Manufacturing method of stack
A method for manufacturing power storage cell stacks with controlled electrolyte distribution and load cycles stabilizes cell thickness, addressing stacking challenges and reducing swelling, ensuring consistent performance.
Patent Information
- Application Number
- JP2023055072
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
The challenge in manufacturing a stack of power storage cells is the difficulty in stacking cells with varying thickness due to inconsistent expansion and contraction, which is not solely determined by the spring constant of the electrode body, leading to swelling during charging and discharging.
A method involving a flat wound electrode body with controlled non-aqueous electrolyte distribution, applying a specific load cycle to stabilize cell thickness variation within 0.051 to 0.055%, ensuring easy stacking and reducing swelling during use.
The method effectively stabilizes cell thickness during assembly and usage, allowing for consistent stacking and minimizing swelling due to charging and discharging.
Smart Images

Figure 2024142761000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a stack. [Background technology]
[0002] In recent years, stacks including a plurality of storage cells have been suitably used as driving power sources mounted on vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), and electric vehicles (BEVs). Patent Document 1 is an example of a related prior art document. Patent Document 1 discloses a technology relating to a nonaqueous electrolyte secondary battery (storage cell) having an electrode body including a housing, a nonaqueous electrolyte (nonaqueous electrolyte), a positive electrode, a negative electrode, and a separator, and the electrode body further includes a low spring constant membrane having a spring constant (second spring constant) lower than the spring constant (first spring constant) of the negative electrode, thereby suppressing the extrusion of the nonaqueous electrolyte inside the electrode body due to the expansion and contraction of the electrode body. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-055806 A Summary of the Invention [Problem to be solved by the invention]
[0004] Incidentally, when stacking a plurality of storage cells in the thickness direction of the storage cells, if there is a large variation in thickness between the storage cells, stacking the storage cells becomes difficult. On the other hand, if a storage cell that suppresses the extrusion of the non-aqueous electrolyte too much is used in a stack, the storage cells stacked in the stack swell (increase in thickness) by repeatedly charging and discharging the stack. In addition, according to the study by the present inventor, it was found that the ease of extrusion of the non-aqueous electrolyte in the electrode body is not determined only by the spring constant of the constituent members of the electrode body as disclosed in Patent Document 1. Therefore, in manufacturing a stack including a plurality of storage cells, it is necessary to consider not only the variation in thickness between the storage cells when stacking the storage cells, but also the suppression of the swelling of the storage cells mounted in the stack when using the stack.
[0005] The technology disclosed herein has been made in consideration of the above circumstances, and its main purpose is to provide a manufacturing method for a stack that achieves both suppression of thickness variations among storage cells during assembly and suppression of swelling of the storage cells when the stack is in use. [Means for solving the problem]
[0006] The technology disclosed herein is a manufacturing method for a stack including a plurality of rectangular storage cells, the method including: a preparation step of preparing the storage cell including a flat-shaped wound electrode body formed by stacking and winding a positive electrode and a negative electrode with a separator interposed therebetween, a non-aqueous electrolyte, and a case for accommodating the wound electrode body and the non-aqueous electrolyte; and a stacking step of stacking a plurality of the storage cells in a thickness direction of the storage cell, and a stacking step of stacking the storage cells in a thickness direction of the storage cell in the preparation step. The method is characterized in that when a process in which a load is applied up to 2.0 MPa at a rate of 0.1 mm / min and then the load is reduced to 0.01 MPa after the application is performed for three cycles, an amount of change ((X1-X3) / X1x100) (hereinafter also referred to as "amount of change in cell thickness") in thickness X3 of the storage cell when 2.0 MPa is applied in the third cycle relative to a thickness X1 of the storage cell when 2.0 MPa is applied in the first cycle is 0.051 to 0.055%.
[0007] The storage cells prepared in the preparation step are 0.051 to 0.055%. In a storage cell having such a configuration, the thickness variation among the storage cells is suppressed at the preparation step. Therefore, the storage cells can be easily stacked (assembled) in the stacking step. On the other hand, a storage cell having a cell thickness change amount within the above range suppresses swelling of the storage cell due to charging and discharging. Therefore, according to the manufacturing method disclosed herein, it is possible to provide a stack in which the thickness variation among the storage cells is suppressed even when the stack is constructed, and the thickness of the storage cells is stable even when the stack is in use. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a perspective view illustrating a stack according to an embodiment. [Diagram 2] FIG. 2 is a perspective view of the electricity storage cell. [Diagram 3] FIG. 3 is a schematic vertical cross-sectional view taken along line III-III in FIG. [Figure 4] FIG. 4 is a perspective view that shows a schematic view of a wound electrode body attached to a sealing plate. [Diagram 5] FIG. 5 is a perspective view showing a schematic diagram of a wound electrode body. [Figure 6] FIG. 6 is a schematic diagram showing the configuration of a wound electrode body. [Figure 7] FIG. 7 is a flow diagram showing a method for manufacturing a stack according to one embodiment. [Figure 8] 8 is a schematic diagram for explaining the change in thickness of the wound electrode body. (A) shows a wound electrode body with a small amount of nonaqueous electrolyte. (B) shows a wound electrode body with a large amount of nonaqueous electrolyte. (C) shows a wound electrode body with a large amount of nonaqueous electrolyte and further with a nonaqueous electrolyte layer. [Figure 9] FIG. 9 is a schematic diagram illustrating the measurement of the cell thickness change amount in the preparation step. [Figure 10] FIG. 10 is a flow diagram showing a method for manufacturing an electricity storage cell according to one embodiment. [Figure 11]FIG. 11 is a graph showing the relationship between the cell thickness change amount and the cell thickness variation. [Figure 12] FIG. 12 is a graph showing the relationship between the amount of change in cell thickness and the cell expansion rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, some preferred embodiments of the stack disclosed herein will be described with reference to the drawings as appropriate. Matters other than those specifically mentioned in this specification and necessary for carrying out the present disclosure (for example, the general configuration and manufacturing process of the storage cell that do not characterize the present disclosure) can be understood as design matters of a person skilled in the art based on the prior art in the field. The stack disclosed herein can be carried out based on the contents disclosed in this specification and the technical common sense in the field.
[0010] In the following drawings, the same reference numerals are used for components and parts having the same function, and duplicated explanations may be omitted or simplified. In addition, in this specification, the expression "A to B" indicating a range includes the meaning of "A or more and B or less," as well as "preferably larger than A" and "preferably smaller than B."
[0011] FIG. 1 is a perspective view showing a stack 500 according to an embodiment. The stack 500 includes a plurality of storage cells 100 and a restraining mechanism 300. Although not shown here for convenience of explanation, the plurality of storage cells 100 of the stack 500 are electrically connected by a bus bar. In the following description, the symbols L, R, F, Rr, U, and D in the drawings represent left, right, front, rear, top, and bottom, and the symbols X, Y, and Z in the drawings represent the short side direction, long side direction perpendicular to the short side direction, and up and down direction of the storage cell 100, respectively. The short side direction X is also the arrangement direction of the storage cells 100. However, these are merely directions for convenience of explanation and do not limit the installation form of the stack 500 in any way.
[0012] The restraining mechanism 300 is configured to apply a prescribed restraining pressure to the multiple energy storage cells 100 from the thickness direction X. Here, the restraining mechanism 300 is configured with a pair of end plates 310, a pair of side plates 320, and multiple screws 330. The pair of end plates 310 are aligned in a predetermined thickness direction X. The pair of end plates 310 are arranged at both ends of the stack 500 in the thickness direction X. The multiple energy storage cells 100 are arranged between the pair of end plates 310 along the thickness direction X. An insulating sheet, an inter-cell separator, or the like may be arranged between the multiple energy storage cells 100.
[0013] The pair of side plates 320 bridge the pair of end plates 310. The pair of side plates 320 are fixed to the end plates 310 by a plurality of screws 330 so that the restraining load is, for example, approximately 5 to 20 kN. As a result, a restraining load is applied to the plurality of energy storage cells 100 and the plurality of porous elastic members 200 from the thickness direction X, and the stack 500 is held integrally. However, the restraining mechanism is not limited to this. The restraining mechanism 300 may include, for example, a plurality of restraining bands, bind bars, or the like, instead of the side plates 320.
[0014] <Electricity storage cell 100> In this specification, the term "storage cell" refers to a device that can be repeatedly charged and discharged. The storage cell includes batteries generally called lithium ion batteries and lithium secondary batteries, as well as lithium polymer batteries and lithium ion capacitors. A secondary battery generally refers to a battery that can be repeatedly charged and discharged by the movement of charge carriers between the positive and negative electrodes. Here, a lithium ion secondary battery is exemplified as one form of storage cell.
[0015] Fig. 2 is a perspective view of the storage cell 100. As shown in Figs. 1 and 2, the multiple storage cells 100 are arranged in the thickness direction X such that first side walls 12b described below face each other. Fig. 3 is a schematic vertical cross-sectional view taken along line III-III in Fig. 2. As shown in Fig. 3, the storage cell 100 includes a case 10, a wound electrode body 20, a non-aqueous electrolyte (not shown), and further includes a positive electrode terminal 30, a negative electrode terminal 40, a positive electrode current collector 50, and a negative electrode current collector 60. Here, the storage cell 100 is a lithium ion secondary battery.
[0016] The case 10 is a housing that houses the wound electrode body 20 and the non-aqueous electrolyte. As shown in FIG. 2, the case 10 has a flat, bottomed rectangular parallelepiped (rectangular) outer shape. The material of the case 10 may be the same as that used conventionally, and is not particularly limited. The case 10 is preferably made of a metal, and more preferably made of, for example, aluminum, an aluminum alloy, iron, an iron alloy, or the like. As shown in FIG. 2, the case 10 includes an exterior body 12 having an opening 12h, and a sealing plate (lid) 14 that seals the opening 12h. As in this embodiment, the case 10 preferably includes an exterior body 12 having an opening 12h, and a sealing plate 14 that seals the opening 12h.
[0017] As shown in Fig. 2, the exterior body 12 includes a bottom 12a, a pair of first side walls 12b extending from the bottom 12a and facing each other, and a pair of second side walls 12c extending from the bottom 12a and facing each other. The bottom 12a is substantially rectangular. The bottom 12a faces the opening 12h. The first side wall 12b is flat. The first side wall 12b extends from a long side of the bottom 12a. The second side wall 12c extends from a short side of the bottom 12a. In a plan view, the area of the first side wall 12b is larger than the area of the second side wall 12c.
[0018] The sealing plate 14 is attached to the exterior body 12 so as to close the opening 12h of the exterior body 12. The sealing plate 14 faces the bottom 12a of the exterior body 12. The sealing plate 14 has a substantially rectangular shape in a plan view. The case 10 is integrated by joining (preferably welding) the sealing plate 14 to the periphery of the opening 12h of the exterior body 12. The case 10 is hermetically sealed (sealed).
[0019] As shown in FIG. 3, the sealing plate 14 is provided with a liquid inlet 15, a drain valve 17, and two terminal outlet holes 18 and 19. The liquid inlet 15 is for injecting a non-aqueous electrolyte after the sealing plate 14 is assembled to the exterior body 12. The liquid inlet 15 is sealed by a sealing member 16. The drain valve 17 is configured to break when the pressure inside the case 10 reaches or exceeds a predetermined value, thereby discharging the gas inside the case 10 to the outside. The terminal outlet holes 18 and 19 penetrate the sealing plate 14 in the vertical direction Z. The terminal outlet holes 18 and 19 each have an inner diameter large enough to insert the positive electrode terminal 30 and the negative electrode terminal 40 before being attached to the sealing plate 14 (before being crimped).
[0020] The non-aqueous electrolyte may be the same as the conventional one, and is not particularly limited. The non-aqueous electrolyte contains a non-aqueous solvent and a supporting salt (electrolyte salt). The non-aqueous electrolyte may further contain additives as necessary. The non-aqueous solvent contains, for example, carbonates such as ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate. The non-aqueous solvent preferably contains carbonates. In particular, it is preferable that the non-aqueous solvent contains a cyclic carbonate and a chain carbonate. The supporting salt is, for example, a fluorine-containing lithium salt such as lithium hexafluorophosphate (LiPF6). Examples of additives that can be contained in the non-aqueous electrolyte include, for example, a film-forming agent, a gas generating agent, a dispersant, and a thickener. Examples of the film-forming agent include carbonate compounds such as vinylene carbonate (VC), vinylethylene carbonate (VEC), fluoroethylene carbonate (FEC), chloroethylene carbonate, and methylphenyl carbonate; and lithium salts having an oxalato complex as the anion, such as lithium bis(oxalato)borate (LiBOB), lithium difluoro(oxalato)borate (LiFOB), and lithium difluorobis(oxalato)phosphate (LPFO).
[0021] The positive electrode terminal 30 is disposed at one end of the sealing plate 14 in the long side direction Y (the left end in FIG. 2 and FIG. 3). The negative electrode terminal 40 is disposed at the other end of the sealing plate 14 in the long side direction Y (the right end in FIG. 2 and FIG. 3). As shown in FIG. 3, the positive electrode terminal 30 and the negative electrode terminal 40 extend from the inside to the outside of the sealing plate 14 through the terminal drawing holes 18 and 19. The positive electrode terminal 30 and the negative electrode terminal 40 are fixed to the sealing plate 14. Here, the positive electrode terminal 30 and the negative electrode terminal 40 are crimped to the peripheral portion surrounding the terminal drawing holes 18 and 19 of the sealing plate 14 by crimping. The crimped portions 30c and 40c are formed at the ends of the positive electrode terminal 30 and the negative electrode terminal 40 on the exterior body 12 side (the lower end in FIG. 3).
[0022] As shown in Fig. 3, the positive electrode terminal 30 is electrically connected to the positive electrode 22 (see Fig. 6) of the wound electrode body 20 via the positive electrode current collector 50 inside the exterior body 12. The negative electrode terminal 40 is electrically connected to the negative electrode 24 (see Fig. 6) of the wound electrode body 20 via the negative electrode current collector 60 inside the exterior body 12. The positive electrode terminal 30 is insulated from the sealing plate 14 by an internal insulating member 80 and a gasket 90. The negative electrode terminal 40 is insulated from the sealing plate 14 by an internal insulating member 80 and a gasket 90.
[0023] A plate-shaped positive electrode external conductive member 32 and a plate-shaped negative electrode external conductive member 42 are attached to the outer surface of the sealing plate 14. The positive electrode external conductive member 32 is electrically connected to the positive electrode terminal 30. The negative electrode external conductive member 42 is electrically connected to the negative electrode terminal 40. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are members to which a bus bar or the like is attached to electrically connect the multiple storage cells 100 to each other. The positive electrode external conductive member 32 and the negative electrode external conductive member 42 are insulated from the sealing plate 14 by an external insulating member 92. Although not shown in FIG. 1, when the stack 500 is used, the adjacent storage cells 100 are electrically connected to each other. For example, among the adjacent storage cells 100, the positive electrode external conductive member 32 of one storage cell 100 and the negative electrode external conductive member 42 of the other storage cell 100 are electrically connected by a bus bar or the like. As a result, the stack 500 is electrically connected. The stack 500 may be connected in series, in parallel, or in a so-called multi-series / multi-parallel connection which is a combination of series and parallel.
[0024] FIG. 4 is a perspective view that shows a schematic diagram of the wound electrode body 20 attached to the sealing plate 14. The wound electrode body 20 has three wound electrode bodies 20 here. However, the number of electrode bodies arranged inside one exterior body 12 is not particularly limited, and may be one or more (two or more). The wound electrode bodies 20 are electrically connected in parallel here. The wound electrode body 20 is arranged inside the exterior body 12 with the winding axis WL (see FIG. 6) oriented substantially parallel to the long side direction Y. The wound electrode bodies 20 are arranged side by side in a direction (short side direction X) in which the thickness direction of the energy storage cell 100 (in other words, a direction substantially perpendicular to the first side wall 12b of the case 10) and the thickness direction of the wound electrode body 20 coincide with each other. The wound electrode body 20 preferably has a flattened outer shape. An end face of the wound electrode body 20 perpendicular to the winding axis WL (in other words, a layered surface where the positive electrode 22 and the negative electrode 24 are layered) faces the second side wall 12c. Although not shown, an insulating sheet is disposed between the wound electrode body 20 and the exterior body 12.
[0025] FIG. 5 is a perspective view showing a schematic diagram of the wound electrode body 20. Note that all the wound electrode bodies 20 housed in the case 10 can have the same configuration. The wound electrode body 20 has a pair of curved portions (R portions) 20r and a flat portion 20f connecting the pair of curved portions 20r. One curved portion 20r (upper side of FIG. 5) faces the sealing plate 14, and the other curved portion 20r (lower side of FIG. 5) faces the bottom portion 12a of the exterior body 12. The flat portion 20f faces the first side wall 12b of the exterior body 12. Here, the flat portions 20f of the multiple wound electrode bodies 20 adjacent to each other in the short side direction X face each other.
[0026] 6 is a schematic diagram showing the configuration of the wound electrode body 20. The wound electrode body 20 has a positive electrode 22, a negative electrode 24, and a separator 26. In this example, the wound electrode body 20 is configured by stacking a strip-shaped positive electrode 22 and a strip-shaped negative electrode 24 with a strip-shaped separator 26 interposed therebetween, and winding them in the longitudinal direction around a winding axis WL. The direction of the winding axis WL is approximately parallel to the long side direction Y.
[0027] As shown in FIG. 6, the positive electrode 22 has a positive electrode core 22c, and a positive electrode active material layer 22a and a positive electrode protective layer 22p fixed on at least one surface of the positive electrode core 22c. However, the positive electrode protective layer 22p is not essential and can be omitted in other embodiments. The positive electrode core 22c is strip-shaped. The positive electrode core 22c is preferably a metal foil, more preferably an aluminum foil or an aluminum alloy foil. The positive electrode core 22c is an aluminum foil here. The number of layers of the positive electrode 22 is preferably 30 or more.
[0028] A plurality of positive electrode tabs 22t are provided at one end of the positive electrode core 22c in the long side direction Y (the left end in FIG. 6). The plurality of positive electrode tabs 22t protrude toward one side of the long side direction Y (the left side in FIG. 6). The plurality of positive electrode tabs 22t protrude in the long side direction Y beyond the separator 26. The positive electrode tab 22t is a part of the positive electrode core 22c here, and is made of a metal foil (aluminum foil). The thickness of the positive electrode core 22c is not particularly limited, but is preferably 5 to 30 μm, and more preferably 10 to 25 μm. As shown in FIG. 3 to FIG. 6, the plurality of positive electrode tabs 22t are stacked at one end of the long side direction Y (the left end in FIG. 3 to FIG. 6) to form a positive electrode tab group 23. The positive electrode tab group 23 is electrically connected to the positive electrode terminal 30 via the positive electrode current collector 50.
[0029] As shown in FIG. 6, the positive electrode active material layer 22a is provided in a strip shape along the longitudinal direction of the positive electrode core 22c. The positive electrode active material layer 22a contains a positive electrode active material capable of reversibly absorbing and releasing charge carriers. Examples of the positive electrode active material include lithium transition metal composite oxides. The positive electrode active material layer 22a may contain various additive components such as optional components other than the positive electrode active material, such as a binder and a conductive material, and preferably contains a conductive material and a binder as additive components. Examples of the binder used in the positive electrode active material layer 22a include polyvinylidene fluoride (PVdF). The conductive material used in the positive electrode active material layer 22a is not particularly limited, but a carbon material is preferably used. The density of the positive electrode active material layer 22a is preferably 3.0 g / cc or more, more preferably 3.5 g / cc or more. On the other hand, the density of the positive electrode active material layer 22a is preferably 3.7 g / cc or less.
[0030] As shown in Fig. 6, the positive electrode protective layer 22p is provided at the boundary between the positive electrode core 22c and the positive electrode active material layer 22a in the long side direction Y. The positive electrode protective layer 22p is provided in a strip shape along the positive electrode active material layer 22a. The positive electrode protective layer 22p contains an inorganic filler (e.g., alumina). The positive electrode protective layer 22p may contain any component other than the inorganic filler, such as a conductive material, a binder, various additive components, and the like.
[0031] As shown in FIG. 6, the negative electrode 24 has a negative electrode core 24c and a negative electrode active material layer 24a fixed on at least one surface of the negative electrode core 24c. The negative electrode core 24c is strip-shaped. The negative electrode core 24c is preferably a metal foil, more preferably a copper foil or a copper alloy foil. The negative electrode core 24c is a copper foil here.
[0032] A plurality of negative electrode tabs 24t are provided at one end of the negative electrode core 24c in the long side direction Y (the right end in FIG. 6). The plurality of negative electrode tabs 24t protrude toward one side of the long side direction Y (the right end in FIG. 6). The plurality of negative electrode tabs 24t protrude in the long side direction Y beyond the separator 26. The negative electrode tab 24t is a part of the negative electrode core 24c here, and is made of a metal foil (copper foil). The thickness of the negative electrode core 24c is not particularly limited, but is preferably 5 to 30 μm, and more preferably 5 to 15 μm. As shown in FIG. 3 to FIG. 6, the plurality of negative electrode tabs 24t are stacked at one end of the long side direction Y (the right end in FIG. 3 to FIG. 6) to form a negative electrode tab group 25. The negative electrode tab group 25 is provided at a position symmetrical to the positive electrode tab group 23 in the long side direction Y. The negative electrode tab group 25 is electrically connected to the negative electrode terminal 40 via the negative electrode current collecting portion 60 .
[0033] As shown in FIG. 6, the negative electrode active material layer 24a is provided in a strip shape along the longitudinal direction of the negative electrode core 24c. The negative electrode active material layer 24a contains a negative electrode active material capable of reversibly absorbing and releasing charge carriers. For example, graphite, a silicon-based material (a silicon-containing material), and a mixed oxide thereof are preferably used as the negative electrode active material. The negative electrode active material layer 24a may contain any component other than the negative electrode active material, for example, various additive components such as a binder, a thickener, and a dispersant. For example, a binder used in the negative electrode active material layer 24a includes styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC). The conductive material used in the negative electrode active material layer 24a is not particularly limited, but a carbon material is preferably used. The density of the negative electrode active material layer 24a is preferably 1.3 g / cc or more, more preferably 1.4 g / cc or more. On the other hand, the density of the negative electrode active material layer 24a is preferably 1.7 g / cc or less.
[0034] The length Ln of the negative electrode active material layer 24a in the width direction Y is equal to or longer than the length La of the positive electrode active material layer 22a in the width direction Y. Here, the length Ln of the negative electrode active material layer 24a in the width direction Y is preferably 20 cm or more. Although details will be described later, this configuration allows the non-aqueous electrolyte in the wound electrode body 20 to be suitably controlled to be pushed out of the wound electrode body 20. In addition, when the length in a direction perpendicular to the winding axis WL direction of the wound electrode body 20 and perpendicular to the thickness direction X of the wound electrode body 20 (here, the Z direction) is defined as the height T of the wound electrode body 20, it is preferable that the ratio (Ln / T) of the length Ln in the width direction of the negative electrode active material layer 24a to the height T of the wound electrode body 20 (hereinafter, also referred to as the "electrode body aspect ratio") is 2.8 to 3.2. This configuration allows the non-aqueous electrolyte in the wound electrode body 20 to be suitably controlled to be pushed out of the wound electrode body 20. In the specification, "height T of the wound electrode body 20" refers to the distance in the Z direction from the uppermost end of one curved portion 20r of the wound electrode body 20 (U side in Figure 5) to the lowermost end of the other curved portion 20r (D side in Figure 5).
[0035] The separator 26 is a member that insulates the positive electrode active material layer 22a of the positive electrode 22 from the negative electrode active material layer 24a of the negative electrode 24. The separator 26 constitutes the outer surface of the wound electrode body 20. The length Ls of the separator 26 in the long side direction Y is equal to or longer than the length Ln of the negative electrode active material layer 24a in the long side direction Y. The separator 26 may have a heat-resistant layer formed on at least one surface thereof, for example, containing ceramic particles and a binder. The separator 26 may also have an adhesive layer formed on at least one surface thereof, which contains a binder. The adhesive layer may be formed to have a shape such as a dot shape, a stripe shape, a wave shape, a band shape (stripes), a dashed line shape, or a combination thereof, in a plan view.
[0036] The separator 26 is preferably a sheet-shaped member of a microporous film. The separator 26 is preferably made of a polyolefin resin. Examples of the polyolefin resin that can be used include polyethylene (PE), polypropylene (PP), and a mixture thereof.
[0037] There is no particular limitation on the thickness of the separator 26. When the non-aqueous electrolyte is not present in the separator 26, the thickness of the separator 26 is preferably about 10 to 30 μm. In addition, in the present specification, the "thickness of the separator 26" refers to the thickness including the adhesive layer and the heat-resistant layer when the separator 26 has an adhesive layer and a heat-resistant layer, and refers to the thickness before the press molding process unless otherwise specified.
[0038] As shown in FIG. 3, the positive electrode current collecting part 50 constitutes a conductive path that electrically connects the positive electrode tab group 23 consisting of a plurality of positive electrode tabs 22t and the positive electrode terminal 30. The positive electrode current collecting part 50 includes a positive electrode first current collecting part 51 and a positive electrode second current collecting part 52. The positive electrode first current collecting part 51 is attached to the inner surface of the sealing plate 14. The positive electrode second current collecting part 52 extends along the second side wall 12c of the exterior body 12. As shown in FIGS. 3 to 5, the positive electrode second current collecting part 52 is attached to the wound electrode body 20.
[0039] 3, the negative electrode current collecting part 60 constitutes a conductive path that electrically connects the negative electrode tab group 25 consisting of the multiple negative electrode tabs 24t to the negative electrode terminal 40. The negative electrode current collecting part 60 includes a negative electrode first current collecting part 61 and a negative electrode second current collecting part 62. The configurations of the negative electrode first current collecting part 61 and the negative electrode second current collecting part 62 may be the same as those of the positive electrode first current collecting part 51 and the positive electrode second current collecting part 52 of the positive electrode current collecting part 50.
[0040] <Stack 500 manufacturing method> 7 is a flow diagram showing a method for manufacturing a stack 500 according to an embodiment. The stack 500 disclosed herein can be manufactured by a manufacturing method including a preparation step S10 and a stacking step S20, and is characterized by performing the preparation step S10. In addition to the above steps, the manufacturing method for the stack 500 disclosed herein may further include other steps at any stage, and the other manufacturing processes may be the same as conventional methods.
[0041] (Preparation step S10) In the preparation step S10, an energy storage cell 100 is prepared, which includes the above-described wound electrode body 20, a non-aqueous electrolyte, and a case 10. In the preparation step S10, the energy storage cell 100 may be purchased and prepared, or the energy storage cell 100 may be manufactured and prepared.
[0042] Here, the storage cell 100 prepared in the preparation step S10 is characterized in that when a load is applied to the storage cell 100 in the thickness direction (X direction in FIG. 1) at a rate of 0.1 mm / min up to 2.0 MPa and the load is then reduced to 0.01 MPa after the load is applied, and the process is repeated for three cycles, the amount of change ((X1-X3) / X1×100) (hereinafter also referred to as "cell thickness change") in the thickness X3 of the storage cell 100 when 2.0 MPa is applied in the third cycle relative to the thickness X1 of the storage cell 100 when 2.0 MPa is applied in the first cycle is 0.051 to 0.055%. In this specification, the "cell thickness change" is determined by measurement using an autograph.
[0043] For example, when there is variation in the ease with which the non-aqueous electrolyte in the wound electrode body 20 is pushed out for each storage cell 100 (i.e., when the cell thickness variation is large), in other words, when there is variation in the thickness (thickness in the X direction) of the storage cells 100, stacking (assembly) of the storage cells 100 becomes difficult in the subsequent stacking step S20. The thickness of the storage cells 100 varies depending on, for example, the thickness of the wound electrode body 20. In more detail, the thickness of the wound electrode body 20 is determined by the ease with which the non-aqueous electrolyte is pushed out when the non-aqueous electrolyte present in the wound electrode body 20 goes out of the wound electrode body 20 when the wound electrode body 20 is pressed in the thickness direction X of the wound electrode body. In other words, it is determined by the amount of non-aqueous electrolyte in the wound electrode body 20 after the pressing.
[0044] FIG. 8 is a schematic diagram for explaining the change in thickness of the wound electrode body 20. In FIG. 8, a part of the wound electrode body 20 is partially enlarged. FIG. 8 (A) shows the wound electrode body 20 with a small amount of nonaqueous electrolyte. FIG. 8 (B) shows the wound electrode body 20 with a large amount of nonaqueous electrolyte. FIG. 8 (C) shows the wound electrode body 20 with a large amount of nonaqueous electrolyte and a nonaqueous electrolyte layer 28. The nonaqueous electrolyte in the wound electrode body 20 may be present, for example, inside the separator 26. When the nonaqueous electrolyte is present inside the separator 26, the thickness of the separator 26 becomes thicker by the amount of the nonaqueous electrolyte present, and the thickness of the wound electrode body 20 changes. As shown in FIG. 8, the thickness of the wound electrode body 20 differs depending on whether the amount of nonaqueous electrolyte is large or small, due to the difference in the thickness of the separator 26. Furthermore, the non-aqueous electrolyte may also be present as a non-aqueous electrolyte layer 28 between the separator 26 and the positive electrode active material layer 22a, or between the separator 26 and the negative electrode active material layer 24a, as shown in Fig. 8(C). When the non-aqueous electrolyte layer 28 is present in the wound electrode body 20, as shown in Fig. 8(C), the thickness of the wound electrode body 20 becomes even greater.
[0045] On the other hand, in order to make the thickness of the energy storage cells 100 constant (to suppress variations), it is conceivable to make it difficult for the non-aqueous electrolyte to be pushed out from the wound electrode body 20 (i.e., to reduce the amount of change in cell thickness). In other words, it is conceivable to make the thickness of the energy storage cells 100 constant by leaving a large amount of non-aqueous electrolyte inside the wound electrode body 20. However, if an excessively large amount of non-aqueous electrolyte remains inside the wound electrode body 20, the energy storage cells 100 stacked in the stack 500 will swell significantly due to charging and discharging when the stack 500 is in use.
[0046] Therefore, the technology disclosed herein is characterized in that the storage cells 100 having a cell thickness variation of 0.051 to 0.055% are prepared. In the storage cells 100 having such a configuration, the thickness variation among the storage cells 100 is suppressed at the preparation step S10, so that the storage cells 100 can be easily stacked (assembled) in the stacking step S20. On the other hand, the storage cells 100 having a cell thickness variation within the above range suppress swelling of the storage cells 100 due to charging and discharging. Therefore, it is possible to provide a stack 500 in which the thickness variation of the storage cells 100 is suppressed even when the stack 500 is constructed, and the thickness of the storage cells 100 is stable even when the stack 500 is used.
[0047] FIG. 9 is a schematic diagram for explaining the measurement of the cell thickness change amount in the preparation step S10. In FIG. 9, the direction in which the autograph 600 applies a load in the thickness direction of the storage cell 100 is illustrated by a white arrow. As shown in FIG. 9, the storage cell 100 is first set in the autograph 600 so that a load is applied in the thickness direction (white arrow direction). As shown in FIG. 9, the storage cell 100 is set so that a pair of first side walls 12b of the storage cell 100 and the autograph 600 abut against each other. When the storage cell 100 is viewed in the horizontal direction, the autograph 600 is set so that a load is applied to the flat portion 20f of the wound electrode body 20 by the autograph 600. Here, the storage cell 100 is set in the autograph 600 so that a load is applied to the portion shown by the imaginary line in FIG. 3. Then, the storage cell 100 is loaded in the thickness direction of the storage cell 100 (illustrated by the white arrow) at a speed of 0.1 mm / min. When the load reaches 2 MPa, the thickness of the energy storage cell 100 is measured by a displacement meter (not shown), and this thickness is designated as X1. Thereafter, the load on the energy storage cell 100 is reduced to 0.01 MPa. The above cycle is counted as one cycle, and the process is repeated three times. Then, in the third cycle, when the load reaches 2 MPa, the thickness of the energy storage cell 100 is designated as X3. Then, the cell thickness change amount (%) is calculated by the following formula (i). Cell thickness change (%) = (X1-X3) / X1×100 Formula (i)
[0048] The means for measuring the thickness displacement of the energy storage cell 100 is not particularly limited, and for example, a laser displacement meter (for example, product name IL-S025 manufactured by Keyence Corporation) or the like can be used. The thickness of the energy storage cell 100 may be measured at one location or at multiple locations (two or more locations). When the thickness displacement of the energy storage cell 100 is measured at multiple locations, X1 and X3 can be determined by calculating average values from the measurements at the multiple locations.
[0049] In the preparation step S10, a storage cell 100 having a cell thickness change amount in the numerical range of 0.051 to 0.055% may be prepared, or the cell thickness change amount may be measured in the preparation step S10 by the method described above to confirm that the cell thickness change amount of the storage cell 100 is in the numerical range of 0.051 to 0.055%.
[0050] (Lamination process S20) In the stacking step S20, the multiple energy storage cells 100 are stacked along the thickness direction X of the energy storage cells 100. The stacking step S20 may be the same as a conventionally known stack manufacturing method. Here, the multiple energy storage cells 100 are sandwiched between a pair of end plates 310 in the arrangement direction X, and are constrained by side plates 320 and multiple screws 330. In this manner, the stack 500 according to this embodiment is manufactured.
[0051] <Method of manufacturing the energy storage cell 100> Although not particularly limited, the storage cell 100 in the preparation step S10 can be prepared, for example, by the manufacturing method shown below. The manufacturing method of the storage cell 100 shown below is an example of the preparation step S10 in this specification. FIG. 10 is a flow diagram showing a manufacturing method of the storage cell 100 according to one embodiment. As shown in FIG. 10, although not particularly limited, the storage cell 100 can be manufactured by a manufacturing method that typically includes, for example, an assembly step S101, a drying step S102, a liquid injection step S103, a degassing and charging step S104, a pressure reduction step S105, a liquid injection hole sealing step S106, an activation step S107, and an aging step S108 in this order. In addition, in the manufacturing method of the storage cell 100 disclosed herein, in addition to the above steps, other steps may be further included at any stage, and the other manufacturing processes may be the same as those of the conventional method.
[0052] (Assembly process S101) In the assembly process S101, the wound electrode body 20 is placed in the case 10 (exterior body 12) to prepare an assembly. In this specification, the term "assembly" refers to an electricity storage cell that has been assembled to a state prior to the liquid injection hole sealing process described later.
[0053] In the assembly process S101, the positive electrode second current collecting portion 52 is attached to the positive electrode tab group 23 of the wound electrode body 20, and further the negative electrode current collecting portion 60 and the negative electrode second current collecting portion 62 are attached to the negative electrode tab group 25. Next, the positive electrode terminal 30 and the negative electrode terminal 40 are attached to the sealing plate 14. Next, the positive electrode terminal 30 and the positive electrode first current collecting portion 51, and the negative electrode terminal 40 and the negative electrode first current collecting portion 61 are respectively joined by a conventionally known method (for example, ultrasonic joining, resistance welding, laser welding, etc.). Next, the wound electrode body 20 is accommodated in an insulating sheet. The insulating sheet can be prepared by folding an insulating resin sheet made of a resin material such as polyethylene (PE) into a bag shape or a box shape. Then, it is preferable to accommodate (insert) the wound electrode body 20 covered with the insulating sheet into the internal space of the exterior body 12. Then, the exterior body 12 of the case 10 and the sealing plate 14 are joined to prepare an assembly. Such joining can be performed by welding, for example, laser welding, etc. In the assembly step S101, the liquid injection hole 15 is not sealed.
[0054] In the assembly process S101, the wound electrode body 20 is preferably arranged side by side in a direction (short side direction X) in which the thickness direction of the energy storage cell 100 (in other words, a direction substantially perpendicular to the first side wall 12b of the case 10) coincides with the thickness direction of the wound electrode body 20. In other words, the wound electrode body 20 is preferably arranged inside the exterior body 12 with the winding axis WL parallel to the bottom 12a of the exterior body 12.
[0055] (Drying process S102) In the drying step S102, the assembly is dried to remove moisture contained in the assembly (e.g., the inside of the wound electrode body 20, etc.). Such a drying method can be performed by a known method. For example, the drying step S102 can be performed by transporting the assembly (the case 10 containing the wound electrode body 20) to a drying furnace (not shown) and heating it.
[0056] The drying temperature and drying time in the drying step S102 can be appropriately adjusted according to the amount of moisture contained in the wound electrode body 20. The drying temperature is not particularly limited as long as it is within a range in which moisture can be removed, but it is desirable to dry at a temperature at which the separator 26 of the wound electrode body 20 is not damaged. In addition, the drying step S102 is preferably performed in a reduced pressure atmosphere. This allows the drying time in the drying step S102 to be shortened. However, this is not limited to this, and the drying step S102 may be performed in an atmospheric pressure atmosphere. Note that the drying step S102 is not an essential step in the technology disclosed herein. In some preferred embodiments, the drying step S102 can be omitted.
[0057] (Liquid injection process S103) In the liquid injection step S103, a non-aqueous electrolyte is injected into the case 10 housing the wound electrode body 20 through the liquid injection hole 15 provided in the sealing plate 14. The liquid injection step S103 may be performed in an atmospheric pressure atmosphere or a reduced pressure atmosphere, but is preferably performed in a reduced pressure atmosphere. This improves the impregnation of the non-aqueous electrolyte into the wound electrode body 20, and the liquid injection step S103 can be performed in a shorter time. In the liquid injection step S103, the non-aqueous electrolyte is injected so that the amount of the non-aqueous electrolyte is sufficient to cover the entire wound electrode body 20. In the liquid injection step S103, a conventionally known non-aqueous electrolyte injection device can be appropriately used. At this time, examples of the pressure-transfer gas that can be used to pressure-transfer the non-aqueous electrolyte include an inert gas such as nitrogen (N2), dry air, and the like, as in the conventional case. After the liquid injection step S103 is completed, it is preferable to appropriately pressurize or depressurize the inside of the case 10.
[0058] (Gas removal and charging process S104) In the degassing charging step S104, the assembly is charged. This allows a coating to be formed on the surface of the negative electrode active material layer 24a. Furthermore, by discharging the gas generated during charging and discharging to the outside of the case 10, the amount of gas generated inside the case 10 after the liquid injection hole 15 is sealed can be reduced, and gas can be prevented from accumulating inside the wound electrode body 20 after the liquid injection hole 15 is sealed. The charging conditions in this step are not particularly limited, and may be the same as those in conventional manufacturing methods. Although not particularly limited, for example, the degassing charging step S104 can be performed by charging at a current of about 0.05C to 1C in a room temperature environment (for example, 25°C) until the SOC (State of Charge) becomes about 5% to 20%.
[0059] (Decompression step S105) In the depressurization step S105, the pressure inside the case 10 is reduced, thereby further discharging gas present inside the case 10 (for example, air or gas generated in the degassing / charging step S104) to the outside of the case 10. The depressurization step S105 may be the same as the means used in the depressurization step in this type of conventional manufacturing method, and is not a particular feature of the technology disclosed herein, so further detailed description will be omitted. Note that the depressurization step S105 is not an essential step in the technology disclosed herein. In some preferred embodiments, the depressurization step S105 can be omitted.
[0060] (Injection hole sealing process S106) In the liquid injection hole sealing step S106, the liquid injection hole 15 of the assembly is sealed. The liquid injection hole sealing step S106 may be the same as a conventionally known method for manufacturing the energy storage cell 100, and is not particularly limited. Here, the liquid injection hole 15 is sealed with a metallic sealing member 16, and is sealed by welding a metal portion of the sealing member 16 to the sealing plate 14 (the peripheral portion of the liquid injection hole 15). However, the method for sealing the liquid injection hole 15 is not limited to this. Although not shown in the drawings, the liquid injection hole 15 may be sealed with a rivet such as a blind rivet.
[0061] (Activation step S107) In the activation step S107, the energy storage cell 100 in which the liquid injection hole 15 has been sealed through the liquid injection hole sealing step S106 is charged while a load is applied in the thickness direction of the energy storage cell 100. This causes a coating to be formed on the surface of the negative electrode active material layer 24a. The activation step S107 is included as an example of the "preparation step S10" in this specification.
[0062] The charging conditions in the activation step S107 are not particularly limited and may be the same as those in conventional manufacturing methods. For example, the activation step S107 can be performed by charging at a current of about 0.05 C to 10 C in a normal temperature environment (e.g., 25° C.) until the SOC (State of Charge) reaches about 20% to 100%.
[0063] In the activation step S107, the load applied to the energy storage cell 100 is preferably 0.5 to 0.7 MPa. With this configuration, the cell thickness change can be kept within a more preferable range (0.051 to 0.055%). The method of applying the load to the energy storage cell 100 is not particularly limited, and any general means that can be used in conventional energy storage cell manufacturing methods can be used. For example, the load can be applied to the energy storage cell 100 by sandwiching a pair of first side walls 12b of the energy storage cell 100 between restraining plates and connecting the restraining plates with a bridging member.
[0064] (Aging process S108) In the aging step S108, the storage cell 100 that has been through the activation step S107 is stored for a predetermined time in a predetermined temperature environment while maintaining the charged state. This makes it possible to more suitably form a coating on the surface of the negative electrode active material layer 24a. Note that in the technology disclosed herein, the aging step S108 is not an essential step. In some preferred embodiments, the aging step S108 can be omitted.
[0065] The conditions of the aging step S108 can be appropriately adjusted according to the required aspect of the coating formation, and are not particularly limited. For example, the cell temperature (aging temperature) in the aging step S108 can be 30°C or higher, preferably 40°C or higher, for example 50°C or higher, and further 60°C or higher. The upper limit of the aging temperature is not particularly limited, but can be set to about 80°C or lower, for example. For temperature management in the aging step S108, for example, a thermostatic bath can be used. The implementation time (aging time) of the aging step S108 can be appropriately changed according to, for example, the aging temperature, and is not particularly limited. For example, when the aging temperature is about 45 to 70°C, the aging time is preferably about 5 to 20 hours. Furthermore, when the aging temperature is about 70 to 75°C, the aging time is preferably about 5 to 15 hours.
[0066] In the aging step S108, aging is preferably performed while applying a load in the thickness direction X of the energy storage cell 100. The amount of load applied to the energy storage cell in the aging step S108 is not particularly limited, but is preferably 0.5 to 0.7 MPa. In addition, the aging step S108 can be performed while maintaining the load applied in the activation step S107.
[0067] The stack 500 can be used for various purposes, but can be suitably used, for example, as a power source (driving power source) for a motor mounted on a vehicle such as a passenger car, a truck, etc. The type of vehicle is not particularly limited, but examples thereof include a plug-in hybrid electric vehicle (PHEV), a hybrid electric vehicle (HEV), and a battery electric vehicle (BEV).
[0068] Hereinafter, examples of the technology disclosed herein will be described, but the technology disclosed herein is not intended to be limited to these examples.
[0069] <Preparing the storage cells> First, 100 storage cells were prepared to construct a stack according to the embodiment. The wound electrode body housed in the storage cell according to the embodiment had a pair of curved parts as shown in FIG. 5, and a strip-shaped positive electrode and a strip-shaped negative electrode were stacked with a strip-shaped separator interposed therebetween and wound in the longitudinal direction. The width (Ln) of the negative electrode active material layer formation region of the storage cell according to the embodiment was set to 28 cm, and the electrode body aspect ratio (the ratio (Ln / T) of the length Ln in the width direction of the negative electrode active material layer to the height T of the wound electrode body) was set to 3.0. The number of stacked positive electrodes in the wound electrode body was set to 100 layers.
[0070] In addition, as Comparative Example 1, 100 storage cells according to Comparative Example 1 were prepared, which were the same as the storage cell according to Example 1 except that an electrode body (i.e., an electrode body that is not a wound electrode body) having a so-called laminated structure in which a substantially rectangular positive electrode and a substantially rectangular negative electrode are laminated in the thickness direction X of the storage cell via a substantially rectangular separator was used, the aspect ratio of the electrode body was 1.6, the shape of the case was changed according to the aspect ratio of the electrode body, and charging and discharging were performed while applying a load of 0.2 MPa in the thickness direction of the storage cell in the activation process. Similarly, as Comparative Example 2, 100 storage cells according to Comparative Example 2 were prepared, which were the same as the storage cell according to Example 1 except that charging and discharging were performed while applying a load of 0.4 MPa in the thickness direction of the storage cell in the activation process.
[0071] <Evaluation of cell thickness change> Three storage cells were randomly sampled from each of Example 1, Comparative Example 1, and Comparative Example 2 (i.e., n=3). The amount of change in cell thickness was evaluated for these storage cells by the above-mentioned method. The autograph used was AG-X Plus (Shimadzu Corporation), and displacement meters for measuring the thickness of the storage cell were installed at two locations on the autograph. First, as shown in FIG. 9, the storage cell was set on the autograph. Then, a load was applied to the storage cell in the thickness direction (shown by the white arrow) at a speed of 0.1 mm / min. The thickness of the storage cell was measured at two points when the load reached 2 MPa. From the measured values, an average value was calculated and set as X1. Then, the load was reduced to 0.01 MPa. This was set as one cycle, and the treatment was performed for three cycles. Then, the amount of change in cell thickness (%) was calculated by the formula (i) using the obtained X1 and X3. The results are shown in Table 1. Cell thickness change (%) = (X1-X3) / X1×100 Formula (i)
[0072] [Table 1]
[0073] <Evaluation of cell thickness variation> Using an autograph, the thickness of the storage cells when a load of 0.2 MPa was applied in the thickness direction of the storage cells according to Example 1, Comparative Example 1, and Comparative Example 2 was measured. The measurement was performed on 100 storage cells prepared in each example. The device used for the measurement was the same as that used for the evaluation of the cell thickness change amount described above. Using the obtained storage cell thickness, the variation in the thickness of the storage cells was evaluated according to formula (ii). The results are shown in Table 1. FIG. 11 shows a graph showing the relationship between the cell thickness change amount and the cell thickness variation. For the cell thickness change amount according to each example in FIG. 11, the average cell thickness change amount for each storage cell was plotted. Cell thickness variation δ (%) = standard deviation / average thickness × 100 Equation (ii)
[0074] <Evaluation of cell swelling rate due to charging and discharging> Here, the cell swelling rate due to charging and discharging was evaluated for the storage cells according to Example 1 and Comparative Examples 1 and 2. Specifically, first, for three storage cells among the storage cells according to Example 1 and Comparative Examples 1 and 2, which were used for the evaluation of the cell thickness change amount, the thickness of the storage cell was measured when a load of 0.2 MPa was applied in the thickness direction of the storage cell, and the measured value was defined as the pre-test cell thickness. The storage cells according to Example 1 and Comparative Examples 1 and 2 were placed in a temperature environment of 40°C, and an operation of charging and discharging at a current rate of 1 / 5C in a range of SOC of 0 to 100% was repeated 1000 cycles. Then, for the storage cells after 1000 cycles of charging and discharging, the thickness of the storage cell after the test when a load of 0.2 MPa was applied in the thickness direction of the storage cell was measured, and the measured value was defined as the post-test cell thickness. The cell swelling rate due to charging and discharging was evaluated using the following formula (iii). The results are shown in Table 1. FIG. 12 shows a graph showing the relationship between the cell thickness change amount and the cell swelling rate. For the amount of change in cell thickness in each example in FIG. 12, the average value of the amount of change in cell thickness for each power storage cell is plotted. Cell swelling rate due to charging and discharging (%) = (cell thickness after test - cell thickness before test) / cell thickness before test × 100 Formula (iii)
[0075] <Result> As can be seen from Table 1, in the energy storage cell in which the cell thickness change amount was within the range of 0.051 to 0.055% as in Example 1, both the variation in the thickness of the energy storage cell and the cell swelling rate after 1000 cycles of charge and discharge were suppressed compared to Comparative Examples 1 and 2. Therefore, in the stack in which the energy storage cells of Example 1 are stacked, the variation in the thickness of the energy storage cells is small, so that the stacking process can be easily performed and thickness change (swelling) due to charge and discharge can be suppressed even after the stack is constructed.
[0076] Although the preferred embodiment of the present disclosure has been described above, the above embodiment is merely an example. The present disclosure can be implemented in various other forms. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes to the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modification, and it is also possible to add another modification to the above-mentioned embodiment. In addition, if the technical feature is not described as essential, it is also possible to delete it as appropriate.
[0077] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Item 1: A manufacturing method for a stack including a plurality of rectangular storage cells, the manufacturing method for a stack including the storage cell comprising: a preparation step of preparing the storage cell including a flat-shaped wound electrode body formed by stacking and winding a positive electrode and a negative electrode with a separator interposed therebetween, a non-aqueous electrolyte, and a case that accommodates the wound electrode body and the non-aqueous electrolyte; and a stacking step of stacking a plurality of the storage cells along a thickness direction of the storage cell, wherein when a process of applying a load to the storage cell prepared in the preparation step in the thickness direction of the storage cell at a rate of 0.1 mm / min up to 2.0 MPa and reducing the load to 0.01 MPa after the application is defined as one cycle, and when the process is performed for three cycles, a change amount ((X1-X3) / X1×100) of a thickness X3 of the storage cell when 2.0 MPa is applied in a third cycle relative to a thickness X1 of the storage cell when 2.0 MPa is applied in a first cycle is 0.051 to 0.055%. Item 2: The method for manufacturing a stack according to item 1, wherein the negative electrode comprises a negative electrode core and a negative electrode active material layer formed on the negative electrode core, and a length Ln of the negative electrode active material layer in a width direction perpendicular to the longitudinal direction of the wound electrode body is 20 cm or more. Item 3: The method for producing a stack according to item 2, wherein, when a length in a direction perpendicular to a winding axis direction of the wound electrode body and perpendicular to a thickness direction of the wound electrode body is defined as a height T of the wound electrode body, a ratio (Ln / T) of a length Ln in a width direction of the negative electrode active material layer to the height T of the wound electrode body is 2.8 to 3.2. Item 4: The method for manufacturing a stack according to any one of Items 1 to 3, wherein the preparation step includes an activation step of charging the storage cells while applying a load to the storage cells in a thickness direction of the storage cells, and the load applied to the storage cells in the activation step is 0.5 to 0.7 MPa. Item 5: The method for producing a stack according to any one of Items 1 to 4, wherein the number of laminations of the positive electrode is 30 or more. [Explanation of symbols]
[0078] 10 Cases 12 Exterior body 14 Sealing plate 20 Wound electrode body 22 Positive electrode 24 Negative electrode 26 Separator 100 Energy Storage Cells 300 Restraint mechanism 500 stack 600 Autograph S10 Preparation process S20 Lamination process S101 Assembly process S102 Drying process S103 Liquid injection process S104 Gas removal and charging process S105 Decompression process S106 Liquid injection hole sealing process S107 Activation process S108 Aging process
Claims
1. A method for manufacturing a stack including a plurality of rectangular storage cells, comprising the steps of: a preparation step of preparing the storage cell including a flat-shaped wound electrode body formed by stacking and winding a positive electrode and a negative electrode with a separator interposed therebetween, a non-aqueous electrolyte, and a case for accommodating the wound electrode body and the non-aqueous electrolyte; A stacking step of stacking a plurality of the storage cells along a thickness direction of the storage cells, A load was applied to the storage cell prepared in the preparation step in a thickness direction of the storage cell at a rate of 0.1 mm / min up to 2.0 MPa, and the load was then reduced to 0.01 MPa, which was defined as one cycle. When the treatment was performed three times, The change in thickness X3 of the storage cell when 2.0 MPa is applied in the third cycle relative to the thickness X1 of the storage cell when 2.0 MPa is applied in the first cycle ((X1-X3) / X1x100) is 0.051 to 0.055%; A method for manufacturing a stack.
2. The negative electrode includes a negative electrode core and a negative electrode active material layer formed on the negative electrode core, The length Ln in the width direction of the negative electrode active material layer perpendicular to the longitudinal direction of the wound electrode body is 20 cm or more. A method for manufacturing the stack according to claim 1 .
3. When the length in a direction perpendicular to the winding axis direction of the wound electrode body and perpendicular to the thickness direction of the wound electrode body is defined as the height T of the wound electrode body, a ratio (Ln / T) of a length Ln in a width direction of the negative electrode active material layer to a height T of the wound electrode body is 2.8 to 3.2; A method for manufacturing the stack according to claim 2 .
4. the preparation step includes an activation step of charging the storage cell while applying a load in a thickness direction of the storage cell, In the activation step, a load applied to the storage cell is 0.5 to 0.7 MPa. A method for manufacturing a stack according to claim 1 or 2.
5. The number of layers of the positive electrode is 30 or more. A method for manufacturing a stack according to claim 1 or 2.
Citation Information
Patent Citations
Lithium secondary battery and fabricating method for electrode plate
JP2000133316A
Manufacturing method of nonaqueous electrolyte secondary battery
JP2005085627A
Method for evaluating internal short circuiting of battery, device for evaluating internal short circuiting of battery, battery, battery pack and their manufacturing methods
JP2008218390A
Sealed lithium secondary battery and manufacturing method of the same
JP2013125650A
Electrodes, batteries, and battery packs
JP7247353B2