Positive electrode material, manufacturing method of positive electrode material, and secondary battery

By depositing a crystalline composite oxide on the surface of the positive electrode active material using a deep eutectic solvent, the method addresses high electrical resistance and heat-induced deterioration, enhancing electron flow and ion mobility for improved battery performance.

JP2024142060AInactive Publication Date: 2024-10-10SHINSHU UNIVERSITY +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023054033
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing positive electrode materials for secondary batteries, such as those described in Patent Documents 1 and 2, suffer from high electrical resistance due to amorphous titanium- or niobium-containing coatings, limiting high-rate characteristics and cycle stability due to hindered electron flow and heat-induced deterioration.

Method used

A crystalline composite oxide, such as titanium and niobium oxide, is deposited on the surface of the positive electrode active material using a deep eutectic solvent, reducing electrical resistance and enhancing electron flow, while maintaining an amorphous interface for improved ion mobility.

Benefits of technology

The method results in a positive electrode material with enhanced high-rate characteristics and cycle stability by allowing increased electron flow and suppressing heat-induced deterioration, thereby improving battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142060000001_ABST
    Figure 2024142060000001_ABST
Patent Text Reader

Abstract

To provide positive electrode material for a secondary battery excellent in high-rate characteristics and cycle characteristics, and a manufacturing method for the same.SOLUTION: Positive electrode material for a secondary battery includes a positive electrode active substance 10 and metallic oxides 20 having crystallinity and attached to a part of a surface of the positive electrode active substance 10.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cathode material for a secondary battery, a method for producing the cathode material, and a secondary battery including the cathode material. [Background technology]

[0002] 2. Description of the Related Art Secondary batteries such as lithium ion secondary batteries are lightweight and have a high energy density, and therefore are used as power sources for personal computers, mobile terminals, and the like, and as power sources for driving vehicles.

[0003] Various materials have been studied for the positive electrode material used in secondary batteries from the viewpoint of increasing capacity and functionality. For example, Patent Document 1 discloses a positive electrode material in which a titanium-containing oxide is attached to the surface of a lithium-containing transition metal oxide, which is a positive electrode active material, and then the resulting material is sintered. It is described that this improves the charging characteristics of the lithium-ion secondary battery when the battery is at a high depth of charge.

[0004] Patent Document 2 discloses a positive electrode material in which niobium oxide or titanium oxide is made to be present on the surface of a lithium nickel composite oxide, which is a positive electrode active material, and then the resulting material is fired, and it is described that this improves the thermal stability of the lithium ion secondary battery. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-224307 A [Patent Document 2] Patent No. 3835412 Summary of the Invention [Problem to be solved by the invention]

[0006] In the positive electrode material disclosed in Patent Document 1, the surface of a lithium-containing transition metal oxide is coated with a sintered titanium-containing oxide, thereby modifying the interface between the positive electrode material and the non-aqueous electrolyte, thereby promoting the lithium ion migration reaction and improving the charging characteristics over a wide range of charge depths.

[0007] Furthermore, in the positive electrode material disclosed in Patent Document 2, the material coating the surface of the lithium nickel composite oxide is niobium oxide or titanium oxide, the melting point of which is equal to or higher than the firing temperature. This allows the niobium or titanium oxide obtained by firing to be stably present on the surface of the lithium nickel composite oxide, thereby obtaining a positive electrode material with high thermal stability.

[0008] However, in the positive electrode materials disclosed in Patent Document 1 and Patent Document 2, the titanium-containing oxide or the oxide of titanium or niobium that coats the surface of the positive electrode active material is formed by sintering or baking, and is therefore amorphous, with high electrical resistance. Therefore, even if the surface of the positive electrode active material is coated with the titanium-containing oxide or the oxide of titanium or niobium, the electrical resistance on the surface of the positive electrode active material cannot be reduced. Therefore, it is difficult to improve the high-rate characteristics because a large amount of electrons cannot flow during charging and discharging. In addition, for the same reason, it is difficult to improve the cycle characteristics because the deterioration of the positive electrode active material due to heat generation during charging and discharging cannot be suppressed.

[0009] The present invention has been made in view of the above-mentioned circumstances, and a main object of the present invention is to provide a positive electrode material for a secondary battery having excellent high-rate characteristics and cycle characteristics, and a method for producing the same. [Means for solving the problem]

[0010] The positive electrode material according to the present invention is a positive electrode material for a secondary battery, and includes a positive electrode active material and a crystalline metal oxide attached to a portion of the surface of the positive electrode active material.

[0011] In a preferred embodiment, the metal oxide is a composite oxide containing multiple types of metals.

[0012] In a preferred embodiment, the metal oxide is a composite oxide containing titanium and a transition metal other than titanium.

[0013] In a preferred embodiment, the transition metal other than titanium is any one of niobium, tantalum, zirconia, molybdenum, and tungsten.

[0014] In a preferred embodiment, the metal oxide is a composite oxide of titanium and niobium.

[0015] The method for producing a positive electrode material according to the present invention is a method for producing a positive electrode material for a secondary battery, and includes the steps of kneading a powder of a positive electrode active material and a powder of a metal oxide in a deep eutectic solvent to obtain a kneaded mixture, and heating the kneaded mixture to precipitate a metal oxide having crystallinity on a portion of the surface of the positive electrode active material.

[0016] In a preferred embodiment, the metal oxide powder contains powders of multiple types of metal oxides, and the metal oxide precipitated on a portion of the surface of the positive electrode active material is a composite oxide of each metal in the multiple types of metal oxides.

[0017] In a preferred embodiment, the metal oxide powder contains a powder of titanium oxide and a powder of an oxide of a transition metal other than titanium, and the metal oxide precipitated on a portion of the surface of the positive electrode active material is a composite oxide containing titanium and the transition metal other than titanium.

[0018] In a preferred embodiment, the oxide of a transition metal other than titanium is any one of niobium oxide, tantalum oxide, zirconia oxide, molybdenum oxide, and tungsten oxide. Effect of the Invention

[0019] According to the present invention, it is possible to provide a positive electrode material for a secondary battery having excellent high-rate characteristics and cycle characteristics, and a method for producing the same. [Brief description of the drawings]

[0020] [Figure 1] 1 is a photograph taken with a scanning electron microscope of a surface of a positive electrode active material after a mixture obtained by kneading a positive electrode active material, titanium oxide, and niobium oxide in a deep eutectic solvent is heated. [Figure 2A] 1 is a TEM photograph of a precipitate attached to the surface of a positive electrode active material. [Figure 2B] 2B is an enlarged photograph of the area indicated by arrow A in FIG. 2A. [Diagram 3] 1 is a graph showing the battery capacity of a lithium ion secondary battery in an example. [Figure 4] 1 is a graph showing cycle characteristics of a lithium ion secondary battery in an example. [Diagram 5] 1 is a graph showing the battery capacity of lithium ion secondary batteries produced by changing the ratio of titanium oxide and niobium oxide to the positive electrode active material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following embodiment.

[0022] The positive electrode material in this embodiment is a positive electrode material for a secondary battery, and includes a positive electrode active material and a crystalline metal oxide attached to a part of the surface of the positive electrode active material. Usually, the positive electrode of a secondary battery is manufactured by mixing this positive electrode material, a conductive material such as carbon, and a binder such as PVDF (polyvinylidene fluoride) in an organic solvent to form a slurry-like positive electrode mixture, and applying this positive electrode mixture to a positive electrode current collector such as aluminum foil.

[0023] The secondary battery includes a lithium ion secondary battery, a lithium sulfur secondary battery, etc. For example, the positive electrode active material of the lithium ion secondary battery is LiCoO2, LiNiO2, LiNi 0.8 Co 0.2Lithium-containing composite oxides such as LiMnO2 and LiMn2O4 can be used. The positive electrode active material is preferably made of two or more types of positive electrode active materials having different particle sizes. The positive electrode active material having a small particle size can be formed, for example, by using a flux method.

[0024] The metal oxide attached to the surface of the positive electrode active material is made of a material that has crystallinity and low electrical resistivity. The electrical resistivity of the metal oxide is 10 5 A value of Ω·cm or less is preferable. This allows the electrical resistance on the surface of the positive electrode active material to be reduced, allowing a large amount of electrons to flow during charging and discharging, resulting in improved high-rate characteristics. In addition, deterioration of the positive electrode active material due to heat generation during charging and discharging can be suppressed, improving cycle characteristics.

[0025] In addition, the interface in contact with the metal oxide positive electrode active material is preferably in an amorphous state. Usually, the crystal lattice of the positive electrode active material is changed to an amorphous state due to the oxidation-reduction reaction accompanying charging and discharging, and shrinkage due to reaction heat. Therefore, if the interface in contact with the metal oxide positive electrode active material is in a crystalline state, lattice mismatch occurs, and the movement of ions and electrons becomes poor. Therefore, by making the interface in contact with the metal oxide positive electrode active material in an amorphous state, the movement of ions and electrons can be improved. This can further improve the high-rate characteristics.

[0026] The metal oxide is formed by precipitating in a crystalline state on the surface of the positive electrode active material using a deep eutectic solvent described later, whereby the metal oxide having low electrical resistivity is attached to the surface of the positive electrode active material.

[0027] As shown in FIG. 1, the metal oxide 20 is attached to a part of the surface of the positive electrode active material 10. Here, FIG. 1 is a photograph of the surface of the positive electrode active material 10 taken with a scanning electron microscope. If the proportion of the metal oxide 20 attached to the surface of the positive electrode active material 10 is too high, it is not preferable because it hinders the movement of lithium ions from the positive electrode active material 10 and leads to a decrease in capacity. Here, "attached" means a state in which the positive electrode active material and the metal oxide are in stable contact with each other, and includes cases in which they are chemically bonded and physically in close contact with each other.

[0028] The metal oxide may be a composite oxide containing a plurality of metals. The metal oxide may be, for example, a composite oxide containing titanium and a transition metal other than titanium. Such a composite oxide is precipitated on the surface of the positive electrode active material in a crystalline state using a deep eutectic solvent. Examples of transition metals other than titanium include niobium, tantalum, zirconia, molybdenum, and tungsten.

[0029] Next, a method for producing the positive electrode material for a secondary battery in this embodiment will be described.

[0030] The method for producing the cathode material in this embodiment includes a step of kneading a powder of a cathode active material and a powder of a metal oxide in a deep eutectic solvent to obtain a kneaded mixture, and a step of heating the obtained kneaded mixture to precipitate a metal oxide having crystallinity on a part of the surface of the cathode active material. Hereinafter, a composite oxide containing titanium and a transition metal other than titanium will be described as an example of the metal oxide attached to the surface of the cathode active material.

[0031] First, a powder of a positive electrode active material, a powder of titanium oxide, and a powder of an oxide of a transition metal other than titanium are kneaded in a deep eutectic solvent to obtain a kneaded mixture. Examples of the oxide of a transition metal other than titanium include niobium oxide, tantalum oxide, zirconia oxide, molybdenum oxide, and tungsten oxide.

[0032] Here, the term "deep eutectic solvent" refers to a compound formed by a mixture of a hydrogen bond donor compound and a hydrogen bond acceptor compound, the melting point of which is significantly lowered by the eutectic and which becomes liquid at around room temperature. Examples of the hydrogen bond donor compound include urea, acetamide, and ethylene glycol. Examples of the hydrogen bond acceptor compound include choline chloride and N-ethyl-2-hydroxy-N.

[0033] Next, the kneaded mixture obtained by kneading is heated to precipitate a composite oxide containing titanium and a transition metal other than titanium on a part of the surface of the positive electrode active material. The kneaded mixture can be heated, for example, by putting a deep eutectic solvent in which the positive electrode active material powder or the like has been kneaded into a tubular furnace and flowing nitrogen into the tubular furnace.

[0034] The kneaded material is preferably heated to a temperature equal to or higher than the temperature at which the deep eutectic solvent is thermally decomposed. This causes the deep eutectic solvent to evaporate, and a composite oxide of titanium oxide and a transition metal other than titanium is precipitated in a crystalline state on the surface of the positive electrode active material. As a result, a positive electrode material is obtained in which a crystalline metal oxide is attached to a part of the surface of the positive electrode active material.

[0035] In addition, since the deep eutectic solvent is still at a high temperature after the composite oxide of titanium oxide and a transition metal other than titanium is precipitated on the surface of the positive electrode active material, the precipitated composite oxide chemically reacts with the positive electrode active material, and the interface of the composite oxide in contact with the positive electrode active material becomes amorphous. EXAMPLES

[0036] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0037] <Production of cathode materials> 1.0 g of a powder of a positive electrode active material (lithium iron phosphate (LFP)), 0.004 g of a powder of titanium oxide, and 0.001 g of a powder of niobium oxide were kneaded in 0.01 g of a deep eutectic solvent (a mixture of choline chloride and urea) for 30 minutes.

[0038] Next, the kneaded mixture was placed in a tubular furnace and heated at 800°C for 3 hours while flowing nitrogen at a flow rate of 0.5 L / min. The thermal decomposition temperature of the deep eutectic solvent is about 400°C, but the heating temperature was set higher at 800°C in order to quickly evaporate the deep eutectic solvent and reduce the residue of the deep eutectic solvent.

[0039] <Observation of deposits on the surface of the positive electrode active material> Fig. 1 is a photograph taken by SEM (scanning electron microscope) of the surface of the positive electrode active material after heating the kneaded material. As shown in Fig. 1, it was confirmed that a precipitate 20 was attached to the surface of the positive electrode active material 10, and this precipitate 20 was confirmed to be a substance containing titanium and niobium by elemental analysis using SEM-EDX (scanning electron microscope-energy dispersive X-ray spectroscopy), and is presumed to be a composite oxide of titanium and niobium. It can be seen that this precipitate 20 is attached to the surface of the positive electrode active material 10 in surface contact.

[0040] Fig. 2A is a TEM (transmission electron microscope) photograph of precipitates (composite oxide of titanium and niobium) 20 attached to the surface of positive electrode active material 10, and Fig. 2B is an enlarged photograph of the area indicated by arrow A in Fig. 2A. As shown in Fig. 2B, it was confirmed that precipitates 20 attached to the surface of positive electrode active material 10 have regularly aligned crystals and have crystallinity.

[0041] <Preparation of lithium ion secondary battery> The cathode material prepared by the above method, a conductive material (acetylene black), and a binder (PVDF) were mixed in a weight ratio of 90:5:5 in an organic solvent (N-methyl-pyrrolidone (NMP)) to prepare a slurry cathode mixture.

[0042] This positive electrode mixture was applied to an aluminum foil, dried at 120° C., and then pressed together with the aluminum foil to prepare a positive electrode plate.

[0043] The negative electrode plate was made of lithium metal foil.

[0044] The positive and negative electrode plates were wound with a separator interposed therebetween to produce an electrode body, and this electrode body was housed in a battery case together with a non-aqueous electrolyte to produce a lithium ion secondary battery (hereinafter referred to as the "lithium ion secondary battery of the example").

[0045] For comparison, a lithium ion secondary battery (hereinafter referred to as the comparative lithium ion secondary battery) was produced in the same manner as above, using a positive electrode active material that had not been treated to adhere a metal oxide (a composite oxide of titanium and niobium) to the surface.

[0046] <Battery capacity measurement> The fabricated lithium ion secondary battery was subjected to three charge / discharge cycles at a charge / discharge rate of 0.05 C to 5 C, and the battery capacity [mAh / g] was measured.

[0047] FIG. 3 is a graph showing the measurement results of battery capacity, where the graph indicated by circles shows the battery capacity of the lithium ion secondary battery of the embodiment, and the graph indicated by squares shows the battery capacity of the lithium ion secondary battery of the comparative example.

[0048] As shown in Fig. 3, it can be seen that the battery capacity of the lithium ion secondary battery of the Example is larger than that of the lithium ion secondary battery of the Comparative Example. In particular, it can be seen that the difference in battery capacity becomes more significant as the current during charging and discharging increases, and the high-rate characteristics are improved. This is thought to be because the metal oxide (composite oxide of titanium and niobium) attached to the surface of the positive electrode active material has a low electrical resistivity, which reduces the electrical resistance on the surface of the positive electrode active material, allowing a large amount of electrons to flow during charging and discharging.

[0049] <Measurement of cycle characteristics> The fabricated lithium-ion secondary battery was repeatedly charged and discharged at a charge / discharge rate of 1C to measure the change in discharge capacity [mAh / g] and to determine the cycle characteristics.

[0050] FIG. 4 is a graph showing the measurement results of the cycle characteristics, where the graph indicated by arrow A shows the cycle characteristics of the lithium ion secondary battery of the example, and the graph indicated by arrow B shows the cycle characteristics of the lithium ion secondary battery of the comparative example.

[0051] 4, the cycle characteristics of the lithium-ion secondary battery of the Example show that the number of cycles at which the discharge capacity starts to decrease is more than twice as high as that of the lithium-ion secondary battery of the Comparative Example. This is believed to be because the metal oxide (composite oxide of titanium and niobium) attached to the surface of the positive electrode active material has a low electrical resistivity, which reduces the electrical resistance on the surface of the positive electrode active material, thereby making it possible to suppress deterioration of the positive electrode active material due to heat generation during charging and discharging.

[0052] <Proportion of metal oxide (composite oxide of titanium and niobium) to positive electrode active material> Positive electrode materials were prepared by varying the ratio of titanium oxide and niobium oxide to the positive electrode active material as shown in Table 1 below, and lithium ion secondary batteries were prepared in the same manner as above.

[0053] [Table 1]

[0054] Figure 5 is a graph showing the results of measuring the battery capacity of lithium-ion secondary batteries fabricated with different ratios (wt%) of titanium oxide and niobium oxide to the positive electrode active material. The horizontal axis shows the ratio of the total mass of titanium oxide and niobium oxide to the mass of the positive electrode active material. The graphs indicated by arrows A, B, C, D, and E show the change in battery capacity when the charge / discharge rates are 0.05C, 0.5C, 1.0C, 2.0C, and 5.0C, respectively.

[0055] 5, when the total mass of titanium oxide and niobium oxide is in the range of 0.2 to 0.7 wt% relative to the mass of the positive electrode active material at all charge / discharge rates, the battery capacity of the lithium ion secondary battery is increased compared to the battery capacity of the comparative lithium ion secondary battery. In particular, when the charge / discharge rate is 5.0 C, the increase in battery capacity is remarkable, and it is clear that the high-rate characteristics are improved.

[0056] In addition, when the ratio of the total mass of titanium oxide and niobium oxide to the mass of the positive electrode active material was less than 0.2 wt%, no increase in battery capacity was observed. This is believed to be because the amount of metal oxide (composite oxide of titanium and niobium) attached to the surface of the positive electrode active material was small, and therefore the electrical resistance on the surface of the positive electrode active material was not reduced. In addition, when the ratio of the total mass of titanium oxide and niobium oxide to the mass of the positive electrode active material exceeded 0.7 wt%, the battery capacity was lower than that of the lithium ion secondary battery of the comparative example. This is believed to be because when the ratio of metal oxide (composite oxide of titanium and niobium) attached to the surface of the positive electrode active material was too high, the movement of lithium ions from the positive electrode active material was hindered, resulting in a decrease in battery capacity.

[0057] Although the present invention has been described above with reference to preferred embodiments, such descriptions are not limiting and various modifications are possible. For example, when a crystalline titanium and niobium composite oxide is precipitated on the surface of a positive electrode active material using a deep eutectic solvent, the ratio (mass ratio) of titanium oxide and niobium oxide can be changed to precipitate a crystalline titanium and niobium composite oxide. In this case, the electrical resistivity of the precipitated titanium and niobium composite oxide is 10 5 The ratio (mass ratio) of titanium oxide and niobium oxide should be set so that the resistivity is Ω·cm or less.

[0058] The metal oxide powder kneaded with the positive electrode active material powder in the deep eutectic solvent may contain a plurality of metal oxide powders. In this case, the metal oxide precipitated on a part of the surface of the positive electrode active material is a composite oxide of each metal in the plurality of metal oxides.

[0059] Moreover, in a secondary battery including a positive electrode plate in which a positive electrode mixture is formed on a positive electrode current collector, the positive electrode mixture containing the positive electrode material of this embodiment can be used.

[0060] Moreover, the metal oxide does not necessarily have to have a crystal structure entirely. [Explanation of symbols]

[0061] 10 Cathode active material 20 Precipitates (metal oxides)

Claims

1. A positive electrode material for a secondary battery, A positive electrode active material; a crystalline metal oxide attached to a portion of the surface of the positive electrode active material; A positive electrode material comprising:

2. The cathode material according to claim 1 , wherein the metal oxide is a composite oxide containing a plurality of metals.

3. The cathode material according to claim 2 , wherein the metal oxide is a composite oxide containing titanium and a transition metal other than titanium.

4. The cathode material according to claim 3, wherein the transition metal other than titanium is any one of niobium, tantalum, zirconia, molybdenum, and tungsten.

5. The cathode material according to claim 3 , wherein the metal oxide is a composite oxide of titanium and niobium.

6. The positive electrode material according to claim 1 , wherein the positive electrode active material is made of two or more types of positive electrode active materials having different particle sizes.

7. The positive electrode material according to claim 1 , wherein the interface of the metal oxide with the positive electrode active material is in an amorphous state.

8. A method for producing a positive electrode material for a secondary battery, comprising the steps of: A step of kneading a powder of a positive electrode active material and a powder of a metal oxide in a deep eutectic solvent to obtain a kneaded product; a step of heating the kneaded mixture to precipitate a crystalline metal oxide on a portion of a surface of the positive electrode active material; A method for producing a positive electrode material, comprising:

9. The metal oxide powder includes a plurality of metal oxide powders, The method for producing a positive electrode material according to claim 8 , wherein the metal oxide precipitated on a portion of the surface of the positive electrode active material is a composite oxide of each metal in the plurality of types of metal oxides.

10. The metal oxide powder includes a titanium oxide powder and an oxide powder of a transition metal other than titanium, The method for producing a positive electrode material according to claim 8, wherein the metal oxide precipitated on a portion of the surface of the positive electrode active material is a composite oxide containing titanium and a transition metal other than titanium.

11. The method for producing a positive electrode material according to claim 10, wherein the oxide of a transition metal other than titanium is any one of niobium oxide, tantalum oxide, zirconia oxide, molybdenum oxide, and tungsten oxide.

12. The oxide of a transition metal other than titanium is niobium oxide, The method for producing a positive electrode material according to claim 11, wherein the total mass of the titanium oxide powder and the niobium oxide powder is in the range of 0.2 to 0.7 wt % with respect to the mass of the positive electrode active material powder.

13. The method for producing a positive electrode material according to claim 12, wherein the crystalline composite oxide precipitated on a portion of the surface of the positive electrode active material is a composite oxide of titanium and niobium.

14. A secondary battery including a positive electrode plate having a positive electrode mixture formed on a positive electrode current collector, The positive electrode mixture comprises the positive electrode material according to any one of claims 1 to 7. A secondary battery.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery and method for manufacturing the same

    JP2009224307A

  • Positive electrode active material using surface-modified lithium-nickel composite oxide, positive electrode material, lithium secondary battery, and method for producing surface-modified lithium-nickel composite oxide

    JP3835412B2