Electro-deposition liquid, and, method for producing electro-deposition film

The electrodeposition liquid with polyimide resin, fluororesin, and polyoxyalkylene alkyl ether surfactant addresses the stability issue, ensuring a uniform and defect-free electrodeposited film with enhanced insulation properties.

JP2024142743APending Publication Date: 2024-10-11MITSUBISHI MATERIALS CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023055048
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Electrodeposition liquids containing polyimide resins and fluorine resins have low storage stability, leading to resin composition non-uniformity and poor appearance of the deposited film due to decreased dispersibility over time.

Method used

An electrodeposition liquid containing a polyimide resin, fluororesin, and a surfactant, specifically polyoxyalkylene alkyl ether, within a specific concentration range, ensures high dispersibility and uniform resin composition, forming an insulating film with excellent insulation properties.

Benefits of technology

The solution prevents the occurrence of defects in the electrodeposited film by maintaining resin dispersibility, resulting in a uniform and defect-free film with improved appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142743000002
    Figure 2024142743000002
  • Figure 2024142743000003
    Figure 2024142743000003
  • Figure 2024142743000004
    Figure 2024142743000004
Patent Text Reader

Abstract

To provide an electro-deposition liquid capable of suppressing the occurrence of poor appearance in an electro-deposition film even when the electro-deposition film is formed with the electro-deposition liquid containing a polyimide-based resin and a fluorine-based resin, and a method for producing the electro-deposition film.SOLUTION: An electrodeposition liquid is used when forming an electro-deposition film on a surface of a conductive substrate, and is characterized in that it contains water, a dispersion medium, a solid component, and a surfactant, the solid component contains a polyimide-based resin and a fluorine-based resin, and the content of the surfactant is within the range of 0.1 mass% or more and 5.0 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrodeposition solution for electrodepositing an electrodeposition film on a conductive substrate, and a method for producing the electrodeposition film. [Background technology]

[0002] Insulated conductors, which are made by covering a conductive substrate with an insulating film made of insulating resin, are widely used as conductive materials and heat sink materials for various electrical devices that require insulation. A mixture of multiple resins is known as a constituent material of the insulating film. For example, an insulating film made of a mixture of a polyimide resin, such as a polyamide-imide resin or a polyimide resin, and a fluorine-based resin is known. By mixing multiple resins, the insulating properties of the insulating film can be improved.

[0003] Electrodeposition is known as a method for forming an insulating coating made of an insulating resin on the surface of a conductive substrate (see, for example, Patent Document 1).

[0004] The electrodeposition method is a method in which a substrate on which an insulating film is to be formed and a counter electrode are immersed in an electrodeposition solution in which the material for the insulating film is dispersed, and a voltage is applied between the substrate and the counter electrode to form an electrodeposition film by depositing the material for the insulating film on the surface of the substrate.The formed electrodeposition film is then heated to bake the electrodeposition film onto the substrate, thereby forming the insulating film. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2022-108653 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, an electrodeposition solution containing a polyimide-based resin and a fluororesin has low storage stability and deteriorates over time. When an electrodeposition film is formed using the deteriorated electrodeposition solution, numerous streaks may appear in the electrodeposition film, resulting in a poor appearance.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide an electrodeposition liquid and a method for producing an electrodeposition film that are capable of suppressing the occurrence of defective appearance of the electrodeposition film, even when the electrodeposition film is formed using an electrodeposition liquid containing a polyimide-based resin and a fluorine-based resin. [Means for solving the problem]

[0008] In order to solve the above problems, the present inventors conducted extensive research and obtained the following findings. In the case of an electrodeposition solution containing a polyimide resin and a fluororesin, the electrodeposition film formed is a mixed film of the two resins. If the electrodeposition solution deteriorates over time, the dispersibility of the polyimide resin or the fluororesin decreases, and the resin composition becomes non-uniform when the film is formed, resulting in poor appearance.

[0009] The present invention has been made based on the above-mentioned findings, and the electrodeposition liquid of aspect 1 of the present invention is an electrodeposition liquid used when forming an electrodeposition film on the surface of a conductive substrate, and is characterized in that it contains water, a dispersion medium, a solid component, and a surfactant, the solid component contains a polyimide-based resin and a fluorine-based resin, and the content of the surfactant is within the range of 0.1 mass % or more and 5.0 mass % or less.

[0010] According to the electrodeposition liquid of the first aspect of the present invention, since it contains a polyimide resin and a fluorine resin as solid components, it is possible to form an insulating film having excellent insulating properties. Furthermore, since the surfactant is contained in the range of 0.1 mass % or more and 5.0 mass % or less, the dispersibility of the polyimide resin or fluororesin is sufficiently high, an electrodeposition film with a uniform resin composition can be formed, and the occurrence of poor appearance of the electrodeposition film can be suppressed.

[0011] The electrodeposition liquid of the second aspect of the present invention is characterized in that in the electrodeposition liquid of the first aspect of the present invention, the surfactant is a polyoxyalkylene alkyl ether.

[0012] According to the electrodeposition liquid of the second aspect of the present invention, since it contains a polyoxyalkylene alkyl ether as the surfactant, it is possible to further improve the dispersibility of the two types of resins, the polyimide resin and the fluorine resin, contained as solid components, and the resin composition becomes more uniform when a film is formed, and the occurrence of defective appearance can be further suppressed.

[0013] The electrodeposition liquid of the third aspect of the present invention is characterized in that in the electrodeposition liquid of the first or second aspect of the present invention, the polyimide-based resin is polyamideimide.

[0014] According to the electrodeposition liquid of the third aspect of the present invention, since the polyimide-based resin contains polyamideimide, together with the fluororesin, an insulating film having excellent insulating properties can be formed.

[0015] The electrodeposition liquid of a fourth aspect of the present invention is the electrodeposition liquid of any one of the first to third aspects of the present invention, characterized in that the fluorine-based resin is polytetrafluoroethylene.

[0016] According to the electrodeposition liquid of the fourth aspect of the present invention, since the fluorine-based resin contains polytetrafluoroethylene, together with the polyimide-based resin, an insulating film having excellent insulating properties can be formed.

[0017] The method for producing an electrodeposited film according to aspect 5 of the present invention is a method for producing an electrodeposited film on the surface of a conductive substrate, and is characterized in that the substrate and a counter electrode are immersed in an electrodeposition solution according to any one of aspects 1 to 4 of the present invention, the substrate is used as an anode and the counter electrode is used as a cathode, and a voltage is applied between the anode and the cathode to form the electrodeposited film on the surface of the substrate.

[0018] According to the method for producing an electrodeposition solution of the fifth aspect of the present invention, since the electrodeposition solution of any one of the first to fourth aspects of the present invention is used, it is possible to produce an electrodeposition film that is free of streaks and has good appearance quality.

[0019] The method for producing an electrodeposition film according to aspect 6 of the present invention is a method for producing an electrodeposition film by forming an electrodeposition film on the surface of a conductive substrate, characterized in that a main electrodeposition liquid containing water, a dispersion medium, and solid components containing a polyimide-based resin and a fluororesin, and a surfactant are stored, and when forming an electrodeposition film, the surfactant is added to the main electrodeposition liquid to form an electrodeposition liquid according to any one of aspects 1 to 4 of the present invention, the substrate and a counter electrode are immersed in this electrodeposition liquid, the substrate is used as an anode and the counter electrode is used as a cathode, and a voltage is applied between the anode and the cathode to form the electrodeposition film on the surface of the substrate.

[0020] According to the method for producing an electrodeposition liquid of the sixth aspect of the present invention, a surfactant is added to the main electrodeposition liquid containing water, a dispersion medium, and solid components including a polyimide resin and a fluororesin. Therefore, even if the main electrodeposition liquid deteriorates over time and the dispersibility of the polyimide resin and the fluororesin decreases, the dispersibility of the polyimide resin and the fluororesin can be improved by adding a surfactant, and an electrodeposition film having no streaks and good appearance quality can be produced. Effect of the Invention

[0021] According to the present invention, it is possible to provide an electrodeposition liquid that can suppress the occurrence of defects in the appearance of an electrodeposition film, even when the electrodeposition film is formed using an electrodeposition liquid containing a polyimide-based resin and a fluorine-based resin, and a method for producing an electrodeposition film. [Brief description of the drawings]

[0022] [Figure 1] FIG. 2 is a flow diagram showing an example of a method for producing an electrodeposition liquid according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a flow diagram showing a method for producing an electrodeposition film and an insulating coating using an electrodeposition liquid according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing an example of the appearance observation result of an electrodeposition film in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] An electrodeposition solution and a method for producing an electrodeposition film according to one embodiment of the present invention will be described below. The electrodeposition liquid of this embodiment is used when forming an electrodeposition film that serves as a precursor of an insulating film on the surface of a conductive substrate.

[0024] The electrodeposition liquid of this embodiment contains water, a dispersion medium, a solid component, and a surfactant. The solid components are said to include two types of resin: a polyimide resin and a fluorine-based resin. The content of the surfactant is set to be within the range of 0.1 mass % to 5.0 mass % based on the entire electrodeposition liquid. The content of the surfactant is more preferably 0.1 mass % or more and 1.0 mass % or less.

[0025] The surfactant improves the dispersibility of the polyimide resin and the fluorine resin, which are solid components. In this embodiment, the surfactant is preferably a polyoxyalkylene alkyl ether having the structure shown below. R-(OCH2CH2)n-OH R: an alkyl group having 1 to 20 carbon atoms, n: an integer from 1 to 20

[0026] Furthermore, in this embodiment, since the solid components contain two types of resin, a polyimide resin and a fluororesin, the electrodeposition film that is formed and the insulating coating formed by baking this electrodeposition liquid are made of a mixed resin of a polyimide resin and a fluororesin, and have excellent insulating properties. In this embodiment, the polyimide resin is preferably polyamideimide, and the fluorine resin is preferably polytetrafluoroethylene.

[0027] The average particle size of the solid components dispersed in water and the dispersion medium may be 50 nm or more and 500 nm or less, more preferably 50 nm or more and 450 nm or less, and even more preferably 50 nm or more and 300 nm or less. The standard deviation of the particle size of the solid components may be 250 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less.

[0028] The water and the dispersion medium are used to disperse the polyimide resin and the fluorine resin, which are solid components. Here, the dispersion medium preferably contains a polar solvent and a base. The polar solvent preferably has a boiling point higher than that of water. Examples of the polar solvent include organic solvents such as N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, dimethylsulfoxide, and N,N-dimethylacetamide.

[0029] Further, examples of the base in the dispersion medium include 2-aminoethanol, 2-(2-aminoethoxy)ethanol, 3-ethoxypropylamine, 6-amino-1-hexanol, tri-n-propylamine, dibutylamine, piperidine, and triethylamine. The content of water in the electrodeposition liquid is preferably 10 to 50 mass%, and more preferably 20 to 40 mass%. The content of the polar solvent in the electrodeposition liquid is preferably 50 to 90 mass%, and the content of the base is preferably 0.01 to 0.30 mass%.

[0030] Next, an example of a method for producing an electrodeposition solution according to this embodiment will be described with reference to FIG.

[0031] (Polyimide resin dispersion manufacturing process S01) First, a polar solvent, an isocyanate component, and an acid component are mixed in a flask equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer, and the mixture is heated to a temperature of, for example, 80 to 130°C and maintained for 2 to 8 hours to react, thereby obtaining polyamideimide.

[0032] Examples of the isocyanate component include aromatic diisocyanates such as diphenylmethane-4,4'-diisocyanate (MDI), diphenylmethane-3,3'-diisocyanate, diphenylmethane-3,4'-diisocyanate, diphenylether-4,4'-diisocyanate, benzophenone-4,4'-diisocyanate, and diphenylsulfone-4,4'-diisocyanate.

[0033] Examples of the acid component include trimellitic anhydride (TMA), 1,2,5-trimellitic acid (1,2,5-ETM), biphenyltetracarboxylic dianhydride, benzophenonetetracarboxylic dianhydride, diphenylsulfonetetracarboxylic dianhydride, oxydiphthalic dianhydride (OPDA), pyromellitic dianhydride (PMDA), and 4,4'-(2,2'-hexafluoroisopropylidene)diphthalic dianhydride. Thereafter, the synthesized polyamideimide is diluted with a polar solvent to prepare a polyamideimide varnish.

[0034] This polyamideimide varnish is then further diluted with a polar solvent, such as N-methyl-2-pyrrolidone, and a basic compound, tri-n-propylamine (TPA), is added, followed by the addition of water to form a polyamideimide dispersion (polyimide-based resin dispersion).

[0035] (Fluororesin dispersion manufacturing process S02) On the other hand, polytetrafluoroethylene (fluorine-based resin) is dispersed in water with an emulsifier to obtain a polytetrafluoroethylene dispersion (fluorine-based resin dispersion).

[0036] (Dispersion liquid mixing step S03) Then, the polytetrafluoroethylene dispersion (fluorine-based resin dispersion) is diluted with water, and then the polyamideimide dispersion (polyimide-based resin dispersion) is mixed therein, and the mixture is further diluted with N-methyl-2-pyrrolidone to obtain the electrodeposition liquid body (mixed resin dispersion).

[0037] (Surfactant addition step S04) A predetermined amount of polyoxyalkylene alkyl ether as a surfactant is added to the electrodeposition liquid body obtained as described above, and the mixture is stirred with a stirrer or the like. The addition of the surfactant and stirring are preferably carried out at room temperature, and the stirring time is preferably within a range of 10 minutes to 2 hours.

[0038] In the manner described above, the electrodeposition solution according to this embodiment is produced. The electrodeposition liquid may be stored in the state in which a surfactant has been added, or the electrodeposition liquid itself and the surfactant may be stored, and the surfactant may be added to the electrodeposition liquid itself to form the electrodeposition liquid just before performing electrodeposition.

[0039] Next, a method for producing an electrodeposited film and an insulating film using the electrodeposition liquid according to this embodiment will be described with reference to FIG.

[0040] As shown in FIG. 2, the method for producing an insulating coating in this embodiment includes a surface pretreatment step S101, an electrodeposition step S102, and a baking step S1030.

[0041] (Surface pretreatment process S101) First, a substrate on which an electrodeposited film (insulating film) is to be formed is prepared. This substrate is conductive and is made of a metal material such as copper or a copper alloy, aluminum or an aluminum alloy, etc. Then, the oil and fat and oxide film adhering to the surface of the above-mentioned base material are removed using a surface treatment liquid such as an organic solvent or a surfactant.

[0042] (Electrodeposition process S102) Next, the substrate and the counter electrode are immersed in the electrodeposition solution of this embodiment, and a voltage is applied between the anode (substrate) and the cathode (counter electrode) with the substrate as the anode and the counter electrode as the cathode, to form an electrodeposition film made of a mixture of a polyimide resin and a fluorine resin on the surface of the substrate.

[0043] The temperature of the electrodeposition liquid (liquid temperature) in the electrodeposition step S102 is preferably adjusted to within a range of 5°C or higher and 35°C or lower. By keeping the liquid temperature at 5°C or higher, it is possible to prevent water from being mixed into the electrodeposition liquid due to condensation. On the other hand, by keeping the liquid temperature at 35°C or lower, the storage stability of the electrodeposition liquid is improved, and the electrodeposition film can be stably formed.

[0044] The voltage applied between the substrate (anode) and the counter electrode (cathode) in the electrodeposition step S102 is preferably within the range of 10V or more and 600V or less. By setting the applied voltage to 10 V or more, the electrodeposition speed can be ensured and productivity can be improved. On the other hand, by setting the applied voltage to 600 V or less, the generation of many bubbles on the surface of the substrate can be suppressed, and the generation of many irregularities in the insulating coating due to the bursting of the bubbles in the subsequent baking step S103 can be suppressed.

[0045] (Baking process S103) In the baking step S103, the substrate on which the electrodeposited film containing the solid components polyamideimide and polytetrafluoroethylene obtained in the electrodeposition step S102 has been formed is dried, for example, within a temperature range of 200°C or higher and lower than the melting point of the solid components to remove the residual electrodeposition liquid, and then the electrodeposited film containing polyamideimide and polytetrafluoroethylene is baked onto the substrate to form an insulating coating.

[0046] The baking temperature in the baking step S103 may be within a temperature range in which the electrodeposited polyamideimide and polytetrafluoroethylene films are hardened to form an insulating film on the substrate, and may be within a range of, for example, 200° C. to 450° C. The baking time may be within a range of, for example, 1 minute to 60 minutes.

[0047] Through the above-mentioned steps, an insulating film containing a mixed resin of polyamideimide, which is a polyimide resin, and polytetrafluoroethylene, which is a fluorine resin, can be formed on a conductive substrate, which results in an insulating film with good insulation properties (e.g., a relative dielectric constant of less than 3.0) and excellent smoothness without cracks.

[0048] According to the electrodeposition liquid of this embodiment having the above-mentioned configuration, since it contains a polyimide-based resin and a fluorine-based resin as solid components, it is possible to form an insulating coating having excellent insulating properties. Furthermore, since the surfactant is contained in the range of 0.1 mass % or more and 5.0 mass % or less, the dispersibility of the polyimide-based resin and the fluororesin in the liquid is sufficiently high, the resin composition in the formed electrodeposition film is uniform, and the occurrence of defective appearance of the electrodeposition film can be suppressed.

[0049] In the electrodeposition liquid of the present embodiment, when the surfactant is a polyoxyalkylene alkyl ether, the dispersibility of the two types of resins, the polyimide resin and the fluorine resin, contained as solid components can be further improved, the resin composition becomes more uniform when a film is formed, and the occurrence of defective appearance can be further suppressed.

[0050] In the electrodeposition solution of the present embodiment, when the polyimide-based resin contained as a solid component is polyamideimide, it is possible to form an insulating film having excellent insulating properties together with the fluorine-based resin. In the electrodeposition solution of the present embodiment, when the fluorine-based resin contained as a solid component is polytetrafluoroethylene, it is possible to form an insulating film having excellent insulating properties together with the polyimide-based resin.

[0051] According to the method for producing an electrodeposited film of the present embodiment, a substrate and a counter electrode are immersed in the electrodeposition solution of the present embodiment, and the substrate is used as the anode and the counter electrode is used as the cathode, and a voltage is applied between the anode (substrate) and the cathode (counter electrode). This makes it possible to form an electrodeposited film on the surface of the substrate, which contains a polyimide-based resin and a fluorine-based resin and has a stable resin composition, and makes it possible to suppress the occurrence of defects in the appearance of the electrodeposited film.

[0052] In this embodiment, when the electrodeposition liquid is formed by adding a surfactant to the main electrodeposition liquid containing water, a dispersion medium, and solid components including a polyimide-based resin and a fluororesin immediately before forming the electrodeposition film, even if the main electrodeposition liquid deteriorates over time and the dispersibility of the polyimide-based resin and the fluororesin decreases, the dispersibility of the polyimide-based resin and the fluororesin can be improved by adding the surfactant, making it possible to produce an electrodeposition film that is free of streaks and has good appearance quality.

[0053] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. EXAMPLES

[0054] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.

[0055] The polyimide resin and fluororesin shown in Table 1 were prepared as solid components, and mixed to obtain a mixed resin dispersion (electrodeposition liquid main body) in the ratio (mass ratio) shown in Table 1. Then, a surfactant was added to the electrodeposition liquid main body as shown in Table 1. In Comparative Examples 1 and 2, no surfactant was added.

[0056] Then, a rectangular bar of oxygen-free copper (1.5 mm x 2.9 mm x 30 cm long) was prepared as a conductive substrate, and a copper plate was prepared as a counter electrode. The substrate and the counter electrode were immersed in the above-mentioned electrodeposition solution, and the temperature of the electrodeposition solution was set to 20° C. and the applied voltage was set to 300 V to form an electrodeposition film. In Examples 1 to 7 of the present invention, a surfactant was added to the electrodeposition solution to prepare the electrodeposition solution, and the electrodeposition film was formed using the electrodeposition film that had been stored at room temperature for 7 days. In Examples 8 to 12 of the present invention, the electrodeposition solution itself was stored at room temperature for 7 days, and a surfactant was added immediately before the formation of a deposited film. In Comparative Examples 1 and 2, the electrodeposition solution obtained by mixing the polyimide resin and the fluorine resin was stored at room temperature for 7 days, and then the electrodeposition film was formed.

[0057] The appearance of the electrodeposited film was observed to check for defects in appearance (streaks). Figure 3 shows a schematic diagram of the electrodeposited film whose appearance was observed. Figure 3(a) shows an electrodeposited film with no streaks and a good appearance. Figure 3(b) shows an electrodeposited film with streaks and a poor appearance.

[0058] [Table 1]

[0059] In Comparative Examples 1 and 2, streaks occurred all over the electrodeposition film, resulting in poor appearance. This is presumably because no surfactant was added to the electrodeposition solution, and storage at room temperature for 7 days reduced the dispersibility of the polyimide resin or fluorine resin in the electrodeposition solution, making it impossible to form an electrodeposition film with a uniform composition. In Comparative Example 3, streaks were partially generated in the electrodeposition film, resulting in poor appearance. This is presumably because the amount of surfactant added to the electrodeposition solution was small, and the electrodeposition solution was stored at room temperature for 7 days, which reduced the dispersibility of the polyimide resin or fluorine resin in the electrodeposition solution, making it impossible to form an electrodeposition film with a uniform composition.

[0060] In contrast, no streaks were generated in the electrodeposited films and the appearance was good in Inventive Examples 1 to 7, 13, and 14. It is presumed that, because the surfactant is contained, the dispersibility of the polyimide resin or fluororesin in the electrodeposition solution did not decrease even after storage at room temperature for 7 days, and an electrodeposition film with a uniform composition could be formed. In addition, in Examples 8 to 12 and 15 of the present invention, no streaks were generated in the electrodeposition film, and the appearance was good. It is presumed that the addition of a surfactant to the electrodeposition solution stored at room temperature for 7 days ensured the dispersibility of the polyimide resin or fluorine resin in the electrodeposition solution, and an electrodeposition film with a uniform composition was formed.

[0061] From the results of the above confirmatory experiments, it was confirmed that, according to the present invention, it is possible to provide an electrodeposition liquid and a method for producing an electrodeposition film that are capable of suppressing the occurrence of defective appearance of the electrodeposition film, even when the electrodeposition film is formed using an electrodeposition liquid containing a polyimide-based resin and a fluororesin.

Claims

1. An electrodeposition solution used in forming an electrodeposition film on a surface of a conductive substrate, comprising: The dispersion medium includes water, a dispersion medium, a solid component, and a surfactant, the solid component includes a polyimide resin and a fluorine resin, The electrodeposition solution is characterized in that the content of the surfactant is within the range of 0.1 mass % or more and 5.0 mass % or less.

2. 2. The electrodeposition solution according to claim 1, wherein the surfactant is a polyoxyalkylene alkyl ether.

3. 2. The electrodeposition solution according to claim 1, wherein the polyimide resin is polyamideimide.

4. 2. The electrodeposition solution according to claim 1, wherein the fluorine-based resin is polytetrafluoroethylene.

5. A method for producing an electrodeposited film for forming an electrodeposited film on a surface of a conductive substrate, comprising the steps of:

5. A method for producing an electrodeposited film, comprising: immersing a substrate and a counter electrode in the electrodeposition solution according to claim 1; using the substrate as an anode and the counter electrode as a cathode; and applying a voltage between the anode and the cathode to form the electrodeposited film on the surface of the substrate.

6. A method for producing an electrodeposited film for forming an electrodeposited film on a surface of a conductive substrate, comprising the steps of: a surfactant is added to the electrodeposition liquid body, the surfactant being added to the electrodeposition liquid body when forming an electrodeposition film; and A method for producing an electrodeposited film, comprising the steps of: immersing the substrate and a counter electrode in the electrodeposition solution; using the substrate as an anode and the counter electrode as a cathode; applying a voltage between the anode and the cathode; and forming the electrodeposited film on the surface of the substrate.

Citation Information

Patent Citations

  • Electro-deposition liquid, and production method of insulation film