the transparent film of the present invention and any of the above-mentioned supports. If the near-infrared absorbing filter further includes a dielectric multilayer film, the near-infrared absorbing filter can exhibit a wide viewing angle and excellent infrared shielding properties. If the near-infrared absorbing filter further includes an ultraviolet absorbing layer, the near-infrared absorbing filter can exhibit excellent ultraviolet shielding properties. As the dielectric multilayer film that the near-infrared absorption filter of the present invention may optionally be provided with, for example, the dielectric multilayer film described in JP-A-2014-41318 can be used. As the ultraviolet absorbing layer that the near-infrared absorbing filter of the present invention may optionally be provided with, for example, the absorbing layer described in WO 2015 / 099060 can be used.

[0050] The near-infrared absorption filter of the present invention can be used in, for example, image sensor parts such as CCDs (Charge Coupled Devices) and CMOSs ​​(Complementary Metal Oxide Semiconductors) built into digital photographing equipment, media requiring high security such as those in which characters or pictures appear or disappear when exposed to desired light, dye-sensitized solar cells, eyeglasses, sunglasses, and the like.

[0051] (Heat shielding filter) The heat shielding filter of the present invention includes the transparent film of the present invention. Since the heat shielding filter of the present invention includes the transparent film of the present invention, it has excellent near-infrared absorbing properties and, as a result, excellent heat shielding properties.

[0052] The heat shielding filter of the present invention may be made of the transparent film of the present invention, but may also be a filter in which the transparent film of the present invention is provided on a support, provided that the object of the present invention is not impaired. The transparent film may be provided on the support via an adhesive layer or the like, although there is no particular limitation thereon. Here, as the support that the heat shielding filter of the present invention may optionally have, the same supports as those mentioned above can be used.

[0053] The heat shielding filter of the present invention can be used, for example, in window materials, aquariums, etc. In particular, by using the heat shielding filter in a window material, for example, it is possible to effectively maintain the brightness of the outside (for example, effectively bring the brightness of the outdoors into the room) while suppressing a temperature rise caused by infrared rays inside the window material (for example, inside a room, etc.). EXAMPLES

[0054] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Various measurements and evaluations in the examples and comparative examples were carried out according to the following methods.

[0055] <Film thickness> The thickness of the film in the examples and comparative examples was measured using a Digimatic Thickness Gauge (ID-C112XBS: manufactured by Mitutoyo Corporation).

[0056] <Arithmetic mean height Sa of film> The arithmetic mean height Sa of the film in the examples and comparative examples was measured using a digital microscope (VHX-6000: manufactured by Keyence Corporation). Specifically, the arithmetic mean height Sa of the film was measured within an arbitrary range of 133.36 μm × 150.00 μm in accordance with ISO 25178, and this was defined as the arithmetic mean height Sa of the film.

[0057] <Light transmittance of film> The light transmittance of the films in the examples and comparative examples was measured using an ultraviolet, visible, near infrared spectrophotometer (V-570: manufactured by JASCO Corporation). The measurement was performed in the wavelength range of 200 nm to 2500 nm. The light transmittance of light with a wavelength of 550 nm and 800 nm was read.

[0058] <Transparency> In the light transmittance of the film measured above, the transparency was evaluated according to the following criteria using the light transmittance value of light with a wavelength of 550 nm. A: The light transmittance value for light with a wavelength of 550 nm was 85% or more. B: The light transmittance value for light with a wavelength of 550 nm was 80% or more and less than 85%. C: The light transmittance value for light with a wavelength of 550 nm was 70% or more and less than 80%. D: The light transmittance value for light with a wavelength of 550 nm was less than 70%.

[0059] <Near infrared absorption> Among the light transmittances of the films measured above, the near infrared absorptivity was evaluated using the light transmittance value of light with a wavelength of 800 nm according to the following criteria. A: The light transmittance value for light with a wavelength of 800 nm was 60% or less. B: The light transmittance value for light with a wavelength of 800 nm was more than 60% and 80% or less. C: The light transmittance value for light with a wavelength of 800 nm was more than 80% and 85% or less. D: The light transmittance value for light with a wavelength of 800 nm was more than 85%.

[0060] <Light absorption selectivity> In the light transmittance of the film measured above, the light absorption selectivity was evaluated according to the following criteria using the value (550 nm-800 nm) obtained by subtracting the light transmittance of light with a wavelength of 800 nm from the light transmittance of light with a wavelength of 550 nm. A: The above value for 550nm-800nm ​​was 20% or more. B: The above value of 550 nm to 800 nm was 10% or more and less than 20%. C: The above value of 550 nm to 800 nm was 5% or more and less than 10%. D: The above value of 550 nm to 800 nm was less than 5%.

[0061] <Smoothness> The surface of the film was visually inspected and the smoothness was evaluated according to the following criteria. A: The film surface was smooth. B: Wrinkles were observed on the surface of the film.

[0062] Example 1 <Preparation of sodium-containing TEMPO-oxidized cellulose nanofiber aqueous dispersion> TEMPO-catalyzed oxidized pulp (oxidized cellulose) was obtained by dispersing 1 g of softwood bleached kraft pulp (dry weight equivalent), 5 mmol of sodium hypochlorite, 0.1 g (1 mmol) of sodium bromide, and 0.016 g (1 mmol) of TEMPO (2,2,6,6-tetramethylpiperidine-1-oxyl) in 100 mL of water, gently stirring at room temperature for 4 hours, and washing with distilled water. The amount of carboxyl groups in the obtained TEMPO-catalyzed oxidized pulp was 1.4 mmol / g. Then, distilled water was added to the undried TEMPO-catalyzed oxidized pulp to prepare an aqueous dispersion with a solid content of 0.1%. The aqueous dispersion was then defibrated using a homogenizer (Microtec Nithion, Hiscotron) at 7.5×1000 rpm for 2 minutes, and an ultrasonic homogenizer (Nissei, Ultrasonic Generator) for 4 minutes with V-LEVEL4, TIP26D while cooling the container with ice to obtain an aqueous dispersion containing TEMPO carboxylated cellulose nanofibers as TEMPO-oxidized cellulose nanofibers. The undefibrated components were then removed from the aqueous dispersion of TEMPO carboxylated cellulose nanofibers by centrifugation (12000G (120×100 rpm / g), 10 minutes, 12℃) using a centrifuge (SAKUMA, M201-1VD, angle rotor 50F-8AL) to obtain an aqueous dispersion of TEMPO carboxylated cellulose nanofibers with a solid content of 0.1% by mass, which was a transparent liquid. The TEMPO carboxylated cellulose nanofibers contained sodium derived from the co-oxidant in the form of a salt. In other words, the above procedure yielded an aqueous dispersion of sodium-containing TEMPO oxidized cellulose nanofibers (hereinafter sometimes simply referred to as "TOCN-Na").

[0063] <Preparation of hydrogen-substituted TEMPO-oxidized cellulose nanofiber aqueous dispersion> To 100 mL of the TOCN-Na aqueous dispersion, 1 mL of 1 M hydrochloric acid was added under stirring to adjust the pH to 1. Then, stirring was continued for 60 minutes. Thereafter, the TEMPO carboxylated cellulose nanofibers that had been gelled by the addition of hydrochloric acid were collected by centrifugation (12,000 G), and the collected TEMPO carboxylated cellulose nanofibers were washed successively with 1 M hydrochloric acid and a large amount of distilled water. Next, 100 mL of distilled water was added to obtain an aqueous dispersion of hydrogen-substituted TEMPO carboxylated cellulose nanofibers (hereinafter, simply referred to as "TOCN-H") with a concentration of 0.1 mass%. The carboxy groups on the surface of TOCN-H were measured by FT-IR (JASCO Corporation, FT / IR-6100) according to Biomacromolecules (2011, Vol. 12, pp. 518-522) and found to be substituted with carboxylic acid groups at least 90%.

[0064] <Preparation of copper-containing TEMPO-oxidized cellulose nanofiber aqueous dispersion (dispersion process)> 50 g of the above-mentioned 0.1% by mass TOCN-H aqueous dispersion was stirred, and 18 g of a 0.1% by mass copper acetate aqueous solution was added thereto, and stirring was continued for 3 hours at room temperature. After that, the carboxylated cellulose nanofibers gelled by the addition of the copper acetate aqueous solution were collected by centrifugation (12000G (120×100 rpm / g), 10 minutes, 12°C) using a centrifuge (SAKUMA, M201-1VD, angle rotor 50F-8AL), and the collected cellulose nanofibers were washed with a 0.1% by mass copper acetate aqueous solution, and then the collected cellulose nanofibers were washed with a large amount of distilled water. Then, 50 mL of distilled water was added, and an ultrasonic homogenizer (Nissei, Ultrasonic Generator) was used to perform ultrasonic treatment (2 minutes) with V-LEVEL4, TIP26D while cooling the container with ice to disperse the copper ion-substituted TEMPO carboxylated cellulose nanofibers. Then, from the copper ion-substituted TEMPO carboxylated cellulose nanofiber aqueous dispersion, the undefibrated components were removed by centrifugation (12000G (120×100 rpm / g), 10 minutes, 12° C.) using a centrifuge (SAKUMA, M201-1VD, angle rotor 50F-8AL). As a result, an aqueous dispersion of copper-containing TEMPO oxidized cellulose nanofibers (hereinafter sometimes simply referred to as “TOCN-Cu”) with a solid content concentration of 0.1% by mass was obtained. Then, this aqueous dispersion was concentrated using an evaporator to obtain an aqueous TOCN-Cu dispersion with a solid content concentration of 0.4% by mass.

[0065] <Film production (drying process)> 20 g of the TOCN-Cu aqueous dispersion obtained above was placed in a 60 mm untreated tissue culture dish manufactured by AGC Technoglass Co., Ltd. This untreated tissue culture dish was then placed in a thermohygrostat at a temperature of 40° C. and a relative humidity of 80% for 4 days to obtain a blue, transparent film with a smooth surface. The obtained film was subjected to various measurements and evaluations, and the results are shown in Table 1 and Figure 1.

[0066] Example 2 In preparing the film, various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that 10 g of the TOCN-Cu aqueous dispersion was placed in a 60 mm untreated tissue culture dish. The results are shown in Table 1 and Figure 2. The obtained film had a smooth surface and was blue and transparent.

[0067] Example 3 In the preparation of the film, the untreated tissue culture dish containing the TOCN-Cu aqueous dispersion was placed in an oven at 40°C for 4 days without humidity control (relative humidity: about 5%), and the other operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1. The obtained film was blue and transparent, but had a wrinkled and wavy surface.

[0068] Comparative Example 1 The TOCN-Na aqueous dispersion having a solid content of 0.1% by mass obtained in the preparation of the sodium-containing TEMPO-oxidized cellulose nanofiber aqueous dispersion described above was concentrated to a solid content of 0.4% using an evaporator to obtain a TOCN-Na aqueous dispersion having a solid content of 0.4%. Then, various operations, measurements, and evaluations were performed in the same manner as in Example 2, except that the TOCN-Na aqueous dispersion having a solid content concentration of 0.4% obtained above was used to prepare a film instead of the TOCN-Cu aqueous dispersion having a solid content concentration of 0.4% by mass. The results are shown in Table 1 and Figure 3. The obtained film had a smooth surface and was colorless and transparent.

[0069] Comparative Example 2 Except for using a polyethylene terephthalate (PET) film (G2R, manufactured by Toyobo Co., Ltd.) as the film, various measurements and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1 and FIG.

[0070] Comparative Example 3 Except for using a cycloolefin polymer (COP) film (ZF-16, manufactured by Zeon Corporation) as the film, various measurements and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1 and FIG.

[0071] Comparative Example 4 A sodium-containing TEMPO oxidized pulp (TOC-Na) with a solid content of 20% was diluted with distilled water to obtain a TOC-Na aqueous dispersion with a solid content of 0.1%. The sodium counterions of the carboxyl groups on the surface of the TOC-Na in this dispersion were replaced with copper ions using copper acetate to obtain a copper ion-substituted TEMPO oxidized pulp (TOC-Cu) aqueous dispersion (solid content of 0.1% by mass). The obtained TOC-Cu aqueous dispersion with a solid content of 0.1% by mass was concentrated to a solid content of 0.4% by mass using an evaporator to obtain a TOC-Cu aqueous dispersion with a solid content of 0.4% by mass. Then, various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the TOC-Cu aqueous dispersion having a solid content concentration of 0.4% obtained above was used to prepare a film instead of the TOCN-Cu aqueous dispersion having a solid content concentration of 0.4% by mass. The results are shown in Table 1. The obtained film had a smooth surface but was blue and opaque.

[0072] In addition, in Table 1, "CNF" stands for cellulose nanofiber. "CMF" refers to cellulose microfiber.

[0073] [Table 1]

[0074] As is clear from Table 1, the films of Examples 1 to 3 are transparent films excellent in near-infrared absorptivity and transparency. [Industrial Applicability]

[0075] According to the present invention, a transparent film having excellent near-infrared absorptivity and transparency can be provided. Furthermore, according to the present invention, a method for producing the transparent film can be provided. Moreover, according to the present invention, a near-infrared absorbing filter including the above transparent film can be provided. Moreover, according to the present invention, a heat shielding filter including the above transparent film can be provided.

Claims

1. A transparent film comprising copper-containing oxidized cellulose nanofibers having a number average fiber diameter of 100 nm or less and containing copper in the form of a salt.

2. The transparent film according to claim 1 , wherein the number average fiber length of the copper-containing oxidized cellulose nanofibers is 50 nm or more and 2000 nm or less.

3. The transparent film according to claim 1 , wherein the average degree of polymerization of the copper-containing oxidized cellulose nanofibers is 100 or more and 2000 or less.

4. The transparent film according to claim 1 , wherein the copper-containing oxidized cellulose nanofibers are copper-containing carboxylated cellulose nanofibers.

5. 2. The transparent film according to claim 1, having a light transmittance of 80% or more for light having a wavelength of 550 nm.

6. 2. The transparent film according to claim 1, having a light transmittance of 80% or less for light having a wavelength of 800 nm.

7. 2. The transparent film according to claim 1, wherein the light transmittance of light with a wavelength of 550 nm minus the light transmittance of light with a wavelength of 800 nm is 10% or more.

8. The transparent film according to claim 1 , having an arithmetic mean height Sa of 60 μm or less.

9. A method for producing a transparent film according to any one of claims 1 to 8, A dispersion step of dispersing copper-containing oxidized cellulose nanofibers having a number average fiber diameter of 100 nm or less and containing copper in the form of a salt in a dispersion medium to obtain a dispersion; a drying step of drying the dispersion to obtain a film; A method for producing a transparent film comprising the steps of:

10. The method for producing a transparent film according to claim 9 , wherein the dispersion medium is water.

11. The method for producing a transparent film according to claim 9 , wherein in the drying step, the relative humidity during drying is 50% or more and 95% or less.

12. A near-infrared absorbing filter comprising the transparent film according to any one of claims 1 to 8.

13. A heat shielding filter comprising the transparent film according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Infrared ray blocking film and infrared ray blocking laminated film